capacitor
By employing an inorganic conductive layer with columnar crystals in capacitors, the ESR and heat resistance issues are addressed, resulting in a more reliable and efficient capacitor design.
Patent Information
- Application Number
- JP2023051880
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional capacitors face challenges in reducing equivalent series resistance (ESR) and improving heat resistance, particularly in solid electrolytic capacitors using conductive polymers.
The use of an inorganic layer composed of crystal grains with columnar crystals in the conductive layer, formed through liquid phase growth, enhances the conductivity and adhesion between electrodes, thereby reducing ESR and improving heat resistance.
The proposed capacitor design achieves lower ESR and higher heat resistance by utilizing an inorganic conductive layer with a high ratio of columnar crystals, ensuring efficient current flow and improved reliability.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to capacitors. [Background technology]
[0002] Various capacitors have been proposed in the past. Claim 1 of Patent Document 1 (JP 2017-103412 A) describes "a solid electrolytic capacitor comprising an anode body, a dielectric layer disposed on a surface of the anode body, and a solid electrolyte layer disposed on the surface of the dielectric layer and made of zinc oxide having a conductivity of 1 (S / cm) or more."
[0003] Claim 1 of Patent Document 2 (JP 2020-35890 A) describes "a solid electrolytic capacitor comprising an anode body made of a valve metal, a dielectric layer formed on the surface of the anode body, a semiconductor layer formed on the dielectric layer, and a cathode layer formed on the semiconductor layer, wherein the semiconductor layer is composed of a p-type inorganic semiconductor." [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-103412 A [Patent Document 2] JP 2020-35890 A Summary of the Invention [Problem to be solved by the invention]
[0005] By using an inorganic layer instead of a solid electrolyte layer formed using a conductive polymer, it is possible to improve the heat resistance of a capacitor. On the other hand, a reduction in equivalent series resistance (ESR) is required for a capacitor. One of the objectives of the present disclosure is to provide a capacitor capable of reducing the ESR. [Means for solving the problem]
[0006] One aspect of the present disclosure relates to a capacitor including a first electrode, a dielectric layer formed on a surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer, the surface layer of the conductive layer being a crystal layer composed of crystal grains made of an inorganic material, the crystal grains including columnar crystals. Effect of the Invention
[0007] According to the present disclosure, a capacitor capable of reducing ESR is obtained. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic view of a part of an example of a capacitor according to this embodiment. [Diagram 2] FIG. 2 shows the results of analyzing an example of the zinc oxide layer produced in Experiment 1 by electron backscatter diffraction. [Diagram 3] FIG. 3 shows the results of analyzing another example of the zinc oxide layer produced in Experiment 1 by electron backscatter diffraction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In the following, the embodiments according to the present disclosure will be described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and other materials may be applied as long as the invention according to the present disclosure can be implemented. In this specification, the description "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "numerical value A or more and numerical value B or less." In the following description, when the lower limit and the upper limit of numerical values related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined as long as the lower limit is not equal to or greater than the upper limit.
[0010] (Capacitor) The capacitor according to this embodiment may be referred to as "capacitor (C)" below. Capacitor (C) includes a first electrode, a dielectric layer formed on the surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer. The surface layer of the conductive layer is a crystal layer composed of crystal grains made of an inorganic material. The crystal grains include columnar crystals.
[0011] The conductive layer can be formed of an inorganic material. Therefore, the conductive layer can be read as an inorganic layer. A preferred example of the conductive layer of the capacitor (C) does not contain an organic material (e.g., a conductive polymer). By forming the conductive layer from an inorganic material, a capacitor (C) with high heat resistance can be obtained. Furthermore, by including columnar crystals in the conductive layer, a capacitor with low equivalent series resistance (ESR) can be obtained. Note that columnar crystals refer to crystals that extend in one direction and are columnar, and do not have to be cylindrical.
[0012] In a cross section of the crystal layer parallel to the thickness direction Dt of the conductive layer, the ratio of the area of crystal grains in which the angle α between the c-axis direction and the thickness direction Dt is less than 60° to the area of the crystal layer (hereinafter, sometimes referred to as "ratio R") is 80% or more. The ratio R is determined by a method described in the examples.
