Intermediate coat layer formation material and surface protection method using intermediate coat layer formation material

The intermediate coating layer forming material enhances load resistance and durability by maintaining tear strength ratios and other properties, addressing the issue of reduced load-bearing capacity after damage in existing coatings.

JP2024140653APending Publication Date: 2024-10-10DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023051908
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing intermediate coating layers for concrete surfaces, as described in Patent Document 1, fail to maintain adequate load-bearing properties after damage.

Method used

An intermediate coating layer forming material is developed, which includes specific composition and curing agent ratios to ensure a tear strength ratio (S80/S30) of 0.60 or more, along with other properties like maximum load and displacement, to maintain load resistance after damage.

Benefits of technology

The material forms a coating film that maintains excellent load resistance even after damage, improving the load-bearing capacity and durability of the intermediate coat layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000015_0000
    Figure 00000015_0000
  • Figure 00000015_0001
    Figure 00000015_0001
Patent Text Reader

Abstract

To provide an intermediate coat layer formation material with which it is possible to form a coating film excellent in maintenance of load resistance after being damaged.SOLUTION: An intermediate coat layer formation material of the invention is used for forming an intermediate coat layer in a surface protection layer including a primer layer, the intermediate coat layer, and a top coat layer formed in this order on a surface of a porous body. The intermediate coat layer formation material includes a main agent and a curing agent, and S80 / S30 that shows a rate of change of tear strength measured according to JIS K7128-1 is 0.60 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an intermediate coat layer-forming material and a surface protection method using the intermediate coat layer-forming material. [Background technology]

[0002] Various developments have been made so far regarding intermediate coating layers used in surface protection members. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a silicone rubber composition for concrete surface coating members having a maximum tear strength of 2.89 to 4.85 N / mm (Claim 1, Table 1 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-147869 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations by the present inventors, it has been found that there is room for improvement in the concrete surface covering member described in the above Patent Document 1 in terms of maintaining load resistance after breakage. [Means for solving the problem]

[0005] As a result of further investigation, the inventors found that by suppressing the change in tear strength over time, it is possible to suppress the decrease in the load resistance of the intermediate coat layer after breakage, and thus completed the present invention.

