Laser welding method
Ultrasonic vibration in laser welding methods addresses heat-induced air bubble issues by direct bonding of base materials, reducing defects and ensuring robust welds.
Patent Information
- Application Number
- JP2023050491
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing laser welding methods face issues with air bubbles becoming large due to excessive heat input, leading to spatter and bonding failures, as well as potential leakage defects.
A method involving ultrasonic vibration to remove oxide films before welding, allowing direct bonding of base materials with reduced heat input, thereby suppressing bubble growth and defects.
Reduces heat input requirements, minimizing bubble size and preventing bonding and leakage defects during laser welding.
Smart Images

Figure 2024139519000001_ABST
Abstract
Description
[Technical field]
[0001] SUMMARY OF THE DISCLOSURE An embodiment of the present invention relates to a laser welding method. [Background technology]
[0002] There is a laser welding method in which a plurality of members are welded together by irradiating them with laser light. In the laser welding method, for example, the plurality of members are temporarily joined together, and then the plurality of members are welded together by irradiating them with laser light.
[0003] In such a laser welding method, if the heat input during temporary fixing or laser beam irradiation is large, the bubbles contained in the members may become large. If the bubbles contained in the members become large, sputtering may occur from the members during laser beam irradiation, causing a joining failure. In addition, if the bubbles contained in the members become large, there is a risk of leakage failure due to the bubbles. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-19046 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a laser welding method capable of suppressing poor joints and leak defects. [Means for solving the problem]
[0006] The laser welding method according to the embodiment is a method for welding a second member to a first member by irradiating a laser beam. The laser welding method according to the embodiment includes a preparation step and a welding step. In the preparation step, a joining member in which the second member is joined to the first member is prepared. In the welding step, the joining member is irradiated with a laser beam to weld the second member to the first member. The first member includes a first base material and a first oxide film formed on a surface of the first base material. The second member includes a second base material and a second oxide film formed on a surface of the second base material. In the preparation step, the first member and the second member are ultrasonically vibrated in a state in which the second member is overlapped on the first member so that the first oxide film and the second oxide film are in contact with each other, thereby removing the first oxide film and the second oxide film, and joining the second base material to the first base material. In the welding step, the second base material is welded to the first base material by irradiating the laser beam to a portion where the second base material is joined to the first base material. [Brief description of the drawings]
[0007] [Figure 1] 1(a) to 1(c) are perspective views illustrating a laser welding method according to a first embodiment. [Diagram 2] FIG. 2 is a plan view showing a welded portion in the laser welding method according to the first embodiment. [Diagram 3] 3(a) and 3(b) are explanatory views for explaining the preparation step and the welding step according to the embodiment. [Figure 4] 4(a) to 4(c) are explanatory diagrams illustrating bonding by ultrasonic vibration. [Diagram 5] 5(a) to 5(c) are perspective views showing a laser welding method according to the second embodiment. [Figure 6] FIG. 11 is a plan view showing a welded portion in a laser welding method according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The drawings are schematic or conceptual, and the relationship between the thickness and width of each part, the size ratio between parts, etc. are not necessarily the same as those in reality. Even when the same part is shown, the dimensions and ratios of each part may be different depending on the drawing. In this specification and each drawing, elements similar to those described above with reference to the previous drawings are given the same reference numerals and detailed descriptions thereof will be omitted as appropriate.
[0009] (First embodiment) 1(a) to 1(c) are perspective views illustrating a laser welding method according to a first embodiment. FIG. 2 is a plan view showing a welded portion in the laser welding method according to the first embodiment. As shown in FIGS. 1(a) to 1(c), the laser welding method according to the embodiment includes a preparation step and a welding step.
[0010] In the laser welding method according to the embodiment, a preparation step is first performed. In the preparation step, a first member 10 and a second member 20 to be welded are prepared as shown in FIG.
[0011] The first member 10 and the second member 20 include at least one of aluminum, magnesium, and copper, for example. The first member 10 and the second member 20 preferably include aluminum, for example. The material of the second member 20 may be the same as the material of the first member 10, or may be different.
