Cation exchange membrane, ion exchange membrane cell and electrodialysis device
A cation exchange membrane with a water content of 0.05 to 0.2 and specific resin structure addresses the lack of selectivity for ammonium ions, enhancing ion concentration efficiency and reducing energy consumption and scale formation.
Patent Information
- Application Number
- JP2023055386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cation exchange membranes lack selectivity for specific cations, particularly ammonium ions, and suffer from high membrane resistance, leading to inefficient energy consumption and scale formation during ion concentration processes.
A cation exchange membrane with a water content of 0.05 to 0.2, composed of a cation exchange resin with a specific structure, such as sulfonated polyether sulfone or sulfonated styrene-divinylbenzene copolymer, exhibits high permselectivity for ammonium ions and low membrane resistance.
The membrane effectively concentrates ammonium ions while minimizing energy consumption and reducing scale formation, achieving selective permeability and low resistance.
Smart Images

Figure 2024142959000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cation exchange membrane having a water content of 0.05 to 0.2, and an ion exchange membrane cell and an electrodialysis device using the cation exchange membrane. [Background technology]
[0002] There are several techniques for concentrating and separating ions in wastewater, including distillation, ion exchange and adsorption, reverse osmosis (RO), forward osmosis (FO), brine concentration (BC), electrodialysis (ED), and Donnan dialysis. Among these, distillation can handle a wide range of salt concentrations and water qualities, and has excellent resistance to contamination, but it requires a large amount of energy and is not suitable for treating dilute solutions. Various ion exchangers and adsorbents have been developed for ion exchange and adsorption, but continuous operation is difficult because a regeneration process is required for the ion exchange material and adsorbent, and equipment and chemicals are required to regenerate the ion exchange material and adsorbent, making it unsuitable for continuous treatment. In the RO membrane method, ions are concentrated by applying a pressure higher than the osmotic pressure to the wastewater to dehydrate it, so concentration from a dilute solution requires high electricity costs. In addition, membrane cleaning and replacement are required frequently for wastewater containing membrane pollutants. In addition, concentration of high salt concentrations is difficult due to the pressure limit of the membrane. In the FO membrane method, ions are concentrated by dehydration, just like in the RO membrane method. The use of a driving force solute (DS) has the advantage of eliminating the need for pressure and electricity, but otherwise has the same problems as the RO membrane. The Brine Concentration (BC) method can concentrate salts to higher concentrations than the RO membrane by connecting FO membrane modules in series in multiple stages, but it requires a larger membrane area than the RO membrane method because part of the concentrated liquid is refluxed. The Donnan dialysis method uses DS to concentrate and separate ions like the FO membrane method, so it does not require electricity, but it is necessary to separate the DS and the target ions. As mentioned above, each method has its own advantages and disadvantages, but since actual treated water contains not only impurities but also various ions, with the exception of the ion exchange method, there are problems with scale formation due to these ions and reduced energy efficiency for concentrating the desired ions.
[0003] The ED method is a technology for concentrating and desalination of ions using an ion exchange membrane. In the case of the concentration process, ions are moved and concentrated, so it is particularly effective in separating and concentrating membrane foulants and specific trace ions. Although high-concentration salt treatment requires electricity, it is a technology that allows high-concentration treatment like the BC method. However, in the ED method, ions other than the target ions are also concentrated at the same time. In this case, when divalent cations such as calcium ions are concentrated, scale is generated in the membrane, on the membrane surface, or in the solution flow path, leading to membrane destruction and a decrease in system efficiency. Therefore, in order to prevent scale generation due to calcium ions, etc., it has been proposed to use a cation exchange membrane that is selectively permeable to monovalent cations (see Patent Document 1). However, when a cation of the same valence as the target ion, for example, a monovalent ammonium ion, is targeted, if a monovalent ion such as sodium ion or potassium ion is present, electricity is consumed to concentrate the ions other than the target ion, so there is a problem that the energy efficiency of separating and concentrating the target ion is reduced. Conventionally, no cation exchange membrane has been proposed that is excellent not only in selectivity between a specific target cation and cations of different valences, but also between cations of the same valence. Therefore, there has been a demand for the development of a cation exchange membrane that selectively allows the passage of specific target cations, such as ammonium ions.