[0006] According to one aspect of the present invention, there is provided the following intermediate coat layer-forming material and surface protection method using the intermediate coat layer-forming material. 1. A surface protective layer formed on the surface of a porous body, the surface protective layer including a primer layer, an intermediate coat layer, and a top coat layer in this order, comprising an intermediate coat layer-forming material used to form the intermediate coat layer, The composition includes a base agent and a curing agent, The percentage change in tear strength, S, is measured according to the following procedure. 80 / S 30 is 0.60 or more. (Measuring procedure for tear strength) The intermediate layer forming material was applied onto the PET sheet using a rubber spatula at a coating amount of 1.0 [kg / m 2 The coating film formed by applying the above formula is then cured (left to stand) for 7 days at 23±2°C and a relative humidity of 50±20% to form a measurement sheet made of the hardened intermediate coating layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained measurement sheet was measured using a tensile tester under the following measurement conditions in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method", and the tear strength (N / mm) at a displacement of 30 mm was recorded as S 30 , the tear strength (N / mm) when the displacement is 80 mm is S 80 Let us assume that. (Measurement conditions) ·Temperature and humidity in the test room: 23±2℃, 50±15% - Test piece size: 100mm x 30mm -Slit length in the center of the test piece: 50±1mm (slit in the longitudinal direction) Test speed: 100mm / min - Distance between test piece grips (initial value): 30 mm -Measure only vertically 2. The intermediate coating layer forming material according to 1., The tear strength when the displacement is 80 mm is S 80 The intermediate coating layer forming material has a strength of 1 N / mm or more and 40 N / mm or less. 3. The intermediate coating layer forming material according to 1. or 2., An intermediate coating layer forming material having an average tear strength of 1 N / mm or more and 40 N / mm or less in a displacement range of 30 mm or more and 80 mm or less. 4. The intermediate coating layer forming material according to any one of 1. to 3., An intermediate coating layer forming material having a maximum displacement of 20.0 mm or more and a maximum load of 0.8 kN or more, as measured according to the following push-out test. (Push-out test) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate is ground from the back side until it reaches a position 5 mm from the front surface, forming a cylindrical punch indenter with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. The intermediate layer forming material was applied to the surface of the test substrate with a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by applying the above procedure is then cured (left to stand) for 14 days at 23±2°C and a relative humidity of 50±20% to obtain a sample consisting of a hardened intermediate layer-forming material. Next, in accordance with JSCE K 533, a load is applied at 1 mm / min at room temperature of 23°C until the bond between the test substrate and the indenter is broken, and then the indenter is applied toward the sample at 5 mm / min. The load and displacement are measured over time. The load is stopped when the sample breaks or when the peeling of the sample reaches the edge of the test substrate. The maximum load from the fracture of the joint to the end of loading is defined as the maximum load (kN), and the amount of displacement at the maximum load is defined as the maximum displacement (mm). 5. The intermediate coating layer forming material according to any one of 1. to 4., The intermediate coat layer forming material, wherein X×Y is 500 or more and 1850 or less, where X (kN) is the maximum load measured in the push-out test and Y (mm) is the peeled circumference when the displacement is 20 mm. 6. The intermediate coating layer forming material according to any one of 1. to 5., An intermediate coating layer-forming material, in which a plate-shaped sample has a transmittance of 20% or less at 370 nm, a transmittance of 70% or more at 450 nm, and a transmittance of 70% or more at 800 nm, as measured according to the following procedure. (Transmittance measurement procedure) The intermediate layer forming material was applied onto the PET sheet using a rubber spatula at a coating amount of 1.0 [kg / m 2 The coating film formed by applying the above formula is then aged (left stationary) for 14 days at 23±2°C and a relative humidity of 50±20% to form a measurement sheet made of the hardened intermediate layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. For the obtained measurement sheet, a spectrophotometer is used to measure the spectral transmittance in the wavelength range of 300 to 800 nm from the normal (90°) direction to the surface of the measurement sheet in accordance with the visible light transmittance test of JIS A 5759. Using the "weighting coefficients for calculating visible light transmittance" specified in JIS A 5759, a weighted average is calculated by multiplying each wavelength by a weighting coefficient to calculate the transmittance (%). 7. The intermediate coating layer forming material according to any one of 1. to 6., The intermediate layer-forming material, wherein the base resin comprises one or more resins selected from the group consisting of urea resins, urethane resins, epoxy resins, (meth)acrylic resins, polyolefins, polypropylene resins, and polyester resins. 8. The intermediate coating layer forming material according to any one of 1. to 7., The intermediate layer-forming material, wherein the curing agent comprises a compound having -CONH- in the molecule. 9. The intermediate coating layer forming material according to any one of 1. to 8., The intermediate coating layer forming material, wherein the porous body is a concrete structure. 10. A step of forming a primer layer, an intermediate coat layer, and a top coat layer in this order on the surface of the porous body, A surface protection method using an intermediate coat layer-forming material, wherein the intermediate coat layer is formed using the intermediate coat layer-forming material according to any one of 1. to 9. 11. A composition comprising a base agent and a curing agent, The percentage change in tear strength, S, is measured according to the following procedure. 80 / S 30 is 0.60 or more, for the material. (Measuring procedure for tear strength) The material was applied to a PET sheet with a rubber spatula at a rate of 1.0 kg / m 2 The coating film formed by applying the above formula is then cured (left to stand) for 7 days at 23±2°C and a relative humidity of 50±20%, to form a measurement sheet made of the hardened material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained measurement sheet was measured using a tensile tester under the following measurement conditions in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method", and the tear strength (N / mm) at a displacement of 30 mm was recorded as S 30 , the tear strength (N / mm) when the displacement is 80 mm is S 80 Let us assume that. (Measurement conditions) ·Temperature and humidity in the test room: 23±2℃, 50±15% - Test piece size: 100mm x 30mm -Slit length in the center of the test piece: 50±1mm (slit in the longitudinal direction) Test speed: 100mm / min - Distance between test piece grips (initial value): 30 mm -Measure only vertically Effect of the Invention

[0007] According to the present invention, there are provided an intermediate layer forming material capable of forming a coating film excellent in maintaining load resistance even after breakage, and a surface protection method using the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing the results of a push-out test for an example and a comparative example. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a test device used in a push-out test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The intermediate layer forming material of this embodiment will be outlined below.

[0010] The intermediate coat layer forming material of this embodiment is a composition used to form an intermediate coat layer among surface protective layers formed on the surface of a porous body and comprising, in that order, a primer layer, an intermediate coat layer, and a top coat layer. The intermediate layer-forming material contains a base agent and a curing agent, and has a tear strength S which represents the rate of change in tear strength measured according to the following procedure. 80 / S 30 is configured to satisfy 0.60 or more. (Measuring procedure for tear strength) The intermediate layer forming material was applied onto the PET sheet using a rubber spatula at a coating amount of 1.0 [kg / m 2 The coating film formed by applying the above formula is then cured (left to stand) for 7 days at 23±2°C and a relative humidity of 50±20% to form a measurement sheet made of the hardened intermediate coating layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained measurement sheet was measured using a tensile tester under the following measurement conditions in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method", and the tear strength (N / mm) at a displacement of 30 mm was recorded as S 30 , the tear strength (N / mm) when the displacement is 80 mm is S 80 Let us assume that. (Measurement conditions) ·Temperature and humidity in the test room: 23±2℃, 50±15% - Test piece size: 100mm x 30mm -Slit length in the center of the test piece: 50±1mm (slit in the longitudinal direction) Test speed: 100mm / min - Distance between test piece grips (initial value): 30 mm -Measure only in the vertical direction (tear direction).