[0012] The first member 10 is, for example, a housing having an opening 16. The first member 10 has, for example, a substantially rectangular box-like structure with an open top. The first member 10 has, for example, a first side portion 11, a second side portion 12, a third side portion 13, a fourth side portion 14, and a bottom portion 15. The bottom portion 15 is located at the bottom of the first member 10. The first side portion 11, the second side portion 12, the third side portion 13, and the fourth side portion 14 are each an upright portion rising upward from the bottom portion 15. The first side portion 11 and the third side portion 13 face each other. The second side portion 12 and the fourth side portion 14 face each other. The first member 10 has, for example, an opening 16 formed by the upper end of the first side portion 11, the upper end of the second side portion 12, the upper end of the third side portion 13, and the upper end of the fourth side portion 14.
[0013] The second member 20 is, for example, a lid that closes the opening 16 of the first member 10. The second member 20 has, for example, a flat plate-like structure. As shown in FIG. 2, the second member 20 has a welded portion 25. In FIG. 2, the welded portion 25 is shown by shading. The welded portion 25 is a portion that is welded to the first member 10 in the welding process. The welded portion 25 is, for example, a portion that is irradiated with laser light 300 in the welding process. The welded portion 25 is provided in a portion of the second member 20 that overlaps with the first member 10. In this example, the welded portion 25 is provided at a position where the opening 16 and the second member 20 (lid) overlap.
[0014] In this example, the first member 10 is a housing and the second member 20 is a lid, but the shapes of the first member 10 and the second member 20 are not limited to this. The shapes of the first member 10 and the second member 20 may be any shapes that can be welded by laser irradiation. For example, both the first member 10 and the second member 20 may be flat.
[0015] In the preparation step, next, as shown in FIG. 1(b), a joining member 50 in which a second member 20 is joined to a first member 10 is prepared. The joining member 50 has a structure in which the second member 20 is welded to the first member 10 via a connection portion 30 provided along a welded portion 25. That is, in the joining member 50, the first member 10 and the second member 20 are joined via the connection portion 30. As will be described later, in the embodiment, the connection portion 30 is a portion where the first member 10 (first base material 10a) and the second member 20 (second base material 20a) are joined (connected) by ultrasonic vibration.
[0016] 2, in this example, in the preparation step, the entire circumference of the overlapping portion of the opening 16 of the housing (first member 10) and the lid (second member 20) is continuously joined. That is, in this example, the connection portion 30 is provided continuously around the entire circumference of the welded portion 25. In other words, the opening 16 of the housing (first member 10) and the lid (second member 20) are continuously joined around the entire circumference.
[0017] In the laser welding method according to the embodiment, a welding step is then performed. The welding step is performed after the preparation step. In the welding step, as shown in Fig. 1(c), a laser beam 300 is irradiated along a welding portion 25 of the joining member 50 to weld the second member 20 to the first member 10. Thereby, for example, as shown in Fig. 2(b), a sealed member 100 is manufactured in which the opening 16 of the first member 10 (housing) is sealed by the second member 20 (lid).
[0018] The laser device for irradiating the laser light 300 used in the welding process may be, for example, a pulsed laser that oscillates a pulsed output at a constant repetition frequency (pulse width), or a CW (Continuous Wave) laser that continuously oscillates a constant output. In the case of a pulsed laser, the pulse width is, for example, several femtoseconds or several picoseconds. The wavelength of the laser light 300 is, for example, 300 nm or more and 1070 nm or less.
[0019] The preparation step and the welding step will be described in more detail below. 3(a) and 3(b) are explanatory views for explaining the preparation step and the welding step according to the embodiment. As shown in FIG. 3(a) and FIG. 3(b), the first member 10 includes a first base material 10a and a first oxide film 10b formed on the surface of the first base material 10a. The first base material 10a includes a metal. The first oxide film 10b is, for example, a natural oxide film. The second member 20 includes a second base material 20a and a second oxide film 20b formed on the surface of the second base material 20a. The second base material 20a includes a metal. The second oxide film 20b is, for example, a natural oxide film. In this manner, oxide films (the first oxide film 10b and the second oxide film 20b) are formed on the surfaces of the first member 10 and the second member 20.
