Vapor chamber

The vapor chamber design with resin and metal convex portions on metal sheet materials improves flexibility, durability, and heat transport, addressing adhesion and capacity issues in conventional vapor chambers.

JP2024142186APending Publication Date: 2024-10-10SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional vapor chambers lack flexibility, adhesion to heat-generating components, and require improvement in heat transport capacity.

Method used

A vapor chamber design involving a container made of joined metal sheet materials with resin and metal convex portions on the inner surfaces, along with a wick structure, optimized for flexibility, durability, and thermal conductivity.

Benefits of technology

The design enhances flexibility, durability, and heat transport ability, ensuring excellent adhesion and reliability to heat-generating components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142186000001_ABST
    Figure 2024142186000001_ABST
Patent Text Reader

Abstract

To provide a vapor chamber which is excellent in flexibility (resilience), has excellent durability and heat transport capacity, and is excellent in reliability.SOLUTION: A vapor chamber 1 of the invention is formed by joining a metallic first sheet material 11 and a metallic second sheet material 21, and includes: a container 2 having a cavity therein; a wick 30 disposed in the cavity part; a plurality of first protruding parts 12 provided on an inner surface of the first sheet material 11 and made of resin; and a plurality of second protruding part 22 provided on an inner surface of the second sheet material 21 and made of resin. It is preferable that an interval of the first protruding parts 12 be smaller than an interval of the second protruding parts 22.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a vapor chamber. [Background technology]

[0002] For example, heat-generating components such as central processing units (CPUs), light-emitting diodes (LEDs), and power semiconductors used in mobile terminals such as mobile terminals and tablet terminals are cooled by heat pipes (see, for example, Patent Document 1).

[0003] In recent years, in order to make mobile devices thinner, vapor chambers, which can be made thinner than heat pipes, have been developed.

[0004] A working fluid is sealed inside the vapor chamber, and this working fluid absorbs heat from the heat-generating components and transfers the heat, thereby cooling the heat-generating components.

[0005] More specifically, the working fluid in the vapor chamber receives heat from the heat-generating component in the part close to the heat-generating component (evaporation part) and evaporates into vapor, and the vapor then moves to a position away from the evaporation part, where it is cooled and condenses into liquid.

[0006] A liquid flow path section with a capillary structure (wick) is provided within the vapor chamber, and the liquefied working fluid passes through this liquid flow path section and is transported toward the evaporation section, where it is again exposed to heat and evaporated.

[0007] In this way, the working fluid circulates inside the vapor chamber while repeatedly undergoing phase changes, i.e. evaporation and condensation, thereby transferring heat from the device and improving heat dissipation efficiency.

[0008] However, conventional vapor chambers lack flexibility, and depending on the shape of the heat-generating component, it may not be possible to achieve sufficient adhesion to the heat-generating component. Also, there is a demand for further improvement in the heat transport capacity of vapor chambers. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] WO2017 / 104819 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a vapor chamber that has excellent flexibility, durability, heat transport capacity, and reliability. [Means for solving the problem]

[0011] Such an object can be achieved by the present invention described below in (1) to (13). (1) A container formed by joining a first metal sheet material and a second metal sheet material and having a hollow space therein; a wick disposed in the cavity; a plurality of first protrusions made of resin provided on an inner surface of the first sheet material; A vapor chamber characterized by having a plurality of second metallic convex portions provided on the inner surface of the second sheet material.

[0012] (2) A vapor chamber according to (1) above, wherein the distance between the first protrusions is smaller than the distance between the second protrusions.

[0013] (3) The vapor chamber according to (1) or (2) above, when the thickness of the first sheet material is T1 [μm] and the distance between the first convex portions is D1 [μm], satisfies the relationship of 10 < D1 < 80.966exp(0.0512T1).

[0014] (4) The vapor chamber according to any one of (1) to (3) above, when the thickness of the second sheet material is T2 [μm] and the distance between the second convex portions is D2 [μm], satisfies the relationship of 10 < D2 < 80.966exp(0.0512T2).

[0015] (5) In a plan view of the vapor chamber, when the total area of the first convex portions is S1 [cm 2 and the total area of the cavity portions is Sw [cm 2 , the vapor chamber according to any one of (1) to (4) above satisfies the relationship of 0.03 < S1 / Sw < 0.3.

[0016] (6) In a plan view of the vapor chamber, when the total area of the second convex portions is S2 [cm 2 and the total area of the cavity portions is Sw [cm 2 , the vapor chamber according to any one of (1) to (5) above satisfies the relationship of 0.03 < S2 / Sw < 0.3.

[0017] (7) The vapor chamber according to any one of (1) to (6) above, wherein the vapor chamber is used such that the first sheet material side contacts a high-temperature member.

[0018] (8) The vapor chamber according to any one of (1) to (7) above, wherein the height of the first convex portion is 5 μm or more and 500 μm or less.

[0019] (9) The vapor chamber according to any one of (1) to (8) above, wherein the height of the second convex portion is 5 μm or more and 500 μm or less.

[0020] (10) A vapor chamber described in any one of (1) to (9) above, in which when the spacing between the first convex portions is D1 [μm] and the width of the second convex portions is W2 [μm], the relationship W2>D1 is satisfied.

[0021] (11) A vapor chamber according to any one of (1) to (10) above, wherein the thickness of the wick is 10 μm or more and 1000 μm or less.

[0022] (12) A vapor chamber according to any one of (1) to (11) above, wherein the wick is made of glass fiber.

[0023] (13) A vapor chamber according to any one of (1) to (12) above, wherein the container is mainly composed of Cu or a Cu alloy. Effect of the Invention

[0024] According to the present invention, it is possible to provide a vapor chamber that has excellent flexibility, durability, heat transport capacity, and reliability. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a schematic configuration example of a vapor chamber of the present invention. [Diagram 2] FIG. 2 is a perspective view showing a schematic example of a method for manufacturing a vapor chamber. [Diagram 3] FIG. 2 is a perspective view showing a schematic example of a method for manufacturing a vapor chamber. [Figure 4] FIG. 2 is a perspective view showing a schematic example of a method for manufacturing a vapor chamber. [Diagram 5] FIG. 2 is a perspective view showing a schematic example of a prepreg used in the manufacturing method of the vapor chamber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Preferred embodiments of the present invention will now be described in detail. [1] Vapor chamber Fig. 1 is a vertical cross-sectional view showing a schematic configuration example of a vapor chamber of the present invention. Fig. 1 corresponds to a vertical cross-sectional view taken along line A-A' in Fig. 4(1i) shown later.

[0027] In the following description, the vapor chamber 1 will be mainly described in the case where the lower surface (surface of the first sheet material 11) in Fig. 1 comes into contact with the member (heat generating member) to which the vapor chamber 1 is applied, but the vapor chamber 1 may also be used so as to come into contact with the member (heat generating member) to which the vapor chamber 1 is applied on the upper surface in Fig. 1. Also, Fig. 1 shows a state in which the first sheet material 11 faces downward, but the orientation of the vapor chamber 1 when in use is not particularly limited, and for example, the vapor chamber 1 may be used in a state in which the first sheet material 11 faces upward.

[0028] The vapor chamber 1 is formed by joining a first metal sheet material 11 and a second metal sheet material 21 together, and has a container 2 having a hollow portion therein, a wick 30 disposed in the hollow portion, a plurality of first resin protrusions 12 provided on the inner surface of the first sheet material 11, and a plurality of second metal protrusions 22 provided on the inner surface of the second sheet material 21.

[0029] The vapor chamber 1 of the present invention has a plurality of first convex portions 12 made of resin provided on the inner surface of the first sheet material 11, thereby enabling the vapor chamber 1 to have excellent flexibility (pliability). Therefore, regardless of the material to which the vapor chamber 1 is applied or the arrangement, etc., the adhesion between the vapor chamber 1 and the material can be excellent, and the substantial heat transport capacity can be excellent.

[0030] In addition, the vapor chamber 1 of the present invention has a plurality of metallic second protrusions 22 provided on the inner surface of the second sheet material 21, so that the vapor chamber 1 has excellent thermal conductivity and can have excellent substantial heat transport capacity as the vapor chamber 1. In addition, the durability of the vapor chamber 1 can be excellent.

[0031] As a result, the present invention can provide a vapor chamber 1 that has excellent flexibility, durability, heat transport capacity, and reliability. In addition, since the vapor chamber 1 can have excellent flexibility, the vapor chamber 1 can be in good contact with the member to which the vapor chamber 1 is applied, regardless of the member or arrangement, etc., and can reliably exhibit excellent heat transport capacity.

[0032] The excellent effects of the present invention can be obtained by the vapor chamber 1 having the above-mentioned configuration, and cannot be obtained if the vapor chamber 1 does not have the above-mentioned configuration.

[0033] For example, if both the first convex portion and the second convex portion are made of metal, the vapor chamber cannot have sufficiently excellent flexibility.

[0034] Furthermore, for example, if both the first convex portion and the second convex portion are made of resin, the thermal conductivity and durability of the vapor chamber cannot be made sufficiently excellent.

[0035] Furthermore, the vapor chamber 1 of the present invention may be manufactured by any method, but can be suitably manufactured by, for example, the method described below.

[0036] [1-1] Container The container 2 stores the wick 30 and the working fluid 40, and mainly functions in the evaporator section to come into contact with a component to be cooled, such as a heat-generating component, and to transfer heat to the working fluid 40 stored inside the container 2, while in the condenser section it has the function of dissipating heat received from the working fluid 40 undergoing a phase transition from a gas state to a liquid state.

[0037] In the illustrated configuration, the container 2 is sealed at its outer periphery between the first sheet material 11 and the second sheet material 21. This seals the hollow portion housing the wick 30 and the working fluid 40, maintaining a liquid-tight and airtight state.

[0038] The container 2 is not particularly limited as long as it is configured by bonding a first metal sheet material 11 and a second metal sheet material 21 together and has a hollow portion inside. In this embodiment, the container 2 is configured by bonding the first sheet material 11 and the second sheet material 21 together via a bonding material.

[0039] In particular, in the illustrated configuration, the container 2 has a first sheet material 11 and a second sheet material 21 bonded together via a metal plating layer 14 and layers 15 and 23 containing an Sn-containing alloy as bonding materials.

