Porous silicone material, electricity storage device and method for producing porous silicone material
A porous silicon material with reduced resistivity is achieved by using an Al-Si-Cr ternary alloy, ensuring efficient electrical conductivity and battery performance through controlled porosity and oxygen content, addressing the inefficiencies of copper-based materials.
Patent Information
- Application Number
- JP2023049655
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing porous silicon materials require a significant amount of copper to achieve low resistivity, leading to increased material costs and potential inefficiencies.
A novel porous silicon material is developed by using an Al-Si-Cr ternary alloy, where Si and Cr silicide coexist, with controlled oxygen content and porosity, to reduce resistivity through a method involving melting, rapid solidification, and selective removal of the Al component.
The resulting porous silicon material exhibits reduced resistivity and improved electrical conductivity, maintaining battery capacity and cycle stability, while minimizing the need for conductive phases.
Smart Images

Figure 2024138928000004 
Figure 2024138928000005 
Figure 2024138928000006
Abstract
Description
[Technical field]
[0001] Disclosed herein are porous silicon materials, electrical storage devices and methods for making the porous silicon materials. [Background technology]
[0002] Conventionally, a porous silicon material has been proposed for silicon anode materials, which is obtained by removing Al by treating AlSiCu alloy powder with hydrochloric acid or the like (for example, Non-Patent Document 1). It is said that this porous silicon material ensures good electronic conductivity of silicon and suppresses volume expansion during charging and discharging by incorporating copper into the porous silicon material. [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] Journal of Power Sources 455 (2020) 227967 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the porous silicon material of the above-mentioned Non-Patent Document 1, although electronic conductivity is ensured by copper, there is a problem that a relatively large amount of copper is required to further reduce the resistivity. For this reason, a new porous silicon material with further reduced resistance has been desired.
[0005] The present disclosure has been made in consideration of such problems, and has as its main object to provide a novel porous silicon material, an electricity storage device, and a method for producing a porous silicon material, which have reduced resistance. [Means for solving the problem]
[0006] As a result of intensive research to achieve the above-mentioned object, the present inventors have found that by melting and rapidly solidifying an Al-Si-Cr ternary alloy raw material having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium diagram, to prepare a silicon alloy precursor, and then removing the Al component, a porous silicon material having a skeleton in which Si and Cr silicide coexist and low resistivity can be obtained. In this case, oxygen may be incorporated into the porous silicon material due to the removal of the Al component, but it has been found that the resistivity can be further reduced by suppressing the amount of oxygen, and thus the porous silicon material, the power storage device, and the method for producing the porous silicon material disclosed herein have been completed.
[0007] That is, the porous silicon material of the present disclosure has: The material has a skeleton in which Si and Cr silicide containing at least an AlSiCr compound coexist, and when the sum of the Si amount, Al amount, and Cr amount is taken as 100 at%, the oxygen amount is 25 at% or less, the O / Cr ratio, which is the ratio of the oxygen amount to the Cr amount, is 10 or less, and the porosity determined by mercury intrusion porosimetry is 55 vol% or more.
[0008] The electricity storage device of the present disclosure comprises: a positive electrode including a positive electrode active material; A negative electrode containing the above-mentioned porous silicon material as a negative electrode active material; an ion conductive medium interposed between the positive electrode and the negative electrode and conducting lithium ions; It is equipped with the following:
[0009] The method of making the porous silicon material of the present disclosure comprises: A method for producing the porous silicon material described above, comprising the steps of: a precursor process for obtaining a precursor of a silicon alloy by melting and rapidly solidifying an Al-Si-Cr ternary alloy raw material having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium phase diagram; a porosity forming step of removing an Al component contained in the silicon alloy to obtain the porous silicon material; It includes. Effect of the Invention
[0010] The present disclosure can provide a novel porous silicon material, a power storage device, and a method for manufacturing a porous silicon material with a further reduced resistivity. The reason why such an effect is obtained is presumed to be as follows. For example, when a raw material of an Al-Si-Cr ternary alloy having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium diagram is melted and rapidly solidified to prepare a precursor of a silicon alloy, and the Al component is removed, a porous silicon material having a skeleton in which Si and Cr silicide coexist is obtained. In such a porous silicon material, since the conductive phase Cr silicide exists along the skeleton that serves as a conductive path, it is presumed that electrical conduction is efficiently performed and the resistivity can be reduced. At that time, when components other than the Al phase are partially removed during the Al removal process, oxygen is taken into the porous silicon material, and an insulating phase such as SiO2 (e.g., amorphous silica) is formed, which may inhibit electrical conduction, but it is presumed that the amount of oxygen taken in can be reduced by removing Al under milder conditions, thereby suppressing the inhibition of electrical conduction and further reducing the resistivity. [Brief description of the drawings]
[0011] [Figure 1] Al-Si-Cr phase diagram at 25at%Si. [Diagram 2] Schematic diagram of the process of microstructure formation in the outermost layer during the cooling process of a molten droplet. [Diagram 3] Al-Si-Cr phase diagram in Al85-ySi15Cry. [Figure 4] Al-Si-Cr phase diagram in Al80-ySi20Cry. [Diagram 5] Al-Si-Cr phase diagram in Al75-ySi25Cry. [Figure 6] Al-Si-Cr phase diagram in Al70-ySi30Cry. [Figure 7] Al-Si-Cr phase diagram in Al60-ySi40Cry. [Figure 8] FIG. 2 is an explanatory diagram of the range of eutectic compositions in the Al-Si-Cr system. [Figure 9] FIG. 2 is an explanatory diagram showing an example of the structure of an electricity storage device 10. [Figure 10] FIG. 2 is an explanatory diagram illustrating electrical conduction in a porous silicon material 20. [Figure 11] XRD pattern of Al73.5Si25Cr1.5 atomized powder. [Figure 12] Graph showing the change in oxygen and chromium content in Al69Si30Cr1 atomized powder with acid treatment time. [Figure 13] XRD patterns of the porous silicon materials of Examples 11, 28, and 29. [Figure 14] 1 shows XRD patterns of samples of the porous silicon materials of Experimental Examples 1 to 4 that were heat-treated at 600°C. [Figure 15] 13 is a cross-sectional secondary electron image of the porous silicon material of Experimental Example 8. [Figure 16] STEM / EDX elemental mapping of the porous silicon material of Example 8. [Figure 17] Electron diffraction results of the porous silicon material of Experimental Example 8. [Figure 18] STEM / EDX elemental mapping of the porous silicon material of Example 4. [Figure 19] STEM / EDX elemental mapping of the porous silicon material of Experimental Example 1. [Figure 20] 1 is a graph showing the effect of chromium silicide concentration on the resistivity of a porous body. [Figure 21] 1 is a graph showing the change in oxygen amount relative to the chromium silicide concentration. [Figure 22] 1 is a graph showing the change in resistivity versus Cr content. [Figure 23] 1 is a graph showing evaluation results of rate characteristics in Experimental Examples 1, 3, and 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Method of manufacturing porous silicon material) The manufacturing method of the porous silicon material of the present disclosure includes a precursor process and a porosity process. In the precursor process, a process is performed in which a raw material of an Al-Si-Cr ternary alloy having a composition in which an Al phase, a Si phase, and a Cr silicide phase containing at least an AlSiCr compound appear at room temperature in an equilibrium diagram is melted and rapidly solidified to obtain a precursor of a silicon alloy. The Cr silicide phase contains at least an AlSiCr compound containing Al, Si, and Cr. The Cr silicide may contain a SiCr compound containing Si and Cr. In the porosity process, a process is performed to remove a part of the Al component contained in the silicon alloy to obtain a porous silicon material. The porous silicon material obtained by this manufacturing method of the porous silicon material has a structure having a skeleton in which, for example, Si and Cr silicide containing at least an AlSiCr compound coexist. Such a structure is also called a coexistence type structure. CrSi2, Cr(Al,Si)2, Al 13 Since Cr silicide phases such as Si4Cr4 are conductive, the electrical conductivity can be improved by making Cr silicide coexist as a conductive phase in the Si skeleton, which is the conductive path. In addition, since the strength of Cr silicide is about twice that of Si, it is expected that the strength of the skeleton can be improved by making Cr silicide coexist as a reinforcing phase in the Si skeleton.
[0013] Figure 1 is an Al-Si-Cr phase diagram at 25at%Si. Figure 2 is a schematic diagram of the microstructure formation process of the outermost surface layer during the cooling process of the molten liquid droplet. The formation of the coexistence structure by adding Cr is influenced by the precipitation order of each phase of the Al-Si-Cr system. Here, we will explain the case where the alloy melt is cooled by the gas atomization method as an example. In the gas atomization method, the high-temperature melt is sprayed into a high-pressure gas from a hole at the tip of the nozzle and cooled. At this time, when the melt (Figure 1(1)) is cooled to the temperature of Figure 1(2), CrSi2 is first crystallized from the low-temperature droplet surface (Figure 2(2)), but CrSi2 gradually coarsens in the coexistence temperature region with the melt (Figure 1(3)) (Figure 2(3)). At that time, if CrSi2 becomes too coarse, the surroundings of the generated silicon powder will be covered with inactive CrSi2 in a shell shape (Figure 2(3-2)), which is not preferable because it reduces the conductive path of the carrier ion (Li) on the active material surface. However, in the phase diagram of the AlSiCr system, when it is cooled to the temperature of Figure 1 (4), CrSi2 decomposes (peritectic reaction) and simultaneously Si and Al 13 Since Si4Cr4 precipitates (eutectic reaction), a conductive path for active carrier ions (i.e., Si phase) is formed on the surface of the active material, which is more preferable. Furthermore, this peritectic reaction generally proceeds as follows: L + CrSi2 ⇒ Al 13 This refers to a reaction in which a molten liquid reacts with a solid phase to produce another solid phase, such as Si4Cr4. However, since the reaction proceeds from the surface of the solid phase particles, fine CrSi2 particles are surrounded by Al 13 A structure is formed in which the shell of Si4Cr4 and Si is coated. Thus, in the temperature region of Figure 1 (5), CrSi2 (which may actually be Cr(Al,Si)2) becomes Al. 13 Since a reaction occurs in which the CrSi4 crystals decompose into CrSi4 and Si, the Si and Al crystals move around the position of the CrSi2 crystal nucleus that was initially formed. 13 A state is created in which cluster particles in which Cr4Si4 nanoparticles coexist in close proximity are dispersed in the melt (Fig. 2(5)). Then, when the Al melt finally solidifies, the Si and Al of the clusters are dissolved. 13The Cr4Si4 nanoparticles are linked together to form a structure in which Si and Cr silicide coexist in the framework, and by removing Al from this by acid treatment, a composite porous material with a coexisting structure is obtained. If the cooling rate is sufficiently high, it is thought that the material will cool before the peritectic reaction is completed, and some of the CrSi2 near the particle surface will remain as a non-equilibrium phase. During the cooling process described above, the peritectic reaction causes Al to surround the fine CrSi2 particles, 13 The formation of a structure in which the Si4Cr4 and Si cores are covered results in a finer microstructure. 13 In addition to the fineness of Si4Cr4, the Al alloy that is the source of the pores is also refined. 13 Since the difference in precipitation temperatures between Si4Cr4 and Al is relatively small (up to 350°C), the crystal growth of these particles is small, and a nano-sized microstructure can be achieved. The solidification structure forms a lamellar structure consisting of SiCr compounds, AlSiCr compounds, AlCr compounds, eutectic Si, primary Si, and primary Al. Compounds that dissolve in acid include primary Al, AlSiCr compounds, and AlCr compounds, and it is presumed that the structure obtained after acid treatment will be a skeletal porous body consisting of the remaining SiCr compounds, eutectic Si, primary Si, as well as undissolved primary Al, AlSiCr compounds, and AlCr compounds.