[0004] Among cations, the separation and concentration of ammonium ions in particular has attracted attention, for the following reasons. Currently, nitrogen compounds in waste gases and wastewater are detoxified by spending a great deal of energy. However, there are cases where nitrogen compounds are released without being treated, or where the treatment is insufficient, which has a large impact on the environment. Therefore, there is a demand for the development of resource ammoniaization technology for nitrogen compounds in wastewater that will realize the detoxification and resource recovery (Clean Earth) of these harmful nitrogen compounds derived from human activities. For this reason, focusing on nitrogen compounds in wastewater, technology is being developed to convert them into ammonia (including ammonium ions) and concentrate them to make them into a form that can be used as a valuable resource (resource ammonia). Among these technologies, the separation and concentration of ammonium ions present in wastewater in an energy-saving manner has attracted attention. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-268337 A Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a cation exchange membrane having high selectivity for specific cations, particularly ammonium ions, and further to provide a cation exchange membrane having high selectivity for specific cations, particularly ammonium ions, and low membrane resistance. [Means for solving the problem]
[0007] The present inventors began to study cation exchange membranes with high selectivity for specific cations, and proceeded with the study of cation exchange membranes with high selective permeability for ammonium ions as the specific cation of interest. Conventionally, methods for increasing the ion selectivity of cation exchange membranes have been performed by forming an oppositely charged layer on the membrane surface, forming a dense layer on the membrane surface, and the like (see Patent Document 1). For example, when a polymer cation layer (positively charged layer) is formed on the surface of a cation exchange membrane, a cation exchange membrane that selectively passes monovalent cations is obtained because divalent cations such as Ca and Mg have a greater electrostatic repulsion with this positively charged layer (oppositely charged layer) than monovalent cations such as Na and K. However, selective permeability such as selectively passing ammonium ions among monovalent cations was not obtained. On the other hand, in a membrane with a dense layer formed on the membrane surface, the permeability of ions with large hydrated ion radius such as Ca and Mg is suppressed more than that of ions with small hydrated ion radius such as Na and K. However, a practical membrane was not obtained because the reduction in ion permeability of Na, K, etc. was also large. The present inventors have been studying whether a cation exchange membrane having selective permeability can be obtained by a method completely different from the conventional method, and have found that selectivity for ammonium ions is expressed by setting the water content of the cation exchange membrane to a specific water content. It was not known at all in the past that the water content of a cation exchange membrane affects the selectivity for ammonium ions. Furthermore, the specific water content found by the present inventors was a low water content at a level that would not be considered for a normal cation exchange membrane. Furthermore, the cation exchange membrane developed by the present inventors had low membrane resistance despite its low water content. The present invention was thus completed.
[0008] That is, the present invention is specified by the following items. [1] A cation exchange membrane having a water content of 0.05 to 0.2, as calculated by the following formula (A): W = (W 2 -W 1 ) / W 1 (A) (In formula (A), W is the water content, W 2 is the wet weight, W 1is the dry weight.) [2]NH 4 NH with Cl concentration of 0.5 mol / L 4 The membrane resistance in a Cl solution at 25°C is 2.0 Ωcm 2 The cation exchange membrane according to the above [1], [3] The cation exchange membrane according to [1] or [2] above, which is a cation exchange membrane for concentrating ammonium ions. [4] The cation exchange membrane according to the above [1] or [2], wherein the cation exchange resin constituting the cation exchange membrane is an aromatic hydrocarbon-based resin having a cation exchange group introduced therein. [5] The cation exchange membrane according to [4] above, wherein the cation exchange resin constituting the cation exchange membrane is a sulfonated polyethersulfone or a sulfonated styrene-divinylbenzene copolymer. [6] An ion exchange membrane cell in which an anion exchange membrane and the cation exchange membrane described above in [1] or [2] are arranged opposite each other. [7] An electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane and an anion exchange membrane, wherein the cation exchange membrane is the cation exchange membrane of [1] or [2] above. Effect of the Invention
