Thermal response ceramic fire-resistant explosion-proof pad and preparation method thereof
Thermal response ceramicized fire-resistant explosion-proof pad prepared by two-step impregnation cross-linking method and freeze-drying method solves the problems of ceramic layer falling off and inorganic filler agglomeration, realizes the dense formation and flame retardant effect of ceramic layer at high temperature, and improves the battery Protection and cable fire resistance.
Patent Information
- Application Number
- CN202411077458.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The different thermal expansion rates of the existing ceramic layer and the polymer lead to shedding, and excessive inorganic fillers are prone to agglomeration, resulting in a deterioration of the mechanical properties of the polymer.
Thermal response ceramic fire-resistant explosion-proof pad is prepared by two-step impregnation cross-linking method. The physical and chemical cross-linking of inorganic nanofibers and PDMS elastomers are formed to form a three-dimensional network structure, and flux is used to promote the formation of high-temperature dense ceramic layers to avoid external force damage. , and the thermal insulation of the aerogel is improved by freeze-drying.
Maintain high toughness and impact resistance at low temperatures, and generate dense ceramic layers at high temperatures to isolate flames and oxygen, achieve flame retardant and fire-resistant effects, and improve battery protection and cable fire-proof and thermal insulation performance.
Smart Images

Figure CN118930220A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of battery protection materials, and specifically relates to a thermally responsive ceramic fire-resistant explosion-proof pad and a preparation method thereof. Background Art
[0002] With the development of social economy and the proposal of "dual carbon" goals, the number of new energy vehicles, large energy storage equipment, electronic equipment and medical equipment powered by battery systems is increasing, which requires higher energy density for battery systems. As a result, the probability of combustion and explosion of battery systems is gradually increasing. The combustion and explosion of battery systems will cause the combustion and explosion of the entire equipment, endangering human life and property safety, and in severe cases, causing death. Among the three mandatory national standards for electric vehicles issued in 2020, "Safety Requirements for Power Batteries for Electric Vehicles" requires that after the battery cell has thermal runaway, the battery system will not catch fire or explode within 5 minutes. Therefore, it is very important to improve the safety of the battery system.
[0003] At present, the most common material for battery flame retardant protection is inorganic aerogel. Although it has the advantages of high strength, high flame retardancy, and high temperature stability, it has poor toughness and is difficult to resist the impact force generated by battery explosion. Although polymer aerogel has high toughness and high elasticity, its thermal stability is very poor. It usually decomposes at 400-500°C and has poor flame retardant properties. In recent years, people have found that ceramic silicone rubber maintains the basic properties of silicone rubber at room temperature, such as impact resistance, shock absorption, excellent toughness and resilience, and is converted into inorganic ceramic materials at high temperatures. It has excellent fire resistance, excellent flame retardancy, excellent electrical insulation, excellent chemical resistance, and excellent mechanical properties. Ceramic silicone rubber is a new type of material prepared by adding special fillers to the silicone rubber matrix. It is widely used in cable insulation, fireproof layer, battery insulation felt and other fields. However, there are many problems in the use of ceramic silicone rubber. For example, if too much inorganic filler is added to ceramic silicone rubber, the inorganic fillers will agglomerate and the mechanical properties of the polymer will decrease. The different thermal expansion coefficients between the ceramic layer and the silicone rubber will cause the ceramic layer to delaminate and fall off. Therefore, researchers have modified the ceramic silicone rubber material, used its ceramicization mechanism at high temperature, and compounded it with inorganic materials to prepare a new battery protection material that is flame retardant, fire resistant and explosion-proof.
[0004] Ceramic silicone rubber has excellent toughness at low temperatures and can be cracked into amorphous ceramics at high temperatures. It has excellent thermal stability, chemical corrosion resistance, waterproofness, electrical insulation, environmental stability and other properties. It has shown broad application prospects in the fields of cable flame retardancy, heat insulation, hydrophobic agent, insulation, etc. The impregnation crosslinking method is a method of quickly building a chemical and physical double crosslinking network to achieve organic material coating of inorganic materials, further improving the bonding stability between inorganic materials while providing elastic support for the three-dimensional crosslinking network. The polymer is coated on the surface of inorganic nanofibers through two-step impregnation crosslinking, which provides elastic support for inorganic nanofibers and improves the bonding force between fibers, so as to achieve energy absorption and shock reduction through the spatial movement of organic chains during low-temperature use. Chemical crosslinking ensures that the structure of the aerogel composite material is not destroyed when it is impacted. During use, the ceramic silicone rubber is eroded by flames to form an amorphous ceramic layer, which prevents external oxygen and flames from contacting the internal polymer, achieving a flame retardant effect. At the same time, inorganic aerogel materials with a stable three-dimensional network are prepared by freeze-drying. Inorganic nanofibers can serve as flux and a stable three-dimensional skeleton to make the ceramic layer denser. Therefore, the preparation of high-temperature thermally responsive nanofiber composite aerogel is very meaningful for the fire resistance and explosion protection of batteries.
