All-solid battery
By integrating expanded metal within the electrode mixture layers with defined angles and orientations, the internal resistance of all-solid-state batteries is substantially reduced, improving their efficiency.
Patent Information
- Application Number
- JP2023051286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
All-solid-state batteries exhibit excessively high internal resistance, necessitating a reduction to enhance performance.
Incorporating expanded metal within the electrode mixture layers of all-solid-state batteries, with specific geometric configurations and orientations relative to the solid electrolyte layer, to increase the contact area and improve conductivity.
The configuration results in an all-solid-state battery with significantly reduced internal resistance, enhancing overall performance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery. [Background technology]
[0002] In recent years, electronics technology has made remarkable progress, and efforts are being made to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries, which serve as the power source for electronic devices, to be smaller, lighter, thinner, and more reliable. Thus, attention is being paid to all-solid-state batteries that use a solid electrolyte as the electrolyte. Conventionally, oxide-based solid electrolytes, complex hydride-based solid electrolytes, and the like are known as solid electrolytes for all-solid-state batteries (for example, Patent Document 1).
[0003] In Patent Document 1, a non-flammable solid electrolyte having the general formula Li 1+x M III x Ti IV 2-x (PO4)3(where 0≦x≦0.6, M III An all-solid-state battery is disclosed that includes a solid electrolyte represented by the formula (I): at least one metal ion selected from the group consisting of Al, Y, Ga, In, and La). This all-solid-state lithium secondary battery includes an active material layer and a solid electrolyte layer bonded to the active material layer by sintering, the active material layer includes a crystalline first material capable of absorbing and releasing lithium ions, and the solid electrolyte layer includes a crystalline second material having lithium ion conductivity. It is also disclosed that the packing rate of the solid electrolyte layer is preferably more than 70%, and the battery is manufactured by sequentially stacking the materials constituting each layer and then sintering them.
[0004] As disclosed in Patent Document 1, it is considered preferable that the solid electrolyte included in the all-solid-state battery is dense.
[0005] On the other hand, it is known that expansion and contraction occurs during charging and discharging of an all-solid-state battery. A method for suppressing cracks in the electrode material of the all-solid-state battery caused by such expansion and contraction during charging and discharging has been studied (for example, Patent Document 2).
[0006] Patent Document 2 discloses a configuration in which a porous metal sheet, which is a metal foam or a sintered metal fiber compact, is provided on a solid electrolyte layer. The all-solid-state battery of Patent Document 2 is produced by a manufacturing method including a step of filling a porous metal sheet with an electrode material. Patent Document 2 discloses that the provision of this configuration can suppress cracks in the electrode material. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2007-005279 A [Patent Document 2] JP 2010-40218 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the all-solid-state batteries disclosed in Patent Documents 1 and 2, the internal resistance is excessively high, and there has been a demand for reducing the internal resistance. The present invention has been made in view of the above circumstances, and has an object to provide an all-solid-state battery with low internal resistance. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems. As a result, it was found that in the method of using a porous metal sheet in Patent Document 2, other materials are not densely formed in the voids inside the porous electrode sheet and around it. It was found that the internal resistance of an all-solid-state battery can be reduced when an expanded metal is provided in the electrode mixture layer and the area of the surface of the expanded metal that is away from the solid electrolyte layer is increased.
[0010] That is, in order to solve the above problems, the present invention provides the following means.
[0011] (1) An all-solid-state battery according to one aspect of the present invention includes a laminate in which a positive electrode mixture layer including a positive electrode active material and a negative electrode mixture layer including a negative electrode active material are laminated with a solid electrolyte layer interposed therebetween, at least one of the positive electrode mixture layer and the negative electrode mixture layer is an electrode mixture layer including an expanded metal and solid electrolyte particles, and in a cross section along a lamination direction of the laminate, the expanded metal is defined by a first side close to the solid electrolyte layer, a second side facing the first side, and a third side and a fourth side connecting the first side and the second side, and a smaller angle X of an angle between the second side and the third side and an angle between the second side and the fourth side satisfies 20°≦X<90°.
[0012] (2) In the all-solid-state battery of (1) above, one of the third side and the fourth side may be inclined with respect to a direction perpendicular to the first side, and a slope (|ab| / c) of the slope (|ab| / c) may be greater than 0.01 and equal to or less than 3, where a is the length of the first side, b is the length of the second side, and c is the distance between the first side and the second side.
[0013] (3) In the all-solid-state batteries of (1) and (2) above, an angle between the second side and the third side and an angle between the second side and the fourth side may be in a range of 20° or more and less than 90°.
[0014] (4) In the all-solid-state batteries according to (1) to (3) above, the expanded metal may contain one or more selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon.
[0015] (5) In the all-solid-state batteries described above in (1) to (4), both the positive electrode mixture layer and the negative electrode mixture layer may contain the expanded metal and the solid electrolyte particles.
[0016] (6) In the all-solid-state batteries according to any one of (1) to (5) above, the angle of the expanded metal with respect to the interface between the electrode mixture layer and the solid electrolyte layer may be 0.5° or more and 15° or less. Effect of the Invention
[0017] According to the present invention, it is possible to provide an all-solid-state battery having low internal resistance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a perspective view showing an example of a configuration of an all-solid-state battery according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view of the all-solid-state battery of FIG. 1 cut along the stacking direction of the power storage element. [Diagram 3] 3 is an enlarged view of a region R1 surrounded by a two-dot chain line in the all-solid-state battery in FIG. 2. [Figure 4] 3 is a plan view showing an example of the configuration of an expanded metal provided in a positive electrode mixture layer in the all-solid-state battery of FIG. 2. [Diagram 5] FIG. 4 is an enlarged view of a region surrounded by a two-dot chain line in FIG. 3, showing a cross-sectional unit structure of the expanded metal. [Figure 6] FIG. 3 is an enlarged view of a region R2 surrounded by a two-dot chain line in the all-solid-state battery of FIG. 2. [Figure 7] FIG. 6 is a cross-sectional view showing a modification of FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the cathode active material layer, the cathode, and the all-solid-state battery of this embodiment will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may be enlarged to show the characteristic parts of the present invention for the sake of convenience in order to make the characteristics of the present invention easier to understand. Therefore, the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are examples, and the present invention is not limited to them, and can be appropriately changed and implemented within the scope that does not change the gist of the present invention.