[0040] In the container 2, the space surrounded by the first sheet material 11, the second sheet material 21, the metal plating layer 14, and the layers 15, 23 containing the Sn-containing alloy becomes a cavity.

[0041] [1-1-1] First sheet material Examples of the metal material constituting the first sheet material 11 include Cu, Al, Mg, Zn, and alloys containing at least one of these metals.

[0042] Among them, the metal material constituting the first sheet material 11 is preferably Cu or a Cu alloy.

[0043] Among various metal materials, Cu or Cu alloy is relatively inexpensive and has particularly excellent thermal conductivity and ductility, so that the vapor chamber 1 can have particularly excellent shape conformability and adhesion to the member to which the vapor chamber 1 is applied (for example, a member to be cooled such as a heat generating member), and the substantial heat transport capacity of the vapor chamber 1 can be further improved. Also, the durability of the vapor chamber 1 can be further improved.

[0044] The thickness of the first sheet material 11 is not particularly limited, but is preferably 12 μm or more and 500 μm or less, and more preferably 18 μm or more and 250 μm or less.

[0045] This is particularly advantageous in terms of making the vapor chamber 1 thinner, further improving its flexibility and heat transport capacity, and reducing the raw material costs of the vapor chamber 1, while also making the vapor chamber 1 more durable and reliable.

[0046] [1-1-2] Second sheet material Examples of the metal material constituting the second sheet material 21 include Cu, Al, Mg, Zn, and alloys containing at least one of these metals.

[0047] Among them, the metal material constituting the second sheet material 21 is preferably Cu or a Cu alloy. This provides the same effect as described above.

[0048] The first sheet material 11 and the second sheet material 21 may be made of different materials, but are preferably made of the same material.

[0049] In particular, it is preferable that the container 2 is mainly made of Cu or a Cu alloy.

[0050] This can further improve the substantial heat transport ability of the vapor chamber 1. Also, the durability of the vapor chamber 1 can be further improved.

[0051] Moreover, the first sheet material 11 and the second sheet material 21 may be of the same thickness, or may be of different thicknesses.

[0052] The thickness of the second sheet material 21 is not particularly limited, but is preferably 12 μm or more and 500 μm or less, and more preferably 18 μm or more and 250 μm or less.

[0053] This is particularly advantageous in terms of making the vapor chamber 1 thinner, further improving its flexibility and heat transport capacity, and reducing the raw material costs of the vapor chamber 1, while also making the vapor chamber 1 more durable and reliable.

[0054] [1-1-3] Bonding material In this embodiment, the first sheet material 11 and the second sheet material 21 are bonded together via, for example, a bonding material.

[0055] In particular, in the illustrated configuration, a first sheet material 11 has, as a portion made of a bonding material, a metal plating layer 14 arranged to surround a plurality of first protrusions 12, and a layer 15 made of a material including an Sn-containing alloy.

[0056] In addition, in the illustrated configuration, the second sheet material 21 has a layer 23 made of a material containing an Sn-containing alloy, which is provided as a portion made of a bonding material and surrounds the multiple second protrusions 22.

[0057] As a result, the first sheet material 11 and the second sheet material 21 are joined together appropriately, and the working fluid 40 can be sealed inside the container 2 appropriately.

[0058] [1-1-3-1] Metal plating layer Examples of materials constituting the metal plating layer 14 include Cu, Al, Mg, Zn, and alloys containing at least one of these.

[0059] Among them, the metal material constituting the metal plating layer 14 is preferably Cu or a Cu alloy.

[0060] This makes it possible to further improve the substantial heat transport capacity of the vapor chamber 1.

[0061] Furthermore, when the first sheet material 11 is made of Cu or a Cu alloy, the bonding strength and adhesion between the first sheet material 11 and the metal plating layer 14 can be improved, and the thermal resistance at the interface between the first sheet material 11 and the metal plating layer 14 can be reduced.

[0062] [1-1-3-2] Layer composed of material containing Sn-containing alloy The illustrated configuration has layers 15 and 23 comprised of an Sn-containing alloy.

[0063] Examples of Sn-containing alloys include lead-free solders whose main component is Sn, such as Sn-Ag, Sn-Cu, Sn-Zn, and Sn-Ag-Cu. Of these, lead-free solders whose main component is Sn and whose secondary component is Ag are preferably used. These lead-free solders have higher metal joint strength and higher connection reliability than other lead-free solders.

[0064] [1-2] First protrusion The first protrusions 12 are made of a resin material, and are formed on the inner surface of the first sheet material 11 in a predetermined pattern.

[0065] Since the first convex portion 12 is disposed in the hollow portion of the container 2, a flow path for the working fluid 40 can be suitably secured in the hollow portion of the container 2, and the flow of the working fluid 40 in the hollow portion can be effectively prevented from being obstructed due to deformation of the container 2.

[0066] The formation pattern of the first protrusions 12 is not particularly limited, but in the example shown in the figure, the first protrusions 12 are formed in a cylindrical shape, and when viewed in a plane, the multiple first protrusions 12 are arranged in a staggered pattern.

[0067] The height of the first protrusions 12 is not particularly limited, but is preferably 5 μm or more and 500 μm or less, more preferably 7 μm or more and 400 μm or less, and even more preferably 10 μm or more and 300 μm or less.

[0068] This makes it possible to more suitably secure the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40) while preventing the vapor chamber 1 from becoming unnecessarily thick.

[0069] The width W1 of the first protrusion 12 is not particularly limited, but is preferably 1 μm or more and 2000 μm or less, more preferably 2.5 μm or more and 1000 μm or less, and even more preferably 5 μm or more and 500 μm or less.

[0070] This makes it possible to sufficiently prevent unintended deformation of the container 2 in the thickness direction, while providing the vapor chamber 1 with particularly excellent flexibility.

[0071] In this specification, the width W1 of the first protrusion 12 refers to the maximum width of the first protrusion 12 in a vertical cross-sectional view, and corresponds to the diameter of the first protrusion 12 when the first protrusion 12 is cylindrical. The same applies to the width W2 of the second protrusion 22 described later.

[0072] The pitch P1 of the first convex portions 12 is not particularly limited, but is preferably 10 μm or more and 3000 μm or less, more preferably 50 μm or more and 2000 μm or less, and even more preferably 100 μm or more and 1000 μm or less.

[0073] As a result, while more suitably securing the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40), the flexibility of the vapor chamber 1 can be made particularly excellent.

[0074] In this specification, the pitch P1 of the first convex portion 12 refers to the distance between the centers of adjacent first convex portions 12. The same applies to the pitch P2 of the second convex portion 22 described later.

[0075] Further, when the thickness of the first sheet material 11 is T1 [μm] and the interval between the first convex portions 12 is D1 [μm], it is preferable to satisfy the relationship of 10 < D1 < 80.966exp(0.0512T1).

[0076] As a result, while sufficiently preventing unwanted deformation in the thickness direction of the container 2, the flexibility of the vapor chamber 1 can be made particularly excellent.

[0077] In a plan view of the vapor chamber 1, when the total area of the first convex portions 12 is S1 [cm 2 , and the total area of the cavity portion of the container 2 is Sw [cm 2 , it is preferable to satisfy the relationship of 0.03 < S1 / Sw < 0.3, more preferably to satisfy the relationship of 0.04 < S1 / Sw < 0.25, and even more preferably to satisfy the relationship of 0.05 < S1 / Sw < 0.2.

[0078] As a result, while making the flexibility of the vapor chamber 1 particularly excellent, the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40) can be more suitably secured.

[0079] The resin material constituting the first convex portion 12 is not particularly limited, but in this embodiment, it includes a cured product of a curable resin (for example, a photopolymerizable resin, a thermosetting resin, etc. as described in detail later), specifically, a second resin cured product 140 formed by curing a resin material 140'' which is a resin composition.

[0080] This makes it possible to improve the durability and reliability of the vapor chamber 1. The first convex portion 12 may also contain an alkali-soluble resin, as will be described in detail later.

[0081] [1-2-1] Resin composition In the following description, a resin composition will be described as the uncured resin material 140''.

[0082] The resin composition exhibits adhesiveness by heat treatment after photolithography (for example, the exposure step and development step in the manufacturing method of the vapor chamber 1 described in detail later).

[0083] This allows the resin composition to be suitably used in the manufacture of a vapor chamber with excellent flexibility (pliability) and durability. In particular, in order to bond the prepreg 100' (fiber-containing cured material 100) used in the manufacturing method of the vapor chamber 1 described later to the first sheet material 11, there is no need to perform adhesion using an adhesive, welding, brazing, or the like, and the productivity of the vapor chamber can be particularly excellent. In addition, the adhesion between the prepreg 100' (fiber-containing cured material 100) after the thermal curing process and the protective mask 52 described later can be excellent, and for example, unintended positional displacement of the protective mask 52 during the processing process can be effectively prevented. In addition, since the flexibility (pliability) of the vapor chamber 1 can be excellent, the adhesion state between the vapor chamber 1 and the member can be good regardless of the member to which the vapor chamber 1 is applied or the arrangement, etc., and the substantial heat transport ability can be more reliably excellent.

[0084] The resin composition may be any composition that contains a curable resin in an uncured state and exhibits adhesive properties through heat treatment after photolithography. It may be a composition in which the curing reaction has progressed to a certain extent (e.g., a B-stage resin), or it may contain a thermoplastic resin in addition to a curable resin in an uncured state.

[0085] In particular, the resin composition preferably contains an alkali-soluble resin, a photopolymerizable resin, and a thermosetting resin different from the alkali-soluble resin.

[0086] This allows a predetermined pattern to be suitably formed in the exposure and development steps, and allows an alkaline aqueous solution with less environmental impact to be suitably used in the development step, instead of an organic solvent that is widely used as a developer. Also, more suitable adhesion can be exhibited, and in the method for producing the vapor chamber 1 described later, the adhesion between the prepreg 100' and the first sheet material 11 in the prepreg application step, and the bonding strength and adhesion between the prepreg 100' and the second protrusion 22 of the second member 20 in the bonding and sealing step can be improved, and the strength and heat resistance of the wick in the vapor chamber 1 can be improved.