[0011] Although the detailed mechanism is unclear, it is believed that even after a break or damage occurs in the coating film, the load-bearing capacity of the undercoat layer can be improved by suppressing the growth of the crack from that point.

[0012] S 80 / S 30 The lower limit of is 0.60 or more, preferably 0.75 or more, and more preferably 0.90 or more. This makes it possible to improve the maintenance of the load resistance of the intermediate coating layer after breakage. On the other hand, the above S 80 / S 30 The upper limit of is, for example, 1.80 or less, preferably 1.60 or less, and more preferably 1.50 or less, whereby a balance with other coating film properties can be achieved.

[0013] The tear strength when the displacement is 80 mm is S 80 The lower limit is, for example, 1 N / mm or more, preferably 5 N / mm or more, and more preferably 10 N / mm or more. This makes it possible to further improve the maintenance of the load resistance of the intermediate coat layer after breakage. On the other hand, the tear strength S 80 The upper limit is, for example, 40 N / mm or less, preferably 30 N / mm or less, and more preferably 20 N / mm or less, whereby a balance with other coating film properties can be achieved.

[0014] The lower limit of the average value of the tear strength in the displacement range of 30 mm to 80 mm is, for example, 1 N / mm or more, preferably 5 N / mm or more, and more preferably 10 N / mm or more, which can further improve the maintenance of the load resistance of the intermediate coating layer after breakage. On the other hand, the upper limit of the average value of the tear strength is, for example, 40 N / mm or less, preferably 30 N / mm or less, and more preferably 20 N / mm or less, which can further improve the maintenance of the load resistance of the intermediate coating layer after breakage.

[0015] The maximum displacement and maximum load of the intermediate coating layer-forming material are measured according to the following push-out test. In this case, the lower limit of the maximum displacement is, for example, 20.0 mm or more, preferably 15 mm or more, more preferably 10 mm or more, and the lower limit of the maximum load is, for example, 0.8 kN or more, preferably 1.0 kN or more. This can further improve the maintenance of the load resistance of the intermediate coat layer after breakage. On the other hand, the upper limit of the maximum displacement may be, for example, 100 mm or less, and / or the upper limit of the maximum load may be, for example, 10.0 kN or less.

[0016] (Push-out test) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate is ground from the back side until it reaches a position 5 mm from the front surface, forming a cylindrical punch indenter with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. The intermediate layer forming material was applied to the surface of the test substrate with a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by applying the above procedure is then cured (left to stand) for 14 days at 23±2°C and a relative humidity of 50±20% to obtain a sample consisting of a hardened intermediate layer-forming material. Next, in accordance with JSCE K 533, a load is applied at 1 mm / min at room temperature of 23°C until the bond between the test substrate and the indenter is broken, and then the indenter is applied toward the sample at 5 mm / min. The load and displacement are measured over time. The load is stopped when the sample breaks or when the peeling of the sample reaches the edge of the test substrate. The maximum load from the fracture of the joint to the end of loading is defined as the maximum load (kN), and the amount of displacement at the maximum load is defined as the maximum displacement (mm).

[0017] The maximum load measured in the above-mentioned push-out test using the intermediate coating layer-forming material is designated as X (kN), and the peeled perimeter when the displacement is 20 mm is designated as Y (mm). In this case, the lower limit of X×Y is, for example, not less than 500, preferably not less than 750, and more preferably not less than 1000. This can further improve the maintenance of the load resistance of the intermediate coat layer after breakage. On the other hand, the upper limit of the above X×Y is, for example, not more than 1850, preferably not more than 1800, and more preferably not more than 1750. This can further improve the maintenance of the load resistance of the intermediate coat layer after breakage.

[0018] According to the following procedure, the transmittance (%) in the wavelength range of 300 nm to 800 nm is measured for a plate-shaped sample using an intermediate coating layer-forming material. In this case, the lower limit of the transmittance at 370 nm is, for example, 20% or less, the lower limit of the transmittance at 450 nm is, for example, 70% or more, and the lower limit of the transmittance at 800 nm is, for example, 70% or more. This can further improve the maintenance of the load resistance of the intermediate coating layer after breakage. Furthermore, the upper limit of the transmittance at 370 nm may be, for example, 40% or more, the upper limit of the transmittance at 450 nm may be, for example, 99% or less, and / or the upper limit of the transmittance at 800 nm may be, for example, 99% or less.

