Eccentric core-sheath conjugated polyester fiber
Eccentric core-sheath composite polyester fibers with controlled curvature and composite ratios address the balance of bulkiness, stretchability, and surface quality issues in fabrics by ensuring independent crimp formation, resulting in a fabric with enhanced properties.
Patent Information
- Application Number
- JP2023054731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing crimp-generating composite fibers, such as those described in Patent Documents 1-4, fail to achieve a balance between bulkiness, stretchability, and surface quality due to interlocking of single fibers or crimp form differences leading to wrinkles and reduced fabric quality.
The use of eccentric core-sheath composite polyester fibers with specific curvature, composite area ratios, and multiple single fiber groups with varying composite ratios, each having a curvature of 15% or less and a composite area ratio of 80:20 to 20:80, ensures independent crimp formation without interlocking, resulting in a fabric with excellent bulkiness and stretchability.
The solution provides a fabric with an elegant surface quality free from grains or wrinkles while maintaining high bulkiness and stretchability, surpassing the limitations of previous technologies.
Smart Images

Figure 00000016_0000 
Figure 00000016_0001 
Figure 00000016_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to an eccentric core-sheath composite polyester fiber which can provide a fabric having an elegant surface quality free of grains and wrinkles, and also having excellent bulkiness and stretchability. [Background technology]
[0002] Polyester has various excellent properties including mechanical properties and dimensional stability, and is therefore used in a variety of fields including clothing applications and industrial materials applications. In particular, for clothing applications, there is a high demand for stretch materials because of their excellent fit and movement-following properties when worn, and there has been active development of high-performance stretch fibers that also have comfort in terms of bulkiness, texture, etc.
[0003] Various methods have been proposed for imparting stretchability to raw yarns constituting fabrics, such as a method of imparting stretchability by mixing polyurethane-based elastic fibers into woven or knitted fabrics. However, when polyurethane-based fibers are mixed in, the texture is hard due to the inherent properties of polyurethane, and the texture and drape of the woven or knitted fabric are deteriorated, and the dyeing process becomes complicated because the fibers are difficult to dye with polyester-based dyes.
[0004] There is also a method of imparting stretchability to woven and knitted fabrics by applying false twist processing to polyester fibers and using fibers that have been given twist / untwist torque. However, when this torque is used in woven fabrics, it can cause wrinkles and creases on the surface of the fabric, which can easily become fabric defects. For this reason, heat treatment or S / Z twisting is used to balance the torque and prevent the occurrence of wrinkles and creases, but this method has the problem of low stretchability.
[0005] In response to these problems, various crimp-producing composite fibers have been proposed, which are made by conjugating polymers with different shrinkage properties or intrinsic viscosities in a side-by-side or eccentric core-sheath type. The crimp-producing composite fibers referred to here are fibers in which, when subjected to heat treatment or the like, a three-dimensional spiral crimp like a coil is produced due to the shrinkage difference between the polymers bonded to the left and right, and this coil-like crimp stretches and shrinks to become a fiber with elasticity.
[0006] Patent Document 1 proposes crimp-expressing conjugate fibers such as side-by-side conjugate fibers made of polyethylene terephthalate (PET) having an intrinsic viscosity difference or an intrinsic viscosity difference, and Patent Document 2 proposes side-by-side conjugate fibers made of polytrimethylene terephthalate (PTT) and PET.
[0007] As a technique for increasing the bulkiness of crimp-developing conjugate fibers, Patent Document 3 proposes a method in which a high-viscosity polyester component and a low-viscosity polyester component are bonded side-by-side to each other, whereby the conjugation ratio is made different between single fibers to impart a random feel, and also proposes a method in which single fibers containing only the high-viscosity polyester component and only the low-viscosity polyester component are mixed.
[0008] Furthermore, Patent Document 4 proposes controlling the curvature of the composite interface as one method for improving the stretchability of such crimp-expressing composite fibers, and describes that the smaller the degree of curvature, the larger the crimp that appears in the coil diameter, making it possible to obtain a fiber with excellent stretchability. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 4-308271 [Patent Document 2] JP 2005-113369 A [Patent Document 3] JP 2008-75224 A [Patent Document 4] WO2018-235754 publication Summary of the Invention [Problem to be solved by the invention]
[0010] In the crimp-producing conjugate fibers proposed in Patent Documents 1 and 2, all of the constituent single fibers have the same composite cross section, so the crimp morphology produced by the single fibers naturally becomes similar between adjacent single fibers. As a result, the single fibers may become entangled so as to interlock with each other, resulting in a crimp-producing conjugate fiber with low bulkiness, as if multiple single fibers were twisted together. Since the single fibers of such a yarn bundle made of multifilaments are bundled together, when the yarn bundle is made into a fabric as is, it is difficult to obtain a high bulkiness, and further, the surface quality and touch may be deteriorated due to crimping or the like.
[0011] On the other hand, in the case of the crimp-expressing conjugate fiber proposed in Patent Document 3 in which the conjugation ratio between single fibers is changed, the difference in crimp morphology between the single fibers according to the conjugation ratio makes it possible to form crimps independently without the crimps interlocking between the single fibers, and therefore the fiber has excellent bulkiness. However, since the cross-sectional shape of the single fiber changes with the change in the conjugation ratio, the fiber may not have excellent spinnability or advanced processability.