[0013] The ratio R is in the range of 80% to 100%. From another viewpoint, in a cross section of the crystal layer parallel to the thickness direction Dt, the ratio of the area of crystal grains whose angle α between the c-axis direction and the thickness direction Dt is greater than 60° to the area of the crystal layer is less than 20%.
[0014] Crystal grains tend to grow along the c-axis. Therefore, columnar crystals usually extend in the c-axis direction. The higher the ratio R, the higher the ratio of columnar crystals extending in a direction close to the thickness direction Dt, making it easier for current to flow along the thickness direction Dt of the conductive layer. Therefore, by making the ratio R 80% or more, the ESR of the capacitor (C) can be made particularly low.
[0015] In a cross section parallel to the thickness direction Dt of the conductive layer, the proportion X of the area of the crystal grains whose c-axis direction and thickness direction Dt are inclined at 20° or more to the area of the crystal layer may be 20% or more (e.g., 30% or more, 40% or more, or 45% or more) or 90% or less (e.g., 80% or less). By making the proportion X 20% or more, the proportion of crystal grains extending away from the direction Dt increases, and as a result, the surface of the surface layer of the conductive layer is appropriately roughened. By roughening the surface of the surface layer of the conductive layer, the adhesion between the conductive layer and the second electrode is increased. As a result, it is possible to improve the reliability of the capacitor (C) and reduce the ESR of the capacitor (C).
[0016] The conductive layer may be made of an inorganic material containing a metal oxide. In that case, the crystal layer on the surface of the conductive layer may be made of the metal oxide, or the entire conductive layer may be made of the metal oxide. The metal oxide may be a conductive metal oxide mainly composed of at least one selected from the group consisting of ZnO, TiO2, SnO2, CuInO2, and CuCrO2, or may be a conductive metal oxide composed of at least one of the above. The metal oxide may be a conductive metal oxide mainly composed of any one selected from the above group, or may be a conductive metal oxide composed of the above. For example, the metal oxide may be a conductive metal oxide mainly composed of ZnO, or may be ZnO. Although ZnO is sometimes classified as a semiconductor, it is treated as a conductive metal oxide in this specification because it has conductivity. With respect to the metal oxide, the main component means that the content is 50 mass% or more. The content of the main component in the metal oxide may be in the range of 80 to 100 mass%, 90 to 100 mass%, or 95 to 100 mass%.
[0017] The conductive metal oxide may contain oxygen vacancies. By containing oxygen vacancies, the conductivity of the conductive metal oxide can be increased. When the conductive metal oxide is mainly composed of zinc oxide (ZnO), ZnO 1-xThe main component may be zinc oxide represented by the formula (0≦x≦0.25), where x may be greater than 0.
[0018] The conductive metal oxide may contain an additive element for improving the conductivity. When the conductive metal oxide is mainly composed of ZnO, at least one element selected from the group consisting of Al, Ga, B, and In may be added to ZnO so that the content of the element is 10 atomic % or less.
[0019] When the conductive metal oxide is mainly composed of TiO2, at least one element selected from the group consisting of Nb and Ta may be added to TiO2 so that its content is 10 atomic % or less. When the conductive metal oxide is mainly composed of SnO2, Sb may be added to SnO2 so that its content is 12.5 atomic % or less. When the conductive metal oxide is mainly composed of CuInO2, Ca may be added to CuInO2 so that its content is 3 atomic % or less. When the conductive metal oxide is mainly composed of CuCrO2, Mg may be added to CuCrO2 so that its content is 5 atomic % or less.
[0020] In the capacitor (C), the first electrode may be an anode and the second electrode may be a cathode. In the capacitor (C), the first electrode may be an aluminum foil or a tantalum sintered body. When the first electrode is an aluminum foil, the dielectric layer may be an aluminum oxide layer.
[0021] In the capacitor (C), the first electrode may have a porous portion on its surface. In this case, the dielectric layer is formed on the surface of the porous portion, and a part of the conductive layer is disposed in the voids of the porous portion. The first electrode having a porous portion on its surface may be an etched aluminum foil or a sintered body of a valve metal (e.g., a tantalum sintered body).
