Manufacturing method for concretion
By using a container with a permeable bottom to introduce calcium ions into a powder layer followed by carbonate and bicarbonate ions, the method ensures uniform solid precipitation within the powder layer, addressing the inefficiencies of existing concretion production methods and reducing environmental impact through seawater utilization and CO2 capture.
Patent Information
- Application Number
- JP2023052925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing methods for producing concretions using calcium and carbonate ions do not effectively precipitate solids within a powder layer, often resulting in incomplete or misplaced solid formation.
A method involving a container with a permeable bottom for calcium ions and a controlled pH environment is used to introduce carbonate and bicarbonate ions, ensuring calcium ions are present in the powder layer first, promoting preferential precipitation of calcium carbonate within the powder layer.
This approach facilitates the formation of concretions by ensuring uniform and complete solid precipitation within the powder layer, reducing environmental impact by utilizing seawater as a calcium ion source and capturing CO2 from cement manufacturing exhaust.
Smart Images

Figure 2024141338000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing concretions. [Background technology]
[0002] In the manufacture of cement products, large amounts of CO2 are generated, including CO2 generated during fuel combustion and CO2 generated during the decarbonation of raw materials, and there is a growing demand to reduce carbon dioxide emissions as a measure to combat global warming.
[0003] It has also been observed in nature that calcium carbonate precipitates between particles of sand and other materials, coagulating to form hardened bodies such as carbonate concretions. Since CO2 is consumed during the formation of concretions, if the concretion production process can be applied to produce hardened bodies that can be used industrially, it is believed that they can be used as an alternative to existing cement products, thereby reducing the environmental burden. Methods for artificially producing concretions are currently being investigated.
[0004] For example, Patent Document 1 discloses a method for producing a hardened body, which comprises the steps of: (I') adding particles containing a Ca source and / or a Mg source to a liquid containing at least water; (II) dissolving CO2 in the liquid obtained in step (I'); thereby obtaining a liquid containing Ca(HCO3)2 and / or Mg(HCO3)2; (III) forming an aggregate into a predetermined shape; (IV) adding the liquid containing Ca(HCO3)2 and / or Mg(HCO3)2 to the predetermined shape obtained in step (III); and (V) changing the environment within the predetermined shape obtained in step (IV); wherein the hardened body is formed from the aggregate and a substance present between the aggregates, and the substance contains carbonate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2022-162955 A Summary of the Invention [Problem to be solved by the invention]
[0006] Seawater, an abundant natural resource, is expected to be used as a calcium ion source. In considering the use of seawater, it is desirable to develop a method for producing concretions using two liquids: a solution containing calcium ions that mimics seawater, and a solution in which CO2 is dissolved. In addition, if it is possible to produce concretions using these two liquids, it would be useful to use CO2 generated in cement production, etc., as it would be possible to fix it in concretions.
[0007] Therefore, an object of the present disclosure is to provide a method for producing concretions using a solution containing calcium ions and a solution containing carbonate ions and bicarbonate ions. [Means for solving the problem]
[0008] The inventors' investigations have revealed that concretions do not form simply by mixing a solution containing calcium ions with a solution containing carbonate ions and hydrogen carbonate ions around powder containing aggregate. Specifically, there are problems in that solid precipitation does not occur or occurs at a location distant from the powder.
[0009] As a result of further intensive research, the inventors have found that by using a container equipped with a cylindrical body and a blocking member that blocks the opening at the lower end of the cylindrical body and is permeable to a first solution containing calcium ions, first filling the container with powder containing aggregate to form a powder layer, then introducing the first solution containing calcium ions into the container from the bottom side of the container to immerse the powder layer in the first solution, and then injecting a solution containing carbonate ions and bicarbonate ions having a predetermined pH from the top side of the container, a solid will precipitate inside the powder layer, thereby producing concretions.