[0012] In addition, the fiber proposed in Patent Document 4 in which the curvature rate of the composite interface is controlled relates to a monofilament intended for use in stockings. When applied to a multifilament, although it has excellent stretchability, the crimp phase is uniform, so that when it is made into a fabric as is, it is difficult to obtain bulkiness, and further, the surface quality and touch are deteriorated due to crimping and the like. [Means for solving the problem]
[0013] (1) In order to solve the above problems, the present invention employs the following configuration. An eccentric sheath-core composite polyester fiber is a multifilament consisting of eccentric sheath-core composite fibers composed of polyester components with different intrinsic viscosities, in which the curvature of the composite interface in the composite cross section of the single fiber is 15% or less, the composite area ratio of the core component to the sheath component is in the range of 80:20 to 20:80, and the eccentric sheath-core composite polyester fiber is composed of three or more types of single fiber groups with different composite area ratios. (2) The eccentric sheath-core composite polyester fiber according to claim 1, wherein the ratio of the number of single fibers in each single fiber group to the total number of single fibers is less than 50%. (3) The eccentric core-sheath composite polyester fiber according to claim 1, characterized in that the CV value of the curvature of the composite interface is 0.40 or less. (4) The eccentric core-sheath composite polyester fiber according to any one of claims 1 to 3, wherein the single fiber fineness is 0.3 to 7.0 dtex. Effect of the Invention
[0014] The eccentric core-sheath composite polyester fiber of the present invention can provide woven and knitted fabrics that have an elegant surface quality free of crimps and wrinkles, and also have excellent bulkiness and stretchability. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a schematic diagram illustrating a composite cross section of an eccentric sheath-core composite fiber of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing measurement of the curvature of the composite interface of the eccentric core-sheath composite fiber of the present invention. [Diagram 3] 1 is an example of a group of single fibers constituting the eccentric core-sheath composite polyester fiber of the present invention. [Figure 4] 1 is an example of distribution holes in a final distribution plate for obtaining a composite cross section of an eccentric sheath-core composite fiber of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below together with preferred embodiments.
[0017] The eccentric sheath-core composite polyester fiber of the present invention is composed of a multifilament made of eccentric sheath-core composite fibers in which polyester components with different intrinsic viscosities are bonded together in an eccentric sheath-core configuration. By bonding polyester components with different intrinsic viscosities together, stress is concentrated on the high-viscosity side during spinning and drawing, resulting in different internal strains between the components. As a result, the high-viscosity side shrinks significantly due to the difference in elastic recovery after drawing and the difference in thermal shrinkage during the heat treatment process of the fabric, and distortion occurs within the single yarn, forming a three-dimensional coil shape, which exhibits stretchability.
[0018] The polyester component in the present invention is not particularly limited as long as it is a fiber-forming polyester that has good interfacial adhesion between the core component (high viscosity component) and the sheath component (low viscosity component) and is stable in spinnability. However, taking into consideration the mechanical properties, chemical properties, and raw material cost, fiber-forming polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT) are preferred. In addition to PET, PTT, and PBT, those copolymerized with a third component, or mixed polymers of these may also be used.
[0019] The PET in the present invention may be a polyester consisting of 90 mol % or more of ethylene terephthalate repeating units, with terephthalic acid as the main acid component and ethylene glycol as the main glycol component. However, it may also contain a copolymerizable component capable of forming other ester bonds at a ratio of 10 mol % or less. Examples of copolymerizable compounds include dicarboxylic acids such as isophthalic acid, cyclohexanedicarboxylic acid, adipic acid, dimer acid, and sebacic acid, while examples of glycol components include, but are not limited to, propanediol, diethylene glycol, butanediol, neopentyl glycol, cyclohexanedimethanol, polyethylene glycol, and polypropylene glycol. In addition, titanium dioxide as a matting agent, fine particles of silica or alumina as a lubricant, hindered phenol derivatives as an antioxidant, and coloring pigments may be added as necessary.
[0020] The PTT in the present invention is a PTT consisting of 90 mol % or more of repeating units of trimethylene terephthalate, and a polyester obtained with 1,3-propanediol as the main glycol component can be used. However, it may contain a copolymerization component capable of forming other ester bonds at a ratio of 10 mol % or less. Examples of copolymerizable compounds include dicarboxylic acids such as isophthalic acid, cyclohexanedicarboxylic acid, adipic acid, dimer acid, and sebacic acid, while examples of glycol components include, but are not limited to, ethylene glycol, diethylene glycol, butanediol, neopentyl glycol, cyclohexanedimethanol, polyethylene glycol, and polypropylene glycol. In addition, titanium dioxide as a matting agent, fine particles of silica or alumina as a lubricant, hindered phenol derivatives as an antioxidant, coloring pigments, and the like can be added as necessary.
[0021] The PBT in the present invention is a PBT consisting of 90 mol % or more of tetramethylene terephthalate repeating units, and a polyester obtained with 1,4-butanediol as the main glycol component can be used. However, it may contain a copolymerization component capable of forming other ester bonds at a ratio of 10 mol % or less. Examples of copolymerizable compounds include dicarboxylic acids such as isophthalic acid, cyclohexanedicarboxylic acid, adipic acid, dimer acid, and sebacic acid, while examples of glycol components include, but are not limited to, ethylene glycol, propanediol, diethylene glycol, neopentyl glycol, cyclohexanedimethanol, polyethylene glycol, and polypropylene glycol. In addition, titanium dioxide as a matting agent, fine particles of silica or alumina as a lubricant, hindered phenol derivatives as an antioxidant, coloring pigments, and the like can be added as necessary.