[0022] The conductive layer may include a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode. The conductive layer may be composed of a first conductive layer and a second conductive layer. The second conductive layer has the above-mentioned crystal layer. The second conductive layer may have a composition different from that of the first conductive layer, or may have the same composition as that of the first conductive layer. The first conductive layer and the second conductive layer may be composed of the above-mentioned conductive metal oxide. When a porous portion is present on the surface layer of the first electrode, at least a part of the first conductive layer may be formed in the recess of the porous portion.
[0023] The conductive layer may have a conductivity of 1 S / cm or more, or 10 S / cm or more. The conductive layer may have a conductivity of 10,000 S / cm or less, or 1,000 S / cm or less. The conductive layer may be an inorganic layer having a conductivity of 1 S / cm or more.
[0024] The thickness of the conductive layer is not particularly limited and may be in the range of 0.1 μm to 100 μm (for example, in the range of 1 μm to 10 μm).
[0025] (Capacitor manufacturing method) The manufacturing method according to this embodiment may be referred to as manufacturing method (M) below. According to manufacturing method (M), a capacitor (C) can be manufactured. However, the capacitor (C) may be manufactured by a method other than manufacturing method (M). The matters described for the capacitor (C) can be applied to manufacturing method (M), so duplicated descriptions will be omitted. The matters described for manufacturing method (M) may also be applied to the capacitor (C).
[0026] The manufacturing method (M) is a method for manufacturing a capacitor including a first electrode and a dielectric layer formed on the surface of the first electrode. The manufacturing method (M) includes steps (i) and (ii) in this order. These steps are described below.
[0027] Step (i) is a step of forming a conductive layer on the dielectric layer formed on the surface of the first electrode. The conductive layer is the conductive layer described for the capacitor (C). In step (i), a conductive layer is formed so that the surface layer of the conductive layer becomes the above-mentioned crystal layer. At least the surface layer of the conductive layer can be formed by a liquid phase growth method. According to the liquid phase growth method, a conductive layer (a crystal layer having conductivity) can be formed by crystal growth. At this time, the above-mentioned crystal layer can be formed by selecting the conditions of the liquid phase growth method.
[0028] When the surface layer is made of a zinc oxide crystal layer, the above-mentioned crystal layer can be formed under the following conditions. First, a solution for liquid phase growth (solution growth) is prepared. Examples of the solution include an aqueous solution in which zinc nitrate and other additives are dissolved. Examples of the additives include hexamethylenetetramine, ammonia, citric acid, ammonium nitrate, aluminum nitrate, gallium nitrate, indium nitrate, and the like. When the above-mentioned additive element is added to ZnO, a compound containing the additive element may be dissolved. The pH of the solution is, for example, in the range of 6 to 11. The concentration of zinc nitrate in the solution is, for example, in the range of 0.01 mol / L to 2 mol / L. The temperature of the first electrode is, for example, in the range of 85°C to 95°C. The temperature of the solution is, for example, 85°C or less. The temperature of the solution may be in the range of 0 to 85°C (for example, in the range of 10 to 50°C or in the range of 10 to 40°C). Furthermore, it is preferable to dispose the first electrode so that the surface on which the conductive layer is to be formed faces downward, and to form the conductive layer in a state in which the solution is circulated. Under the above conditions, the above-mentioned crystal layer can be formed.
[0029] The above-mentioned ratio R can be changed by changing the orientation of the first electrode during liquid phase growth, whether or not the solution is circulated, etc. The ratio R can be increased by arranging the first electrode so that the surface on which the conductive layer is to be formed faces downward. In addition, the ratio R can be increased by forming the conductive layer while the solution is circulating.
[0030] Before forming the zinc oxide layer, a base layer made of zinc oxide may be formed in advance. For example, the base layer made of zinc oxide may be formed by a gas phase method. Examples of the gas phase method include atomic layer deposition (ALD), sputtering, and chemical vapor deposition (CVD). The use of the base layer makes it easier to form the zinc oxide layer by a liquid phase deposition method. The ALD method is preferable because it is easy to form a layer in the recesses of the porous portion.