[0087] The alkali-soluble resin will now be described. Examples of the alkali-soluble resin include novolak resins such as cresol type, phenol type, bisphenol A type, bisphenol F type, catechol type, resorcinol type, and pyrogallol type; acrylic resins such as phenol aralkyl resins, hydroxystyrene resins, methacrylic acid resins, and methacrylic acid ester resins; cyclic olefin resins containing a hydroxyl group, a carboxyl group, or the like; polyamide resins (specifically, resins having at least one of a polybenzoxazole structure and a polyimide structure and having a hydroxyl group, a carboxyl group, an ether group, or an ester group in the main chain or side chain, resins having a polybenzoxazole precursor structure, resins having a polyimide precursor structure, resins having a polyamic acid ester structure, and the like), phenol-modified silicone resins, and carboxyl-modified silicone resins.

[0088] As the alkali-soluble resin, for example, a resin having an alkali-soluble group and a double bond can be suitably used.

[0089] As a result, when removing resin whose double bond moieties have not reacted in the development step, an alkaline aqueous solution, which has a lower environmental impact, can be used instead of an organic solvent that is normally used as a developer. Furthermore, since the double bond moieties contribute to the curing reaction, the second resin cured product 140 made from the resin composition has particularly excellent heat resistance.

[0090] Examples of the resin having an alkali-soluble group and a double bond include curable resins that can be cured by both light and heat.

[0091] Examples of the alkali-soluble group include a hydroxyl group, a carboxyl group, etc. The alkali-soluble group can also contribute to the thermosetting reaction.

[0092] Examples of such resins include thermosetting resins having a photoreactive group such as an acryloyl group, a methacryloyl group, or a vinyl group, and photocurable resins having a thermally reactive group such as a phenolic hydroxyl group, an alcoholic hydroxyl group, a carboxyl group, or an acid anhydride group. The photocurable resin may further have a thermally reactive group such as an epoxy group, an amino group, or a cyanate group. Specific examples of such resins include (meth)acrylic modified phenolic resins, (meth)acryloyl group-containing acrylic acid polymers, and carboxyl group-containing (epoxy)acrylates.

[0093] Among these, the alkali-soluble resin is preferably one containing a (meth)acrylic group and a phenolic hydroxyl group, or one containing a (meth)acrylic group and a carboxyl group, more preferably one containing a (meth)acrylic group and a phenolic hydroxyl group, and even more preferably a (meth)acrylic-modified phenolic resin.

[0094] This makes it possible to more effectively remove unreacted resin in the development step using an alkaline aqueous solution, thereby improving the productivity and reliability of the vapor chamber 1.

[0095] In particular, when the alkali-soluble resin contains a (meth)acrylic group and a phenolic hydroxyl group, the above-mentioned effects can be obtained, and the resolution of the resin material 140'' in the method for manufacturing a vapor chamber, i.e., the reproducibility of the pattern in the exposure step, can be made more excellent. Such effects are more pronounced when a (meth)acrylic-modified phenolic resin is used among alkali-soluble resins containing a (meth)acrylic group and a phenolic hydroxyl group.

[0096] The (meth)acrylic modified phenolic resin can be obtained, for example, by reacting a phenolic hydroxyl group of a novolac resin such as a phenol novolac resin, a cresol novolac resin, or a bisphenol A novolac resin with a compound having a glycidyl group and a (meth)acrylic group such as glycidyl acrylate or glycidyl methacrylate. Among these, preferred are methacrylic modified phenolic resins obtained by reacting phenol novolac with glycidyl methacrylate and bisphenol A novolac resin with glycidyl methacrylate.

[0097] This makes the above-mentioned effects more pronounced. That is, the unreacted resin can be more suitably removed in the development process using an alkaline aqueous solution, the productivity and reliability of the vapor chamber 1 can be more excellent, and the reproducibility of the pattern in the exposure process can be more excellent. As a result, the method can be more suitably applied to the manufacture of the vapor chamber 1 equipped with a wick having a fine pattern.

[0098] When a thermosetting resin having a photoreactive group is used as the alkali-soluble resin, the modification rate (substitution rate) of the photoreactive group is not particularly limited, but is preferably 20 mol % or more and 80 mol % or less, and more preferably 30 mol % or more and 70 mol % or less, of the total reactive groups of the resin having the alkali-soluble group and the double bond.

[0099] This makes it possible to improve the resolution of the resin composition (resin material 140'') in the method for producing a vapor chamber, that is, the reproducibility of the pattern in the exposure step.

[0100] On the other hand, when a photocurable resin having a thermally reactive group is used, the modification rate (substitution rate) of the thermally reactive group is not particularly limited, but is preferably from 20 mol% to 80 mol%, and more preferably from 30 mol% to 70 mol%, of the total reactive groups of the resin having an alkali-soluble group and a double bond.

[0101] This makes it possible to improve the resolution of the resin composition (resin material 140'') in the method for producing a vapor chamber, i.e., the reproducibility of the pattern in the exposure process. As a result, this method can be more suitably applied to the production of a vapor chamber 1 equipped with a wick having a fine pattern.

[0102] The weight average molecular weight of the resin having an alkali-soluble group and a double bond is not particularly limited, but is preferably 300,000 or less, and more preferably 5,000 or more and 150,000 or less.

[0103] This makes it possible to ensure that the shape of the resin material 140'' in the prepreg 100' is sufficiently stable, while also more suitably removing the uncured resin material 140'' in the development step.

[0104] The weight average molecular weight can be evaluated, for example, by using GPC, and can be calculated from a calibration curve prepared in advance using a styrene standard substance. In particular, the weight average molecular weight can be measured using tetrahydrofuran (THF) as a measurement solvent at a temperature of 40°C.

[0105] The content of the alkali-soluble resin in the resin composition is not particularly limited, but is preferably from 10% by mass to 80% by mass, and more preferably from 15% by mass to 70% by mass.

[0106] This makes it possible to improve the resolution in the exposure step and the developability in the development step while ensuring sufficiently excellent shape stability of the resin material 140'' in the prepreg 100'. Furthermore, the heat treatment in the vapor chamber manufacturing process can improve the bonding strength and adhesion between the prepreg 100' (fiber-containing cured material 100) and the first sheet material 11.

[0107] Next, the photopolymerizable resin will be described. When the resin composition contains a photopolymerizable resin in addition to the alkali-soluble resin, the patterning properties can be improved.

[0108] Examples of photopolymerizable resins include unsaturated polyesters, acrylic compounds such as acrylic monomers and oligomers having at least one acryloyl group or methacryloyl group in one molecule, and vinyl compounds such as styrene. One or a combination of two or more selected from these can be used.

[0109] Among these, ultraviolet-curable resins containing an acrylic compound as a main component are preferred. Acrylic compounds have a high curing rate when irradiated with light (exposure light), and can suitably pattern the resin composition (resin material 140″ in prepreg 100′) with a relatively small amount of exposure light.

[0110] Examples of the acrylic compound include monomers of acrylic acid esters and methacrylic acid esters, and more specifically, bifunctional acrylates such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, glycerin diacrylate, glycerin dimethacrylate, 1,10-decanediol diacrylate, and 1,10-decanediol dimethacrylate, and polyfunctional acrylates such as trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexaacrylate, and dipentaerythritol hexamethacrylate.

[0111] Among these, (meth)acrylic acid esters are preferred, and acrylic acid esters and methacrylic acid alkyl esters having an ester moiety with 1 to 15 carbon atoms are more preferred. This can improve the reactivity and the sensitivity in the exposure step.

[0112] The photopolymerizable resin is not particularly limited, but is preferably liquid at room temperature (23° C.).

[0113] This can improve the curing reactivity with exposure light (especially ultraviolet light). In addition, it can facilitate the mixing with other compounding components (e.g., alkali-soluble resin). Examples of photopolymerizable resins that are liquid at room temperature include the above-mentioned ultraviolet curable resins mainly composed of acrylic compounds.

[0114] The weight average molecular weight of the photopolymerizable resin is not particularly limited, but is preferably 5,000 or less, and more preferably 150 or more and 3,000 or less.

[0115] This can improve the reactivity of the resin composition (resin material 140'' in prepreg 100'), improve the sensitivity in the exposure process, and improve the resolution of the resin composition (resin material 140'' in prepreg 100').

[0116] The content of the photopolymerizable resin in the resin composition is not particularly limited, but is preferably from 9% by mass to 40% by mass, and more preferably from 13% by mass to 30% by mass.

[0117] This makes it possible to achieve a higher level of both heat resistance and flexibility for the second resin cured product 140 formed by curing the resin material 140'' (resin material 140'' which is a resin composition) in the prepreg 100'. Also, the resolution of the resin material 140'' in the vapor chamber manufacturing method, i.e., the reproducibility of the pattern in the exposure step, can be made more excellent. As a result, this method can be more suitably applied to the manufacture of a vapor chamber 1 equipped with a wick having a fine pattern.

[0118] When the content of the alkali-soluble resin in the resin composition is XA [mass%] and the content of the photopolymerizable resin in the resin composition is XP [mass%], it is preferable to satisfy the relationship of 0.15≦XP / XA≦0.90, it is more preferable to satisfy the relationship of 0.19≦XP / XA≦0.87, and it is even more preferable to satisfy the relationship of 0.22≦XP / XA≦0.33.

[0119] This makes it possible to achieve an even better balance between the shape stability of the resin material 140'' in the prepreg 100', the resolution in the exposure process, the developability in the development process, the bonding strength and adhesion between the prepreg 100' (fiber-containing cured material 100) and the first sheet material 11, and the heat resistance and flexibility of the second resin cured material 140 formed by curing the resin material 140''.

[0120] Examples of the thermosetting resin (thermosetting resin different from alkali-soluble resin) include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin; phenolic resins such as resol phenolic resin; bisphenols such as bisphenol F, bisphenol A, 4,4'-ethylidene-bisphenol, 4,4'-cyclohexylidene bisphenol, and 4,4',4''-ethylidine trisphenol; bisphenol-type epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin; novolac epoxy resin; and cresol novolac epoxy resin. Examples of the epoxy resin include novolac epoxy resins such as biphenyl epoxy resins, stilbene epoxy resins, triphenolmethane epoxy resins, alkyl-modified triphenolmethane epoxy resins, triazine nucleus-containing epoxy resins, and dicyclopentadiene-modified phenolic epoxy resins; urea resins, resins having a triazine ring such as melamine resins; unsaturated polyester resins, bismaleimide resins, polyurethane resins, diallyl phthalate resins, silicone resins, resins having a benzoxazine ring, and cyanate ester resins; and one or more selected from these may be used in combination. Among these, epoxy resins and bisphenols are particularly preferred as the thermosetting resin. This can improve the heat resistance of the second resin cured product 140 obtained by curing the resin material 140'' (resin material 140'' which is a resin composition) in the prepreg 100', and the adhesion of the second resin cured product 140 obtained by curing the resin material 140'' to the fibers 131 and the first sheet material 11.