[0022] In addition, the eccentric core-sheath composite fiber of the present invention is preferably a composite fiber in which at least one component constituting a single fiber is PTT and the other component is another polyester. That is, a combination of PTT and another polyester, or a combination of PTTs is preferable. The coil crimp property of the fiber is dominated by the stretch property of the high viscosity component with the low viscosity component as the fulcrum. Therefore, in order to obtain a coil crimp property of the fiber that can exhibit stretchability and bulkiness, the polymer used for the high viscosity component is required to have particularly high extensibility and recovery. PTT has mechanical properties and chemical properties equivalent to those of PET and PBT fibers, and has extremely excellent elongation recovery, and can exhibit good stretch performance.
[0023] The eccentric sheath-core composite fiber in the present invention means a fiber having an eccentric sheath-core composite cross section in which the composite cross section of a single fiber is composed of two types of polymers, the sheath component polymer B completely covers the core component polymer A, and the center of gravity of the core component is located at a position different from the center of the cross section of the single fiber. Specifically, it refers to a form as shown in Figure 1.
[0024] When such a fiber having an eccentric core-sheath type composite cross section is subjected to heat treatment or the like, the single fiber is significantly curved in accordance with the difference in shrinkage between the core and sheath components, and a coil-like crimp is generated, resulting in a fiber with elasticity.
[0025] The degree of this coiled crimp increases as the center-of-gravity distance, which is the distance between the center of gravity of the core component polymer A and the center of the cross section of the composite fiber, increases. In order to obtain a composite fiber having excellent bulkiness and stretchability, which is the objective of the present invention, it is preferable to have a thin-skinned eccentric core-sheath cross section that allows for a longer center-of-gravity distance.
[0026] The thin-skin eccentric sheath-core cross section referred to here means an eccentric sheath-core cross section that satisfies the following requirements. (A) The ratio S / D of the minimum thickness S of the sheath component covering the core component to the fiber diameter D of the single fiber is 0.01 to 0.10. (B) The perimeter portion having a thickness within 1.05 times the minimum thickness S accounts for 20% or more of the total perimeter of the cross section of a single fiber.
[0027] The fiber diameter D, the minimum thickness S of the sheath component, and the ratio S / D of the minimum thickness S of the sheath component to the fiber diameter D of the single fiber are determined as follows.
[0028] That is, the eccentric core-sheath composite polyester fibers are embedded in an embedding agent such as epoxy resin while remaining as a yarn bundle, and images of all the single fibers are taken of the cross section at a magnification such that 10 or more single fibers can be observed using a scanning electron microscope (SEM) or the like. For each image taken, the cross-sectional area Af of the single fiber is measured using image analysis software "WinROOF2015" manufactured by Mitani Shoji Co., Ltd., and the diameter of a perfect circle having the same area as this area Af is calculated, and the value is rounded off to one decimal place in μm to become the fiber diameter D in the present invention.
[0029] Furthermore, the minimum thickness S in the present invention is the value obtained by measuring the minimum thickness of the sheath component covering the core component using each image in which the fiber diameter D of the single fiber is measured. Furthermore, the fiber diameter D and minimum thickness S of the single fiber are measured in units of μm, and S / D is calculated for the same single fiber. The above operation is calculated for all single fibers to determine a simple number average value, which is then rounded off to two decimal places.
[0030] In the case of a side-by-side type composite cross section, the distance between the center of gravity of the core component polymer A and the center of the composite fiber cross section is large, so it has excellent stretchability. However, when creating differences in the crimp morphology between single fibers by changing the conjugation ratio between the single fibers, the cross-sectional shape of the single fiber changes with the change in conjugation ratio, making the spinnability and high-level processability unstable.
[0031] The eccentric core-sheath composite polyester fiber of the present invention must have a curvature of the composite interface of 15% or less. The curvature referred to here is calculated for all single fibers by the following procedures (A) to (C), a simple number average value is calculated, and the value is rounded off to the first decimal place, and indicates the degree of curvature of the composite interface between the core component polymer A and the sheath component polymer B. Hereinafter, an explanation will be given with reference to FIG. 2.
[0032] (A) Using each image in which the fiber diameter D of a single fiber was measured, a tangent line A was drawn to the most convex point a of the core contour on the side where the thickness of the sheath component is greatest on the contour of the core, which is the core-sheath composite interface. (B) Draw line B parallel to tangent line A, connecting the two points (point b-1, point b-2) where the inner diameter of the core is the largest. (C) Curvature rate (%) = (distance between lines A and B / fiber diameter) x 100 That is, the smaller the curvature ratio, the smaller the degree of curvature at the interface, and by setting the curvature ratio at 15% or less, a crimp with a large coil diameter is generated. If the curvature ratio exceeds 15%, the coil diameter becomes small, and sufficient bulkiness and stretchability cannot be obtained. The curvature ratio is preferably 0 to 10%, and more preferably 0 to 7%.
[0033] In the eccentric core-sheath composite fiber of the present invention, the composite area ratio of the core component to the sheath component must be in the range of 80:20 to 20:80. If it is outside this range, the spinnability and stretchability will be insufficient. The range is preferably 70:30 to 30:70.