[0014] 3 to 7 are phase diagrams of Al-Si-Cr alloys when the contents of Si and Cr are changed. 85-y S 15 Cr y FIG. 4 shows the Al-Si-Cr phase diagram. 80-y S 20 Cr y FIG. 5 shows the Al-Si-Cr phase diagram. 75-y S 25 Cr y FIG. 6 shows the Al-Si-Cr phase diagram. 70-y S 30 Cr y FIG. 7 shows the Al-Si-Cr phase diagram. 60-y S 40 Cr yFIG. 8 is an explanatory diagram of the range of eutectic compositions in Al-Si-Cr system compositions. To realize a coexisting structure, as described above, it is necessary to go through a state in which cluster particles of Si and Cr silicide are dispersed in the Al melt or a state close to that, and the ideal composition range is one in which Si and Cr silicide are precipitated simultaneously by a eutectic reaction. As shown in FIGS. 3 to 7, the Al 100-x-y S x Cr y In the basic composition, when the Si content x is less than 18 at%, the composition does not show a eutectic reaction between Si and silicide. On the other hand, when the Si content x is 18 at% or more, especially 25 at% or more, depending on the Cr content y, the composition shows the following reactions: L ⇒ Si + CrSi2 (eutectic reaction 1) and L ⇒ Si + Al 13 There exists a composition that causes the eutectic reaction of Si4Cr4 (eutectic reaction 2). Figure 8 shows the relationship between the amount of Si x and the amount of Cr y that causes these eutectic reactions 1 and 2. In the composition region shown by the diagonal lines, in addition to Si and CrSi2 crystallizing at relatively close temperatures, the reaction CrSi2+L⇒Al 13 It is presumed that this is a more preferable composition range because a peritectic reaction of Si4Cr4 occurs, resulting in a finer pore structure. 100-x-y S x Cr y In the above, x and y are in the ranges of 18≦x≦40 and 0.1≦y≦15. Also, based on Fig. 8, Cr is preferably 0.1 at% or more, more preferably 0.5 at% or more, and even more preferably 1 at% or more, relative to the total of Al and Si. Furthermore, in Fig. 8, among the composition regions shown by hatching, the composition region where Cr is 10 at% or less, that is, the composition region surrounded by a thick line and colored gray, is more preferable from the viewpoint of increasing the capacity of the electricity storage device, since the amount of silicide that does not contribute to the charge and discharge reaction does not become too large.
[0015] (Precursor process) In the precursor process, a raw material of an Al-Si-Cr ternary alloy having a composition in which an Al phase, a Si phase, and a Cr silicide phase appear at room temperature is melted and rapidly solidified to obtain a precursor of a silicon alloy. The precursor of the silicon alloy may be, for example, a precursor in which Si and Cr silicide coexist in the skeleton portion that forms the pores. In this process, a raw material may be used that contains Cr in the range of 0.1 at% to 20 at% and Al in the range of 40 at% to 90 at% and the remainder is Si, when the total of Si, Al, and Cr is 100 at%. In the raw material composition, Cr is preferably 0.1 at% or more, further preferably 0.5 at% or more, and more preferably 1 at% or more. As described above, the raw material composition is represented by the basic composition formula Al 100-x-y S x Cr yIn the above, it is more preferable that x / y is in the range of 18≦x≦40 and 0.1≦y≦15. Of these, it is more preferable that x / y≧8 is satisfied. The value of x / y may be 10 or more, or 20 or more. The value of x / y may be 50 or less, or 40 or less. The raw material may contain unavoidable impurities. The unavoidable impurities are components that inevitably remain during the purification of any of Si, Cr, and Al, and examples of such impurities include Fe, C, Cu, Ni, and P. It is preferable that the amount of unavoidable impurities is as small as possible, and for example, when the total amount of Si, Cr, and Al is 100 at%, it is preferably 5 at% or less, and more preferably 2 at% or less. The compounding ratio of Cr is, for example, preferably 0.1 at% or more, and may be 0.5 at% or more. The compounding ratio of Cr is preferably 10 at% or less, and may be 5 at% or less, or may be 3 at% or less. The compounding ratio of Al is preferably 50 at% or more, and may be 55 at% or more or 60 at% or more. The compounding ratio of Al is preferably 85 at% or less, more preferably 80 at% or less, and may be 77.5 at% or less. The compounding ratio of Si is, for example, preferably 15 at% or more, more preferably 18 at% or more, and may be 20 at% or more or 25 at% or more. The compounding ratio of Si is, for example, preferably 59 at% or less, more preferably 50 at% or less, and may be 40 at% or less or 30 at% or less. A silicon alloy containing Al and Cr in such a range is preferable because it can increase the porosity and obtain voids of a more suitable shape and size. If the content of Al is high, when the alloy is melted to form an alloy and then rapidly cooled, a single phase of Al is largely precipitated, so that many voids can be formed. The cooling rate is preferably more rapid, for example, 10% or less from the molten state. 2 ℃ / s or more 10 8 ° C. / s or less.
[0016] In this process, when melting the raw material, high-frequency crucible melting in an inert gas atmosphere such as Ar is preferable, but any melting method may be used. The production of the master alloy requires melting of the raw material powder, and high-frequency melting is more preferable to produce a uniform sample, but melting may simply be performed by heating and melting in an electric furnace or using an electron beam. In the precursor process, the alloy obtained from the raw material may be granulated. In this granulation process, the molten metal of the raw material of the silicon alloy may be cast into a mold, and the obtained ingot may be crushed and granulated. In addition, the method of granulating the silicon alloy may be one or more of the gas atomization method, water atomization method, and roll quenching method. In the gas atomization method and the water atomization method, an alloy powder is obtained. On the other hand, since the roll quenching method produces a thin strip alloy, it may be crushed and powdered afterwards. Since the powder obtained by the roll quenching method has a fine alloy structure, porous silicon having fine pores can be obtained after the elution process. Of these, the gas atomization method is more preferable as the method of granulating the silicon alloy. In gas atomization, it is preferable to carry out the molten metal in an Ar atmosphere, and the granulation in an Ar or He atmosphere.
[0017] In the precursor process, the silicon alloy is preferably granulated to have a particle size in the range of 0.1 μm to 100 μm. The silicon alloy particles preferably have an average particle size in the range of 0.5 μm to 10 μm, and may have an average particle size in the range of 1 μm to 5 μm or 2 μm to 5 μm. In this process, the particle size of the silicon alloy particles may be 100 μm or less, 10 μm or less, or 5 μm or less by classification. In this process, the particle size of the silicon alloy particles may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, or 2 μm or more by classification. The silicon alloy particles may be appropriately selected according to the characteristics required for the power storage device. Here, the average particle size of the particles is determined by observing the particles with a scanning electron microscope (SEM), tallying the major axis of each particle as the diameter of the particle, and dividing it by the number of particles to obtain an average value. The particles obtained by this particulation process have an average particle size of the aggregate of porous particles that is to be finally obtained.
[0018] In this precursor process, a raw material containing a second element including one or more of Ca, Mg, Na, Sr, and P in addition to Al, Cr, and Si may be used. Among these, the second element is preferably one or more of Ca, Na, and Sr. The content of the second element is preferably less than that of Al or Cr, and is preferably in the range of 10 mass% or less, more preferably 5 mass% or less, based on the entire silicon alloy. In this precursor process, a raw material having a composition in which a part of Cr is replaced with another transition metal element M may be used. In this case, the transition metal element M may be half or less of Cr in molar ratio, 20% or less, or 10% or less. Examples of the transition metal element M include Ti, V, Nb, Mo, Ni, Mn, Fe, Co, and Zn.
[0019] (Porous process) In the porosity forming step, a removal treatment is carried out to remove the Al component contained in the silicon alloy prepared above. Examples of the Al component to be removed in this step include Al and its compounds.
