Vinyl chloride-based resin composition and vinyl chloride-based resin molding

The vinyl chloride resin composition with organotin stabilizers and sodium salt of aliphatic carboxylic acid particles addresses thermal stability and mold corrosion issues, ensuring improved mechanical strength and heat resistance in molded products.

JP2024139708APending Publication Date: 2024-10-09SEKISUI CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024026613
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-02-26
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Vinyl chloride resin compositions face challenges in thermal stability during hot molding due to hydrogen chloride generation, leading to mechanical strength reduction and mold corrosion, and existing stabilizers like organic tin compounds and alkali metal salts of fatty acids have limitations in dispersibility and thermal stability.

Method used

A vinyl chloride resin composition incorporating organotin stabilizers and particles of sodium salts of aliphatic carboxylic acids with controlled particle size, porosity, and aspect ratio to enhance dispersibility and thermal stability, reducing hydrogen chloride corrosion and improving heat resistance.

Benefits of technology

The composition improves thermal stability during hot molding, prevents mold corrosion, and enhances the mechanical strength and heat resistance of molded products, allowing for long-term production without discoloration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139708000001
    Figure 2024139708000001
Patent Text Reader

Abstract

To provide a vinyl chloride-based resin composition which can enhance dispersibility of particles of a sodium salt of an aliphatic carboxylic acid, and can enhance thermal stability in heating and molding.SOLUTION: A vinyl chloride-based resin composition contains a vinyl chloride-based resin, an organotin-based stabilizer, and particles of a sodium salt of an aliphatic carboxylic acid. In the particle size distribution based on the volume of the particles of the sodium salt of the aliphatic carboxylic acid, a particle diameter D50 is 5 μm or more and 50 μm or less and a particle diameter D90 is 85 μm or less, and the porosity of the particles of the sodium salt of the aliphatic carboxylic acid is 65 or more and 90 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vinyl chloride resin composition containing a vinyl chloride resin, and also to a vinyl chloride resin molded article using the vinyl chloride resin composition. [Background technology]

[0002] PVC resins have excellent mechanical strength, weather resistance, heat resistance, and chemical resistance, and are therefore processed into various molded articles such as pipes, plates, and containers, and are used in many fields.

[0003] However, when a molded article is obtained using a vinyl chloride resin, stable molding may be difficult because the vinyl chloride resin has low thermal stability and is prone to thermal decomposition due to the elimination of hydrogen chloride during hot molding, which may result in a decrease in mechanical strength of the molded article obtained or discoloration of the molded article.

[0004] In order to improve the thermal stability of the vinyl chloride resin, a thermal stabilizer may be used together with the vinyl chloride resin. Known examples of the thermal stabilizer include tin-based stabilizers, lead-based stabilizers, calcium-zinc-based stabilizers, barium-zinc-based stabilizers, and barium-cadmium-based stabilizers.

[0005] Patent Document 1 discloses a vinyl chloride resin composition containing a vinyl chloride copolymer and an organotin compound that is liquid at 23° C. The vinyl chloride copolymer contained in the vinyl chloride resin composition is a copolymer of a vinyl chloride monomer and a second monomer having a polyalkylene glycol group and an alkyl ether skeleton or an allyl ether skeleton at one end. In the vinyl chloride resin composition, the content of the organotin compound is 3 parts by weight or more per 100 parts by weight of the vinyl chloride copolymer.

[0006] Patent Document 2 discloses a halogen-containing polymer stabilizing composition containing an alkali metal salt of adipic acid and an alkali metal salt of a carboxylic acid having 1 to 22 carbon atoms. Patent Document 2 discloses polyvinyl chloride (PVC) and chlorinated polyvinyl chloride (C-PVC) as the halogen-containing polymer. The stabilizing composition may be used in combination with a conventional heat stabilizer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-165868 A [Patent Document 2] EP2363431A1 Summary of the Invention [Problem to be solved by the invention]

[0008] In Patent Document 1, the decomposition of the vinyl chloride resin is suppressed by an organotin compound, and the thermal stability of the vinyl chloride resin composition can be increased to a certain degree. In Patent Document 2, the thermal stability of the vinyl chloride resin composition can be increased to a certain degree by using a specific stabilizing composition.

[0009] However, when an organotin compound is used as in Patent Document 1, hydrogen chloride generated during hot molding cannot be sufficiently captured, and the thermal stability of the vinyl chloride resin composition is insufficient. In addition, the hydrogen chloride may corrode the metal surface of a mold or the like. As a result, there is a problem that it is difficult to produce molded articles using the vinyl chloride resin composition for a long period of time.

[0010] In addition, the melting point of the alkali metal salt of the fatty acid as described in Patent Document 2 may be higher than the processing temperature range (up to about 200°C) of the vinyl chloride resin composition, and the alkali metal salt of the fatty acid may continue to exist as a solid during processing of the vinyl chloride resin composition. Furthermore, the particles of the alkali metal salt of the fatty acid tend to form aggregates. Therefore, when obtaining a vinyl chloride resin composition, it is difficult to disperse the alkali metal salt of the fatty acid well in the vinyl chloride resin, and it is difficult to sufficiently increase the thermal stability of the obtained vinyl chloride resin composition during heat molding.

[0011] An object of the present invention is to provide a vinyl chloride resin composition which can enhance the dispersibility of particles of a sodium salt of an aliphatic carboxylic acid and can enhance the thermal stability during hot molding. Another object of the present invention is to provide a vinyl chloride resin molded article using the vinyl chloride resin composition. [Means for solving the problem]

[0012] This specification discloses the following vinyl chloride resin composition and vinyl chloride resin molded article.

[0013] Item 1. A vinyl chloride resin composition comprising a vinyl chloride resin, an organotin stabilizer, and particles of a sodium salt of an aliphatic carboxylic acid, wherein in a volume-based particle size distribution of the particles of the sodium salt of an aliphatic carboxylic acid, the particles have a particle size D50 of 5 μm or more and 50 μm or less and a particle size D90 of 85 μm or less, and the particles of the sodium salt of an aliphatic carboxylic acid have a porosity of 65 or more and 90 or less.

[0014] Item 2. The vinyl chloride resin composition according to Item 1, wherein the content of the particles of the sodium salt of the aliphatic carboxylic acid is 0.1 parts by weight or more and 3.0 parts by weight or less per 100 parts by weight of the vinyl chloride resin.

[0015] Item 3. The vinyl chloride resin composition according to Item 1 or 2, wherein the aspect ratio of the particles of the sodium salt of an aliphatic carboxylic acid is 1.00 or more and 1.8 or less.