[0121] The content of the thermosetting resin in the resin composition is not particularly limited, but is preferably from 10% by mass to 60% by mass, and more preferably from 15% by mass to 55% by mass.

[0122] This makes it possible to achieve a higher level of both heat resistance and toughness in second cured resin 140 obtained by curing resin material 140'' (resin material 140'' which is a resin composition) in prepreg 100'.

[0123] When the content of the alkali-soluble resin in the resin composition is XA [mass%] and the content of the thermosetting resin in the resin composition is XT [mass%], it is preferable to satisfy the relationship of 0.20≦XT / XA≦1.5, it is more preferable to satisfy the relationship of 0.30≦XT / XA≦1.2, and it is even more preferable to satisfy the relationship of 0.55≦XT / XA≦0.80.

[0124] This makes it possible to achieve an even better balance in the shape stability of resin material 140'' (resin material 140'' which is a resin composition) in prepreg 100', the resolution in the exposure process, the developability in the development process, the heat resistance and toughness of second resin cured material 140 obtained by curing resin material 140'', and the bonding strength and adhesion between prepreg 100' (fiber-containing cured material 100) and first sheet material 11.

[0125] The first protrusion 12 may contain components other than the resin material 140″ (the resin material 140″ which is a resin composition). Examples of such components include a filler, an ultraviolet absorbing agent, a leveling agent, a coupling agent, a flame retardant, and an antioxidant.

[0126] However, the content of components other than the resin material 140'' in the first convex portion 12 (if multiple types of components are contained, the total content of these components) is preferably 10.0 mass% or less, more preferably 7.0 mass% or less, and even more preferably 5.0 mass% or less.

[0127] [1-3] Second protrusion The second protrusions 22 are made of a metal material and are formed on the inner surface of the second sheet material 21 in a predetermined pattern.

[0128] Since the second convex portion 22 is disposed in the hollow portion of the container 2, a flow path for the working fluid 40 can be suitably secured in the hollow portion of the container 2, and the flow of the working fluid 40 in the hollow portion can be effectively prevented from being obstructed due to deformation of the container 2.

[0129] Examples of the metal material constituting the second protrusion 22 include Cu, Al, Mg, Zn, and alloys containing at least one of these metals.

[0130] Among them, the metal material constituting the second protrusion 22 is preferably Cu or a Cu alloy.

[0131] This can further improve the substantial heat transport ability of the vapor chamber 1. Also, the durability of the vapor chamber 1 can be further improved.

[0132] Furthermore, if at least the portion of the second protrusion 22 that comes into contact with the wick 30 is made of Cu or a Cu alloy, the adhesion between the second protrusion 22 and the wick 30, and the durability and reliability of the vapor chamber 1 can be improved.

[0133] The second convex portion 22 and the second sheet material 21 may be made of the same material or different materials, but are preferably made of the same material.

[0134] This makes it possible to improve the bonding strength and adhesion between the second sheet material 21 and the second convex portion 22, and also makes it possible to reduce the thermal resistance at the interface between the second sheet material 21 and the second convex portion 22.

[0135] The formation pattern of the second protrusions 22 is not particularly limited, but in the example shown in the figure, the second protrusions 22 are formed in a cylindrical shape, and when viewed in a plane, the multiple second protrusions 22 are arranged in a staggered pattern.

[0136] The height of the second protrusion 22 is not particularly limited, but is preferably 5 μm or more and 500 μm or less, more preferably 7 μm or more and 400 μm or less, and even more preferably 10 μm or more and 300 μm or less.

[0137] This can more suitably secure the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40) while preventing the vapor chamber 1 from becoming thicker than necessary.

[0138] The width W2 of the second convex portion 22 is not particularly limited, but is preferably 100 μm or more and 10,000 μm or less, more preferably 500 μm or more and 5,000 μm or less, and even more preferably 1,000 μm or more and 3,000 μm or less.

[0139] This can make the flexibility (flexibility) of the vapor chamber 1 particularly excellent while sufficiently preventing unwanted deformation in the thickness direction of the container 2.

[0140] The pitch P2 of the second convex portion 22 is not particularly limited, but is preferably 100 μm or more and 30,000 μm or less, more preferably 500 μm or more and 20,000 μm or less, and even more preferably 1,000 μm or more and 10,000 μm or less.

[0141] This can make the flexibility (flexibility) of the vapor chamber 1 particularly excellent while more suitably securing the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40).

[0142] When the thickness of the second sheet material 21 is T2 [μm] and the interval between the second convex portions 22 is D2 [μm], it is preferable to satisfy the relationship of 10 < D2 < 80.966exp(0.0512T2).

[0143] This can make the flexibility (flexibility) of the vapor chamber 1 particularly excellent while sufficiently preventing unwanted deformation in the thickness direction of the container 2.

[0144] In a plan view of the vapor chamber 1, the total area of the second convex portions 22 is S2 [cm 2 , and the total area of the hollow portion of the container 2 is Sw [cm2 When [condition], it is preferable to satisfy the relationship of 0.03 < S2 / Sw < 0.3, more preferably to satisfy the relationship of 0.04 < S2 / Sw < 0.25, and even more preferably to satisfy the relationship of 0.05 < S2 / Sw < 0.2.

[0145] As a result, while making the flexibility of the vapor chamber 1 particularly excellent, it is possible to more suitably secure the flow path portion of the working fluid 40 (particularly, the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40). In addition, the substantial heat transport capacity as the vapor chamber 1 can be made even more excellent.

[0146] In the vapor chamber 1, the average value of the interval D1 between the first convex portions 12 is preferably smaller than the average value of the interval D2 between the second convex portions 22. In other words, it is preferable to satisfy the relationship of D1 < D2.

[0147] As a result, when a force is applied in the thickness direction of the vapor chamber 1, the second convex portion 22 is supported by the first convex portion 12, so that the deformation of the wick 30, the first sheet material 11, and the second sheet material 21 can be more reliably prevented, and the unintended deformation in the thickness direction of the container 2 can be more reliably prevented. Such an effect is more显著 when the relationship of D1 - D2 < -500 is satisfied.

[0148] Further, in the vapor chamber 1, when the interval between the first convex portions 12 is D1 [μm] and the width of the second convex portions 22 is W2 [μm], it is preferable to satisfy the relationship of W2 > D1, more preferably to satisfy the relationship of W2 - D1 > 50, and even more preferably to satisfy the relationship of W2 - D1 > 100.

[0149] As a result, when a force is applied in the thickness direction of the vapor chamber 1, the second convex portion 22 is supported by the first convex portion 12, so that the deformation of the wick 30, the first sheet material 11, and the second sheet material 21 can be more reliably prevented, and the unintended deformation in the thickness direction of the container 2 can be more reliably prevented.

[0150] In this specification, the interval D1 between the first protrusions 12 refers to the distance between the opposing side surfaces of adjacent first protrusions 12.

[0151] The interval D1 between the first protrusions 12 is not particularly limited, but is preferably 1 μm to 3000 μm, more preferably 5 μm to 2000 μm, and even more preferably 10 μm to 1000 μm. This makes it possible to make the above-mentioned effects more pronounced.

[0152] [1-4] Wick The wick 30 is a component that has the function of preventing deformation of the container 2 in the thickness direction, and is also a component that allows the flow of working fluid 40 associated with heat transport, in particular the flow of working fluid 40 that has been vaporized by receiving heat in the evaporator section of the container 2, and the flow of working fluid 40 that has condensed by receiving heat in the condenser section of the container 2.

[0153] [1-4-1] Fiber In this embodiment, the wick 30 includes fibers 131 .

[0154] The fiber 131 may be made of any material. Examples of the material for the fiber 131 include cotton, linen, wool, polyester resin, polyamide resin, acrylic resin, aromatic resin containing a heterocycle in the molecule, glass, carbon, iron, silver, copper, etc., and one or more types selected from these may be used in combination.

[0155] Among them, when the fiber 131 is a glass fiber, the durability of the vapor chamber 1 can be improved. Furthermore, since glass fiber generally has excellent transparency to light including ultraviolet light, in the manufacturing method of the vapor chamber described in detail later, it is possible to effectively prevent the curing reaction of the resin composition from being unintentionally inhibited in the exposure step, and the productivity and yield of the vapor chamber 1 can be particularly improved. Furthermore, the glass fiber has excellent adhesion to the second resin cured product 140 of the resin composition.

[0156] The thickness of the fibers 131 is not particularly limited, but is preferably 3 μm or more and 20 μm or less, more preferably 3.5 μm or more and 19 μm or less, and even more preferably 4 μm or more and 18 μm or less.

[0157] This prevents the wick 30 from becoming thicker than necessary, while ensuring more suitable gaps between the fibers 131, and improves the transport capacity of the liquid working fluid 40 by capillary action in the vapor chamber 1. As a result, the heat transport capacity of the vapor chamber 1 can be improved.

[0158] In the wick 30, the fibers 131 may be, for example, in a state where a plurality of fibers 131 are bundled together, that is, included as a fiber bundle. Examples of the fiber bundle include a multiple-ply yarn, a single-ply yarn, a lange-ply yarn, a braided cord, and the like.

[0159] This prevents the wick 30 from becoming thicker than necessary, while ensuring more suitable gaps between the fibers 131, and improves the transport capacity of the liquid working fluid 40 by capillary action in the vapor chamber 1. As a result, the heat transport capacity of the vapor chamber 1 can be improved.

[0160] In the illustrated configuration, the fibers 131 form a sheet-like fiber base material (fiber sheet) 130.

[0161] In particular, the wick 30 preferably includes a fiber substrate (fiber sheet) 130 made of glass fiber.