[0005] Lin et al. (Xin-Cen Lin, Shu-Liang Li, Wen-Xiong Li, et al. Thermo-Responsive Self-Ceramifiable Robust Aerogel with Exceptional Strengthening and Thermal Insulating Performance at Ultrahigh Temperatures [J]. ADVANCED FUNCTIONAL MATERIALS, 2023, 33 (2214913): 1-11) prepared polyorganosiloxane aerogel by freeze drying, and added ammonium polyphosphate / zinc borate (APP / ZB) as fluxing components and montmorillonite (MMT) / mica as refractory components into the aerogel to obtain a thermal protective aerogel with unique thermal response ceramicization ability, excellent thermal insulation performance and high strength at high temperature. However, too much inorganic filler is added to the aerogel, and the inorganic filler is easy to agglomerate during the preparation process, resulting in reduced mechanical properties of the polyorganosiloxane aerogel.
[0006] He Chunjiang (He Chunjiang. Effect of mica powder / glass powder / sintering aid combined use on the performance of silicone rubber [J]. Rubber Industry, 2022, 69(01): 34-38) The use of a mica powder / glass powder / sintering aid combined system promotes the rapid formation of a uniform, dense, and continuous ceramic layer of silicone rubber at high temperatures, which can block heat and oxygen from entering the interior of the silicone rubber and achieve the purpose of flame retardancy. However, the combined system introduces too much inorganic filler, which reduces the tensile properties of silicone rubber.
[0007] The Chinese patent "A ceramic flame-retardant coating coated silicone rubber foam and its preparation process" (application number: 202210886260.8, authorization number: CN115073921B, announcement date: 2024.01.26) discloses a ceramic flame-retardant coating coated silicone rubber foam and its preparation process. First, the silicone rubber foam is prepared, and then the ceramic coating slurry is used to coat the sandwich structure of the silicone rubber foam, and the silicone rubber foam with a limiting oxygen index of 42% is obtained. However, this method requires supercritical foaming in a nitrogen atmosphere, the preparation process is complicated, and the temperature range that the silicone rubber matrix can withstand is low, and it is difficult to provide a stable support structure. Summary of the invention
[0008] The purpose of the present invention is to provide a thermally responsive ceramic fireproof explosion-proof pad and a preparation method thereof, which solves the problems in the prior art of falling off due to different thermal expansion rates between the ceramic layer and the polymer, and excessive agglomeration of inorganic fillers leading to a decrease in the mechanical properties of the polymer.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] A thermally responsive ceramic fireproof explosion-proof pad and a preparation method thereof, which is specifically implemented according to the following steps:
[0011] Step 1, preparation of dispersion
[0012] Dispersing inorganic nanofibers and flux in deionized water and uniformly mixing by ultrasonic mixing to obtain a uniform dispersion;
[0013] Step 2: Preparation of inorganic nanofiber aerogel
[0014] Adding a frozen binder to the dispersion prepared in step 1, heating in a water bath to mix evenly, and then placing in a refrigerator for pre-freezing to obtain a wet gel; pouring the wet gel into a freezing mold, and placing the mold in a freeze dryer for freeze drying to obtain an inorganic nanofiber aerogel;
[0015] Step 3, Aerogel Prepreg
[0016] The silane coupling agent, the organic solvent and the deionized water are uniformly mixed to obtain a pre-impregnation solution, and the inorganic nanofiber aerogel prepared in step 2 is impregnated in the pre-impregnation solution until the inorganic nanofiber aerogel is completely saturated, and then the inorganic nanofiber aerogel is placed in a drying oven to dry, and the dried inorganic nanofiber aerogel is repeatedly cleaned with an anhydrous ethanol solution;
[0017] Step 4: Impregnation with silicone
[0018] The hydroxyl-terminated PDMS, the vinyl-terminated PDMS, the catalyst and the organic solvent are mixed uniformly with the aid of ultrasound and stirring to obtain a silica gel impregnation solution; the inorganic nanofiber aerogel obtained in step 3 is immersed in the silica gel impregnation solution until saturated, and then placed in a high-temperature reactor for cross-linking reaction; the inorganic nanofiber aerogel is then immersed in a mixed solution of anhydrous ethanol and ethylene glycol, and the mixed solution of anhydrous ethanol and ethylene glycol is replaced multiple times to achieve solvent replacement;
[0019] Step 5: Drying and curing
[0020] The impregnated cross-linked aerogel prepared in step 4 is placed in a drying oven for drying and curing to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0021] Furthermore, in step 1, the inorganic nanofiber is SiO 2 、TiO 2 、Si 3 N 4 , SiC and other nanofibers; the flux is boron trioxide B 2 O 3 、Zinc borate Zn 3 B 2 O 6 , boric acid H 3 BO 3 、Vanadium pentoxide V 2 O 5 、Silicon dioxide SiO 2 Any of the following:
[0022] The mass ratio of flux to inorganic nanofiber is 1:10-1:15, the mass ratio of inorganic nanofiber to deionized water is 1:10-1:20, the ultrasonic time is 15-30 minutes, the ultrasonic power is 200-300W, and the frequency is 140-160Hz.