[0016] Item 4. The vinyl chloride resin composition according to any one of Items 1 to 3, wherein the particles of the sodium salt of an aliphatic carboxylic acid are particles of disodium adipate.

[0017] Item 5. The vinyl chloride resin composition according to any one of Items 1 to 4, wherein the content of the organotin stabilizer is 0.1 parts by weight or more and 3.0 parts by weight or less based on 100 parts by weight of the vinyl chloride resin.

[0018] Item 6. The vinyl chloride resin composition according to any one of Items 1 to 5, wherein the organotin stabilizer is a tin mercapto stabilizer.

[0019] Item 7. The vinyl chloride resin composition according to any one of Items 1 to 6, which is a vinyl chloride resin composition for injection molding.

[0020] Item 8. A vinyl chloride resin molded article, which is a molded article of the vinyl chloride resin composition according to any one of items 1 to 7. Effect of the Invention

[0021] The vinyl chloride resin composition according to the present invention includes a vinyl chloride resin, an organotin stabilizer, and particles of sodium salt of aliphatic carboxylic acid. In the vinyl chloride resin composition according to the present invention, the particles of the sodium salt of aliphatic carboxylic acid have a particle size distribution based on volume of 5 μm or more and 50 μm or less, and a particle size D90 of 85 μm or less, and a porosity of 65 or more and 90 or less. Since the vinyl chloride resin composition according to the present invention has the above-mentioned configuration, it is possible to increase the dispersibility of the particles of the sodium salt of aliphatic carboxylic acid and to increase the thermal stability during hot molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below.

[0023] (Vinyl chloride resin composition) The vinyl chloride resin composition according to the present invention includes a vinyl chloride resin, an organotin stabilizer, and particles of a sodium salt of an aliphatic carboxylic acid. In the vinyl chloride resin composition according to the present invention, the particles of the sodium salt of an aliphatic carboxylic acid have a particle size distribution on a volume basis in which the particle size D50 is 5 μm or more and 50 μm or less and the particle size D90 is 85 μm or less, and the porosity of the particles of the sodium salt of an aliphatic carboxylic acid is 65 or more and 90 or less.

[0024] The vinyl chloride resin composition using the conventional organotin stabilizer has a problem of insufficient thermal stability. In addition, hydrogen chloride may corrode the metal surface of a mold or the like, resulting in a problem of long-term production being difficult. Furthermore, depending on the amount of organotin stabilizer added, the heat resistance of the vinyl chloride resin composition may decrease.

[0025] In order to enhance the thermal stability of the vinyl chloride resin composition, it is considered to use an alkali metal salt of a fatty acid together with an organotin stabilizer. However, the melting point of the alkali metal salt of a fatty acid may be higher than the processing temperature range (up to about 200°C) of the vinyl chloride resin composition, and the alkali metal salt of a fatty acid may continue to exist as a solid during processing of the vinyl chloride resin composition. Furthermore, the particles of the alkali metal salt of a fatty acid are likely to form aggregates. Therefore, when obtaining a vinyl chloride resin composition, it is difficult to disperse the alkali metal salt of a fatty acid well in the vinyl chloride resin, and it is difficult to sufficiently enhance the thermal stability of the obtained vinyl chloride resin composition during heat molding.

[0026] In order to disperse the alkali metal salt of the fatty acid well in the vinyl chloride resin, it is considered to reduce the particle size of the alkali metal salt of the fatty acid. However, if the particle size of the alkali metal salt of the fatty acid is simply reduced, a plurality of particles will aggregate during storage of the alkali metal salt of the fatty acid, and the handling property will be reduced. For this reason, work to break down the aggregates may be required. In addition, when obtaining a vinyl chloride resin composition, it becomes difficult to weigh a predetermined amount of the alkali metal salt of the fatty acid, and the dispersibility of the particles of the alkali metal salt of the fatty acid in the vinyl chloride resin composition will also be reduced. Furthermore, the physical properties such as thermal stability during heat molding of the obtained vinyl chloride resin composition will vary, and the content of the alkali metal salt of the fatty acid will vary in the molded body obtained by molding the vinyl chloride resin composition.

[0027] Since the vinyl chloride resin composition according to the present invention has the above-mentioned configuration, it is possible to enhance the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid and to enhance the thermal stability during hot molding. Therefore, the physical properties such as the thermal stability during hot molding of the obtained vinyl chloride resin composition are unlikely to vary, and the content of the alkali metal salt of the fatty acid is unlikely to vary in the vinyl chloride resin molded article obtained by molding the vinyl chloride resin composition. As a result, the mechanical strength of the obtained molded article can be increased, and discoloration of the vinyl chloride resin molded article can be prevented.

[0028] In addition, the vinyl chloride resin composition according to the present invention can suppress corrosion of a metal surface. For example, it can suppress corrosion of the surface of a mold used for molding the vinyl chloride resin composition. As a result, vinyl chloride resin molded articles can be produced over a long period of time. Furthermore, when the vinyl chloride resin composition and the vinyl chloride resin molded article obtained are in contact with a metal, corrosion of the metal can be suppressed.

[0029] Furthermore, the vinyl chloride resin composition according to the present invention can improve the heat resistance of the molded article obtained. Since the vinyl chloride resin composition according to the present invention has the above-mentioned configuration, discoloration of the molded article obtained by molding the vinyl chloride resin composition according to the present invention can be suppressed even if the molded article is exposed to high temperatures.

[0030] The vinyl chloride resin composition is preferably used to obtain a vinyl chloride resin molded article. The vinyl chloride resin composition is preferably used to obtain an injection-molded vinyl chloride resin molded article. The vinyl chloride resin composition is preferably injection molded. The vinyl chloride resin composition is preferably a vinyl chloride resin composition for injection molding.

[0031] Hereinafter, each component contained in the vinyl chloride resin composition will be described.

[0032] <Vinyl chloride resin> The vinyl chloride resin has a chlorine atom. The vinyl chloride resin may be a chlorinated vinyl chloride resin or a non-chlorinated vinyl chloride resin. From the viewpoint of improving heat resistance, the vinyl chloride resin is preferably a chlorinated vinyl chloride resin. The chlorinated vinyl chloride resin is a resin obtained by chlorinating a vinyl chloride resin. The vinyl chloride resin may be used alone or in combination of two or more kinds.

[0033] Examples of the vinyl chloride resin include a homopolymer of a vinyl chloride monomer, and a copolymer of a vinyl chloride monomer and a vinyl monomer copolymerizable with the vinyl chloride monomer.

