METHOD OF MANUFACTURING SiC EXTENDED INGOT
By joining mirror-polished SiC ingots and aligning notches for uniformity, the method addresses the challenge of producing long SiC ingots with superior workability and quality, enhancing the manufacturing process beyond conventional growth-based methods.
Patent Information
- Application Number
- JP2023052511
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Conventional methods for manufacturing SiC single crystal ingots face limitations in achieving long ingots and maintaining crystal quality due to issues with temperature uniformity and adhesive bonding, which can affect the subsequent processing and quality of SiC ingots.
The method involves joining ground SiC ingots in the axial direction by polishing their end surfaces to a mirror finish and bonding them together, forming a crystal bond to extend the ingot without relying on crystal growth, and optionally aligning notches on the side surfaces for uniform diameter matching.
This approach allows for the production of long SiC ingots with excellent workability and maintained crystal quality, enabling precise cutting and uniform outer diameters, thus overcoming the limitations of traditional growth-based methods.
Smart Images

Figure 2024141069000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an extended SiC ingot, which is formed by joining and extending a single SiC ingot that has been ground into a cylindrical shape in the axial direction, and to a method for manufacturing the extended SiC ingot. [Background technology]
[0002] Conventionally, as disclosed in Patent Document 1 below, a method for producing a SiC single crystal ingot is known which involves a sublimation method in which a high thermal conductivity raw material layer comprising a high thermal conductivity raw material is disposed in the lower part of a crucible, and a low thermal conductivity raw material layer comprising a low thermal conductivity raw material is disposed on at least one of the upper and lower sides of the high thermal conductivity raw material layer to form a raw material section, and heating is performed so that the maximum temperature of the raw material section is reached in the high thermal conductivity raw material layer, thereby growing a SiC single crystal ingot. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-083704 A Summary of the Invention [Problem to be solved by the invention]
[0004] According to such a conventional method for producing a SiC single crystal ingot, it is possible to improve the temperature uniformity of the raw materials placed in the crucible, make effective use of the raw materials, and improve the growth potential of the crystal.
[0005] However, even if some improvement in growth is achieved in the case of SiC crystals, which contributes to the increase in length, there are limitations to growth and length, and it is difficult to obtain long ingots like those of silicon.
[0006] On the other hand, as in the production of SOI wafers, it is possible to simply bond the mirror surfaces of silicon wafers together with an adhesive or to bond them by applying heat treatment without using an adhesive (because the adhesion is not perfect). However, there is a risk that the use of adhesives or heat treatment will affect the subsequent processing steps of the SiC ingot or lead to a deterioration in the quality of the crystal itself.
[0007] In view of the above circumstances, the present invention aims to provide an extended ingot and a method for manufacturing a SiC extended ingot that can obtain a long ingot without relying on crystal growth properties and achieve excellent workability while maintaining crystal quality. [Means for solving the problem]
[0008] The SiC extension ingot of the first invention is an SiC extension ingot obtained by joining a single SiC ingot ground into a cylindrical shape in the axial direction and extending it, The single SiC ingot has an end surface ground to a mirror finish, The SiC ingot is characterized in that it is extended by joining end faces of the SiC ingot which have been ground to a mirror finish.
[0009] According to the first invention of the extended SiC ingot, the end faces of a single SiC ingot are joined together to be extended, so that an ingot of the desired length can be obtained by repeating the joining process without relying on the growth properties of the crystal itself.
[0010] In addition, the bonding is a crystalline bond formed by bonding mirror-finished end faces together, which makes it possible to realize a strong bond while still maintaining the shape when cutting wafers from the elongated SiC ingot, resulting in an ingot with excellent workability.
[0011] In this way, according to the SiC extended ingot of the first invention, a long ingot can be obtained without depending on the crystal growth property, and further, excellent workability can be achieved while maintaining the crystal quality.
[0012] The SiC elongated ingot of the second invention is the same as that of the first invention, The single SiC ingot has a notch cut into its side surface, The SiC ingots are extended by joining end faces that have been ground to a mirror finish with the notches aligned.
[0013] According to the SiC extended ingot of the second invention, it is desirable for the extended ingot that is joined and extended to have a uniform outer diameter shape from the standpoint of processability. However, by providing one or more notches on the side of a single SiC ingot and aligning the notches, the outer diameter shapes of the single SiC ingots can be aligned when joining them together, and thus a SiC extended ingot with a uniform outer diameter shape can be obtained.
[0014] In this way, according to the SiC extended ingot of the second invention, a long ingot can be obtained without relying on the growth of the crystal, and further, excellent and higher workability can be achieved while maintaining the quality of the crystal.
