Estimation method for coke strength
By estimating coke strength through the particle size distribution of broken powder, particularly focusing on the ratio and average size of fine particles, the method addresses the inefficiencies of conventional methods, allowing for more frequent and accurate coke strength measurement, enhancing blast furnace stability and reducing costs.
Patent Information
- Application Number
- JP2023050124
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Conventional methods for estimating coke strength in blast furnaces are time-consuming, require large sample sizes, and are inaccurate due to fluctuations in operating conditions, making it difficult to frequently measure and stabilize coke strength for stable blast furnace operation.
Estimating coke strength based on the particle size distribution of broken powder generated by coke destruction, specifically focusing on the proportion and average particle size of fine particles, using a method that involves measuring the ratio of fine particles to coarse particles and applying a laser diffraction technique for accurate estimation.
Enables quick and frequent measurement of coke strength, reducing the need for large sample sizes and minimizing the impact of operating conditions, thereby stabilizing coke production and blast furnace operation, leading to cost savings and improved efficiency.
Smart Images

Figure 2024139259000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for estimating coke strength, which is the most important quality of coke. [Background technology]
[0002] Generally, coke for steelmaking is produced by carbonizing coal in a coke oven to a temperature of about 900℃ or higher, and is mainly used in blast furnaces. The coke charged into the blast furnace is required to function as a reducing agent to reduce iron ore, the main raw material in the pig iron making process. The blast furnace is a countercurrent reaction device of solids, liquids, and gases, and coke also plays the role of a spacer to ensure gas permeability and liquid permeability. In particular, the role of the spacer is important for the smooth operation of the blast furnace. If the function as a spacer is impaired, the gas permeability in the blast furnace will be poor, the flow of reducing gas in the blast furnace will be hindered, and the dripping of molten pig iron and slag in the blast furnace will be hindered, causing operational problems. In order to maintain its function as a spacer, the coke is required to have high strength. If the strength of the coke is low, it will be powdered in the blast furnace, and the resulting powder will remain between the lumps of coke, hindering the gas permeability and liquid permeability.
[0003] As an evaluation method for the strength of coke, for example, the drum strength index, particularly the drum index: DI (150 / 15), specified in JIS K 2151 is known. This DI (150 / 15) value is also widely adopted as a control index for coke strength in coke plants. Therefore, the coke produced every day is sampled multiple times and the DI (150 / 15) value is obtained by drum strength testing.
[0004] In this drum strength test, first, coke is sampled and divided to prepare 10 kg or more of coke with a particle size of 50 mm or more or 25 mm or more. Then, the sample (coke) is subjected to 150 revolutions of impact in a cylindrical drum with an inner diameter and depth of 1500 mm and a height of 250 mm containing six blades. After that, the collected coke is sieved and the weight ratio (x 100) of coke with a particle size of 15 mm or more is calculated as the DI (150 / 15) index.
[0005] This drum strength test is very time-consuming, and there is a limit to how often it can be measured per day. However, if the strength of the coke supplied to the blast furnace can be measured quickly and fed forward quickly to blast furnace operation, it can contribute to stable operation of the blast furnace. In addition, if the temporal fluctuation of coke strength can be grasped at shorter intervals and feedback can be provided to coke operation to stabilize the coke strength, it can also contribute to stable operation of the blast furnace. As a result, there is a demand for rapid and frequent measurement of such drum strength indexes in order to save energy and reduce CO2 emissions.
[0006] Therefore, attempts have been made to measure or estimate the coke strength in a simpler manner. For example, Patent Document 1 proposes a method of measuring the fineness and particle size of the coke at at least two or more arbitrary positions during the transport process, and estimating the drum strength of the coke from the mechanical impact force received during the transport process and the change in the particle size distribution of the finely granulated coke. Patent Document 2 discloses a method for estimating drum strength from the amount of coke powder recovered from circulating gas using a dust collector, which is generated as a result of the destruction of quenched coke in a coke dry quenching system (CDQ). This method utilizes the correlation between the proportion of collected dust and coke strength for quenched coke, creates a calibration curve in advance between the fine yield (proportion of collected dust per processing amount) generated in CDQ and drum strength, and estimates drum strength from the measured value of fine yield. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 4-23736 [Patent Document 2] Japanese Patent Application Publication No. 2-216455 Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, the drum strength index of coke has been evaluated in the past by a labor-saving method of the complicated drum strength test, but these conventional techniques have the following problems.