[0162] As a result, for example, the wick 30 can include the fiber base material 130 in a state in which the fibers 131 are not only contained in an independent state, but also in which a plurality of fibers 131 are entangled, and for example, the gaps between the fibers 131 in the wick can be easily adjusted to a state in which the liquid working liquid 40 is likely to generate capillary action, and the arrangement portion of the fibers 131 in the wick can be easily adjusted. Therefore, the flow path portion of the gaseous working liquid 40 and the flow path portion of the liquid working liquid 40 can be more preferably coexisted, and the above-mentioned effect can be more reliably achieved. In addition, the wick can be easily manufactured, and the arrangement and distribution of the fibers 131 in the wick can be easily adjusted, and for example, unintended uneven distribution of the fibers 131 in each portion of the wick (for example, the fibers 131 are not sufficiently present in the portion that should be the flow path portion, etc.) can be preferably prevented. Furthermore, since the fiber base material 130 is in sheet form, it is possible to effectively prevent the wick 30 from becoming unnecessarily thick, and it is also possible to more effectively prevent unintended deformation of the fiber base material 130 during the manufacture of the vapor chamber and unintended movement of the fibers 131 within the wick 30.

[0163] The fiber substrate 130 may be, for example, a nonwoven fabric or a woven fabric. When the fiber base material 130 is a woven fabric, examples of the woven fabric include plain weave, twill weave, satin weave, leno weave, mock weave, twill weave, double weave, and the like.

[0164] The thickness of the fiber base material 130 is preferably 10 μm or more and 1000 μm or less, more preferably 15 μm or more and 500 μm or less, and even more preferably 20 μm or more and 200 μm or less.

[0165] This prevents the wick 30 from becoming thicker than necessary, while ensuring more suitable gaps between the fibers 131, and further improves the transport capacity of the liquid working fluid 40 by capillary action in the vapor chamber 1. As a result, the heat transport capacity of the vapor chamber 1 can be further improved.

[0166] The fiber base material 130 may have a portion having a different fiber density. For example, the fiber base material 130 may have a portion having a different fiber density in the thickness direction.

[0167] The wick 30 may include a plurality of fiber substrates 130. In this case, these fiber substrates 130 may be of the same condition or may be of different conditions. When the wick 30 includes a plurality of fiber substrates 130, the plurality of fiber substrates 130 may be stacked in the thickness direction of the wick 30, for example.

[0168] The wick 30 may include a fiber substrate 130 , or may further include fibers 131 independent of the fiber substrate 130 .

[0169] The thickness of the wick 30 is preferably 10 μm or more and 1000 μm or less, more preferably 15 μm or more and 500 μm or less, and even more preferably 20 μm or more and 200 μm or less.

[0170] This prevents the vapor chamber 1 from becoming thicker than necessary, while improving the transport ability of the liquid working fluid 40 by capillary action in the vapor chamber 1. As a result, the heat transport ability of the vapor chamber 1 can be improved.

[0171] [1-5] Hydraulic fluid The working fluid 40 mainly has a function of transporting heat in the cavity of the container 2 .

[0172] Examples of the working fluid 40 include water, hydrochlorofluorocarbons such as HCFC-22, hydrofluorocarbons such as HFCR134a, HFCR407C, HFCR410A, and HFC32, hydrofluoroolefins such as HFO1234yf, hydrofluoroethers, alcohols such as ethanol and methanol, acetone, carbon dioxide gas, ammonia, and propane.

[0173] [1-6] Overall configuration of the vapor chamber The thickness of the vapor chamber 1 is preferably 100 μm or more and 3000 μm or less, more preferably 130 μm or more and 2000 μm or less, and even more preferably 150 μm or more and 1000 μm or less.

[0174] This allows the working fluid 40 (gaseous working fluid 40 and liquid working fluid 40) to move more smoothly while preventing the vapor chamber 1 from becoming thick. As a result, the heat transport capacity of the vapor chamber 1 can be made particularly excellent. In addition, the durability of the vapor chamber 1 can be made even more excellent.

[0175] In particular, when the thickness of the vapor chamber 1 is relatively thin (for example, when the thickness of the vapor chamber 1 is 50 μm or more and less than 500 μm), better flexibility (pliability) is exhibited, and when the thickness of the vapor chamber 1 is relatively thick (for example, when the thickness of the vapor chamber 1 is 500 μm or more and 2100 μm or less), the three-dimensional formability of the vapor chamber 1 can be made better.

[0176] [2] How to manufacture a vapor chamber Next, a method for manufacturing the vapor chamber will be described.

[0177] The vapor chamber as described above can be suitably manufactured, for example, by the method described below.

[0178] 2 to 4 are perspective views each showing a typical example of a method for producing a vapor chamber, and Fig. 5 is a perspective view each showing a typical example of a prepreg used in the method for producing a vapor chamber.

[0179] In this embodiment, the method for manufacturing the vapor chamber 1 includes, for example, a prepreg application process (1a) of applying a prepreg 100' containing an uncured resin material 140'' onto a first metal sheet material 11, an exposure process (1b) of irradiating the prepreg 100' with light E in a predetermined pattern, a development process (1c) of removing the uncured resin material 140'' from the prepreg 100' that was not exposed in the exposure process and developing a pattern having a plurality of first protrusions 12 made of the resin material 140'', a heat curing process (1d) of heat curing the resin material 140'' remaining in the development process, and a heat curing process (1e) of the prepreg 100' that has been subjected to the heat curing process. The method includes processing steps (1e, 1f) of removing a portion, a bonding material application step (1g) of applying a bonding material to the area on the first sheet material 11 from which the prepreg 100' has been removed in the processing step, and a joining and sealing step (1h, 1i) of joining, via an Sn-containing alloy, a second member 20 having a second metal sheet material 21 and a plurality of second metal protrusions 22 on the surface opposite to the surface on which the first sheet material 11 of the first member 10 obtained through a series of steps including at least the prepreg application step or the bonding material application step is provided, and injecting a working fluid 40 into the space between the first sheet material 11 and the second sheet material 21 to seal it.

[0180] This makes it possible to manufacture a highly reliable vapor chamber 1 that has excellent flexibility, durability, and heat transport capacity. In addition, because the vapor chamber 1 has excellent flexibility, the vapor chamber 1 can be in good contact with the member to which it is applied, regardless of the member or arrangement, etc., and the vapor chamber 1 can reliably exhibit excellent heat transport capacity.

[0181] In addition, in the method of this embodiment, the vapor chamber can be manufactured by photolithography (exposure process and development process) and bonding via an Sn-containing alloy (bonding and sealing process). In other words, in the method of this embodiment, the vapor chamber can be manufactured at a relatively low temperature without using laser processing. This does not require high energy, so that it is possible to reduce the amount of CO2 emissions and reduce the environmental load. In addition, since no laser is irradiated, it is possible to prevent unintended deterioration of the material constituting the vapor chamber due to heat. Furthermore, a resin material can be used as the material constituting the first protrusion 12, and the options for the material constituting the vapor chamber can be expanded.

[0182] [2-1] Prepreg application process In the prepreg application step, a prepreg 100' containing an uncured resin material 140'' is applied onto a first sheet material 11 (1a).

[0183] [2-1-1] Prepreg In the following description, the prepreg used in the method for manufacturing the vapor chamber of this embodiment will be described. FIG. 5 is a perspective view that illustrates an example of a prepreg.

[0184] The prepreg 100 ′ includes an uncured resin material 140 ″ and fibers 131 . In particular, in the illustrated configuration, the prepreg 100 ′ includes a fiber base material 130 made of fibers 131 and an uncured resin material 140 ″ that impregnates the fiber base material 130 .

[0185] In the illustrated configuration, the fiber base material 130 is in the form of a sheet, but the shape of the fiber base material 130 is not particularly limited.

[0186] In the illustrated configuration, the prepreg 100' is in a sheet shape, and in particular has a shape corresponding to the sheet-shaped fiber base material 130, but the shape of the prepreg 100' is not particularly limited.

[0187] [2-1-1―1] Resin materials The prepreg 100' includes the resin composition described above as the uncured resin material 140''.

[0188] The content of the resin material 140'' in the prepreg 100' is preferably 10% by mass to 95% by mass, more preferably 15% by mass to 90% by mass, and even more preferably 20% by mass to 85% by mass.

[0189] In particular, when the fibers 131 are composed of an inorganic material, the content of the resin material 140'' in the prepreg 100' is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or less, and even more preferably 20% by mass or more and 40% by mass or less.

[0190] Furthermore, when the fibers 131 are made of an organic material, the content of the resin material 140'' in the prepreg 100' is preferably 50% by mass or more and 95% by mass or less, more preferably 55% by mass or more and 90% by mass or less, and even more preferably 60% by mass or more and 85% by mass or less.

[0191] By satisfying the above content conditions, the ratio between the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40 in the vapor chamber 1 manufactured using the prepreg 100' can be made more suitable.

[0192] [2-1-1-2] Fiber The prepreg 100 ′ includes fibers 131 . The fibers 131 contained in the prepreg 100 ′ preferably satisfy the same conditions as those of the fibers 131 described above as the constituent material of the wick 30 . This provides the same effect as described above.

[0193] The content of the fibers 131 in the prepreg 100' is preferably 1% by mass to 80% by mass, more preferably 3% by mass to 75% by mass, and even more preferably 5% by mass to 70% by mass.

[0194] In particular, when the fibers 131 are made of an inorganic material, the content of the fibers 131 in the prepreg 100' is preferably 40% by mass or more and 80% by mass or less, more preferably 45% by mass or more and 75% by mass or less, and even more preferably 50% by mass or more and 70% by mass or less.

[0195] Furthermore, when the fibers 131 are made of an organic material, the content of the fibers 131 in the prepreg 100' is preferably 1% by mass or more and 40% by mass or less, more preferably 3% by mass or more and 35% by mass or less, and even more preferably 5% by mass or more and 30% by mass or less.

[0196] By satisfying the above content conditions, the ratio between the flow path portion of the gaseous working liquid 40 and the flow path portion of the liquid working liquid 40 in the manufactured vapor chamber 1 (wick) can be made more suitable.

[0197] When the content of fiber 131 in prepreg 100' is Xf [mass %] and the content of resin material 140'' is Xr [mass %], it is preferable to satisfy the relationship of 0.01≦Xf / Xr≦8.0, it is more preferable to satisfy the relationship of 0.1≦Xf / Xr≦5.0, and it is even more preferable to satisfy the relationship of 0.3≦Xf / Xr≦3.0.

