Scarfing device and method

The fusing device and method address the challenge of achieving thin fusing thickness in steel materials by injecting oxygen and flammable gas, ensuring stable cutting with minimal thickness and improved yield through controlled oxygen slot thickness and speed.

JP2024142252APending Publication Date: 2024-10-10NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023054367
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for treating surface defects in steel materials, such as cracks and surface oxides, do not effectively achieve a thin fusing thickness, leading to yield loss and quality issues in high-grade steel products.

Method used

A fusing device and method that injects oxygen and flammable gas to the steel material's surface, utilizing combustion heat and oxidation reaction heat, with the oxygen slot thickness d satisfying the relational expressions d<5.2(mm) and d<0.52Vs, where Vs is the conveying speed, to achieve a thin cutting thickness.

Benefits of technology

The method allows for stable, thin fusing thicknesses of 2.0 mm or less, even at low conveying speeds, reducing defects and improving yield by removing surface imperfections like Cu-enriched layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a scarfing device and a method capable of achieving a thin scarfing thickness.SOLUTION: There is provided a scarfing device for ejecting oxygen and combustible gas to a surface of a steel product, for scarfing the surface of the steel product by combustion heat and oxidation reaction heat of the steel product, where a thickness d of an oxygen slot for ejecting oxygen, satisfies a following expression (1): (1) d<5.2(mm).SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cutting apparatus and a cutting method. [Background technology]

[0002] Patent Document 1 describes a surface cleaning method for a thin slab continuous casting slab, in which a surface layer of a slab 7 having a thickness of 100 mm or less that is continuously drawn from the lower end of a thin slab continuous casting mold 5 is heated and remelted by a slab surface heating device 8, 8A during cooling. Patent Document 1 also describes that heating is preferably performed at a position from the end 16 of a thin slab continuous casting machine 15 or after the position where the slab is completely solidified to the slab cutting device 9 or the entrance side or exit side of a heating furnace 10, and that the slab surface heating device uses plasma or a laser as a heat source.

[0003] Patent Document 2 describes a method for removing defects in the surface layer of a slab, in which a high-temperature slab after continuous casting is heated to a higher temperature to oxidize defects in the surface layer of the slab, and then high-pressure water is sprayed onto the slab to remove the oxides. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-170020 [Patent Document 2] Japanese Patent Application Publication No. 9-174500 Summary of the Invention [Problem to be solved by the invention]

[0005] In the steel manufacturing process, the surface of the steel may be treated. For example, cracks on the surface of the steel are quality defects and must be removed. In particular, in high-grade steel and steel sheets for automobiles, which place importance on surface quality, it is required to remove surface cracks. In addition, for example, surface defects such as iron oxide on the surface of the slab 1A, inclusions and casting powder that have become embedded in the surface layer during casting, or air bubble marks are removed by surface treatment.

[0006] When applying shave to a steel manufacturing process as a surface treatment method, it is necessary to achieve a thin shave thickness in order to avoid a decrease in yield. However, the techniques described in Patent Documents 1 and 2 do not mention shave, and do not consider the shave conditions for achieving a thin shave thickness.

[0007] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a laser cutting device and a laser cutting method that can achieve a thin laser cutting thickness. [Means for solving the problem]

[0008] In order to solve the above problems, according to one aspect of the present invention, there is provided a thermal cutting device that sprays oxygen and a combustible gas onto a surface of a steel material, thereby thermally cutting the surface of the steel material using the heat of combustion and the heat of the oxidation reaction of the steel material, wherein the thickness d of an oxygen slot for spraying the oxygen satisfies the following relational expression (1). d<5.2(mm) (1)

[0009] The thickness d of the oxygen slot may further satisfy the following relational expression (2): d<0.52Vs (2) Where, Vs: conveying speed Vs (m / min)

[0010] A conveying speed Vs of the steel material to be cut by the cutting device may be set to 10 m / min or less.

[0011] The above-mentioned laser cutting device may be provided downstream of a heating furnace of a hot rolling facility.