[0034] The composite area ratio referred to here is calculated as follows: For each image in which the fiber diameter D of the single fiber was measured, the composite area ratio (%) of each component was calculated using image analysis software "WinROOF2015" manufactured by Mitani Shoji Co., Ltd., and the value obtained by rounding off to the first decimal place was determined as the composite area ratio in the present invention.
[0035] The eccentric core-sheath conjugated polyester fiber of the present invention has three or more groups of single fibers having different conjugated area ratios. For example, as shown in Fig. 3, in a multifilament, there are three or more groups of single fibers having different conjugated area ratios of two polymer components constituting the conjugated fiber.
[0036] The monofilament group referred to here is classified based on the composite area ratio, i.e., the crimp morphology. However, since there is no significant difference in the crimp morphology when the composite area ratios are approximately the same, the classification is performed in the following steps (A) to (C). (A) All single fibers are arranged in ascending order of the area ratio of the core component, and those fibers whose area ratio differs by 5% or less based on the smallest area ratio are considered to be in one group. (B) The next group is classified in the same manner based on the single fiber with the smallest area ratio among the single fibers excluding the single fibers of the above group. (C) The following groups are further classified in the same manner as (B): If there are less than three types, the number of single fiber groups with different crimp morphologies is small, so that the fabric made from the fibers is unlikely to be bulky, and further the surface quality is reduced due to crimping, etc. In order to make the effects of the present invention more pronounced, four or more types, preferably five or more types, are used.
[0037] In the eccentric core-sheath composite polyester fiber of the present invention, the ratio of the number of single fibers in each single fiber group to the total number of single fibers is preferably less than 50%. When there is a single fiber group with a ratio of the number of single fibers of 50% or more to the total number of single fibers, the number of single fibers with the same crimp phase will be more than half, so when made into a fabric, it is difficult to achieve bulkiness, and further the surface quality will be reduced due to crimping, etc. It is preferably less than 40%, more preferably less than 30%.
[0038] The eccentric core-sheath composite polyester fiber of the present invention preferably has a CV value of the curvature of the composite interface of 0.40 or less. The CV value of the curvature referred to here is a value obtained by calculating the curvatures of all single fibers, dividing the standard deviation by the average value, and rounding off to two decimal places. If the CV value exceeds 0.40, the bulkiness improvement and crimping elimination effects due to the difference in crimp morphology produced by single fiber groups with different composite area ratios are not fully exhibited. More preferably, it is 0.20 or less.
[0039] The eccentric core-sheath composite polyester fiber of the present invention preferably has a single fiber fineness of 0.3 to 7.0 dtex. If the single fiber fineness is less than 0.3 dtex, the crimp becomes too fine, resulting in insufficient bulkiness and stretchability. If the single fiber fineness is more than 7.0 dtex, the softness decreases and wearing comfort is poor. From the viewpoints of bulkiness, stretchability and softness, the single fiber fineness is more preferably 1.0 to 5.0 dtex.
[0040] The eccentric sheath-core composite polyester fiber of the present invention preferably has a certain level of toughness or higher in consideration of processability in advanced processing and practical use after processing into a fabric, and the strength and elongation at break of the fiber are preferably as follows.
[0041] The strength is the value obtained by dividing the load value at break by the fineness when the load-elongation curve of the fiber is obtained under the conditions specified in JIS L1013 (2010), and the elongation is the value obtained from the elongation at the point showing the maximum strength. Here, the fineness means the value calculated as the weight per 10,000 m from the simple average value obtained by measuring the weight of a unit length of the fiber multiple times.
[0042] The strength and elongation referred to here are preferably adjusted by controlling the conditions of the production process described below depending on the intended use, etc., but the preferred ranges for the eccentric core-sheath composite polyester fiber of the present invention are a strength of 0.5 to 10.0 cN / dtex and an elongation of 5 to 700%.
[0043] When the eccentric core-sheath composite polyester fiber of the present invention is used for general clothing applications such as innerwear and outerwear, the strength is preferably 1.0 to 4.0 cN / dtex and the elongation is preferably 20 to 40%. For sports clothing applications in harsh environments, the strength is preferably 3.0 to 5.0 cN / dtex and the elongation is preferably 10 to 40%.
[0044] The eccentric core-sheath composite polyester fiber of the present invention can be used alone, but is preferably used in combination with a cellulose fiber such as rayon or cupra, or in combination with wool, since this can impart moisture absorption / release properties and heat retention, thereby improving wearing comfort.
[0045] The form of the fabric of the present invention can be appropriately selected depending on the purpose, such as woven fabric, knitted fabric, nonwoven fabric, and even cushioning material, and can be suitably used for shirts, blouses, pants, suits, blousons, etc.
[0046] Next, a preferred method for producing the eccentric core-sheath composite polyester fiber of the present invention will be described. The eccentric sheath-core composite fiber of the present invention is prepared by combining two types of polyester components, polyester A as the core component and polyester B as the sheath component, above the nozzle hole using a spinneret to form an eccentric sheath-core composite flow, which is then discharged from the round nozzle hole so as to have a circular cross section. The discharged yarn is cooled and solidified, and may be produced by a two-step method in which it is taken up and then drawn, or it may be produced by a direct spinning-drawing method in which it is drawn as is after being spun and drawn.