[0009] First, the method of estimating drum strength based on particle size measurement proposed in Patent Document 1 can estimate relatively quickly and easily, but a large amount of sampling is required to measure coke with a large particle size, and the device becomes large-scale. In addition, there is a problem that the measurement work and the processing of the remaining sample are time-consuming. Statistically, in the case of coke with a maximum particle size of 63 mm, it is required to measure a minimum of 250 kg of sample to perform a representative particle size measurement. Patent Document 1 also mentions the possibility of determining the particle size distribution of coke from a coke image. However, there is a problem in that, although it is possible to analyze lumps with a large particle size, it is difficult to analyze powdery coke, and sufficient accuracy cannot be obtained. As a result, Patent Document 1 requires collecting a large amount of coke samples, sieving them, and measuring the particle size distribution, and only omits the drum rotation work in the drum strength measurement.
[0010] In addition, the method described in Patent Document 2, which estimates drum strength by measuring the fine yield from the fines collected by CDQ, has the advantage that it can be estimated relatively quickly and easily, and does not require the addition of special auxiliary equipment. However, it is known that the amount of fine generated and the amount of collected fine are affected not only by the drum strength of the coke but also by the operating conditions of the CDQ, such as the amount of coke processed and the flow rate of the reflux inert gas. Therefore, when the operating conditions change, the amount of fine generated and the amount of collected fine fluctuate depending on the CDQ operating conditions, and there is a problem that the accuracy of the estimation of the coke strength decreases. In addition, the amount of collected fine cannot be accurately obtained unless the fine is collected for a certain period of time and the weight of the collected fine is measured. Therefore, Patent Document 2 has the problem that it is difficult to increase the frequency of estimating coke strength, and the fine yield cannot be calculated accurately unless the amount of coke processed during the period in which the fine is collected is accurately grasped.
[0011] The present invention has been made in consideration of the above-mentioned problems associated with the conventional techniques, and an object of the present invention is to provide a technique for estimating the strength of a target coke sample in a simpler and faster manner than conventional techniques. [Means for solving the problem]
[0012] The method for estimating coke strength according to the present invention, which advantageously solves the above-mentioned problems, is characterized in that it measures the proportion of fine particles smaller than the particle size of coarse particles having a particle size of 15 mm or less among the broken particles generated by the destruction of coke, and estimates the coke strength based on a previously obtained relationship between the coke strength and the proportion of fine particles.
[0013] The method for measuring coke strength according to the present invention is characterized in that the average particle size of coke powder generated by the destruction of coke, which is equal to or smaller than any particle size of 10 mm or less, is measured, and the coke strength is estimated based on a relationship between the previously obtained coke strength and the average particle size of the coke powder.
[0014] The method for measuring coke strength according to the present invention is as follows: (1) The particle size of the coarse powder is equal to or smaller than 10 mm, and the particle size of the fine powder is equal to or smaller than 0.7 times the maximum particle size of the coarse powder and equal to or smaller than 1 mm; (2) The particle size of the coke powder is 6 mm or less; (3) The broken powder is powder recovered from the circulating gas of a dry quenching system for coke; (4) determining the particle size distribution of the broken powder by a laser diffraction method, and determining the proportion of the fine powder, which is smaller than the coarse powder, in the coarse powder from the particle size distribution obtained; (5) determining the particle size distribution of the broken powder by a laser diffraction method, and determining the average particle size of the coke powder having a particle size of 10 mm or less from the particle size distribution obtained; This is thought to be a more preferable solution. Effect of the Invention