[0010] In some aspects, the present invention provides the following [1] to [7]. [1] A method for producing concretions, comprising the steps of: A step of filling a container including a cylindrical body and a blocking member for blocking an opening at a lower end side of the cylindrical body and allowing a first solution containing calcium ions to permeate therethrough with powder containing aggregate to form a powder layer; a step of inserting the container into the first solution from the lower end side of the cylindrical body to introduce the first solution into the container through the closing member and immersing the powder layer in the first solution; and injecting a second solution containing carbonate ions and bicarbonate ions into the container from an opening on the upper end side of the cylindrical body, thereby precipitating a solid inside the powder bed. The method of manufacturing, wherein the pH of the second solution is greater than 8.30. [2] The manufacturing method described in [1], wherein the concentration of calcium ions in the first solution is 0.9 mol / L or more. [3] The manufacturing method according to [1] or [2], wherein the total concentration of carbonate ions and bicarbonate ions in the second solution is 1.0 mol / L or more. [4] The manufacturing method according to any one of [1] to [3], further comprising a step of neutralizing a raw powder containing an aggregate to obtain a powder. [5] The manufacturing method according to any one of [1] to [4], wherein the aggregate has a coarse aggregate ratio of 2.00 or less. [6] The manufacturing method according to any one of [1] to [5], wherein the second solution is produced by a method comprising adding carbon dioxide recovered from exhaust gas of a cement plant to a solvent containing water. [7] The manufacturing method according to any one of [1] to [6], further comprising a step of preparing a first solution from seawater. Effect of the Invention
[0011] According to the present disclosure, a method for producing concretions can be provided using a solution containing calcium ions and a solution containing carbonate ions and bicarbonate ions. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view showing one embodiment of a method for producing concretions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. However, the following embodiment is an example for explaining the present disclosure, and is not intended to limit the present disclosure to the following contents. In the description, the same elements or elements having the same functions are designated by the same reference numerals, and overlapping descriptions are omitted in some cases. In addition, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of each element are not limited to the ratios shown in the drawings.
[0014] Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more. In addition, in this specification, a numerical range indicated by the symbol "-" includes a lower limit and an upper limit. In other words, a numerical range indicated by "x-y" means a range equal to or greater than x and equal to or less than y.
[0015] The present disclosure provides a method for producing concretions, which includes contacting a first solution containing calcium ions with a second solution containing carbonate ions and bicarbonate ions in a powder layer containing aggregates to form concretions. In the method according to the present disclosure, the first solution containing calcium ions is brought into contact with the powder layer in advance, thereby enabling carbonates and the like to be preferentially precipitated in the powder layer, and providing desired concretions. The reason why such an effect is obtained is not necessarily clear, but according to the study by the present inventors, when the second solution is brought into contact with the powder layer in advance, concretions may not be formed. Therefore, the present inventors speculate that the above-mentioned effect is obtained by first having calcium ions present in the powder layer, so that carbonate ions and bicarbonate ions in the second solution react with calcium ions while diffusing in the solution in the powder layer, or by unevenly distributing the site of reaction between calcium ions and carbonate ions, etc. on the surface of aggregates, etc., so that calcium carbonate generated by the reaction between calcium ions and carbonate ions, etc. can be preferentially precipitated inside the powder layer.
[0016] One embodiment of the method for producing concretions includes a step of filling a container having a cylindrical body and a blocking member that blocks the opening at the lower end side of the cylindrical body and allows a first solution containing calcium ions to penetrate into the container with powder containing aggregates to form a powder layer (hereinafter also referred to as the "first step"); a step of introducing the first solution into the container through the blocking member by inserting the container from the lower end side of the cylindrical body to immerse the powder layer in the first solution (hereinafter also referred to as the "second step"); and a step of injecting a second solution containing carbonate ions and bicarbonate ions into the container from the opening at the upper end side of the cylindrical body to precipitate a solid inside the powder layer (hereinafter referred to as the "third step"). The pH of the second solution is greater than 8.30.
[0017] Fig. 1 is a schematic cross-sectional view for explaining one embodiment of the method for producing concretions. As shown in Fig. 1, the container 1 in the first step includes a cylindrical body 2 and a blocking member (first blocking member) 3 that blocks the opening on the lower end side of the cylindrical body 2.