[0019] (Transmittance measurement procedure) The intermediate layer forming material was applied onto the PET sheet using a rubber spatula at a coating amount of 1.0 [kg / m 2 The coating film formed by applying the above formula is then aged (left stationary) for 14 days at 23±2°C and a relative humidity of 50±20% to form a measurement sheet made of the hardened intermediate layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. For the obtained measurement sheet, a spectrophotometer is used to measure the spectral transmittance in the wavelength range of 300 to 800 nm from the normal (90°) direction to the surface of the measurement sheet in accordance with the visible light transmittance test of JIS A 5759. Using the "weighting coefficients for calculating visible light transmittance" specified in JIS A 5759, a weighted average is calculated by multiplying each wavelength by a weighting coefficient to calculate the transmittance (%).

[0020] In this embodiment, for example, by appropriately selecting the type and amount of each component contained in the intermediate coating layer forming material, the preparation method of the intermediate coating layer forming material, etc., the S 80 / S 30 It is possible to control the average tear strength, the maximum load and maximum displacement in the push-out test, the maximum load x peel circumference, and the transmittance at each wavelength. Among these, for example, adjusting the content of the base agent having three or more functionalities, including polyamide amine in the curing agent, etc., can be used to control the S 80 / S 30 These include factors for setting the average value of tear strength, the maximum load and maximum displacement in a push-out test, the maximum load x peel circumference, and the transmittance at each wavelength within the desired numerical range.

[0021] The porous body is preferably a concrete structure, but is not limited thereto. The porous body may be a member having independent pores and / or continuous pores formed on the surface. At least the surface of such a member may be made of an inorganic material. Furthermore, examples of concrete structures include, but are not limited to, parts of viaduct structures and the like, and include those used outdoors.

[0022] Each component of the intermediate layer-forming material of this embodiment will be described in detail below.

[0023] The intermediate layer forming material is a composition containing a base agent and a curing agent.

[0024] The base resin may contain one or more resins selected from the group consisting of urea resin, urethane resin, epoxy resin, (meth)acrylic resin, polyolefin, polypropylene resin, and polyester resin. Among these, from the viewpoint of curability in a room temperature environment and / or adhesion to concrete, urea resin, urethane resin, or epoxy resin is preferred, and epoxy resin is more preferred. An example of the base resin may contain, for example, 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more of an epoxy resin in 100% by mass of the base resin. In this specification, the term "(meth)acrylic" means at least one of acrylic and methacrylic.

[0025] As the epoxy resin, an epoxy compound having two or more epoxy groups in the molecule is used. The epoxy compound may be any of a monomer, an oligomer, and a polymer. From the viewpoint of flexibility of the intermediate coat layer, it is preferable to use a bifunctional epoxy compound having two epoxy groups in the molecule, and from the viewpoint of mechanical strength of the intermediate coat layer, a polyfunctional epoxy compound having three or more epoxy groups in the molecule may be used. In addition, taking into consideration the balance of various properties, an example of an epoxy resin may contain only a difunctional epoxy compound, or, when it contains both a difunctional epoxy compound and a polyfunctional epoxy compound, the polyfunctional epoxy compound may be contained in an amount of, for example, 40 mass% or less, preferably 30 mass% or less, and more preferably 25 mass% or less, based on 100 mass% of the epoxy resin.

[0026] Specific examples of epoxy compounds include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol A bis(polypropylene glycol glycidyl ether) ethers, bisphenol A bis(polyethylene glycol glycidyl ether) ethers, hydrogenated bisphenol A type epoxy resins, hydrogenated bisphenol F type epoxy resins, biphenyl type epoxy resins, aliphatic epoxy resins, urethane modified epoxy resins, rubber modified epoxy resins, alkyl glycidyl ethers, cresyl glycidyl ethers, phenyl glycidyl ethers, alkyl diglycidyl ethers, polyethylene glycol diglycidyl ethers, polypropylene glycol diglycidyl ethers, glycerin triglycidyl ethers, trimethylolpropane triglycidyl ethers, etc. These may be used alone or in combination of two or more.

[0027] The urethane resin may be any polymer having a urethane bond structure formed by the reaction of an isocyanate group with a hydroxyl group. The method of reacting the polyol compound and the polyisocyanate compound, which are raw materials for the urethane resin, is not particularly limited, and any known method can be used. For example, a urethane polymer having two or more isocyanate groups at the molecular chain terminals can be obtained by mixing the polyol compound and the polyisocyanate compound in a solvent or without a solvent. As the polyisocyanate compound, a dimer or trimer of an isocyanate compound, or a reaction product or polymer of an isocyanate compound (for example, a dimer or trimer of diphenylmethane diisocyanate, a reaction product of trimethylolpropane and tolylene diisocyanate, etc.) can also be used. The polyol compound is not particularly limited and any known and commonly used polyol compound can be used. Among these, polyol compounds not having a polypropylene glycol skeleton are particularly preferred.