[0012] In order to solve the above problem, according to another aspect of the present invention, there is provided a method for thermal cutting, which comprises spraying oxygen and a combustible gas onto a surface of a steel material, thereby thermally cutting the surface of the steel material using the heat of combustion and the heat of an oxidation reaction of the steel material, wherein a thickness d of an oxygen slot for spraying the oxygen satisfies the following relational expression (3). d<5.2(mm) (3)

[0013] The thickness d of the oxygen slot may further satisfy the following relational expression (4): d<0.52Vs (4) Where, Vs: conveying speed Vs (m / min) Effect of the Invention

[0014] As described above, according to the present invention, a cutting device and a cutting method capable of achieving a thin cutting thickness are provided. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram showing an example of a schematic configuration of hot rolling equipment according to a first embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing an example of a schematic configuration of a laser cutting apparatus according to a first embodiment of the present invention. [Diagram 3] 1 is a graph showing an example of the relationship between a cutting speed and a cutting thickness. [Figure 4] FIG. 2 is a schematic diagram showing an example of a state of thermal cutting. [Diagram 5] FIG. 2 is a schematic diagram showing an example of a state of thermal cutting. [Figure 6] 1 is a schematic diagram showing an example of a schematic configuration of a laser cutting apparatus according to a first embodiment of the present invention. [Figure 7] 1 is a graph showing an example of the relationship between the limiting thickness of the thermal cutting and the oxygen slot thickness. [Figure 8]1 is a graph showing an example of the relationship between the limiting thickness of the thermal cutting and the oxygen slot thickness. [Figure 9] 1 is a graph showing an example of a relationship between a gradient and a cutting speed. [Figure 10] 1 is a graph showing an example of the relationship between a cutting speed and a cutting thickness. [Figure 11] FIG. 2 is a schematic diagram showing an example of a target region according to the first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.

[0017] <First embodiment> First, a schematic configuration of a hot rolling facility 10 according to a first embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a diagram showing a schematic configuration of the hot rolling facility 10.

[0018] As shown in FIG. 1 as an example, the hot rolling equipment 10 is equipment for hot rolling a steel material 1. The hot rolling equipment 10 includes a heating furnace 20, a slag cutting device 30, a descaling device 40, a rough rolling device 50, and a finish rolling device 60. The heating furnace 20 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length to a predetermined temperature. The slab 1A is heated by the heating furnace 20 while being transported by a transport roll 22. Here, the steel material 1 is a steel material containing Cu, for example, a steel material containing 0.15 wt% or more of Cu, particularly a steel material containing 0.25 wt% or more of Cu. Note that, although the slab 1A is given as an example of the steel material 1 here, this is merely an example, and the steel material 1 may be a billet.

[0019] The slag cutting device 30 performs slag cutting on the slab 1A discharged from the heating furnace 20 to remove the surface portion of the slab 1A. The slag cutting device 30 will be described in detail later. The slag cutting device 30 is located downstream of the heating furnace 20 in the conveying direction of the slab 1A. The slag cutting device 30 is also located upstream of the descaling device 40. More specifically, the slag cutting device 30 is located downstream of the heating furnace 20 and upstream of the vertical rolls 24 that roll the slab 1A heated in the heating furnace 20 in the width direction. In this specification, the term "removal" includes complete removal, and refers to removal in the sense of insufficient removal within a range generally acceptable in the technical field to which the present invention belongs, and including insufficient removal to a degree that does not go against the spirit of the present invention.

[0020] The descaling device 40 removes scale (i.e., oxide film) formed on the surface of the slab 1A before rough rolling by the rough rolling device 50. The descaling device 40 removes scale by spraying a fluid (e.g., cooling water) from a nozzle 42 onto the slab 1A. That is, the descaling device 40 sprays cooling water W, which is supplied from a cooling water tank (not shown) and has a predetermined water pressure using a pump (not shown), onto the slab 1A from the nozzle 42. The descaling device 40 removes scale from the surface of the slab 1A, and the temperature of the surface of the slab 1A is set to 1100°C or less by heat extraction by the cooling water. Here, the surface temperature of the slab 1A after scale removal by the descaling device 40 (e.g., the side surface in the width direction of the slab 1A) is measured by a radiation thermometer.