[0023] Furthermore, in step 2, the frozen binder is any one of polyvinyl alcohol PVA and polyvinyl pyrrolidone PVP, the mass fraction of the frozen binder is between 7wt.% and 15wt.%, the mass ratio of the frozen binder to the dispersion is 1:20 to 1:30, the water bath temperature is 50 to 80°C, the stirring time is 30 to 60 minutes, the refrigerator compartment temperature is 0 to 10°C, the refrigeration time is 1 to 3 hours, the freezing temperature of the freeze dryer is -50 to -40°C, and the freezing time is 24 to 48 hours.
[0024] Furthermore, in step 3, the silane coupling agent is any one of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(β-methoxyethoxy) silane, γ-aminopropyl triethoxysilane, γ-(2,3-epoxypropoxy)propyl trimethoxysilane, and γ-methacryloxypropyl trimethoxysilane, the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile, tetrahydrofuran, and dimethylformamide, and the pre-impregnation solution is composed of the following substances by mass percentage: 20% to 30% of silane coupling agent, 40% to 50% of organic solvent, and 20% to 30% of deionized water, the sum of the above components is 100%, the inorganic nanofiber aerogel impregnation time is 12 to 18 hours, the drying temperature is 50 to 70° C., the drying time is 2 to 4 hours, and the number of washing times with anhydrous ethanol is 10 to 20 times.
[0025] Furthermore, in step 4, the catalyst is any one of tetrabutylammonium difluorotriphenylsilicate and organic cyclic polyphosphazene base, and the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile, tetrahydrofuran, and dimethylformamide; the silica gel impregnation solution includes 5% to 7% of terminal hydroxyl PDMS, 4% to 8% of terminal vinyl PDMS, 20% to 30% of catalyst and 55% to 71% of organic solvent by mass percentage, and the sum of the above components is 100%; ultrasonication is performed in an ultrasonic machine with a power of 200 to 300 W and a frequency of 140 to 160 Hz for 20 to 30 minutes, and then the stirring time is 30 to 60 minutes, the immersion time of the inorganic nanofiber aerogel is 12 to 18 hours, the crosslinking temperature is 80 to 90° C., the crosslinking time is 3 to 4 hours, the single immersion time of the inorganic nanofiber aerogel in the mixed solution of anhydrous ethanol and ethylene glycol is 20 to 30 minutes, and the mixed solution of anhydrous ethanol and ethylene glycol is replaced 3 to 5 times;
[0026] Anhydrous ethanol and ethylene glycol solution are mixed in a ratio of 1:1, with 50 to 100 ml of anhydrous ethanol and ethylene glycol solution.
[0027] Furthermore, the impregnated cross-linked aerogel in step 5 is placed in a drying oven at 60 to 120° C. and dried for 3 to 5 hours.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The thermally responsive ceramic fireproof explosion-proof pad prepared by the present invention can make the aerogel maintain high toughness and excellent impact resistance at low temperature. The PDMS elastomer is used to physically and chemically cross-link and wrap the three-dimensional network of inorganic materials. When external force impacts, energy dissipation can be achieved through the elongation or contraction of the chain and the slippage between fibers. The chemical cross-linking avoids the damage of the material structure by external force, so that the material can maintain high toughness. At high temperature, the PDMS on the surface will be cracked, and dense SiO 2 The ceramic layer can isolate the internal material from external high-temperature flames and oxygen, thereby achieving flame retardant and fire-resistant effects. It has broad application prospects in battery protection, cable fire prevention, heat insulation, impact resistance and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a partial cross-sectional schematic diagram of the thermally responsive ceramic fire-resistant and explosion-proof composite aerogel prepared by the present invention;
[0031] Figure 2 It is an XRD spectrum of a ceramic layer generated after the PDMS impregnation layer of the thermally responsive ceramic fire-resistant explosion-proof composite aerogel prepared by the present invention is burned.