[0034] Examples of vinyl monomers copolymerizable with the vinyl chloride monomer include vinyl esters such as vinyl acetate, vinyl propionate, and vinyl ether; cyano group-containing compounds such as acrylonitrile; halogen compounds such as vinylidene chloride and vinyl fluoride; olefins such as ethylene and propylene; carboxyl group-containing compounds such as itaconic acid, maleic acid, and fumaric acid; non-aromatic carboxylic acid anhydrides such as maleic anhydride; acrylic acid esters such as methyl methacrylate and ethyl methacrylate; and imide compounds such as maleimide. Only one type of the vinyl monomer may be used, or two or more types may be used in combination.

[0035] The polymerization method of the vinyl chloride monomer or the polymerization method of the vinyl chloride monomer and the vinyl monomer is not particularly limited. The polymerization method includes suspension polymerization, emulsion polymerization, solution polymerization, bulk polymerization, and precipitation polymerization. From the viewpoint of efficiently obtaining the vinyl chloride resin, the polymerization method is preferably suspension polymerization, emulsion polymerization, solution polymerization, or precipitation polymerization.

[0036] The chlorinated vinyl chloride resin is preferably obtained by polymerizing the vinyl chloride monomer or the vinyl chloride monomer and the vinyl monomer to obtain a vinyl chloride resin, and then chlorinating the vinyl chloride resin.

[0037] The method of chlorinating the vinyl chloride resin is not particularly limited. The method of chlorinating the vinyl chloride resin includes a method of putting the vinyl chloride resin into an aqueous solvent to obtain a suspension, and then adding chlorine to react the vinyl chloride resin with chlorine. This chlorination reaction proceeds under heating conditions or light irradiation conditions.

[0038] From the viewpoint of enhancing the thermal stability of the resulting chlorinated vinyl chloride resin, the chlorination reaction is preferably carried out under heating conditions.

[0039] From the viewpoint of increasing the efficiency of the chlorination reaction, the temperature during the heating is preferably 80°C or higher and preferably 140°C or lower.

[0040] The chlorine content of the vinyl chloride resin is preferably 56.8% by weight or more, preferably 72% by weight or less. The chlorine content of the vinyl chloride resin is the content of chlorine atoms in 100% by weight of the vinyl chloride resin. When the chlorine content of the vinyl chloride resin is equal to or more than the lower limit, the heat resistance of the obtained molded article can be further improved. When the chlorine content of the vinyl chloride resin is equal to or less than the upper limit, the moldability can be improved, and the impact resistance and surface smoothness of the obtained molded article can be improved.

[0041] When the vinyl chloride resin is a chlorinated vinyl chloride resin, the chlorine content of the chlorinated vinyl chloride resin is preferably 56.8% by weight or more, more preferably 60% by weight or more, even more preferably 61.5% by weight or more, and preferably 72% by weight or less, more preferably 67.5% by weight or less. When the chlorine content of the chlorinated vinyl chloride resin is equal to or more than the lower limit, the heat resistance of the obtained molded article can be further improved. When the chlorine content of the chlorinated vinyl chloride resin is equal to or less than the upper limit, the moldability can be improved, and the impact resistance and surface smoothness of the obtained molded article can be improved.

[0042] The chlorine content of the vinyl chloride resin (when the vinyl chloride resin is a chlorinated vinyl chloride resin, the chlorine content of the chlorinated vinyl chloride resin) can be determined by potentiometric titration in accordance with JIS K7229.

[0043] The degree of polymerization of the vinyl chloride resin is preferably 500 or more, more preferably 600 or more, and preferably 2000 or less, more preferably 1200 or less. When the degree of polymerization is equal to or more than the lower limit, the mechanical strength of the molded article can be increased. When the degree of polymerization is equal to or less than the upper limit, it is not necessary to raise the temperature during molding, and moldability can be improved.

[0044] In 100% by weight of the vinyl chloride resin composition, the content of the vinyl chloride resin is preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 85% by weight or more, particularly preferably 90% by weight or more, most preferably 92% by weight or more, and preferably 99.8% by weight or less, more preferably 99% by weight or less, even more preferably 98.5% by weight or less, particularly preferably 98% by weight or less, most preferably 97% by weight or less. When the content of the vinyl chloride resin is equal to or more than the lower limit, the adhesive strength and mechanical strength of the obtained molded article can be increased. When the content of the vinyl chloride resin is equal to or less than the upper limit, it is not necessary to raise the temperature during molding, and moldability can be improved.

[0045] The vinyl chloride resin contained in the vinyl chloride resin composition is preferably in the form of particles. In the particle size distribution of the vinyl chloride resin particles on a volume basis, the particle size D50 is preferably 0.1 μm or more and preferably 500 μm or less. When the particle size D50 of the vinyl chloride resin particles is the lower limit or more, the handling property can be improved. When the particle size D50 of the vinyl chloride resin particles is the upper limit or less, the moldability can be improved.

[0046] The particle size D50 of the vinyl chloride resin particles is the average diameter measured on a volume basis, and is the value of the median diameter (D50) at 50%. The particle size D50 of the vinyl chloride resin particles can be measured by a laser diffraction / scattering method or the like. The particle size D50 of the vinyl chloride resin particles is the value of the diameter equivalent to 50% of the particle size distribution on a volume basis, calculated from the small particle size side. A laser diffraction particle size distribution measuring device is preferably used as a measuring device. Commercially available products of the laser diffraction particle size distribution measuring device include "HELOS-KR" manufactured by Nippon Laser Co., Ltd. When "HELOS-KR" manufactured by Nippon Laser Co., Ltd. is used, the measurement can be performed at a dispersion pressure of 3.0 bar.

[0047] <Organotin stabilizer> The vinyl chloride resin composition contains an organotin stabilizer that inhibits decomposition of the vinyl chloride resin and captures hydrogen chloride generated during decomposition of the vinyl chloride resin.

[0048] The organotin stabilizer is preferably an organotin heat stabilizer.

[0049] Examples of the organic tin stabilizer include tin mercapto stabilizers, tin malate stabilizers, and tin carboxylate stabilizers. Examples of the tin mercapto stabilizers include monoalkyltin mercapto, dialkyltin mercapto, monoalkyltin mercapto polymer, dialkyltin mercapto polymer, monoalkyltin mercapto sulfide, and dialkyltin mercapto sulfide. Examples of the tin malate stabilizers include monoalkyltin malate, dialkyltin malate, monoalkyltin malate polymer, and dialkyltin malate polymer. Examples of the tin carboxylate stabilizers include monoalkyltin carboxylate and dialkyltin carboxylate. The organic tin stabilizers may be used alone or in combination of two or more.