[0009] The cation exchange membrane of the present invention has excellent selective permeability to specific cations, particularly ammonium ions. The cation exchange membrane of the present invention also has excellent selective permeability to specific cations, particularly ammonium ions, and low membrane resistance. The ion exchange membrane cell of the present invention can be used in an apparatus for electrodialysis or the like to selectively concentrate specific cations, particularly ammonium ions. The electrodialysis apparatus of the present invention can selectively concentrate specific cations, particularly ammonium ions. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of the use of the ion exchange membrane cell of the present invention. [Diagram 2] FIG. 2 is a diagram showing the measuring device and measuring conditions for the membrane resistance used in the examples and comparative examples. [Diagram 3] FIG. 3 is a diagram showing an electrodialysis test apparatus used in the examples and comparative examples. [Figure 4] FIG. 4 is a photograph of the membrane produced in Example 1. [Diagram 5] FIG. 5 shows the results of an electrodialysis test using the membrane prepared in Example 1. [Figure 6] FIG. 6 shows the results of an electrodialysis test using the membrane prepared in Example 2. [Figure 7] FIG. 7 is a diagram showing the results of an electrodialysis test using the membrane prepared in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The cation exchange membrane of the present invention has a structure in which W=(W 2 -W 1 ) / W 1 The moisture content is 0.05 to 0.2. Here, W represents the moisture content, and W 1 represents the dry mass, and W 2 represents the wet mass. Wet mass (W 2 The dry mass (W) was measured after the Na-type cation exchange membrane was fully equilibrated in water. 1 ) is the mass at which further drying operation will only change the mass within the range of measurement error. The cation exchange membrane of the present invention has an excellent selective permeability to ammonium ions because the water content of the cation exchange membrane is in the specific range of 0.05 to 0.2. From the viewpoint of achieving a better selective permeability to ammonium ions, the water content of the cation exchange membrane of the present invention is preferably 0.09 to 0.17, and more preferably 0.10 to 0.15. From the viewpoint of reducing the energy consumption when concentrating ammonium ions by electrodialysis, the cation exchange membrane of the present invention has an NH 4 NH with Cl concentration of 0.5 mol / L 4 The membrane resistance in Cl solution is 2.0Ωcm 2 It is preferable that the resistance is 0.2 to 1.1 Ωcm or less. 2 More preferably, the resistance is 0.3 to 0.9 Ωcm. 2The cation exchange membrane of the present invention has excellent selective permeability to ammonium ions, and is therefore suitable as a cation exchange membrane for concentrating ammonium ions, which is used for concentrating ammonium ions using an electrodialysis (ED) device or the like.
[0012] The cation exchange membrane of the present invention is composed of a cation exchange resin or a cation exchange resin and a support. The cation exchange resin in the present invention is not particularly limited as long as it is a resin having cation exchange ability, but for example, an aromatic hydrocarbon resin having an aromatic ring in the main chain or side chain and a structure in which a cation exchange group is introduced into the aromatic ring can be mentioned. The hydrocarbon resin having an aromatic ring in the main chain is not particularly limited as long as it is a resin to which a cation exchange group can be introduced, but for example, polysulfone, polyphenylene sulfide, polyether ketone, polyether ether ketone, polyether imide, polyphenylene oxide, polyether sulfone, polybenzimidazole, etc. can be mentioned, and the resin having an aromatic ring in the side chain can be polystyrene, a copolymer of styrene and other monomers, and further a resin obtained by cross-linking copolymerization of these with divinylbenzene, etc. can be mentioned. The cation exchange group is a functional group that can become positively charged in an aqueous solution, and the cation exchange group is not particularly limited, but examples thereof include sulfonic acid groups, carboxylic acid groups, and phosphonic acid groups, and the strongly acidic sulfonic acid group is preferably mentioned. Examples of the cation exchange resin in the present invention include sulfonated polyethersulfone in which a sulfonic acid group is introduced into polyethersulfone, a polymer in which styrene and divinylbenzene are cross-linked copolymerized, or a polymer in which styrene, another monomer, and divinylbenzene are cross-linked copolymerized, and sulfonated styrene-divinylbenzene copolymer in which a sulfonic acid group is introduced into the styrene-divinylbenzene copolymer, and the like, and specific examples of the sulfonated styrene-divinylbenzene copolymer include sulfonated styrene-divinylbenzene copolymer, sulfonated (styrene-chloromethylstyrene-divinylbenzene copolymer), and the like. From the viewpoint of further improving the selective permeability to ammonium ions and keeping the membrane resistance low, the cation exchange resin in the present invention is preferably sulfonated polyether sulfone, sulfonated styrene-divinylbenzene copolymer, or sulfonated (styrene-chloromethylstyrene-divinylbenzene copolymer).