[0020] This porosity forming step is preferably carried out under conditions where the increase in oxygen is 7 at% or less. The increase in oxygen may be 5 at% or less, 4 at% or less, or 2 at% or less. The increase in oxygen may be smaller, for example, 1.8 at% or less, 1.5 at% or less, or 1.3 at% or less. The increase in oxygen may be 0.1 at% or more, 0.5 at% or more, or 0.9 at% or more. When it is assumed that the amount of Si is unchanged before and after the removal process, the increase in oxygen may be calculated from the ratio of the amount of oxygen (element ratio) after the removal process to the amount of Si (element ratio) based on the amount of Si (element ratio) before the removal process. Specifically, the increase in oxygen GO [at%] is a value calculated from the formula GO=O2×S1 / S2-O1. Here, the element ratios of Al, Si, Cr, and O obtained by EDX for the silicon alloy before the removal process are A1 [at%], S1 [at%], C1 [at%], and O1 [at%] (where A1 + S1 + C1 = 100), and the element ratios of Al, Si, and Cr obtained by EDX for the porous silicon material after the removal process are A2 [at%], S2 [at%], C2 [at%], and O2 [at%] (where A2 + S2 + C2 = 100), respectively. Note that, for example, since Si does not dissolve in hydrochloric acid, when the removal process is performed by acid treatment with hydrochloric acid, it can be assumed that the amount of Si remains unchanged before and after the removal process.
[0021] The porosity forming step may be performed under conditions where the amount of Cr reduction is 60% or less of the amount of Cr reduction when Cr is completely removed. The amount of Cr reduction may be 55% or less of the amount of Cr reduction when Cr is completely removed, or may be 50% or less. The amount of Cr reduction is preferably as small as possible, but may be 5% or more, 20% or more, or 30% or more of the amount of Cr reduction when Cr is completely removed. The porosity forming step may be performed under conditions where the amount of Cr reduction is 0.5 at% or less than the amount of Cr reduction when Cr is completely removed. The amount of Cr reduction may be 0.6 at% or more, or 0.7 at% or more less than the amount of Cr reduction when Cr is completely removed. The amount of Cr reduction may be 1.0 at% or less, 0.9 at% or less, or 0.8 at% or less less than the amount of Cr reduction when Cr is completely removed. The amount of Cr reduction may be, for example, -0.6 at% or less. The amount of Cr reduction is preferably as small as possible, but may be, for example, -0.1 at% or more, -0.3 at% or more, or -0.4 at% or more. This porosity forming step may be performed under conditions where the amount of Al reduction exceeds 90% of the amount of Al reduction when Al is completely removed, or may be 95 at% or more. The amount of Al reduction may be, for example, -40 at% or more and -75 at% or less, or -50 at% or more and -70 at% or less.
[0022] Here, when it is assumed that the amount of Si is unchanged before and after the removal process, the amount of Cr and the amount of Al decreased may be calculated from the ratio of the amount of Cr or Al (element ratio) after the removal process to the amount of Si (element ratio) based on the amount of Si (element ratio) before the removal process. Specifically, the amount of Cr decreased LC [at %] is a value calculated by the formula LC = C2 × S1 / S2-C1, and the amount of Al decreased LA [at %] is a value calculated by the formula LA = A2 × S1 / S2-A1. Here, the element ratios of Al, Si, and Cr obtained by EDX for the silicon alloy before the removal process are A1 [at%], S1 [at%], and C1 [at%], respectively (where A1+S1+C1=100), and the element ratios of Al, Si, and Cr obtained by EDX for the porous silicon material after the removal process are A2 [at%], S2 [at%], and C2 [at%], respectively (where A2+S2+C2=100). Note that, for example, since Si does not dissolve in hydrochloric acid, when the removal process is performed by acid treatment with hydrochloric acid, it can be assumed that the amount of Si remains unchanged before and after the removal process.
[0023] In the porosity forming step, it is preferable to selectively remove the Al component, that is, the Al phase and its compounds, by using an acid or an alkali. The removal treatment using an acid is also called an acid treatment, and the removal treatment using an alkali is also called an alkali treatment. The acid or alkali used is preferably one that dissolves elements and / or compounds other than silicon in the silicon alloy and does not dissolve silicon, and examples of such acids include hydrochloric acid, sulfuric acid, and sodium hydroxide. This acid or alkali is preferably an aqueous solution. The concentration of the acid or alkali is not particularly limited as long as it is within a range that can remove the Al component, and may be, for example, 0.01 mol / L or more, 0.02 mol / L or more, or 0.05 mol / L or more. The concentration of the acid or alkali may be, for example, 5 mol / L or less, 3 mol / L or less, or 1.5 mol / L or less. The concentration of the acid or alkali is preferably low from the viewpoint of suppressing the incorporation of oxygen into the porous silicon material, and may be, for example, less than 1 mol / L, more preferably less than 0.5 mol / L, further preferably less than 0.2 mol / L, or may be 0.1 mol / L or less. The temperature during the removal process may be, for example, less than 40°C, 35°C or less, or 30°C or less. The temperature during the removal process may be, for example, 0°C or more, 5°C or more, or 10°C or more. The time during the removal process may be, for example, 1 hour or more, or 2 hours or more. The time during the removal process may be, for example, 24 hours or less, 12 hours or less, or 10 hours or less. This removal process is preferably performed by immersing the silicon alloy in an acid or alkali solution and stirring as necessary. The obtained porous silicon material is then washed and dried.
[0024] (Porous silicon material) The porous silicon material of the present disclosure may be one produced by the above-mentioned manufacturing method. This porous silicon material has a skeleton in which Si and Cr silicide containing at least an AlSiCr compound coexist. Cr silicide is a semiconductor with relatively high conductivity, and therefore, the effect of reducing resistance can be expected. In particular, since such Cr silicide coexists with Si and the Cr silicide exists along the skeleton that serves as a conductive path, it is presumed that electrical conduction is performed efficiently and the resistivity can be further reduced. The Cr silicide phase may be a CrSi compound or an AlCrSi compound, but an AlCrSi compound is preferred. The Cr silicide phase may be CrSi2, Cr(Si,Al)2, Al 13 Cr4Si4, Cr(Si,Al)2, Al 13 The porous silicon material may be one or more of Cr4Si4. The Cr silicide may be present as an amorphous phase. The porous silicon material may include an Al phase. Since Al has high conductivity as a metal phase, it is expected to have an effect of reducing resistance. In addition, since Al has charge / discharge capacity as an active material of an electricity storage device, it is expected to have an effect of mitigating the decrease in capacity due to the coexistence of a conductive phase.
[0025] In this porous silicon material, when the total of the Si amount, the Al amount, and the Cr amount is taken as 100 at%, the oxygen amount is 25 at% or less, and the O / Cr ratio, which is the ratio of the oxygen amount to the Cr amount, is 10 or less. The smaller the oxygen amount is, and the lower the ratio of the oxygen amount to the Cr amount is, the lower the resistivity tends to be, and this is presumably due to the fact that there is less insulating phase SiO2 and the like. The above-mentioned oxygen amount is preferably 20 at% or less, and may be 18 at% or less, 15 at% or less, or 10 at% or less. The oxygen amount may be 3 at% or more, 5 at% or more, or 10 at% or more. The above-mentioned O / Cr ratio may be 9 or less, 8 or less, or 5 or less. The O / Cr ratio may be 2 or more, or 3 or more. The porous silicon material preferably satisfies one or more of (1) the above-mentioned oxygen amount is 10 at% or less, or (2) the O / Cr ratio is 5 or less. If any of these is satisfied, the resistivity can be further reduced.
[0026] In this porous silicon material, when the sum of the Si amount, Al amount, and Cr amount is taken as 100 at%, the Cr amount is more than 0 at% and 5 at% or less, and the Al / Cr ratio, which is the ratio of the Al amount to the Cr amount, may be 2 or more and 7 or less. This Al / Cr ratio may be 6 or less, 5 or less, or 4 or less. This Al / Cr ratio may be 3 or more. Note that the Al / Cr ratio may be 30 or less, 20 or less, or 10 or less.
[0027] In the porous silicon material, from the viewpoint of reducing resistivity, it is preferable that the Al content is high. For example, when the total of the Si content, the Al content, and the Cr content is 100 at%, the Al content may be 6 at% or more, 7 at% or more, or 10 at% or more. This Al content may be, for example, 50 at% or less, 30 at% or less, 25 at% or less, 20 at% or less, or 15 at% or less. In addition, in the porous silicon material, from the viewpoint of increasing strength, it is preferable that the Cr content is high. For example, when the total of the Si content, the Al content, and the Cr content is 100 at%, the Cr content may be 0.5 at% or more, 0.7 at% or more, or 1 at% or more. This Cr content may be, for example, 10 at% or less, 7 at% or less, or 5 at% or less. In this porous silicon material, when the total amount of Si, Al and Cr is taken as 100 at%, the amount of Si may be 93 at% or less, 92 at% or less, or 90 at% or less, and the amount of Si may be 50 at% or more, 70 at% or more, or 75 at% or more.
[0028] In this porous silicon material, when the total of the Si phase, the Cr silicide phase, the SiO2 phase, and the Al phase is taken as 100 mol%, the content of the Cr silicide phase may be 10 mol% or less, 7 mol% or less, 6 mol% or less, or 2 mol% or less. The content of the Cr silicide phase may be 0.1 mol% or more, 0.5 mol% or more, or 1 mol% or more. In this porous silicon material, the content of the Si phase may be 96 mol% or less, 90 mol% or less, or 85 mol% or less. The content of the Si phase may be 65 mol% or more, 70 mol% or more, or 75 mol% or more. In this porous silicon material, the content of the SiO2 phase may be 15 mol% or less, 12 mol% or less, or 10 mol% or less. The content of the SiO2 phase may be 0.5 mol% or more, 1 mol% or more, or 3 mol% or more. It is preferable that the porous silicon material does not contain an Al phase. Not containing an Al phase means that no peak of the Al phase is confirmed in X-ray diffraction measurement (XRD). Even if the porous silicon material contains an Al phase, it is preferably 30 mol% or less, more preferably 10 mol% or less, even more preferably 5 mol% or less, and even more preferably 3 mol% or less. The contents of the Si phase, Cr silicide phase, SiO2 phase, and Al phase may be obtained, for example, as follows. The porous silicon material after heat treatment at 600°C is measured by XRD to obtain the ratio of the Si phase, Cr(Al,Si)2 phase, and Al phase, and further the ratio of the SiO2 phase to the Cr(Al,Si)2 phase is obtained from the element ratio of Cr and O, and the content of each phase may be calculated by taking the total of the Si phase, Cr(Al,Si)2 phase, Al phase, and SiO2 phase as 100 mol%. Note that, when it is confirmed that the Al phase is not contained in the XRD, it may be calculated from the element ratio of Al, Si, Cr, and O on the assumption that the phases present in the sample are Si, Cr(Al,Si)2, and SiO2. In this case, it may be assumed that the Si phase contains (is substituted with) 5 at % Al, and the remaining Al is entirely contained in the Cr(Al,Si)2 phase. 80 S 20When an AlSi alloy that does not contain Cr, such as the above, is treated with acid, the XRD results confirm only the Si phase and no Al phase, but the composition analysis results confirm the presence of approximately 5 at% Al. Similar results were obtained when an AlSi alloy with a different composition was used, and it is believed that Al is in solid solution with the Si phase. It is presumed that in the AlSiCr system, it can be assumed that the Si phase similarly contains 5 at% Al.