[0028] The urea resin may be a polymer having a urea bond structure formed by the reaction of an isocyanate group with an amino group, or an isocyanate group with a ketimine group. The compound having an amino group is not particularly limited, but may be a primary amine or a secondary amine such as an aliphatic amine or an aromatic amine. The compound having two or more ketimine groups (ketimine compound) is not particularly limited as long as it is obtained by dehydration condensation of an amine compound having two or more primary amino groups in the molecule and a ketone compound.

[0029] The curing agent is not limited as long as it contains a component that cures the base agent. When the base resin includes an epoxy resin, the curing agent may include, for example, an amine-based curing agent.

[0030] As the amine compound, an amine compound having a primary amino group, a secondary amino group, and / or a tertiary amino group is used. Specific examples of the amine compound include aliphatic amines, alicyclic amines, modified aliphatic polyamines, modified alicyclic amines, polyamidoamines, etc. Polyamidoamine refers to an amine compound having an amide bond and an amino group in the molecule. These may be used alone or in combination of two or more. Among these, the amine-based curing agent may contain an amine compound having -CONH- in the molecule, and preferably a polyamidoamine having -CONH- in the molecule, from the viewpoint of the viscosity of the coating film under load. From the viewpoint of accelerating the curing reaction, the amine-based curing agent may contain an amine compound having a tertiary amino group.

[0031] The base agent and the curing agent may be mixed so that the ratio of the active hydrogen equivalent of the amine compound (a component that cures the epoxy compound) to the epoxy equivalent of the epoxy compound is, for example, 0.5 to 1.5, or preferably 0.8 to 1.2. The active hydrogen equivalent of an amine compound indicates the mass (g) of the amine compound per mole of active hydrogen. When two or more types are used in combination, the active hydrogen equivalent of the amine compound is calculated from the total mass of the amine compounds and the total active hydrogen.

[0032] The intermediate layer forming material may contain additives in addition to the above-mentioned base agent and curing agent. Examples of additives include fillers, curing accelerators, light stabilizers, light absorbers, antioxidants, deterioration inhibitors, pigments, dyes, silane coupling agents, defoamers, leveling agents, dispersants, rheology control agents, waxes, solvents, water, etc. These may be used alone or in combination of two or more. Among these, fillers and rheology control agents may be used.

[0033] The filler includes an organic filler and an inorganic filler. Examples of the organic filler include resin particles such as (meth)acrylic acid ester particles and polystyrene particles. Examples of inorganic fillers include fumed silica, calcium carbonate, talc, clay, metal oxides, metal hydroxides, and silica. Among these, from the viewpoint of transparency, one or more of the group consisting of silica and fumed silica is preferred, and fumed silica is more preferred. Among fumed silica, hydrophobic fumed silica is more preferred.

[0034] The intermediate layer forming material can be obtained, for example, by mixing the above-mentioned base agent and hardener. During mixing, additives may be added if necessary.

[0035] The surface protection method of this embodiment will be described. An example of a surface protection method includes the steps of forming a primer layer, an intermediate coat layer, and a top coat layer in this order on the surface of a porous body. A specific surface protection method may include, for example, a step of applying a primer composition onto the surface of a porous body such as a concrete structure to form a primer layer, a step of applying an intermediate coat layer forming material onto the primer layer to form an intermediate coat layer, and a step of applying a top coat layer paint onto the intermediate coat layer to form a top coat layer.

[0036] In the step of forming a primer layer, a primer composition generally used for surface treatment can be used to form a primer layer on the surface of the concrete structure.

[0037] Examples of the primer composition include epoxy primers, urethane primers, (meth)acrylic primers, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of excellent adhesion to the surface of the structure, one or more of the group consisting of epoxy primers and (meth)acrylic primers are preferred, and epoxy primers are more preferred. The primer composition may contain one or more of the same components as the main component contained in the intermediate layer-forming material.

[0038] In the step of forming the intermediate coat layer, the intermediate coat layer can be formed on the primer layer using the intermediate coat layer forming material described above. At this time, the intermediate coat layer forming material may be subjected to at least one of the following curing treatments: mixing of a curing agent, heat curing, solvent evaporation, moisture curing, anaerobic curing, or ultraviolet curing. These may be used alone or in combination of two or more. In this way, the intermediate coat layer can be formed. As a specific example of the hardening treatment, the intermediate layer forming material may be cured under predetermined temperature and humidity conditions for a predetermined period of time.

[0039] In the step of forming the topcoat layer, a topcoat layer paint such as a general protective paint or topcoat paint can be used to form the topcoat layer on the intermediate coat layer.

[0040] The topcoat layer is not particularly limited, and may contain, for example, one or more selected from the group consisting of fluororesin, (meth)acrylic resin, (meth)acrylic silicone resin, (meth)acrylic urethane resin, urethane resin, olefin resin, vinyl acetate resin, ethylene-vinyl acetate copolymer resin, silicone resin, and modified resins thereof.