[0013] In the present invention, when the cation exchange membrane has a support, the support is not particularly limited as long as it has an opening, and examples thereof include various porous membranes such as nets, nonwoven fabrics, woven fabrics, and porous resin films. By having a support, the mechanical strength of the cation exchange membrane is improved. The support may be in the cation exchange resin layer, or on one or both sides of the cation exchange resin layer, and the openings of the porous membrane as the support may be filled with a cation exchange resin. The thickness of the cation exchange membrane of the present invention is preferably 1 to 100 μm, more preferably 10 to 80 μm, and even more preferably 10 to 50 μm.
[0014] The method for producing the cation exchange membrane of the present invention is not particularly limited, and for example, a normal method for forming a resin membrane can be used. For example, a method of forming a membrane by coating a liquid in which a cation exchange resin is dissolved in a solvent on a substrate, or when a support is used, a method of coating a liquid in which a cation exchange resin is dissolved in a solvent on a support, or a method of filling an opening of a support can be used. In addition, a production method (called a paste method) can be adopted in which a polymerizable composition in which a polymerization initiator is added to a monomer such as styrene, chloromethylstyrene, or divinylbenzene is filled in the opening of a support, and these monomers are polymerized in situ and then sulfonic acid groups are introduced. The water content of a cation exchange membrane varies depending on the type of cation exchange resin and the structure of the cation exchange membrane, but for the same type of cation exchange membrane, generally, when the ion exchange capacity is increased, the osmotic pressure due to the fixed charged group of the membrane increases, and the water content increases. On the other hand, when the crosslinking density is increased, the swelling pressure due to the osmotic pressure is suppressed, and the water content decreases. Therefore, the water content can be adjusted by controlling the ion exchange capacity and crosslinking conditions. On the other hand, the membrane resistance of a cation exchange membrane usually increases as the water content decreases, provided that the type of cation exchange resin and the structure of the membrane are the same. In the present invention, the membrane resistance can be prevented from becoming extremely high by adjusting the cation exchange capacity, crosslinking degree, crosslinking density, and membrane thickness of the cation exchange membrane.
[0015] In the ion exchange membrane cell of the present invention, an anion exchange membrane and a cation exchange membrane of the present invention are arranged opposite to each other. The anion exchange membrane in the ion exchange membrane cell of the present invention is not particularly limited as long as it is a membrane that selectively permeates anions. FIG. 1 shows an example of the use of the ion exchange membrane cell of the present invention, in which the ion exchange membrane cells of the present invention are stacked for an electrodialysis device. In the electrodialysis device of FIG. 1, a dilute side solution is passed through the anode side of the cation exchange membrane of the present invention, and a concentrated side solution is passed through the cathode side. A solution containing various ions is introduced into the dilute side, and while the introduced solution passes between the anion exchange membrane and the cation exchange membrane of the present invention, for example, ammonium ions selectively pass through the cation exchange membrane of the present invention as a specific cation in the solution and move to the concentrated side. In this way, ammonium ions are concentrated on the concentrated side. Various ions may be present in the dilute side solution, and specific cations can be selectively concentrated by the selectivity of the cation exchange membrane of the present invention. The various cations present in the dilute solution are not particularly limited, but may include, for example, alkali metal ions, alkaline earth metal ions, and other monovalent to trivalent cations, such as ammonium ions, sodium ions, potassium ions, lithium ions, calcium ions, magnesium ions, hydrogen ions, silver ions, and heavy metal ions such as copper, zinc, and mercury. The various anions present in the dilute solution are not particularly limited, but may include, for example, hydroxide ions, chloride ions, bromine ions, fluorine ions, iodide ions, carbonate ions, nitrate ions, sulfate ions, and phosphate ions. The solution introduced into the concentrate side is not particularly limited, but may include, for example, raw water to be concentrated, water in which specific ions in the raw water are concentrated, or water, and may contain the various ions contained in the dilute solution. Tap water, industrial water, pure water, etc. can be used as the water.
