Liquid discharge head manufacturing method
The use of metal-assisted chemical etching in the manufacturing process addresses the challenges of miniaturization and ejection performance in liquid ejection heads by precisely forming constricted portions and channels, resulting in a smaller and more efficient ink delivery system.
Patent Information
- Application Number
- JP2023051085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing liquid ejection heads face challenges in miniaturization and maintaining high ejection performance due to difficulties in microfabricating liquid flow paths with precise control over flow path resistance and aspect ratios, leading to unstable ink ejection and residual vibrations.
A manufacturing method for a liquid ejection head that utilizes metal-assisted chemical etching to form constricted portions and channels with high precision, allowing for precise control of flow path resistance and stabilization of meniscus movement, thereby enhancing ejection performance and reducing head size.
The method enables the production of a smaller liquid ejection head with improved ejection speed and stability by accurately forming constricted portions and channels, ensuring efficient ink delivery and reduced residual vibrations.
Smart Images

Figure 2024140090000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a liquid ejection head. [Background technology]
[0002] In recent years, inkjet printers have been attracting attention not only for printing purposes but also as devices capable of applying liquefied materials to any location. Inkjet printers are equipped with a liquid ejection head that ejects liquid. A known liquid ejection head is one that ejects liquid filled in a pressure chamber from a nozzle by vibrating a vibration plate that constitutes the wall of the pressure chamber using a piezoelectric element.
[0003] The liquid ejection head described in Patent Document 1 has an upper substrate and an intermediate substrate. A plurality of pressure chambers are formed in the upper substrate. The intermediate substrate is joined to the lower surface of the upper substrate. A manifold and a plurality of communication holes are formed in the intermediate substrate. The manifold supplies ink to the plurality of pressure chambers via the plurality of communication holes. Furthermore, each of the upper substrate and the intermediate substrate is made of a silicon substrate.
[0004] The liquid ejection head described in Patent Document 2 has a cavity substrate and a reservoir substrate. A plurality of pressure chambers are formed in the cavity substrate. The reservoir substrate is bonded to the cavity substrate. A reservoir and a supply port are formed in the reservoir substrate. The reservoir supplies ink to the pressure chambers via the supply port. The cavity substrate and the reservoir substrate are each made of single crystal silicon. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-107902 A [Patent Document 2] JP 2007-331167 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the liquid ejection heads described in Patent Documents 1 and 2, the pressure chambers and the manifolds or reservoirs for supplying ink to the pressure chambers are formed on different substrates, which allows the substrates to be made smaller, and therefore the ejection head to be made smaller.
[0007] In order to further miniaturize the ejection head while increasing the speed of liquid ejection, it is necessary to increase the ejection amount per unit time or the ejection cycle. To achieve this, it is conceivable to enlarge the pressure chamber to reduce the flow path resistance. However, if the flow path resistance is reduced, it takes time to attenuate the residual vibration, which is the vibration that remains inside the nozzle after the ejection of the droplets. As a result, it takes time to stabilize the meniscus at the nozzle tip. This may result in a decrease in ejection performance. To solve this problem, it is conceivable to increase the flow path resistance of the ink flow path by, for example, miniaturizing the liquid flow path provided between the pressure chamber and the manifold or reservoir.
[0008] However, when miniaturizing the ejection head, it is very difficult to finely process the liquid flow path. For example, the liquid flow path is formed in the substrate by dry etching. In this case, the inflow of the etching gas decreases as the processing depth increases, so the processing time becomes very long. In addition, the liquid flow path is formed in the substrate by anisotropic wet etching along the crystal orientation of the substrate. In this case, it is difficult to control the aspect ratio of the liquid flow path.
[0009] Therefore, it is difficult to form liquid flow paths with high precision, and it is difficult to manufacture a small liquid ejection head that has excellent ejection performance. [Means for solving the problem]
[0010] A preferred embodiment of the present invention provides a method for manufacturing a liquid ejection head having a plurality of individual flow paths, each of which has a pressure chamber extending in a first direction, a nozzle connected to one end of the pressure chamber, and a throttling portion connected to the other end of the pressure chamber, extending in a second direction intersecting the first direction, and having a smaller cross-sectional area than the pressure chamber, and a common flow path connected in common to the plurality of individual flow paths, the method including a first step of forming a metal film on a first portion of a first surface of a semiconductor substrate that corresponds to the throttling portion, and performing metal-assisted chemical etching in a state in which the metal film is not formed on a surface of a second portion of the first surface that does not correspond to the throttling portion, to form the throttling portion. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram illustrating a configuration of a liquid ejection device according to a first embodiment. [Diagram 2] FIG. 2 is an exploded perspective view of the liquid ejection head shown in FIG. [Diagram 3] FIG. 3 is a cross-sectional view taken along line aa in FIG. [Figure 4] FIG. 4 is a plan view of the communication plate shown in FIG. [Diagram 5] 5 is an enlarged view of a portion of the communication plate shown in FIG. [Figure 6] 4 is a diagram showing a flow of a method for manufacturing the communicating plate shown in FIG. 3. [Figure 7] FIG. 7 is a diagram showing the flow of the first step shown in FIG. 6. [Figure 8] 8 is a diagram for explaining the steps from the oxide film forming step to the resist layer patterning step in FIG. 7. FIG. [Figure 9] 8 is a diagram for explaining the oxide film etching step to the metal-assisted chemical etching step in FIG. 7. FIG. [Figure 10] FIG. 1 is a diagram for explaining a metal-assisted chemical etching process. [Figure 11] FIG. 7 is a diagram showing the flow of the second step shown in FIG. 6. [Figure 12] 12A to 12C are diagrams for explaining the steps from the second oxide film forming step to the second resist layer patterning step in FIG. 11. [Figure 13] 12 is a diagram for explaining the second oxide film etching step to the metal-assisted chemical etching step in FIG. 11. FIG. [Figure 14] FIG. 11 is a view for explaining a first step of the second embodiment. [Figure 15] FIG. 11 is a diagram showing the flow of a second step in the second embodiment. [Figure 16] FIG. 11 is a view for explaining a second step of the second embodiment. [Figure 17] 13A to 13C are diagrams illustrating a flow of a manufacturing method of the communicating plate according to the third embodiment. [Figure 18] FIG. 13 is a diagram showing the flow of a third step in the third embodiment. [Figure 19] FIG. 13 is a view for explaining a third step of the third embodiment. [Figure 20] FIG. 13 is a view for explaining a third step of the third embodiment. [Figure 21] 5A to 5C are diagrams illustrating the flow of a liquid ejection head manufacturing method. [Figure 22] 6 is a table illustrating an embodiment of the throttle portion of FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] 1. First embodiment 1-1. Overall configuration of liquid ejection device 1 FIG. 1 is a configuration diagram illustrating a liquid ejection device 1 according to a first embodiment. In the following, for convenience of explanation, an X-axis, a Y-axis, and a Z-axis that are perpendicular to each other will be appropriately used. Moreover, one direction along the X-axis will be referred to as the X1 direction, and the direction opposite to the X1 direction will be referred to as the X2 direction. Similarly, one direction along the Y-axis will be referred to as the Y1 direction, and the direction opposite to the Y1 direction will be referred to as the Y2 direction. One direction along the Z-axis will be referred to as the Z1 direction, and the direction opposite to the Z1 direction will be referred to as the Z2 direction.
[0013] In addition, "element α and element β are in communication" includes cases where element α and element β are in direct communication with each other, as well as cases where element α and element β are in indirect communication with each other via another element. "Element β on element A" is not limited to a configuration where element α and element β are in direct contact with each other, but also includes a configuration where element A and element β are not in direct contact with each other.
[0014] The liquid ejection device 1 is an inkjet printing device that ejects ink, which is an example of a liquid, onto a medium 12. The medium 12 is typically printing paper, but any printing target made of any material, such as a resin film or fabric, can be used as the medium 12. As illustrated in Fig. 1, the liquid ejection device 1 is provided with a liquid container 14 that stores ink. For example, a cartridge that can be attached to and detached from the liquid ejection device 1, a bag-shaped ink pack made of a flexible film, or an ink tank that can be refilled with ink can be used as the liquid container 14.
[0015] The liquid ejection device 1 includes a control unit 20, a transport mechanism 22, a moving mechanism 24, and a liquid ejection head 3. The control unit 20 includes one or more processing circuits, such as a CPU (Central Processing Unit) or an FPGA (Field Programmable Gate Array), and one or more storage circuits, such as a semiconductor memory, and performs overall control of each element of the liquid ejection device 1. The transport mechanism 22 transports the medium 12 in a direction along the Y axis under the control of the control unit 20.