[0021] The rough rolling device 50 performs rough rolling on the slab 1A to thin it down to a predetermined thickness. Specifically, the rough rolling device 50 rolls the slab 1A, which has been rolled in the width direction by the vertical rolls 24, from above and below to form a rough bar 1B. In the example shown in FIG. 1, the rough rolling device 50 includes four rolling mills 51-54. The rough rolling device 50 sandwiches the slab 1A between the rolls from above and below and continuously rolls it using the rolling mills 51-54. In the rough rolling device 50, the slab 1A is thinned down to a plate thickness of, for example, about 25-50 mm, and formed into a rough bar 1B.

[0022] The finishing rolling device 60 continuously hot-finish-rolls the rough bar 1B to a predetermined thickness. Specifically, the rough bar 1B, which has been reheated by the rough bar heating device 62 and transported, is finish-rolled to a thickness of about several mm (for example, 1 to 2 mm). These finishing rolling devices 60 pass the rough bar 1B through gaps between finishing rolling rolls 64 arranged vertically in a straight line across 6 to 7 stands, and gradually roll it down. The steel strip 1C obtained by finish-rolling to a predetermined thickness by this finishing rolling device 60 is sent to a cooling device 70. Note that, here, an example of the finishing rolling device 60 having 6 to 7 stands is shown, but this is merely an example, and the finishing rolling device 60 may have 5 stands.

[0023] The cooling device 70 cools the steel strip 1C after the finish rolling with cooling water W. The cooling device 70 is, for example, a pipe laminar nozzle type cooling device. The steel strip 1C cooled by the cooling device 70 is wound into a coil by a winding device 80 and transported from the hot rolling equipment 10 to the next process as a hot rolled coil 1D.

[0024] In the hot rolling equipment 10 according to the present embodiment, the surface of the slab 1A is removed by the scavenging device 30. As shown in FIG. 2 as an example, the scavenging device 30 has a scarfer unit 31 arranged to face the surface of the steel material 1. The scarfer unit 31 includes a preheating gas ejection section 34 and an oxygen slot 36. In the preheating process, the preheating gas ejection section 34 ejects preheating oxygen 32 and a combustible gas 33. In addition, in the scavenging process, the preheating gas ejection section 34 ejects a front shielding gas 35. That is, in the scavenging process, the preheating gas ejection section 34 functions as a shielding gas ejection section. The oxygen slot 36 ejects scavenging oxygen 37.

[0025] As shown in Figure 2, the flow of oxygen for cutting 37 ejected from the oxygen slot 36 is positioned so as to collide forward in the conveying direction Y of the steel material 1 relative to the flow of preheating oxygen 32 and combustible gas 33 ejected from the preheating gas ejection section 34.

[0026] In the sintering device 30, first, a preheating process is performed as shown on the left side of Fig. 2. In the preheating process, preheating oxygen 32 and combustible gas 33 are ejected from a preheating gas ejection part 34 of the scarfer unit 31 toward the surface of the steel material 1, and the combustible gas 33 is burned. Then, a part of the surface of the steel material 1 is melted by the heat of the burning combustible gas 33, and a basin portion 1E is formed.

[0027] The length of the well portion 1E formed on the surface of the steel material 1 along the conveying direction Y is set to, for example, within a range of about 20 mm to 30 mm.

[0028] Next, as shown on the right side of FIG. 2, a laser cutting process is performed. In the laser cutting process, laser cutting oxygen 37 is ejected from the oxygen slot 36 of the scarfer unit 31 toward the surface of the steel material 1, and the steel material 1 on which the basin portion 1E is formed is transported in the transport direction Y. At this time, a front shielding gas 35 is ejected from the preheating gas ejection portion 34. The front shielding gas 35 contains a combustible gas 35B and oxygen 35A. The flow of the front shielding gas 35 is located on the front side of the laser cutting oxygen 37 in the laser cutting advancement direction (i.e., the opposite direction to the Y direction, which is the transport direction). The front shielding gas 35 is ejected as a protective gas for maintaining the oxygen concentration of the laser cutting oxygen 37. In addition, a rear shielding gas 38 is ejected on the rear side of the laser cutting oxygen 37 in the laser cutting advancement direction. The rear shielding gas 38 is ejected as a protective gas for maintaining the oxygen concentration of the laser cutting oxygen 37. The rear shielding gas 38 is a combustible gas, for example, LPG. In other words, the front shielding gas 35 and the rear shielding gas 38 suppress the inflow of air (e.g., mainly nitrogen) from the outside into the cutting oxygen 37, or the outflow of oxygen to the outside, thereby suppressing changes in the oxygen concentration of the cutting oxygen 37.