[0015] According to the third aspect of the present invention, a method for producing an extended SiC ingot is provided, in which a single SiC ingot ground into a cylindrical shape is joined in the axial direction to extend the ingot, a grinding process step of grinding an end surface of the single SiC ingot into a mirror surface; a bonding process for bonding end surfaces of the SiC ingot that has been ground to a mirror finish by the grinding process; The method is characterized in that the single SiC ingot is elongated in the axial direction by the bonding process.
[0016] According to the manufacturing method of the third invention for producing an extended SiC ingot, the end faces of a single SiC ingot are joined together to be extended, so that the desired long ingot can be obtained by repeating the joining process without relying on the growth properties of the crystal itself.
[0017] In addition, the bonding is a crystalline bond formed by bonding mirror-finished end faces together, which makes it possible to realize a strong bond while still maintaining the shape when cutting wafers from the elongated SiC ingot, resulting in an ingot with excellent workability.
[0018] Thus, according to the manufacturing method of the SiC extended ingot of the third invention, a long ingot can be obtained without relying on the growth properties of the crystal, and further, excellent workability can be achieved while maintaining the quality of the crystal. [Brief description of the drawings]
[0019] [Figure 1] 1 is a flowchart showing the entire manufacturing process of a SiC wafer (semiconductor crystal wafer) according to the present embodiment. [Diagram 2] 2 is an explanatory diagram showing the contents of a first-side processing step and a second-side processing step in the manufacturing process of the SiC wafer of FIG. 1. [Diagram 3] 2 is an explanatory diagram showing the contents of a first-side processing step and a second-side processing step in the method for producing the SiC wafer of FIG. 1. [Figure 4] 2A to 2C are schematic diagrams showing a processed state in a first-side processing step and a second-side processing step in the manufacturing method of the SiC wafer in FIG. 1. [Figure 5A] 2A to 2C are schematic diagrams showing a processed state in a first-side processing step and a second-side processing step in the manufacturing method of the SiC wafer in FIG. 1. [Figure 5B] 1A to 1C are schematic diagrams showing the processed states in a first-side processing step and a second-side processing step in a conventional SiC wafer manufacturing method. [Figure 6]2 is an explanatory diagram showing a state in which wafers obtained by the first-side processing step and the second-side processing step in the SiC wafer manufacturing method of FIG. 1 are crystal-bonded to each other. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] As shown in FIG. 1, in this embodiment, the manufacturing method for a SiC wafer, which is a semiconductor crystal wafer, is a method for obtaining a SiC wafer by removing waviness from one surface of a wafer sliced from a SiC ingot ground into a cylindrical shape, and includes a groove processing step (STEP 100 / FIG. 1), a cutting step (STEP 110 / FIG. 1), a first surface processing step (STEP 120 / FIG. 1), and a second surface processing step (STEP 130 / FIG. 1).
[0021] The processing in the first surface machining step in STEP 120 and the second surface machining step in STEP 130, i.e., mechanical polishing (high-precision grinding), corresponds to the grinding process and grinding step characteristic of the present invention. Meanwhile, the groove machining step in STEP 100 and the cutting step in STEP 110 are described in the applicant's Patent Nos. 7104909 and 7100864, etc., and therefore detailed description here will be omitted and only an outline will be provided below.
[0022] First, in the groove processing step of STEP 100, a cylindrical SiC ingot is prepared by performing cylindrical grinding on a pre-crystallized SiC crystal with the crystal orientation determined in the ingot processing step.
[0023] Then, in the groove processing step of STEP 100, a plurality of grooves are formed around the entire side surface of the SiC ingot.
[0024] Specifically, in the groove machining process of STEP 100, groove machining drum grinding wheels, each having a convex portion corresponding to the groove formed on its side, are rotated on mutually parallel rotation axes while being pressed against a SiC ingot to form a groove.
[0025] It is preferable to perform a damage-free mirror finish on the SiC ingot (especially the grooves) obtained in the groove processing step by a chemical processing method.
[0026] Next, in the cutting step of STEP 110, the SiC ingot is cut into slices by a plurality of wires arranged in the plurality of grooves formed in the groove processing step, thereby obtaining SiC wafers 100.
[0027] Specifically, in the cutting process, the wire saw device, which is a cutting processing device, has a wire saw section that aligns multiple wires with the multiple grooves formed in the groove processing process, and cuts the SiC ingot into slices by moving the wires forward while rotating them.
[0028] Next, as shown in FIG. 2, in the first surface processing step of STEP 120, one surface 110 of the cut surfaces is used as a support surface, and the remaining other surface 120 is subjected to mechanical polishing (high-precision grinding).