[0015] According to the present invention having the above configuration, the coke strength can be estimated from the particle size analysis results of the broken powder generated by the breakage of the coke, so that it is not necessary to analyze a large amount of coke, and the coke strength can be estimated more simply and quickly than in the past. Moreover, it becomes possible to measure the coke strength more frequently than in the past. Furthermore, according to the present invention, it is possible to increase the frequency of control by the operating conditions based on the coke strength, which can contribute to the stabilization of the coke strength, leading to the stabilization of the coke production process and the operation of the blast furnace, and it is expected to have the effect of enabling cost reduction. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a graph showing the relationship between the ratio of fine particles with a particle size of 0.5 mm or less to the coarse particles with a particle size of 1 mm or less and coke strength. [Diagram 2] FIG. 1 is a graph showing the relationship between the ratio of fine particles having a particle size of 0.5 mm or less or 1 mm or less among coarse particles having a particle size of 3 mm or less and coke strength. [Diagram 3]FIG. 1 is a graph showing the relationship between the proportion of fine powder having a particle size of 0.5 mm or less, 1 mm or less, or 3 mm or less among coarse powder having a particle size of 6 mm or less, and coke strength. [Figure 4] FIG. 1 is a graph showing the relationship between the proportion of fine powder with particle sizes of 0.5 mm or less, 1 mm or less, 3 mm or less, or 6 mm or less among coarse powder with a particle size of 15 mm or less, and coke strength. [Diagram 5] This is a graph showing the relationship between the proportion of fine powder with particle sizes of 0.5 mm or less, 1 mm or less, 3 mm or less, 6 mm or less, or 15 mm or less among coarse powder with a particle size of 25 mm or less, and coke strength. [Figure 6] FIG. 13 is a graph showing the relationship between the first particle size and the coefficient of determination when the second particle size is 0.5 mm. [Figure 7] FIG. 1 is a graph showing the relationship between the average particle size of coke breeze having a particle size of 1 mm or less, 3 mm or less, 6 mm or less, 15 mm or less, or 25 mm or less, and coke strength. [Figure 8] This is a graph showing the relationship between the ratio of fine powder with a particle size of 0.5 mm or less to the coarse powder with a particle size of 6 mm or less among the broken powder recovered from an actual coke oven, and the drum strength index DI (150 / 15). [Figure 9] This is a diagram showing the relationship between the drum strength index: estimated DI (150 / 15) estimated by the method of the present invention based on the relationship between the drum strength index: actual DI (150 / 15) shown in Figure 8 and the proportion of fine powder with a particle size of 0.5 mm or less among coarse powder with a particle size of 6 mm or less among the broken powder, and the actual DI (150 / 15). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiment of the present invention will be specifically described. The method for estimating coke strength according to the present invention is characterized in that it focuses on the particle size distribution of the broken powder generated by the destruction of coke. Conventional methods for measuring coke strength focus on the amount of remaining coke lump or the amount of broken powder generated after applying an impact force to the coke using a drum test machine or the like, but do not pay any attention to the particle size distribution of the broken powder generated. Therefore, the inventors applied an impact force or other force to the coke to destroy it, and studied in detail the particle size distribution of the broken powder generated at that time. As a result, they applied the same impact to cokes having different strengths, and found that there is an extremely strong correlation between the information on the particle size of the broken powder generated by the destruction of the coke and the drum strength index of the coke, which led to the development of the present invention.
[0018] [Relationship between coke strength and particle size distribution of crushed powder] First, the inventors applied the same impact to cokes having different strengths and investigated in detail the particle size of the broken powder generated by the destruction of the cokes. As a result, they found that when the broken powder shows a specific particle size ratio or a specific average particle size, it shows a strong correlation with the coke strength, and developed the present invention. The details are described below.
[0019] The results of the experiments carried out to collect basic data are described below. The coke used in the tests was prepared as follows: Single coal and blended coal raw materials with an average maximum vitrinite reflectance (Ro), an index of coal rank, of 0.65-1.59% were adjusted so that the proportion of particles with a particle size of 3 mm or less was 65-100% by mass, and the raw materials were carbonized in a small carbonization furnace with a furnace wall temperature of 1,050°C for 6 hours, and then cooled in a nitrogen gas atmosphere to produce coke (39 levels in total).
[0020] The coke thus obtained was charged into a drum strength tester, and the drum was rotated 150 times to give each coke the same impact. The broken powder generated at this time was collected and the particle size distribution was measured. That is, the relationship between the drum strength index DI (150 / 15), which is calculated from the ratio of the coke lump having a particle size of 15 mm or more to the amount charged after 150 rotations, and the particle size distribution of the collected broken powder was investigated. As a result, it was found that the higher the coke strength, the higher the proportion of fine powder in the broken powder. However, when the coke strength is high, the total amount of broken powder generated from the coke is small, so that the amount of fine powder alone cannot be used as an index of correlation with coke strength.