[0018] The cylindrical body 2 functions as a side part of the container 1. The cylindrical body 2 is tubular with both ends in the extension direction of the cylindrical body 2 open. The cylindrical body 2 may be, for example, a square tube, a cylindrical shape, or an elliptical tube shape. The shape of the cylindrical body 2 is not limited thereto, and may be, for example, a shape that matches the shape of the concretion to be manufactured. The shape of the cross section perpendicular to the extension direction of the cylindrical body 2 (the shape of the opening formed by the inner wall of the cylindrical body 2) is not particularly limited, and may be, for example, a polygon such as a rectangle, a square, or a hexagon, a circle, or an ellipse. The shape of the cross section can also be the shape (product shape) in which the concretion is used. By making the shape of the cross section the product shape, it can be used without subsequent processing, etc., which can contribute to reducing the amount of CO2 generated.
[0019] The area of the opening in the cross section perpendicular to the extending direction of the cylindrical body 2 can be adjusted according to the application of the concretion to be manufactured. When the concretion to be manufactured is used as a building material such as aggregate or roadbed material, the area of the opening is, for example, 1500 to 4000000 mm. 2 , 1500~1000000mm 2 , or 1,000,000 to 4,000,000 mm 2 By using a cylinder having an opening area within the above numerical range, for example, plate-shaped concretions having a thickness of several centimeters to several tens of centimeters can be produced, and aggregates and the like can be produced by crushing the concretions. In addition, when the produced concretions are used as they are as industrial materials and the like, the opening area is, for example, 0.09 to 25 m2. 2 , 0.09~4m 2 , or 4~25m 2 It may be.
[0020] The material of the cylindrical body 2 may be any material that is impermeable to the first solution, the second solution, and the powder described below, thereby reducing contact between the first solution and the second solution in places other than the powder layer 4 and enabling the desired concretions to be formed more sufficiently. The material constituting the cylindrical body 2 may be, for example, wood, glass, plastic (polyvinyl chloride, etc.), or metal (steel, etc.).
[0021] The blocking member 3 functions as the bottom of the container 1 in which the powder is filled. In other words, the blocking member 3 is impermeable to the powder. On the other hand, the blocking member 3 is permeable to the first solution containing calcium ions. The blocking member 3 may have a path (e.g., a hole) through which the first solution containing calcium ions can pass along the extension direction of the cylindrical body 2. When the blocking member 3 has a hole, the maximum diameter of the hole may be, for example, 3 μm or more. The maximum diameter of the hole may be smaller than the maximum particle size of the aggregate contained in the powder, and may be, for example, 50 μm or less, or 30 μm or less. The blocking member 3 may be, for example, paper, foam, woven fabric, nonwoven fabric, net, mesh, etc. Examples of materials constituting the blocking member 3 include natural fibers containing cellulose, synthetic resins (polypropylene, etc.) and synthetic fibers containing the same, and metals.
[0022] In FIG. 1, the blocking member 3 is shown as being disposed so as to cover the opening at the lower end side of the cylindrical body 2, but it may be disposed inside the cylindrical body 2. In FIG. 1, the blocking member 3 is shown as being disposed so that the upper surface of the blocking member 3 is perpendicular to the extending direction of the cylindrical body 2, but this is not limited thereto, and the blocking member 3 may be disposed so that the upper surface of the blocking member 3 is inclined with respect to the extending direction of the cylindrical body 2. In FIG. 1, the surface of the blocking member 3 that blocks the opening of the cylindrical body 2 is formed in a flat shape, but the shape of the surface is not limited thereto. The surface may be provided with recesses, protrusions, etc. according to the shape of the concretions to be manufactured. The blocking member 3 may also function as a mold member that fixes the shape of the powder layer 4.
[0023] In the first step, the container 1 is filled with powder containing aggregate to form the powder layer 4. When forming the powder layer 4, pressure or the like may be applied in order to reduce the gaps between the particles constituting the powder. In this case, the powder layer 4 can also be called a compressed powder layer. The powder contains aggregate. The aggregate may be, for example, coarse aggregate, fine aggregate, etc. The aggregate, coarse aggregate, and fine aggregate are defined by JIS A 0203:2019.