[0016] The movement mechanism 24 reciprocates the liquid ejection head 3 along the X axis under the control of the control unit 20. The X axis intersects with the Y axis along the direction in which the medium 12 is transported. The movement mechanism 24 in the first embodiment includes a substantially box-shaped transport body 242 that houses the liquid ejection head 3, and a transport belt 244 to which the transport body 242 is fixed. Note that a configuration in which a plurality of liquid ejection heads 3 are mounted on the transport body 242, or a configuration in which the liquid container 14 is mounted on the transport body 242 together with the liquid ejection head 3, may also be employed.
[0017] The liquid ejection heads 3 eject ink supplied from a liquid container 14 from multiple nozzles onto the medium 12 under the control of a control unit 20. An image is formed on the surface of the medium 12 by each liquid ejection head 3 ejecting ink onto the medium 12 in parallel with the transportation of the medium 12 by the transportation mechanism 22 and the repeated reciprocating motion of the transportation body 242.
[0018] 1-2. Overall configuration of liquid ejection head 3 FIG. 2 is an exploded perspective view of the liquid ejection head 3 shown in FIG. 1. FIG. 3 is a cross-sectional view taken along line aa in FIG. 2. The cross section shown in FIG. 3 is a cross section parallel to the XZ plane. The Z axis is an axis along the direction in which ink is ejected by the liquid ejection head 3. The X1 direction or the X2 direction is an example of a "first direction". The Z2 direction is an example of a "second direction". In addition, a view from the Z1 direction or the Z2 direction is referred to as a "planar view".
[0019] As illustrated in FIG. 2, the liquid ejection head 3 includes a plurality of nozzles N arranged along the Y axis. The plurality of nozzles N are divided into a first row La and a second row Lb arranged in parallel with each other at intervals along the X axis. Each of the first row La and the second row Lb is a collection of a plurality of nozzles N arranged linearly along the Y axis. The liquid ejection head 3 has a structure in which elements related to each nozzle N of the first row La and elements related to each nozzle N of the second row Lb are arranged substantially symmetrically with respect to a plane. The nozzles N belonging to the first row La are arranged in a line with a density of, for example, 300 dpi. Similarly, the nozzles N belonging to the second row Lb are arranged in a line with a density of, for example, 300 dpi. The nozzles N belonging to the second row Lb are arranged with a shift of, for example, 600 dpi with respect to the nozzles N belonging to the first row La. In the following description, the elements corresponding to the first row La will be described with emphasis, and the description of the elements corresponding to the second row Lb will be omitted as appropriate.
[0020] As illustrated in FIGS. 2 and 3, the liquid ejection head 3 includes a flow path structure 30, a plurality of piezoelectric elements , a sealing substrate 35, a housing portion , and a wiring substrate .
[0021] The flow path structure 30 is a structure in which a flow path is formed for supplying ink to each of the multiple nozzles N. The flow path structure 30 is composed of a communication plate 31, a pressure chamber substrate 32, a vibration plate 33, a nozzle substrate 37, and a vibration absorber .
[0022] Each member constituting the flow path structure 30 is a long plate-like member along the Y axis. A pressure chamber substrate 32 and a housing part 36 are provided on a surface of the communication plate 31 in the Z2 direction. A nozzle substrate 37 and a vibration absorber 38 are provided on a surface of the communication plate 31 in the Z1 direction. The members are fixed together by, for example, an adhesive.
[0023] The nozzle substrate 37 is a plate-like member in which a plurality of nozzles N are formed. Each of the plurality of nozzles N is a circular through-hole that ejects ink. For example, the nozzle substrate 37 is manufactured by processing a single crystal substrate of silicon (Si) using semiconductor manufacturing techniques such as photolithography and etching.
[0024] The communication plate 31 is formed with a plurality of throttle portions 312, a plurality of communication channels 314, a communication space Ra, and a common channel Rb. Each of the throttle portions 312 and the communication channels 314 extends in the Z1 direction and is a through hole formed for each nozzle N. The communication channel 314 overlaps the nozzle N in a plan view. The communication space Ra is an opening formed in an elongated shape along the Y axis. The communication space Ra extends along the Y axis. The common channel Rb communicates with the communication space Ra and overlaps with the communication space Ra in a plan view. The common channel Rb extends along the Y axis. The common channel Rb communicates with the plurality of throttle portions 312. In addition, the communication space Ra communicates the common channel Rb with an external channel of the liquid ejection head 3 via a space Rc described later.
[0025] A plurality of pressure chambers C1 are formed in the pressure chamber substrate 32. The pressure chamber C1 is a space located between the communication plate 31 and the vibration plate 33 and formed by the wall surface 320 of the pressure chamber substrate 32. The pressure chamber C1 is formed for each nozzle N. The pressure chamber C1 is an elongated space extending in the X1 direction. The plurality of pressure chambers C1 are arranged along the Y axis. One end of the pressure chamber C1 in the X1 direction is connected to the nozzle N via a communication flow path 314. The other end of the pressure chamber C1 in the X1 direction is connected to a throttle portion 312. The throttle portion 312 has a smaller cross-sectional area than the pressure chamber C1. In addition, the pressure chamber C1, the nozzle N, the communication flow path 314, and the throttle portion 312 form an individual flow path 300 for each nozzle N. By providing the communication flow passage 314 and the throttle portion 312 in the Z1 direction for the pressure chamber C1, it is possible to arrange the nozzles at a high density, and the liquid ejection head 3 can be made smaller and more dense.
[0026] The communication plate 31 and the pressure chamber substrate 32 are manufactured by processing a semiconductor substrate such as a silicon single crystal substrate.
[0027] An elastically deformable vibration plate 33 is disposed above the pressure chamber C1. The vibration plate 33 is laminated on the pressure chamber substrate 32 and contacts the surface of the pressure chamber substrate 32 opposite to the communicating plate 31. The vibration plate 33 is a plate-like member formed in a long rectangular shape along the Y axis in a plan view. The thickness direction of the vibration plate 33 is parallel to the Z1 direction. The pressure chamber C1 communicates with the communicating flow path 314 and the throttle portion 312. Therefore, the pressure chamber C1 communicates with the nozzle N via the communicating flow path 314, and communicates with the communicating space Ra via the throttle portion 312. Note that, for ease of explanation, the pressure chamber substrate 32 and the vibration plate 33 are illustrated in FIG. 2 as separate substrates, but in reality, they are laminated on a single silicon substrate.
[0028] A piezoelectric element 34 is formed for each pressure chamber C1 on the surface of the vibration plate 33 opposite to the pressure chamber C1. The piezoelectric element 34 is an elongated passive element along the X-axis in a plan view. The piezoelectric element 34 is an example of an energy generating element that generates energy for ejecting ink when a drive signal is applied to it. Although a piezoelectric element that generates mechanical energy is described here as the energy generating element, an electrothermal conversion element that generates thermal energy may also be used as long as it is a system that has the vibration plate 33. The piezoelectric element 34 is also a driving element that is driven when a drive signal is applied to it.
[0029] The housing 36 is a case for storing ink to be supplied to the multiple pressure chambers C1, and is formed by, for example, injection molding of a resin material. A space Rc and a supply port 361 are formed in the housing 36. The supply port 361 is a conduit through which ink is supplied from the liquid container 14, and communicates with the space Rc. The space Rc in the housing 36 and the communication space Ra in the communication plate 31 communicate with each other. The communication space Ra, the common flow path Rb, and the space Rc described above form a common space R that is shared by the multiple nozzles N. The common space R functions as a liquid storage chamber that stores ink to be supplied to the multiple pressure chambers C1. The ink stored in the common space R branches off to each throttle section 312 and is supplied to and filled in parallel with the multiple pressure chambers C1.
[0030] The vibration absorber 38 is a flexible film that constitutes the wall surface of the communication space Ra, and absorbs pressure fluctuations of the ink in the common space R. The vibration absorber 38 is, for example, a laminate of an ink-resistant resin film, a SUS (stainless steel) member that holds the resin film and has spring properties, and a fixed plate that protects the resin film and the SUS member. By providing the vibration absorber 38, the natural frequency of the individual flow path 300 that runs from the nozzle N through the pressure chamber C1 to the throttle section 312 is stabilized regardless of the nozzle N that is driven.