[0029] In the laser cutting process, the jet of laser cutting oxygen 37 ejected from oxygen slot 36 collides with the molten iron in the well 1E of the steel material 1 being transported, causing an oxidation reaction between the molten iron and the laser cutting oxygen 37. The surface of the steel material 1 melts one after another due to the heat of this oxidation reaction, and the surface of the steel material 1 is laser cut. That is, the rear side of the well 1E in the transport direction Y is laser cut by the heat of the oxidation reaction. In this way, the surface of the slab 1A after it has been heated in the heating furnace 20 is laser cut by the laser cutting device 30.

[0030] Incidentally, when performing a thin swarf cutting on the steel material 1, it is possible to consider a method of increasing the conveying speed of the steel material 1 during swarf cutting (hereinafter also simply referred to as the "swarf cutting speed") or decreasing the pressure of the swarf cutting oxygen 37. In general, when the swarf cutting speed is increased, the swarf cutting thickness becomes thinner in inverse proportion to the speed. As an example, as shown in FIG. 3, at a swarf cutting speed of 15 m / min or more, swarf cutting of less than 2.0 mm can be achieved (see high pressure (e.g., 0.76 MPa) in the figure). However, when the swarf cutting speed is further increased to 20 m / min or more, the swarf cutting reaction is interrupted, the swarf cutting area is not continuous, and intermittent swarf cutting defects (so-called tiger cutting phenomenon) occur. Thus, the swarf cutting phenomenon has a swarf cutting limit (see dotted line in FIG. 3) at which swarf cutting suddenly becomes impossible when a certain swarf cutting speed is exceeded.

[0031] On the other hand, when the pressure of the oxygen for cutting 37 is lowered (see low pressure (e.g., 0.49 MPa) in the figure), the cutting thickness can be reduced at a low speed, but the cutting limit at which the cutting reaction stops also shifts to a low speed, and as a result, the achievable cutting thickness becomes thicker than when the pressure of the oxygen for cutting 37 is increased, and a cutting thickness of less than 2.0 mm cannot be achieved. Therefore, when there is a mechanical constraint on the cutting speed (e.g., an upper limit on the conveying speed), it is difficult to achieve a cutting thickness below the cutting limit even if the cutting conditions are adjusted, such as by lowering the oxygen pressure.

[0032] In general, to reduce the thickness of the shave, as shown in Fig. 4, the shave area WR is narrowed or the angle θ (=tan -1 It is necessary to make the ratio (thickness of swarfing t1 / length of swarfing area) gentle. For example, if the swarfing speed is increased, the time during which the swarfing area WR is exposed to the swarfing oxygen 37 is shortened, and the angle θ of the swarfing area WR becomes gentle. However, if the swarfing speed is increased, this is contrary to the objective of achieving a conveying speed of 10 m / min or less.

[0033] In addition, when the pressure of the oxygen 37 for slag cutting is reduced, the slag cutting progress speed in the thickness direction is suppressed and the angle θ becomes gentle. However, when the pressure of the oxygen 37 for slag cutting is reduced, the momentum of the oxygen jet decreases, and the molten iron 1F generated by slag cutting cannot be removed, so that slag cutting defects are likely to occur. As a result, the minimum slag cutting thickness becomes thick. Therefore, the inventors of the present invention have studied diligently and come up with the idea of ​​physically narrowing the slag cutting region WR in order to reduce the slag cutting thickness t1 while maintaining a sufficient pressure of the oxygen 37 for slag cutting without increasing the slag cutting speed, and have devised a method of reducing the thickness of the jet of the oxygen 37 for slag cutting, as shown in FIG. 5 as an example.

