Hydraulic composition, hardened body, and method for producing hydraulic composition

A hydraulic composition using calcined allophane or halloysite with specific iron and silicon-to-aluminum ratios addresses the scarcity of kaolin, achieving low-carbon and high-strength cement alternatives.

JP2024143002AActive Publication Date: 2024-10-11MITSUBISHI UBE CEMENT CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023055450
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The limited availability of kaolin, a key material for producing low-carbon cement, necessitates the development of alternative inorganic minerals that can achieve equivalent or better compressive strength in hydraulic compositions.

Method used

A hydraulic composition using calcined minerals like allophane or halloysite, with specific iron and silicon-to-aluminum ratios, along with alkaline stimulants, to enhance compressive strength and reduce carbon footprint.

Benefits of technology

The composition provides a low-carbon hydraulic material with sufficient compressive strength, utilizing readily available minerals like allophane or halloysite, overcoming the limitations of kaolin scarcity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143002000001
    Figure 2024143002000001
  • Figure 2024143002000002
    Figure 2024143002000002
Patent Text Reader

Abstract

To provide a low-carbon hydraulic composition which is produced using an inorganic mineral other than kaolin and has sufficient compressive strength development.SOLUTION: A hydraulic composition contains: 10 to 90 mass% of a calcined inorganic mineral that is a calcined product of an inorganic mineral having a mass ratio of trivalent iron ions to divalent iron ions (Fe3+ / Fe2+) of 2.0 to 6.0 as measured by absorptiometry, and has a mass ratio of SiO2 to Al2O3 (SiO2 / Al2O3) of 0.5 to 3.0, based on the total amount of the calcined inorganic mineral and an alkali stimulant; and 10 to 90 mass% of the alkali stimulant based on the total amount of the calcined inorganic mineral and the alkali stimulant.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydraulic composition, a hardened product, and a method for producing a hydraulic composition. [Background technology]

[0002] Limestone Calcined Clay Cement (LC3) is known as a technology that uses inorganic minerals to calcinate them to increase their reactivity and replace cement admixtures such as blast furnace slag and fly ash (for example, Non-Patent Document 1). This cement can be called a low-carbon cement, and compared to ordinary Portland cement, it can reduce carbon dioxide emissions (CO2) associated with its production. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Karen Scrivener et al.: Calcined clay limestone cements (LC3), Cement and Concrete Research,Vol.114,pp.49-56 (2018) Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, with regard to the above-mentioned technology, it has been shown that a material containing metakaolin, which is calcined kaolin as an inorganic mineral, can achieve good strength development. However, since kaolin is produced in limited regions and countries, the search for a material to replace kaolin has become an issue.

[0005] The present invention has been made in consideration of the above circumstances, and aims to provide a low-carbon hydraulic composition that is produced using an inorganic mineral other than kaolin and has sufficient compressive strength development. Another aim of the present invention is to provide a hardened body obtained from the hydraulic composition, and a method for producing the hydraulic composition. [Means for solving the problem]

[0006] The inventors focused on minerals such as allophane, which is usually said to inhibit the reaction of cement, as a material other than kaolin, and found that hydraulic compositions containing such minerals may have properties equivalent to or superior to those containing kaolin, and that it may be possible to reduce the amount of cement to be mixed as an alkaline activator when preparing a hydraulic composition, and thus completed the present invention.