[0031] The sealing substrate 35 is a structure that protects the piezoelectric elements 34 and reinforces the mechanical strength of the pressure chamber substrate 32 and the vibration plate 33, and is fixed to the surface of the vibration plate 33 with, for example, an adhesive. The piezoelectric elements 34 are housed inside a recess formed on the surface of the sealing substrate 35 facing the vibration plate 33. The wiring substrate 40 is inserted through a through hole 362 of the housing portion 36 and a through hole 353 of the sealing substrate 35. The wiring substrate 40 is bonded to the surface of the vibration plate 33. The wiring substrate 40 is a mounting component on which a plurality of wirings for electrically connecting the control unit 20 and the liquid ejection head 3 are formed. For example, a TCP (Tape Carrier Package) or an FPC (Flexible Printed Circuit) is used as the wiring substrate 40. A drive signal and a reference voltage for driving the piezoelectric elements 34 are supplied to each piezoelectric element 34 from the wiring substrate 40.
[0032] In the liquid ejection head 3, when the piezoelectric element 34 contracts due to energization, the vibration plate 33 is bent and deflected in a direction that reduces the volume of the pressure chamber C1, and the pressure inside the pressure chamber C1 rises, causing an ink droplet to be ejected from the nozzle N. At this time, pressure also propagates from the pressure chamber C1 toward the throttle portion 312, and ink also flows into the common flow path Rb through the throttle portion 312. After the ink is ejected, the piezoelectric element 34 returns to its original position. At this time, the ink in the common flow path Rb from the nozzle N also vibrates. Then, at the same time that the meniscus of the nozzle N returns to its original state, ink is supplied from the throttle portion 312. Through the above series of operations, ink is ejected from the nozzle N.
[0033] 1-3.Communication plate 31 FIG. 4 is a plan view of the communication plate 31 shown in FIG. 3. As shown in FIG. 4, the communication plate 31 is formed with a communication space Ra, a common flow path Rb, a plurality of throttling portions 312, and a plurality of communication flow paths 314. The communication space Ra extends in the Y1 direction. The common flow path Rb extends in the Y1 direction and overlaps with the communication space Ra and the plurality of throttling portions 312 in a plan view. The plurality of throttling portions 312 and the plurality of communication flow paths 314 are provided in one-to-one correspondence with the plurality of nozzles N, for example. Note that several throttling portions 312 may correspond to one nozzle N. In addition, the plurality of throttling portions 312 are spaced apart from each other and aligned along the Y1 direction. The plurality of communication flow paths 314 are spaced apart from each other and aligned in the Y1 direction. In addition, the plurality of communication flow paths 314 are spaced apart from the common flow path Rb and the plurality of throttling portions 312.
[0034] Fig. 5 is an enlarged view of a portion of the communicating plate 31 shown in Fig. 4. As shown in Fig. 5, the cross-sectional area of the throttle portion 312 parallel to the XY plane is smaller than the cross-sectional area of the communicating flow path 314 parallel to the XY plane. In addition, the cross-sectional area of the throttle portion 312 parallel to the XY plane is smaller than the cross-sectional area of the common flow path Rb along the Z axis. In addition, the shape, etc. of the common flow path Rb are designed so that the flow path resistances of the multiple throttle portions 312 are equal to each other.
[0035] In the series of ink ejection operations described above, in the individual flow paths 300 shown in Fig. 3, vibrations occurring when ink is ejected are attenuated by the flow path resistance in the individual flow paths 300. The flow path resistance in the individual flow paths 300 is mainly caused by the flow path resistance of the throttling portion 312. This is because the cross-sectional area of the throttling portion 312 parallel to the XY plane is smaller than the cross-sectional area of the common flow path Rb parallel to the Z axis and the cross-sectional area of the pressure chamber C1 along the Z axis. By adjusting the number or cross-sectional area of the throttling portions 312, the flow path resistance in the individual flow paths 300 can be adjusted. Therefore, the throttling portion 312 functions as a fluid resistance portion.
[0036] As described above, the throttle section 312 also serves as a supply port that supplies ink from the common flow path Rb to the individual flow paths 300. The throttle section 312, which is such a supply port, functions as a fluid resistance section, so that there is no need to provide a separate fluid resistance section in the pressure chamber C1. This allows the pressure chamber C1 to be made smaller, and therefore the liquid ejection head 3 to be made smaller. In addition, since there is no need to provide a separate fluid resistance section in the pressure chamber C1, it is easy to increase the length of the piezoelectric element 34 without changing the volume of the pressure chamber C1. This allows the ink ejection capacity to be increased without increasing the size of the liquid ejection head 3. This allows the liquid ejection head 3 to be made smaller and faster.
[0037] Furthermore, by providing the communicating plate 31 in the Z1 direction of the pressure chamber substrate 32, it is possible to provide the throttle portion 312 in the Z1 direction of the pressure chamber C1. This makes it easy to increase the number or cross-sectional area of the throttle portion 312 in order to adjust the flow path resistance.
[0038] Fig. 22 is a table for explaining examples of the throttling portion 312 in Fig. 5. In Fig. 22, the cross-sectional shape of the throttling portion 312, the number of the throttling portions 312 corresponding to one nozzle N, the cross-sectional dimensions of the throttling portion 213, and the fluid resistance at the throttling portion 312 are shown for each example.
[0039] The fluid resistance can be calculated from the length of the throttle portion 312 in the Z1 direction relative to the cross-sectional shape of the throttle portion 312 along the XY plane, and the physical properties of the ink, such as viscosity and density. The fluid resistance includes flow path resistance, flow path resistance ratio, and inertance ratio. The calculation results are shown in Figure 22. The flow path resistance is indicated by R, and the inertance is indicated by M. The calculation was performed assuming that the length of the throttle portion 312 in the Z1 direction was 200 μm. The unit of flow path resistance is [N·s / m 2 〕.
[0040] It is most efficient for ink ejection to balance the flow path resistance of the throttling section 312 and the fluid resistance of the nozzle N. For this reason, the cross-sectional dimensions of the throttling section 312 are set so that the flow path resistance of the throttling section 312 is approximately the same as the fluid resistance of the nozzle N. The fluid resistance of the nozzle N, specifically, the flow path resistance at the opening of the nozzle N in the Z1 direction, is Rn = 8.7 × 1012 [N s / m 2 Each example shows the results of setting the cross-sectional dimensions of the throttle portion 312 so that the fluid resistance of the throttle portion 312 approaches this value. Note that the viscosity of the ink at 25° C. in this case is η25=3.36×10 -3 [Pa / s].
[0041] The cross-sectional dimensions of the throttle portion 312 in the first embodiment are larger than those in the other embodiments. Therefore, the fluid resistance, flow path resistance ratio, and inertance ratio of the throttle portion 312 are the smallest. Therefore, the frequency of ink ejection, specifically the number of ejected droplets per nozzle N that can be ejected per second, can be maximized. However, due to the small flow path resistance, the damping of residual vibration is weak. Therefore, there are cases where the residual vibration of the ink in the pressure chamber C1 is difficult to settle. As a result, there is a risk that the ink ejection will become unstable.
[0042] In consideration of the problems of Example 1, in Example 2, the cross-sectional dimensions of the throttle portion 312 are made smaller than those of Example 1. Specifically, in Example 2, the ink flow path resistance is set to 15 times that of Example 1. Example 2 allows for more stable ink ejection than Example 1. On the other hand, Example 2 has a larger inertance than Example 1. Therefore, Example 2 has a lower frequency of ink ejection than Example 1.
[0043] In the third embodiment, two throttle portions 312 having the same shape as the throttle portion 312 in the second embodiment are provided in parallel. In the third embodiment, the increase in inertance with respect to the increase in flow path resistance can be suppressed compared to the second embodiment. By increasing the number of throttle portions 312, the flow path resistance can be increased. Therefore, the damping capacity of the residual vibration in the pressure chamber C1 after the ink is ejected can be improved. Therefore, it is possible to maintain the frequency of ink ejection at a high level.
[0044] In Example 4, the number of throttle portions 312 is further increased compared to Example 3. By further increasing the number of throttle portions 312, an optimal design of the throttle portions 312 is realized.
[0045] 22, by increasing the number of throttling portions 312 corresponding to one nozzle N, the fluid resistance of the throttling portions 312 can be optimized. This makes it possible to realize a liquid ejection head 3 with excellent ejection performance. On the other hand, there is a disadvantage in that the processing of the throttling portions 312 is difficult, making it difficult to realize.
[0046] 1-4. Manufacturing method of the communication plate 31 FIG. 6 is a diagram showing the flow of a method for manufacturing the communicating plate 31 shown in FIG. 3. The liquid ejection head manufacturing method includes a method for manufacturing the communicating plate 31. As shown in FIG. 6, the method for manufacturing the communicating plate 31 includes a first step S1 and a second step S2. In the first step S1, metal-assisted chemical etching is used, which will be described later. Metal-assisted chemical etching is abbreviated as MACE. By using metal-assisted chemical etching, it is possible to realize the narrowed portion 312 having a configuration that is difficult to process by conventional methods. The method for manufacturing the communicating plate 31 includes a method for manufacturing the narrowed portion 312.