[0029] In this porous silicon material, the porosity is 55% by volume or more. This porosity is a value measured by a mercury porosimeter. This porosity may be, for example, 60% by volume or more, 65% by volume or more, or 70% by volume or more. The porosity may be, for example, 85% by volume or less, 80% by volume or less, or 75% by volume or less. A larger porosity is more responsive to volume changes when carrier ions are absorbed, and a smaller porosity is preferable because the amount of Si present per unit volume increases.
[0030] In this porous silicon material, the average pore diameter may be 100 nm or less. In this porous silicon material, the pore diameter may be in the range of 1 nm or more and 300 nm or less. The average pore diameter and the pore diameter are values measured by a mercury porosimeter. The average pore diameter may be 65 nm or less, or 60 nm or less. The average pore diameter may be 10 nm or more, 20 nm or more, or 30 nm or more. The pore diameter range may be, for example, 5 nm or more, 10 nm or more, or 20 nm or more. The pore diameter range may be, for example, 200 nm or less, or 100 nm or less. A small pore diameter is preferable because the pores are less likely to collapse. A large pore diameter is preferable because the volume change can be further suppressed when carrier ions are absorbed.
[0031] The porous silicon material may have a resistivity of 10000 Ωcm or less. The resistivity of the porous silicon material is determined by a four-terminal method. When the porous silicon material is a powder, the porous silicon powder is pressed at 200 MPa to produce a green compact, and the resistivity of the green compact determined by a four-terminal method is determined as the resistivity of the porous silicon material. The resistivity may be 2000 Ωcm or less, 1000 Ωcm or less, 500 Ωcm or less, or 200 Ωcm or less.
[0032] The porous silicon material may include skeletal silicon having a three-dimensional network structure with voids, and may include a SiCr compound and / or an AlSiCr compound as the Cr silicide. It is presumed that the Cr silicide reinforces the silicon skeleton. It is preferable that the amount of Cr silicide is as large as possible from the viewpoint of supplementing the reinforcement of the skeleton, and it is preferable that the amount of Cr silicide is as small as possible from the viewpoint of the charge / discharge capacity of the power storage device.
[0033] The porous silicon material preferably has 20% or more by volume of pores of 1 μm or less by mercury intrusion porosimetry. It is preferable that the porous silicon material has a larger number of such fine pores. The porous silicon material more preferably has 30% or more by volume of pores of 1 μm or less by mercury intrusion porosimetry, more preferably 40% or more by volume, and even more preferably 45% or more by volume. The porous silicon material may also have 90% or less by volume of pores of 1 μm or less by mercury intrusion porosimetry.
[0034] When the porous silicon material is subjected to a confining pressure of 1 GPa as an electrode, the amount of pore change is preferably less than 25 volume %, more preferably less than 20 volume %, and even more preferably less than 10 volume %. From the viewpoint of skeleton strength, it is preferable that the amount of pore reduction of the porous silicon material is as small as possible when subjected to a confining pressure.
[0035] The porous silicon material may contain one or more of Ca, Mg, Na, Sr, and P as a second element in a range of 15 mass% or less. The porous silicon material may also contain inevitable impurities in addition to Si, Al, and Cr. It is preferable that the second element and the inevitable impurities are less. The porous silicon material may have a part of Cr substituted with another transition metal element M. In that case, the transition metal element M may be half or less of Cr in molar ratio, 20% or less, or 10% or less. Examples of the transition metal element M include Ti, V, Nb, Mo, Ni, Mn, Fe, Co, and Zn.
[0036] (Electrodes for electricity storage devices) The electrode for a power storage device includes the porous silicon material described above as an electrode active material. This electrode is either a positive electrode or a negative electrode based on the potential of the counter electrode relative to the potential of the electrode active material, but when lithium is used as a carrier, it is preferable to use the electrode as a negative electrode. This electrode can be used, for example, in a lithium ion secondary battery, a hybrid capacitor, an air battery, etc. The electrode for a power storage device may be one in which the porosity of the porous silicon material is compressed to a range of 5 volume % or more and 50 volume % or less. In this electrode, the porosity of the porous silicon material may be reduced by compressing during production. For example, when porous silicon particles are used as a negative electrode active material for a lithium ion secondary battery, the smaller the pores are, the more uniform the alloying of lithium ions is, so that stress concentration is reduced and deterioration of the electrode itself can be prevented. The porosity of the porous silicon material after compression may be appropriately adjusted according to the characteristics required for the electrode for a power storage device, and may be, for example, 5 volume % or more or 10 volume % or more. The porosity of the porous silicon material after compression may be, for example, 30 volume % or less or 20 volume % or less.
[0037] The electrode for the power storage device may be one in which the porous silicon material is formed on a current collector and fixed on the current collector. This electrode can be produced by a process in which the porous silicon material is mixed with a conductive material and a binder in a solvent as necessary to form a paste and then coated on the current collector, or a process in which the porous silicon material is mixed with a conductive material and a binder as necessary and then pressed onto the current collector. In this electrode, the content of the porous silicon material is preferably higher, preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more. The conductive material is not particularly limited as long as it is an electron conductive material that does not adversely affect the battery performance, and for example, a mixture of one or more of graphite such as natural graphite (scale graphite, scale graphite) and artificial graphite, acetylene black, carbon black, ketjen black, carbon whisker, needle coke, carbon fiber, and metal (copper, nickel, aluminum, silver, gold, etc.) can be used. The binder plays a role of binding the active material particles and the conductive material particles, and may be, for example, fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, or thermoplastic resins such as polypropylene and polyethylene, ethylene propylene diene rubber (EPDM), sulfonated EPDM rubber, natural butyl rubber (NBR), or the like, either alone or as a mixture of two or more kinds. In addition, a cellulose-based aqueous binder or an aqueous dispersion of styrene butadiene rubber (SBR) may also be used. As the solvent, for example, an organic solvent such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, ethylene oxide, or tetrahydrofuran may be used. In addition, a dispersant, a thickener, or the like may be added to water, and the active material may be slurried with latex such as SBR. Examples of the application method include roller coating such as an applicator roll, screen coating, doctor blade method, spin coating, bar coater, and the like, and any of these can be used to obtain any thickness and shape.The current collector may be appropriately selected according to the potential of the active material or the like. For example, in addition to aluminum, titanium, stainless steel, nickel, iron, copper, fired carbon, conductive polymers, conductive glass, etc., for the purpose of improving adhesion, conductivity, and oxidation resistance, those obtained by treating the surface of aluminum or copper with carbon, nickel, titanium, silver, etc. can be used. It is also possible to subject these to surface oxidation treatment. Examples of the shape of the current collector include foil, film, sheet, net, punched or expanded, lath, porous body, foam, and formed body of fiber group. The thickness of the current collector is, for example, 1 to 500 μm. The formation amount of the active material composite may be appropriately set according to the desired performance required for the power storage device.
[0038] In this electrode, the electrode active material may contain, in addition to the porous silicon material, an active material other than the porous silicon material within a range where both low restraint pressure and capacity retention rate can be achieved. For example, as the electrode active material, a carbonaceous material, Li4Ti5O 12 etc. may be included. However, from the viewpoint of further increasing the battery capacity, it is preferable that the porous silicon material occupies 50% by mass or more, preferably 90% by mass or more, with the total electrode active material being 100% by mass.
[0039] (Power storage device) The power storage device of the present disclosure includes an electrode having the above-described porous silicon material. This power storage device may include a positive electrode, a negative electrode, and an ion conduction medium interposed between the positive electrode and the negative electrode for conducting carrier ions. The porous silicon material can be used as a negative electrode active material. This power storage device may be any of a lithium ion secondary battery, a hybrid capacitor, an air battery, etc. In the positive electrode, as the positive electrode active material, sulfides containing transition metal elements, oxides containing lithium and transition metal elements, etc. can be used. Specifically, transition metal sulfides such as CrS2, CrS3, MoS3, FeS2, basic composition formula Li (1-x) MnO2 (0 < x < 1, etc., the same below) and Li (1-x)Lithium manganese composite oxide such as Mn2O4, with the basic composition formula Li (1-x) Lithium cobalt composite oxide with CoO2, etc., with the basic composition formula Li (1-x) Lithium nickel composite oxide such as NiO2, with the basic composition formula Li (1-x) Ni a Co b Mn c Lithium nickel cobalt manganese composite oxides having a basic composition formula of LiO2 (a+b+c=1), lithium vanadium composite oxides having a basic composition formula of LiV2O3, transition metal oxides having a basic composition formula of V2O5, etc. can be used. Among these, lithium transition metal composite oxides, for example, LiCoO2, LiNiO2, LiMnO2, Li (1-x) Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc. are preferred. The term "basic composition formula" means that other elements such as Al and Mg may also be included. Alternatively, the positive electrode active material may be a carbonaceous material used in capacitors, lithium ion capacitors, etc. Examples of carbonaceous materials include activated carbons, cokes, glassy carbons, graphites, non-graphitizable carbons, pyrolytic carbons, carbon fibers, carbon nanotubes, and polyacenes. Of these, activated carbons exhibiting a high specific surface area are preferred. Activated carbons as carbonaceous materials have a specific surface area of 1000 m 2 / g or more, and 1500m 2 / g or more. 2 The specific surface area of this activated carbon is 3000 m2 for ease of preparation. 2 / g or less, and 2 The conductive material, binder, solvent, current collector, and the like used in the positive electrode can be appropriately selected from those exemplified for the electrode described above.