[0020] [All-solid battery] Fig. 1 is a perspective view showing an example of the configuration of an all-solid-state battery according to one embodiment of the present invention. The all-solid-state battery 100 shown in Fig. 1 includes an energy storage element 10 and an exterior body 20. The energy storage element 10 is accommodated in an accommodation space K within the exterior body 20. For ease of understanding, Fig. 1 illustrates a state immediately before the energy storage element 10 is accommodated in the exterior body 20. The energy storage element 10 has external terminals 12, 14 that are electrically connected to the outside.
[0021] The exterior body 20 has, for example, a metal foil and a resin layer 24 laminated on both sides of the metal foil 22 (see FIG. 2). The exterior body 20 is a metal laminate film in which a metal foil is coated on both sides with a polymer film (resin layer). The metal foil 22 is, for example, an aluminum foil. The resin layer 24 is, for example, a polymer film such as polypropylene. The resin layer 24 may be different on the inside and outside. For example, the outside resin layer may be made of a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inside resin layer may be made of a material with high heat resistance, oxidation resistance, and reduction resistance, such as polyethylene (PE) or polypropylene (PP).
[0022] Fig. 2 is a cross-sectional view of the all-solid-state battery of Fig. 1 cut along the stacking direction of the storage element. The all-solid-state battery 100 shown in Fig. 2 includes a laminate 30 in which a positive electrode mixture layer 11B containing a positive electrode active material and a negative electrode mixture layer 13B containing a negative electrode active material are stacked via a solid electrolyte layer 15, and at least one of the positive electrode mixture layer 11B and the negative electrode mixture layer 13B is an electrode mixture layer containing an expanded metal and solid electrolyte particles. In a cross section along the stacking direction of the laminate 30, the expanded metal is defined by a first side M1 close to the solid electrolyte layer 15, a second side M2 facing the first side M1, and a third side M3 and a fourth side M4 connecting the first side M1 and the second side M2, and the smaller angle X of the angle X1 between the second side M2 and the third side S3 and the angle X2 between the second side M2 and the fourth side M4 satisfies 20°≦X<90° (see Fig. 5).
[0023] The all-solid-state battery 100 includes an energy storage element 10 and an exterior body 20. The exterior body 20 covers the periphery of the energy storage element 10. The energy storage element 10 is connected to the outside via a pair of connected external terminals 12, 14. The all-solid-state battery 100 may have any other shape as long as it is a laminated battery. For example, the all-solid-state battery 100 can be applied to a laminated battery, a square battery, a coin battery, a button battery, etc.
[0024] <Electricity storage element> The energy storage element 10 includes a solid electrolyte layer 15, a positive electrode layer 11, and a negative electrode layer 13. The energy storage element 10 is charged or discharged by the exchange of ions between the positive electrode layer 11 and the negative electrode layer 13 via the solid electrolyte layer 15 and the exchange of electrons via an external circuit.
[0025] (Positive electrode layer) 2, the positive electrode layer 11 has, for example, a plate-shaped (foil-shaped) positive electrode current collector 11A and a positive electrode mixture layer 11B. The positive electrode mixture layer 11B is formed, for example, so as to be in contact with at least one surface of the positive electrode current collector 11A.
[0026] ·Positive electrode current collector The positive electrode current collector 11A may be made of any electronically conductive material that is resistant to oxidation during charging and is not easily corroded. The positive electrode current collector 11A may be made of, for example, a metal such as aluminum, stainless steel, nickel, or titanium, or a conductive resin. The positive electrode current collector 11A may be in any form such as powder, foil, punching, or expanded metal.
[0027] Positive electrode mixture layer Fig. 3 is an enlarged view of a region R1 surrounded by a two-dot chain line in the all-solid-state battery of Fig. 2. Fig. 4 is a plan view showing an example of the configuration of an expanded metal provided in an electrode mixture layer in the all-solid-state battery of Fig. 2. Fig. 5 is an enlarged view of the region surrounded by a two-dot chain line in Fig. 3, and shows a unit structure (cross-sectional unit structure) when the expanded metal is viewed in cross section. 3, the positive electrode mixture layer 11B is provided between the positive electrode current collector 11A and the solid electrolyte layer 15, and contains a positive electrode mixture 1 and an expanded metal 2. The positive electrode mixture 1 contains a positive electrode active material and solid electrolyte particles, and may further contain one or both of a binder and a conductive assistant. The binder and the conductive assistant may be known ones.
[0028] The thickness of the positive electrode mixture layer 11B is 300 μm or less, preferably 30 μm or more, or 40 μm or more and 295 μm or less, preferably 50 μm or more, or 100 μm or more and 260 μm or less, and more preferably 150 μm or more and 200 μm or less. The thickness of the positive electrode mixture layer 11B is measured using a cross-sectional SEM image in the direction perpendicular to the surface of the positive electrode mixture layer 11B.
[0029] The positive electrode active material is not particularly limited as long as it can reversibly absorb and release, and insert and remove (intercalate and deintercalate) lithium ions, and any positive electrode active material used in known lithium ion secondary batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.
[0030] Lithium-containing metal oxides include, for example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and lithium manganese oxides represented by the general formula: LiNi x Co y Mn z O2 (x+y+z=1), lithium vanadium compounds (LiVOPO4, Li3V2(PO4)3), olivine-type LiMPO4 (where M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li4Ti5O 12 ) etc.
[0031] The positive electrode active material may not contain lithium. Examples of such positive electrode active materials include non-lithium-containing metal oxides (MnO2, V2O5, etc.), non-lithium-containing metal sulfides (MoS2, etc.), non-lithium-containing fluorides (FeF3, VF3, etc.), and sulfur-modified polyacrylonitrile. When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.