[0032] In the figure, 1-PDMS impregnation layer, 2-inorganic nanofiber. DETAILED DESCRIPTION
[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] A method for preparing a thermally responsive ceramic fire-resistant explosion-proof pad is specifically implemented according to the following steps:
[0035] Step 1, preparation of dispersion
[0036] The flux and inorganic nanofibers are dispersed in deionized water, and ultrasonicated for 15 to 20 minutes using an ultrasonic machine with an ultrasonic power of 200 to 300 W and a frequency of 140 to 160 Hz to obtain a uniform dispersion. 2 、TiO 2 、Si 3 N 4 , SiC and other nanofibers, the flux is boron trioxide (B 2 O 3 ), zinc borate (Zn 3 B 2 O 6 ), boric acid (H 3 BO 3 ), vanadium pentoxide (V 2 O 5 ), silicon dioxide (SiO2 ), the mass ratio of the inorganic nanofibers to the deionized water is 1:10 to 1:20, and the mass ratio of the flux to the inorganic nanofibers is 1:10 to 1:15.
[0037] Step 2: Preparation of inorganic nanofiber aerogel
[0038] The dispersion obtained in step 1 is added with a freezing binder, the mass ratio of the freezing binder to the dispersion is 1:20 to 1:30, stirred in a water bath at 50 to 80°C for 30 to 60 minutes and then cooled to room temperature, and then the mixed solution is placed in a refrigerator at 0 to 10°C for pre-freezing for 1 to 3 hours to obtain a wet gel; the wet gel is poured into a freezing mold, and the mold is placed in a freeze dryer for freeze drying to obtain an inorganic nanofiber aerogel. The freeze drying temperature is -50 to -40°C, and the freeze drying time is 24 to 48 hours. The freezing binder is any one of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polystyrene (PS), etc., and the mass fraction of the freezing binder should be between 7wt.% and 15wt.%.
[0039] Step 3, Aerogel Prepreg
[0040] The silane coupling agent, the organic solvent and the deionized water are uniformly mixed to obtain a pre-impregnation solution, which is prepared according to the following mass percentages: 20% to 30% of the silane coupling agent, 40% to 50% of the organic solvent, 20% to 30% of the deionized water, and the total of the above components is 100%.
[0041] The inorganic nanofiber aerogel in step 2 is immersed in the above-mentioned pre-impregnation solution for 12 to 18 hours until the inorganic nanofiber aerogel is completely saturated, and then the inorganic nanofiber aerogel is placed in a drying oven at 50 to 70° C. and dried for 2 to 4 hours, and then the inorganic nanofiber aerogel is repeatedly cleaned 10 to 20 times with anhydrous ethanol solution. The silane coupling agent is any one of vinyl triethoxysilane (A151), vinyl trimethoxysilane (A171), vinyl tri(β-methoxyethoxy) silane (A172), γ-aminopropyl triethoxysilane (KH550), γ-(2,3-epoxypropoxy)propyl trimethoxysilane (KH560), γ-methacryloxypropyl trimethoxysilane (KH570), etc., and the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile (ACN), tetrahydrofuran (THF), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc.
[0042] Step 4: Impregnation with silicone
[0043] The hydroxyl-terminated PDMS, the vinyl-terminated PDMS, the catalyst and the organic solvent are ultrasonicated for 20 to 30 minutes in an ultrasonic machine with a power of 200 to 300 W and a frequency of 140 to 160 Hz, and then stirred for 30 to 60 minutes to obtain a silica gel impregnation solution, wherein the silica gel impregnation solution is configured according to the following mass percentages: 5% to 7% of the hydroxyl-terminated PDMS, 4% to 8% of the vinyl-terminated PDMS, 20% to 30% of the catalyst and 55% to 71% of the organic solvent, and the sum of the above components is 100%.
[0044] The inorganic nanofiber aerogel obtained in step 3 is immersed in the above solution for 12 to 18 hours until the inorganic nanofiber aerogel is completely saturated with the impregnation solution, and is placed in a high-temperature reactor for cross-linking at 80 to 90° C. for 3 to 4 hours to obtain an impregnated cross-linked aerogel; 50 to 100 ml of anhydrous ethanol and 50 to 100 ml of ethylene glycol solution are uniformly mixed, and the impregnated cross-linked aerogel is placed in the mixed solution of anhydrous ethanol and ethylene glycol and immersed for 20 to 30 minutes, and then the mixed solution of anhydrous ethanol and ethylene glycol is replaced, and the impregnated cross-linked aerogel is repeatedly placed in the mixed solution of anhydrous ethanol and ethylene glycol and immersed for 3 to 5 times. The ratio of anhydrous ethanol to ethylene glycol is 1:1, the catalyst is any one of tetrabutylammonium difluorotriphenylsilicate (TBAT) and organic cyclic polyphosphazene base, and the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile (ACN), tetrahydrofuran (THF), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc.
[0045] Step 5: Drying and curing
[0046] The impregnated cross-linked aerogel obtained in step 4 is placed in a drying oven at 60 to 120° C. and dried for 3 to 5 hours to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0047] Figure 1 Schematic diagram of a partial cross section of a heat-responsive fire-resistant and impact-resistant composite material prepared by the present invention. Figure 1 It can be seen that after two-step impregnation and cross-linking, the thermal responsive PDMS impregnation layer 1 is evenly coated on the surface of the inorganic nanofibers 2, and the bonding force between the fibers depends on PDMS.