[0040] The ion-conducting medium may be a non-aqueous electrolyte solution containing a supporting salt, a non-aqueous gel electrolyte solution, etc. Examples of the solvent for the non-aqueous electrolyte solution include carbonates, esters, ethers, nitriles, furans, sulfolanes, and dioxolanes, which may be used alone or in combination. Specific examples of carbonates include cyclic carbonates such as ethylene carbonate, propylene carbonate, vinylene carbonate, butylene carbonate, and chloroethylene carbonate; chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl-n-butyl carbonate, methyl-t-butyl carbonate, di-i-propyl carbonate, and t-butyl-i-propyl carbonate; cyclic esters such as γ-butyl lactone and γ-valerolactone; chain esters such as methyl formate, methyl acetate, ethyl acetate, and methyl butyrate; ethers such as dimethoxyethane, ethoxymethoxyethane, and diethoxyethane; nitriles such as acetonitrile and benzonitrile; furans such as tetrahydrofuran and methyltetrahydrofuran; sulfolanes such as sulfolane and tetramethylsulfolane; and dioxolanes such as 1,3-dioxolane and methyldioxolane. Among these, a combination of cyclic carbonates and chain carbonates is preferred. This combination not only provides excellent cycle characteristics, which represent the battery characteristics during repeated charging and discharging, but also allows the viscosity of the electrolyte, the electric capacity of the resulting battery, and the battery output to be well balanced. Examples of the supporting salt include LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiSbF6, LiSiF6, LiAlF4, LiSCN, LiClO4, LiCl, LiF, LiBr, LiI, and LiAlCl4. Among these, it is preferred to use one or more salts selected from the group consisting of inorganic salts such as LiPF6, LiBF4, LiAsF6, and LiClO4, and organic salts such as LiCF3SO3, LiN(CF3SO2)2, and LiC(CF3SO2)3 in combination in terms of electrical properties.The concentration of the supporting salt in the non-aqueous electrolyte is preferably 0.1 mol / L or more and 5 mol / L or less, more preferably 0.5 mol / L or more and 2 mol / L or less. When the concentration of the supporting salt is 0.1 mol / L or more, a sufficient current density can be obtained, and when the concentration is 5 mol / L or less, the electrolyte can be more stabilized. In addition, a phosphorus-based or halogen-based flame retardant may be added to the non-aqueous electrolyte.
[0041] Also, instead of the liquid ion-conducting medium, a solid ion-conducting polymer can be used as the ion-conducting medium. As the ion-conducting polymer, for example, a polymer gel composed of a polymer such as acrylonitrile, ethylene oxide, propylene oxide, methyl methacrylate, vinyl acetate, vinylpyrrolidone, vinylidene fluoride, and a supporting salt can be used. Furthermore, an ion-conducting polymer can be used in combination with a non-aqueous electrolyte. As the ion-conducting medium, in addition to the ion-conducting polymer, an inorganic solid electrolyte, a mixed material of an organic polymer electrolyte and an inorganic solid electrolyte, or an inorganic solid powder bound by an organic binder can be used.
[0042] The power storage device may have a separator between the negative electrode and the positive electrode. The separator is not particularly limited as long as it has a composition that can withstand the range of use of the lithium secondary battery, and examples thereof include polymer nonwoven fabrics such as polypropylene nonwoven fabrics and polyphenylene sulfide nonwoven fabrics, and thin microporous films of olefin resins such as polyethylene and polypropylene. These may be used alone or in combination.
[0043] The shape of the electricity storage device is not particularly limited, but examples thereof include coin type, button type, sheet type, laminated type, cylindrical type, flat type, and square type. The electricity storage device may also be applied to large devices used in electric vehicles and the like. FIG. 9 is an explanatory diagram showing an example of the structure of an electricity storage device 10. The electricity storage device 10 has a positive electrode 12, a negative electrode 15, and an ion conductive medium 18. The positive electrode 12 has a positive electrode active material 13 and a current collector 14. The negative electrode 15 has a negative electrode active material 16 and a current collector 17. The negative electrode active material 16 is the porous silicon material 20 described above, which has a skeleton 25 in which Si 22 and Cr silicide 24 coexist, and voids 26. In the porous silicon material 20, as shown in FIG. 10A, the conductive phase Cr silicide 24 exists along the skeleton 25, which is a conductive path, so that the resistivity can be reduced with a smaller amount of conductive phase, and it is considered that the reduction in battery capacity can also be suppressed. An Al-Si-Cr based master alloy composition is suitable for producing a porous silicon material 20 having such a coexistence type structure. For example, a part of Cr in the Al-Si-Cr based master alloy composition may be replaced with another transition metal element M (Ti, V, Nb, Mo, Ni, Mn, Fe, Co, Zn, etc.). In that case, the porous silicon material 20 may have a dispersed structure in which the silicide of the transition metal element M is dispersed between the skeletons 25 in addition to the above-mentioned coexistence type structure. Incidentally, in a porous silicon material, when the oxygen content exceeds 25 at% or the O / Cr ratio exceeds 10, the conductive phase of the skeleton 25, Cr silicide 24, is divided by the insulating phase, SiO2 28, etc., as in the porous silicon material 20F in Figure 10B, and the resistance may increase. However, in the porous silicon material 20, when the sum of the Si content, Al content, and Cr content is 100 at%, the oxygen content is 25 at% or less, and the O / Cr ratio, which is the ratio of the oxygen content to the Cr content, is 10 or less, and this increase in resistance is suppressed.
[0044] This power storage device preferably has a higher initial charge-discharge efficiency. For example, 1000 mAh / g or more is preferable, 1200 mAh / g or more is more preferable, and 1500 mAh / g or more is even more preferable. This power storage device preferably has a high initial charge-discharge efficiency. For example, 60% or more is preferable, 65% or more is more preferable, and 70% or more is even more preferable. This power storage device preferably has a high capacity retention rate after cycling. For example, the capacity retention rate after 50 cycles is preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more. Also, for example, the capacity retention rate after 100 cycles is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more.
[0045] (All-solid-state lithium-ion secondary battery) This power storage device is preferably an all-solid-state lithium-ion secondary battery. In an all-solid-state battery, changes in performance due to the electrolyte can be more effectively suppressed, and furthermore, the safety can be enhanced, which is preferable. This all-solid-state lithium-ion secondary battery may include a positive electrode containing a positive electrode active material, a negative electrode using the above-described porous silicon material as a negative electrode active material, and a solid electrolyte interposed between the positive electrode and the negative electrode for conducting lithium ions. The positive electrode can use any of those shown in the above-described power storage device. Also, the negative electrode can use the above-described porous silicon material as the negative electrode active material.
[0046] The solid electrolyte may be, for example, a garnet-type oxide containing at least Li, La, and Zr. This solid electrolyte has a basic composition of Li 7.0+x-y (La 3-x , A x )(Zr 2-y , T y )O 12 and may be of this type. However, A is one or more of Sr and Ca, T is one or more of Nb and Ta, and it satisfies 0 < x ≦ 1.0 and 0 < y < 0.75. Alternatively, the solid electrolyte has a basic composition (Li 7-3z+x-y M z )(La 3-x A x )(Zr 2-y Ty )O 12 Or, (Li 7-3z+x-y M z )(La 3-x A x )(Y 2-y T y )O 12 In the formula, the element M may be one or more of Al and Ga, the element A may be one or more of Ca and Sr, and T may be one or more of Nb and Ta, and 0≦z≦0.2, 0≦x≦0.2, and 0≦y≦2 may be satisfied. In this basic composition formula, it is more preferable that 0.05≦z≦0.1 is satisfied. In this basic composition formula, it is more preferable that 0.05≦x≦0.1 is satisfied. In addition, in this basic composition formula, it is more preferable that 0.1≦y≦0.8 is satisfied. In such a range, the ion conductivity can be more suitable.
[0047] Alternatively, the solid electrolyte may be, for example, Li3N, a common Li-ion battery called LISICON. 14 Zn(GeO4)4, Li sulfide 3.25 Ge 0.25 P 0.75 S4, perovskite-type La 0.5 Li 0.5 CrO3, (La 2 / 3 Li 3x □ 1 / 3-2x )CrO3(□: atomic vacancy), garnet-type Li7La3Zr2O 12 , LiCr2(PO4)3, also known as NASICON type, Li 1.3 M 0.3 Cr 1.7 (PO3)4 (M = Sc, Al), etc. Also, Li7P3S obtained from glass with the composition 80Li2S 20P2S5 (mol%), which is a glass ceramic, 11 Furthermore, Li, a sulfide-based material with high electrical conductivity, 10Examples of glass-based inorganic solid electrolytes include Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li4SiO4, Li2S-P2S5, Li3PO4-Li4SiO4, Li3BO4-Li4SiO4, and those that use SiO2, GeO2, B2O3, or P2O5 as the glass-based substance and Li2O as the network modifier. In addition, examples of thiolithium solid electrolytes include Li2S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S2, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-SbS5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2S-P2S5, Li2S-Al2S3, LiS-SiS2-Al2S3, Li2S-SiS2-P2S5, etc. These solid electrolytes may be formed into a plate shape and placed between the positive electrode and the negative electrode.
[0048] The all-solid-state lithium-ion secondary battery may further include a restraining member that restrains a stack of a positive electrode, a solid electrolyte, and a negative electrode in a stacking direction. The restraining member may include, for example, a pair of plate-shaped parts that sandwich the stack from both ends in the stacking direction of the stack, a rod-shaped part that connects the pair of plate-shaped parts, and an adjustment part that is connected to the rod-shaped part and adjusts the gap between the pair of plate-shaped parts by a screw structure or the like.