[0032] The solid electrolyte may have a Young's modulus in the range of 10 GPa to 20 GPa, and preferably in the range of 12 GPa to 16 GPa. Such a solid electrolyte may include one or more selected from halide-based solid electrolytes and sulfide-based solid electrolytes. With a Young's modulus of 20 GPa or less, the expanded metal is formed in the positive electrode mixture layer 11B, and a configuration with a large contact area between the expanded metal 2 and the solid electrolyte can be realized.
[0033] As the halide-based solid electrolyte, for example, one represented by the following formula (2) can be used. Li a E b G c X d (2)
[0034] In the halide-based solid electrolyte represented by formula (2), when E is Al, Sc, Y, or a lanthanoid, a is preferably 2.0≦a≦4.0, and more preferably 2.5≦a≦3.5. When E is Zr or Hf, a is preferably 1.0≦a≦3.0, and more preferably 1.5≦a≦2.5. In the solid electrolyte represented by formula (2), a is 0.5≦a<6, so that the content of Li in the compound is appropriate, and the ionic conductivity is high.
[0035] In the halide-based solid electrolyte represented by formula (2), E is an essential element and is an element that forms the framework of the halide-based solid electrolyte represented by formula (2). E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). By including E, a solid electrolyte having a wide potential window and high ionic conductivity is obtained. As E, in order to obtain a solid electrolyte with higher ionic conductivity, it is preferably included Al, Sc, Y, Zr, Hf, La, and particularly preferably includes Zr and Y.
[0036] In the halide-based compound represented by formula (2), 0 < b < 2. Since the effect of including E can be obtained more effectively, it is preferably 0.6 ≤ b. Further, E is an element that forms the framework of the halide-based solid electrolyte in the positive electrode mixture layer 11B represented by formula (2) and is an element with relatively high density. When b ≤ 1, a solid electrolyte with low density is obtained, which is preferable.
[0037] In the halide-based solid electrolyte represented by formula (2), G is a group that may be included. G is, for example, OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , Si6O 18 , PO3, PO4, P2O7, P3O 10, SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, CH3COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-COO, C6H5SO3, OOC-CH=CH-COO, C(OH)(CH2COOH)2COO, AsO4, BiO4, CrO4, MnO4, PtF6, PtCl6, PtBr6, PtI6, SbO4, SeO4, TeO4, and at least one group selected from the group consisting of HCOO. G is preferably at least one group selected from the group consisting of OH, SO4, CH3COO, CF3COO, HCOO, and O, and since G has a strong covalent bond with E, and thus becomes a compound in which E ions are difficult to reduce, it is preferably at least one group selected from the group consisting of SO4, BO2, CO3, BF4, and PF6, and is particularly preferably SO4 or O. When G is contained, the potential window on the reduction side of the halide-based solid electrolyte becomes wider, and reduction becomes difficult.
[0038] In the halide-based solid electrolyte represented by formula (2), c satisfies 0≦c≦6. c is preferably 0.1≦c, and more preferably 0.5≦c, because the effect of widening the potential window on the reduction side by including G becomes more pronounced. c is preferably c≦3 so that the ionic conductivity of the solid electrolyte is not reduced due to an excessively high G content.
[0039] In the halide solid electrolyte represented by formula (2), X is an essential component. X is at least one selected from the group consisting of F, Cl, Br, and I. X has a large ionic radius per valence. Therefore, when the halide solid electrolyte represented by formula (2) contains X, the effect is obtained that lithium ions flow easily and the ionic conductivity becomes high. As X, it is preferable to contain Cl in order to obtain a solid electrolyte with high ionic conductivity. Further, when X contains F, since X becomes a solid electrolyte with high ionic conductivity, it is preferable that X contains F and two or more selected from the group consisting of Cl, Br, and I.
[0040] When X is F, it becomes a solid electrolyte with sufficiently high ionic conductivity and excellent oxidation resistance. When X is Cl, it becomes a solid electrolyte with high ionic conductivity and a good balance between oxidation resistance and reduction resistance. When X is Br, it becomes a solid electrolyte with sufficiently high ionic conductivity and a good balance between oxidation resistance and reduction resistance. When X is I, it becomes a solid electrolyte with high ionic conductivity.
[0041] In the halide solid electrolyte represented by formula (2), d satisfies 0 < d ≦ 6.1. It is preferable that 1 ≦ d. When 1 ≦ d, when the solid electrolyte is pressure-molded into a pellet shape, the strength of the pellet becomes high. Also, when 1 ≦ d, the ionic conductivity of the solid electrolyte becomes high. Further, it is preferable that d ≦ 5 so that the potential window of the solid electrolyte does not become narrow due to an excessive content of X causing a shortage of G.
[0042] The halide solid electrolyte represented by formula (2) is, for example, Li2ZrCl6, Li2ZrSO4Cl4, Li2ZrCO3Cl4, Li2Zr((COO)2) 0.5 Cl5, Li2Zr(CH3COO) 0.2 Cl 5.8 , Li2Zr(CF3COO) 0.2 Cl 5.8 , Li2Zr(HCOO) 0.4 Cl 5.6, Li2ZrBO2Cl5, Li2ZrBF4Cl5, Li3YSO4Cl4, Li3YCO3Cl4, Li3YBO2Cl5, Li3YBF4Cl5, Li2ZrOCl4.
[0043] The solid electrolyte may be a sulfide-based solid electrolyte, and a compound containing Li, S, Si and / or P may be used as the sulfide-based solid electrolyte. The sulfide-based solid electrolyte may further contain Ge, Cl, Br, or I. The sulfide-based solid electrolyte may be amorphous, crystalline, or of the argyrodite type. Examples of sulfide-based solid electrolytes include Li2S-P2S5-based solid electrolytes (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 solid electrolytes (Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x (1.0≦x≦1.9).
[0044] As the sulfide-based solid electrolyte, one represented by the following formula (3) can be used. Li q M r P s O t X u S v (3) In formula (3), Li is lithium, M is a tetravalent metal, P is phosphorus, O is oxygen, S is sulfur, X is at least one selected from the group consisting of F, Cl, Br, and I, and q, r, s, t, u, and v are numbers that satisfy 1≦q≦20, 0≦r≦2, 1≦s≦5, 0≦t≦5, 0≦u≦5, and v=q / 2+2×r+2.5×stu / 2. M is preferably Si or Ge.