[0031] A conductive layer other than a zinc oxide layer (for example, a conductive layer made of the conductive metal oxide described above) can also be formed by liquid phase epitaxy. In that case, a solution appropriate for the conductive metal oxide to be formed may be selected.
[0032] The method of forming the conductive layer other than the crystal layer is not limited. The conductive layer other than the surface layer may be formed by a gas phase method or a liquid phase method. Examples of the gas phase method include the gas phase method described above. The entire conductive layer may be formed by a liquid phase growth method, or the entire conductive layer may be formed under the same conditions as the conditions for forming the surface layer described above. When the entire conductive layer is formed by the liquid phase growth method, as described above, a base layer may be formed in advance on the dielectric layer. Alternatively, a first conductive layer having a certain thickness may be formed on the dielectric layer by an ALD method, and then a second conductive layer may be formed by a liquid phase growth method. In either case, the surface layer of the conductive layer is formed under the conditions for forming the crystal layer.
[0033] When the conductive layer includes a first conductive layer and a second conductive layer, the first conductive layer and the second conductive layer may be formed by the same formation method or different formation methods. For example, the first conductive layer and the second conductive layer having different compositions may be formed by the same formation method. Alternatively, the first conductive layer and the second conductive layer having the same composition may be formed by different formation methods.
[0034] Step (ii) is a step of forming a second electrode on the conductive layer. At this time, the second electrode is formed on the surface layer of the conductive layer. By forming the second electrode on the surface layer having a rough surface, it is possible to firmly fix the conductive layer and the second electrode.
[0035] The second electrode is formed using a material having electrical conductivity. The material of the second electrode is not particularly limited, and may be any material that can be used as an electrode of a capacitor. The method of forming the second electrode is not particularly limited, but it is preferable to use a method of forming the second electrode that firmly connects the conductive layer and the second electrode. For example, the second electrode may be formed by applying a conductive paste containing conductive particles. Alternatively, the second electrode may be formed by a vapor phase method, a plating method, or the like.
[0036] The second electrode may include a carbon layer and a silver particle layer laminated in order from the conductive layer side. In that case, first, a carbon paste containing conductive carbon particles is applied. Next, a silver paste containing silver particles is applied. Then, a heat treatment is performed to form a carbon layer and a silver particle layer. In this way, the second electrode is formed. Note that, if necessary, heat treatment may be performed not only after application of the silver paste but also before application of the silver paste. The carbon paste and silver paste are not limited, and known carbon paste and silver paste may be used.
[0037] Through the above steps, a capacitor element including a first electrode, a dielectric layer, a conductive layer, and a second electrode is formed. After step (ii), if necessary, a lead may be connected, or the capacitor element may be housed in an exterior body. In this manner, a capacitor (C) is obtained.
[0038] Examples of the configuration and constituent members of the capacitor (C) are described below. Known constituent members may be used for the constituent members other than those characteristic of the present disclosure.
[0039] (1st electrode) The first electrode can be formed using a valve metal, an alloy containing a valve metal, a compound containing a valve metal, or the like. These materials may be used alone or in combination of two or more. For example, aluminum, tantalum, niobium, and titanium are preferably used as the valve metal. For the first electrode, a foil of the above material (for example, a metal foil such as an aluminum foil) may be used.
[0040] The first electrode having a porous portion on its surface can be obtained, for example, by roughening the surface of a metal foil containing a valve metal. The roughening may be performed by electrolytic etching or the like.
[0041] The first electrode may be formed by sintering particles of the above material. For example, the first electrode may be a sintered body of tantalum. When the first electrode is a sintered body, a porous portion exists on the surface of the first electrode. When the first electrode is a sintered body, the capacitor (C) may include an anode wire partially embedded in the sintered body.
[0042] (Dielectric layer) The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer may be formed by anodizing a valve metal on the surface of the first electrode (e.g., a metal foil). The dielectric layer may be formed so as to cover at least a part of the first electrode. The dielectric layer is usually formed on the surface of the first electrode. When a porous portion exists on the surface of the first electrode, the dielectric layer is formed on the surface of the porous portion of the first electrode.