[0047] Furthermore, in order to stably produce the eccentric core-sheath composite fiber of the present invention, the intrinsic viscosity of each component and the intrinsic viscosity difference between the components are important. Even composite fibers are not practical if the viscosity of one component is too low to allow fiber formation, or conversely, is too high, requiring a special spinning device. In addition, the viscosity difference between the components determines the degree of bending of the yarn immediately below the nozzle hole, which greatly affects spinnability. For this reason, it is preferable that the intrinsic viscosity IV of each component be combined to satisfy the following formula: 0.30X≦Y≦0.45X+0.30 0.80≦X≦2.00, 0.45≦Y Where, X is the intrinsic viscosity IV of the core component polyester A, and Y is the intrinsic viscosity IV of the sheath component polyester B. In the case of conjugate spinning, it is preferable to set the intrinsic viscosity IV of the sheath component polyester B to 0.45 or more in order to obtain stable spinnability. More preferably, Y≧0.50. To obtain even better stretchability, Y≦0.70 is preferable. On the other hand, in order to achieve stable melt extrusion, the intrinsic viscosity IV of the core component polyester A is preferably in the range of 0.80 to 2.00, more preferably 1.10 to 1.70.
[0048] In addition, as a combination of the intrinsic viscosities of the two components, a value of Y greater than Y=0.30X is preferable because it prevents the spun yarn from bending excessively toward the high-viscosity component and enables stable spinning over a long period of time, whereas a value of Y smaller than Y=0.45X+0.30 is preferable because it provides excellent stretchability.
[0049] In order to control the curvature and curvature CV value of the composite interface within the above ranges in the eccentric sheath-core composite fiber of the present invention even if the composite area ratio is not 50:50, it is important to use a distribution plate having distribution holes as exemplified in FIG. 4 and to use a spinneret incorporating a metering plate and a discharge plate in which holes with different pressure losses are drilled according to the desired number of single filament groups.
[0050] The distribution plate referred to here is one which is exemplified in JP-A-2011-174215, JP-A-2011-208313, and JP-A-2012-136804 and which is capable of precisely controlling the distance between the center points of gravity in the cross section of each of the constituent single fibers.
[0051] In the method using such a distributor plate, the cross-sectional form of the single fiber can be controlled by the arrangement of the distribution holes in the final distributor plate, which is the most downstream of the multiple distributor plates. That is, the cross-sectional form can be controlled by the arrangement of the distribution holes of the core component polymer A and the sheath component polymer B. Specifically, as illustrated in FIG. 4, the distribution holes 4-(b) of the sheath component polymer B are arranged so as to surround the distribution holes 4-(a) of the core component polymer A in the eccentric sheath-core composite cross section, thereby making it possible to form the eccentric sheath-core composite cross section required in the present invention. In addition, by arranging 4-(b) so as to thinly surround 4-(a), the thin-skinned eccentric sheath-core cross section preferably used in the present invention can be achieved. Furthermore, since the polymer flow rate can be changed by changing the hole diameter of the distribution holes, the hole diameter of the distribution holes forming the core and sheath components can be designed based on the viscosity to change the curvature to a desired value, and by combining it with a metering plate and a discharge plate having holes with different pressure losses, it becomes possible to control the curvature, curvature CV value, and composite area ratio for each single fiber.
[0052] The spinning temperature is preferably 245 to 270°C for PTT or PBT, and 265 to 290°C for PET. If necessary, a 2 to 20 cm heating cylinder, an MO (monomer, oligomer) suction device, or an inert gas generator such as air, steam, or N2 may be installed below the nozzle.
[0053] The range in which the eccentric core-sheath composite polyester fiber of the present invention can be stably discharged when being spun can be, for example, 0.1 g / min / hole to 20.0 g / min / hole per discharge hole, and it is preferable to determine the range according to the desired fiber diameter while taking into consideration the winding conditions, draw ratio, etc.
[0054] The composite polymer stream discharged from the composite spinneret with precisely controlled discharge rate and cross section is cooled and solidified by cooling air whose speed and temperature are kept constant. The speed and temperature of the cooling air may be determined taking into consideration the cooling efficiency of the yarn and the stabilization of the solidification point atmosphere.
[0055] The cooled and solidified yarns are simultaneously bundled and oiled. The oiling method, amount, and type of oil to be used may be determined taking into consideration winding conditions, advanced processing, processability, etc. Furthermore, to promote uniform application of the oil, slight intertwining may be imparted using an interlace nozzle, etc.
[0056] The yarn to which the oil has been applied is taken up by a roller having a specified peripheral speed. The take-up speed may be determined based on the discharge rate, the desired fiber diameter, the advanced processing process, etc., but is preferably in the range of 100 to 7000 m / min in order to stably produce the eccentric core-sheath composite polyester fiber of the present invention. From the viewpoint of achieving high orientation and improving mechanical properties, drawing may be performed after winding once, or drawing may be performed continuously without winding once.
[0057] As the stretching conditions, for example, in a stretching machine consisting of one or more pairs of rollers, the fiber is stretched reasonably in the fiber axis direction by a peripheral speed ratio of a first roller set at a temperature between the glass transition temperature and the melting point and a second roller set at a temperature equivalent to the crystallization temperature, and then the fiber is heat-set and wound up. From the viewpoint of increasing the stretch ratio and improving the mechanical properties, it is also preferable to carry out this stretching process in multiple stages.