[0024] The aggregate may have a coarse particle ratio of 1.00 or more, 1.05 or more, 1.10 or more, or 1.15 or more. When the aggregate has a coarse particle ratio of 1.00 or more, the aggregate has excellent handleability in production and can produce concretions more efficiently. The aggregate may have a coarse particle ratio of 5.00 or less, 4.00 or less, 3.00 or less, 2.80 or less, 2.60 or less, 2.40 or less, 2.20 or less, 2.00 or less, 1.80 or less, 1.60 or less, 1.40 or less, or 1.20 or less. When the aggregate has a coarse particle ratio of 1.00 or more, the concretions can be produced more quickly because the voids in the powder layer 4 (i.e., the voids to be filled by the solid precipitated in the third step described later) are smaller when the aggregate has a coarse particle ratio of 1.00 to 5.00, or 1.05 to 3.00, for example. The coarse aggregate ratio is measured in accordance with JIS A 1102:2014.
[0025] The maximum particle size of the aggregate may be 50 μm or more, 80 μm or more, or 100 μm or more. When the maximum particle size of the aggregate is equal to or more than the lower limit, voids suitable for the production of concretions are easily formed inside the powder layer 4. The maximum particle size of the aggregate may be 250 mm or less, 100 mm or less, or 40 mm or less. When the maximum particle size of the aggregate is equal to or less than the upper limit, voids inside the powder layer 4 (i.e., voids to be filled by the solid precipitated in the third step described later) become smaller, so that concretions can be produced more quickly. The maximum particle size (maximum dimension) of the aggregate is measured in accordance with JIS A 1102:2014.
[0026] Examples of coarse aggregates include gravel, crushed stone, blast furnace slag coarse aggregate, electric furnace oxidized slag coarse aggregate, molten slag coarse aggregate, recycled coarse aggregate, etc. Examples of fine aggregates include silica sand, river sand, land sand, sea sand, crushed sand, blast furnace slag fine aggregate, copper slag fine aggregate, electric furnace oxidized slag fine aggregate, recycled fine aggregate, etc.
[0027] The powder containing aggregate may contain only aggregate, or may contain aggregate and other materials. Examples of the other materials include inorganic minerals, fillers, concrete admixtures (excluding those that fall under the above-mentioned aggregates), organic fibers such as synthetic fibers, industrial by-products, etc. The content of the other materials may be, for example, 10% by mass or less, or 1% by mass or less, based on the total amount of the powder.
[0028] In order to facilitate precipitation of a solid inside the powder layer 4 in the third step described below, it is preferable that the powder does not substantially contain an acidic substance. According to the study by the present inventors, depending on the type of raw material powder of the powder, the supernatant liquid when the raw material powder is immersed in water may be acidic. In such a case, it is preferable to neutralize the raw material powder.
[0029] The above-mentioned manufacturing method may further include a step of obtaining a powder by neutralizing the raw powder containing aggregate. The method of neutralizing the raw powder may include a step of immersing the raw powder in a solvent containing water such as water or seawater. In this step, the raw powder may be immersed in a solvent containing water and left until the pH of the supernatant is 7.00 or more, the solvent may be replaced several times until the pH of the supernatant is 7.00 or more, or after immersion, the pH of the supernatant may be adjusted to 7.00 or more using an acid or alkali. The time for immersing the raw powder in the solvent containing water may be, for example, 1 hour or more, or may be 1 day or less. After the neutralization treatment as described above, the powder may be used in a state containing the solvent, but preferably the content of the solvent is reduced or removed before use as the powder. By reducing or removing the content of the solvent, it is expected that the adhesion of calcium ions to the powder surface when the first solution is contacted with the powder is more likely to occur, and the powder can be more homogenized.
[0030] In Fig. 1, the powder layer 4 is formed in a columnar shape (rectangular columnar, cylindrical, etc.), but the shape of the powder layer 4 is not limited thereto. The shape of the powder layer 4 may be adjusted to be the same as the shape of the concretions to be produced. In this case, for example, a mold member or the like for adjusting the shape of the upper surface side of the powder layer 4 may be used.