[0050] From the viewpoints of further improving the thermal stability during hot molding, preventing initial coloration of the resulting molded body, and further enhancing the heat resistance of the molded body, the above-mentioned organotin stabilizer is preferably a tin mercapto stabilizer, more preferably a dialkyltin mercapto, and even more preferably dioctyltin mercapto.

[0051] In 100% by weight of the vinyl chloride resin composition, the content of the organotin stabilizer is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 0.5% by weight or more, particularly preferably 0.8% by weight or more, and most preferably 1.0% by weight or more, and is preferably 5.0% by weight or less, more preferably 2.5% by weight or less, even more preferably 2.4% by weight or less, particularly preferably 2.2% by weight or less, and most preferably 2.0% by weight or less. When the content of the organotin stabilizer is equal to or more than the lower limit and equal to or less than the upper limit, the thermal stability during hot molding can be more effectively improved, and the heat resistance of the obtained molded body can be further improved.

[0052] The content of the organotin stabilizer relative to 100 parts by weight of the vinyl chloride resin in the vinyl chloride resin composition is preferably 0.1 parts by weight or more, more preferably 0.5 parts by weight or more, even more preferably 0.8 parts by weight or more, particularly preferably 1.0 parts by weight or more, and is preferably 3.0 parts by weight or less, more preferably 2.4 parts by weight or less, even more preferably 2.2 parts by weight or less, particularly preferably 2.0 parts by weight or less. When the content of the organotin stabilizer is equal to or more than the lower limit and equal to or less than the upper limit, the thermal stability during hot molding can be more effectively improved, and the heat resistance of the obtained molded article can be more effectively improved.

[0053] The vinyl chloride resin composition may contain a stabilizer other than the organotin stabilizer. Examples of the stabilizer other than the organotin stabilizer include lead stabilizers, calcium-zinc stabilizers, barium-zinc stabilizers, and barium-cadmium stabilizers. Examples of the lead stabilizers include tribasic lead sulfate, tetrabasic lead sulfate, basic lead sulfite, dibasic lead phosphite, dibasic lead phthalate, tribasic lead maleate, dibasic lead stearate, and basic sulfite and phosphite.

[0054] <Particles of sodium salt of aliphatic carboxylic acid> The vinyl chloride resin composition includes particles of sodium salt of aliphatic carboxylic acid. The material of the particles of sodium salt of aliphatic carboxylic acid is sodium salt of aliphatic carboxylic acid. The sodium salt of aliphatic carboxylic acid includes sodium. Specifically, the sodium salt of aliphatic carboxylic acid includes at least one sodium. The aliphatic carboxylic acid in the sodium salt of aliphatic carboxylic acid may be a monocarboxylic acid or a polycarboxylic acid. The polycarboxylic acid may be a dicarboxylic acid.

[0055] The sodium salt of the aliphatic carboxylic acid neutralizes hydrogen chloride generated during decomposition of vinyl chloride resin with sodium, thereby suppressing corrosion of metal surfaces of dies and the like caused by hydrogen chloride, thereby enabling the long-term production of vinyl chloride resin molded articles.

[0056] Examples of the sodium salts of the aliphatic carboxylic acids include disodium adipate, disodium sebacate, disodium azelaate, disodium suberate, and disodium pimelate, etc. The sodium salts of the aliphatic carboxylic acids may be used alone or in combination of two or more.

[0057] From the viewpoint of more effectively suppressing corrosion of the metal surface, the number of sodium atoms in the sodium salt of the aliphatic carboxylic acid is preferably two or more, and more preferably 2. The number of sodium atoms in the sodium salt of the aliphatic carboxylic acid may be 5 or less, 4 or less, or 3 or less.

[0058] From the viewpoint of further increasing the thermal stability during hot molding and further increasing the heat resistance of the obtained molded body, the number of carbon atoms in the sodium salt of the aliphatic carboxylic acid is preferably 4 or more, more preferably 5 or more, even more preferably 6 or more, and is preferably 16 or less, more preferably 12 or less, even more preferably 8 or less.

[0059] From the viewpoints of further increasing the dispersibility of the particles of the sodium salt of aliphatic carboxylic acid, further increasing the thermal stability during heat molding, and further increasing the heat resistance of the obtained molded body, it is preferable that the number of COONa groups in the sodium salt of aliphatic carboxylic acid is 2 and the number of carbon atoms in the sodium salt of aliphatic carboxylic acid is 6 or more and 16 or less. From the viewpoints of further increasing the dispersibility of the particles of the sodium salt of aliphatic carboxylic acid, further increasing the thermal stability during heat molding, and further increasing the heat resistance of the obtained molded body, it is preferable that the sodium salt of aliphatic carboxylic acid has a chain hydrocarbon skeleton having a carbon number of 2 or more and 14 or less.

[0060] Examples of the sodium salt of an aliphatic carboxylic acid having the above-mentioned preferred embodiment include disodium adipate, disodium sebacate, disodium azelaate, disodium suberate, and disodium pimelate, etc. From the viewpoint of more effectively suppressing corrosion of the metal surface, more effectively increasing the thermal stability during hot molding, and more effectively increasing the heat resistance of the obtained molded body, it is particularly preferable that the sodium salt of the aliphatic carboxylic acid is disodium adipate, and it is particularly preferable that the particles of the sodium salt of the aliphatic carboxylic acid are particles of disodium adipate.

[0061] In the particle size distribution based on volume of the particles of the sodium salt of the aliphatic carboxylic acid, the particle size D50 is 5 μm or more and 50 μm or less. Since the particle size D50 of the particles of the sodium salt of the aliphatic carboxylic acid is equal to or more than the lower limit and equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is improved, the thermal stability during heat molding is improved, and the heat resistance of the obtained molded body can be further improved.

[0062] The particle diameter D50 of the particles of the sodium salt of the aliphatic carboxylic acid is preferably 10 μm or more, more preferably 12 μm or more, even more preferably 15 μm or more, particularly preferably 18 μm or more, and is preferably 45 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less. When the particle diameter D50 of the particles of the sodium salt of the aliphatic carboxylic acid is equal to or more than the lower limit and equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is further improved, and the thermal stability during hot molding is further improved, and the heat resistance of the obtained molded body is further improved.

[0063] In the particle size distribution based on volume of the particles of the sodium salt of the aliphatic carboxylic acid, the particle size D90 is 85 μm or less. Since the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid is equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is improved, the thermal stability during hot molding is improved, and the heat resistance of the obtained molded body can be further improved.