[0016] The electrodialysis apparatus of the present invention is an electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane, and an anion exchange membrane, the cation exchange membrane being the cation exchange membrane of the present invention. In the electrodialysis apparatus of the present invention, the anode, cathode, and anion exchange membrane are not particularly limited, and for example, a normal anode, cathode, and anion exchange membrane used in electrodialysis apparatus can be used. The solution treatment section of the electrodialysis apparatus of the present invention can be produced by stacking the ion exchange membrane cells of the present invention. EXAMPLES
[0017] The present invention will be specifically described below by way of examples of the present invention, but the technical scope of the present invention is not limited to these examples.
[0018] [Example 1] [Preparation of sulfonated polyethersulfone (SPES) membrane] SPES was dissolved in N,N-dimethylacetamide (DMAc) at 60°C while stirring to prepare a solution with a SPES concentration of 10% by mass. The prepared solution was applied to a glass plate with a film applicator to a predetermined thickness, and then dried on a plate heater at 50°C for 171 minutes. The resulting solution was immersed in ion-exchanged water and peeled off to prepare a SPES film.
[0019] [Example 2] [Preparation of sulfonated (styrene-chloromethylstyrene-divinylbenzene copolymer) membrane] A polymerizable composition was prepared by mixing the components according to the following formulation. Styrene 48.6 parts by weight Chloromethylstyrene 40.0 parts by mass Divinylbenzene 11.4 parts by weight Ethylene glycol diglycidyl ether 5.0 parts by mass t-Butylperoxy-2-ethylhexanoate 5.0 parts by mass 500g of this polymerizable composition was placed in a 1000ml glass container, and a polyethylene porous film (thickness 25μm, porosity 44%, average pore size 0.03μm) was immersed therein as a support, and the voids in the film were filled with the polymer composition. Next, the porous film filled with the polymer composition was taken out, and both sides of the porous substrate film were covered with a polyester film having a thickness of 100μm as a release agent, and then the film was heated and polymerized at 90℃ for 5 hours under nitrogen pressure of 0.4MPa. The membrane obtained by peeling off the polyester film was immersed in a mixture of sulfuric acid and chlorosulfonic acid at a weight ratio of 1:1 at 40℃ for 60 minutes to sulfonate, and the cation exchange membrane of the present invention was obtained.
[0020] [Comparative Example 1] A standard cation exchange membrane (Neosepta (registered trademark) CSE, manufactured by Astom Corporation) was used as the ion exchange membrane of Comparative Example 1.
[0021] (Film thickness measurement) The thickness of the resulting film was measured using a film thickness meter (Mitutoyo ABS Digimatic Blade Thickness).
[0022] (Measurement of membrane resistance) Figure 2 shows the measurement device and conditions for the membrane resistance. First, an acrylic cell (current-carrying area 1 cm ) with platinum electrodes was used. 2 ) to NH 4 Cl aqueous solution (NH 4 The solution resistance (R 0 After that, the sample film was sandwiched between the two cells, and the resistance (R 1 The membrane resistance (R m ) is calculated from the following formula (1), and the membrane resistance obtained is divided by the membrane thickness to obtain the membrane specific resistance K from formula (2). m [Ωcm] was calculated. In the formula (1), R 1 [Ωcm 2 ] is the resistance measured by sandwiching the sample film between two cells, and R 0 [Ωcm 2 ] is the solution resistance measured without the sample film, and R m[Ωcm 2 ] is the membrane resistance. In equation (2), K m [Ωcm] is the film resistivity and d [cm] is the film thickness.
