Method for manufacturing titanium-iron solid solution layer

By coating titanium materials with iron and heating them to form a titanium-iron solid solution layer, a thicker, hardened surface layer is achieved, addressing the limitations of existing methods and improving the mechanical properties of titanium materials.

JP2024139837APending Publication Date: 2024-10-10OSAKA RES INST OF IND SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023050751
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods fail to effectively form a thick surface hardened layer on titanium materials, limiting their enhanced functionality.

Method used

A method involving coating titanium materials with iron and heating them to form a titanium-iron solid solution layer, which includes specific coating and heating processes under controlled conditions to achieve a hardened layer with a Vickers hardness of 200 HV or more at a depth of 100 μm from the surface.

Benefits of technology

The method results in a thicker, hardened surface layer on titanium materials, enhancing their mechanical properties and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
Patent Text Reader

Abstract

To provide a method for forming a thicker surface hardened layer on a titanium material.SOLUTION: A method for manufacturing a titanium-iron solid solution layer that includes: a coating step (A) of applying coating treatment to a surface to be treated of a titanium material with iron; and a heating step (B) for heating a coated surface that is formed in the coating step (A) in this order.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a titanium-iron solid solution layer. [Background technology]

[0002] Titanium has a relatively low specific gravity among metals, is relatively strong, and has excellent corrosion resistance, so it is used in a wide range of applications and is expected to be used in an even wider variety of applications in the future.

[0003] In order to further enhance the functionality of titanium materials, attempts have been made to improve the surface strength of titanium materials by carrying out specific treatments on the titanium material surface.

[0004] For example, Patent Document 1 discloses a surface hardening technique in which the surface of a titanium material is subjected to an oxygen treatment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-153497 A Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above circumstances, an object of the present invention is to provide a method for forming a thicker surface-hardened layer on a titanium material. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the inventors have discovered that a thick surface-hardened layer can be formed on the surface of a titanium material by coating the surface of the titanium material with iron and then heating it. Based on this knowledge, the inventors have conducted further research and have completed the present invention.

[0008] That is, the present invention provides the following method for producing a titanium-iron solid solution layer. Section 1. A coating process (A) of coating the treated surface of the titanium material with iron; and The method for producing a titanium-iron solid solution layer comprises, in this order, a heating step (B) of heating the coated surface formed in the coating step (A). Section 2. 2. The method for producing a titanium-iron solid solution layer according to item 1, wherein the coating step (A) is carried out by any one of the following methods (I) to (III): (I): Iron plating is applied to the treated surface of the titanium material. (II): Place iron powder on the treated surface of the titanium material. (III): Iron plating is applied to the surface of the titanium material to be treated, and iron powder is placed on the iron-plated surface. Section 3. 3. The method for producing a titanium-iron solid solution layer according to item 1 or 2, wherein the heating step (B) is carried out in an inert gas atmosphere. Section 4. 3. The method for producing a titanium-iron solid solution layer according to item 1 or 2, wherein the heating step (B) is carried out at a temperature condition of 900 to 1500°C. Section 5. 3. The method for producing a titanium-iron solid solution layer according to Item 1 or 2, further comprising a heating step (C) of subjecting the titanium-iron solid solution layer obtained in the heating step (B) to at least one type of heat treatment selected from the group consisting of laser heating, high-frequency induction heating, and gas burner heating. Section 6. A titanium-iron solid solution layer formed on the surface of a titanium material, The titanium-iron solid solution layer has a Vickers hardness of 200 HV or more at a depth of 100 μm from the outer surface of the titanium-iron solid solution layer. Effect of the Invention

[0009] According to the method for producing a titanium-iron solid solution layer according to the present invention described above, a thick surface-hardened layer can be formed on the surface of a titanium material. [Brief description of the drawings]