[0047] Fig. 7 is a diagram showing the flow of the first step S1 shown in Fig. 6. As shown in Fig. 7, the first step S1 includes an oxide film forming step S10, a protective film forming step S11, a resist layer forming step S12, a resist layer patterning step S13, an oxide film etching step S14, a metal film forming step S15, a resist layer removing step S16, and a metal-assisted chemical etching step S17.
[0048] 8 is a diagram for explaining the oxide film forming step S10 to the resist layer patterning step S13 in FIG. 7. First, a semiconductor substrate 31a such as an N-type single crystal silicon substrate with a crystal orientation of 100 is prepared as a base material for the communicating plate 31. The semiconductor substrate 31a has a first surface 301 and a second surface 302. The second surface 302 is the surface opposite to the first surface 301.
[0049] Fig. 8(a) is a diagram for explaining the oxide film forming step S10. As shown in Fig. 8(a), in the oxide film forming step S10, an oxide film 41 is formed on the first surface 301 of the semiconductor substrate 31a. Specifically, the oxide film 41 is a silicon oxide film. For example, the oxide film 41 is formed by a chemical vapor deposition (CVD) method or thermal oxidation. The thickness of the oxide film 41 is not particularly limited, but is, for example, 0.02 µm or more and 0.2 µm or less.
[0050] Fig. 8(b) is a diagram for explaining the protective film forming step S11. As shown in Fig. 8(b), in the protective film forming step S11, a protective film 42 is formed on the second surface 302 of the semiconductor substrate 31a. The protective film 42 is made of, for example, diamond-like carbon or the like. Diamond-like carbon is abbreviated as DLC. For example, the protective film 42 is formed by a CVD method or a sputtering method.
[0051] Fig. 8(c) is a diagram for explaining the resist layer forming step S12. As shown in Fig. 8(c), in the resist layer forming step S12, a resist layer 43 is formed on the first surface 301 of the semiconductor substrate 31a. Specifically, the resist layer 43 is formed on the oxide film 41 formed on the first surface 301. A resist is applied onto the oxide film 41, and the resist layer 43 is formed on the oxide film 41 by utilizing centrifugal force. The thickness of the resist layer 43 is not particularly limited, but is, for example, 1 µm or more and 3 µm or less.
[0052] 8(d) and 8(e) are diagrams for explaining the resist layer patterning step S13. As shown in FIG. 8(d), in the resist layer patterning step S13, the resist layer 43 is patterned by removing a part of the resist layer 43.
[0053] The first surface 301 of the semiconductor substrate 31a includes a first portion 3011, a second portion 3012, a third portion 3013, and a sixth portion 3014. The first portion 3011 corresponds to the narrowed portion 312. The third portion 3013 corresponds to the communicating space Ra. The sixth portion 3014 corresponds to the communicating flow path 314. The second portion 3012 does not correspond to the narrowed portion 312, the communicating flow path 314, and the communicating space Ra. The first portion 3011, the third portion 3013, and the sixth portion 3014 are portions that are removed by metal-assisted chemical etching, which will be described later. The second portion 3012 is a portion that is not removed by metal-assisted chemical etching.
[0054] In the resist layer patterning step S13, the resist layer 43 is patterned so as to have openings in the first portion 3011, the third portion 3013, and the sixth portion 3014, and to have no opening in the second portion 3012.
[0055] 8(e), reflow baking is performed after the resist layer 43 is patterned. As a result, the surface of the patterned resist layer 43 in the Z2 direction is narrower than the surface in the Z1 direction due to surface tension.
[0056] FIG. 9 is a diagram for explaining the oxide film etching step S14 to the metal-assisted chemical etching step S17 in FIG.
[0057] Fig. 9(a) is a diagram for explaining the oxide film etching step S14. As shown in Fig. 9(a), in the oxide film etching step S14, a part of the oxide film 41 is removed by etching, thereby patterning the oxide film 41. For example, the part of the oxide film 41 is removed by wet etching using buffered hydrofluoric acid, using the resist layer 43 as a mask. Buffered hydrofluoric acid is abbreviated as BHF.
[0058] In the oxide film etching step S14, a gap G is formed between the first surface 301 and the resist layer 43. That is, in the oxide film etching step S14, a part of the oxide film 41 is removed to such an extent that the gap G is formed. In particular, when the semiconductor substrate 31a contains silicon, the gap G is easily formed by performing wet etching using hydrofluoric acid. In addition, by forming the gap G, the patterned oxide film 41 is covered with the patterned resist layer 43 in a plan view.
[0059] Fig. 9(b) is a diagram for explaining the metal film forming step S15. As shown in Fig. 9(b), in the metal film forming step S15, a metal film 44 is formed on the first surface 301 of the semiconductor substrate 31a. Specifically, the metal film 44 is formed on the resist layer 43 on the first surface 301. The metal film 44 is formed by, for example, a sputtering method or the like. The metal film 44 contains, for example, platinum, ruthenium, palladium, molybdenum, chromium, copper, tantalum, titanium, or iridium.
[0060] As described above, a gap G is formed between the first surface 301 and the resist layer 43. Therefore, the metal film 44 includes a portion 441 in contact with the first surface 301 and a portion 442 in contact with the resist layer 43. By providing the gap G, the portion 441 and the portion 442 are not continuous but are separated from each other.
[0061] 9(c) is a diagram for explaining the resist layer removal step S16. As shown in FIG. 9(c), in the resist layer removal step S16, the resist layer 43 is removed. Along with this removal, the portions 442 of the metal film 44 in contact with the resist layer 43 are also removed at the same time. As a result, the metal film 44 composed of a plurality of portions 441 is formed on the first surface 301.
[0062] The metal film 44 is formed on the surfaces of the first portion 3011, the third portion 3013, and the sixth portion 3014, but is not formed on the surface of the second portion 3012. Therefore, in a plan view, the metal film 44 overlaps the first portion 3011, the third portion 3013, and the sixth portion 3014, but does not overlap the second portion 3012. In addition, the metal film 44 is in contact with the first portion 3011, the third portion 3013, and the sixth portion 3014, but is not in contact with the second portion 3012.
[0063] 9(d) and (e) are diagrams for explaining the metal-assisted chemical etching step S17. As shown in FIG. 9(d), in the metal-assisted chemical etching step S17, a part of the semiconductor substrate 31a is removed by metal-assisted chemical etching. For example, metal-assisted chemical etching using a solvent containing hydrogen fluoride and an oxidizing agent is optimal.
[0064] In metal-assisted chemical etching, the following processes are repeated: oxidation of the semiconductor substrate 31a by the catalytic action of the material of the metal film 44, etching of the oxide of the semiconductor substrate 31a by a solvent, and adsorption of the metal film 44 and the semiconductor substrate 31a by Coulomb force. By repeating these processes, it is possible to form holes in the Z1 direction.
[0065] 9(e), after removing a portion of the semiconductor substrate 31a, the metal film 44 is removed. Furthermore, the oxide film 41 is removed by, for example, wet etching using buffered hydrofluoric acid. The protective film 42 is removed by, for example, plasma ashing. As a result, the narrowed portion 312, a portion of the communicating flow path 314, and the communicating space Ra are formed in the semiconductor substrate 31a.
[0066] 10 is a diagram for explaining the metal-assisted chemical etching step S17. As shown in FIG. 10(a), the above-mentioned metal film 44 has a plurality of through holes H. Each through hole H penetrates the metal film 44 in the Z1 direction. The plurality of through holes H are provided by making the metal film 44 porous, and may be formed in the resist layer removal step S16, or may be formed in the metal film 44 formed in the metal film formation step S15. In the following, the metal-assisted chemical etching will be explained using an example in which a solvent containing hydrogen fluoride and an oxidizing agent is used.
[0067] As shown in FIG. 10(a), hydrogen fluoride contained in the solvent reacts with the metal film 44, and the semiconductor substrate 31a is oxidized by the catalytic action of the material of the metal film 44. As a result, an oxide of the semiconductor substrate 31a is formed. As shown by the arrows in FIG. 10(b), the solvent moves through the through holes H of the metal film 44. The solvent penetrates between the semiconductor substrate 31a and the metal film 44 from the through holes H. The oxide of the semiconductor substrate 31a is dissolved by the oxidizing agent contained in the penetrating solvent. As shown in FIG. 10(c), the metal film 44 is adsorbed to the semiconductor substrate 31a due to the Coulomb force between the metal film 44 and the semiconductor substrate 31a. The states shown in FIG. 10(a), (b), and (c) are repeated to form holes in the Z1 direction.