[0020] For example, when the first member 10 and the second member 20 contain aluminum, the first base material 10a and the second base material 20a are mainly made of aluminum. For example, when the first member 10 and the second member 20 contain aluminum, the first oxide film 10b and the second oxide film 20b are mainly made of aluminum oxide.
[0021] The melting point of aluminum oxide (2072°C) is higher than the melting point of aluminum (660°C). Therefore, when an oxide film (first oxide film 10b or second oxide film 20b) is formed on the surface of a base material (first base material 10a or first base material 20a), in order to weld the second member 20 to the first member 10, it is necessary to input heat up to about 2000°C, which is close to the melting point of aluminum oxide, during laser light irradiation.
[0022] In addition, in the laser welding method, for example, a plurality of members are temporarily joined together and then irradiated with a laser beam to weld the plurality of members. Conventionally, temporary joining has been performed by a method such as temporary welding that irradiates a laser beam.
[0023] However, if the heat input during temporary fixing or laser light irradiation is large, the bubbles contained in the components may become large. If the bubbles contained in the components become large, sputtering may occur from the components during laser light irradiation, which may cause poor bonding. Furthermore, if the bubbles contained in the components become large, there is a risk of leaking due to the bubbles.
[0024] Therefore, in the embodiment, as shown in FIG. 3(a), in the preparation step, the first member 10 and the second member 20 are ultrasonically vibrated in a state where the second member 20 is overlapped on the first member 10 so that the first oxide film 10b and the second oxide film 20b are in contact with each other. As a result, the first oxide film 10b and the second oxide film 20b are removed, and the second base material 20a is directly bonded to the first base material 10a. Then, as shown in FIG. 3(b), in the welding step, the portion where the second base material 20a is bonded to the first base material 10a is irradiated with laser light 300, thereby welding the second base material 20a to the first base material 10a.
[0025] In this way, by performing ultrasonic vibration in the preparation process, the first oxide film 10b and the second oxide film 20b can be removed, and the second base material 20a can be directly bonded to the first base material 10a. This makes it possible to prepare a bonding member 50 in which the first member 10 and the second member 20 are bonded, without performing temporary welding by irradiating laser light. Therefore, the amount of heat input in the preparation process can be reduced compared to the case of performing temporary welding by irradiating laser light. This makes it possible to prevent bubbles contained inside the first member 10 and the second member 20 from becoming larger, and to prevent bonding failures and leak failures.
[0026] In addition, by removing the first oxide film 10b and the second oxide film 20b in the preparation process, the second member 20 can be welded to the first member 10 without heat input to a temperature close to the melting point of the first oxide film 10b and the second oxide film 20b in the welding process (just by heat input to a temperature close to the melting point of the first base material 10a and the second base material 20a). More specifically, for example, when the first member 10 and the second member 20 contain aluminum, the second member 20 can be welded to the first member 10 without heat input to about 2000°C, which is close to the melting point of aluminum oxide, in the preparation process (just by heat input to about 600°C, which is close to the melting point of aluminum). Therefore, the amount of heat input in the welding process can be reduced compared to the case where temporary welding is performed by irradiating laser light without performing joining by ultrasonic vibration. This makes it possible to suppress the enlargement of bubbles contained inside the first member 10 and the second member 20, and to suppress poor joining and leaking.
[0027] In addition, in the welding method according to the embodiment, in the welding step, the laser light 300 is irradiated to the portion where the first base material 10a and the second base material 20a are joined. That is, in the preparation step, ultrasonic vibration is performed on at least a part of the portion to be irradiated with the laser light 300 in the welding step. In other words, the portion to which the ultrasonic vibration is performed in the preparation step overlaps with at least a part of the portion to be irradiated with the laser light 300 in the welding step. As a result, it is possible to suppress the enlargement of bubbles contained inside the first member 10 and the second member 20, and to suppress poor joining and leaking, compared to a case where the portion to which the ultrasonic vibration is performed in the preparation step and the portion to which the laser light 300 is irradiated in the welding step are different (do not overlap).