[0021] In order to consider the particle size distribution of the broken powder generated by the destruction of the coke, the ratio of broken powder defined by two particle sizes was used as an index. Specifically, the ratio of fine powder having a particle size smaller than a predetermined particle size (hereinafter referred to as "second particle size") in the broken powder, which is less than the coarse powder having a particle size less than the coarse powder, was measured, and the correlation between the ratio of the fine powder and the coke strength was investigated. Here, the fact that the fine powder having a particle size less than the second particle size is smaller than the coarse powder having a particle size less than the first particle size means that the particle having the maximum particle size in the fine powder is smaller (has a smaller particle size) than the particle having the maximum particle size in the coarse powder. As a result, the inventors discovered that by using the ratio of fine powder to coarse powder as one of the indicators, coke strength can be accurately estimated without being affected by the total amount of broken powder.
[0022] In the present invention, the particle size is defined as the size of the smallest sieve through which the particle can pass. The particle size may be measured using a measuring instrument such as a laser diffraction analyzer. In addition, since there is no significant difference between the major axis and minor axis of the particles in the crushed coke powder, the definition of the particle size does not significantly change the measurement results of the particle size distribution.
[0023] For example, assuming that the first particle size is 1 mm and the second particle size is 0.5 mm, the amount of coarse powder (including relatively coarse powder) equal to or smaller than the first particle size and the amount of fine powder equal to or smaller than the second particle size are calculated, and then the ratio of the amount of fine powder equal to or smaller than the second particle size to the amount of coarse powder equal to or smaller than the first particle size is calculated. The relationship between the ratio of fine powder to coarse powder thus calculated ((amount of fine powder equal to or smaller than 0.5 mm in particle size) / (amount of coarse powder equal to or smaller than 1 mm in particle size)×100 (mass%) and the coke strength DI (150 / 15) is shown in FIG. 1.
[0024] In FIG. 1, a linear regression equation is also shown that shows the relationship between the amount of fine particles, which are equal to or smaller than the second particle size, in the coarse particles, which are equal to or smaller than the first particle size, and the coke strength DI (150 / 15). As a result, the coefficient of determination R 2 The value was 0.789, which indicates that the coke strength can be estimated with a fairly high degree of accuracy from the fine powder fraction.
[0025] However, it was found that the accuracy of estimating coke strength varies depending on how the first and second particle sizes are selected. Therefore, the first and second particle sizes were changed to obtain the ratio of fine particles having the second particle size or smaller to the coarse particles having the first particle size or smaller, and the relationship between this ratio and coke strength was investigated.
[0026] Fig. 2 shows the relationship between the ratio of fine particles having a second particle size or smaller to the coarse particles having a first particle size or smaller, and the coke strength, when the first particle size is 3 mm and the second particle size is 0.5 mm or 1 mm. As shown in Fig. 2, a relatively good correlation was observed in this example as well.
[0027] FIG. 3 is a graph showing the relationship between the proportion of fine powder having a second particle size or less in the coarse powder having a first particle size or less and the coke strength when the first particle size is 6 mm and the second particle size is 0.5 mm, 1 mm, or 3 mm.
[0028] In the example shown in Fig. 3, it is also possible to predict coke strength from the proportion of fine powder. However, when the second particle size was set to 3 mm, the correlation became slightly worse, and the correlation tended to worsen as the second particle size became larger.
[0029] FIG. 4 is a graph showing the relationship between the proportion of fine powder having a second particle size or smaller in the coarse powder having a first particle size or smaller and the coke strength when the first particle size is 15 mm and the second particle size is 0.5 mm, 1 mm, 3 mm, or 6 mm.
[0030] In the example shown in Figure 4, it is also possible to predict coke strength from the proportion of fine powder equal to or smaller than the second particle size. However, as in the case of Figure 3, the correlation tends to worsen as the second particle size increases.
[0031] Figure 5 shows the relationship between the ratio of fine particles having a second particle size or smaller to the coarse particles having a first particle size or smaller and coke strength when the first particle size is 25 mm and the second particle size is 0.5 mm, 1 mm, 3 mm, 6 mm, or 15 mm. In the examples of Figure 5, the correlation is poor, and there are also cases (Figure 5 (2) to (5)) where a correlation opposite to that in the examples of Figures 1 to 4 is observed. Therefore, it was found that when the first particle size is 25 mm, coke strength cannot be estimated well.