[0068] Fig. 11 is a diagram showing the flow of the second step S2 shown in Fig. 6. The second step S2 includes a second oxide film forming step S20, a second protective film forming step S21, a second resist layer forming step S22, a second resist layer patterning step S23, a second oxide film etching step S24, a second metal film forming step S25, a second resist layer removing step S26, and a metal-assisted chemical etching step S27.
[0069] FIG. 12 is a diagram for explaining the second oxide film forming step S20 to the second resist layer patterning step S23 in FIG. 11. FIG. 12(a) is a diagram for explaining the second oxide film forming step S20. As shown in FIG. 12(a), in the second oxide film forming step S20, a second oxide film 51 is formed on the entire outer surface of the semiconductor substrate 31a. Specifically, the second oxide film 51 is a silicon oxide film. Therefore, the second oxide film 51 is formed on the first surface 301 and the second surface 302 of the semiconductor substrate 31a. For example, the second oxide film 51 is formed by a CVD method or thermal oxidation. The thickness of the second oxide film 51 is not particularly limited, but is, for example, 0.2 μm or more and 1.0 μm or less.
[0070] Fig. 12(b) is a diagram for explaining the second protective film forming step S21. As shown in Fig. 12(b), in the second protective film forming step S21, the second protective film 52 is formed on the first surface 301 of the semiconductor substrate 31a. Specifically, the second protective film 52 is formed on the second oxide film 51 on the first surface 301. The second protective film 52 is made of, for example, diamond-like carbon, or a resist having high chemical resistance, or a multi-layer film thereof. For example, the second protective film 52 is formed by a CVD method, a sputtering method, or a spin coating method.
[0071] Fig. 12(c) is a diagram for explaining the second resist layer forming step S22. As shown in Fig. 12(c), in the second resist layer forming step S22, a second resist layer 53 is formed on the second surface 302 of the semiconductor substrate 31a. Specifically, the second resist layer 53 is formed on the second oxide film 51 formed on the second surface 302. A resist is applied onto the second oxide film 51, and the second resist layer 53 is formed on the second oxide film 51 by utilizing centrifugal force. The thickness of the second resist layer 53 is not particularly limited, but is, for example, 1 µm or more and 3 µm or less.
[0072] 12(d) and 12(e) are diagrams for explaining the second resist layer patterning step S23. As shown in FIG. 12(d), in the second resist layer patterning step S23, the second resist layer 53 is patterned by removing a part of the second resist layer 53.
[0073] The second surface 302 of the semiconductor substrate 31a includes a fourth portion 3021, a fifth portion 3022, and a seventh portion 3023. The fourth portion 3021 is a portion corresponding to the communicating space Ra, the common flow path Rb, and the communicating flow path 314. The seventh portion 3023 is a portion corresponding to the communicating flow path 314. The fifth portion 3022 is a portion not corresponding to the communicating flow path 314 and the communicating space Ra. The fourth portion 3021 and the seventh portion 3023 are portions that are removed by metal-assisted chemical etching, which will be described later. The fifth portion 3022 is a portion that is not removed by metal-assisted chemical etching.
[0074] In the second resist layer patterning step S23, the resist layer 43 is patterned so that openings are formed in the fourth portion 3021 and the seventh portion 3023 and so that an opening is not formed in the fifth portion 3022.
[0075] 12(e), the second resist layer 53 is patterned and then reflow baked. As a result, the patterned second resist layer 53 has a surface area in the Z1 direction narrower than a surface area in the Z2 direction due to surface tension.
[0076] FIG. 13 is a diagram for explaining the second oxide film etching step S24 to the metal-assisted chemical etching step S27 in FIG.
[0077] Fig. 13(a) is a diagram for explaining the second oxide film etching step S24. As shown in Fig. 13(a), in the second oxide film etching step S24, a part of the second oxide film 51 is removed by etching, thereby patterning the second oxide film 51. For example, the part of the second oxide film 51 is removed by wet etching using buffered hydrofluoric acid, using the second resist layer 53 as a mask.
[0078] In the second oxide film etching step S24, a gap G is formed between the second surface 302 and the second resist layer 53. That is, in the second oxide film etching step S24, a part of the second oxide film 51 is removed to such an extent that the gap G is formed. In particular, when the semiconductor substrate 31a contains silicon, the gap G is easily formed by performing wet etching using hydrofluoric acid.
[0079] Fig. 13(b) is a diagram for explaining the second metal film forming step S25. As shown in Fig. 13(b), in the second metal film forming step S25, a second metal film 54 is formed on the second surface 302 of the semiconductor substrate 31a. Specifically, the second metal film 54 is formed on the second resist layer 53 on the second surface 302. The second metal film 54 is formed by, for example, a sputtering method. The second metal film 54 contains, for example, platinum, ruthenium, platinum, palladium, molybdenum, chromium, copper, tantalum, titanium, or iridium.
[0080] As described above, a gap G is formed between the second surface 302 and the second resist layer 53. Therefore, the second metal film 54 includes a portion 541 in contact with the second surface 302 and a portion 542 in contact with the second resist layer 53. By providing the gap G, the portion 541 and the portion 542 are not continuous but are separated from each other.
[0081] 13(c) is a diagram for explaining the second resist layer removal step S26. As shown in FIG. 13(c), in the second resist layer removal step S26, the second resist layer 53 is removed. With this removal, the portions 542 of the second metal film 54 in contact with the second resist layer 53 are also removed at the same time. As a result, the second metal film 54 composed of the multiple portions 541 is formed on the second surface 302.
[0082] The second metal film 54 is formed on the surfaces of the fourth portion 3021 and the seventh portion 3023, but is not formed on the surface of the fifth portion 3022. Therefore, in a plan view, the second metal film 54 overlaps the fourth portion 3021 and the seventh portion 3023, but does not overlap the fifth portion 3022. In addition, the second metal film 54 is in contact with the fourth portion 3021 and the seventh portion 3023, but is not in contact with the fifth portion 3052.
[0083] 13(d) and (e) are diagrams for explaining the metal-assisted chemical etching step S27. As shown in FIG. 13(d), in the metal-assisted chemical etching step S27, a part of the semiconductor substrate 31a is removed by metal-assisted chemical etching. For example, metal-assisted chemical etching using a solvent containing hydrogen fluoride and an oxidizing agent is optimal.
[0084] In the metal-assisted chemical etching, the following processes are repeated: oxidation of the semiconductor substrate 31a by the catalytic action of the material of the second metal film 54, etching of the oxide of the semiconductor substrate 31a by a solvent, and adsorption of the second metal film 54 and the semiconductor substrate 31a by Coulomb force. By repeating these processes, it is possible to form holes in the Z2 direction.
[0085] 13(e), after removing a portion of the semiconductor substrate 31a, the second metal film 54 is removed, whereby the remaining portion of the communication flow path 314 and the common flow path Rb are formed in the semiconductor substrate 31a.
[0086] In this manner, the communication plate 31 having the throttle portion 312, the communication flow passage 314, the common flow passage Rb, and the communication space Ra is manufactured.
[0087] As described above, the manufacturing method of the communicating plate 31 includes a first step S1 of forming the drawn portion 312 by performing metal-assisted chemical etching. In the first step S1, a metal film 44 is formed on the surface of a first portion 3011 corresponding to the drawn portion 312 of the first surface 301 of the semiconductor substrate 31a, and metal-assisted chemical etching is performed in a state in which the metal film 44 is not formed on the surface of a second portion 3012 not corresponding to the drawn portion 312 of the first surface 301. Thus, the metal film 44 is formed so as to be in contact with the first portion 3011, and is not in contact with the second portion 3012.
[0088] By using metal-assisted chemical etching, it is possible to finely process semiconductor through holes with a high aspect ratio, and the throttling portion 312 can be formed with high precision. In addition, dry etching, which processes each wafer, takes a huge amount of processing time, which may reduce productivity and investment efficiency in vacuum equipment for manufacturing. However, metal-assisted chemical etching makes it possible to etch a large number of wafers at once, and reduces the need for such a huge amount of processing time. In addition, it is difficult to control the aspect ratio of the throttling portion 312 with anisotropic wet etching along the crystal orientation, but metal-assisted chemical etching makes it easy to form the throttling portion 312 with the desired aspect ratio. Therefore, by using metal-assisted chemical etching, the throttling portion 312 of the through hole with the desired aspect ratio can be formed with high precision. Therefore, it is possible to realize the throttling portion 213 with a fine structure as in each of the above-mentioned embodiments. Therefore, it is possible to control the movement of the meniscus by the throttling portion 312, and it is possible to provide a liquid discharge head 3 that is small in size and has excellent discharge performance.