[0049] As described above in detail, the present disclosure can provide a novel porous silicon material, a power storage device, and a method for manufacturing a porous silicon material with reduced resistivity. The reason why such an effect is obtained is presumed to be as follows. For example, when a raw material of an Al-Si-Cr ternary alloy having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium diagram is melted and rapidly solidified to prepare a precursor of a silicon alloy, and the Al component is removed, a porous silicon material having a skeleton in which Si and Cr silicide coexist is obtained. In such a porous silicon material, since the conductive phase Cr silicide exists along the skeleton that serves as a conductive path, it is presumed that electrical conduction is efficiently performed and the resistivity can be reduced. At that time, oxygen is taken into the porous silicon material with the removal of the Al component, and an insulating phase such as SiO2 is formed, which may inhibit electrical conduction, but it is presumed that the inhibition of electrical conduction is suppressed and the resistivity can be further reduced by reducing the amount of oxygen taken in. In addition, since the Cr silicide contains an AlSiCr alloy, it is presumed that the resistivity can be effectively reduced with a smaller conductive phase. Although AlSiCr alloys are easily dissolved by acid treatment, and as a result, amorphous silica is generated during the removal process, which can reduce conductivity, the present disclosure is able to reduce the amount of amorphous silica generated, so that it is believed that the resistivity can be reduced even with a smaller conductive phase, and the battery capacity of the negative electrode is not impaired. In addition, it is believed that the reduced resistivity can be expected to improve the rate characteristics, making it possible to fabricate higher performance batteries.
[0050] In addition, the manufacturing method of the porous silicon material of the present disclosure uses an Al-Si-Cr ternary alloy as the mother alloy. The Al-Si-Cr ternary alloy is phase-separated into an Al phase, a Si phase, and a Cr silicide phase at room temperature, but the crystallization order is that the Si phase and the Cr silicide phase crystallize first, and then the Al phase crystallizes. Therefore, in the process of cooling the alloy melt, a state in which cluster particles of Si and Cr silicide are dispersed in the Al melt is generated, and when the Al melt solidifies, a structure in which the cluster particles are connected to each other is formed. From this, it is considered that a composite porous body in which Cr silicide is segregated in the Si skeleton portion is formed by selectively removing the Al component. Since Cr silicide is a semiconductor with a relatively high conductivity, the coexistence of Cr silicide can be expected to reduce the resistivity. In addition, in the past, the porousness of silicon particles has been considered from the viewpoint of mitigating the expansion and contraction of silicon, but generally, porous silicon tends to have a higher resistance than non-porous silicon. In order to solve this problem, it has been considered to reduce the resistance by combining with a conductive phase, but in general methods, the resistance decreases as the amount of conductive phase increases, but the battery capacity is often sacrificed. In contrast, in the present disclosure using an Al-Si-Cr ternary alloy, the conductive phase Cr silicide exists along the silicon skeleton, which is the conductive path, so it is presumed that the resistivity can be reduced with a smaller amount of conductive phase without impairing the battery capacity.
[0051] Furthermore, the present disclosure is expected to further suppress the deterioration of charge / discharge characteristics in materials containing Si. The reason for such an effect is presumed to be as follows. For example, the theoretical capacity of a silicon negative electrode for a lithium-ion secondary battery is 4199 mAh / g, which is about 10 times the theoretical capacity of general graphite, 372 mAh / g, and further increases in capacity and energy density are expected. On the other hand, silicon that has absorbed lithium ions has a low charge / discharge characteristic of Li 4.4The porous silicon material is Si, and its volume expands to about four times that of silicon before lithium absorption. A high-capacity Si negative electrode may lose its current collecting ability due to expansion and contraction during charging and discharging, resulting in a decrease in capacity. The porous silicon material of the present disclosure has nanopores, which can relieve the stress associated with the expansion and contraction of silicon during charging and discharging. At the same time, by introducing a Cr silicide phase that is inactive against carrier ions into the silicon skeleton, the skeleton strength can be improved and the silicon pore structure can be prevented from collapsing due to the stress associated with expansion and contraction during charging and discharging. This can further improve the cycle characteristics. Furthermore, by improving the strength of the particles, it is possible to suppress the collapse of the pores due to roll pressing or the like during the preparation of the composite electrode. Therefore, in the present disclosure, a high-performance electricity storage device can be easily obtained, such as by mitigating the expansion and contraction of the volume and improving the cycle characteristics.
[0052] It goes without saying that the present disclosure is in no way limited to the above-described embodiment, and can be embodied in various forms as long as it falls within the technical scope of the present disclosure.
[0053] For example, the present disclosure may be any one of the following [1] to
[10] . [1] A porous silicon material having a skeleton in which Si and Cr silicide including at least an AlSiCr compound coexist, in which when the sum of the Si content, the Al content, and the Cr content is taken as 100 at%, the oxygen content is 25 at% or less, the O / Cr ratio, which is the ratio of the oxygen content to the Cr content, is 10 or less, and the porosity, as determined by mercury intrusion porosimetry, is 55 vol% or more. [2] The porous silicon material according to [1], which satisfies one or more of the following (1) to (2): (1) The amount of oxygen is 10 at % or less. (2) The O / Cr ratio is 5 or less. [3] The porous silicon material according to [1] or [2], wherein the Cr amount is more than 0 at% and 5 at% or less, and an Al / Cr ratio, which is the ratio of the Al amount to the Cr amount, is 2 or more and 7 or less. [4] The porous silicon material according to any one of [1] to [3], having an average pore diameter of 60 nm or less as determined by mercury intrusion porosimetry. [5] The Cr silicide is CrSi2, Cr(Si,Al)2, Al 13 Cr4Si4 or more, and the content of the Cr silicide is 6 mol % or less. [6] The porous silicon material according to any one of [1] to [5], having a resistivity of 1000 Ωcm or less. [7] A positive electrode including a positive electrode active material; A negative electrode containing the porous silicon material according to any one of [1] to [6] as a negative electrode active material; an ion conductive medium interposed between the positive electrode and the negative electrode and conducting lithium ions; A power storage device comprising: [8] A method for producing a porous silicon material according to any one of [1] to [6], comprising the steps of: a precursor process for obtaining a precursor of a silicon alloy by melting and rapidly solidifying an Al-Si-Cr ternary alloy raw material having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium phase diagram; a porosity forming step of removing an Al component contained in the silicon alloy to obtain the porous silicon material; 1. A method for producing a porous silicon material, comprising: [9] In the precursor process, the basic composition formula Al 100-x-y S x Cr y The method for producing a porous silicon material according to [8], wherein the raw material satisfies 18≦x≦40, y≧0.1, and x / y≧8.
[10] The method for producing a porous silicon material according to [8] or [9], wherein in the porosity-providing step, the Al component is removed with hydrochloric acid having a concentration of less than 0.5 mol / L. EXAMPLES
[0054] Specific examples of the porous silicon and electricity storage device according to the present disclosure that have been fabricated will be described below as experimental examples. Experimental Examples 1 to 8, 11 to 12, 14 to 27, and 29 correspond to examples of the present disclosure, and Experimental Examples 9 to 10, 13, and 28 correspond to comparative examples.
[0055] [Preparation of porous silicon materials] The raw materials of Al, Si and Cr are classified into the basic composition formula Al 100-x-y S x Cr y The alloys were weighed out to have the composition (x = 15-40, y = 0-10) and melted in an arc melting furnace. Before melting, the temperature in the arc melting furnace was 8 × 10 -3 After reducing the pressure to less than 1 Pa, the material powders were melted, and high-frequency melting was performed to prepare a uniform sample. The obtained master alloy was melted by heating to 1000-1300°C in an Ar atmosphere, and then melted by gas atomization. 2 The alloy was quenched and solidified at a rate of 1000 K / sec or more to obtain an AlSiCr alloy powder (precursor process). The obtained alloy was immersed in a 0.1-3 mol / L hydrochloric acid solution and acid-treated (removal process) for 1-48 hours at any temperature between room temperature (25°C) and 80°C to selectively remove the Al component. The residue was transferred to a filter, and the acid after treatment was removed by pressure filtration, followed by washing with distilled water four or more times, and the washing water was removed by the same pressure filtration method to obtain porous silicon (porosity process).
[0056] (Experimental Examples 1 to 4) A porous silicon material prepared under conditions of a mother alloy composition of x=30 and y=1 in the above basic composition formula, a hydrochloric acid concentration of 0.1 mol / L, an acid treatment temperature of 25° C., and an acid treatment time of 22 hours was designated as Experimental Example 1. A porous silicon material prepared in the same manner as Experimental Example 1 was designated as Experimental Example 2, except that the mother alloy composition was a composition of x=25 and y=1.5 in the above basic composition formula, and the acid treatment time was 20 hours. A porous silicon material prepared in the same manner as Experimental Example 1 was designated as Experimental Example 3, except that the mother alloy composition was a composition of x=30 and y=3 in the above basic composition formula, and the acid treatment time was 20 hours. A porous silicon material prepared in the same manner as Experimental Example 1 was designated as Experimental Example 4, except that the mother alloy composition was a composition of x=25 and y=3 in the above basic composition formula, and the acid treatment time was 20 hours.
[0057] (Experimental Examples 5 to 9) A porous silicon material was prepared as Experimental Example 5 under the conditions of a mother alloy composition of x=30 and y=1 in the above basic composition formula, a hydrochloric acid concentration of 3 mol / L, an acid treatment temperature of 80°C, and an acid treatment time of 5 hours. A porous silicon material was prepared in the same manner as Experimental Example 5 except that the mother alloy composition was a composition of x=25 and y=1.5 in the above basic composition formula. A porous silicon material was prepared in the same manner as Experimental Example 5 except that the mother alloy composition was a composition of x=30 and y=3 in the above basic composition formula. A porous silicon material was prepared in the same manner as Experimental Example 7 except that the mother alloy composition was a composition of x=25 and y=3 in the above basic composition formula. A porous silicon material was prepared in the same manner as Experimental Example 5 except that the mother alloy composition was a composition of x=25 and y=3 in the above basic composition formula. A porous silicon material was prepared in the same manner as Experimental Example 9 except that the mother alloy composition was a composition of x=20 and y=0 in the above basic composition formula.
[0058] (Experimental Example 10) The Si powder (Kojundo Chemical Co., Ltd., SIE23PB) having an average particle size of 5 μm was used as it was in Experimental Example 10.