[0032] From the above results, a guideline was obtained for how to select the first and second particle sizes in order to estimate coke strength. Table 1 shows the first and second particle sizes and the coefficient of determination R obtained under each condition in each correlation shown in Figures 1 to 5. 2 The following is a summary of the coefficient of determination R 2 The figures are rounded off to two decimal places.
[0033] [Table 1]
[0034] From Table 1, for the first particle size, the smaller the particle size, the higher the coefficient of determination R 2, and a high correlation is observed. When the first particle size is 15 mm, the coefficient of determination is sufficiently high if the second particle size is 0.5 mm, and it is preferable that the first particle size is 15 mm or less. Figure 6 shows the relationship between the first particle size and the coefficient of determination R when the second particle size is 0.5 mm. 2 From Fig. 6, when the first particle size is 10 mm or less, the coefficient of determination R 2 Since it is estimated that the correlation coefficient is 0.75 or more, a more preferable first particle size is 10 mm or less. An even more preferable first particle size is 6 mm or less. In addition, the smaller the particle size is, the higher the correlation is, so that the second particle size is preferably 1 mm or less, and more preferably 0.5 mm or less. From the results, it was found that, under the condition that the first particle size is 15 mm or less and the second particle size is 1 mm or less, there is a high correlation between the ratio of fine powder of the second particle size in the coarse powder of the first particle size or less and the coke strength.
[0035] As a numerical value expressing the particle size of the broken powder, the average particle size of the coke powder below a certain particle size (hereinafter referred to as the "third particle size") can also be used. The third particle size of the broken powder is set to 1 mm, 3 mm, 6 mm, 15 mm, or 25 mm, and FIG. 7 shows the relationship between the average particle size of the coke powder below the third particle size and the coke strength (DI(150 / 15)). The average particle size on the horizontal axis is logarithmic. Here, the average particle size is the arithmetic mean particle size calculated from the mass ratio of the coke powder in each particle size range.
[0036] As can be seen from Fig. 7, when the third particle size is 1 mm, 3 mm, or 6 mm, there is a tendency for the coke strength to increase as the average particle size becomes smaller. This coincides with the tendency shown in Figs. 1 to 5 that the coke strength increases as the proportion of fine powder of the second particle size or less in the coarse powder of the first particle size or less increases. Note that the coefficient of determination R of the correlation between the average particle size of coke powder of the third particle size or less and coke strength when the third particle size is 6 mm (Fig. 7(3)), 3 mm (Fig. 7(2)), and 1 mm (Fig. 7(1)) is 2The coefficient of determination R was 0.57 or more in both cases, indicating a good correlation. On the other hand, when the third particle size was set to 15 mm (Figure 7 (4)) and 25 mm (Figure 7 (5)), the coefficient of determination R 2 was found to be small and the correlation was low.
[0037] From the above results, it was found that by setting the third particle size to 10 mm, it is possible to predict the coke strength from the average particle size of the coke breeze that is equal to or smaller than the third particle size. A more preferable value of the third particle size is 1 mm to 6 mm.
[0038] According to conventional knowledge, the broken powder with a particle size of 0.5 mm or less is mainly generated by compression fracture, and the broken powder with a particle size of 6 mm or more is mainly generated by volume fracture. The broken powder with a particle size of 0.5 mm to 6 mm is considered to be intermediate between the two broken powders. The relationship between the coke strength and the size of the broken powder generated by the destruction of the coke has not been elucidated until now, but the experiment conducted by the present inventors revealed for the first time that the proportion of fine powder due to compression fracture in the broken powder increases with the coke's drum strength index DI (150 / 15). In addition, a high proportion of fine powder in the broken powder generated by the destruction of the coke means that the weight loss of the coke lump tends to be small, and it is considered that the lump yield after impact is high.