[0089] As described above, the first step S1 includes a resist layer forming step S12, a resist layer patterning step S13, and a metal film forming step S15. In the resist layer forming step S12, a resist layer 43 is formed on the first surface 301 of the semiconductor substrate 31a. In the resist layer patterning step S13, after the resist layer 43 is formed, the resist layer 43 is patterned so as to open in the first portion 3011 and not to open in the second portion 3012. In the metal film forming step S15, after the resist layer 43 is patterned, a metal film 44 is formed on the first surface 301.
[0090] By using the patterned resist layer 43, it is possible to form the metal film 44 corresponding to the first portion 3011 without touching the surface of the second portion 3012, which is a non-etching region, even once during the process. In other words, it is possible to form the metal film 44 only in the desired locations without diffusing and leaving metal at the atomic level in areas other than the desired locations where the metal film 44 is to be formed.
[0091] As described above, the first step S1 includes an oxide film forming step S10 and an oxide film etching step S14. In the oxide film forming step S10, an oxide film 41 is formed on the first surface 301 before forming a resist layer 43. Then, in a resist layer forming step S12, a resist layer 43 is formed on the oxide film 41. In addition, in the oxide film etching step S14, after patterning the resist layer 43 and before forming the metal film 44, the oxide film 41 is etched to open a portion of the oxide film 41 above the first portion 3011.
[0092] Therefore, an oxide film 41 is formed between the first surface 301 and the resist layer 43. The formation of the oxide film 41 facilitates peeling of the resist layer 43 from the oxide film 41 in a later step, i.e., patterning of the metal film 44 on the surface of the first surface 301 by resist peeling. Specifically, each of the resist layer 43 and the oxide film 41 has an opening in the first portion 3011, which facilitates the formation of the metal film 44 corresponding to the first portion 3011, as described above.
[0093] Furthermore, in the oxide film etching step S14, the oxide film 41 is etched to form a gap G between the first surface 301 and the resist layer 43. The formation of the gap G makes it easier to pattern the metal film 44 in a later step compared to a case where the gap G is not formed. The provision of the gap G allows the metal film 44 to be separated into a portion 441 in contact with the first surface 301 and a portion 442 in contact with the resist layer 43 during the formation of the metal film 44, and the metal film 44 can be easily divided while keeping its outline clear when the resist layer 43 is peeled off.
[0094] The first step S1 includes a resist layer removal step S16. In the resist layer removal step S16, the metal film 44 is formed on the first surface 301, and then the resist layer 43 is removed. By removing the resist layer 43 as described above, the metal film 44 composed of the portions 442 is formed on the first surface 301. This makes it possible to easily form a patterned metal film 44. Even if the metal film 44 has a fine shape, this method makes it possible to easily and highly accurately form the metal film 44 having a desired shape and arrangement pattern.
[0095] In the first step S1, it is preferable to perform metal-assisted chemical etching using a solvent containing hydrogen fluoride and an oxidizing agent. By using hydrogen fluoride, oxides on the semiconductor substrate 31a can be easily removed by etching. By using an oxidizing agent, the semiconductor substrate 31a can be oxidized using the metal film 44 as a catalyst. Therefore, the metal-assisted chemical etching can be performed efficiently.
[0096] The oxidizing agent is not particularly limited, but may be, for example, hydrogen peroxide (H2O2) or nitric acid (HNO3). In particular, when the semiconductor substrate 31a contains silicon oxide, the oxidizing agent is preferably hydrogen peroxide for efficient formation of an oxide of the semiconductor substrate 31a. The type of the solvent is not limited to one containing hydrogen fluoride and an oxidizing agent.
[0097] As described above, the metal film 44 contains, for example, platinum, ruthenium, palladium, molybdenum, chromium, copper, tantalum, titanium, or iridium. Among these, the metal film 44 is preferably made of gold. This is because gold is particularly excellent in catalytic reactions. Furthermore, when the oxidizing agent contained in the solvent is hydrogen peroxide, the catalytic reaction of gold can be suitably exhibited.
[0098] The semiconductor substrate 31a is not particularly limited as long as it is a substrate containing a semiconductor material, but is preferably a silicon substrate, and is particularly preferably an N-type single crystal silicon substrate. By adopting the N-type, metal-assisted chemical etching can be efficiently performed by the action of carrier electrons. In addition, even with a high etching rate, surface roughness is unlikely to occur, and the substrate is of high quality.
[0099] As described above, in the first step S1, in addition to the first portion 3011, the metal film 44 is formed on the third portion 3013 of the first surface 301 corresponding to the communicating space Ra, and then metal-assisted chemical etching is performed to form the throttling portion 312 and the communicating space Ra. With metal-assisted chemical etching, the difference in etching rate due to the difference in the planar section formation area of the etching pattern, that is, the microloading effect, does not occur as in dry etching, so that the throttling portion 312 and the communicating space Ra can be easily and quickly formed all at once. In other words, holes with different cross-sectional areas parallel to the XY plane can be easily and quickly formed all at once. This allows the processing time to be shortened.
[0100] The manufacturing method of the communication plate 31 also includes a second step S2 of forming the common flow path Rb by performing metal-assisted chemical etching. In the second step S2, the second metal film 54 is formed on the surface of the fourth portion 3021 of the second surface 302 of the semiconductor substrate 31a, which corresponds to the common flow path Rb, and the metal-assisted chemical etching is performed in a state in which the second metal film 54 is not formed on the surface of the fifth portion 3022 of the second surface 302, which does not correspond to the common flow path Rb. Thus, the second metal film 54 is formed so as to be in contact with the fourth portion 3021, and is not in contact with the fifth portion 3022.
[0101] By using metal-assisted chemical etching, it is possible to form the common flow path Rb with high precision as a laminated flow path structure having a free planar shape that communicates with the communication space Ra and the throttle portion 312. Therefore, it is possible to realize a liquid ejection head 3 that is small in size and has excellent ejection performance.
[0102] In the manufacturing method of the communication plate 31, the first step S1 and the second step S2 are performed in this order, and the narrowed portion 312 and the common flow path Rb are directly connected. By using metal-assisted chemical etching, processing with high positional accuracy is realized. Therefore, by processing the first surface 301 and the second surface 302 in order, it is possible to directly connect the narrowed portion 312 and the common flow path Rb, and the common flow path Rb and the communication space Ra at the same time.
[0103] 2. Second embodiment The second embodiment will be described below. In the following example, for elements having the same actions and functions as those in the first embodiment, the reference numerals used in the description of the first embodiment will be used and detailed descriptions of each will be omitted as appropriate.
[0104] FIG. 14 is a diagram for explaining the first step S1 of the second embodiment. FIG. 14 shows the resist layer removal step S16 and the metal-assisted chemical etching step S17. In this embodiment, an SOI substrate is used as the semiconductor substrate 31b. The specifications of the SOI substrate are not particularly limited. For example, the semiconductor substrate 31b is a laminate of an N-type single crystal silicon substrate 303 with a crystal orientation of 100, a silicon oxide film 304, and a P-type single crystal silicon substrate 305 with a crystal orientation of 110. By making the specifications of the SOI substrate the same as the example, the N-type single crystal silicon substrate 303 with a crystal orientation of 100 of the SOI substrate can be processed into uniform and vertical silicon holes by MACE, and the P-type single crystal silicon substrate 305 with a crystal orientation of 110 can be processed into silicon grooves with high accuracy by anisotropic wet etching that configures the channel walls with 111 faces. Thus, the specifications of the SOI substrate can be configured to enable optimal silicon processing that can create the respective channel shapes and dimensions.
[0105] 14(a) is a diagram for explaining the resist layer removal step S16, and shows the state after removal of the resist layer 43. As in the first embodiment, a portion 412 that is a part of the metal film 44 on the resist layer 43 is removed together with the resist layer 43, so that a metal film 44 composed of a plurality of portions 441 is formed on the first surface 301.
[0106] 14(b) and (c) are diagrams for explaining the metal-assisted chemical etching step S17. As shown in FIG. 14(b), similar to the first embodiment, the N-type single crystal silicon substrate 303, which is a part of the semiconductor substrate 31b, is removed by metal-assisted chemical etching. At this time, the metal-assisted chemical etching is performed until the silicon oxide film 304 is reached. As shown in FIG. 14(c), after the part of the semiconductor substrate 31b is removed, the metal film 44 is removed. As a result, similar to the first embodiment, the narrowed portion 312, a part of the communicating flow path 314, and the communicating space Ra are formed in the semiconductor substrate 31b.