[0064] The particle diameter D90 of the particles of the sodium salt of the aliphatic carboxylic acid is preferably 80 μm or less, more preferably 75 μm or less, and even more preferably 70 μm or less. When the particle diameter D90 of the particles of the sodium salt of the aliphatic carboxylic acid is equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is further improved, the thermal stability during heat molding is further improved, and the heat resistance of the obtained molded body is further improved. The particle diameter D90 of the particles of the sodium salt of the aliphatic carboxylic acid is the same as or larger than the particle diameter D50 of the particles of the sodium salt of the aliphatic carboxylic acid.

[0065] The particle size D50 and the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid are average diameters measured on a volume basis, and are the 50% median diameter (D50) and the 90% median diameter (D90). The particle size D50 and the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid can be measured by a laser diffraction / scattering method or the like. That is, the particle size D50 and the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid are the diameter values ​​corresponding to 50% and 90% of the particle size distribution on a volume basis, calculated from the smaller particle size side. A laser diffraction particle size distribution measuring device is preferably used as the measuring device. Commercially available products of the laser diffraction particle size distribution measuring device include "HELOS-KR" manufactured by Nippon Laser Co., Ltd. When "HELOS-KR" manufactured by Nippon Laser Co., Ltd. is used, the measurement can be performed at a dispersion pressure of 3.0 bar.

[0066] The particles of the sodium salt of the aliphatic carboxylic acid can be obtained, for example, by subjecting an aqueous solution containing the sodium salt of the aliphatic carboxylic acid to hot air drying or fluidized bed drying. The method for obtaining the particles of the sodium salt of the aliphatic carboxylic acid is not limited to the above-mentioned method.

[0067] The particle size D50 and the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid can be controlled, for example, by sorting the particles using a sieve. The particle size D50 and the particle size D90 of the particles of the sodium salt of the aliphatic carboxylic acid can be controlled by the following methods, etc. A method of controlling the temperature of hot air when drying an aqueous solution containing the sodium salt of the aliphatic carboxylic acid with hot air to obtain the particles of the sodium salt of the aliphatic carboxylic acid. A method of controlling the volume of hot air when drying an aqueous solution containing the sodium salt of the aliphatic carboxylic acid with hot air to obtain the particles of the sodium salt of the aliphatic carboxylic acid.

[0068] The porosity of the particles of the sodium salt of an aliphatic carboxylic acid is from 65 to 90. Since the porosity of the sodium salt of an aliphatic carboxylic acid is equal to or more than the lower limit and equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of an aliphatic carboxylic acid is improved, the thermal stability during hot molding is improved, and the heat resistance of the obtained molded body can be further improved.

[0069] The porosity of the particles of the sodium salt of aliphatic carboxylic acid is preferably at least 67, more preferably at least 70, even more preferably at least 72, and is preferably at most 88, more preferably at most 86, even more preferably at most 85. When the porosity of the particles of the sodium salt of aliphatic carboxylic acid is at least the above lower limit and is at most the above upper limit, the dispersibility of the particles of the sodium salt of aliphatic carboxylic acid is further improved, the thermal stability during hot molding is further improved, and the heat resistance of the obtained molded body is further improved.

[0070] The porosity of the particles of the sodium salt of an aliphatic carboxylic acid can be measured as follows.

[0071] Method: Mercury porosimetry Equipment: Micromeritics Autopore V 9620 pore size distribution analyzer Procedure: After placing 0.10g of sample in a 5cc powder cell, evacuate the cell and fill it with mercury. Next, pressurize the cell at a pressure range of 4kPa to 1,200,000kPa, and measure the amount of mercury that penetrates into the pores of the sample.

[0072] The porosity of the particles of the sodium salt of an aliphatic carboxylic acid can be controlled by the following methods, etc.: A method of controlling the temperature of hot air when drying an aqueous solution containing the sodium salt of an aliphatic carboxylic acid with hot air to obtain the particles of the sodium salt of an aliphatic carboxylic acid; A method of controlling the volume of hot air when drying an aqueous solution containing the sodium salt of an aliphatic carboxylic acid with hot air to obtain the particles of the sodium salt of an aliphatic carboxylic acid.

[0073] The aspect ratio of the particles of the sodium salt of the aliphatic carboxylic acid is preferably 1.00 or more, more preferably 1.02 or more, even more preferably 1.04 or more, particularly preferably 1.06 or more, and is preferably 1.8 or less, more preferably 1.7 or less, even more preferably 1.6 or less, particularly preferably 1.5 or less. When the aspect ratio of the particles of the sodium salt of the aliphatic carboxylic acid is equal to or more than the lower limit and equal to or less than the upper limit, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is further improved, the thermal stability during hot molding is further improved, and the heat resistance of the obtained molded body is further improved.

[0074] The aspect ratio is the value of major axis / minor axis. The aspect ratio of the particles of the sodium salt of an aliphatic carboxylic acid is determined by averaging the major axis / minor axis values ​​of a plurality of particles of the sodium salt of an aliphatic carboxylic acid.

[0075] The aspect ratio of the particles of the sodium salt of an aliphatic carboxylic acid can be controlled by the following methods, etc.: A method of controlling the temperature of hot air when drying the aqueous solution containing the sodium salt of an aliphatic carboxylic acid with hot air, and A method of controlling the volume of hot air when drying the aqueous solution containing the sodium salt of an aliphatic carboxylic acid with hot air to obtain the particles of the sodium salt of an aliphatic carboxylic acid.

[0076] In 100% by weight of the vinyl chloride resin composition, the content of the particles of the sodium salt of the aliphatic carboxylic acid is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 0.3% by weight or more, particularly preferably 0.7% by weight or more, most preferably 1.0% by weight or more, and preferably 3.0% by weight or less, more preferably 2.0% by weight or less, even more preferably 1.8% by weight or less, particularly preferably 1.6% by weight or less, most preferably 1.5% by weight or less. When the content of the particles of the sodium salt of the aliphatic carboxylic acid is the above lower limit or more and the above upper limit or less, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is further increased, the thermal stability during hot molding is further increased, and the heat resistance of the obtained molded body is further increased. Furthermore, the corrosion of the metal surface is more effectively suppressed.