[0031] In the first step, after the powder layer 4 is formed, a second blocking member that blocks the opening of the cylindrical body 2 may be placed on the powder layer 4. The second blocking member may function as a mold member that fixes the shape of the powder layer 4, for example. In the second blocking member, the surface that blocks the opening of the cylindrical body 2 may be perpendicular to the extension direction of the cylindrical body 2, or may be inclined with respect to the extension direction of the cylindrical body 2. In the second blocking member, the surface that blocks the opening of the cylindrical body 2 may be formed in a flat shape. In addition, the surface of the second blocking member on the powder layer 4 side may have a shape that matches the shape of the concretion to be manufactured, may be an inclined surface, and may be provided with a recess, a protrusion, or the like. The shape and material of the second blocking member may be the same as or different from the first blocking member. The shape and material of the second blocking member can be applied to the contents described for the first blocking member.
[0032] In the second step, the container 1 is inserted into the first solution 5 from the lower end side (the side where the first closing member 3 is provided) of the cylindrical body 2, so that the first solution 5 is introduced into the container 1 through the closing member 3, and the powder layer 4 is immersed in the first solution 5. Although FIG. 1 shows an example in which the first solution 5 is contained in a water tank 6, the water tank 6 is not essential. For example, when seawater is used as the first solution 5, the second step can be performed by inserting the container 1 into the sea.
[0033] In the third step, the second solution 7 is poured into the container 1 from the opening at the upper end side of the cylinder 2, and a solid is precipitated in the powder layer 4. Since the powder layer 4 is a layer formed by filling with powder, there are voids therein. When the first solution 5 and the second solution 7 come into contact with each other in the container 1 in the third step, a reaction between the calcium ions contained in the first solution 5 and the carbonate ions contained in the second solution 7 proceeds in the voids in the powder layer 4, and a solid containing calcium carbonate is precipitated. In this way, the solid precipitated in the third step fills some or all of the voids in the powder layer 4, and concretions are formed.
[0034] The inventors have found that when the operations in the second step and the third step are interchanged, that is, when the powder layer is formed, the second solution is poured into the container to immerse the powder layer in the first solution, and then the container is inserted into the first solution from the lower end side of the cylinder, the intended concretions may not be obtained due to the segregation of solids containing calcium carbonate outside the powder layer. Therefore, in the above-mentioned manufacturing method, it is important to pour the second solution into the container in the third step after immersing the powder layer in the first solution in the second step.
[0035] The present inventors have found that one of the reasons why concretions are not generated when the operations in the second step and the third step are interchanged is that solid precipitation is likely to occur under the contact interface between the first solution 5 and the second solution 7. Therefore, from the viewpoint of easily manufacturing concretions of the intended shape, in the second step, it is preferable that the powder layer 4 is immersed in the first solution 5 up to the top of the powder layer 4. In addition, it is preferable that the third step is performed after the powder layer 4 is immersed in the first solution 5 up to the top of the powder layer 4. In the third step, the injection of the second solution may be started immediately after the top of the powder layer 4 is immersed in the first solution.
[0036] The second step may include confirming that the top of the powder layer 4 is immersed in the first solution 5. By moving to the third step after confirming that the liquid level of the first solution 5 has reached the top of the powder layer 4, the solid generated by the contact between the first solution 5 and the second solution 7 can be precipitated more uniformly throughout the powder layer, and the quality of the concretions obtained can be further improved. Methods for confirming that the top of the powder layer 4 is immersed in the first solution 5 include, for example, visual inspection, excavating the powder layer, and installing a moisture meter. For example, a means for detecting the liquid level position of the first solution may be provided on the inner wall of the cylinder 2.
[0037] Furthermore, the inventors have found that even when the first solution and the second solution are interchanged, that is, when the powder layer is immersed in a solution containing carbonate ions and bicarbonate ions in the second step and then a solution containing calcium ions is poured into the container in the third step, no concretions are generated. Therefore, in the above-mentioned manufacturing method, it is important to use the first solution containing calcium ions in the second step and the second solution containing carbonate ions and bicarbonate ions in the third step.