[0045] Conductive additives The conductive assistant contained in the positive electrode mixture 1 is not particularly limited as long as it improves the electronic conductivity of the positive electrode mixture layer 11B, and a known conductive assistant can be used. Examples of the conductive assistant include carbon-based materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO, and mixtures thereof. The conductive assistant may be in the form of powder or fiber. In addition, from the viewpoint of not lowering the current collecting function of the conductive assistant, it is preferable to dehydrate the conductive assistant by heating and vacuum drying in a glove box in which argon gas is circulated, and then store the conductive assistant in a glass bottle or an aluminum laminate bag. The dew point in the glove box is preferably -30°C or lower and -90°C or higher.
[0046] ·binder The binder contained in the positive electrode mixture 1 bonds the positive electrode current collector 11A and the positive electrode mixture layer 11B, the positive electrode mixture layer 11B and the solid electrolyte layer, and various materials constituting the positive electrode mixture layer 11B.
[0047] It is preferable to use a binder within a range that does not impair the function of the positive electrode mixture layer 11B. The binder may be any binder capable of the above-mentioned bonding, and examples thereof include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). In addition to the above, examples of the binder may include cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, and the like. In addition, a conductive polymer having electronic conductivity or an ion conductive polymer having ion conductivity may be used as the binder. Examples of the conductive polymer having electronic conductivity include polyacetylene. In this case, the binder also functions as the conductive assistant particles, so that it is not necessary to add a conductive assistant. Examples of the ion conductive polymer having ion conductivity include those that conduct lithium ions, etc., and include monomers of polymer compounds (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) and LiClO4, LiBF4, LiPF 6、 Examples of the polymerization initiator used for the composite include a photopolymerization initiator or a thermal polymerization initiator that is compatible with the above-mentioned monomers. The properties required for the binder include resistance to oxidation and reduction and good adhesiveness.
[0048] The content of the binder in the positive electrode mixture layer 11B is preferably 0.5 to 30% by volume of the positive electrode mixture layer 11B in order to reduce the resistance of the positive electrode mixture layer 11B. Moreover, in order to improve the energy density, the content of the binder in the positive electrode mixture layer 11B is preferably 0% by volume.
[0049] The content of the solid electrolyte in the positive electrode mixture layer 11B is, for example, 5% by volume to 70% by volume, preferably 20% by volume to 60% by volume, and more preferably 40% by volume to 55% by volume. The content of the positive electrode active material in the positive electrode mixture layer 11B is, for example, 25% by volume to 95% by volume, and preferably 55% by volume to 40% by volume.
[0050] The expanded metal 2 has strands 51 formed to surround voids G, and a plurality of bonds 52 at which the strands 51 are joined. The expanded metal 2 has a shape in which, for example, the length in one direction in the plane of the voids G is longer than the direction perpendicular to that direction. In Fig. 4, the center-to-center distance between the nearest bonds 52 in the long direction in which the length of the voids G is greater is represented by the symbol LW, and the center-to-center distance between the nearest bonds 52 in the short direction perpendicular to the long direction is represented by the symbol SW.
[0051] The center-to-center distance SW in the short direction of the expanded metal 2 is, for example, 0.4 mm or more and 1.5 mm or less. The center-to-center distance LW in the short direction of the expanded metal 2 is, for example, 0.5 mm or more and 3.0 mm or less. The pitch width w of the expanded metal 2 is, for example, 0.05 or more and 0.3 or less. The thickness of the expanded metal 2 is, for example, 10 μm or more and 300 μm or less.
[0052] The gaps G of the expanded metal are filled with, for example, the positive electrode mixture 1.
[0053] The expanded metal 2 may contain, for example, one or more materials selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon, and is preferably a material selected from the group consisting of Al, Ni, and Ti, and is more preferably composed of Al or Ti.
[0054] The expanded metal 2 is preferably formed so as to be inclined with respect to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15. The inclination angle θ1 of the expanded metal 2 with respect to the interface S1 between the positive electrode mixture layer 11B and the solid electrolyte layer 15 is preferably 0.5° or more and 20° or less, more preferably 1° or more and 15° or less, and even more preferably 10° or less. When the inclination angle θ1 of the expanded metal 2 is within the above range, an all-solid-state battery having excellent conductivity in the stacking direction and particularly excellent internal resistance is obtained.
[0055] The ratio of the volume of the expanded metal 2 to the volume of the positive electrode mixture layer 11B is, for example, not less than 1% and not more than 85%.
[0056] As described above, Fig. 5 is an enlarged view of the area surrounded by the two-dot chain line in Fig. 3, and is a diagram showing a cross-sectional unit structure of the expanded metal. Fig. 5 shows an enlarged view of a part of the strand 51 or bond 52 of the expanded metal 2. In a cross section along the stacking direction of the laminate 30, the expanded metal 2 is defined by a first side M1 close to the solid electrolyte layer 15, a second side M2 facing the first side M1, and a third side M3 and a fourth side M4 connecting the second side M2 and the first side M1. In the cross section shown in Fig. 3, the expanded metal 2 has cross-sectional unit structures, which are the areas defined by the first side M1 to the fourth side M4, arranged in a row.
[0057] Among the angle X1 between the second side M2 and the third side M3 and the angle X2 between the second side M2 and the fourth side M4, the smaller angle X satisfies 20°≦X<90°, preferably satisfies 30°≦X≦80°, more preferably satisfies 40°≦X≦70°, and further preferably satisfies 50°≦X≦60°. If the angle X is too small, the density of the mixture does not increase much during press molding, and the internal resistance becomes higher than when the angle is sufficiently large. On the other hand, if the angle X is too large, the length of the second side M2 becomes shorter than when the angle X is sufficiently small, and the area of the surface of the expanded metal 2 close to the positive electrode collector 11A relative to the area of the positive electrode collector or the contact area with the positive electrode collector 11A becomes smaller, and the internal resistance becomes higher.