[0077] The content of the particles of the sodium salt of the aliphatic carboxylic acid is preferably 0.1 parts by weight or more, more preferably 0.3 parts by weight or more, even more preferably 0.7 parts by weight or more, particularly preferably 1.0 parts by weight or more, and preferably 3.0 parts by weight or less, more preferably 2.8 parts by weight or less, even more preferably 1.8 parts by weight or less, particularly preferably 1.6 parts by weight or less, and most preferably 1.5 parts by weight or less, relative to 100 parts by weight of the vinyl chloride resin in the vinyl chloride resin composition. When the content of the particles of the sodium salt of the aliphatic carboxylic acid is the above lower limit or more and the above upper limit or less, the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid is further increased, the thermal stability during hot molding is further increased, and the heat resistance of the obtained molded body is further increased. Furthermore, the corrosion of the metal surface is more effectively suppressed.

[0078] In 100% by weight of the vinyl chloride resin composition, the sodium content is preferably 0.08% by weight or more, more preferably 0.10% by weight or more, even more preferably 0.15% by weight or more, particularly preferably 0.20% by weight or more, and preferably 0.50% by weight or less, more preferably 0.45% by weight or less, even more preferably 0.40% by weight or less, particularly preferably 0.35% by weight or less. When the sodium content is equal to or more than the lower limit and equal to or less than the upper limit, the corrosion of the metal surface can be more effectively suppressed. In addition, the sodium content in the vinyl chloride resin composition can be measured using ICP emission spectrometry, ICP mass spectrometry, fluorescent X-ray spectrometry, etc.

[0079] The vinyl chloride resin composition may contain a compound containing sodium (hereinafter sometimes referred to as compound (A)) other than the particles of the sodium salt of the aliphatic carboxylic acid, or particles of the compound (A). In the vinyl chloride resin composition, the compound (A) or particles of the compound (A) may contain sodium.

[0080] Case (1) refers to the case where the sodium contained in the vinyl chloride resin composition is only sodium derived from the sodium salt of the aliphatic carboxylic acid. In case (1), the content of sodium in 100% by weight of the vinyl chloride resin composition indicates the content of sodium derived from the sodium salt of the aliphatic carboxylic acid. Case (2) refers to the case where the sodium contained in the vinyl chloride resin composition is both sodium derived from the sodium salt of the aliphatic carboxylic acid and sodium derived from the compound (A). In case (2), the content of sodium in 100% by weight of the vinyl chloride resin composition indicates the sum of the content of sodium derived from the sodium salt of the aliphatic carboxylic acid and the content of sodium derived from the compound (A).

[0081] <Inorganic filler> The vinyl chloride resin composition does not contain an inorganic filler or contains an inorganic filler. The vinyl chloride resin composition may not contain an inorganic filler or may contain an inorganic filler.

[0082] Examples of the inorganic filler include calcium carbonate, silica, talc, titanium oxide, zinc oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, clay, mica, wollastonite, zeolite, carbon black, graphite, glass beads, glass fibers, hydrocarbons, and metal fibers. From the viewpoint of improving the appearance of the vinyl chloride resin composition and the resulting molded article and increasing the mechanical strength of the resulting molded article, the inorganic filler is preferably calcium carbonate. Only one type of the inorganic filler may be used, or two or more types may be used in combination.

[0083] The inorganic filler is preferably an inorganic particle. The aspect ratio of the inorganic filler is preferably 2.0 or less, more preferably 1.5 or less, and further preferably 1.2 or less.

[0084] The aspect ratio is the value of major axis / minor axis, and is determined by averaging the major axis / minor axis values ​​of a plurality of the inorganic fillers.

[0085] When the vinyl chloride resin composition contains the inorganic filler, the content of the inorganic filler in 100% by weight of the vinyl chloride resin composition is preferably 2% by weight or more, more preferably 4% by weight or more, and preferably 30% by weight or less, more preferably 20% by weight or less, and even more preferably 15% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit, the mechanical strength of the obtained molded article can be increased. When the content of the inorganic filler is equal to or less than the upper limit, the appearance of the vinyl chloride resin composition and the obtained molded article can be improved. The content of the inorganic filler may be 0% by weight (unused). It is particularly preferable that the vinyl chloride resin composition does not contain an inorganic filler or contains 15% by weight or less of an inorganic filler in 100% by weight of the vinyl chloride resin composition.

[0086] The content of the inorganic filler is preferably 2 parts by weight or more, more preferably 4 parts by weight or more, and preferably 30 parts by weight or less, more preferably 20 parts by weight or less, and even more preferably 15 parts by weight or less, relative to 100 parts by weight of the vinyl chloride resin in the vinyl chloride resin composition. When the content of the inorganic filler is equal to or more than the lower limit, the mechanical strength of the obtained molded article can be increased. When the content of the inorganic filler is equal to or less than the upper limit, the appearance of the vinyl chloride resin composition and the obtained molded article can be improved. The content of the inorganic filler may be 0 parts by weight (unused).

[0087] In the particle size distribution of the inorganic filler on a volume basis, the particle size D50 is preferably 10 nm or more and preferably 3 μm or less. When the particle size D50 of the inorganic filler is equal to or more than the lower limit, the handling property can be improved. When the particle size D50 of the inorganic filler is equal to or less than the upper limit, the moldability can be improved.

[0088] The particle size D50 of the inorganic filler is the average diameter measured on a volume basis, and is the value of the median diameter (D50) at 50%. The particle size D50 of the inorganic filler can be measured by a laser diffraction / scattering method or the like. The particle size D50 of the inorganic filler is the value of the diameter equivalent to 50% of the particle size distribution on a volume basis, calculated from the small particle size side. A laser diffraction type particle size distribution measuring device is preferably used as a measuring device. Commercially available products of the laser diffraction type particle size distribution measuring device include "HELOS-KR" manufactured by Nippon Laser Corporation. When "HELOS-KR" manufactured by Nippon Laser Corporation is used, the measurement can be performed at a dispersion pressure of 3.0 bar.

[0089] <Other ingredients> The vinyl chloride resin composition may contain various additives as necessary. Examples of the additives include heat stabilizing aids, lubricants, processing aids, impact modifiers, heat resistance improvers, antioxidants, ultraviolet absorbers, antistatic agents, light stabilizers, fillers other than inorganic fillers, pigments, flame retardants, and plasticizers. The additives may be used alone or in combination of two or more.

[0090] The heat stabilization assistant is not particularly limited, and examples thereof include epoxidized soybean oil, phosphoric acid ester, polyol, hydrotalcite, zeolite, etc. The heat stabilization assistant may be used alone or in combination of two or more kinds.