[0048] Figure 2 This is the XRD spectrum of the ceramic layer generated after the PDMS impregnation layer is burned. Figure 2 It can be seen that after the PDMS is burned, a pure amorphous SiO2 ceramic layer is generated, which does not contain carbon impurities.
[0049] The present invention selects inorganic nanofibers to construct a stable three-dimensional network. When PDMS undergoes phase transition at high temperature, the stable three-dimensional network can support the PDMS structure without collapse, thereby reducing SiO2 The cracking probability of the ceramic layer is reduced. At the same time, the inorganic nanofibers can be used as flux to promote the formation of a dense ceramic layer. The inorganic nanofiber aerogel is prepared by freeze-drying to ensure the thermal insulation of the aerogel. When the outer layer of aerogel is eroded by flame, the good thermal insulation performance can enable the aerogel to form a ceramic layer, while the internal aerogel still maintains its high toughness and high resilience, thereby being able to resist the impact caused by the battery explosion. The inorganic nanofiber network is coated with a layer of PDMS elastomer with high toughness by the impregnation cross-linking method. Its physical cross-linking can achieve effective energy dissipation, while the chemical cross-linking can enhance the bonding force between the fibers. When impacted, it can dissipate energy to a certain extent but ensure that the three-dimensional network is not destroyed, thereby realizing the fire-resistant and explosion-proof integrated function of the composite aerogel.
[0050] The present invention prepares a highly elastic fire-resistant and explosion-proof composite aerogel with high-temperature thermal response through freeze drying and two-step impregnation cross-linking, fully utilizes the three-dimensional network of inorganic fibers as a supporting skeleton to ensure that the ceramic layer does not crack due to excessive shrinkage of the polymer during high-temperature phase change, and at the same time uniformly coats the PDMS elastomer on the outside of the three-dimensional network, with the purpose of utilizing the physical cross-linking of the elastomer to ensure reversible energy dissipation when impacted, while chemical cross-linking increases the bonding force between nanofibers to prevent stratification between fibers. The composite aerogel has broad application prospects in the fields of battery fire and explosion prevention, cable fire insulation, battery thermal shock resistance, and aerospace device insulation.
[0051] Example 1 Preparation of SIO 2 / PDMS composite aerogel
[0052] First, 5g SiO 2 Inorganic nanofibers and 0.5 g B 2 O 3 The flux was dispersed in 50 ml of deionized water and ultrasonicated for 30 min using an ultrasonic machine with a power of 200 W and a frequency of 140 Hz to obtain a uniform dispersion;
[0053] Then, 2.7775 g of PVA solution with a mass fraction of 7 wt.% was added to the above dispersion, and the mixture was stirred in a water bath at 50°C for 60 min and then cooled to room temperature. The mixed solution was placed in a refrigerator at 10°C for pre-freezing for 3 h to obtain a wet gel. The wet gel was poured into a directional freeze-drying mold, placed in a freeze dryer at -50°C for freeze-drying for 24 h to obtain SiO 2 Fiber aerogel;
[0054] Mix 2.36g KH560, 5.9g DMF, and 5ml deionized water evenly, and then add SiO 2The fiber aerogel was immersed in the mixed solution for 12 h until SiO 2 The fiber aerogel was completely saturated with the solution, and then SiO 2 The fiber aerogel was placed in a drying oven at 50 °C for 2 h, and the SiO 2 The fiber aerogel was repeatedly cleaned 10 times;
[0055] 5.0 g of hydroxyl-terminated PDMS, 4.0 g of vinyl-terminated PDMS, 20.0 g of TBAT, and 71.0 g of DMF solution were ultrasonicated for 30 min using an ultrasonic machine with a power of 200 W and a frequency of 140 Hz, and then stirred for 30 min to obtain a silica gel impregnation solution; 50 ml of anhydrous ethanol and 50 ml of ethylene glycol solution were uniformly mixed, and then SiO 2 The fiber aerogel was placed in the mixed solution and soaked for 20 min, then the anhydrous ethanol and ethylene glycol solutions were replaced to 2 The fiber aerogel was re-immersed in the replaced anhydrous ethanol and ethylene glycol solutions, and the replacement of the anhydrous ethanol and ethylene glycol solutions was repeated 5 times;
[0056] After repeated immersion, SiO 2 The fiber aerogel was placed in a drying oven at 60°C and dried for 5 hours to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0057] Example 2 Preparation of SIC / PDMS composite aerogel
[0058] First, 4.0 g SiC inorganic nanofibers were mixed with 0.33 g Zn 3 B 2 O 6 The flux was dispersed in 60 ml of deionized water and ultrasonicated for 20 min using an ultrasonic machine with a power of 250 W and a frequency of 150 Hz to obtain a uniform dispersion;
[0059] Then, 2.57 g of PVP solution with a mass fraction of 12 wt.% was added to the above dispersion, and the mixture was stirred in a water bath at 60°C for 40 min and then cooled to room temperature. The mixed solution was placed in a refrigerator at 6°C for pre-freezing for 2 h to obtain a wet gel. The wet gel was poured into a mold for directional freeze drying, placed in a freeze dryer and freeze dried at -45°C for 36 h to obtain SiC fiber aerogel.