[0058] 5, since the cross-sectional view is an isosceles trapezoid with X1=X2, both angles X1 and X2 correspond to the above angle X and satisfy the above numerical range. In this way, it is preferable that both angles X1 and X2 of the expanded metal 2 satisfy the above numerical range. That is, angles X1 and X2 satisfy 20°≦X<90°, preferably satisfy 30°≦X≦80°, more preferably satisfy 40°≦X≦70°, and further preferably satisfy 50°≦X≦60°.
[0059] The cross-sectional unit structure of the expanded metal 2 is, for example, a trapezoid in which the second side M2 is longer than the first side M1. In Fig. 5, the length of the first side M1 is indicated by the symbol a, the length of the second side M2 is indicated by the symbol b, and the distance between the first side M1 and the second side M2 is indicated by the symbol c. Here, in this embodiment, the distance between the first side M1 and the second side M2 is measured from the midpoint m of the first side M1 in a direction perpendicular to the first side M1. M1 From the midpoint m of the second side M2 M2 represents the distance to
[0060] In the cross-sectional unit structure of the expanded metal, the slope (|ab| / c) is, for example, more than 0.01 and not more than 6, preferably 0.1 to 3, more preferably 0.5 to 2.5, and even more preferably 1.0 to 2.0.
[0061] (Negative electrode layer) The negative electrode layer 13 has, for example, a plate-shaped (foil-shaped) negative electrode current collector 13A and a negative electrode mixture layer 13B. The negative electrode mixture layer 13B is formed, for example, so as to be in contact with at least one surface of the negative electrode current collector 13A. In the following description of the negative electrode layer, description of components common to the positive electrode layer may be omitted.
[0062] ·Negative electrode current collector The negative electrode current collector 13A may have electronic conductivity. The negative electrode current collector 13A may be made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 13A may be in the form of a powder, a foil, a punching, or an expanded metal.
[0063] Negative electrode mixture layer Fig. 6 is an enlarged view of a region R2 surrounded by a two-dot chain line in the all-solid-state battery in Fig. 2. As shown in Fig. 6, the negative electrode mixture layer 13B is provided between the negative electrode current collector 13A and the solid electrolyte layer 15, and includes the negative electrode mixture 3 and the expanded metal 4.
[0064] The negative electrode mixture 3 includes a negative electrode active material and a solid electrolyte having a Young's modulus of 10 GPa or more and 20 GPa or less, and may further include one or both of a binder and a conductive assistant. Known binders and conductive assistants can be used. The type and amount of the binder and conductive assistant in the negative electrode mixture layer 13B may be the same as the type and amount of the binder and conductive assistant in the positive electrode mixture layer 11B.
[0065] The thickness of the negative electrode mixture layer 13B is, for example, 300 μm or less, and preferably 30 μm or more. The thickness of the negative electrode mixture layer 13B is measured using a cross-sectional SEM image taken in a direction perpendicular to the surface of the negative electrode mixture layer 13B.
[0066] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. The negative electrode active material may be any negative electrode active material used in known lithium ion secondary batteries.
[0067] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies; metals that can be combined with lithium, such as Si, SiOx, Sn, and aluminum; alloys of these; composite materials of these metals and carbon materials; and lithium titanate (Li4Ti5O 12 ), oxides such as SnO2, sulfur-modified polyacrylonitrile, metallic lithium, etc. The negative electrode active material is natural graphite or lithium titanate (Li4Ti5O 12 ) is preferred.
[0068] The content of the solid electrolyte in the negative electrode mixture layer 13B is, for example, 5 volume % to 70 volume % or less, preferably 30 volume % to 65 volume % or less, and more preferably 40 volume % to 55 volume % or less. The content of the negative electrode active material in the negative electrode mixture layer 13B is, for example, 30 volume % to 70 volume % or less, and preferably 40 volume % to 60 volume % or less.
[0069] The solid electrolyte may have a Young's modulus in the range of 10 GPa to 20 GPa, and preferably in the range of 12 GPa to 16 GPa. Such a solid electrolyte may include one or more selected from halide-based solid electrolytes and sulfide-based solid electrolytes. With a Young's modulus of 20 GPa or less, the expanded metal is formed in the positive electrode mixture layer 11B, and a configuration with a large contact area between the expanded metal 2 and the solid electrolyte can be realized.
[0070] The halide-based solid electrolyte may be one represented by the above formula (2), and the sulfide-based solid electrolyte may be one represented by the above formula (3). Two or more of the halide-based solid electrolyte represented by the above formula (2) and the sulfide-based solid electrolyte represented by the above formula (3) may be used in combination. The solid electrolyte contained in the negative electrode mixture layer 13B may be the same as the solid electrolyte contained in the positive electrode mixture layer 11B.
[0071] The shape and material of the expanded metal 4 may be the same as those of the expanded metal 2, for example.
[0072] The expanded metal 4 is preferably formed so as to be inclined with respect to the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15. The inclination angle θ2 of the expanded metal 4 with respect to the interface S2 between the negative electrode mixture layer 13B and the solid electrolyte layer 15 is preferably 0.5° or more and 20° or less, more preferably 1° or more and 15° or less, and even more preferably 10° or less. When the inclination angle θ2 of the expanded metal 4 is within the above range, an all-solid-state battery having excellent conductivity in the stacking direction and particularly excellent internal resistance is obtained.
[0073] The ratio of the volume of the expanded metal 4 to the volume of the negative electrode mixture layer 13B is, for example, not less than 1% and not more than 85%.
[0074] The expanded metal 4 may be inclined in the same direction as the expanded metal 2 with respect to the solid electrolyte layer 15, or may be inclined in a different direction.
[0075] The cross-sectional unit structure of the expanded metal 4 in the negative electrode mixture layer 13B can be the same as the cross-sectional unit structure of the expanded metal 2 in the positive electrode mixture layer 11B. That is, in a cross section along the stacking direction of the laminate 30, the expanded metal 4 is defined by a first side M1 close to the solid electrolyte layer 15, a second side M2 facing the first side M1, and a third side M3 and a fourth side M4 connecting the second side M2 and the first side M1. In the expanded metal 4, the regions defined by the first side M1 to the fourth side M4 are aligned in a row.