[0091] The lubricant includes an internal lubricant and an external lubricant. The internal lubricant is used to reduce the flow viscosity of the molten resin during molding and to prevent frictional heat generation. The internal lubricant is not particularly limited, and examples thereof include butyl stearate, lauryl alcohol, stearyl alcohol, epoxy soybean oil, glycerin monostearate, stearic acid, and bisamide. The external lubricant is used to increase the sliding effect between the molten resin and the metal surface during molding. The external lubricant is not particularly limited, and examples thereof include paraffin wax, polyolefin wax, ester wax, and montanic acid wax. The lubricant may be used alone or in combination of two or more.

[0092] The processing aid is not particularly limited, and examples thereof include acrylic processing aids. Examples of the acrylic processing aids include alkyl acrylate-alkyl methacrylate copolymers having a weight average molecular weight of 100,000 to 2,000,000, and specific examples thereof include n-butyl acrylate-methyl methacrylate copolymers and 2-ethylhexyl acrylate-methyl methacrylate-butyl methacrylate copolymers. The processing aids may be used alone or in combination of two or more.

[0093] The impact modifier is not particularly limited, and examples thereof include methyl methacrylate-butadiene-styrene copolymer (MBS), chlorinated polyethylene, acrylic rubber, etc. The impact modifier may be used alone or in combination of two or more kinds.

[0094] The heat resistance improver is not particularly limited, and examples thereof include α-methylstyrene-based and N-phenylmaleimide-based resins, etc. The heat resistance improver may be used alone or in combination of two or more kinds.

[0095] The antioxidant is not particularly limited, and examples thereof include phenol-based antioxidants, etc. The antioxidants may be used alone or in combination of two or more kinds.

[0096] The ultraviolet absorbing agent is not particularly limited, and examples thereof include salicylic acid ester ultraviolet absorbing agents, benzophenone ultraviolet absorbing agents, benzotriazole ultraviolet absorbing agents, and cyanoacrylate ultraviolet absorbing agents, etc. The ultraviolet absorbing agents may be used alone or in combination of two or more kinds.

[0097] The light stabilizer is not particularly limited, and examples thereof include hindered amine light stabilizers, etc. The light stabilizers may be used alone or in combination of two or more kinds.

[0098] The pigment is not particularly limited, and examples thereof include organic pigments and inorganic pigments. Examples of the organic pigments include azo-based organic pigments, phthalocyanine-based organic pigments, threne-based organic pigments, and dye lake-based organic pigments. Examples of the inorganic pigments include oxide-based inorganic pigments, molybdenum chromate-based inorganic pigments, sulfide-selenide-based inorganic pigments, and ferrocyanide-based inorganic pigments. From the viewpoint of further increasing transparency, it is preferable that the vinyl chloride resin composition does not contain the above pigments.

[0099] The plasticizer may be added to improve the processability during molding. The addition of a plasticizer may reduce the heat resistance of the molded product, so it is preferable to add a small amount of plasticizer. The plasticizer is not particularly limited, and examples thereof include dibutyl phthalate, di-2-ethylhexyl phthalate, and di-2-ethylhexyl adipate. The plasticizer may be used alone or in combination of two or more.

[0100] (Vinyl chloride resin molding) The vinyl chloride resin molded article is formed using the vinyl chloride resin composition. The vinyl chloride resin composition can be used to obtain the vinyl chloride resin molded article. The vinyl chloride resin molded article is obtained by molding the vinyl chloride resin composition. The vinyl chloride resin molded article is a molded article of the vinyl chloride resin composition.

[0101] The vinyl chloride resin molded article is not particularly limited, and examples thereof include pipes, plates, containers, etc. The vinyl chloride resin molded article is preferably in the form of a plate, and more preferably in the form of a flat plate. The plate-like shape includes a sheet-like shape and a film-like shape.

[0102] The molding method of the vinyl chloride resin composition is not particularly limited, and examples thereof include extrusion molding, injection molding, calendar molding, press molding, etc. From the viewpoint of more effectively suppressing corrosion of the metal surface, the molding method of the vinyl chloride resin composition is preferably an injection molding method with a long residence time.

[0103] The vinyl chloride resin molded article is preferably an injection molded article.

[0104] The molding machine used for molding is not particularly limited, and examples thereof include a single screw extruder, a twin screw counter-rotating parallel extruder, a twin screw counter-rotating conical extruder, a twin screw co-rotating extruder, a plunger type injection molding machine, a pre-plunger type injection molding machine, and a screw type injection molding machine. When molding is performed using the above molding machine, the mold for forming, the resin temperature, etc. are not particularly limited.

[0105] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0106] The following materials were prepared:

[0107] (Vinyl chloride resin) Polyvinyl chloride resin (Tokuyama Sekisui Kogyo Co., Ltd. "TS-800E", chlorine content 56.8% by weight, polymerization degree 800)

[0108] (Organotin stabilizer) Dioctyltin mercapto stabilizer ("STANN ONZ-7F" manufactured by Nitto Kasei Kogyo Co., Ltd.)

[0109] (Particles of sodium salts of aliphatic carboxylic acids) <Type A> Disodium adipate, particle size D50: 12.2 μm, particle size D90: 37 μm, porosity: 79, aspect ratio: 1.2 <Type B> Disodium adipate, particle size D50: 21.0 μm, particle size D90: 39 μm, porosity: 82, aspect ratio: 1.1 <Type C> Disodium adipate, particle size D50: 27.1 μm, particle size D90: 65 μm, porosity: 80, aspect ratio: 1.3 <Type D> Disodium adipate, particle size D50: 9.1 μm, particle size D90: 94 μm, porosity: 59, aspect ratio: 2.1 <Type E> Disodium adipate, particle size D50: 1.5 μm, particle size D90: 4.2 μm, porosity: 59, aspect ratio: 2.6

[0110] (lubricant) <Type W1> Polymer composite ester wax (Emery Oleochemicals "LOXIOL VPN963") <Type W2> High density oxidized polyethylene wax (Honeywell "AC-316A")

[0111] (Examples 1 to 3, and Comparative Examples 1 and 2) The types and amounts of the ingredients shown in Table 1 below were added to a Henschel mixer (Kawada Kogyo Co., Ltd.) and mixed for 5 minutes to obtain a vinyl chloride resin composition.