[0041] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0042] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0043] <Adjustment of materials for forming intermediate layer> The base agent and the curing agent were mixed according to the raw materials and composition ratios shown in Table 1 to obtain an intermediate layer forming material.

[0044] The information on the raw materials in Table 1 is shown below. (Main ingredient) Base resin 1: Bisphenol A type epoxy resin (bifunctional, ADEKA Resin EP4100, manufactured by ADEKA Corporation, epoxy equivalent: 190g / ep, viscosity at 25°C: 13,000mPa s) Base resin 2: Bisphenol A type epoxy resin (bifunctional, ADEKA Resin EP4000, manufactured by ADEKA Corporation, epoxy equivalent: 320g / ep, viscosity at 25°C: 4,500mPa s) Base resin 3: Aliphatic epoxy resin (bifunctional, diluent, ADEKA Glysilol ED503, manufactured by ADEKA, epoxy equivalent: 165g / ep, viscosity at 25°C: 25mPa s) Base 4: Aliphatic epoxy resin (trifunctional, diluent, ADEKA Glysilol ED505, manufactured by ADEKA, epoxy equivalent: 150g / ep, viscosity at 25°C: 150mPa·s) (hardening agent) Curing agent 1: Polyamidoamine (polyamidoamine represented by the following chemical formula, active hydrogen equivalent: 200g / ep, viscosity at 25°C: 10,000-14,000mPa·s, mixture of amine compounds having primary amino groups and amine compounds having secondary amino groups)

[0045] [ka]

[0046] Hardener 2: Triethanolamine (trifunctional amine compound, manufactured by Showa Chemical Co., Ltd., viscosity at 25°C: 600 mPa s)

[0047] [Table 1]

[0048] The obtained intermediate layer-forming material was evaluated for the following items.

[0049] (Measurement of tear strength) The intermediate layer forming material obtained above was applied onto a PET sheet using a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula was left to stand at 23±2°C and a relative humidity of 50±20% for 7 days to form a measurement sheet made of a hardened intermediate layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained test sheet was measured in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method" using a tensile tester (RTG-1310, manufactured by A&D Co., Ltd.) under the following measurement conditions. However, the grip of the tensile tester pulls the long leg of the slit of the test piece vertically, and the tear strength is measured only in this vertical direction. The tear strength was measured five times using a different evaluation sheet. The tear strength at a displacement of 30 mm (S 30), tear strength at a displacement of 80 mm (S 80 ) The average of three points out of five measured values, excluding the maximum and minimum values, is shown in Table 1. The displacement means the distance (mm) that the gripping tools of the test piece move away from each other in the vertical direction from the initial value (30 mm). In the test pieces of Examples 1 to 5, the displacement was maintained at 100 mm or more even though the unslit length in the longitudinal direction of the test piece was 50 mm. This is presumably because the test piece was stretched without being torn when a tensile stress in the vertical direction was applied. In addition, in Examples 1 to 5, the average tear strength was calculated by averaging the measured values ​​of 1,500 points with a displacement between 30 mm and 80 mm. On the other hand, when measuring the tear strength of Comparative Example 1, a long cut was made in the horizontal direction (short direction of the test piece) perpendicular to the vertical direction, and the tear strength could not be measured with a displacement of 40 mm or more. 80 , S 80 / S 30 The average tear strength is indicated as "-". 80 S of Comparative Example 1, where it was not possible to measure 80 / S 30 means zero. (Measurement conditions) ·Temperature and humidity in the test room: 23±2℃, 50±15% - Test piece size: 100mm x 30mm -Slit length in the center of the test piece: 50±1mm (slit in the longitudinal direction) Test speed: 100mm / min - Distance between test piece grips (initial value): 30 mm