[0076] Of the angle X1 between the second side M2 and the third side M3 and the angle X2 between the second side M2 and the fourth side M4, the smaller angle X satisfies 20°≦X<90°, preferably satisfies 30°≦X≦80°, more preferably satisfies 40°≦X≦70°, and further preferably satisfies 50°≦X≦60°.
[0077] Both of the angles X1 and X2 correspond to the above angle X and satisfy the above numerical range. In this way, it is preferable that the expanded metal 4 has both of the angles X1 and X2 satisfying the above numerical range.
[0078] The cross-sectional unit structure of the expanded metal 4 is, for example, a trapezoid in which the second side M2 is longer than the first side M1. When the length of the first side M1 is a, the length of the second side M2 is b, and the distance between the first side M1 and the second side M2 is c, the slope (|ab| / c) in the cross-sectional unit structure of the expanded metal is, for example, more than 0.01 and not more than 6, preferably 0.1 to 3, more preferably 0.5 to 2.5, and even more preferably 1.0 to 2.0. Here, in this embodiment, the distance between the first side M1 and the second side M2 is measured from the midpoint m of the first side M1 in a direction perpendicular to the first side M1. M1 From the midpoint m of the second side M2 M2 represents the distance to
[0079] (Solid electrolyte layer) The solid electrolyte layer 15 is sandwiched between the positive electrode layer 11 and the negative electrode layer 13. The solid electrolyte layer 15 includes a solid electrolyte that can move ions by an externally applied voltage. For example, the solid electrolyte conducts lithium ions and inhibits the movement of electrons.
[0080] The solid electrolyte constituting the solid electrolyte layer 15 contains, for example, lithium. The solid electrolyte may be, for example, an oxide-based material, a sulfide-based material, a halide-based material, or a complex hydride-based material. As the solid electrolyte provided in the solid electrolyte layer 15, it is preferable to use one or both of a halide-based material and a sulfide-based material. As the halide-based solid electrolyte, one represented by the above formula (2) may be used. As the sulfide-based solid electrolyte, one represented by the above formula (3) may be used.
[0081] [Manufacturing method of all-solid-state batteries] Next, a method for manufacturing the all-solid-state battery according to the present embodiment will be described. The all-solid-state battery according to the present embodiment is manufactured by, for example, a powder molding method. The powder molding method is performed in a glove box.
[0082] The manufacturing method of the all-solid-state battery according to the present embodiment includes a solid electrolyte layer forming step of forming a solid electrolyte layer by pressing, a positive electrode mixture forming step of synthesizing a positive electrode mixture containing one or both of a halide-based solid electrolyte and a sulfide-based solid electrolyte, a negative electrode mixture forming step of forming a negative electrode mixture containing one or both of a halide-based solid electrolyte and a sulfide-based solid electrolyte, a positive electrode mixture layer forming step of placing a positive electrode mixture on one side of the solid electrolyte layer, further placing an expanded metal, and compacting the powder using a punch or the like, and a negative electrode mixture layer forming step of placing a negative electrode mixture on one side of the solid electrolyte layer, further placing an expanded metal, and compacting the powder using a punch or the like. In the manufacturing method of the all-solid-state battery according to the present embodiment, an expanded metal of a predetermined shape can be used. In addition, the cross-sectional shape can be adjusted by adjusting the way pressure is applied to the expanded metal. For example, the cross-sectional shape of the expanded metal can be made into a predetermined shape by performing laser processing. With laser processing, for example, it is possible to round off the corners of the expanded metal when viewed in cross section.
[0083] According to the above embodiment, an expanded metal is formed on an electrode mixture layer comprising an electrode active material and a solid electrolyte, and the expanded metal has a predetermined cross-sectional shape, so that the electrode active material is in close contact with the expanded metal, and the area of the surface of the expanded metal that is closer to the electrode current collector can be increased relative to the area of the electrode current collector, and it is also possible to increase the contact area between the expanded metal and the electrode current collector, making it possible to provide an all-solid-state battery with low internal resistance.
[0084] (Modification) Figures 7(a), 7(b) and 7(c) are cross-sectional views showing a modified example of Figure 5. In the modified example, the same configurations as those in the above embodiment are given the same reference numerals and the description will be omitted. All of Figures 7(a) to 7(c) are enlarged views of a portion of the cross section of the expanded metals 2A to 2C, and the actual cross-sectional shapes of the expanded metals 2A to 2C are a row of the shapes shown in these figures.
[0085] The expanded metal provided in the all-solid-state battery of the above embodiment may have a rounded corner structure as shown in Fig. 7(a), may have a configuration in which the first side M1 and the second side M2 are not parallel, or the length of the third side M3 and the length of the fourth side M4 are different as shown in Fig. 7(b), or may have a configuration in which the lengths of the third side M3 and the fourth side M4 are different, or may have a configuration in which the sizes of the angles X1 and X2 are different as shown in Fig. 7(c). When the sizes of the angles X1 and X2 are different, it is sufficient that the smaller angle X of the angles X1 and X2 is within a range of 20° or more and less than 90°, and it is preferable that both the angles X1 and X2 are within a range of 20° or more and less than 90°.
[0086] Even when the electrode mixture layer includes expanded metals having the structures shown in Figs. 7(a) to 7(c) arranged in a row, it is possible to provide an all-solid-state battery with low internal resistance.
[0087] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES
[0088] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0089] [Example 1] -Synthesis of solid electrolyte- In a glove box with argon gas circulating at a dew point of -90°C, an oxygen concentration of 1 ppm, and atmospheric pressure, the synthesis of solid electrolyte, the mixing of the positive electrode mixture layer material, the mixing of the negative electrode mixture layer material, and the preparation of an all-solid-state battery were carried out. First, Li2SO4 and ZrCl4 were weighed out as raw material powder so that the molar ratio was 1:1. Next, the weighed raw material powder was placed in a Zr container together with a Zr ball having a diameter of 5 mm, and mechanochemical milling was carried out using a planetary ball mill. The treatment was carried out at a rotation speed of 500 rpm for 50 hours, and then sieved through a 200 μm mesh sieve. As a result, a powder of Li2ZrSO4Cl4 was obtained as a solid electrolyte.