[0029] Specifically, in the first surface processing step, grinding is performed by a mechanical polishing device 50 (ultra-high synthesis, high-precision grinding device) that performs mechanical polishing.
[0030] 3, the mechanical polishing device 50 includes a spindle 51 and a platen 52, which is a grinding table, and diamond polishing grains 53 are provided on the platen 52. The platen 52 has an uneven structure with radial grooves on the polishing surface, and the flat area of the protruding parts is larger than that of the recessed grooves, and is configured to contribute to the temperature rise caused by friction, which will be described later.
[0031] First, one surface 110 is set as the upper surface and adsorbed and supported by a vacuum porous chuck 54, which is an adsorption plate of a spindle 51, which is a wafer support stand, and the other surface 120 is set as the lower surface and is ground by diamond polishing grains 53.
[0032] At this time, the spindle 51 and the platen 52 are rotated by a drive device (not shown), and the spindle 51 is pressed against the platen 52 by a compressor (not shown) or the like, thereby subjecting the remaining other surface 120 to grinding.
[0033] After the grinding process, the diamond polishing grains 53 may be dressed using a dresser or the like.
[0034] Furthermore, the mechanical polishing apparatus 50 may have functional water supply pipes so that a plurality of types of functional water can be used during processing, if necessary.
[0035] Next, in the second surface processing step of STEP 130, the other surface 120 that has been subjected to the high-precision grinding process in the first surface processing step is used as the upper surface, and the one surface 110 is subjected to the same high-precision grinding process as in the first surface processing step.
[0036] That is, the other surface 120 is attached to the vacuum porous chuck 54 which is an attachment plate of the spindle 51 with the other surface 120 serving as the upper surface, and the one surface 110 is ground with the diamond grindstone 53 with the one surface 110 serving as the lower surface.
[0037] In this case as well, dressing may be performed by pressing a dresser or the like against the diamond grindstone 53, if necessary.
[0038] In the mechanical polishing (high-precision grinding) process in the first surface machining step in STEP 120 and the second surface machining step in STEP 130, as shown in FIG. 4, in this embodiment, (1) The particle size of the diamond abrasive grains (diamond grinding wheels) 53 used for grinding, (2) a pressing force that presses the wafer 100 against the platen 52 via the spindle 51; (3) the speed at which the spindle 51 advances relative to the platen 52; Then, a plastic deformation region 100A is formed on the surface of the wafer 100 facing the platen 52 (grinding table) due to a temperature rise (for example, 700° C. or higher but lower than the melting point) caused by friction between the platen 52 and the diamond abrasive grains 53.
[0039] That is, by controlling (1) the particle size of diamond polishing grains 53 used for grinding (e.g., #1000 to #5000 for SiC wafers, more preferably #1500 to #4000), (2) the pressing force with which wafer 100 is pressed against platen 52 via spindle 51 (several hundred g / cm2, which is larger than the normal load of less than 100 g / cm2, e.g., 200 g / cm2 to 800 g / cm2 for SiC wafers), and (3) the advancing speed of spindle 51 relative to platen 52 (a few tenths of a micrometer to several tens of micrometers / min for SiC wafers), a plastic deformation region 100A is actively formed on the surface of wafer 100 facing platen 52.
[0040] In the figure, an intermediate region 100B is a region that is in an intermediate state between the plastically deformed state and the original state of the wafer 100 (elastic state).
[0041] In the plastically deformed region 100A on the surface of the wafer 100 thus formed, unlike surface polishing without plastic deformation, the grinding efficiency is significantly improved by the diamond polishing grains 53, and a mirror finish with high flatness can be achieved in one go. In other words, the complicated manufacturing process, such as multiple lappings (first to fourth), can be significantly simplified.
[0042] Here, (3) it is important that the advancing speed of the spindle 51 relative to the platen 52 does not exceed the depth of the plastic deformation region.
[0043] As shown diagrammatically in FIG. 5A, (3) the advancing speed of the spindle 51 relative to the platen 52 is controlled so as not to exceed the depth of the plastic deformation region 100A, i.e., by constantly keeping the plastic deformation region 100A present on the surface of the wafer 100 (assuming, of course, that no particle size of the diamond polishing grains 53 is adopted that exceeds the region width of the plastic deformation region 100A (the layer thickness of the plastic deformation region 100A, which is synonymous with the depth of the plastic deformation region 100A)), it is possible to continuously form the plastic deformation region 100A while achieving a highly flat mirror finish in one go using the diamond polishing grains 53.