[0050] (Push-out test) A push-out test was carried out using a test device shown in FIG. 2 in accordance with JSCE K 533, and the displacement (mm) and load (kN) were measured for the sample 20 formed on the surface of the test substrate 10. FIG. 2(a) is a cross-sectional view of the test device, and FIG. 2(b) is a perspective view of the test device. The specific procedure for the push-through test was as follows. In accordance with the preparation of test specimens in JSCE K 533, concrete with a water / cement ratio of 44% and a sand / cement ratio of 2.7 was placed in a metal formwork with internal dimensions of 400 mm length x 600 mm width x 60 mm thickness, and cured for 24 hours at a temperature of 20±2°C and a relative humidity of 80% or more, after which it was demolded and cured in water for 6 days at a temperature of 20±2°C. After the underwater curing was completed, it was cured for 7 days or more at a temperature of 23±2°C and a relative humidity of 50±5%, to produce a concrete plate (porous body) in the shape of a top cover for a top cover type U-shaped gutter (not shown) as specified in JIS A 5372 Appendix E (Type 1, 300). Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, forming a cylindrical punch indenter 30 with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate 10. Next, the surface (the application surface) of the test substrate 10 was scraped using a disk sander, and then degreased. The intermediate layer forming material obtained above was applied to the surface of the test substrate 10 with a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula was then aged (left to stand) for 14 days at 23±2° C. and a relative humidity of 50±20%, to obtain Sample 20 consisting of a hardened intermediate layer-forming material. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate 10 and the punch indenter 30 was broken at room temperature of 23° C., and then the punch indenter 30 was applied toward the sample 20 at 5 mm / min. At this time, the load and the amount of displacement were measured over time. The load was terminated when the sample 20 broke or when the peeling of the sample 20 reached the end face of the test substrate 10. The maximum load from the fracture of the joint to the end of loading was defined as the maximum load (kN), and the amount of displacement at the maximum load was defined as the maximum displacement (mm). The load and displacement were recorded every 0.05 kN, and the load was temporarily interrupted every 10 mm of displacement, and the peeled area was marked on the sample 20 and the load was recorded. The peeled circumference of sample 20 was measured when the displacement was 20 mm. The results of the push-out tests on Sample 20 of Examples 1 to 5 and Comparative Example 1 are shown in a graph in FIG. 1, with the vertical axis representing load (kN) and the horizontal axis representing displacement (mm).

[0051] (Transmittance measurement) The intermediate layer forming material obtained above was applied onto a PET sheet using a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula was left to stand at 23±2°C and a relative humidity of 50±20% for 14 days to form a measurement sheet made of a hardened intermediate layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The obtained measurement sheet was measured for spectral transmittance in the wavelength range of 300 to 800 nm from the normal (90°) direction to the surface of the measurement sheet in accordance with the visible light transmittance test of JIS A 5759 using a UV-VIS-NIR spectrophotometer SolidSpec-3700 manufactured by Shimadzu Corporation, and the transmittance (%) was calculated by multiplying each wavelength by a weighting coefficient and taking a weighted average using the "weighting coefficient for calculating visible light transmittance" specified in JIS A 5759. The calculated transmittances are shown in Table 1.

[0052] (Evaluation of load-bearing capacity after breakage) In Figure 1, which shows the results of the above-mentioned push-out test, the displacement at which a hole of φ1 mm or more was formed in the coating film (sample 20) (displacement at breakage) is indicated by a circle. After such breakage occurred in the coating film, the load was continued to be applied, and the displacement (breakage displacement) at which the coating film broke (load became zero) was measured. During the push-out test, if a hole of φ1 mm or more appeared in the coating film and the load reduction continued to be 50% or more of the maximum load even after the displacement continued, the test was judged as good, and if not, the test was judged as poor.

[0053] The intermediate coat layer-forming materials of Examples 1 to 5 showed results that, compared to Comparative Example 1, the decrease in the load resistance of the coating film after breakage was suppressed.

[0054] 10 Test Board 20 Samples 30 Push-out indenter

Claims

1. A surface protective layer formed on the surface of a porous body, the surface protective layer including a primer layer, an intermediate coat layer, and a top coat layer in this order, the intermediate coat layer being formed from an intermediate coat layer-forming material ... The composition includes a base agent and a curing agent, S, which represents the rate of change in tear strength, measured according to the following procedure 80 / S 30 is 0.60 or more. (Procedure for measuring tear strength) The intermediate layer forming material was applied onto a PET sheet using a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula] is aged (left stationary) for 7 days at 23±2° C. and a relative humidity of 50±20% to form a measurement sheet made of a cured product of the intermediate coating layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained measurement sheet was measured using a tensile tester under the following measurement conditions in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method", and the tear strength (N / mm) at a displacement of 30 mm was recorded as S 30 , the tear strength (N / mm) when the displacement is 80 mm is S 80 Let us assume that. (Measurement conditions) Test room temperature and humidity: 23±2°C, 50±15% ・Test piece dimensions: 100mm x 30mm Slit length in the center of the test piece: 50 ± 1 mm (slit in the longitudinal direction) Test speed: 100 mm / min Distance between test piece grips (initial value): 30 mm ・Measure only in the vertical direction

2. The intermediate coating layer forming material according to claim 1, The tear strength when the displacement is 80 mm is S 80 The intermediate coating layer forming material has a surface tension strength of 1 N / mm or more and 40 N / mm or less.

3. The intermediate coating layer forming material according to claim 1 or 2, An intermediate coating layer-forming material having an average tear strength of 1 N / mm or more and 40 N / mm or less in a displacement range of 30 mm or more and 80 mm or less.