[0010] [Figure 1] 4 shows the results of Vickers hardness measurement evaluation test for Examples 1 and 2 and Comparative Examples 1 and 2. [Diagram 2] FIG. 2 is a cross-sectional view of the first and second embodiments. [Diagram 3] 4 shows the results of Vickers hardness measurement evaluation test for Examples 3 and 4 and Comparative Example 3. [Figure 4] FIG. 1 is a cross-sectional view of Examples 3 and 4. [Diagram 5] EPMA line analysis results of Example 2. [Figure 6] EPMA line analysis results for Example 3. [Figure 7] EPMA surface analysis results of Example 2. [Figure 8] EPMA surface analysis results of Example 3. [Figure 9] 4 shows the results of Vickers hardness measurement evaluation test for Examples 5 and 6 and Comparative Example 4. [Figure 10] EPMA line analysis results for Example 5. [Figure 11] EPMA surface analysis results of Example 5. [Figure 12] EPMA line analysis results for Comparative Example 4. [Figure 13] EPMA surface analysis results for Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of." In addition, in this specification, when a numerical range is shown as "A to B," it means A or more and B or less.

[0012] (Production method of titanium-iron solid solution layer) The method for producing a titanium-iron solid solution layer according to the present invention includes, in this order, a coating step (A) of coating a surface of a titanium material with iron, and a heating step (B) of heating the coated surface formed in the coating step (A).

[0013] Coating process (A) The coating step (A) is a step of coating the treated surface of the titanium material with iron.

[0014] The titanium material used may be either pure titanium (α type, β type) or titanium alloy, and is not particularly limited. Examples of titanium alloys include α+β type titanium alloys, α type titanium alloys, and β type titanium alloys. Examples of α+β type titanium alloys include Ti-6Al-4V, Ti-8Mn, Ti-6Al-6V-2Sn, Ti-10V-2Fe-3Al, etc. Examples of α type titanium alloys include Ti-5Al-2.5Sn. Examples of β type titanium alloys include Ti-13V-11Cr-3Al, Ti-15Mo-5Zr-3Ai, Ti-15V-3Cr-3Al-3Sn, Ti-22V-4Al, etc.

[0015] The coating step (A) is preferably carried out by any one of the methods (I) to (III) below. (I): Iron plating is applied to the treated surface of the titanium material. (II): Place iron powder on the treated surface of the titanium material. (III): Iron plating is applied to the surface of the titanium material to be treated, and iron powder is placed on the iron-plated surface.

[0016] In the above (I), the method for applying iron plating can be a wide variety of known methods and is not particularly limited. Specific examples of the method include hot-dip plating, wet plating, and dry plating.

[0017] The iron plating layer formed by applying iron plating may be pure iron or an iron-based alloy having an iron purity of preferably 90% by mass or more, more preferably 95% by mass or more. There is no particular limitation on such an iron-based alloy, and examples of such an iron-based alloy include Fe-Ni, Fe-Co, and Fe-Ni-Co.

[0018] The thickness of the iron plating layer is preferably 1 μm or more, more preferably 5 μm or more, in order to prevent oxidation of the titanium material surface, and is preferably 200 μm or less, more preferably 50 μm or less, in order to prevent peeling of the iron plating layer.

[0019] In the above (II), the iron powder placed on the surface to be treated may be pure iron, as in the case of the iron plating layer, or an iron-based alloy having an iron purity of preferably 90% by mass or more, more preferably 95% by mass or more. There are no particular limitations on such iron-based alloy, and examples of such alloy include Fe-C, Fe-Ni, Fe-Co, and Fe-Ni-Co.

[0020] The size of the iron powder is preferably 10 μm or more, more preferably 50 μm or more, in terms of average particle size, while the average particle size is preferably 200 μm or less, more preferably 100 μm or less.

[0021] The amount of iron powder to be placed on the titanium material is set to 1 cm2 of the treated surface of the titanium material in order to distribute the powder evenly over the entire surface. 2 The amount of iron powder is preferably 0.03 g or more, and more preferably 0.20 g or more, per 1 cm of the treated surface of the titanium material. If the treated area has a complex shape, titanium material may be mixed into the powder. There is no upper limit to the amount of iron powder, and the amount is set at 1 cm per 1 cm of the treated surface of the titanium material. 2 It should be 3g or less per serving.

[0022] The conditions for iron plating and placing the iron powder on the surface to be treated in (III) above can be set in the same manner as in (I) and (II) above.