[0058] The eccentric sheath-core composite polyester fiber of the present invention produced as described above can be made into a fiber product such as a woven or knitted fabric, and then heat-treated to cause crimping of the single fiber, thereby exerting the effects of the present invention.
[0059] In this case, from the viewpoint of actualizing the crimping of each single fiber, it is preferable to determine the heat treatment temperature from the range of (Tg+10) to (Tg+100°C) based on the glass transition temperature Tg of the polymer having the higher glass transition temperature Tg of the two polymers used.
[0060] Furthermore, in the heat treatment step, in order to favorably develop crimp in the single fibers, it is preferable to carry out a relaxation heat treatment in which the heat treatment is carried out in a state in which no tension is applied to the yarn bundle.
[0061] In the present invention, by setting the heat treatment conditions as described above, all of the single fibers in the yarn bundle can exhibit good crimping, and a fabric can be provided that has the desired refined surface quality free of grain and wrinkles, as well as excellent bulkiness and stretchability. EXAMPLES
[0062] The eccentric core-sheath composite polyester fiber of the present invention will be described in detail below with reference to examples. The examples and comparative examples were evaluated as follows.
[0063] (1) Intrinsic viscosity IV The definition formula for ηr is as follows: 0.8 g of sample polymer was dissolved in 10 mL of o-chlorophenol (hereinafter abbreviated as OCP) with a purity of 98% or higher at 25°C, and the relative viscosity ηr was calculated using an Ostwald viscometer at 25°C according to the following formula to calculate the intrinsic viscosity (IV). For PTT, 0.8 g of sample polymer was dissolved in 10 mL of OCP with a purity of 98% or higher at 160°C, and after cooling to 25°C, the relative viscosity ηr was calculated using an Ostwald viscometer according to the following formula to calculate the intrinsic viscosity IV. ηr=η / η0=(t×d) / (t0×d0) Intrinsic viscosity IV=0.0242ηr+0.2634 Here, η is the viscosity of the polymer solution, η0 is the viscosity of the OCP, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0: OCP fall time (sec), d0: OCP density (g / cm 3 ).
[0064] (2) Total fineness of multifilament The weight of 100 m of the polyester fiber to be evaluated was measured, and the fineness was calculated by multiplying it by 100. This was repeated 10 times, and the simple average value was rounded off to the first decimal place to determine the fineness.
[0065] (3) Fiber strength and breaking elongation The fiber samples were measured using a tensile tester (Orientec's "TENSILON" UCT-100) under the constant-speed elongation conditions specified in JIS L1013 (2010) 8.5.1 standard time test. The gripping distance was 20 cm, the pulling speed was 20 cm / min, and the number of tests was 10. The elongation was calculated from the elongation at the point showing the maximum strength on the tensile strength-elongation curve of the fiber. The strength was calculated by dividing the maximum strength by the total fineness.
[0066] (4) Fabric manufacturing method A plain weave fabric was produced using eccentric core-sheath composite polyester fibers for the weft and warp threads with a weft density of 90 threads / 2.54 cm. The fabric was scoured at 80°C for 20 minutes, relaxed at 120°C for 20 minutes, and then set at 180°C for 1 minute.
[0067] (5) Fabric evaluation (bulkiness) The bulkiness of the woven fabric samples prepared above was evaluated by 10 experts through a sensory evaluation, with 4 points for ◎, 2 points for ◯, 1 point for △, and 0 points for ×, with a total score of 30 or more being ◎, ◯ for 20 to 29 points, △ for 10 to 19 points, and × for 0 to 9 points. The pass level is △ or higher. The conventional product below refers to a side-by-side type composite fiber that does not use a distribution plate consisting of a single fiber group with a composite area ratio of a single fiber group as described in Patent Document 2. ◎: Better than conventional products. 〇: Slightly better than conventional products. △: Same level as conventional products. ×: Inferior to conventional products.
[0068] (6) Fabric evaluation (stretchability) Stretchability was evaluated by a sensory assessment that took into account the stretch-back property as well as the appropriate firmness and resilience, with ◎ being 4 points, 〇 being 2 points, △ being 1 point, and × being 0 points, with a total score of 30 or more being ◎, 20-29 points being 〇, 10-19 points being △, and 0-9 points being ×. The pass level is △ or above. ◎: Better than conventional products. 〇: Slightly better than conventional products. △: Same level as conventional products. ×: Inferior to conventional products.
[0069] (7) Fabric evaluation (surface quality) The surface quality was evaluated sensorily for the presence or absence of grain and wrinkles, with ◎ being given 4 points, 〇 being given 2 points, △ being given 1 point, and × being given 0 points. A total score of 30 or more was ◎, 20-29 points was 〇, 10-19 points was △, and 0-9 points was ×. The pass level was △ or above. ◎: High quality with no grain or wrinkles. Good: Almost no grain or wrinkles, good quality. △: There are some grains and wrinkles, but the quality is not affected. ×: Grains and wrinkles are clearly visible, low quality.
[0070] [Example 1] The eccentric core-sheath composite polyester fiber was made of all single fibers, of which the core component was PTT with an intrinsic viscosity IV of 1.38 and containing 0.35% by weight of titanium oxide as a matting agent, and the sheath component was PET with an intrinsic viscosity IV of 0.51 and containing 0.35% by weight of titanium oxide.