[0060] 2.48 g KH570, 4.46 g ethylene glycol, and 5 ml deionized water were mixed evenly, and the SiC fiber aerogel was immersed in the mixed solution for 17 h until the SiC fiber aerogel was completely saturated with the mixed solution. The SiC fiber aerogel was then placed in a 60 ° C drying oven for 3 h, and the SiC fiber aerogel was repeatedly washed 15 times with anhydrous ethanol solution.
[0061] 5.03 g of hydroxyl-terminated PDMS, 5.0 g of vinyl-terminated PDMS, 20.95 g of TBAT, and 48.3 g of acetonitrile solution were ultrasonicated for 25 min using an ultrasonic machine with a power of 250 W and a frequency of 150 Hz, and then stirred for 40 min to obtain a silica gel impregnation solution; 70 ml of anhydrous ethanol and 70 ml of ethylene glycol solution were uniformly mixed, and then the SiC fiber aerogel was placed in the mixed solution and soaked for 25 min, and then the anhydrous ethanol and ethylene glycol solutions were replaced, and the SiC fiber aerogel was re-immersed in the replaced anhydrous ethanol and ethylene glycol solutions, and the replacement of the anhydrous ethanol and ethylene glycol solutions was repeated 4 times;
[0062] The SiC fiber aerogel after repeated immersion was placed in a drying oven at 90°C for 4 hours to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0063] Example 3 Preparation of SI 3 N 4 / PDMS composite aerogel
[0064] First, 2.8 g Si 3 N 4 Inorganic nanofibers and 0.18 g H 3 BO 3 The flux was dispersed in 50 ml of deionized water and ultrasonicated for 15 min using an ultrasonic machine with a power of 300 W and a frequency of 160 Hz to obtain a uniform dispersion;
[0065] Then, 1.77 g of PVA solution with a mass fraction of 15 wt.% was added to the above dispersion, and the mixture was stirred in a water bath at 80°C for 30 min and then cooled to room temperature. The mixed solution was placed in a refrigerator at 1°C for pre-freezing for 1 h to obtain a wet gel. The wet gel was poured into a directional freeze-drying mold and placed in a freeze dryer for freeze-drying at -40°C for 48 h to obtain Si 3 N 4 Fiber aerogel;
[0066] Mix 6.42A171, 10.7g ethylene glycol, and 10ml deionized water. 3 N 4 The fiber aerogel was immersed in the mixed solution for 18 h until Si 3 N 4 The fiber aerogel is completely saturated with the solution, and then Si 3 N 4 The fiber aerogel was placed in a drying oven at 70 °C for 2 h and anhydrous ethanol solution was used to 3 N 4 The fiber aerogel was washed repeatedly 20 times;
[0067] 4.96 g of hydroxyl-terminated PDMS, 5.67 g of vinyl-terminated PDMS, 14.17 g of organic cyclic polyphosphazene base, and 46.06 g of n-butanol solution were ultrasonicated for 20 min using an ultrasonic machine with a power of 300 W and a frequency of 160 Hz, and then stirred for 60 min to obtain a silica gel impregnation solution; 100 ml of anhydrous ethanol and 100 ml of ethylene glycol solution were uniformly mixed, and then the silica gel was impregnated with 100 ml of anhydrous ethanol and 100 ml of ethylene glycol solution. 3 N 4 The fiber aerogel was placed in the mixed solution and soaked for 30 min, then the anhydrous ethanol and ethylene glycol solutions were replaced. 3 N 4 The fiber aerogel was re-immersed in the replaced anhydrous ethanol and ethylene glycol solutions, and the replacement of the anhydrous ethanol and ethylene glycol solutions was repeated 5 times;
[0068] After repeated immersion, Si 3 N 4 The fiber aerogel was placed in a drying oven at 120°C and dried for 3 hours to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0069] Example 4 Preparation of TIO 2 / PDMS composite aerogel
[0070] First, 3.97 g TiO 2 Inorganic nanofibers and 0.283 g H 3 BO 3 The flux was dispersed in 75 ml of deionized water and ultrasonicated for 20 min using an ultrasonic machine with a power of 300 W and a frequency of 160 Hz to obtain a uniform dispersion;
[0071] Then, 7.01 g of PVA solution with a mass fraction of 12 wt.% was added to the above dispersion, and the mixture was stirred in a water bath at 60°C for 50 min and then cooled to room temperature. The mixed solution was placed in a refrigerator at 5°C for pre-freezing for 2 h to obtain a wet gel. The wet gel was poured into a directional freeze-drying mold, placed in a freeze dryer at -50°C for freeze-drying for 48 h to obtain TiO 2 Fiber aerogel;