[0198] In particular, when the fibers 131 are made of an inorganic material, it is preferable that the relationship satisfies 0.8≦Xf / Xr≦8.0, it is more preferable that the relationship satisfies 1.0≦Xf / Xr≦7.0, and it is even more preferable that the relationship satisfies 2.0≦Xf / Xr≦6.0.

[0199] Furthermore, when the fibers 131 are made of an organic material, it is preferable that the relationship satisfies 0.01≦Xf / Xr≦0.8, it is more preferable that the relationship satisfies 0.05≦Xf / Xr≦0.6, and it is even more preferable that the relationship satisfies 0.10≦Xf / Xr≦0.4.

[0200] By satisfying the above-mentioned content relationship, the ratio between the flow path portion of the gaseous working fluid 40 and the flow path portion of the liquid working fluid 40 in the vapor chamber 1 manufactured using the prepreg 100' can be made more suitable.

[0201] [2-1-1-3] Hardener (photosensitive agent) The prepreg 100' may further include a curing agent.

[0202] The curing agent (photosensitive agent) is not particularly limited as long as it cures the resin material 140'', and examples thereof include benzophenone, acetophenone, benzoin, benzoin isobutyl ether, benzoin methyl benzoate, benzoin benzoic acid, benzoin methyl ether, benzyl phenyl sulfide, benzyl, dibenzyl, diacetyl, etc., and one or more selected from these may be used in combination.

[0203] The content of the curing agent (photosensitizer) in the prepreg 100' is not particularly limited, but is preferably from 0.1% by mass to 50% by mass, more preferably from 0.5% by mass to 40% by mass, and even more preferably from 1.0% by mass to 30% by mass.

[0204] This makes it possible to ensure that the storage stability of the prepreg 100' is sufficiently excellent, while at the same time allowing the photopolymerization reaction to be more suitably initiated and progressed during the manufacture of the vapor chamber.

[0205] [2-1-1-4] Thermosetting resin curing catalyst The prepreg 100' may further contain a curing catalyst for the thermosetting resin.

[0206] The curing catalyst for the thermosetting resin is not particularly limited as long as it catalyzes the curing reaction of the thermosetting resin constituting the resin material 140″. For example, tertiary amines such as triethylamine, tributylamine, and diazabicyclo[2,2,2]octane, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2-ethyl-4-ethylimidazole, 2-phenyl ... and imidazoles such as 2-phenyl-4-methyl-5-hydroxyimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxyimidazole, 1-benzyl-2-phenylimidazole, 2-phenyl-1H-imidazole-4,5-dimethanol, and 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole. One or more selected from these may be used in combination.

[0207] The content of the curing catalyst for the thermosetting resin in the prepreg 100' is not particularly limited, but is preferably from 0.01% by mass to 10% by mass, more preferably from 0.04% by mass to 5.0% by mass, and even more preferably from 0.1% by mass to 3.0% by mass.

[0208] This allows the storage stability of the prepreg 100' to be sufficiently excellent, while allowing the thermosetting reaction to be more suitably initiated and progressed during the manufacture of the vapor chamber.

[0209] [2-1-1-5] Other ingredients The prepreg 100' may contain components other than the above-mentioned components (hereinafter, also referred to as "other components"). Examples of such components include fillers, ultraviolet absorbers, leveling agents, coupling agents, flame retardants, antioxidants, etc., and one or more selected from these may be used in combination.

[0210] However, the content of other components in the prepreg 100' is preferably 7.0% by mass or less, more preferably 5.0% by mass or less, and even more preferably 3.0% by mass or less.

[0211] [2-1-1-6] Overall structure of prepreg 100' The shape of the prepreg 100' is not particularly limited, but in the illustrated configuration, it is in a sheet form.

[0212] This makes it possible to suitably manufacture a sheet-shaped vapor chamber (wick). Also, it is possible to more suitably prevent unintended deformation of the prepreg 100' during manufacture of the vapor chamber and unintended movement of the fibers 131 in the prepreg 100'.

[0213] In this embodiment, the prepreg 100' is in a sheet shape, and the sheet-like fiber base material 130 (fibers 131) is preferably unevenly distributed on one surface side of the prepreg 100' as shown in Fig. 5. In the example shown in the figure, the fiber base material 130 is unevenly distributed on the second surface 102 side of the prepreg 100'.

[0214] This makes it possible to suitably form the first protrusions 12 and the wick 30 made of the second cured resin 140.

[0215] The fiber base material 130 (fibers 131) may be present throughout almost the entire thickness of the prepreg 100', or may be concentrated near the center of the thickness of the prepreg 100'. Alternatively, the sheet-like fiber base material 130 (fibers 131) may be concentrated on both sides of the prepreg 100', and the content of fibers 131 near the center of the thickness of the prepreg 100' may be lower than in these areas.

[0216] The thickness of the prepreg 100' is preferably 10 μm or more and 2000 μm or less, more preferably 20 μm or more and 1000 μm or less, and even more preferably 30 μm or more and 500 μm or less.

[0217] This makes it possible to more suitably form the flow path portion for the gaseous working fluid 40 and the flow path portion for the liquid working fluid 40 while preventing the vapor chamber 1 manufactured using the prepreg 100' from becoming unnecessarily thick.

[0218] In a later joining and sealing process, the prepreg 100 ′ is joined to a first sheet material 11 on one of its surfaces, that is, a first surface 101 .

[0219] In other words, the prepreg 100' is bonded to the first sheet material 11 in the subsequent bonding and sealing process so that the sheet-like fiber base material 130 that is biased toward the other surface, the second surface 102, is on the side farther from the first sheet material 11.

[0220] A protective mask 50 may be placed on the prepreg 100 ′ applied onto the first sheet material 11 .

[0221] This makes it possible to effectively prevent unintended deformation of the prepreg 100' during the subsequent exposure and development steps.

[0222] For example, a thin plate made of a light-transmitting resin material can be used as the protective mask 50. Since the protective mask 50 is peeled off from the prepreg 100′ after the exposure step, it is preferable that the protective mask 50 has excellent releasability.

[0223] An example of the resin material that constitutes the protective mask 50 is polyethylene terephthalate (PET).

[0224] [2-2] Exposure process In the exposure step, the prepreg 100' bonded to the first sheet material 11 is irradiated with light E in a predetermined pattern (1b).

[0225] In the exposure process, it is preferable to perform exposure so that the pattern made of the first resin cured product 140' formed in the development process has a plurality of first convex portions 12 and a frame portion 13 surrounding these.

[0226] As a result, the portions of the resin material 140'' irradiated with the light E are selectively cured to become a first cured resin material 140'. That is, in a pattern corresponding to the irradiation pattern of the light E, the portions corresponding to the portions that are to become the first protrusions 12 and the portions corresponding to the portions that are to become the frame portions 13 that surround these can be formed as portions made of the first cured resin material 140'. In particular, by providing the frame portions 13 that surround the first protrusions 12, it is possible to more effectively prevent defects such as deformation and breakage from occurring in the first protrusions 12 in the subsequent processing steps, and to perform the processing steps with excellent workability.

[0227] The curing reaction in this step is allowed to proceed to an extent that the uncured resin material 140'' can be removed in a subsequent developing step while leaving the first cured resin material 140', but is not allowed to proceed completely. In other words, after the curing reaction in this step, the curing reaction of the first cured resin material 140' is allowed to proceed in a thermal curing step to form the second cured resin material 140.

[0228] The type of light E irradiated in this step is determined according to the type of resin material 140'', but is preferably ultraviolet light.

[0229] This allows the resin material 140'' to be cured suitably with a relatively short exposure process, and the productivity of the vapor chamber 1 can be improved.

[0230] The exposure step may be carried out, for example, by scanning the light E in a predetermined pattern, but can be suitably carried out by using a photomask 51 .

[0231] Photomask 51 is formed in a film shape using a material containing a resin material such as polyethylene terephthalate (PET), and when photomask 51 is viewed in a plane, transmitting portions 51a and shielding portions 51b are formed in a predetermined pattern. The pattern of transmitting portions 51a and shielding portions 51b is set according to the pattern to be formed, in other words, the planar shape of a plurality of first protrusions 12 and frame portion 13 surrounding them.

[0232] The pattern of the photomask 51 is not particularly limited, but in the example shown in the figure, the photomask 51 has a pattern in which a plurality of circular parts arranged in a staggered pattern and a frame-shaped part surrounding them are made to be the transmission parts 51a, and the other parts are made to be the shielding parts 51b when viewed from above. With this configuration, a plurality of columnar (particularly, cylindrical) first protrusions 12 and the frame part 13 surrounding them can be suitably formed in a later process. The pattern of the photomask 51 may be, for example, a pattern in which a plurality of circular parts as the transmission parts 51a are arranged in a lattice pattern. Also, the pattern of the photomask 51 may have, for example, a portion having a longitudinal shape as the transmission parts 51a corresponding to the first protrusions 12. This allows the wall-shaped first protrusions 12 to be suitably formed in a later process.

[0233] The photomask 51 may be formed integrally with the protective mask 50 .

[0234] [2-3]Developing process In the development process, the uncured resin material 140'' in the prepreg 100' that was not irradiated with light E in the exposure process is removed, and a pattern having multiple first protrusions 12 made of the first cured resin 140' is developed (1c).

[0235] This makes it possible to remove the resin material 140'' while leaving behind the first cured resin product 140' and the fibers 131. As a result, a predetermined pattern, i.e., a pattern made of the first cured resin product 140' formed in accordance with the irradiation pattern of the light E, appears as a plurality of first protrusions 12 and areas that will become the frame portion 13 surrounding these.

[0236] The developing step can be suitably carried out by using a developer that selectively dissolves the resin material 140'' and does not dissolve the first cured resin material 140'.

[0237] The composition of the developer varies depending on the resin material 140″, the first resin cured product 140′, etc., but for example, when the resin material 140″ contains an alkali-soluble resin as described above, an alkaline aqueous solution of sodium hydroxide, tetramethylammonium hydroxide, etc. can be suitably used.

[0238] [2-4] Heat curing process In the thermal curing process, the first cured resin 140 ′ remaining in the developing process is thermally cured to form the second cured resin 140 .