[0034] As an example, as shown in Fig. 6, a scarfer unit 31 in a laser cutting device 30 includes an upper block 31A, a lower block 31B, and a shoe 31C. A preheating gas ejection part 34 is formed at the tip of the upper block 31A. An oxygen slot 36 is formed between the upper block 31A and the lower block 31B. The oxygen slot 36 is an opening having a preset oxygen slot thickness d. Laser cutting oxygen 37 is ejected toward the steel material 1 through the oxygen slot 36.

[0035] FIG. 7 shows the relationship between various oxygen slot thicknesses d and the minimum slag cutting thickness h at which slag cutting can be performed stably without slag cutting defects (e.g., slag cutting) when the slag cutting speed is 10 m / min and the amount of slag cutting oxygen 37 is reduced. As an example, as shown in FIG. 7, the relationship between the oxygen slot thickness d and the minimum slag cutting thickness h is linear. In the example shown in FIG. 7, the slag cutting thickness h at which slag cutting can be performed stably can be expressed as h>0.39d. This shows that in order to achieve a slag cutting thickness of 2.0 mm or less at a slag cutting speed of 10 m / min, the oxygen slot thickness d should be set to 5.2 mm or less.

[0036] Figure 8 shows the relationship between the oxygen slot thickness d and the minimum scalding thickness h when the scalding speed is 25 m / min. As an example, as shown in Figure 8, it can be seen that the region where scalding is possible is expanded compared to when the scalding speed is 10 m / min. And, as shown in Figures 7 and 8, the relationship between the limit scalding thickness (i.e., the minimum scalding thickness) h and the oxygen slot thickness d at each scalding speed can be expressed as follows: h>0.39d (Vs=10m / min) ···(1) h>0.16d (Vs=25m / min) ···(2)

[0037] Figure 9 shows the relationship between the cutting speed and the gradient. As an example, as shown in Figure 9, the coefficients on the right side of the above formula (1) and formula (2) are inversely proportional to each other, decreasing as Vs increases. The coefficients of this formula can be further rearranged from Figure 9 to be expressed as the following formula. h>3.8d / Vs (3) From the above formula (3), the condition for performing surface cutting at 2.0 mm or less is as shown in the following formula (4). d<0.52Vs (4)

[0038] By setting the oxygen slot thickness d to a value that satisfies the above formula (4), it is possible to stably achieve a swarf cutting thickness of 2.0 mm or less by adjusting operational parameters such as the pressure of the swarf cutting oxygen 37. Figure 10 shows the relationship between the swarf cutting speed and the swarf cutting thickness when swarf cutting is performed with oxygen slot thickness d = 4 mm and high-pressure oxygen. As an example, as shown in Figure 10, when the oxygen slot thickness d is 4 mm, the swarf cutting thickness is 1.6 mm at a swarf cutting speed of 10 m / min. The limit line (see dashed line in the figure) at which the swarf cutting thickness transitions to 0 due to swarf cutting failure transitions to the lower speed side when the oxygen slot thickness d is 4 mm, and thin swarf cutting is achieved at a low speed.

[0039] In recent years, iron sources other than iron ore have come to be used in order to reduce carbon dioxide emissions in the steel manufacturing process. For example, increasing the proportion of scrap iron used as the iron source has been considered.

[0040] However, when scrap iron is used as an iron source, surface defects may occur during the steel manufacturing process due to copper (Cu) contained in the scrap iron. For example, during the hot rolling process, red embrittlement cracking occurs due to the concentration of Cu on the surface of the steel, resulting in a decrease in the surface quality of the steel. For this reason, it is difficult to increase the proportion of scrap iron containing Cu in the iron source, which is an obstacle to realizing an environmentally friendly steel manufacturing process.

[0041] Therefore, the Cu-enriched layer on the surface of the slab 1A is removed after heating in the heating furnace 20 in the hot rolling. That is, in the thermal history of the hot rolling, after the steel material 1 leaves the heating furnace 20 and becomes 1000°C or less in the rough rolling process, it is not heated to 1000°C or more again. Therefore, if the Cu-enriched layer is removed after heating in the heating furnace 20, the generation of scale in the subsequent processes is suppressed. As a result, the Cu concentration phenomenon is suppressed, and red-heat embrittlement cracking is also suppressed.