[0039] From the above study results, the inventors found that if the ratio of fine powder having a second particle size or less in the coarse powder having a first particle size or less and the particle size of the broken powder, such as the average particle size, are known, the drum strength of the coke can be estimated using the ratio as an index. For example, as shown in Patent Document 1, a method of estimating coke strength using the particle size distribution of the coke has been known in the past, but in the case of the present invention, the strength of the coke can be estimated by determining the particle size distribution of a part of the broken powder generated by the destruction of the coke. Therefore, there is an advantage that the coke strength can be estimated with a small amount of sample. For example, if the broken powder has a maximum particle size of 6 mm, a sample of about several kg can be enough to estimate the coke strength. Therefore, the technology according to the present invention can reduce the amount of sample to be sampled, measured, and post-treated compared to the prior art, and can achieve miniaturization of the device and simplification and speed of the work.
[0040] [Method of estimating coke strength] A method for estimating coke strength based on the above findings will be described below. In the above-mentioned confirmation of the principle of the present invention, the coke was destroyed using a drum test machine, but the coke is destroyed by various forces, such as impact force and compression force. For example, the coke is destroyed by impacts received during the production and transportation process (charged into a coke dry quenching system (CDQ system), impacts received during the process of unloading, impacts received during a drop when changing conveyor belts, charge when storing in a hopper, impacts received during the process of unloading, etc.). Therefore, in the present invention, the broken powder generated by the above-mentioned impacts may be collected and used. Also, a dedicated impact mechanism may be provided, and the broken powder may be obtained from the coke sampled by the mechanism. In particular, the impact in the CDQ system is theoretically closer to the mechanism of impact received in a blast furnace than the conventional rotation test, so that the coke strength in blast furnace operation can be estimated more accurately by using the information on the broken powder generated by the impacts than the conventional rotation strength index. Furthermore, the CDQ system is advantageous in terms of cost because it does not require the addition of special equipment, and is a particularly effective method.
[0041] The location for sampling the broken powder may be any location in the transportation process from the coke oven to the blast furnace, but it is preferable to sample the broken powder when it has been subjected to a certain amount of impact and a large amount of broken powder has been generated, because this makes it easier to collect the broken powder. For example, the location may be inside the CDQ facility or its outlet, on the belt conveyor, at the junction of the belt conveyor, inside the debris tank or its outlet, or in a sieving device.
[0042] Incidentally, when the broken fines generated in the CDQ plant are the subject of the research, the recovery amount of the broken fines is considered to depend not only on the strength of the coke drum but also on the operating conditions of the CDQ plant. For example, if the amount of broken fines generated and the flow rate of the reflux gas change with an increase or decrease in the amount of coke processed, the dust collection efficiency in the dust collector is expected to change. Therefore, in the method of estimating drum strength from the total amount of dust collected by a dust collection facility as in Patent Document 2, there is a concern that the estimation accuracy may decrease due to the influence of operating conditions.
[0043] On the other hand, in the estimation method of the present invention, the impacts received in the CDQ equipment are mainly the drop when the coke is charged into the pre-chamber at the top of the equipment and the abrasion when the coke is lowered inside the equipment (between the coke lumps and between the coke and the equipment inner wall), both of which are specific to the equipment and are considered to be less affected by the operating conditions of the CDQ equipment. Therefore, according to the present invention, it is possible to stably estimate the drum strength, and in addition, although it is necessary to obtain information on a certain particle size among the generated broken powder, information on the total amount of broken powder is not necessarily required. Therefore, it can be said that the present invention is a simpler and more advantageous method.
[0044] The value representing the particle size distribution may change depending on the generation state of the broken powder, the method of collecting the broken powder, etc. Therefore, it is necessary to collect information on the particle size of the actually collected broken powder and obtain a correlation between the index value of the particle size distribution of the broken powder and the coke strength in advance. The correlation may be obtained in the same manner as the method of obtaining the relationship between the broken powder and the coke strength using the drum test machine described above. In this way, in the present invention, by obtaining the correlation between the particle size of the broken powder and the coke strength in advance, the coke strength can be estimated based on the correlation from the particle size distribution of the collected broken powder.
[0045] The coke strength to be estimated is not limited to DI (150 / 15) as defined by JIS. The number of rotations of the drum may be changed, or the sieve size measured after the drum is rotated may be different. For example, since a rotating drum similar to that defined by JIS is used in the ASTM and Micam tests, the estimation method of the present invention can be suitably applied. The estimation method of the present invention can also be used for a strength index that represents the pulverization caused by the drop impact of an I-type drum or the pulverization characteristics caused by abrasion. In the present invention, the correlation between the coke strength and the index that represents the particle size distribution of the broken powder exemplified in the present invention is obtained in advance, so that the present invention can be suitably applied to any strength index that has a good correlation.