[0239] As a result, a plurality of first protrusions 12 and a frame portion 13 surrounding these are formed, each of which is made of the second cured resin 140 (1d).

[0240] The heating temperature in the thermal curing step is preferably 80°C or higher and 250°C or lower, more preferably 90°C or higher and 220°C or lower, and even more preferably 100°C or higher and 200°C or lower.

[0241] The heating time in the thermal curing step is preferably from 0.1 to 600 minutes.

[0242] This makes it possible to more effectively prevent undesired deterioration of the constituent materials of the vapor chamber 1 due to heat, while more significantly exhibiting the effects described above. In addition, the productivity of the vapor chamber 1 can be improved.

[0243] [2-5] Processing process In the processing step, a part of the fiber-containing cured material 100, which is the prepreg 100' that has been subjected to the heat curing step, is removed (1e, 1f).

[0244] The processing step is preferably performed with a protective mask 52 placed on the fiber-containing cured material 100, which is the prepreg 100' that has been subjected to the thermal curing step, and then a portion of the protective mask 52 is removed together with a portion of the fiber-containing cured material 100.

[0245] This makes it possible to suitably suppress unintended deformation of the fiber-containing cured material 100 when removing the fiber-containing cured material 100, particularly when processing the outer periphery of the fiber-containing cured material 100.

[0246] The protective mask 52 may be, for example, a thin plate made of a material containing polyethylene terephthalate (PET).

[0247] This makes it possible to more suitably suppress unintended deformation of the fiber-containing cured material 100 when removing the fiber-containing cured material 100, particularly when processing the outer periphery of the fiber-containing cured material 100.

[0248] The processing step is preferably carried out in a state where the fiber-containing cured material 100 and the protective mask 52 are pressed in the layering direction.

[0249] This makes it possible to prevent the fiber-containing cured product 100 from being misaligned with the protective mask 52, and also makes it possible to more suitably prevent unintended deformation of the fiber-containing cured product 100.

[0250] The pressure applied when pressing the protective mask 52 placed on the fiber-containing cured material 100 is not particularly limited, but it is preferable to apply a pressure that does not cause the fiber-containing cured material 100 to deform in the thickness direction, in other words, in the stacking direction of the fiber-containing cured material 100 and the protective mask 52.

[0251] This makes it possible to effectively prevent unintended deformation of the fiber-containing cured material 100 and to make the above-mentioned effects more pronounced.

[0252] In the processing step, it is preferable to remove the fiber-containing cured material 100, which is the prepreg 100' that has been subjected to the thermal curing step, so that a part of the frame 13 and the plurality of first protrusions 12 remain.

[0253] In the processing step, by not removing the entire frame portion 13 but leaving a part of the frame portion 13 surrounding the multiple first protrusions 12, when the bonding material is applied to the area on the first sheet material 11 from which the fiber-containing cured material 100 has been removed in the subsequent bonding material application step, the remaining frame portion 13 acts as a protective wall, which preferably prevents the bonding material from being inadvertently applied into the gaps between the multiple first protrusions 12.

[0254] [2-6] Bonding material application process In the bonding material application step, a bonding material is applied (1g) to the area on the first sheet material 11 from which the fiber-containing cured material 100 has been removed in the processing step.

[0255] In this embodiment, a bonding material is applied onto the first sheet material 11 so as to surround the multiple first protrusions 12. In particular, in the illustrated configuration, a metal plating layer 14 and a layer 15 made of a material containing an Sn-containing alloy are formed as the portion made of the bonding material. In other words, in this embodiment, the first member 10 to be subjected to the subsequent bonding and sealing process is obtained as a member having a layer 15 made of a material containing an Sn-containing alloy provided on the metal plating layer 14.

[0256] This makes it possible to more suitably join the first member 10 and the second member 20 and more suitably seal in the hydraulic fluid 40 in the joining and sealing step described below.

[0257] The metal plating layer 14 can be formed by, for example, electrolytic plating. In the bonding material application step, it is preferable to form the metal plating layer 14 that is thicker than the thickness of the prepreg 100' (fiber-containing cured material 100).

[0258] This makes it possible to more suitably join the first member 10 and the second member 20 and more suitably seal the working fluid 40 in the joining and sealing step described below. In particular, the second protrusions 22 of the second member 20 are not pressed excessively against the fiber-containing cured material 100, and the contact state between the second protrusions 22 and the fiber-containing cured material 100 can be made more favorable.

[0259] The difference between the thickness of the metal plating layer 14 and the thickness of the fiber-containing cured material 100 is preferably 5 μm or more and 500 μm or less, more preferably 7 μm or more and 400 μm or less, and even more preferably 10 μm or more and 300 μm or less. This makes the above-mentioned effects even more pronounced.

[0260] The thickness of the metal plating layer 14 is not particularly limited, but is preferably 30 μm or more and 2500 μm or less, more preferably 40 μm or more and 1500 μm or less, and even more preferably 50 μm or more and 500 μm or less.

[0261] The metal plating layer 14 is preferably formed with a protective mask 52 placed on the fiber-containing cured material 100 .

[0262] This makes it possible to effectively prevent the unintended formation of a metal plating layer 14 on the fiber-containing cured material 100 or inside the fiber-containing cured material 100 (particularly, in the spaces between the fibers 131 and the spaces between the first convex portions 12 formed of the second resin cured material 140), and makes it possible to form the metal plating layer 14 with high selectivity in the desired locations.

[0263] In this embodiment, a layer 15 made of a material containing an Sn-containing alloy is further formed on the metal plating layer 14.

[0264] At this time, it is preferable to form the layer 15 made of the material containing the Sn-containing alloy while the protective mask 52 remains in place on the fiber-containing cured material 100 .

[0265] Examples of Sn-containing alloys include lead-free solders containing Sn as a main component, as explained in [1-1-3-2] above.

[0266] The layer 15 made of a material containing an Sn-containing alloy can be formed on the metal plating layer 14 by, for example, a coating method, a printing method, or the like.

[0267] At this time, the layer 15 made of the material containing an Sn-containing alloy is formed so that the upper surface of the layer 15 made of the material containing an Sn-containing alloy is higher than the upper surface of the fiber-containing cured material 100.

[0268] This makes it possible to more suitably join the first member 10 and the second member 20 and more suitably seal the working fluid 40 in the joining and sealing step described below. In particular, the second protrusions 22 of the second member 20 are not pressed excessively against the fiber-containing cured material 100, and the contact state between the second protrusions 22 and the fiber-containing cured material 100 can be made more favorable.

[0269] The thickness of the layer 15 made of a material containing an Sn-containing alloy is not particularly limited, but is preferably 0.1 μm or more and 100 μm or less, more preferably 0.5 μm or more and 75 μm or less, and even more preferably 1 μm or more and 50 μm or less. This makes the above-mentioned effects more pronounced.

[0270] After the layer 15 made of the material containing an Sn-containing alloy is formed on the metal plating layer 14, the protective mask 52 placed on the fiber-containing cured material 100 is removed.

[0271] This makes it possible to suitably prevent the metal plating layer 14 or the layer 15 made of a material containing an Sn-containing alloy from being unintentionally formed on the fiber-containing cured material 100 .

[0272] As a result of the above, a first member 10 is produced, which has a first sheet material 11, a plurality of first protrusions 12 formed on the first sheet material 11 and made of the second resin cured material 140, a fiber-containing cured material 100, and a bonding material applied onto the first sheet material 11.

[0273] In the first component 10, the portion of the uncured resin material 140'' contained in the prepreg 100' that has been cured through the exposure process, development process, and heat curing process (second cured resin 140) becomes the first convex portion 12. The uncured resin material 140'' in the prepreg 100' is removed in the development process, and the remaining portion of the fiber base material 130 becomes the wick 30 in the vapor chamber 1 to be manufactured.

[0274] [2-7]Joining / sealing process In the joining and sealing process, the first component 10 obtained through a series of processes including at least the prepreg application process or the bonding material application process is joined to the second component 20 having the second sheet material 21 via an Sn-containing alloy on the side opposite to the side on which the first sheet material 11 is provided, and the working fluid 40 is injected into the space between the first sheet material 11 and the second sheet material 21 to seal it (1h, 1i).

[0275] This makes it possible to suitably join the first member 10 and the second member 20 in the joining and sealing step and suitably seal in the hydraulic fluid 40. In other words, it is possible to suitably join the first member 10 and the second member 20 without using laser welding and at a lower temperature than that of laser welding, and to suitably seal in the hydraulic fluid 40.

[0276] [2-7-1] Second component The second member that is joined to the first member in the joining and sealing step will be described below.

[0277] The second member 20 has a second sheet material 21 and a plurality of second protrusions 22 made of metal provided on the second sheet material 21.

[0278] The second protrusions 22 are formed in a predetermined pattern on the side of the second sheet material 21 that comes into contact with the first member 10.

[0279] The method for forming such a second protrusion 22 is not particularly limited, but examples include a method of preparing a metal plate and integrally forming the second sheet material 21 and the second protrusion 22 by etching, and a method of forming the second protrusion 22 on the second sheet material 21 by partial plating.

[0280] In particular, in the manufacturing method of the vapor chamber of this embodiment, by forming a plurality of first protrusions 12 made of resin on the first member 10 and forming a plurality of second protrusions 22 made of a metal material on the second member 20, it is possible to more effectively reduce the amount of carbon dioxide emissions during the manufacturing of the vapor chamber.

[0281] [2-7-1-1] A layer composed of a material containing an Sn-containing alloy In this embodiment, the second member 20 is provided with a layer 23 made of a material including an Sn-containing alloy.

[0282] This makes it possible to more suitably join the first member 10 and the second member 20 and more suitably seal in the hydraulic fluid 40 in the joining and sealing step described below.

[0283] In this embodiment, a layer 23 made of a material containing an Sn-containing alloy is formed on a second sheet material 21 so as to surround a plurality of second protrusions 22.

[0284] This makes it possible to more suitably join the first member 10 and the second member 20 in the joining and sealing step, and to more suitably seal in the hydraulic fluid 40.

[0285] In particular, it is preferable that layer 23 be provided in a portion corresponding to metal plating layer 14 and layer 15 of first member 10 (a portion in contact with layer 15) when first member 10 and second member 20 are joined in a subsequent joining and sealing process. This ensures that the above-mentioned effects are achieved more reliably.