[0028] An ultrasonic vibration device is used as the means for ultrasonically vibrating the first member 10 and the second member 20. The ultrasonic vibration device applies ultrasonic vibration to the first member 10 and the second member 20, for example, by vibrating an anvil 200 attached to the second member 20 so as to be in contact with the second member 20 at high speed. The anvil 200 of the ultrasonic vibration device may be attached to be in contact with the first member 10, or may be attached to be in contact with both the first member 10 and the second member 20, for example.
[0029] 4(a) to 4(c) are explanatory diagrams illustrating bonding by ultrasonic vibration. 4(a) to 4(c) are enlarged views of the region R1 shown in FIG. 3(a). As shown in Fig. 4(a), before ultrasonic vibration is applied, a first oxide film 10b is formed on the surface of the first substrate 10a, and a second oxide film 20b is formed on the surface of the second substrate 20a. That is, before ultrasonic vibration is applied, the first substrate 10a and the second substrate 20a are separated by the first oxide film 10b and the second oxide film 20b. In other words, before ultrasonic vibration is applied, the first substrate 10a and the second substrate 20a are not in direct contact with each other.
[0030] 4(b), when the ultrasonic vibration is started, a part of the first oxide film 10b and a part of the second oxide film 20b are destroyed and removed by the ultrasonic vibration. Then, by removing a part of the first oxide film 10b and a part of the second oxide film 20b, the first base material 10a and the second base material 20a, which were separated by the first oxide film 10b and the second oxide film 20b, come into direct contact with each other.
[0031] 4(c), after the ultrasonic vibration is applied, the first base material 10a and the second base material 20a are bonded in a state of being in direct contact with each other. Therefore, as described above, in the welding process, the second member 20 can be welded to the first member 10 without inputting heat to a temperature close to the melting points of the first oxide film 10b and the second oxide film 20b (only by inputting heat to a temperature close to the melting points of the first base material 10a and the second base material 20a).
[0032] In the laser welding method according to the first embodiment, in addition to the ultrasonic vibration, temporary welding by irradiation of laser light may be performed in the preparation step. By performing temporary welding by irradiation of laser light, for example, it is possible to prepare a joining member 50 in which the second member 20 is more firmly joined to the first member 10.
[0033] In this case, it is preferable to perform bonding by ultrasonic vibration before temporary welding. By performing bonding by ultrasonic vibration before temporary welding, the amount of heat input during temporary welding can be reduced, so the amount of heat input in the preparation process can be reduced compared to the case where temporary welding is performed by irradiating laser light without performing bonding by ultrasonic vibration. Therefore, it is possible to prevent air bubbles contained inside the first member 10 and the second member 20 from becoming larger, and to prevent bonding failure and leakage failure.
[0034] Second embodiment 5(a) to 5(c) are perspective views showing a laser welding method according to the second embodiment. FIG. 6 is a plan view showing a welded portion in the laser welding method according to the second embodiment. 5(a) to 5(c) and 6, in the laser welding method according to the second embodiment, in a preparation step, the entire circumference of the overlapping portion between the opening 16 of the housing (first member 10) and the lid (second member 20) is discontinuously joined at multiple locations. Other than that, the laser welding method is substantially the same as the laser welding method according to the first embodiment.
[0035] That is, in this example, the connection parts 30 are provided at multiple locations discontinuously around the entire circumference of the welded portion 25. In other words, the opening 16 of the housing (first member 10) and the lid (second member 20) are joined discontinuously around the entire circumference. In this example, the connection parts 30 are provided at equal intervals around the entire circumference of the welded portion 25. Note that the intervals between the multiple connection parts 30 do not have to be equal.
[0036] In this example, the first oxide film 10b and the second oxide film 20b are removed by applying ultrasonic vibration in the preparation step, and the second base material 20a can be directly bonded to the first base material 10a. This makes it possible to prepare a bonding member 50 in which the first member 10 and the second member 20 are bonded to each other without performing temporary welding by irradiating a laser beam. Therefore, the amount of heat input in the preparation step can be reduced compared to the case of performing temporary welding by irradiating a laser beam. This makes it possible to prevent bubbles contained inside the first member 10 and the second member 20 from becoming larger, and to prevent bonding failures and leak failures.
[0037] The embodiment may include the following features.