[0046] The first particle size for obtaining information on the particle size of the broken powder is preferably 15 mm or less, more preferably 10 mm or less, as revealed by the above-mentioned drum strength tester test of the broken powder. The second particle size is smaller than the first particle size. If the second particle size and the first particle size are close to each other, the ratio of fine powders equal to or less than the second particle size will be close to 100%, and the detection sensitivity when measuring the ratio of particles equal to or less than the second particle size may decrease. Therefore, the second particle size is preferably 0.7 times or less than the first particle size, more preferably 0.5 times or less, and a specific value is preferably 1 mm or less, more preferably 0.5 mm or less. The same applies to the third particle size, and as revealed by the above-mentioned drum strength tester test of the broken powder, the third particle size may be 10 mm or less, more preferably 6 mm or less. In practice, when determining the correlation between the coke strength and the particle size of the broken powder in advance, the first, second and third particle sizes can be determined so that the correlation is highly expressed. Regarding the average particle size, various representative values of particle size distribution, such as the arithmetic mean diameter, harmonic mean diameter, median value, mode value, etc., can also be used.
[0047] There is no particular designation for the method of sampling the broken powder, so long as the representativeness of the sample can be guaranteed. For example, broken powder generated in a CDQ facility can be sampled by the following method. In a CDQ facility, an inert gas (nitrogen) is circulated to extinguish the coke and recover heat, and broken powder is entrained in the circulating gas. Therefore, a method of aspirating and sampling the broken powder entrained in the circulating gas can be used. As mentioned above, the broken powder is generally collected using a dust collector installed in the circulating gas flow path of the CDQ facility. Another method is to sample the broken powder after collection using an appropriate sampler. Other suitable methods include sampling the broken powder at the rear of the sieving device or below the sieve.
[0048] The method for measuring the particle size of the broken powder is not particularly limited as long as it can accurately measure a specific particle size distribution range (particularly, in the case of the present invention, particle size distribution of 15 mm or less). For example, the broken powder may be sieved to determine the mass ratio of each particle size, and examples of a quick and simple measurement method include the use of an automatic sieving device, measurement by image processing, and measurement by laser diffraction. In particular, the particle size measurement method by laser diffraction is particularly preferred because it can be measured easily and accurately in a short time of less than 1 minute.
[0049] The laser diffraction method is particularly preferable because it is possible to measure the particle size of the broken powder accompanying the return gas of the CDQ equipment in-line, and therefore the particle size distribution of the broken powder can be measured in real time. However, since the return gas is at high temperatures, exceeding 900°C in some places, it is necessary to provide the particle size distribution measuring device with appropriate heat resistance. In addition, since fine powder has a tendency to aggregate, it is necessary to properly eliminate the aggregation state of the fine powder in order to measure the particle size distribution with high accuracy. Therefore, it is desirable to eliminate the aggregation state by performing pre-treatment such as drying the sample and crushing or dispersing the pseudo particles before measuring the particle size distribution.
[0050] <Example> This example shows an example of estimating the drum strength of coke from the particle size distribution of broken fines intermittently collected by the CDQ equipment. The amount of coke charged into the CDQ equipment was treated as the same lot in units of about 125 t (approximately the amount of coke for five coke chambers), and while the coke of that lot was being cooled, broken fines were collected from the flow path of the circulating gas, and the coke was sampled at the outlet side of the CDQ equipment. The drum strength of the cooled coke was investigated. Note that the conditions such as the charging rate of the coke into the CDQ equipment and the flow rate of the circulating gas were kept constant.
[0051] Sampling and particle size measurement of the broken powder was carried out by branching a part of the circulating gas pipe of the CDQ equipment, introducing a part of the circulating gas into the branch pipe and cooling it, and measuring the particle size of the broken powder accompanying the circulating gas after cooling by laser diffraction. The broken powder accompanying the circulating gas of the CDQ equipment contained a small amount of powder with a particle size of about 5 mm, but the total amount was 6 mm or less. In addition, since it was in a dry state, it was not necessary to eliminate the agglomeration state.