[0072] Mix 4.05g A151, 7.29g anhydrous ethanol and 10ml deionized water evenly, and add TiO 2 The fiber aerogel was immersed in the mixed solution for 18 h until the TiO 2 The fiber aerogel was completely saturated with the mixed solution, and then TiO 2 The fiber aerogel was placed in a drying oven at 60 °C for 2 h, and the TiO 2 The fiber aerogel was repeatedly cleaned 15 times;
[0073] 4.87 g of hydroxyl-terminated PDMS, 4.17 g of vinyl-terminated PDMS, 17.39 g of organic cyclic polyphosphazene base, and 43.13 g of n-butanol solution were ultrasonicated for 25 min using an ultrasonic machine with a power of 200 W and a frequency of 140 Hz, and then stirred for 30 min to obtain a silica gel impregnation solution; 100 ml of anhydrous ethanol and 100 ml of ethylene glycol solution were uniformly mixed, and then TiO 2 The fiber aerogel was placed in the mixed solution and soaked for 30 min, then the anhydrous ethanol and ethylene glycol solutions were replaced to 2 The fiber aerogel was re-immersed in the replaced anhydrous ethanol and ethylene glycol solutions, and the replacement of the anhydrous ethanol and ethylene glycol solutions was repeated 5 times;
[0074] After repeated immersion, the TiO 2 The fiber aerogel was placed in a drying oven at 120°C and dried for 3 hours to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
[0075] Table 1 is a comparison of the flame retardant and mechanical properties of the battery protection aerogel materials in Examples 1-4. As can be seen from Table 1, in terms of mechanical properties, the PDMS-impregnated inorganic nanofiber aerogel has excellent room temperature tensile strength and high temperature tensile strength, and at high temperatures, PDMS, flux and inorganic nanofibers synergize to generate a dense ceramic layer, so that the high temperature tensile strength is higher than the room temperature tensile strength, and the ceramic layer can resist the impact of the explosion to a certain extent. At the same time, according to the data of heat release rate, total heat release rate and limiting oxygen index, it can be seen that the ceramic layer generated by PDMS at high temperature can isolate external oxygen and heat, and play a certain flame retardant effect.
[0076] Table 1 Flame retardant and mechanical properties of battery protection aerogel materials in Examples 1-4
[0077]
[0078]
[0079] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a thermally responsive ceramic fire-resistant explosion-proof pad. It is characterized in that Follow the steps below to implement it: Step 1, preparation of dispersion Dispersing inorganic nanofibers and flux in deionized water and uniformly mixing by ultrasonic mixing to obtain a uniform dispersion; Step 2: Preparation of inorganic nanofiber aerogel Adding a frozen binder to the dispersion prepared in step 1, heating in a water bath to mix evenly, and then placing in a refrigerator for pre-freezing to obtain a wet gel; pouring the wet gel into a freezing mold, and placing the mold in a freeze dryer for freeze drying to obtain an inorganic nanofiber aerogel; Step 3, Aerogel Prepreg The silane coupling agent, the organic solvent and the deionized water are uniformly mixed to obtain a pre-impregnation solution, and the inorganic nanofiber aerogel prepared in step 2 is impregnated in the pre-impregnation solution until the inorganic nanofiber aerogel is completely saturated, and then the inorganic nanofiber aerogel is placed in a drying oven to dry, and the dried inorganic nanofiber aerogel is repeatedly cleaned with an anhydrous ethanol solution; Step 4: Impregnation with silicone The hydroxy-terminated PDMS, the vinyl-terminated PDMS, the catalyst and the organic solvent are uniformly mixed by ultrasonic stirring to obtain a silica gel impregnation solution; the inorganic nanofiber aerogel obtained in step 3 is immersed in the silica gel impregnation solution until saturated, and then placed in a high-temperature reactor for cross-linking reaction; then the inorganic nanofiber aerogel is immersed in a mixed solution of anhydrous ethanol and ethylene glycol, and the mixed solution of anhydrous ethanol and ethylene glycol is replaced multiple times to achieve solvent replacement; Step 5: Drying and curing The impregnated cross-linked aerogel prepared in step 4 is placed in a drying oven for drying and curing to obtain a thermally responsive ceramic fire-resistant explosion-proof pad.