[0059] (Experimental Examples 11-29) A porous silicon material was prepared as Experimental Example 11, in which the mother alloy composition was a composition of x=30 and y=1 in the above basic composition formula, the hydrochloric acid concentration was 0.1 mol / L, the acid treatment temperature was 25°C, and the acid treatment time was 18 hours. A porous silicon material was prepared in the same manner as Experimental Example 11, except that the acid treatment time was 24 hours, as Experimental Example 12. A porous silicon material was prepared in the same manner as Experimental Example 11, except that the hydrochloric acid concentration was 1 mol / L and the acid treatment time was 2 hours, as Experimental Example 13. A porous silicon material was prepared in the same manner as Experimental Example 13, except that the acid treatment time was 5 hours, 8 hours, 10 hours, 12 hours, 18 hours, and 24 hours, as Experimental Example 14, Experimental Example 15, Experimental Example 16, Experimental Example 17, Experimental Example 18, and Experimental Example 19. A porous silicon material was prepared in the same manner as Experimental Example 11, except that the hydrochloric acid concentration was 3 mol / L and the acid treatment time was 2 hours. Experimental Examples 21, 22, and 23 were prepared in the same manner as in Experimental Example 20, except that the acid treatment time was set to 5 hours, 12 hours, and 24 hours. Experimental Example 24 was prepared in the same manner as in Experimental Example 11, except that the hydrochloric acid concentration was set to 3 mol / L, the acid treatment temperature was set to 80° C., and the acid treatment time was set to 1 hour. Experimental Examples 25, 26, and 27 were prepared in the same manner as in Experimental Example 24, except that the acid treatment time was set to 2.5 hours, 4 hours, and 7.3 hours. Experimental Examples 28 and 29 were prepared in the same manner as in Experimental Example 11, except that the acid treatment time was set to 5 hours and 20 hours.
[0060] (XRD measurement) The atomized powder before the acid treatment and the porous silicon powder after the acid treatment were subjected to X-ray diffraction measurement using an X-ray diffractometer (Rigaku Corporation, Ultima IV) with a Cu tube in the range of 2θ = 20° to 60° at a rate of 20° / min. 13 The proportion of each phase, Cr4Si4 phase and Cr(Al,Si)2 phase, was calculated by mass ratio from the XRD peak intensity ratio of each phase using an alumina standard material. The proportion of each phase was measured after heat treatment at 600°C to crystallize the amorphous phase.
[0061] (SEM / EDX measurement) The atomized powder before the acid treatment and the porous silicon powder after the acid treatment were pressed into a disk shape using a carbide mold, and the pressed surface was observed using a scanning electron microscope (SEM, Hitachi S-4300) and energy dispersive X-ray analysis (EDX, Hitachi S-4300) to perform composition analysis.
[0062] (SEM observation) The porous silicon powder after the acid treatment was embedded in resin, a cross section was extracted by polishing, and SEM observation was performed using the above-mentioned scanning electron microscope.
[0063] (Pore distribution measurement) The pore distribution of the porous silicon powder after the acid treatment was measured using a mercury porosimeter (Quantachrome POREMASTER60GT). The average pore size was also calculated from the volume fraction of each size of pores in the pore size distribution data. Generally, porous material powders contain pores within particles and pores between particles, but the pore size distribution data does not allow for a distinction between the two. Here, by comparing with the pore size distribution measurement results of the atomized powder before the acid treatment, the pore ratio of 300 nm or less was determined to be intraparticle pores, and the two were distinguished, and the intraparticle porosity and average pore size were calculated. Although not shown in the figure, the pore size distribution had peaks at 700 to 800 nm and around 100 nm. Based on the pore size distribution data of the atomized powder before acid treatment and comparison with SEM, the peak near 100 nm was determined to be the peak of intraparticle pores, and based on the border between the two peaks at 300 nm, pores of 300 nm or less were determined to be intraparticle pores as described above. Note that by comparing the pore size distribution data of the sample before and after acid treatment, it is possible to distinguish between intraparticle pores and interparticle pores and to determine the intraparticle porosity and average pore size.
[0064] (STEM / EDX measurement) The porous silicon powder after the acid treatment was subjected to elemental image mapping and structure observation using a scanning transmission electron microscope (STEM, JEM2100F manufactured by JEOL Ltd.).
[0065] (Resistivity measurement) The porous silicon powder after the acid treatment was pressurized at 200 MPa to produce a 3 x 1 x 1 mm green compact, to which a copper wire was baked using silver paste, and the resistivity was evaluated using the four-terminal method. When the porosity before and after pressurization was evaluated using a mercury porosimeter, it was found that there was almost no change in the porosity at a pressurization of 200 MPa, suggesting that the pore structure of the porous silicon powder was maintained. The resistivity was measured at 25°C.
[0066] (Battery characteristic evaluation) The battery characteristics were evaluated using the porous silicon powder after the acid treatment. 60 parts by mass of the porous silicon powder, 20 parts by mass of the carbon black conductive assistant, and 20 parts by mass of the polyimide binder were mixed, and the viscosity was adjusted with N-methylpyrrolidone to form a slurry, which was then applied to a copper current collector foil and dried to prepare a composite electrode. The composite electrode was punched out with a diameter of 16 mm to prepare a negative electrode, and a porous polyethylene separator was sandwiched between the negative electrode and metallic lithium was placed as a counter electrode. An electrolyte was then poured into the negative electrode to prepare a lithium secondary battery using a small Tomcell-type battery cell. The electrolyte used was a mixed solvent containing 1.5 parts by volume of fluoroethylene carbonate (FEC), 3 parts by volume of ethylene carbonate (EC), 4 parts by volume of dimethyl carbonate (DMC), and 3 parts by volume of ethyl methyl carbonate (EMC), to which LiPF6 was added at a concentration of 1 mol / L. The obtained lithium secondary battery was repeatedly charged and discharged for 100 cycles at a current density of 0.2C in a battery voltage range of 0.005V to 1.5V. The reaction in which the porous silicon powder absorbs lithium is called charging, and the reaction in which the porous silicon powder releases lithium is called discharging. The initial discharge capacity, initial charge / discharge efficiency, initial area capacity, capacity retention rate after 50 cycles, and capacity retention rate after 100 cycles were obtained. The capacity here is the discharge capacity (specific capacity) per active material mass (mass of material excluding binder and conductive assistant on copper current collector foil) contained in the negative electrode. The initial discharge capacity was the capacity per mass of the porous silicon powder. The initial charge / discharge efficiency was the ratio of the discharge capacity of the discharge following the initial charge to the initial charge capacity. The initial area capacity was the discharge capacity of the total mass per area of the negative electrode. The capacity retention rate after 50 cycles and the capacity retention rate after 100 cycles were defined as the ratio of the discharge capacity at the 50th cycle and the 100th cycle to the initial discharge capacity, respectively. Furthermore, the lithium secondary battery prepared in the same manner as above was charged and discharged at a battery voltage in the range of 0.01 V to 1.5 V, with the current per mass of the porous silicon powder being changed to 0.1 A / g, 0.2 A / g, 0.5 A / g, 1 A / g, 2 A / g, and 0.1 A / g every 10 cycles, to evaluate the rate characteristics.
[0067] (Results and Discussion) The experimental results of Experimental Examples 1 to 29 are summarized in Tables 1 to 3. The experimental results are discussed below. First, the crystal phase of the atomized powder was examined using the XRD measurement results. As an example, FIG. 11 shows the crystal phase of Al, which is the precursor of the porous silicon material of Experimental Example 2. 73.5 S 25 Cr 1.5 The XRD pattern of the atomized powder is shown (Fig. 11(a)). Figure 11 also shows the XRD pattern of a sample that was heat-treated at 200°C (Fig. 11(b)). In the atomized powder, only diffraction peaks of the Si and Al phases were observed, but when the atomized powder was heat-treated at 200°C or higher, Al phase, Si phase, and Al phase were observed. 13 The diffraction peak of the Cr4Si4 phase appeared, indicating the existence of the room temperature equilibrium phase in the phase diagram. From this, it was inferred that the silicide phase in the atomized powder exists in an amorphous state due to rapid cooling. Furthermore, elemental analysis revealed that the atomized powder contains almost no oxygen.
[0068] The effect of the acid treatment conditions (hydrochloric acid concentration, treatment time, and temperature) on the composition of the product was examined using the EDX measurement results of the porous silicon materials of Experimental Examples 5 and 13 to 27. 69 S 30 The changes in oxygen and chromium content in the Cr1 atomized powder were shown. As the treatment time increased and the powder became more porous, the amount of oxygen increased and the chromium content decreased. The dissolution of Cr was more pronounced with higher concentrations of acid, and in high-concentration hydrochloric acid of 3 mol / L, about half of the Cr in the master alloy composition was dissolved. On the other hand, when treated with low-concentration hydrochloric acid of 0.1 mol / L, it was found that the dissolution of Cr could be suppressed by about half. The acid concentration after acid treatment also increased with the acid treatment, but the amount was linked to the change in the amount of Cr dissolved, indicating that oxidation occurred with the dissolution of the chromium silicide phase. However, XRD did not confirm the oxide phase even when heated, suggesting that amorphous SiO2 was formed. As for oxygen, the content decreased with lower-concentration hydrochloric acid treatment, and it was found that low-concentration hydrochloric acid of 0.1 mol / L was particularly effective.
[0069] The dissolution of Al during acid treatment was examined using the XRD measurement results of the porous silicon materials of Experimental Examples 11, 28, and 29. 69 S 30 As an example showing the change in the contained phase with the treatment time when Cr1 atomized powder is treated with 0.1 mol / L hydrochloric acid solution, the XRD patterns of the porous silicon materials of Experimental Examples 11, 28, and 29 are shown. A strong Al diffraction peak was confirmed after 5 hours of treatment, but the intensity of the Al peak decreased as the treatment time was increased, indicating that Al dissolution progresses. After 20 hours of treatment, the Al diffraction peak completely disappeared, and the porosity treatment was completed. However, composition analysis of the sample at this stage showed that more than 5 at% Al remained, and the amount hardly changed even when the acid treatment time was increased, indicating that a certain amount of Al remained in the form of a solid solution or the like even after porosity was formed.