[0023] Heating process (B) In the heating step (B), the coated surface formed in the coating step (A) is heated.

[0024] In this case, the heating temperature is preferably 900° C. or higher, and more preferably 950° C. or higher. On the other hand, the heating temperature is preferably 1500° C. or lower, and more preferably the solidus temperature or lower in the Ti-Fe equilibrium diagram.

[0025] The heating time can be appropriately set depending on the heating temperature, and is not particularly limited. For example, it is preferably 10 seconds or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. On the other hand, the heating time is preferably 5 hours or less, and more preferably 3 hours or less.

[0026] The heating method can be any method known in the steel processing field and is not particularly limited. Specifically, it is preferable to perform overall heating by furnace heating or low-frequency heating. Examples of the furnace to be used include a gas furnace and an electric furnace.

[0027] Moreover, the heating step (B) is preferably carried out in an inert atmosphere, particularly preferably in an argon atmosphere, in order to prevent oxidation of the surface of the titanium material.

[0028] By carrying out the heating step (B), a titanium-iron solid solution layer is formed.

[0029] Heating process (C) It is also preferable to provide a heating step (C) after the heating step (B) in which the titanium-iron solid solution layer obtained in the heating step (B) is subjected to at least one type of heat treatment selected from the group consisting of laser heating, high-frequency induction heating, and gas burner heating.

[0030] By providing the heating process (C), the titanium-iron solid solution layer is hardened, and the segregation of iron is improved.

[0031] The heating step (C) is preferably performed locally, for example, in the region to which wear resistance is to be imparted. Examples of such a heating method include heating by laser, high-frequency induction, gas burner, electron beam, etc. Among the local heating methods, at least one selected from the group consisting of laser heating, high-frequency induction heating, and gas burner heating is preferred.

[0032] In order to homogenize the iron segregation structure, the heating temperature in the heating step (C) is preferably set to a temperature equal to or higher than the β transformation point of the Ti-Fe alloy, more preferably set to a temperature 50°C or higher than the β transformation point of the Ti-Fe alloy, and even more preferably set to a temperature 100°C or higher than the β transformation point of the Ti-Fe alloy. On the other hand, in order to prevent the titanium material, which is the base material, from melting, the heating temperature is preferably set to a temperature equal to or lower than the solidus temperature of the titanium material, and more preferably set to a temperature 50°C or lower than the solidus temperature of the titanium material. More specifically, the heating temperature is preferably set to 900°C or higher, and more preferably set to 1000°C or higher. Also, the heating temperature is preferably set to 1600°C or lower, and more preferably set to 1500°C or lower.

[0033] The heating time in the heating step (C) is not particularly limited, and may be appropriately set depending on the specific embodiment of the heat treatment.

[0034] Examples of the laser for laser heating include CO2 laser, YAG laser, excimer laser, UV laser, semiconductor laser, fiber laser, LD laser, and LD excited solid-state laser heat. Specifically, when heating with a semiconductor laser as local heating, it is preferable to perform the heating under the conditions of output: 300 to 1000 W, moving speed: 6 mm / s, so as not to melt the treated surface of titanium. The laser heating device may be a commercially available product. For example, in addition to a high-power semiconductor laser with an oscillator LDL160-1000 (Laser Line), various laser heating devices manufactured by Sakaguchi Dennetsu Co., Ltd. and Hamamatsu Photonics K.K. may be used.

[0035] High-frequency induction heating involves heating by induction heating of high-frequency current from an AC power source. Commercially available high-frequency induction heating devices can be used. There are no particular limitations on the gas burner, so long as it is one that mixes fuel gas (e.g., hydrocarbon gases such as methane, ethane, propane, butane, etc.) with air and burns it. Commercially available gas burner devices can be used. Heating by electron beam involves irradiating an object with a highly densely focused electron beam in a vacuum to heat it. Commercially available electron beam heating devices can be used.

[0036] Aging treatment process (D) It is also preferable to provide an aging treatment step (D) after the heating step (C). The aging treatment can be carried out by a wide variety of known methods used in the technical field, and is not particularly limited.