[0043] A typical dielectric layer includes an oxide of a valve metal. The first electrode may be formed of a valve metal, and the dielectric layer may be formed of an oxide of the valve metal. For example, when tantalum is used as the material of the first electrode, the dielectric layer may be a tantalum oxide layer. When aluminum is used as the material of the first electrode, the dielectric layer may be an aluminum oxide layer. However, the dielectric layer is not limited to these, and may be any layer that functions as a dielectric layer.
[0044] (2nd electrode) The second electrode is a layer having electrical conductivity. The second electrode may be formed using conductive carbon or metal. Specifically, the second electrode may be formed using a carbon paste containing conductive carbon particles or a metal paste containing metal particles. Alternatively, the second electrode may include a layer made of only metal (a vapor deposition layer or a metal foil). Examples of conductive carbon include graphite, carbon black, graphene flakes, and carbon nanotubes. Examples of metal paste include a silver paste containing silver particles.
[0045] The second electrode may include a first layer formed on the conductive layer and a second layer formed on the first layer. In this case, the first layer may be a carbon layer containing conductive carbon, and the second layer may be a layer formed of a metal paste.
[0046] (Leads and case) The capacitor (C) may include other components as necessary, for example, leads and an exterior body. There are no particular limitations on the leads and exterior body, and known leads and exterior bodies may be used.
[0047] (Capacitor (C) structure) The capacitor (C) may include only one capacitor element. Alternatively, the capacitor (C) may include multiple capacitor elements. For example, the capacitor element (C) may include multiple capacitor elements connected in parallel. The multiple capacitor elements (C) are usually connected in parallel in a stacked state and covered with an exterior body.
[0048] Examples of embodiments according to the present disclosure will be specifically described below with reference to the drawings. The above-mentioned components can be applied to the components of the examples described below. The examples described below can be modified based on the above description. The matters described below may be applied to the above-mentioned embodiments. In the embodiments described below, components that are not essential to the capacitor of the present disclosure may be omitted. Note that the following figures are schematic and may differ from the actual configuration.
[0049] (Embodiment 1) Fig. 1 is a cross-sectional view showing a schematic view of a portion of the capacitor according to embodiment 1. Capacitor 10 shown in Fig. 1 includes a first electrode 111, a dielectric layer 112, and capacitor element 100 includes first electrode 111, dielectric layer 112, conductive layer 120, and second electrode 131. Note that an actual capacitor usually includes leads and an exterior body, but Fig. 1 shows only a portion of the capacitor element.
[0050] The dielectric layer 112 is formed so as to cover at least a portion of the surface of the first electrode 111. The conductive layer 120 is formed so as to cover at least a portion of the dielectric layer 112. The second electrode 131 is formed so as to cover at least a portion of the conductive layer 120. The conductive layer 120 is the conductive layer described above.
[0051] The first electrode 111 in the example shown in Fig. 1 has a porous portion 111a on the surface. The actual porous portion 111a may have a more complicated shape, but the porous portion 111a is depicted in a simplified form in Fig. 1. At least the surface layer 120a of the conductive layer 120 is the above-mentioned crystalline layer.
[0052] (Additional Note) Based on the above description, the following techniques are disclosed. (Technology 1) A capacitor, A first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; a second electrode disposed on the conductive layer; a surface layer of the conductive layer is a crystal layer composed of crystal grains made of an inorganic material, The crystal grains include columnar crystals. (Technology 2) The capacitor according to Technology 1, wherein in a cross section of the crystal layer parallel to a thickness direction Dt of the conductive layer, the area of the crystal grains in which the angle α between the c-axis direction and the thickness direction Dt is less than 60° accounts for 80% or more of the area of the crystal layer. (Technology 3) the conductive layer is made of an inorganic material containing a metal oxide, The capacitor according to claim 1 or 2, wherein the crystal layer is made of the metal oxide. (Technology 4) The capacitor according to technology 3, wherein the metal oxide is a conductive metal oxide mainly composed of at least one selected from the group consisting of ZnO, TiO2, SnO2, CuInO2, and CuCrO2. (Technology 5) The capacitor according to claim 4, wherein the conductive metal oxide contains an additive element for improving conductivity. (Technology 6) The capacitor according to any one of Techniques 1 to 5, wherein the first electrode is an anode and the second electrode is a cathode. (Technology 7) The capacitor according to any one of Techniques 1 to 6, wherein the first electrode is an aluminum foil or a tantalum sintered body. (Technology 8) the first electrode has a porous portion on a surface layer, the dielectric layer is formed on a surface of the porous portion, The capacitor according to any one of Techniques 1 to 7, wherein a part of the conductive layer is disposed in the voids of the porous portion. (Technology 9) the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode; The capacitor according to any one of techniques 1 to 8, wherein the second conductive layer has the crystal layer and a composition different from a composition of the first conductive layer. EXAMPLES
[0053] The capacitor (C) according to the present disclosure will be described in more detail with reference to examples.