[0038] The reason why it is important to use a first solution containing calcium ions in the second step and a second solution containing carbonate ions and bicarbonate ions in the third step is not clear, but it is considered that in the manufacturing method according to one embodiment, the powder layer is immersed in a solution containing calcium ions in the second step, and the calcium ions are adsorbed to the powder layer 4, resulting in a state in which sufficient calcium ions are present in the voids of the powder layer 4. For this reason, it is considered that when carbonate ions and bicarbonate ions are supplied around the calcium ions in the subsequent third step, solids are likely to precipitate inside the powder layer 4.
[0039] The first solution 5 contains calcium ions. Since the first solution 5 is a source of Ca, the concentration of the first solution 5 may be low when calcium ions can be continuously supplied, such as when seawater is used. On the other hand, in cases where the size of the production equipment is limited, the concentration of calcium ions in the first solution 5 may be, for example, 0.01 mol / L or more, 0.1 mol / L or more, 0.7 mol / L or more, or 0.9 mol / L or more, from the viewpoint of sufficient supply of calcium ions. The concentration of calcium ions in the first solution 5 may be, for example, 7.0 mol / L or less, from the viewpoint of preventing supersaturation and precipitation of solutes in the first solution 5. The concentration of calcium ions in the first solution 5 may be 0.1 to 7.0 mol / L.
[0040] The pH of the first solution may be 6.50 or more, 6.80 or more, or 6.90 or more from the viewpoint of more easily precipitating a solid in the third step. The pH of the first solution may be 9.00 or less, 8.80 or less, 8.50 or less, or 8.00 or less from the viewpoint of creating conditions that facilitate the formation of concretions. The pH of the first solution may be 6.50 to 9.00, or 6.80 to 8.50. In this specification, pH means a value measured by a pH meter.
[0041] The temperature of the first solution may be 0° C. or higher, or 5° C. or higher. The temperature of the first solution may be 40° C. or lower, or 30° C. or lower. The temperature of the first solution may be, for example, 10 to 40° C.
[0042] The first solution can be prepared, for example, by dissolving a compound (a compound having calcium as a constituent atom) that is a source of calcium ions in a solvent containing water. Examples of compounds having calcium as a constituent atom include calcium halides such as CaCl2, CaBr2, and CaI2. Seawater, brine generated during the production of table salt, sludge water or recycled water generated in a ready-mix concrete plant, etc. can also be used as the first solution.
[0043] The first solution may also be prepared using seawater as a raw material. The above-mentioned manufacturing method may further include a step of preparing the first solution from seawater. The step of preparing the first solution from seawater may be, for example, a step of preparing a compound having calcium as a constituent atom, such as calcium chloride, from seawater and dissolving it in a solvent such as water to prepare the first solution, a step of extracting calcium ions from seawater and adding it to a solvent such as water to prepare the first solution, or a step of concentrating seawater to increase the concentration of calcium ions to prepare the first solution.
[0044] The second solution contains carbonate ions and bicarbonate ions. From the viewpoint of facilitating precipitation of a solid in the third step, the total concentration of carbonate ions and bicarbonate ions in the second solution may be 0.1 mol / L or more, 0.3 mol / L or more, 1.0 mol / L or more, 1.1 mol / L or more, or 1.2 mol / L or more. The total concentration of carbonate ions and bicarbonate ions in the second solution may be, for example, 1.9 mol / L or less. The concentration of carbonate ions and bicarbonate ions in the second solution may be 0.1 to 1.9 mol / L.
[0045] The pH of the second solution is more than 8.30. The pH of the second solution may be higher than the pH of the first solution. From the viewpoint of more easily precipitating a solid, the pH of the second solution may be 8.50 or more, 9.00 or more, more than 9.00, 9.50 or more, 10.00 or more, 11.00 or more, 11.50 or more, or 11.60 or more. From the viewpoint of more easily precipitating a solid by increasing the concentration of carbonate ions in the second solution, the pH of the second solution may be more than 9.00. From the viewpoint of safety, the pH of the second solution may be, for example, 14.00 or less, 13.00 or less, or 12.00 or less. The pH of the second solution may be more than 8.30 and 14.00 or less, or 9.00 to 13.00.