[0037] (Titanium-iron solid solution layer) The present invention includes an invention relating to a titanium-iron solid solution layer. The titanium-iron solid solution layer of the present invention is a titanium-iron solid solution layer formed on the surface of a titanium material, and has a Vickers hardness of 200 HV or more at a depth of 100 μm from the outer surface of the titanium-iron solid solution layer.

[0038] The titanium-iron solid solution layer of the present invention can be obtained, for example, by the same method as that for the titanium-iron solid solution layer described above. As for the titanium material to be used, the same titanium material as that described above may be used.

[0039] The titanium-iron solid solution layer of the present invention is formed on the surface of a titanium material, and the solid solution layer has a greater thickness than conventional ones.

[0040] As a result, the Vickers hardness at a depth of 100 μm from the outer surface of the titanium-iron solid solution layer formed on the outer surface of the titanium material is 200 HV or more, preferably 300 HV or more, more preferably 400 HV or more, and even more preferably 450 HV or more. There is no particular upper limit to the Vickers hardness, and for example, it is preferably 900 HV or less, more preferably 800 HV or less, even more preferably 700 HV or less, even more preferably 650 HV or less, and particularly preferably 550 HV or less.

[0041] Although the embodiment of the present invention has been described above, the present invention is not limited to these examples, and it is needless to say that the present invention can be embodied in various forms without departing from the gist of the present invention. EXAMPLES

[0042] Hereinafter, the embodiments of the present invention will be described more specifically based on examples, but the present invention is not limited to these.

[0043] Example 1 A 30μm thick iron plating layer was formed on a part of the surface of a titanium material made of JIS type 2 titanium (pure titanium) by electroplating.The titanium material was then placed in an electric furnace and heated at 1000℃ for 2 hours in an argon atmosphere to obtain a titanium-iron solid solution layer.

[0044] Example 2 An iron plating layer was formed on the same titanium material as in Example 1 in the same manner as in Example 1. 2 The substrate was placed in an electric furnace in the same manner as in Example 1 and heated at 1000°C for 2 hours in an argon atmosphere to obtain a titanium-iron solid solution layer.

[0045] Comparative Example 1 In the above Example 1, in the areas where the iron plating layer was not formed (i.e., the areas where the iron plating layer was not formed), no titanium-iron solid solution layer was formed, and the outer surface of those areas was designated as Comparative Example 1.

[0046] Comparative Example 2 In the above Example 2, in the areas where the iron plating layer was not formed, no titanium-iron solid solution layer was formed, and the outer surface of those areas was designated as Comparative Example 2.

[0047] Vickers hardness measurement evaluation test Using a Vickers hardness tester (manufactured by Future Tech, Cat No. M-310ARS-F), hardness measurements were performed on a cut surface perpendicular to the longitudinal direction (60 mm) of a 20 × 60 × 3 mm test piece from just below the central surface toward the inside of the piece for each of the examples and comparative examples.

[0048] Cross-sectional image evaluation test Using an inverted metallurgical microscope (Nikon, Cat No. MA-100), images of the vicinity of the cross section of the surface layer of each of the examples and comparative examples were taken.

[0049] The results of the Vickers hardness of Examples 1 and 2 and Comparative Examples 1 and 2 are shown in FIG. 1, and the results of the cross-sectional image evaluation of Examples 1 and 2 are shown in FIG.

[0050] Example 3 A part of the surface of a titanium material made of JIS type 2 titanium (pure titanium) is iron-plated, and then 0.30 g / cm is applied to the iron-plated layer. 2 The iron powder was placed on the specimen in an amount of 1000°C, and heated in an argon atmosphere at 1000°C for 2 hours in the same manner as in Example 1 to form a titanium-iron solid solution layer. The titanium-iron solid solution layer was then hardened with a laser. The laser irradiation conditions were an output of 600 W and a spot angle of 5 mm, and the surface of a 20 x 60 mm test piece was irradiated (temperature: approximately 1100°C), and the center of the test piece was moved in the longitudinal direction of the test piece at a speed of 10 mm / s.