[0042] The Cu-enriched layer is formed only in the surface layer of less than 2 mm, and red embrittlement cracking can be suppressed by performing laser cutting to a thickness of at most about 2 mm, or to a thickness of 1.0 mm or less depending on the Cu content or heating conditions.

[0043] 11 as an example, the laser cutting device 30 removes a target area T which is an area including a Cu-enriched layer R. Here, the target area T is a range of a predetermined distance from the surface of the steel material 1 (i.e., the surface of the scale S) in the thickness direction t of the steel material 1. The predetermined distance is, for example, greater than 0 mm and equal to or less than 3 mm, preferably greater than 0 mm and equal to or less than 2 mm, and more preferably greater than 0 mm and equal to or less than 1 mm.

[0044] When the steel material 1 is a rough bar 1B, the thickness of the steel material 1 is, for example, about 25 to 50 mm. Therefore, by removing a region that is 1 mm or less away from the surface of the steel material 1 as the target region T, it is possible to suppress a reduction in the thickness of the steel material 1 and improve the yield.

[0045] 11 shows an example in which one surface in the thickness direction of the steel material 1 is scarified, but the scarifying device 30 according to this embodiment also scarifies other surfaces in the thickness direction of the steel material 1. In this case, the scarifying device 30 includes scarfer units 31 at positions facing each of the one surface and the other surface of the steel material 1.

[0046] As described above, in this embodiment, since the oxygen slot thickness d satisfies a predetermined condition, even at a low cutting speed, cutting is performed with a thin cutting thickness below the critical cutting thickness. This makes it possible to stably perform cutting of 2 mm or less, preferably 1 mm or less, when removing the target region T that is a region including the Cu-enriched layer R present on the surface of the steel material 1.

[0047] In addition, in hot rolling equipment, transportation may be performed at a low speed of 10 m / min or less in some parts. In this case, if the oxygen slot thickness d does not satisfy the predetermined condition, it is difficult to perform stably at a shave thickness of 2 mm or less because of the shave limit (see FIG. 3). However, in this embodiment, the oxygen slot thickness d satisfies the predetermined condition, so that the minimum shave thickness can be reduced, and stable shave thickness of 2 mm or less can be realized.

[0048] As described above, in the laser cutting apparatus 30 according to this embodiment, the oxygen for laser cutting 37 is sprayed onto the surface of the steel material 1, and the surface of the steel material 1 is laser cut by the combustion heat and the oxidation reaction of the steel material 1. In the laser cutting apparatus 30, the oxygen slot thickness d for spraying the oxygen for laser cutting 37 is set so as to satisfy the following relational expression (5). d<5.2(mm) (5) When the oxygen slot thickness d satisfies the above relational expression (5), the thickness of the jet of the oxygen for laser cutting 37 becomes thin, and the laser cutting region WR becomes physically narrower without increasing the laser cutting speed and while maintaining a sufficient pressure of the oxygen for laser cutting 37. This allows laser cutting to be performed with a thin laser cutting thickness that is below the critical laser cutting thickness.

[0049] Moreover, in the surface-cutting apparatus 30 according to this embodiment, the oxygen slot thickness d further satisfies the following relational expression (6). d<0.52Vs (6) When the oxygen slot thickness d satisfies the above relational expression (6), stable thermal cutting to a thickness of 2.0 mm or less can be achieved.

[0050] In addition, in the cutting device 30 according to this embodiment, the conveying speed of the steel material 1 to be cut is set to 10 m / min or less. At a conveying speed of 10 m / min or less, cutting defects (e.g., tiger cutting) may occur, and cutting may become unstable (see FIG. 3). That is, at a cutting speed of 10 m / min or less, the limit cutting thickness at which cutting can be performed stably becomes large, and cutting at a thin cutting thickness is difficult. In this configuration, by making the oxygen slot thickness d satisfy a predetermined condition, cutting at a thin cutting thickness below the limit cutting thickness is realized even at a low cutting speed.