[0023]
number
[0024]
number
[0025] (Electrodialysis) As shown in Figure 3, the effective membrane area is 4.0 cm 2 The measurement membrane was sandwiched between the (2.0 cm x 2.0 cm) device and placed in a 0.1 MNH 4 Cl, 0.1M NaCl and 0.1M CaCl 2 The mixed salt solution was placed in two cells, and electrodialysis was performed between the Ag·AgCl electrodes at a constant current of 90 mA using a DC stabilized power supply (PMC35-2A, Kikusui Electronics Co., Ltd.) for approximately 120 minutes. The solution in the cells was sampled at regular intervals. After that, the NH 4+ , Na + and Ca 2+ The concentration of these ions was quantified to measure the change in concentration over time. The flux of each ion was calculated from these values using the following formula. In formula (3), J i [mol m -2 ·s -1 ] represents the permeation flux, and V[m 3 ] represents the volume of the concentrated solution, and S [m 2 ] represents the effective membrane area, t [s] represents the time during which the current was passed, and ΔC i / Δt [mol m -3 ·s -1 ] represents the initial concentration gradient. Also, i is NH 4 + , Na + or Ca 2+ In formulas (4) and (5), P NH4 Na and PNH4 Ca represents the ion selective permeability coefficient [-]. In equation (6), η [-] represents the current efficiency, and z i [-] represents the valence of the cation, I [A] represents the electric current, and F [C mol -1 ] represents the Faraday constant.
[0026]
number
[0027]
number
[0028]
number
[0029]
number
[0030] (Water content of cation exchange membrane) To calculate the water content of the cation exchange membrane, the sample membrane was immersed in a 0.5 mol / L NaCl aqueous solution for 8 hours or more, rinsed with ion exchange water, and then the water on the surface was wiped off with tissue paper to measure the wet weight W 2 The same sample film was then dried under reduced pressure at 60°C for 5 hours to measure the dry weight W 1 The moisture content W was calculated from the dry weight and the wet weight according to the following formula (A).
[0031]
number
[0032] (Results of Example 1) Figure 4 shows a photograph of the SPES membrane produced in Example 1. The membrane had a thickness of 29 μm and a water content of 0.11. The membrane resistance was 0.81 Ωcm. 2The membrane resistivity was 279 Ωcm. The results of electrodialysis using this membrane are shown in Figure 5. 4+ , Na + and Ca 2+ The graph shows the time change in ion concentration of each ion in the concentrated side and the diluted side. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na is 2.40, P NH4 Ca was 1.64. This is Na + 2.4 times more NH 4+ is selectively permeable to Ca 2+ 1.64 times more NH 4+ This indicates that the selective permeation of the ZnO-based ZnO-based nanotubes was observed. The current efficiency was 0.97.
[0033] (Results of Example 2) The membrane prepared in Example 2 had a thickness of 28 μm and a water content of 0.17. The membrane resistance was 0.94 Ω cm. 2 The membrane resistivity was 336 Ωcm. The results of electrodialysis using this membrane are shown in Figure 6. 4+ , Na + and Ca 2+ The graph shows the time change in ion concentration of each ion in the concentrated side and the diluted side. All three types of cations move from the diluted side to the concentrated side due to the applied DC voltage. The flux was calculated from the slope of the time-concentration curve using equation (3), and the ion selectivity coefficient was calculated using equations (4) and (5). As a result, P NH4 Na is 2.03, P NH4 Ca was 1.45. This is Na + 2.03 times more NH 4+ is selectively permeable to Ca 2+ 1.45 times more NH 4+ This indicates that the selective permeation of the ZnO-containing polymer was observed. The current efficiency was 0.83.
[0034] (Results of Comparative Example 1) The membrane thickness of the standard cation exchange membrane (CSE) was 160 μm, the water content was 0.41, and the membrane resistance was 1.8 Ω cm 2 The membrane resistivity was 113Ω. The results of electrodialysis using this membrane are shown in Figure 7. NH4 Na is 1.53, P NH4 Ca The current efficiency was 0.92.