[0054] (Experiment 1) In experiment 1, we fabricated and evaluated several capacitors (capacitor elements) with different conductive layers. The conductive layers were ZnO layers formed under different conditions.
[0055] (Capacitor A1) Capacitor A1 was fabricated by the following method. First, an aluminum foil was prepared with a dielectric layer (aluminum oxide layer) formed on its surface. The aluminum foil used had porous portions formed on its surface by etching. The aluminum oxide layer was formed by subjecting the aluminum foil to a chemical conversion treatment.
[0056] Next, a base layer made of zinc oxide was formed on the dielectric layer by the ALD method. Next, a crystalline layer (conductive layer) made of zinc oxide (ZnO) was formed on the base layer. The size of the zinc oxide layer was about 1 cm x 2 cm. Specifically, the aluminum foil on which the base layer was formed was immersed in a specified solution and held for 6 hours, thereby forming a crystalline layer made of zinc oxide on the base layer.
[0057] The solution used was an aqueous solution of zinc nitrate hexahydrate and hexamethylenetetramine dissolved in a molar ratio of 1:1. The concentration of zinc nitrate hexahydrate in the solution was 0.05 mol / L. The pH of the solution was 6.5 to 7.5. The temperature of the solution was room temperature (approximately 24°C). During the growth of zinc oxide, a heater was placed in contact with the back side of the aluminum foil (the side opposite to the growth surface of zinc oxide) to heat the aluminum foil to a constant temperature (approximately 85°C).
[0058] 2 L of the above solution was placed in a tank and liquid phase growth was performed. Zinc oxide was grown by immersing an aluminum foil in the solution with the surface on which the zinc oxide layer was to be formed facing downward. The solution was circulated at a flow rate of 1 L / min.
[0059] After the zinc oxide layer was grown in liquid phase, the aluminum foil on which the zinc oxide layer was formed was washed. Next, a second electrode (silver particle layer) was formed on the zinc oxide layer. The second electrode was formed by forming circular silver particle layers with a diameter of 3 mm at eight locations on the zinc oxide layer. The silver particle layers were formed from silver paste. In this manner, the capacitor A1 was produced.
[0060] (Capacitor R1) Capacitor R1 was fabricated in the same manner and under the same conditions as capacitor A1, except that the method for forming the zinc oxide layer (conductive layer) was different. The zinc oxide layer of capacitor R1 was formed in the same manner and under the same conditions as the conductive layer of capacitor A1, except that the orientation of the aluminum foil was changed and the solution was not circulated. The zinc oxide layer of capacitor R1 was formed with the surface on which the zinc oxide layer was to be formed facing upwards.
[0061] The ratio R of the zinc oxide layer Za1 of the capacitor A1 was obtained by the following method. First, the zinc oxide layer Za1 was formed by the above-mentioned method. Next, the sample on which the zinc oxide layer Za1 was formed was cut, and the exposed cross section was processed with an ion beam in the same manner as observation with a general transmission electron microscope. Next, the cross section of the zinc oxide layer Za1 was analyzed by electron backscatter diffraction (EBSD) method. Table 1 shows the ratio of the area of the crystal grains in which the angle α between the direction of the c axis of the crystal grain and the thickness direction Dt is within a predetermined range to the area of the crystal layer (zinc oxide layer Za1). The zinc oxide layer Zr1 of the capacitor R1 was also analyzed by the same method as above. Table 1 shows the evaluation results of the zinc oxide layer Zr1.