[0051] In addition, the laser cutting device 30 according to this embodiment is provided downstream of the heating furnace 20 in the hot rolling equipment 10 in the conveying direction. By providing the laser cutting device 30 downstream of the heating furnace 20, the removal of the Cu-enriched layer on the surface of the steel material 1 is performed after heating by the heating furnace 20 in hot rolling. If the Cu-enriched layer is removed after heating by the heating furnace 20, the generation of scale in the subsequent process is suppressed. As a result, the Cu-enriched phenomenon is suppressed, and red embrittlement cracking is also suppressed. In addition, the Cu-enriched layer is generated only in the surface layer of less than 2 mm, and red embrittlement cracking can be suppressed by performing laser cutting with a thickness of at most about 2 mm, or 1.0 mm or less depending on the Cu content or heating conditions.

[0052] For example, when performing shave cutting in a hot rolling facility, it may be necessary to perform thin shave cutting of less than 2.0 mm at a conveying speed of 10 m / min. In order to prevent red embrittlement cracking specific to steel material 1 containing Cu, shave cutting with a thickness exceeding 2 mm has no merit in terms of quality and rather reduces the yield. In addition, a conveying speed of 10 m / min or less is generally used in the conveying process before the rough rolling process of hot rolling. This is because the steel material 1 (e.g., slab 1A) after heating has warpage or bending, and if it is conveyed at a speed exceeding 10 m / min, there is a possibility that the equipment will be damaged by collision with the steel material 1. In this configuration, even if the conveying speed is 10 m / min, shave cutting with a thin shave thickness below the limit shave thickness is realized even at a low shave cutting speed by satisfying a predetermined condition for the oxygen slot thickness d.

[0053] In the above embodiment, an example in which the slag cutting by the slag cutting device 30 is performed between the heating process by the heating furnace 20 and the rough rolling process in the hot rolling process has been described, but this is merely one example. For example, the slag cutting by the slag cutting device 30 may be performed during the rough rolling process. Specifically, the slag cutting device 30 is provided between each of the rolling mills that form the rough rolling device 50. In addition, for example, the slag cutting of the steel material 1 by the slag cutting device 30 may be performed after rough rolling and before finish rolling, or may be performed during the finish rolling process.

[0054] In the above embodiment, an example in which the slag cutting is performed by the slag cutting device 30 in the hot rolling process has been described, but this is merely one example. The slag cutting method according to this embodiment may be applied to a steelmaking process or before a heating furnace in a hot rolling process. Furthermore, the slag cutting method according to this embodiment does not have to be applied to a manufacturing line for the steel material 1, and the steel material 1 to be slag cut may be a steel pipe or an H-beam instead of a steel strip. EXAMPLES

[0055] In order to evaluate the performance of the slag cutting device according to the present invention, slag cutting experiments were carried out to examine the slag cutting thickness while changing slag cutting conditions.

[0056] The cutting conditions were as follows: the oxygen slot thickness d was 6, 4, or 3 mm, and the pressure of the oxygen 37 for cutting was at two levels: high pressure of 0.76 MPa and low pressure of 0.42 MPa.

[0057] In addition, the cutting speed was reduced to the condition where cutting was impossible under each cutting condition, and the cutting speed where cutting was impossible was defined as (cutting speed where cutting was impossible) - (1 m / min). The condition where cutting was impossible was a condition where cutting failure occurred in some areas, such as interruption of cutting. In this case, for example, even if almost the entire surface was cut, the cutting thickness was set to 0 mm.

[0058] In the swarf cutting experiment, only the center of the test steel plate was swarfed, and the swarf thickness was measured by measuring the depression of the swarfed area relative to the unswarfed area using a laser distance meter. The swarf thickness was the average value measured at 10 points in the longitudinal direction (i.e., the direction in which the swarf cutting proceeded).

[0059] Table 1 shows the results of changing the oxygen slot thickness d and the pressure of the oxygen 37 for cutting. In Comparative Example 1, the thinnest cutting thickness was 2.2 mm, and cutting was interrupted at a speed higher than that. In Comparative Example 2, the cutting thickness during high-speed cutting was 1.6 mm, achieving 2.0 mm or less, but at a cutting speed of 10 m / min or less, the cutting thickness was thick, and thin cutting at low speed was not realized. In Examples 1 and 2, cutting was performed under the condition of an oxygen slot thickness d of 4 mm or 3 mm. In both cases, cutting to a cutting thickness of 2.0 mm or less was realized at a cutting speed of 10 m / min or less. In addition, under the condition of an oxygen slot thickness d of 4 mm in Inventive Example 1, cutting was possible at a cutting speed of 10 m / min or less, and cutting thinner than 1.6 mm was also realized.