[0035] The results of Examples 1 and 2 and Comparative Example 1 are summarized in Table 1. From this comparison, the membrane water content increases in the order of Example 1, Example 2, and Comparative Example 1. In addition, the membrane prepared in Example 1 does not have a support, while the membrane prepared in Example 2 and the membrane of Comparative Example 1 have supports. In terms of the selective permeability of ammonium ions relative to sodium ions, the membrane prepared in Example 1 showed a selective permeability 57% higher than that of the membrane of Comparative Example 1, and the membrane prepared in Example 2 showed a selective permeability 31% higher than that of the membrane of Comparative Example 1. It was shown that ammonium ions selectively permeate more than sodium ions even with the same monovalent ions because the water content is within the range of the present invention. In particular, the membrane prepared in Example 1, which has a low water content, showed high ammonium ion selectivity.
[0036] The selective permeability of ammonium ions relative to divalent calcium ions was 1.64 for the membrane prepared in Example 1 and 1.45 for the membrane prepared in Example 2, while that of the membrane prepared in Comparative Example 1 was 0.68. In general, divalent cations are distributed more in the cation exchange membrane than monovalent cations due to Donnan equilibrium, and therefore their permeability is greater than that of monovalent ions. The selectivity of the membrane of Comparative Example 1 is 1 or less, which indicates that calcium ions, which are divalent ions, selectively permeate more than monovalent ammonium ions. However, the selectivity of the membrane prepared in Example 1 and the membrane prepared in Example 2 was 1 or more, resulting in the permeability of ammonium ions, which are monovalent cations, exceeding calcium ions, which are divalent cations. Thus, it was shown that ions with small hydrated ion radii selectively permeate more than ions with large hydrated ion radii when the water content is within the range of the present invention.
[0037] In the membrane of Comparative Example 1, the water content of the membrane was 0.41 and the membrane resistance was 1.8 Ω cm 2 On the other hand, the membrane resistance of the membrane prepared in Example 1 was 0.81 Ωcm 2 In the membrane prepared in Example 2, the membrane resistance was 0.94 Ω cm 2 Although these membranes had a low water content, they had a low membrane resistance.
[0038] [Table 1] [Industrial Applicability]
[0039] The cation exchange membrane of the present invention has excellent selective permeability for ammonium ions, and can therefore be used in various applications for concentrating ammonium ions, such as in various water treatments for wastewater, etc. For example, it is possible to highly efficiently concentrate ammonium ions in wastewater in which divalent cations such as calcium ions and magnesium ions, and monovalent cations such as sodium ions and potassium ions coexist, and to inhibit scale formation, and therefore it can be suitably used in various fields that utilize ion exchange membranes, such as the concentration and separation of ammonium ions from wastewater. In addition, the cation exchange membrane of the present invention can be suitably used in electrodialysis devices, Donnan dialysis devices, etc.
Claims
1. A cation exchange membrane having a water content of 0.05 to 0.2 as calculated by the following formula (A). ==(W 2 -W 1 ) / W 1 (A) (In formula (A), W is the water content, W 2 is the wet weight, W 1 is the dry weight.)
2. N.H. 4 NH with Cl concentration of 0.5 mol / L 4 The membrane resistance in a Cl aqueous solution at 25°C is 2.0 Ωcm 2 2. The cation exchange membrane according to claim 1, wherein:
3. 3. The cation exchange membrane according to claim 1, which is a cation exchange membrane for concentrating ammonium ions.
4. 3. The cation exchange membrane according to claim 1, wherein the cation exchange resin constituting the cation exchange membrane is an aromatic hydrocarbon resin having a structure in which cation exchange groups have been introduced.
5. 5. The cation exchange membrane according to claim 4, wherein the cation exchange resin constituting the cation exchange membrane is a sulfonated polyether sulfone or a sulfonated styrene-divinylbenzene copolymer.
6. 3. An ion exchange membrane cell comprising an anion exchange membrane and the cation exchange membrane according to claim 1 or 2 disposed opposite each other.
7. 3. An electrodialysis apparatus comprising an anode, a cathode, a cation exchange membrane and an anion exchange membrane, wherein the cation exchange membrane is the cation exchange membrane according to claim 1 or 2.
Citation Information
Patent Citations
Electric deionizer
JP2007268337A