[0007] One aspect of the present invention is as follows [1] to

[10] . [1] The mass ratio of ferric ions to divalent ions (Fe 3+ / Fe 2+ The hydraulic composition comprises 10 to 90 mass% of a calcined inorganic mineral which is a calcined product of an inorganic mineral having a SiO2 to Al2O3 mass ratio (SiO2 / Al2O3) of 2.0 to 6.0 and a mass ratio of SiO2 to Al2O3 of 0.5 to 3.0 based on the total amount of the calcined inorganic mineral and an alkaline irritant, and 90 to 10 mass% of an alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant. [2] The hydraulic composition according to [1], wherein the hydraulic composition further contains a carbonate, and the mass ratio of the carbonate to the mass of the calcined inorganic mineral (carbonate / calcined inorganic mineral) is 2.0 or less. [3] The hydraulic composition according to [1] or [2], wherein the calcined inorganic mineral is a clay mineral calcined at 500 to 950°C. [4] The hydraulic composition according to any one of [1] to [3], wherein the alkaline activator contains Portland cement. [5] The hydraulic composition according to any one of [1] to [4], wherein the calcined inorganic mineral includes calcined allophane or calcined halloysite. [6] The hydraulic composition according to [5], wherein the content of the calcined allophane or the calcined halloysite in the calcined inorganic mineral is 60 mass% or more. [7] A hardened body obtained by hardening a paste containing the hydraulic composition according to any one of [1] to [6] and water. [8] The mass ratio of ferric ions to divalent ions (Fe 3+ / Fe 2+ a calcined inorganic mineral having a SiO2 to Al2O3 mass ratio (SiO2 / Al2O3) of 2.0 to 6.0 and a SiO2 to Al2O3 mass ratio of 0.5 to 3.0, and an alkaline irritant, to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of the alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant. [9] The method according to [8], further comprising a calcination step of calcining the inorganic mineral at 500 to 950°C prior to the preparation step to obtain the calcined inorganic mineral.

[10] The method according to [9], wherein the inorganic mineral is a clay mineral. Effect of the Invention

[0008] According to the present invention, it is possible to provide a low-carbon hydraulic composition which is produced using an inorganic mineral other than kaolin and has sufficient compressive strength development. Also, according to the present invention, it is possible to provide a hardened body obtained from the hydraulic composition and a method for producing the hydraulic composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Preferred embodiments of the present disclosure will be described in detail below, however, the present disclosure is not limited to the following embodiments. In the following description, when it is written "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0010] <Hydraulic composition> The hydraulic composition has a mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ The calcined inorganic mineral has a mass ratio of SiO2 to Al2O3 (SiO2 / Al2O3) of 2.0 to 6.0, and the mass ratio of SiO2 to Al2O3 is 0.5 to 3.0 or less, and an alkaline irritant. Based on the total amount of the calcined inorganic mineral and the alkaline irritant (100 mass%), the content of the calcined inorganic mineral is 10 to 90 mass%, and the content of the alkaline irritant is 90 to 10 mass%.

[0011] (calcined inorganic minerals) Calcined inorganic minerals are obtained by calcining inorganic minerals at a specified temperature. Calcination increases the compressive strength of the inorganic minerals, but does not substantially change the SiO2 and Al2O3 contents, the SiO2 / Al2O3 mass ratio, etc. of the inorganic minerals.

[0012] Examples of inorganic minerals (excluding kaolin) having a mass ratio of SiO2 / Al2O3 of 0.5 to 3.0 include allophane, halloysite, imogolite, illite, montmorillonite, pyrophyllite, etc. Among these, from the viewpoint of reactivity with an alkaline irritant, the inorganic mineral preferably contains allophane or halloysite, and more preferably contains allophane. That is, the calcined inorganic mineral (excluding metakaolin) preferably contains calcined allophane or calcined halloysite, and more preferably contains calcined allophane.

[0013] From the viewpoint of easily exhibiting sufficient compressive strength, the content of calcined allophane or calcined halloysite in the calcined inorganic mineral (which can also be said to be the content of allophane or halloysite in the inorganic mineral) is preferably 60 mass% or more, more preferably 80 mass% or more, and may be 100 mass% (calcined inorganic mineral substantially composed of calcined allophane or calcined halloysite). The content of allophane in an inorganic mineral or the content of calcined allophane in a calcined inorganic mineral can be measured by an acid-alkali alternating dissolution method, and the content of halloysite in an inorganic mineral or the content of calcined halloysite in a calcined inorganic mineral can be measured by XRD Rietveld analysis.

[0014] The inorganic mineral may be a mineral produced by weathering a volcanic ejecta, i.e., a mineral derived from a volcanic ejecta. Examples of the volcanic ejecta include volcanic ash, volcanic lapilli, pumice, pyroclastic flow deposits, and the like. The inorganic mineral may be a mineral produced by weathering an igneous rock. Examples of the igneous rock include granite, and the like. In general, allophane is produced by weathering a volcanic ejecta or an igneous rock, halloysite is produced by further weathering of allophane, and kaolin is produced by further weathering of halloysite. Kaolin, allophane, and halloysite are clay minerals.