[0062] [Table 1]
[0063] FIG. 2 shows the result of coloring the crystal grains in the zinc oxide layer Za1 according to the size of the angle α. FIG. 2 conceptually shows the angle α between the c-axis direction and the thickness direction Dt. Similarly, FIG. 3 shows the result of coloring the crystal grains in the zinc oxide layer Zr1 according to the size of the angle α. As shown in Table 1, in the zinc oxide layer Za1, the ratio R of the area of crystal grains having an angle α of less than 60° to the area of the crystal layer was 91%. Also, in the zinc oxide layer Za1, the ratio X of the area of crystal grains having an angle α of 20° or more to the area of the crystal layer was 71%.
[0064] The ratio R in the zinc oxide layer Zr1 was 49%. In addition, in the zinc oxide layer Zr1, the ratio X of the area of crystal grains having an angle α of 20° or more to the area of the crystal layer (zinc oxide layer Zr1) was 96%.
[0065] Electron microscope images of the surfaces of the zinc oxide layers of capacitors A1 and R1 were observed. From the above analysis results and the electron microscope images of the surface of zinc oxide layer Za1, it was found that the surface layer of zinc oxide layer Za1 of capacitor A1 was a crystalline layer having columnar crystals extending in the c-axis direction. On the other hand, from the above analysis results and the electron microscope images of the surface of zinc oxide layer Zr1, it was found that the surface layer of zinc oxide layer Zr1 of capacitor R1 was composed of particulate zinc oxide.
[0066] The capacitance and electrical resistance of the produced capacitors A1 and R1 were measured. The average capacitance and electrical resistance of each of the eight capacitors were calculated. The measurement results are shown in Table 2.
[0067] [Table 2]
[0068] Capacitor A1 is the capacitor (C) according to the present disclosure. Capacitor R1 is a comparative example. As shown in Table 2, the capacitance of capacitor A1 was significantly higher than that of capacitor R1. Furthermore, the electrical resistance of capacitor A1 was significantly lower than that of capacitor R1. [Industrial Applicability]
[0069] The present disclosure can be used for capacitors. [Explanation of symbols]
[0070] 10: Capacitor 111: 1st electrode 111a: Porous part 112: Dielectric layer 120: Conductive layer 120a: Surface layer 131:Second electrode Dt: Thickness direction
Claims
1. A capacitor, A first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; a second electrode disposed on the conductive layer; a surface layer of the conductive layer is a crystal layer composed of crystal grains made of an inorganic material, The crystal grains include columnar crystals.
2. 2. The capacitor of claim 1, wherein in a cross section of the crystal layer parallel to a thickness direction Dt of the conductive layer, the area of the crystal grains in which the angle α between the c-axis direction and the thickness direction Dt is less than 60° accounts for 80% or more of the area of the crystal layer.
3. the conductive layer is made of an inorganic material containing a metal oxide, The capacitor according to claim 1 , wherein the crystal layer is made of the metal oxide.
4. The metal oxide is ZnO, TiO 2 , SnO 2 , CuInO 2 , and CuCrO 2 4. The capacitor according to claim 3, wherein the conductive metal oxide is composed mainly of at least one selected from the group consisting of:
5. The capacitor of claim 4 , wherein the conductive metal oxide includes an additive element for improving electrical conductivity.
6. 3. The capacitor of claim 1, wherein the first electrode is an anode and the second electrode is a cathode.
7. 3. The capacitor according to claim 1, wherein the first electrode is an aluminum foil or a tantalum sintered body.
8. the first electrode has a porous portion on a surface layer, the dielectric layer is formed on a surface of the porous portion, The capacitor according to claim 1 , wherein a part of the conductive layer is disposed within the voids of the porous portion.
9. the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode; The capacitor according to claim 1 , wherein the second conductive layer includes the crystalline layer and has a composition different from a composition of the first conductive layer.
Citation Information
Patent Citations
Solid electrolytic capacitor
JP2017103412A
Solid electrolytic capacitor and method of manufacturing the same
JP2020035890A