[0107] Fig. 15 is a diagram showing the flow of the second step S2 of the second embodiment. In Fig. 15, the second step S2 of the first embodiment includes a wet etching step S28 and a second oxide film removal step S29, instead of the second metal film formation step S25, the second resist layer removal step S26, and the metal-assisted chemical etching step S27. In this embodiment, the second protective film formation step S21 may be omitted.
[0108] Fig. 16 is a diagram for explaining the second step S2 of the second embodiment. Fig. 16(a) is a diagram for explaining the second resist layer patterning step S23. Prior to this step, similarly to the first embodiment, a second oxide film 51 is formed on the entire outer surface of the semiconductor substrate 31b. Then, a second protective film 52 is formed on the second oxide film 51 formed on the first surface 301. Then, a second resist layer 53 is formed on the second oxide film 51 formed on the second surface 302. Then, in this step, the second resist layer 53 is patterned by removing a part of the second resist layer 53.
[0109] Similar to the first embodiment, the second surface 302 of the semiconductor substrate 31b includes a fourth portion 3021, a fifth portion 3022, and a seventh portion 3023. In the second resist layer patterning step S23, the resist layer 43 is patterned so as to be open at the fourth portion 3021 and the seventh portion 3023, and not to be open at the fifth portion 3022. In this embodiment, reflow baking is omitted.
[0110] Fig. 16(b) is a diagram for explaining the second oxide film etching step S24. As shown in Fig. 16(b), in the second oxide film etching step S24, a part of the second oxide film 51 is removed by etching, thereby patterning the second oxide film 51. For example, the second oxide film 51 is partly removed by wet etching using buffered hydrofluoric acid, using the resist layer 43 as a mask. After the second oxide film 51 is patterned, the second resist layer 53 is removed.
[0111] In this step, the second oxide film 51 is not formed on the fourth portion 3021 and the seventh portion 3023, but is formed on the fifth portion 3022. Therefore, in a plan view, the second oxide film 51 does not overlap the fourth portion 3021 and the seventh portion 3023, but overlaps the fifth portion 3022.
[0112] Fig. 16(c) is a diagram for explaining the wet etching step S28. In the wet etching step S28 shown in Fig. 16(c), the P-type single crystal silicon substrate 305, which is a part of the semiconductor substrate 31b, is removed by wet etching using, for example, potassium hydroxide.
[0113] Fig. 16(d) is a diagram for explaining the second oxide film removal step S29. As shown in Fig. 16(d), after removing a portion of the semiconductor substrate 31b, the second oxide film 51 is removed. At the same time as removing the second oxide film 51, a portion of the silicon oxide film 304 of the semiconductor substrate 31b is removed. For example, the second oxide film 51 and a portion of the silicon oxide film 304 are removed by wet etching using buffered hydrofluoric acid. As a result, the narrowed portion 312, the remaining portion of the communicating flow path 314, and the communicating space Ra are formed in the semiconductor substrate 31b.
[0114] In this manner, the communication plate 31 having the throttle portion 312, the communication flow passage 314, the common flow passage Rb, and the communication space Ra is manufactured.
[0115] As described above, in the second step S2, the second oxide film 51 is not formed on the fourth portion 3021 corresponding to the common flow path Rb of the second surface 302 of the semiconductor substrate 31b, and the second oxide film 51 is formed on the fifth portion 3022 of the second surface 302 not corresponding to the common flow path Rb, and wet etching is performed. As a result, the common flow path Rb is formed. The cross-sectional area of the common flow path Rb along the Z1 direction is larger than the cross-sectional area of the throttle portion 312 along the Z1 direction. Therefore, the flow path can be formed by a highly accurate flow path wall using crystal anisotropic wet etching without using metal-assisted chemical etching suitable for microfabrication. Therefore, the common flow path Rb can be easily and quickly formed by a flow path formation method that is optimal for each flow path configuration, and the flow path structure 30 including the throttle portion 312 can be formed.
[0116] In addition, since the etching of each is stopped by the silicon oxide film 304 of the SOI substrate, the dimension along the Z axis can be determined by the thickness of each of the single crystal silicon substrates 303, 305 constituting the SOI substrate, so that by increasing the thickness precision of the SOI substrate, it becomes possible to form the dimensions of the flow path with high precision. That is, it becomes possible to form the length of the throttle portion 312 in the Z1 direction with high precision, and a highly accurate flow path resistance can be created. At the same time, the depth of the common flow path Rb can also be finished with high precision in the Z2 direction, and a small and highly accurate flow path structure 30 can be realized.
[0117] 3. Third embodiment The third embodiment will be described below. In the following exemplary embodiment, for elements having the same actions and functions as those in the first embodiment, the reference numerals used in the description of the first embodiment will be used and detailed descriptions of each will be omitted as appropriate.
[0118] 17 is a diagram showing the flow of a manufacturing method of the communicating plate 31 of the third embodiment. As shown in FIG. 17, this embodiment further includes a third step S3. In the first step S1, similar to the first embodiment, the narrowed portion 312, a part of the communicating flow path 314, and the communicating space Ra are formed in the semiconductor substrate 31a. Although not shown, in the second step S2, a semiconductor substrate 31c separate from the semiconductor substrate 31a is prepared. Then, in the second step S2, similar to the first embodiment, the remaining part of the communicating flow path 314 and the common flow path Rb are formed in the semiconductor substrate 31c.
[0119] Fig. 18 is a diagram showing the flow of the third step S3 of the third embodiment. As shown in Fig. 18, the third step S3 includes a bonding step S30, a polishing step S31, a third oxide film forming step S32, a third oxide film etching step S33, a wet etching step S34, and a third oxide film removing step S35.
[0120] 19 and 20 are diagrams for explaining the third step S3 of the third embodiment. FIG. 19(a) is a diagram for explaining the bonding step S30. As shown in FIG. 19(a), in the bonding step S30, a semiconductor substrate 31a of the first step S1 and a semiconductor substrate 31b of the second step S2 are bonded together to form a structure 31d. For example, when each of the semiconductor substrates 31a and 31c is a silicon substrate, they are bonded together by silicon direct bonding.
[0121] Fig. 19(b) is a diagram for explaining the polishing step S31. As shown in Fig. 19(b), in the polishing step S31, polishing is performed from the semiconductor substrate 31b side of the structure 31d. As a result, a part of the structure 31d is removed.
[0122] Fig. 19(c) is a diagram for explaining the third oxide film forming step S32. As shown in Fig. 19(c), in the third oxide film forming step S32, a third oxide film 61 is formed on the outer surface of the structure 31d. For example, the third oxide film 61 is formed by thermal oxidation.
[0123] Fig. 19(d) is a diagram for explaining the third oxide film etching step S33. As shown in Fig. 19(d), in the third oxide film etching step S33, the third oxide film 61 formed on the semiconductor substrate 31a side of the structure 31d is removed by etching. For example, it is removed by buffered hydrofluoric acid.
[0124] Fig. 20(a) is a diagram for explaining the wet etching step S34. As shown in Fig. 20(a), in the wet etching step S34, for example, the third oxide film 61 is used as a mask to remove the semiconductor substrate 31a side of the structure 31d by wet etching using potassium hydroxide.
[0125] Fig. 20(b) is a diagram for explaining the third oxide film removal step S35. As shown in Fig. 20(b), in the third oxide film removal step S35, for example, the third oxide film 61 is removed by wet etching using buffered hydrofluoric acid. In this manner, the communication plate 31 having the narrowed portion 312, the communication flow path 314, the common flow path Rb, and the communication space Ra is manufactured.
[0126] In this embodiment, too, metal-assisted chemical etching is used in the first step S1 and the second step S2, which allows the narrowed portion 312 to be formed with high precision.
[0127] 4. Manufacturing method of liquid ejection head 3 21 is a diagram showing the flow of a manufacturing method of the liquid ejection head 3. As described above, the liquid ejection head 3 has a pressure chamber substrate 32 including a pressure chamber C1, a communication plate 31 laminated on the pressure chamber substrate 32 and including a throttle portion 312 and a common flow path Rb, and a nozzle substrate 37 laminated on the communication plate 31 and including a nozzle N. In the example of the first embodiment, the communication plate 31 is formed from a semiconductor substrate 31a,
[0128] In the example shown in FIG. 21, in step SS1, a pressure chamber substrate wafer including a plurality of pressure chamber substrates 32, a nozzle substrate wafer including a plurality of nozzle substrates 37, and a communicating plate wafer including a plurality of communicating plates 31 are each formed individually. In step SS2, these wafers are directly bonded together. Thereafter, a liquid protective layer is formed on the wall surfaces that form each flow path including the throttle portion 312 and the common flow path Rb. Note that the liquid protective layer may be formed before the direct bonding. Also, in step SS3, a sealing substrate wafer including a plurality of sealing substrates 35 is formed, and a liquid protective layer is formed on each flow path including the communicating space Ra, etc.