[0051] Example 4 A part of the surface of titanium material made of JIS type 2 titanium (pure titanium) is not electroplated and is coated with 0.30 g / cm 2 After that, the substrate was placed in an electric furnace in the same manner as in Example 1 and heated at 900° C. for 2 hours in an argon atmosphere to form a titanium-iron solid solution layer.

[0052] Comparative Example 3 In the above Example 3, in the areas where the iron plating layer was not formed, no titanium-iron solid solution layer was formed, and the outer surface of those areas was designated as Comparative Example 1.

[0053] The Vickers hardness measurement evaluation test and the cross-sectional image evaluation test were also carried out for the above-mentioned Examples 3 and 4 and Comparative Example 3. The results are shown in FIGS.

[0054] EPMA line analysis test A field emission electron probe microanalyzer (FE-EPMA) (manufactured by JEOL Ltd., JXA-8530F) was used to carry out an EPMA line analysis test near the surface where hardness was measured. The results of Example 2 are shown in FIG. 5, and the results of Example 3 are shown in FIG. 6.

[0055] EPMA surface analysis test An EPMA surface analysis test was carried out near the surface where the hardness was measured. The results of Example 4 are shown in FIG. 7, and the results of Example 3 are shown in FIG.

[0056] Example 5 A part of the surface of titanium material made of JIS 60 type titanium (Ti-6Al-4V) is electroplated to a thickness of 0.30 g / cm 2 After that, the substrate was placed in an electric furnace and heated at 1000°C for 2 hours in an argon atmosphere to form a titanium-iron solid solution layer, as in Example 3. The titanium-iron solid solution layer thus obtained was then laser hardened under the same conditions as in Example 3.

[0057] Example 6 A part of the surface of titanium material made of JIS 60 type titanium (Ti-6Al-4V) is electroplated to a thickness of 0.30 g / cm 2 After that, the substrate was placed in an electric furnace in the same manner as in Example 2 and heated at 1000° C. for 2 hours in an argon atmosphere to form a titanium-iron solid solution layer.

[0058] Comparative Example 4 The outer surface of the titanium material made of JIS type 60 titanium (Ti-6Al-4V) in the above-mentioned Example 5 where no solid solution layer was formed was used as Comparative Example 4.

[0059] A Vickers hardness measurement evaluation test was performed on the above-mentioned Examples 5 and 6 and Comparative Example 4, and an EPMA line analysis was performed on Example 5. The results of the Vickers hardness measurement evaluation test are shown in Fig. 9, the results of the EPMA line analysis and the EPMA area analysis of Example 5 are shown in Figs. 10 and 11, and the results of the EPMA line analysis and the EPMA area analysis of Comparative Example 4 are shown in Figs. 12 and 13.

Claims

1. A coating process (A) for coating the treated surface of the titanium material with iron; and a heating step (B) of heating the coated surface formed in the coating step (A), in this order.

2. 2. The method for producing a titanium-iron solid solution layer according to claim 1, wherein the coating step (A) is carried out by any one of the following methods (I) to (III): (I): Iron plating is applied to the treated surface of the titanium material. (II): Place iron powder on the surface of the titanium material to be treated. (III): The surface of the titanium material to be treated is iron-plated, and iron powder is then placed on the iron-plated surface.

3. 3. The method for producing a titanium-iron solid solution layer according to claim 1, wherein the heating step (B) is carried out in an argon atmosphere.

4. 3. The method for producing a titanium-iron solid solution layer according to claim 1, wherein the heating step (B) is carried out at a temperature condition of 900 to 1500°C.

5. 3. The method for producing a titanium-iron solid solution layer according to claim 1 or 2, further comprising a heating step (C) of subjecting the titanium-iron solid solution layer obtained in the heating step (B) to at least one type of heat treatment selected from the group consisting of laser heating, high-frequency induction heating, and gas burner heating.

6. A titanium-iron solid solution layer formed on a titanium material surface, The titanium-iron solid solution layer has a Vickers hardness of 200 HV or more at a depth of 100 μm from the outer surface of the titanium-iron solid solution layer.

Citation Information

Patent Citations

  • Surface hardening process for titanium

    JP1981081665A

  • Method for hardening titanium material

    JP1990250951A

  • Rolling bearing

    JP2020153497A