[0046] The temperature of the second solution may be 10° C. or higher, or 20° C. or higher. The temperature of the second solution may be 40° C. or lower, or 30° C. or lower. The temperature of the second solution may be, for example, 10 to 40° C.
[0047] The second solution may be prepared, for example, by dissolving a compound that is a source of carbonate ions or bicarbonate ions in a solvent containing water. Examples of compounds that are sources of carbonate ions include alkali metal carbonates such as Na2CO3 and K2CO3, (NH4)2CO3, etc. Examples of compounds that are sources of bicarbonate ions include alkali metal bicarbonates such as NaHCO3 and KHCO3, Ca(HCO3)2, NH4HCO3, etc.
[0048] The second solution may be prepared by using a compound that generates carbonate ions or hydrogen carbonate ions, or may be prepared by using carbon dioxide contained in exhaust gas from a cement factory as a raw material. In this case, the above-mentioned production method may further include a step of preparing the second solution by using carbon dioxide contained in exhaust gas from the cement factory as a raw material.
[0049] An example of a method for preparing a second solution using carbon dioxide contained in exhaust gas from a cement factory as a raw material is a method that includes adding carbon dioxide recovered from exhaust gas from a cement factory to a solvent containing water. Examples of a method for recovering carbon dioxide from exhaust gas from a cement factory include a method of recovering carbon dioxide gas as liquefied carbon dioxide gas from the exhaust gas from a cement factory and adding the liquefied carbon dioxide gas to a solvent containing water, and a method of adsorbing carbon dioxide contained in exhaust gas from a cement factory to a carbon dioxide adsorbent, desorbing the carbon dioxide, and adding it to a solvent containing water. For example, an amine compound can be used as the carbon dioxide adsorbent.
[0050] The second step may be carried out at a temperature of 0 to 40° C. or 10 to 30° C. Also, the second step may be carried out under atmospheric pressure. The third step may be carried out at a temperature of 10 to 40° C. or 20 to 30° C. Also, the third step may be carried out under atmospheric pressure.
[0051] The third step may include controlling the internal pressure of the cylindrical body 2. The control of the internal pressure of the cylindrical body 2 may be, for example, by increasing the internal pressure of the cylindrical body 2. In the third step, if precipitation of a solid progresses in the voids in the upper part of the powder layer 4, the second solution is prevented from descending, making it difficult to supply carbonate ions and bicarbonate ions to the voids in the lower part of the powder layer 4. In such a case, by increasing the internal pressure of the cylindrical body 2, it may be possible to supply carbonate ions and bicarbonate ions to the voids in the lower part of the powder layer 4. EXAMPLES
[0052] The present disclosure will be described in more detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the following examples.
[0053] [Powder preparation] A quantity of water was added to the raw powder (manufactured by Nippyo Mining Co., Ltd., product name "Silica Sand N60", coarse particle ratio 1.06, maximum particle size 0.3 mm) so that the raw powder was completely submerged. After confirming that the pH of the supernatant liquid was 7.00 or higher, the powder was obtained by filtration.