[0129] The liquid protective layer includes, for example, tantalum oxide or hafnium oxide. The chemical formula of tantalum oxide is represented by TaOx. The chemical formula of hafnium oxide is represented by HfOx. The liquid protective layer is formed, for example, by an ALD (Atomic Layer Deposition) method.
[0130] In step SS4, a sealing substrate wafer is bonded to the pressure chamber substrate wafer, nozzle substrate wafer, and communicating plate wafer to manufacture a structure including these wafers. In step SS5, the structure is cut into chips by laser scrubbing or the like. In step SS6, the chips are mounted on the mounting pads by COF. COF stands for Chip On Film. Then, in step SS7, the vibration absorber 38, housing 36, and case parts such as ink piping parts are assembled by bonding or the like. This results in the liquid ejection head 3.
[0131] 5. Variations The above-described embodiment may be modified in various ways. Specific modified aspects that may be applied to the above-described embodiment are illustrated below. Two or more aspects selected from the following examples may be combined as appropriate to the extent that they are not mutually contradictory.
[0132] The liquid ejection head 3 may be a so-called circulation type head. In this case, the liquid ejection head 3 further includes a circulation mechanism 26. In this case, the throttle section 312 functions as a supply port, but may also function as a discharge port.
[0133] The metal film 44 is formed by a sputtering method or the like, but may be formed by electroless plating. In this case, the formation of the oxide film 41 may be omitted. A resist film is used as a mask.
[0134] The liquid ejection device 1 exemplified in the first embodiment can be adopted in various devices such as facsimile machines and copy machines, in addition to devices dedicated to printing. The use of the liquid ejection device is not limited to printing. For example, a liquid ejection device that ejects a solution of a color material is used as a manufacturing device that forms a color filter of a display device such as a liquid crystal display panel. Also, a liquid ejection device that ejects a solution of a conductive material is used as a manufacturing device that forms wiring and electrodes of a wiring board. Also, a liquid ejection device that ejects a solution of an organic matter related to a living body is used as a manufacturing device that manufactures, for example, a biochip. [Explanation of symbols]
[0135] 1...liquid ejection device, 3...liquid ejection head, 12...medium, 14...liquid container, 20...control unit, 22...transport mechanism, 24...movement mechanism, 30...flow path structure, 31...communicating plate, 31a...semiconductor substrate, 31b...semiconductor substrate, 31c...semiconductor substrate, 31d...structure, 32...pressure chamber substrate, 33...diaphragm, 34...piezoelectric element, 35...sealing substrate, 36...casing, 37...nozzle substrate, 38...vibration absorber, 40...wiring substrate, 41...oxide film, 42...protective film, 43...resist layer, 44...metal film, 51...second oxide film, 52...second protective film, 53...second resist layer, 54...second metal film, 61...third Oxide film, 100...crystal orientation, 110...crystal orientation, 213...throttled portion, 242...transport body, 244...transport belt, 300...individual flow path, 301...first surface, 302...second surface, 303...N-type single crystal silicon substrate, 304...silicon oxide film, 305...P-type single crystal silicon, 312...throttled portion, 314...communicating flow path, 320...wall surface, 361...supply port, 412...portion, 441...portion, 442...portion, 541...portion, 542...portion, 3011...first portion, 3012...second portion, 3013...third portion, 3014...sixth portion, 3021...fourth portion, 3022...fifth portion, 3023...seventh Part, C1...pressure chamber, G...gap, H...through hole, La...first row, Lb...second row, N...nozzle, R...common space, Ra...communicating space, Rb...common flow path, Rc...space, S1...first step, S10...oxide film forming step, S11...protective film forming step, S12...resist layer forming step, S13...resist layer patterning step, S14...oxide film etching step, S15...metal film forming step, S16...resist layer removing step, S17...metal-assisted chemical etching step, S2...second step, S20...second oxide film forming step, S21...second protective film forming step, S22...second resist layer forming step, S2 3... second resist layer patterning step, S24... second oxide film etching step, S25... second metal film formation step, S26... second resist layer removal step, S27... metal-assisted chemical etching step, S28... wet etching step, S29... second oxide film removal step, S3... third step, S30... bonding step, S31... polishing step, S32... third oxide film formation step, S33... third oxide film etching step, S34... wet etching step, S35... third oxide film removal step, SS1... step, SS2... step, SS3... step, SS4... step, SS5... step,SS6... Step, SS7... Step.
Claims
1. A method for manufacturing a liquid ejection head having a plurality of individual flow paths, each of which has a pressure chamber extending in a first direction, a nozzle communicating with one end of the pressure chamber, and a throttle portion communicating with the other end of the pressure chamber, extending in a second direction intersecting the first direction, and having a smaller cross-sectional area than the pressure chamber, and a common flow path commonly communicating with the plurality of individual flow paths, comprising: The method includes a first step of forming a metal film on a first portion of a first surface of a semiconductor substrate, the first portion corresponding to the drawn portion, and performing metal-assisted chemical etching in a state in which the metal film is not formed on a second portion of the first surface that does not correspond to the drawn portion, thereby forming the drawn portion. A method for manufacturing a liquid ejection head.
2. The first step comprises: forming a resist layer on the first surface; After forming the resist layer, the resist layer is patterned so as to have an opening in the first portion and no opening in the second portion; forming the metal film on the first surface after patterning the resist layer; 2. The method for manufacturing a liquid ejection head according to claim 1.
3. forming an oxide film on the first surface before forming the resist layer; forming a resist layer on the oxide film; after patterning the resist layer and before forming the metal film, etching the oxide film to open a portion of the oxide film above the first portion; 3. The method for manufacturing a liquid ejection head according to claim 2.
4. forming a gap between the first surface and the resist layer by etching the oxide film; 4. The method for manufacturing a liquid ejection head according to claim 3.
5. In the first step, After forming the metal film on the first surface, the resist layer is removed.
3. The method for manufacturing a liquid ejection head according to claim 2.
6. In the first step, the metal-assisted chemical etching is performed using a solvent containing hydrogen fluoride and an oxidizing agent.
2. The method for manufacturing a liquid ejection head according to claim 1.
7. The metal film is made of gold.
2. The method for manufacturing a liquid ejection head according to claim 1.
8. The nozzle further includes a communication space extending in the second direction and communicating the common flow path with an external flow path, In the first step, the metal film is formed on the first portion and on a third portion of the first surface corresponding to the communication space, and the metal-assisted chemical etching is performed to form the narrowed portion and the communication space.
2. The method for manufacturing a liquid ejection head according to claim 1.
9. a second step of forming a second metal film on a fourth partial surface of a second surface of the semiconductor substrate opposite to the first surface, the fourth partial surface corresponding to the common flow path, and performing metal-assisted chemical etching in a state in which the second metal film is not formed on a fifth partial surface of the second surface not corresponding to the common flow path, to form the common flow path; 2. The method for manufacturing a liquid ejection head according to claim 1.
10. 10. The method of manufacturing a liquid ejection head according to claim 9, wherein the first step and the second step are carried out in that order, and the restrictor portion and the common flow path are directly connected to each other.
11. a second step of forming a second oxide film on a fourth portion of a second surface of the semiconductor substrate opposite to the first surface, the fourth portion corresponding to the common flow path, and performing wet etching in a state in which the second oxide film is not formed on a fifth portion of the second surface not corresponding to the common flow path, to form the common flow path; 2. The method for manufacturing a liquid ejection head according to claim 1.
12. a pressure chamber substrate including the pressure chamber; a communication plate that is laminated on the pressure chamber substrate and includes the throttle portion and the common flow path; a nozzle substrate laminated on the communication plate and including the nozzle; The communication plate is formed from the semiconductor substrate.
2. The method for manufacturing a liquid ejection head according to claim 1.
Citation Information
Patent Citations
Liquid droplet-delivering head, liquid droplet-delivering apparatus, method for manufacturing liquid droplet-delivering head and method for manufacturing liquid droplet-delivering apparatus
JP2007331167A
Liquid discharge device
JP2019107902A