[0052] The lump coke samples for drum strength measurement were taken in five increments (samples) for each lot by an automatic sampler installed on the belt conveyor at the CDQ facility outlet. Approximately 250 kg was taken per increment. These samples were divided into samples for drum test by an automatic dividing machine conforming to JIS, and the samples were used for the drum test.
[0053] First, for 10 lots, the correlation between the ratio (mass%) of fine powder with a particle size of 0.5 mm or less to the coarse powder with a particle size of 6 mm or less and the drum strength index DI (150 / 15) was obtained in the same manner as in the investigation using the drum test machine described above. The results are shown in Figure 8.
[0054] As shown in Figure 8, a high positive correlation was confirmed between the ratio (mass%) of fine powder with a particle size of 0.5 mm or less to the coarse powder with a particle size of 6 mm or less and the drum strength index DI (150 / 15). The regression equation obtained from this relationship is shown in the following equation (1). Estimated DI (150 / 15) = (proportion (mass%) of fine powder with a particle size of 0.5 mm or less among coarse powder with a particle size of 6 mm or less) × 0.1192 + 78.162 (1) This correlation is different from the correlation shown in Fig. 3, which is thought to be due to the difference in the coke used in the test, the difference in the crushing morphology, the difference in the method of recovering the crushed powder, etc.
[0055] Next, for another lot of coke, the broken powder was collected while the coke was being cooled, and the ratio (mass%) of fine powder with a particle size of 0.5 mm or less to the coarse powder with a particle size of 6 mm or less was measured. In addition, the coke strength DI (150 / 15) of the cooled and collected lump coke was actually measured (actual DI) in the same manner as in determining the above correlation.
[0056] Based on the correlation shown in Fig. 8, coke strength was estimated (estimated DI) from the proportion of fine particles with a particle size of 0.5 mm or less among coarse particles with a particle size of 6 mm or less, and the relationship between the estimated DI and the measured DI was plotted, as shown in Fig. 9. From the results in Fig. 9, a good correlation was confirmed between the estimated DI and the measured DI, and it was confirmed that the method of the present invention makes it possible to estimate the drum strength index from information on the particle size of the broken powder.
Claims
1. A method for estimating coke strength, comprising: measuring a proportion of fine particles smaller than the particle size of coarse particles having a particle size of 15 mm or less among the broken particles generated by the destruction of coke; and estimating coke strength based on a previously determined relationship between the coke strength and the proportion of fine particles.
2. 2. The method for estimating coke strength according to claim 1, characterized in that the particle size of the coarse powder is equal to or smaller than any particle size of 10 mm or less, and the particle size of the fine powder is equal to or smaller than any particle size of 0.7 times the maximum particle size of the coarse powder and 1 mm or less.
3. A method for estimating coke strength, comprising: measuring an average particle size of coke powder generated by the destruction of coke, the average particle size of which is equal to or smaller than any particle size of 10 mm or less; and estimating the coke strength based on a relationship between a previously determined coke strength and the average particle size of the coke powder.
4. 4. The method for estimating coke strength according to claim 3, wherein the particle size of the coke breeze is 6 mm or less.
5. The method for estimating coke strength according to any one of claims 1 to 4, characterized in that the broken powder is powder recovered from the circulating gas of a coke dry quenching facility.
6. The method for estimating coke strength according to claim 1 or 2, characterized in that the particle size distribution of the broken powder is determined by a laser diffraction method, and the proportion of the fine powder, which is smaller than the coarse powder, in the coarse powder is determined from the particle size distribution obtained.
7. The method for estimating coke strength according to claim 3 or 4, characterized in that the particle size distribution of the broken powder is obtained by a laser diffraction method, and the average particle size of the coke powder having a particle size of 10 mm or less is obtained from the obtained particle size distribution.
Citation Information
Patent Citations
Pulverized coal boiler coking prediction method based on coal ash fusibility and particle size influence
CN111982762A
Method for estimating coke strength
JP1997263764A
Method for estimating coke strength
JP2007284615A
Quality control method of blast furnace coke
JP2020012132A
Quality evaluation method of coke for blast furnace
JP2024125585A
Cited By
Strength estimation device for granular material, strength estimation method for granular material, manufacturing method of granular material and manufacturing method of coke
JP2024140885A
Granular material strength estimation device, granular material strength estimation method, granular material manufacturing method, and coke manufacturing method
JP7803305B2