[0070] As mentioned above, chromium silicide exists in an amorphous state, so no peaks of chromium silicide were observed in the sample after acid treatment (Figure 13). Using samples obtained by heat-treating the porous silicon materials of Experimental Examples 1 to 4 at 600°C, the phases contained in the samples after acid treatment were examined. Figure 14 shows the phases of Al 69 S 30 Cr1, Al 73.5 S 25 Cr 1.5 , Al 67 S 30 Cr3, Al 72 S 25 The XRD patterns of the porous silicon materials of Experimental Examples 1 to 4, which are samples obtained by treating each atomized powder of Cr3 with a 0.1 mol / L hydrochloric acid aqueous solution, were obtained by heat-treating the materials at 600°C. By heating at 200°C or higher, the samples after the acid treatment showed that the Al 13 It was found that chromium silicide Cr(Al,Si)2, which is different from the Cr4Si4 phase (see FIG. 11), had crystallized.
[0071] The pore distribution was examined using the results of measurements of the porous silicon materials of Experimental Examples 5 to 8 using a mercury porosimeter and the results of SEM observation of Experimental Example 5. Table 2 shows the Al 69S 30 Cr1, Al 73.5 S 25 Cr 1.5 , Al 67 S 30 Cr3, Al 72 S 25 The porosity and average pore size of the porous silicon materials of Experimental Examples 5 to 8, which are samples obtained by acid-treating and porousifying each atomized powder of Cr3, are summarized. In Experimental Examples 5 to 8, the porosity is in the range of 65 to 75 vol%, and the average pore size tends to decrease with an increase in the Cr content. It was found that all samples had fine pores with a diameter of 100 nm or less. Figure 15 shows a cross-sectional secondary electron image taken by SEM of the porous silicon material of Experimental Example 8. In Figure 15, a spherical structure in which pores with a diameter of 100 nm or less are uniformly distributed is observed.
[0072] Next, the element distribution in the pores of the porous silicon material of Experimental Example 8 was measured by STEM / EDX. 72 S 25STEM / EDX elemental mapping of the porous silicon material of Experimental Example 8, which is a sample obtained by acid-treating and porousifying Cr3 atomized powder, is shown. FIG. 16A is a STEM image, and FIGS. 16B-D are mapping images of Si, Cr, and Al, respectively. FIG. 17 summarizes the electron beam diffraction results of the porous silicon material of Experimental Example 8. As shown in FIG. 16, it was found that each element of Al, Si, and Cr was segregated in the skeleton portion. Furthermore, the electron beam diffraction of the skeleton portion obtained a pattern as shown in FIG. 17, and the value of the interplanar spacing showed that crystalline Si and Cr(Al,Si)2 were present in the skeleton portion. From these results, it was clear that a coexisting composite nanoporous Si was formed as expected. In addition, the elemental distribution of the pore portion of the porous silicon materials of Experimental Examples 1 and 3 was measured by STEM / EDX. FIG. 18 shows the STEM / EDX elemental mapping of the porous silicon material of Experimental Example 4. FIG. 19 shows the STEM / EDX elemental mapping of the porous silicon material of Experimental Example 1. Figures 18A and 19A are cross-sectional secondary electron images taken by SEM, Figures 18B and 19B are STEM photographs, Figures 18C and 19C are superimposed element mapping images, and Figures 18D-F and 19D-F are mapping images of Si, Cr, and Al, respectively. Figures 18 and 19 reveal that coexisting composite nanoporous Si was formed in Experimental Examples 1 and 4 as well.
[0073] Next, the resistivity was examined using the porous silicon materials of Experimental Examples 1 to 9. Figure 20 shows the effect of the chromium silicide concentration on the resistivity of the porous body. The chromium silicide concentration was calculated from the element ratio of Al, Si, Cr, and O, assuming that the phases present in the sample were Si, Cr(Al,Si)2, and SiO2. It was found that the resistivity was lower in the composition containing the conductive phase than in the case without the conductive phase. In addition, the resistivity was lower in the case of treatment with 0.1 mol / L hydrochloric acid than in the case of treatment with 3 mol / L hydrochloric acid. Furthermore, the resistivity was minimum when the chromium silicide concentration was 1 to 2 mol%, and tended to increase as the chromium silicide concentration was increased. These behaviors are thought to be related to the amount of SiO2 generated by dissolving the chromium silicide during acid treatment. Figure 21 shows the change in the amount of oxygen with respect to the chromium silicide concentration. The oxygen concentration also increased as the amount of chromium silicide increased, and the amount of oxygen was high in the sample treated with 3 mol / L hydrochloric acid. Chromium silicide, as a conductive phase, reduces resistivity, but when the amount of chromium silicide is increased by increasing the amount of Cr at the time of preparation, the generation of SiO2 phase due to the dissolution of chromium silicide increases, which suggests that the resistivity is increased. From this, it was thought that the ratio of the oxygen content O, which is correlated with the amount of SiO2, to the Cr content, which is correlated with the amount of chromium silicide (O / Cr ratio), affects the resistivity. Figure 22 shows the change in resistivity with respect to the Cr content of the porous sample. From Figure 22, it was shown that when organized by the O / Cr ratio, the resistivity is lower when the O / Cr ratio is smaller, even with the same Cr content. When the O / Cr ratio is about 3 to 4, a low resistivity of less than 1000 Ω cm is achieved, and it was found that a lower chromium silicide concentration is required to achieve the same resistivity.
[0074] Finally, the porous silicon materials of Experimental Examples 1 to 5 and 9 were used to fabricate batteries, and the battery characteristics were examined. Table 2 summarizes the battery characteristics of Experimental Examples 1 to 5 and 9. Specifically, the initial discharge capacity, initial charge / discharge efficiency, initial areal capacity, capacity retention rate after 50 cycles, and capacity retention rate after 100 cycles are summarized. Compared to Si powder without pores, the porous body sample showed a higher capacity retention rate. Furthermore, it was found that the capacity decreases as the composition increases in chromium silicide, but when the chromium silicide conductive phase is 2 mol% or less, a capacity comparable to that of pure Si can be obtained. In addition, FIG. 23 shows the evaluation results of the rate characteristics of Experimental Examples 1, 3 and 9. From FIG. 23, it was found that Experimental Examples 1 and 3, which have low resistivity, have not only a high capacity and a high capacity retention rate, but also good rate characteristics, compared to Experimental Example 9, which has high resistivity.
[0075] [Table 1]
[0076] [Table 2]
[0077] [Table 3]
[0078] It goes without saying that the present disclosure is in no way limited to the above-described experimental examples, and can be embodied in various forms as long as they fall within the technical scope of the present disclosure. [Industrial Applicability]
[0079] The present disclosure is applicable to the technical field of secondary batteries. [Explanation of symbols]
[0080] 10 Energy storage device, 12 Positive electrode, 13 Positive electrode active material, 14 Current collector, 15 Negative electrode, 16 Negative electrode active material, 17 Current collector, 18 Ion conductive medium, 20,20F Porous silicon material, 22 Si, 24 Cr silicide, 25 Framework, 26 Vacancy, 28 SiO2.
Claims
1. A porous silicon material having a skeleton in which Si and Cr silicide including at least an AlSiCr compound coexist, wherein when the sum of the amount of Si, the amount of Al and the amount of Cr is taken as 100 at%, the amount of oxygen is 25 at% or less, an O / Cr ratio which is a ratio of the amount of oxygen to the amount of Cr is 10 or less, and a porosity determined by mercury intrusion porosimetry is 55 volume% or more.
2. The porous silicon material according to claim 1, which satisfies one or more of the following (1) to (2): (1) The amount of oxygen is 10 at % or less. (2) The O / Cr ratio is 5 or less.
3. 3. The porous silicon material according to claim 1, wherein the Cr content is greater than 0 at % and 5 at % or less, and an Al / Cr ratio, which is a ratio of the Al content to the Cr content, is 2 or more and 7 or less.
4. 3. The porous silicon material according to claim 1, having an average pore diameter of 60 nm or less as determined by mercury intrusion porosimetry.
5. The Cr silicide is CrSi 2 , Cr(Si,Al) 2 , Al 13 Cr 4 S 4 3. The porous silicon material according to claim 1, wherein the content of Cr silicide is 6 mol % or less.
6. 3. The porous silicon material according to claim 1, having a resistivity of 1000 Ωcm or less.
7. a positive electrode including a positive electrode active material; A negative electrode comprising the porous silicon material according to claim 1 or 2 as a negative electrode active material; an ion conductive medium interposed between the positive electrode and the negative electrode and conducting lithium ions; A power storage device comprising:
8. A method for producing the porous silicon material according to claim 1 or 2, comprising the steps of: a precursor process for obtaining a precursor of a silicon alloy by melting and rapidly solidifying a raw material of an Al-Si-Cr ternary alloy having a composition in which Al, Si, and Cr silicide containing at least an AlSiCr compound appear at room temperature in an equilibrium phase diagram; a porosity forming step of removing an Al component contained in the silicon alloy to obtain the porous silicon material; 1. A method for producing a porous silicon material, comprising:
9. In the precursor step, the basic composition formula Al 100-x-y S x Cr y 9. The method for producing a porous silicon material according to claim 8, wherein the raw material satisfies 18≦x≦40, y≧0.1, and x / y≧8.
10. The method for producing a porous silicon material according to claim 8 , wherein in the porosity forming step, the Al component is removed with hydrochloric acid having a concentration of less than 0.5 mol / L.
Citation Information
Patent Citations
Porous silicon particle and method for manufacturing the same
JP2012082125A
Si ALLOY POWDER FOR LITHIUM ION SECONDARY BATTERY NEGATIVE ELECTRODE AND MANUFACTURING METHOD FOR THE SAME
JP2012150910A
Negative electrode material of power storage device
JP2015176676A
Method for producing porous silicon material, porous silicon material, and electricity storage device
JP2022150481A
Method for producing porous silicon material, porous silicon material, and electricity storage device
JP2022187360A