[0090] -Synthesis of positive electrode mixture- Next, the positive electrode mixture was weighed and mixed in a glove box with argon gas circulating at a dew point of -85°C and an oxygen concentration of 1 ppm. The materials were weighed out so that the ratio of lithium cobalt oxide (LiCoO2):Li2ZrSO4Cl4:carbon black was 77:18:5 parts by weight, and mixed in an agate mortar for 5 minutes to obtain a positive electrode mixture.
[0091] -Synthesis of negative electrode mixture- Next, the negative electrode mixture was weighed and mixed in a glove box with argon gas circulating at a dew point of -85°C and an oxygen concentration of 1 ppm. 12 ): Li2ZrSO4Cl4: carbon black = 72:22:6 parts by weight, and mixed in an agate mortar for 5 minutes to obtain a negative electrode mixture.
[0092] -Molding process- Next, using the above solid electrolyte, positive electrode mixture, negative electrode mixture, and expanded metal, a power storage element composed of a positive electrode current collector / positive electrode mixture layer / electrolyte layer / negative electrode mixture layer / negative electrode current collector was produced by a powder molding method.
[0093] First, a die made of SKD11 material with a 30 x 40 mm through hole in the center was prepared, along with a lower punch and an upper punch made of the same material, measuring 29.9 x 39.9 mm. The lower punch was inserted into the through hole of the die, and 400 mg of solid electrolyte was added from the opening side. The upper punch was then inserted on top of the solid electrolyte. This first unit was placed in a press machine and pressed at a pressure of 373 MPa to form a solid electrolyte layer. The first unit was removed from the press machine, and the upper punch was removed.
[0094] Next, 750 mg of the negative electrode mixture was poured onto the solid electrolyte layer (upper punch side) from the open side of the resin holder.
[0095] Next, an expanded metal made of aluminum was placed on the negative electrode mixture. The expanded metal had a center-to-center distance SW between the nearest bonds in the short direction, which is the shortest length in the gap, of 1 mm, a center-to-center distance LW between the nearest bonds in the long direction perpendicular to the short direction, a pitch width of 150 μm, and a thickness of 50 μm. That is, the product SW×LW of the center-to-center distance SW in the short direction and the center-to-center distance LW in the long direction of the expanded metal used in Example 1 was 2 mm. 2 It is.
[0096] Next, an upper punch was inserted on top of it. This second unit was placed in a press and molded at a pressure of 373 MPa. Next, the second unit was removed, turned upside down, and the lower punch was removed.
[0097] Next, 750 mg of a positive electrode mixture was placed on the solid electrolyte layer (on the lower punch side).
[0098] Next, an expanded metal made of aluminum was placed on the positive electrode mixture. The expanded metal had a center-to-center distance SW between the nearest bonds of 1 mm in the short direction where the gap length was small, a center-to-center distance LW between the nearest bonds of 2 mm in the long direction perpendicular to the short direction, a pitch width of 150 μm, and a thickness of 50 μm.
[0099] Next, a lower punch was inserted onto the third unit, and the third unit was placed in a press and molded at a pressure of 373 MPa.
[0100] Next, the electricity storage element composed of the positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer was removed from the die.
[0101] -Containment process- Next, the obtained electricity storage element was housed in an outer casing in a dry room with a dew point of -50°C.
[0102] An aluminum laminate bag was prepared as an exterior body to be enclosed. In addition, an aluminum foil (width 4 mm, length 40 mm, thickness 100 μm) wrapped with maleic anhydride grafted polypropylene (PP) was welded to the negative electrode current collector (aluminum foil, 30 × 40 mm, thickness 20 μm) and the positive electrode current collector (aluminum foil, 30 × 40 mm, thickness 20 μm) as an external terminal. The layers were laminated to form a positive electrode current collector / positive electrode mixture layer / solid electrolyte layer / negative electrode mixture layer / negative electrode current collector, and inserted into the aluminum laminate bag. Finally, the opening was heat sealed while the inside of the exterior body was evacuated, to produce the all-solid-state battery of Example 1.
[0103] [Examples 2 to 8] An all-solid-state battery was produced in the same manner as in Example 1, except that an expanded metal having a different cross-sectional unit structure was used.
[0104] [Examples 9 to 12] An all-solid-state battery was produced in the same manner as in Example 1, except that an expanded metal made of a different material was used.
[0105] [Example 13] An all-solid-state battery was produced in the same manner as in Example 1, except that an expanded metal was not formed on the negative electrode mixture layer, and an expanded metal was formed only on the positive electrode mixture layer.
[0106] [Example 14] An all-solid-state battery was produced in the same manner as in Example 1, except that an expanded metal was not formed on the positive electrode mixture layer, and an expanded metal was formed only on the negative electrode mixture layer.
[0107] [Examples 15 to 22] The electrode mixture was placed on the solid electrolyte layer, and the expanded metal was placed on the electrode mixture, and the orientation of the expanded metal was adjusted when the surface of the electrode mixture powder was leveled before the punch was inserted. In this way, an all-solid-state battery was produced in the same manner as in Example 1, except that the inclination θ1 of the expanded metal with respect to the interface between the positive electrode mixture layer and the solid electrolyte layer, and the inclination θ2 of the expanded metal with respect to the interface between the negative electrode mixture layer and the solid electrolyte were changed.
[0108] [Comparative Example 1 and Comparative Example 2] An all-solid-state battery was produced in the same manner as in Example 1, except that an expanded metal having a different cross-sectional unit structure was used.
[0109] (Internal resistance measurement) The internal resistance was measured by electrochemical impedance spectroscopy (EIS) under the following conditions for the all-solid-state batteries of Examples 1 to 22 and Comparative Examples 1 and 2. Specifically, the all-solid-state batteries were held in a thermostatic chamber at 25° C., and the real component Z′ of the impedance at a measurement frequency of 1 kHz was measured as the internal resistance [Ω].