[0060] [Table 1]

[0061] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to the above examples. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified examples or application examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.

[0062] In addition to the above-described embodiment, the following supplementary notes are further disclosed.

[0063] <Appendix 1> A cutting device that cuts the surface of a steel material by injecting oxygen and a combustible gas onto the surface of the steel material using the heat of combustion and the heat of an oxidation reaction of the steel material, The thickness d of the oxygen slot for injecting the oxygen satisfies the following relational expression (A). Melting equipment. d<5.2(mm)...(A) <Appendix 2> The thickness d of the oxygen slot further satisfies the following relation (B): 2. The scouring apparatus of claim 1. d<0.52Vs (B) Where, Vs: conveying speed (m / min) <Appendix 3> The conveying speed Vs of the steel material to be shave by the shave device is set to 10 m / min or less. 3. The scouring apparatus according to claim 2. <Appendix 4> The above-mentioned slag cutting device is provided downstream of the heating furnace of the hot rolling equipment. 4. The laser cutting apparatus according to claim 1, [Explanation of symbols]

[0064] 1 Steel material 1A Slab 1B coarse bar 1C steel strip 1D hot rolled coil 1E Bathtub 1F Molten Iron 10. Hot rolling equipment 11 Continuous casting machine 20 Furnace 22 Transport roll 24 Vertical Roll 30 Cutting equipment 31 Scarfer Unit 31A Upper Block 31B Lower Block 31C Shoe 32 Preheating oxygen 33 Flammable gases 34 Preheating gas outlet 35 Forward shielding gas 35A Oxygen 35B Flammable gas 36 Oxygen Slots 37 Oxygen for cutting 38 Rear Shielding Gas 40 Descaling device 42 Nozzle 50 Rough rolling equipment 51, 52, 53, 54 Rolling mill 60 Finishing rolling equipment 62 Rough bar heating device 64 Finishing Roll 70 Cooling device 80 Winding device θ angle R Cu enriched layer S scale T Target area Vs conveying speed W Cooling water WR cutting area Y Arrow t thickness direction d Oxygen slot thickness

Claims

1. A thermal cutting device that thermally cuts a surface of a steel material by injecting oxygen and a combustible gas onto the surface of the steel material using combustion heat and oxidation reaction heat of the steel material, The thickness d of the oxygen slot for injecting oxygen satisfies the following relational expression (1): Melting equipment. d<5.2(mm)...(1)

2. The thickness d of the oxygen slot further satisfies the following relational expression (2): The cutting apparatus of claim 1 . d<0.52Vs...(2) Where, Vs: conveying speed (m / min)

3. The conveying speed Vs of the steel material to be shave by the shave device is set to 10 m / min or less. The cutting apparatus of claim 2.

4. The slag cutting device is provided downstream of the heating furnace of the hot rolling equipment. The cutting apparatus according to any one of claims 1 to 3.

5. A method for thermal cutting a surface of a steel material by spraying oxygen and a combustible gas onto the surface of the steel material, the method comprising the steps of: The thickness d of the oxygen slot for injecting oxygen satisfies the following relational expression (3). Melting method. d<5.2(mm)...(3)

6. The thickness d of the oxygen slot further satisfies the following relation (4): The method of claim 5. d<0.52Vs...(4) Where, Vs: conveying speed (m / min)

Citation Information

Patent Citations

  • Ingot cutting and slag scraping device

    JP1981086677A

  • Method for scarfing steel having rectangular cross section

    JP1990274377A

  • Manufacture of thin steel sheet excellent in surface property and manufacturing equipment line therefor

    JP1994315702A

  • Method of gas-scarfing burr on cast slab

    JP1998272544A

  • Device for removing scarfing burr

    JP1999123545A