[0038] (Configuration 1) A method for welding a second member to a first member by irradiating a laser beam, comprising: a preparation step of preparing a joint member in which the second member is joined to the first member; a welding process of welding the second member to the first member by irradiating the joining member with a laser beam; Equipped with the first member includes a first base material and a first oxide film formed on a surface of the first base material; the second member includes a second base material and a second oxide film formed on a surface of the second base material, In the preparation step, the second member is placed on the first member such that the first oxide film and the second oxide film are in contact with each other, and the first member and the second member are ultrasonically vibrated to remove the first oxide film and the second oxide film, thereby bonding the second base material to the first base material; A laser welding method, in which, in the welding step, the laser light is irradiated to a portion where the second base material is joined to the first base material, thereby welding the second base material to the first base material.
[0039] (Configuration 2) the first member is a housing having an opening, the second member is a lid that closes the opening, 2. The laser welding method according to claim 1, wherein the housing and the lid are welded at a position where the opening and the lid overlap.
[0040] (Configuration 3) In the preparation step, the entire periphery of the overlapping portion of the opening and the lid is continuously joined; 3. The laser welding method according to claim 2, wherein in the welding step, the laser beam is continuously irradiated to an entire circumference of an overlapping portion of the opening and the lid.
[0041] (Configuration 4) In the preparation step, the opening and the lid are discontinuously joined at a plurality of locations around an entire periphery of the overlapping portion, 3. The laser welding method according to claim 2, wherein in the welding step, the laser beam is continuously irradiated to an entire circumference of an overlapping portion of the opening and the lid.
[0042] (Configuration 5) 5. The laser welding method according to any one of configurations 1 to 4, wherein the first member and the second member contain aluminum.
[0043] As described above, according to the embodiment, a laser welding method capable of suppressing poor joints and leak defects is provided.
[0044] The laser welding method according to the embodiment can be suitably used for manufacturing devices such as secondary batteries, heat exchangers such as heat sinks, gas generators used in airbags, and rotors for air conditioners.
[0045] Although the embodiment of the present invention has been illustrated above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This new embodiment can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0046] 10: First member 10a: 1st base material 10b: First oxide film 11~14: 1st~4th side part 15: Bottom part 16: Opening 20: Second member 20a: Second base material 20b: Second oxide film 25: Welded part 30: Connection 50: Joint material 100: Sealing member 200: Anvil 300: Laser light
Claims
1. A method for welding a second member to a first member by irradiating a laser beam, comprising: a preparation step of preparing a joint member in which the second member is joined to the first member; a welding step of welding the second member to the first member by irradiating the joining member with a laser beam; Equipped with The first member includes a first base material and a first oxide film formed on a surface of the first base material, the second member includes a second base material and a second oxide film formed on a surface of the second base material, In the preparation step, the second member is placed on the first member such that the first oxide film and the second oxide film are in contact with each other, and the first member and the second member are ultrasonically vibrated to remove the first oxide film and the second oxide film, thereby bonding the second base material to the first base material; A laser welding method, in which, in the welding step, the laser light is irradiated to a portion where the second base material is joined to the first base material, thereby welding the second base material to the first base material.
2. the first member is a housing having an opening, the second member is a lid that closes the opening, The laser welding method according to claim 1 , wherein the housing and the lid are welded at a position where the opening and the lid overlap.
3. In the preparation step, the entire periphery of the overlapping portion of the opening and the lid is continuously joined; The laser welding method according to claim 2 , wherein in the welding step, the laser beam is continuously irradiated onto an entire circumference of an overlapping portion between the opening and the lid.
4. In the preparation step, the opening and the lid are discontinuously joined at a plurality of locations around an entire periphery of the overlapping portion, The laser welding method according to claim 2 , wherein in the welding step, the laser beam is continuously irradiated onto an entire circumference of an overlapping portion between the opening and the lid.
5. 5. The laser welding method according to claim 1, wherein the first member and the second member contain aluminum.
Citation Information
Patent Citations
Method for joining metallic thin sheet
JP1999077337A
Battery and manufacture thereof
JP2000090893A
Joining method, joining device and structure
JP2020019046A