[0054] [Concrete manufacturing] <Examples 1-1 and 1-2> The following experiment was carried out under atmospheric pressure and at a temperature of 20°C. First, a cylinder (5 cm long x 5 cm wide x 25 cm high, material: polyvinyl chloride) was prepared. Next, the opening at the lower end of the cylinder was covered with filter paper (manufactured by Toho Separator Co., Ltd., product name "Filtration #6008", pore size: 8-10 μm, material: polypropylene), and the filter paper was fixed to the cylinder using an epoxy adhesive to prepare a container. The container was filled with the powder obtained by the neutralization treatment described above, and a powder layer (4.0 cm long x 4.0 cm wide x 4.0 cm high) was formed. After that, the container was inserted into a first solution (CaCl2 aqueous solution, calcium ion concentration: 1.0 mol / L, temperature: 20°C) contained in a 5 L capacity beaker with handles, and the first solution was introduced into the container through the filter paper, and the powder layer was immersed in the first solution. Immediately after the entire powder layer was immersed in the first solution, the second solution (Na2CO3 aqueous solution, total concentration of carbonate ion and bicarbonate ion: 1.7 mol / L, temperature: 20°C) was poured into the container from the opening on the upper end side of the container. Immediately after this, a pH meter (manufactured by METTLER TOLEDO Co., Ltd., product name "pH meter FiveEasy F20") was inserted into the first solution and the second solution, and the pH was measured. Seven days after the injection of the second solution, the container was pulled up and the concretion generation status was evaluated. Specifically, the container was disassembled and the powder layer was checked by touch with the fingers to see if it had solidified, and if it had solidified, the layer was further immersed in water to check whether it had crumbled. Evaluation was performed according to the following criteria, and it was determined that concretions had been generated in the case of A or B. The results are shown in Table 1. A: The powder layer is solid and will not crumble even when immersed in water. B: The powder layer is solidified, but some of it crumbles when immersed in water. C: The powder layer is solidified, but it completely crumbles when immersed in water. D: The powder layer is not solidified.
[0055] <Examples 2-1 and 2-2> The same experiments as in Examples 1-1 and 1-2 were carried out except that the concentration of the second solution (Na2CO3 aqueous solution) was changed. The results are shown in Table 1.
[0056] <Comparative Examples 1-1 and 1-2> The same experiments as in Examples 1-1 and 1-2 were carried out, except that the first solution and the second solution were exchanged so that the powder layer was brought into contact with the second solution first. The results are shown in Table 1.
[0057] [Table 1]
[0058] As shown in Table 1, in Examples 1-1 and 1-2, and Examples 2-1 and 2-2, concretions could be produced. On the other hand, in Comparative Examples 1-1 and 1-2 in which the first solution and the second solution were replaced, no concretions were produced. From the above results, it was found that in order to produce concretions, it is necessary to use a solution containing calcium ions as the first solution and a solution containing carbonate ions and bicarbonate ions as the second solution. In Example 1-2, concretions of about 1 cm length x about 1 cm width x about 1 cm height were produced, whereas in Example 1-1, concretions of about 4 cm length x 4 cm width x about 1.5 cm height were produced, which was a more desirable result. [Explanation of symbols]
[0059] 1...container, 2...cylinder, 3...closing member, 4...powder bed, 5...first solution, 6...water tank, 7...second solution.
Claims
1. A method for producing concretions, comprising the steps of: A step of filling a container including a cylindrical body and a blocking member that blocks an opening at a lower end side of the cylindrical body and is permeable to a first solution containing calcium ions with powder containing aggregate to form a powder layer; a step of inserting the container into the first solution from a lower end side of the cylindrical body to introduce the first solution into the container through the closing member and immersing the powder layer in the first solution; and injecting a second solution containing carbonate ions and bicarbonate ions into the container from an opening on the upper end side of the cylinder, thereby precipitating a solid inside the powder bed. The method of manufacturing, wherein the pH of the second solution is greater than 8.
30.
2. The method according to claim 1 , wherein the concentration of calcium ions in the first solution is 0.9 mol / L or more.
3. The method according to claim 1 or 2, wherein a total concentration of the carbonate ions and the bicarbonate ions in the second solution is 1.0 mol / L or more.
4. The method according to claim 1 or 2, further comprising a step of neutralizing a raw powder containing aggregate to obtain the powder.
5. The method according to claim 1 or 2, wherein the aggregate has a coarse particle ratio of 2.00 or less.
6. 3. The method of claim 1 or 2, wherein the second solution is made by a process comprising adding carbon dioxide recovered from exhaust gases of a cement plant to a solvent comprising water.
7. The method of claim 1 or 2, further comprising the step of preparing the first solution from seawater.
Citation Information
Patent Citations
Soil-stabilizing chemical and grouting thereof
JP1991199286A
Hardening treatment agent for fishing bait including krill and production of fishing bait including krill by using the hardening treatment agent
JP1997028311A
Treatment of concrete waste
JP1999319765A
Concrete and concrete curing method
JP2008056538A
Method for producing material comprising cement hardened body
JP2014214030A