2. A method for preparing a thermally responsive ceramic fireproof explosion-proof pad according to claim 1, It is characterized in that In step 1, the inorganic nanofiber is SiO 2 、TiO 2 、Si 3 N 4 , SiC and other nanofibers; the flux is boron trioxide B 2 O 3 、Zinc borate Zn 3 B 2 O 6 , boric acid H 3 BO 3 、Vanadium pentoxide V 2 O 5 、Silicon dioxide SiO 2 Any one of the following; the mass ratio of flux to inorganic nanofibers is 1:10-1:15, the mass ratio of inorganic nanofibers to deionized water is 1:10-1:20, the ultrasonic time is 15-30min, the ultrasonic power is 200-300W, and the frequency is 140-160Hz.
3. A method for preparing a thermally responsive ceramic fire-resistant explosion-proof pad according to claim 1, It is characterized in that In step 2, the freezing binder is any one of polyvinyl alcohol PVA and polyvinyl pyrrolidone PVP, the mass fraction of the freezing binder is between 7wt.% and 15wt.%, the mass ratio of the freezing binder to the dispersion is 1:20 to 1:30, the water bath temperature is 50 to 80°C, the stirring time is 30 to 60min, the refrigerator compartment temperature is 0 to 10°C, the refrigeration time is 1 to 3h, the freezing temperature of the freeze dryer is -50 to -40°C, and the freezing time is 24 to 48h.
4. A method for preparing a thermally responsive ceramic fireproof explosion-proof pad according to claim 1, It is characterized in that In step 3, the silane coupling agent is any one of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(β-methoxyethoxy) silane, γ-aminopropyl triethoxysilane, γ-(2,3-epoxypropoxy)propyl trimethoxysilane, and γ-methacryloxypropyl trimethoxysilane, the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile, tetrahydrofuran, and dimethylformamide, and the pre-impregnation solution is composed of the following substances by mass percentage: 20% to 30% of silane coupling agent, 40% to 50% of organic solvent, and 20% to 30% of deionized water, the sum of the above components is 100%, the inorganic nanofiber aerogel impregnation time is 12 to 18 hours, the drying temperature is 50 to 70° C., the drying time is 2 to 4 hours, and the number of washing times with anhydrous ethanol is 10 to 20 times.
5. A method for preparing a thermally responsive ceramic fire-resistant explosion-proof pad according to claim 1, It is characterized in that In step 4, the catalyst is any one of tetrabutylammonium difluorotriphenylsilicate and organic cyclic polyphosphazene base, and the organic solvent is any one of ethylene glycol, anhydrous ethanol, n-butanol, acetonitrile, tetrahydrofuran, and dimethylformamide; the silica gel impregnation solution includes 5% to 7% of hydroxyl-terminated PDMS, 4% to 8% of vinyl-terminated PDMS, 20% to 30% of catalyst and 55% to 71% of organic solvent by mass percentage, and the sum of the above components is 100%; at a power of 200 to 300 W and a frequency of Ultrasonication is performed in an ultrasonic machine at 140 to 160 Hz for 20 to 30 minutes, and then the stirring time is 30 to 60 minutes. The immersion time of the inorganic nanofiber aerogel is 12 to 18 hours. The cross-linking temperature is 80 to 90° C. and the cross-linking time is 3 to 4 hours. The inorganic nanofiber aerogel is immersed in a mixed solution of anhydrous ethanol and ethylene glycol for 20 to 30 minutes at a time. The mixed solution of anhydrous ethanol and ethylene glycol is replaced 3 to 5 times. The anhydrous ethanol and ethylene glycol solutions are mixed in a ratio of 1:
1.
6. A method for preparing a thermally responsive ceramic fireproof explosion-proof pad according to claim 1, It is characterized in that The impregnated cross-linked aerogel in step 5 is placed in a drying oven at 60 to 120° C. and dried for 3 to 5 hours.
7. A thermally responsive ceramic fire-resistant explosion-proof pad prepared according to the method for preparing a thermally responsive ceramic fire-resistant explosion-proof pad according to any one of claims 1 to 6.
Citation Information
Patent Citations
High-performance aerogel composite material, preparation method and equipment thereof
CN103435320A
SiO<2> nanofiber aerogel heat insulation material based on electrostatic spinning and preparation and application thereof
CN108840656A
Preparation method of ceramic aerogel material with high strength and low thermal conductivity
CN115849949A
Flexible silicon dioxide aerogel compounded ceramic fiber carrier roller gasket and preparation method thereof
CN116332615A
SiO2 aerogel / TiO2-basalt fireproof heat-insulation composite fabric as well as preparation method and application thereof
CN117626678A
Cited By
Anti-explosion thermal insulation material for battery based on three-dimensional fiber preform as well as preparation method and application of anti-explosion thermal insulation material
CN122576527A
An explosion-proof thermal insulation material for a battery based on a three-dimensional fiber preform, and a preparation method and application thereof
CN122576527B