[0071] In Example 1, a spinneret was used that incorporated a distribution plate having distribution holes as shown in Fig. 4, and a metering plate and a discharge plate that had three types of holes with different pressure losses drilled therein so that the core:sheath combined area ratios were 35:65, 50:50, and 65:35. After the polymers were individually melted, they were metered by a pump so that the total core:sheath area ratio was 50:50, and the polymers were allowed to flow into the spinneret and discharged at a spinning temperature of 270°C.
[0072] The distributor plate used in Example 1 is such that, when composite fibers are made, a portion of the polymer of component B covering component A becomes uniform, forming a composite cross section (Fig. 1) that satisfies the requirements for an eccentric core-sheath cross section in the present invention. All of the nozzle holes have a round shape (irregularity degree 1.00), and 24 nozzle holes with a hole diameter of 0.40 mm are drilled, and a spinneret was used in which three types of nozzle holes with different composite area ratios are randomly arranged on the spinneret surface in groups of 8 holes each.
[0073] The discharged composite polymer stream was cooled, and then an oil was added thereto. The stream was then wound up at a speed of 1000 m / min to obtain an undrawn yarn having 170.0 dtex-24 filaments.
[0074] The wound undrawn yarn was drawn 3.0 times at a drawing speed of 600 m / min between rollers heated to 70° C. and 130° C. to obtain an eccentric core-sheath composite polyester fiber of the present invention having 56.0 dtex-24 filaments.
[0075] The obtained eccentric core-sheath bicomponent polyester fiber had sufficient mechanical properties for practical use, with a single fiber fineness of 2.3 dtex, strength of 3.5 cN / dtex, and elongation of 31%, and the curvature of the composite interface was 5%, and the curvature CV value was 0.10. Furthermore, when the cross section of the multifilament (yarn bundle) was observed, it was found to be composed of three types of single fiber groups with different composite area ratios in the yarn bundle, with the composite area ratios of core:sheath for the first group being 33:67 to 37:63, for the second group being 48:52 to 52:48, and for the third group being 63:37 to 67:33.
[0076] When the eccentric core-sheath composite polyester fiber was made into a fabric and subjected to a heat treatment, each single fiber crimped according to its composite state, creating gaps in the yarn bundle and providing good bulkiness. Furthermore, because the curvature was small, each single fiber effectively crimped, providing good stretchability. The surface quality was also good, with almost no grain or wrinkles.
[0077] [Example 2] In Example 2, eccentric core-sheath composite polyester fibers of the present invention were obtained in the same manner as in Example 1, except that the hole diameter of the distributor plate was changed to give the curvature ratio shown in Table 1.
[0078] The fabric made of the obtained eccentric core-sheath composite polyester fiber showed a slight decrease in stretchability due to the increased curvature, but had good bulkiness. In addition, the surface quality was good with almost no grain or wrinkles.
[0079] [Example 3] In Example 3, eccentric core-sheath composite polyester fibers of the present invention were obtained in the same manner as in Example 1, except that a metering plate and a discharge plate with changed pressure loss were used so that the core:sheath composite area ratios were 40:60, 50:50, and 60:40.
[0080] The fabric made of the obtained eccentric core-sheath composite polyester fiber showed a slight decrease in bulkiness due to the smaller difference in the composite area ratio between the core and the sheath, but had good stretchability. In addition, the surface quality was good with almost no grain or wrinkles.
[0081] [Example 4] In Example 4, eccentric core-sheath composite polyester fibers of the present invention were obtained in the same manner as in Example 1, except that a metering plate and a discharge plate with changed pressure loss were used so that the core:sheath composite area ratios were 30:70, 50:50, and 70:30.
[0082] The fabric made of the obtained eccentric core-sheath composite polyester fiber had a large difference in the composite area ratio between the core and the sheath, so it had good bulkiness and good stretchability. In addition, the surface quality was good with almost no grain or wrinkles.
[0083] [Example 5] In Example 5, an eccentric core-sheath composite polyester fiber of the present invention was obtained in the same manner as in Example 1, except that a metering plate and a discharge plate were used in which three types of holes with different pressure losses, 6, 12, and 6 holes, respectively, were drilled so that the ratio of the number of single fibers in each single fiber group to the total number of single fibers was 25% for the first group, 50% for the second group, and 25% for the third group.
[0084] The fabric made of the obtained eccentric core-sheath composite polyester fiber had a reduced bulkiness and surface quality due to the presence of single yarn groups in which the ratio of the number of single fibers to the total number of single fibers was 50%, but the stretchability was good.
[0085] [Example 6] In Example 6, an eccentric core-sheath composite polyester fiber of the present invention was obtained in the same manner as in Example 1, except that a metering plate and a discharge plate having four types of holes with different pressure losses were used so that the core:sheath composite area ratios were 35:65, 45:55, 55:45, and 65:35.
[0086] The fabric made of the eccentric core-sheath composite polyester fiber had excellent surface quality without crimps or wrinkles because the interlocking of the single fibers was suppressed by increasing the number of single fiber groups and decreasing the ratio of the number of single fibers in each single fiber group to the total number of single fibers. In addition, the fabric had good bulkiness and stretchability.
[0087] [Example 7] In Example 7, an eccentric core-sheath composite polyester fiber of the present invention was obtained in the same manner as in Example 1, except that a metering plate and a discharge plate each having holes with different pressure losses were used so that the single fiber groups were evenly distributed in a core:sheath composite area ratio in the range of 40:60 to 60:40.