4. The intermediate coating layer forming material according to claim 1 or 2, An intermediate coating layer-forming material having a maximum displacement of 20.0 mm or more and a maximum load of 0.8 kN or more, as measured according to the following push-out test. (Push-out test) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate is ground from the back side until it reaches a position 5 mm from the front surface, to form a cylindrical punch indenter with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. The intermediate layer forming material was applied to the surface of the test substrate with a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula] is then aged (left stationary) for 14 days at 23±2° C. and a relative humidity of 50±20% to obtain a sample made of a hardened product of the intermediate coating layer-forming material. Next, in accordance with JSCE K 533, a load is applied at 1 mm / min at room temperature of 23° C. until the bond between the test substrate and the punch indenter breaks, and then the punch indenter is applied toward the sample at 5 mm / min. At this time, the load and the amount of displacement are measured over time. The load is terminated when the sample breaks or when the peeling of the sample reaches the edge of the test substrate. The maximum value of the load from the destruction of the joint to the end of loading is defined as the maximum load (kN), and the amount of displacement at the maximum load is defined as the maximum displacement (mm).

5. The intermediate coating layer forming material according to claim 4, The intermediate coat layer forming material, wherein X×Y is 500 or more and 1850 or less, where X is the maximum load measured in the push-out test (kN) and Y is the peeled circumference when the displacement is 20 mm (mm).

6. The intermediate coating layer forming material according to claim 1 or 2, An intermediate layer-forming material, which has a transmittance of 20% or less at 370 nm, a transmittance of 70% or more at 450 nm, and a transmittance of 70% or more at 800 nm, when measured according to the following procedure, of a plate-shaped sample. (Transmittance measurement procedure) The intermediate layer forming material was applied onto a PET sheet using a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by coating with the above formula] is aged (left stationary) for 14 days at 23±2° C. and a relative humidity of 50±20% to form a measurement sheet made of a cured product of the intermediate coating layer-forming material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. For the obtained measurement sheet, the spectral transmittance in the wavelength range of 300 to 800 nm is measured from the normal (90°) direction to the surface of the measurement sheet in accordance with the visible light transmittance test of JIS A 5759 using a spectrophotometer, and the transmittance (%) is calculated by multiplying each wavelength by a weighting coefficient and taking a weighted average using the "weighting coefficient for calculating visible light transmittance" specified in JIS A 5759.

7. The intermediate coating layer forming material according to claim 1 or 2, The intermediate layer-forming material, wherein the base resin contains one or more resins selected from the group consisting of urea resins, urethane resins, epoxy resins, (meth)acrylic resins, polyolefins, polypropylene resins, and polyester resins.

8. The intermediate coating layer forming material according to claim 1 or 2, The intermediate layer-forming material, wherein the curing agent contains a compound having --CONH-- in the molecule.

9. The intermediate coating layer forming material according to claim 1 or 2, The intermediate coating layer forming material, wherein the porous body is a concrete structure.

10. The method includes forming a primer layer, an intermediate coat layer, and a top coat layer in this order on a surface of a porous body; A surface protection method using an intermediate coat layer-forming material, wherein the intermediate coat layer is formed using the intermediate coat layer-forming material according to claim 1 or 2.

11. The composition includes a base agent and a curing agent, S, which represents the rate of change in tear strength, measured according to the following procedure 80 / S 30 is 0.60 or greater. (Procedure for measuring tear strength) The material was applied onto a PET sheet using a rubber spatula in an amount of 1.0 [kg / m 2 The coating film formed by applying the above formula 1 is then aged (left stationary) for 7 days at 23±2° C. and a relative humidity of 50±20% to form a measurement sheet made of a hardened material. Thereafter, the PET sheet was peeled off to obtain a measurement sheet having a thickness of 1 mm. The tear strength (N / mm) of the obtained measurement sheet was measured using a tensile tester under the following measurement conditions in accordance with JIS K 7128-1 "Plastics - Test method for tear strength of films and sheets - Part 1: Trouser tear method", and the tear strength (N / mm) at a displacement of 30 mm was recorded as S 30 , the tear strength (N / mm) when the displacement is 80 mm is S 80 Let us assume that. (Measurement conditions) Test room temperature and humidity: 23±2°C, 50±15% ・Test piece dimensions: 100mm x 30mm Slit length in the center of the test piece: 50 ± 1 mm (slit in the longitudinal direction) Test speed: 100 mm / min Distance between test piece grips (initial value): 30 mm ・Measure only in the vertical direction

Citation Information

Patent Citations

  • Construction method for preventing concrete from falling

    JP2017119998A

  • Concrete exfoliation material and concrete exfoliation method

    JP2021130940A

  • Structure with coating layer, manufacturing method thereof and a set of resin composition for coating

    JP2022061323A

  • Multi-layer coating system having a top layer comprising a two-component reaction resin

    US20110217516A1

  • Silicone rubber composition for concrete surface-coated member, concrete surface-coated member using the same, and method of coating concrete surface

    JP2019147869A