[0110] (Cross-section observation of an all-solid-state battery) The all-solid-state batteries of Examples 1 to 22 and Comparative Examples 1 and 2 were cut along the lamination direction, and cross-sectional SEM images were taken. Using the cross-sectional SEM images, the cross-sectional unit structure of the expanded metal was confirmed, and the angle of the expanded metal provided on the positive electrode mixture layer relative to the interface between the positive electrode mixture layer and the solid electrolyte layer, and the angle of the expanded metal provided on the negative electrode mixture layer relative to the interface between the negative electrode mixture layer and the solid electrolyte layer were measured.
[0111] In confirming the cross-sectional unit structure of the expanded metal, first, a region of the expanded metal defined by a first side M1 close to the solid electrolyte layer, a second side M2 facing the first side M1, and a third side M3 and a fourth side M4 connecting the second side M2 and the first side M1 was selected. Next, the angle X1 between the second side M2 and the third side M3 and the angle X2 between the second side M2 and the fourth side M4 were measured from the cross-sectional SEM image. Of X1 and X2, the size of the smaller angle X was measured.
[0112] In addition, from the cross-sectional SEM image, the slope (|ab| / c) was calculated when the length of the first side in the cross-sectional unit structure of the expanded metal was a, the length of the second side was b, and the distance between the first side and the second side was c.
[0113] Table 1 summarizes the measurement results of the size of the angle X in the cross-sectional unit structure of the expanded metal in Examples 1 to 22, Comparative Example 1, and Comparative Example 2, the inclination (|ab| / c), the angle θ1 of the expanded metal with respect to the interface S1 of the electrode mixture layer, the positive electrode mixture layer, and the solid electrolyte layer on which the expanded metal is formed, the angle θ2 of the expanded metal with respect to the interface S2 of the negative electrode mixture layer and the solid electrolyte layer, and the internal resistance. In Examples 1 to 22 and Comparative Example 2, the expanded metal formed in the positive electrode mixture layer and the negative electrode mixture layer of the all-solid-state battery had the same shape of the cross-sectional unit structure, an isosceles trapezoid. The cross-sectional unit structure of the expanded metal formed in the positive electrode mixture layer and the negative electrode mixture layer of the all-solid-state battery in Comparative Example 1 was rectangular.
[0114] [Table 1]
[0115] As can be seen from Table 1, in the cross-sectional unit structure of the expanded metal formed on the electrode mixture layer, Examples 1 to 22 in which the angle X is in the range of 20°≦X<90° were confirmed to exhibit significantly lower internal resistance than Comparative Example 1 in which the angle X is 90° and Comparative Example 2 in which the angle X is less than 20°. Moreover, Examples 2 and 3 in which the angle X is in the range of 30° or more and 60° or less exhibited lower internal resistance than Examples 1 and 4 which were outside the above range.
[0116] Moreover, Examples 5 and 6, in which the slope (|ab| / c) is greater than 0.5 and equal to or less than 3, exhibited lower internal resistance than Examples 7 and 8, which are outside the above range. Moreover, Examples 1 and 9, in which the expanded metal is composed of Al or Ni, exhibited particularly low internal resistance. Compared with Example 13, in which the expanded metal is formed only in the positive electrode mixture layer, Example 14, in which the expanded metal is formed only in the negative electrode mixture layer, exhibited lower internal resistance, confirming the effectiveness of forming an expanded metal of a predetermined shape in the negative electrode mixture layer.
[0117] Furthermore, it was confirmed that Examples 15 to 19, in which the inclinations θ1 and θ2 of the expanded metal relative to the interface between the electrode mixture layer and the solid electrolyte layer were 0.5° or more and 10° or less, showed particularly excellent internal resistance, and Examples 15 to 17, in which the inclinations were 0.5° or more and 5° or less, showed even better internal resistance. [Explanation of symbols]
[0118] 1: positive electrode mixture, 2, 4: expanded metal, 3: negative electrode mixture, 10: electricity storage element, 11: positive electrode layer, 11A: positive electrode current collector, 11B: positive electrode mixture layer, 13: negative electrode layer, 13A: negative electrode current collector, 13B: negative electrode mixture layer, 15: solid electrolyte layer, 12, 14: external terminal, 20: exterior body, 22: metal foil, 24: resin layer, 51: strand, 52: bond, 100: all-solid-state battery, M1: first side, M2: second side, M3: third side, M4: fourth side, X1: angle between the second side and the third side, X2: angle between the second side and the fourth side
Claims
1. a positive electrode mixture layer including a positive electrode active material and a negative electrode mixture layer including a negative electrode active material are laminated with a solid electrolyte layer interposed therebetween; At least one of the positive electrode mixture layer and the negative electrode mixture layer is an electrode mixture layer including an expanded metal and solid electrolyte particles, In a cross section of the laminate along the lamination direction, the expanded metal is defined by a first side close to the solid electrolyte layer, a second side opposite to the first side, and a third side and a fourth side connecting the first side and the second side, an angle X between the second side and the third side and an angle between the second side and the fourth side, which is a smaller angle, satisfies 20°≦X<90°.
2. The all-solid-state battery according to claim 1, wherein one of the third side and the fourth side is inclined with respect to a direction perpendicular to the first side, and a slope (|a-b| / c) is greater than 0.01 and is equal to or less than 3, where a is the length of the first side, b is the length of the second side, and c is the distance between the first side and the second side.
3. The all-solid-state battery according to claim 1 , wherein an angle between the second side and the third side and an angle between the second side and the fourth side are in a range of 20° or more and less than 90°.
4. 2. The all-solid-state battery according to claim 1, wherein the expanded metal contains one or more selected from the group consisting of Al, Ni, Cu, Mo, Pt, Ti, SUS, and carbon.
5. 2. The all-solid-state battery according to claim 1, wherein both the positive electrode mixture layer and the negative electrode mixture layer contain the expanded metal and the solid electrolyte particles.
6. 2. The all-solid-state battery according to claim 1, wherein an angle of the expanded metal with respect to an interface between the electrode mixture layer and the solid electrolyte layer is 0.5° or more and 15° or less.
Citation Information
Patent Citations
Laminate including active material layer and solid electrolyte layer, and all solid lithium secondary battery using it
JP2007005279A
Electrode material sheet for lithium battery, solid lithium battery, and device with the solid lithium battery
JP2010040218A