[0286] In particular, since the first component 10 has a layer 15 made of a material containing an Sn-containing alloy on the metal plating layer 14, and the second component 20 has a layer 23 made of a material containing an Sn-containing alloy (at a portion that comes into contact with layer 15 in the joining and sealing process described below), the effects described above act synergistically to obtain better results.

[0287] An example of an alloy containing Sn is a lead-free solder containing Sn as a main component, as described above in [1-1-3-2].

[0288] The Sn-containing alloy applied to the first component 10 and the Sn-containing alloy applied to the second component 20 may be made of different materials, but are preferably made of the same material.

[0289] This makes it possible to improve the bonding strength and adhesion between the first member 10 and the second member 20 via the Sn-containing alloy, and also to reduce the thermal resistance at the bonding interface between the first member 10 and the second member 20.

[0290] The layer 23 made of a material containing an Sn-containing alloy can be formed on the second sheet material 21 by, for example, a coating method, a printing method, or the like.

[0291] The thickness of the layer 23 made of a material containing an Sn-containing alloy is not particularly limited, but is preferably 0.1 μm or more and 100 μm or less, more preferably 0.5 μm or more and 75 μm or less, and even more preferably 1 μm or more and 50 μm or less.

[0292] This makes it possible to improve the bonding strength and adhesion between the first member 10 and the second member 20 in the bonding and sealing process.

[0293] In the joining and sealing process, a first member 10 formed with a layer 15 made of a material containing an Sn-containing alloy and a second member 20 formed with a layer 23 made of a material containing an Sn-containing alloy are opposed to each other, bonded together, and heated, so that the Sn-containing alloy can be heated (reflowed) and joined.

[0294] At this time, not all of the sites where the Sn-containing alloy is applied are joined, and a part is left without being joined as an injection portion for the working fluid 40. This injection portion is sealed after the injection of the working fluid 40.

[0295] The heating temperature of the Sn-containing alloy in the joining and sealing process is not particularly limited, but it is preferably a temperature lower than the thermal decomposition temperature of the second cured resin 140. For example, it can be 200°C or higher and 280°C or lower.

[0296] The injection of the working fluid 40 can be preferably performed, for example, in a state where the interior of the container 2, that is, the space between the first sheet material 11 and the second sheet material 21, is depressurized by evacuation.

[0297] By depressurizing the space between the first sheet material 11 and the second sheet material 21, the boiling point of the working fluid 40 can be lowered, and the cycle of evaporation and condensation of the working fluid 40 can be performed more efficiently. Therefore, the heat transfer effect and the heat equalization effect can be further enhanced.

[0298] At this time, for example, when the average value (average pitch) of the pitch P1 between the first convex portions 12 is smaller than the average value (average pitch) of the pitch P2 between the second convex portions 22, that is, when the relationship P1 < P2 is satisfied, when the interior of the container 2 is depressurized, the second convex portions 22 are supported by the first convex portions 12. Therefore, deformation of the wick 30, the first sheet material 11, and the second sheet material 21 can be more reliably prevented, and unintended deformation in the thickness direction of the container 2 can be more reliably prevented. Such an effect is more显著 when the relationship P1 - P2 < -500 is satisfied.

[0299] Furthermore, for example, when the interval between the first protrusions 12 is D1 [μm] and the width of the second protrusions 22 is W2 [μm], by satisfying the relationship W2>D1, when the pressure inside the container 2 is reduced, the second protrusions 22 are supported by the first protrusions 12, which more reliably prevents deformation of the wick 30, the first sheet material 11, and the second sheet material 21, and more reliably prevents unintended deformation in the thickness direction of the container 2. This effect is more pronounced when the relationship W2-D1>50 is satisfied, and even more pronounced when the relationship W2-D1>100 is satisfied.

[0300] After the hydraulic fluid 40 is injected, the injection portion for the hydraulic fluid 40 is sealed, and the space containing the hydraulic fluid 40 is sealed liquid-tight and air-tight.

[0301] In the above explanation, the joining and sealing process has been mainly described as being performed by first applying an Sn-containing alloy to both the first member 10 and the second member 20, then placing them opposite each other and bonding and sealing them by heating (reflow). However, for example, the Sn-containing alloy may be applied to only one of the first member 10 and the second member 20 to bond and seal them, or the Sn-containing alloy may not be applied to the first member 10 and the second member 20, and the first member 10 and the second member 20 may be bonded and sealed by sandwiching an Sn-containing alloy between them.

[0302] [3] How to use the vapor chamber Next, examples of usage of the vapor chamber of the present invention will be described.

[0303] The vapor chamber may be used, for example, for the purpose of transferring heat from a heat-generating component to a specified location, or for the purpose of equalizing the heat of a localized high-temperature portion of the heat-generating component.

[0304] The following description will focus on the case where the vapor chamber is used for the purpose of transferring heat from a specific component (heat-generating component).

[0305] When used for the purpose of cooling a heat-generating component (such as a CPU), the vapor chamber is used with part of its surface (the evaporation part) in contact with the heat-generating component itself or with a component made of a highly thermally conductive material (such as a thermally conductive sheet) that is in contact with the heat-generating component itself.

[0306] The side of the vapor chamber that comes into contact with a high-temperature component such as a heat-generating component requires a higher thermal conductivity, as well as conformability to the shape of the component to which the vapor chamber 1 is applied and adhesion thereto.

[0307] Therefore, the vapor chamber 1 of this embodiment is preferably used such that the first sheet material 11 side is in contact with a high-temperature member (for example, a heat-generating member or the like).

[0308] This allows the material to have sufficiently excellent shape conformability and adhesion to the heat-generating component, and can more reliably exhibit excellent heat transport capacity.

[0309] In addition, the vapor chamber may be in a state where the condensation section, which is a section different from the evaporation section, i.e., the section that dissipates heat received from the heat-generating component, is in contact with a heat dissipation component (e.g., a heat sink, etc.) or a component made of a highly thermally conductive material (e.g., a thermally conductive sheet, etc.) that is in contact with the heat dissipation component.

[0310] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to the above, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention.

[0311] For example, the vapor chamber of the present invention may further include other components in addition to the components described above.

[0312] In addition, in the above-described embodiment, a case has been described in which the first sheet material and the second sheet material constituting the container are joined via a joining material, but the first sheet material and the second sheet material may be sealed by a sealing portion formed, for example, by plating up, laser welding, seam welding, cold welding, diffusion bonding, brazing, or adhesion.

[0313] Also, for example, the method for manufacturing a vapor chamber may further include other steps in addition to the steps described above.

[0314] In the above embodiment, a case has been described in which one prepreg is applied onto the first sheet material, but for example, a plurality of prepregs may be applied in a superimposed manner.

[0315] In addition, in the above-described embodiment, the explanation has been centered on the case where one vapor chamber is formed on one sheet material, but, for example, multiple vapor chambers may be formed on a large sheet material and cut into individual pieces.

[0316] In addition, in the above-described embodiment, the vapor chamber has been mainly described as being used for the purpose of transferring heat from a heat-generating component to a specified location, but the vapor chamber may also be used for the purpose of, for example, equalizing the heat of a localized high-temperature portion of a heat-generating component. [Explanation of symbols]

[0317] 1: Vapor chamber 2: Container 10: First member 11: First sheet material 12: First protrusion 13: Frame 14: Metal plating layer 15: Layer composed of a material containing an Sn-containing alloy 20: Second member 21: Second sheet material 22: Second protrusion 23: Layer composed of a material containing an Sn-containing alloy 30: Wick 40: Hydraulic fluid 50: Protective mask 51: Photomask 51a:Transparent part 51b: Shield part 52: Protective mask 100': Prepreg 100: Fiber-containing cured product 101: First Side 102: The second side 130: Fiber base material 131: Fiber 140'': Resin material (resin composition) 140': First resin cured product 140:Second resin cured product E: light P1, P2: Pitch T1, T2: Thickness W1, W2: Width D1,D2: Interval

Claims

1. A container formed by joining a first metal sheet material and a second metal sheet material and having a hollow portion therein; a wick disposed in the cavity; a plurality of first protrusions made of resin provided on an inner surface of the first sheet material; and a plurality of second metallic protrusions provided on the inner surface of the second sheet material.

2. The vapor chamber according to claim 1 , wherein the distance between the first protrusions is smaller than the distance between the second protrusions.

3. 3. The vapor chamber according to claim 1 or 2, wherein when the thickness of the first sheet material is T1 [μm] and the distance between the first convex portions is D1 [μm], the relationship 10<D1<80.966exp(0.0512T1) is satisfied.

4. The vapor chamber according to claim 1 or 2, wherein when the thickness of the second sheet material is T2 [μm] and the distance between the second convex portions is D2 [μm], the relationship 10 < D2 < 80.966 exp (0.0512T2) is satisfied.

5. In a plan view of the vapor chamber, the total area of ​​the first convex portion is S1 [cm 2 ], the total area of ​​the cavity is Sw [cm 2 3. The vapor chamber according to claim 1 or 2, which satisfies the relationship 0.03<S1 / Sw<0.

3.

6. In a plan view of the vapor chamber, the total area of ​​the second protrusions is S2 [cm 2 ], the total area of ​​the cavity is Sw [cm 2 3. The vapor chamber according to claim 1 or 2, which satisfies the relationship 0.03<S2 / Sw<0.

3.

7. The vapor chamber according to claim 1 or 2, wherein the vapor chamber is used such that the first sheet material side is in contact with a high-temperature member.

8. The vapor chamber according to claim 1 or 2, wherein the height of the first convex portion is 5 μm or more and 500 μm or less.

9. The vapor chamber according to claim 1 or 2, wherein the height of the second convex portion is 5 μm or more and 500 μm or less.

10. 3. The vapor chamber according to claim 1 or 2, wherein when the spacing between the first convex portions is D1 [μm] and the width of the second convex portions is W2 [μm], the relationship W2 > D1 is satisfied.

11. The vapor chamber according to claim 1 or 2, wherein the thickness of the wick is 10 μm or more and 1000 μm or less.

12. The vapor chamber according to claim 1 or 2, wherein the wick is made of glass fiber.

13. 3. The vapor chamber according to claim 1 or 2, wherein the container is mainly composed of Cu or a Cu alloy.

Citation Information

Patent Citations

  • Vapor chamber

    WO2017104819A1