[0044] On the other hand, as shown diagrammatically in FIG. 5B, if a diamond abrasive grain 53' having a particle size that exceeds the width of the plastic deformation region 100A (left side of the figure), or if the advancing speed of the spindle 51 relative to the platen 52 is increased beyond the depth of the plastic deformation region 100A (right side of the figure), cracks will propagate, resulting in a wafer 100' with a work-affected layer after processing.
[0045] In this way, according to the grinding method for SiC wafers, which are semiconductor crystal wafers, of the present embodiment, it is possible to actually provide a grinding method for semiconductor crystal wafers that can achieve higher grinding accuracy by managing plastic deformation, which has been conventionally disliked, as a plastic deformation mechanism of the wafer surface.
[0046] According to the grinding method for a SiC wafer of this embodiment, the wafer 100 after grinding has a mirror finish with high flatness, so that the mirror surfaces of the wafer 100 can be extended by crystal bonding (strong adhesion between mirror-polished metal surfaces) as shown in FIG. 6.
[0047] Here, such crystal bonding (strong adhesion of mirror-polished metal surfaces) is not limited to the wafer 100, so when it is difficult to obtain a long SiC ingot due to low crystal growth, the end faces of the SiC ingot can be ground to a mirror finish using the above-mentioned grinding method, and the end faces of the SiC ingot that have been ground to a mirror finish can be bonded together to extend the ingot.
[0048] Then, by subjecting the thus obtained SiC extended ingot to the series of processing steps from STEP 100 to STEP 130, a SiC wafer with a highly flat mirror finish can be obtained in one go from the SiC extended ingot.
[0049] In other words, the end faces of a single SiC ingot are joined together to extend it, so that the desired long ingot can be obtained by repeating the joining process without relying on the growth properties of the crystal itself.
[0050] Furthermore, the bonding here is a crystalline bond in which the end faces that have been ground to a highly flat mirror surface are bonded together, so a strong bond can be achieved while still maintaining the shape when cutting wafers from the elongated SiC ingot, resulting in an ingot with excellent workability.
[0051] In addition, when joining the end faces of a SiC ingot to extend it, it is preferable to form a notch in the side of a single SiC ingot, and when joining them, align the notches to join the end faces that have been ground to a mirror finish and extend them.
[0052] This allows the outer diameters of the bonded SiC ingots to be uniform, and an extended SiC ingot with a uniform outer diameter and no deviation from the central axis can be obtained.
[0053] In other words, from the perspective of processability, it is desirable for the extended ingot that is joined and extended to have a uniform outer diameter shape. By providing one or more notches on the side of a single SiC ingot and aligning the notches, the outer diameter shape of the single SiC ingots can be aligned when joining them together, and ultimately an extended SiC ingot with a uniform outer diameter shape can be obtained.
[0054] In this way, by applying this to an extended SiC ingot and a manufacturing method for an extended SiC ingot, it is possible to obtain a long ingot without relying on the growth of the crystal, and further, it is possible to achieve excellent and higher workability while maintaining the quality of the crystal.
[0055] In addition, in this embodiment, a grinding method for a SiC wafer has been described in terms of producing a SiC wafer from a SiC ingot. However, the semiconductor crystal is not limited to SiC, and may be gallium phosphate, indium phosphide, silicon, or other compound semiconductors. [Explanation of symbols]
[0056] 50...mechanical polishing device (ultra-high synthesis high precision grinding device), 51...spindle (wafer support table), 52...platen (grinding table), 53...diamond abrasive grains, 54...vacuum porous chuck (suction plate), 100...SiC wafer (semiconductor crystal wafer), 110...one side, 120...other side.
Claims
1. A SiC extended ingot is formed by joining a single SiC ingot that has been ground into a cylindrical shape in an axial direction and extending the ingot, The single SiC ingot has an end surface ground to a mirror surface, A SiC extended ingot, characterized in that the end faces of the SiC ingot, which have been ground to a mirror finish, are joined together to extend the ingot.
2. The SiC ingot according to claim 1, The single SiC ingot has a notch cut into its side surface, The SiC extended ingot is characterized in that the SiC ingots are extended by joining their mirror-ground end faces with the notches aligned.
3. A method for manufacturing an extended SiC ingot by joining a single SiC ingot ground into a cylindrical shape in an axial direction and extending the ingot, comprising: a grinding process step of grinding an end surface of the single SiC ingot into a mirror surface; a bonding step of bonding end surfaces of the SiC ingot that has been ground to a mirror finish by the grinding step; The method for producing an extended SiC ingot comprises: extending the single SiC ingot in the axial direction by the bonding process.
Citation Information
Patent Citations
MANUFACTURING METHOD OF SiC SINGLE CRYSTAL INGOT
JP2020083704A