[0112] (evaluation) (1) Disintegration of aggregates of particles of sodium salts of aliphatic carboxylic acids A weight equivalent to 200 mL of the particles of the sodium salt of aliphatic carboxylic acid was placed in a 300 mL beaker, and a 6.1 kg weight was placed directly on the particles of the sodium salt of aliphatic carboxylic acid to prepare a test specimen. The test specimen was placed in an oven ("DRK632DC" manufactured by ADVANTEC) and left to stand at 50°C for 30 days. After 30 days, the test specimen was removed and allowed to cool to room temperature (23°C), and then an aggregate of the particles of the sodium salt of aliphatic carboxylic acid (hereinafter sometimes referred to as "aggregate") was removed. A weight was placed on the aggregate, and the weight of the weight required for the aggregate to disintegrate was measured. The disintegrability of the aggregate of the particles of the sodium salt of aliphatic carboxylic acid was evaluated according to the following criteria.

[0113] In addition, when the weight of the weight required to break down the aggregates is 3.0 kg or more, the aggregates tend to remain when the particles of the sodium salt of the aliphatic carboxylic acid are used, and the dispersibility of the particles of the sodium salt of the aliphatic carboxylic acid in the vinyl chloride resin composition becomes poor. Therefore, when the weight of the weight required to break down the aggregates is 3.0 kg or more, the following evaluation items (2), (3), and (4) were not performed.

[0114] <Criteria for determining disintegrability of aggregates of particles of sodium salts of aliphatic carboxylic acids> ○: The weight of the weight required to break up the aggregates is less than 3.0 kg ×: The weight of the weight required to break up the aggregates is 3.0 kg or more.

[0115] (2) Dispersibility of particles of sodium salts of aliphatic carboxylic acids The obtained vinyl chloride resin composition was kneaded under the following kneading conditions to obtain a sheet having a thickness of 1 mm.

[0116] [Mixing conditions] Roll: Yasuda Seiki Seisakusho mixing roll Roll temperature: 190℃ Roll time: 3 minutes (after wrapping)

[0117] A plurality of the obtained sheets having a thickness of 1 mm were stacked and pressed under the following pressing conditions to obtain a pressed sheet having a thickness of 3 mm.

[0118] [Press conditions] Press machine: Kodaira Manufacturing hydraulic press machine Temperature: 190℃ Press time: 2 minutes Cooling time: 3 minutes

[0119] The cross section of the obtained press sheet was microtomed and then observed with a SEM (Hitachi High-Tech Corporation "SU-3500"). The obtained SEM image was processed to calculate the average area of ​​the agglomerates of the sodium salt of aliphatic carboxylic acid particles present in an area of ​​1.3 mm length x 1.0 mm width. The dispersibility of the sodium salt of aliphatic carboxylic acid particles was evaluated according to the following criteria.

[0120] <Criteria for determining dispersibility of particles of sodium salt of aliphatic carboxylic acid> ○: The average area of ​​the aggregates is 40 μm 2 less than ×: The average area of ​​the aggregates is 40 μm 2 End

[0121] (3) Thermal stability of vinyl chloride resin compositions 70 g of the obtained vinyl chloride resin composition was placed in a plastomill ("Labo Plastomill 4C150" manufactured by Toyo Seiki Seisakusho) and kneaded under the following kneading conditions.

[0122] [Mixing conditions] Plastomill (Toyo Seiki "Labo Plastomill 4C150") Temperature: 210℃ Screw rotation speed: 50 rpm Preheat time: 2 minutes

[0123] The time when the torque during kneading increased by 20% from the steady torque was determined as the decomposition time. The thermal stability of the vinyl chloride resin composition was evaluated according to the following criteria.

[0124] <Criteria for determining thermal stability of vinyl chloride resin compositions> 〇: Decomposition time is 20 minutes or more ×: Decomposition time is less than 20 minutes

[0125] (4) Thermal stability of polyvinyl chloride resin molded products The obtained vinyl chloride resin composition was injection molded to obtain a cylindrical molded body (vinyl chloride resin molded body, socket with a diameter of 25 A). The thermal stability of the obtained molded body (socket with a diameter of 25 A) was evaluated.

[0126] [Molding conditions] The molded body (socket with a diameter of 25A) was obtained by injection molding using a conventional molding method.

[0127] [Method for evaluating thermal stability] The obtained molded body (25A socket) was placed in an oven (ADVANTEC Corp. "DRK632DC") and the temperature was set to 210°C. Every 10 minutes, the molded body was taken out and the brown discoloration time (the time it took for the molded body to turn brown) was determined. For example, if the molded body had not turned brown after 40 minutes and had turned brown after 50 minutes, the brown discoloration time was 50 minutes. The thermal stability of the vinyl chloride resin molded body was judged according to the following criteria.

[0128] <Criteria for determining the thermal stability of vinyl chloride resin molded products> ○: Brown discoloration time is 50 minutes or more ×: Browning time is 40 minutes or less

[0129] The types and amounts of the ingredients and the evaluation results are shown in Table 1 below.

[0130] [Table 1]

Claims

1. The present invention relates to a polyvinyl chloride resin, an organotin stabilizer, and particles of a sodium salt of an aliphatic carboxylic acid, In a particle size distribution on a volume basis of the particles of the sodium salt of the aliphatic carboxylic acid, a particle size D50 is 5 μm or more and 50 μm or less, and a particle size D90 is 85 μm or less, The polyvinyl chloride resin composition, wherein the porosity of the particles of the sodium salt of the aliphatic carboxylic acid is 65 or more and 90 or less.

2. 2. The vinyl chloride resin composition according to claim 1, wherein the content of the particles of the sodium salt of an aliphatic carboxylic acid is 0.1 parts by weight or more and 3.0 parts by weight or less based on 100 parts by weight of the vinyl chloride resin.

3. 3. The vinyl chloride resin composition according to claim 1, wherein the aspect ratio of the particles of the sodium salt of an aliphatic carboxylic acid is 1.00 or more and 1.8 or less.

4. 3. The vinyl chloride resin composition according to claim 1, wherein the particles of the sodium salt of an aliphatic carboxylic acid are particles of disodium adipate.

5. 3. The vinyl chloride resin composition according to claim 1, wherein the content of the organotin stabilizer is 0.1 parts by weight or more and 3.0 parts by weight or less based on 100 parts by weight of the vinyl chloride resin.

6. 3. The vinyl chloride resin composition according to claim 1, wherein the organotin stabilizer is a tin mercapto stabilizer.

7. 3. The vinyl chloride resin composition according to claim 1, which is a vinyl chloride resin composition for injection molding.

8. A vinyl chloride resin molded article which is a molded article of the vinyl chloride resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Composition comprising alkali metal carboxylates for stabilizing halogen-containing polymers

    EP2363431A1

  • Vinyl chloride-based resin composition and vinyl chloride-based resin molding

    JP2017165868A