[0088] The fabric made of the obtained eccentric core-sheath composite polyester fiber had excellent surface quality without crimps or wrinkles due to the increase in the number of single fiber groups and the decrease in the ratio of the number of single fibers in each single fiber group to the total number of single fibers. The bulkiness was slightly decreased due to the decrease in the difference in the composite area ratio between the core and sheath, but the stretchability was good.
[0089] [Examples 8 and 9] In Examples 8 and 9, eccentric core-sheath composite polyester fibers of the present invention were obtained in the same manner as in Example 7, except that the hole arrangement of the distributor plate was changed so as to obtain the curvature CV values shown in Table 2.
[0090] The fabric made of the eccentric core-sheath composite polyester fiber obtained in Example 8 showed a decrease in the difference in crimp morphology between the individual single fiber groups due to an increase in the curvature CV value, and a slight decrease in bulkiness was observed, but the stretchability was good and the surface quality was good with almost no crimps or wrinkles. The fabric obtained in Example 9 showed a further decrease in bulkiness due to an increase in the curvature CV value, but the stretchability was good. In addition, the surface quality had some crimps and wrinkles, but there were no problems with the quality.
[0091] [Examples 10 and 11] In Examples 10 and 11, eccentric core-sheath composite polyester fibers of the present invention were obtained in the same manner as in Example 1, except that the number of nozzle holes in the spinneret was 72 and 12, respectively.
[0092] The fabric made of the eccentric core-sheath composite polyester fiber obtained in Example 10 exhibited reduced bulkiness and stretchability due to a small single fiber fineness, but had good surface quality with almost no crimps or wrinkles. The fabric obtained in Example 11 exhibited improved bulkiness and stretchability due to a large single fiber fineness, and had good surface quality with almost no crimps or wrinkles.
[0093] [Example 12] In Example 12, the core component polymer was changed to PBT (intrinsic viscosity 1.30), and the same spinneret as in Example 1 was used. The spinning conditions and draw ratio were set so that the elongation would be 30 to 40%, and an eccentric core-sheath composite polyester fiber of the present invention was obtained.
[0094] The fabric made of the obtained eccentric core-sheath composite polyester fiber had soft stretchability due to the polymer properties of PBT, good bulkiness, and good surface quality with almost no grain or wrinkles.
[0095] [Comparative Example 1] In Comparative Example 1, an eccentric core-sheath composite polyester fiber was obtained in the same manner as in Example 1, except that the hole diameter of the distribution plate was changed to obtain the curvature ratio shown in Table 1.
[0096] The fabric made of the obtained eccentric core-sheath composite polyester fiber had a smaller coil diameter due to an increase in the curvature, so the bulkiness was reduced and the stretchability was poor. The surface quality was good with almost no grain or wrinkles.
[0097] [Comparative Example 2] In Comparative Example 2, an eccentric core-sheath composite polyester fiber was obtained in the same manner as in Example 1, except that a metering plate and a discharge plate having only holes with the same pressure loss were used.
[0098] The fabric made of the obtained eccentric core-sheath composite polyester fiber had good stretchability, but since all the single fibers formed crimps of the same size, the fabric generally converged, and the fabric was inferior in bulkiness and surface quality.
[0099] [Comparative Example 3] In Comparative Example 3, an eccentric core-sheath composite polyester fiber of the present invention was obtained in the same manner as in Example 1, except that a metering plate and a discharge plate whose pressure loss was changed so that the core:sheath composite area ratio was 40:60 and 60:40 were used.
[0100] The fabric made of the obtained eccentric core-sheath composite polyester fiber had good stretchability, but due to the decrease in the number of single fiber groups and the increase in the ratio of the number of single fibers in each single fiber group to the total number of single fibers, the single fibers interlocked with each other, and the bulkiness was reduced to a level that did not impair the object of the present invention, but the surface quality was poor.
[0101] [Table 1]
[0102] [Table 2] [Explanation of symbols]
[0103] A: Core B: Scabbard part D: Fiber diameter S: Minimum thickness of sheath component 4-(a): Distribution hole of core component polymer A 4-(b): Distribution hole of sheath component polymer B
Claims
1. The multifilament is made of eccentric sheath-core conjugated fibers composed of polyester components having different intrinsic viscosities, and in the composite cross section of a single fiber, the curvature of the composite interface is 15% or less, the composite area ratio of the core component to the sheath component is in the range of 80:20 to 20:80, and the eccentric sheath-core conjugated polyester fiber is composed of three or more types of single fiber groups having different composite area ratios.
2. 2. The eccentric core-sheath composite polyester fiber according to claim 1, wherein the ratio of the number of single fibers in each single fiber group to the total number of single fibers is less than 50%.
3. 2. The eccentric core-sheath composite polyester fiber according to claim 1, wherein a CV value of a curvature of the composite interface is 0.40 or less.
4. The eccentric core-sheath composite polyester fiber according to any one of claims 1 to 3, wherein the single fiber fineness is 0.3 to 7.0 dtex.
Citation Information
Patent Citations
Randomly crimped yarn
JP1997041233A
Bulky polyester conjugated yarn
JP2008075224A
Eccentric core-sheath composite fibers
JP2021055231A
Polyurethane-nylon 6 eccentric sheath-core conjugate fiber
WO2018235754A1
Production of elastic woven fabric
JP1992308271A