[0015] Allophane is an amorphous inorganic mineral. Allophane generally has a particle size of 0.05 to 0.2 μm and a melting point of 250 to 600 m. 2 / g BET specific surface area. Halloysite is a crystalline inorganic mineral. Halloysite generally has a particle size of 0.1-0.3 μm and a crystallinity of 40-100 μm. 2 / g BET specific surface area.

[0016] The SiO2 / Al2O3 mass ratio in the above range is likely to improve the reactivity between the calcined inorganic mineral and the alkaline irritant. From this viewpoint, the SiO2 / Al2O3 mass ratio is 0.5 or more, preferably 0.6 or more, and more preferably 0.7 or more. The SiO2 / Al2O3 mass ratio is 3.0 or less, preferably 2.5 or less, and more preferably 2.3 or less.

[0017] The SiO2 content in the inorganic mineral is preferably 30% by mass or more and 55% by mass or less from the viewpoint of reactivity with the alkaline irritant. The Al2O3 content in the inorganic mineral is preferably 20% by mass or more and 60% by mass or less from the viewpoint of reactivity with the alkaline irritant.

[0018] The mass ratio of ferric to divalent ions in inorganic minerals, measured by spectrophotometry, Fe 3+ / Fe 2+ When the mass ratio Fe is in the above range, the calcined inorganic mineral, i.e., the calcined product, and the alkali irritant react easily. 3+ / Fe 2+ The mass ratio Fe is 2.0 or more. 3+ / Fe 2+ is 6.0 or less, preferably 5.7 or less, and more preferably 5.5 or less.

[0019] Ferrous ion (Fe) in inorganic minerals as determined by spectrophotometry 3+ From the viewpoint of the content of clay minerals contained in the inorganic minerals, the content of Fe can be 0.5% by mass or more, preferably 0.55% by mass or more, and more preferably 0.6% by mass or more. 3+The content of can be 2.0 mass% or less, preferably 1.9 mass% or less, and more preferably 1.8 mass% or less, from the viewpoint that the content of clay minerals contained in inorganic minerals decreases as the amount of Fe compounds adsorbed on the clay mineral surface increases.

[0020] Ferrous ion (Fe) in inorganic minerals, measured by spectrophotometry 2+ From the viewpoint of the content of clay minerals contained in the inorganic minerals, the content of Fe can be 0.13% by mass or more, preferably 0.14% by mass or more, and more preferably 0.15% by mass or more. 2+ The content of can be 0.8 mass% or less, preferably 0.7 mass% or less, and more preferably 0.6 mass% or less, from the viewpoint that the content of clay minerals contained in inorganic minerals decreases as the amount of Fe compounds adsorbed on the clay mineral surface increases.

[0021] Mass ratio Fe 3+ / Fe 2+ is the amount of ferric ion (Fe) based on the total amount of inorganic compounds measured by spectrophotometry. 3+ The amount (mass%) of divalent iron ions Fe 2+ It is calculated by dividing the amount (mass%) of

[0022] Based on the total amount of the calcined inorganic mineral and the alkaline irritant, the content of the calcined inorganic mineral is equal to or more than the lower limit, so that good compressive strength can be obtained, and the content is equal to or less than the upper limit, so that good fluidity can be maintained. From these viewpoints, the content is 10% by mass or more, preferably 20% by mass or more, and more preferably 30% by mass or more. In addition, the content is 90% by mass or less, preferably 80% by mass or less, and more preferably 70% by mass or less.

[0023] Calcined inorganic minerals are obtained by calcining inorganic minerals at a predetermined temperature as described above. The fact that an inorganic mineral is calcined means that 27This can be confirmed by analyzing with Al-NMR. Specifically, in calcined inorganic minerals, 27 When the sum of the peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al analyzed by Al-NMR is taken as 100%, the proportion of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 30 to 50%.

[0024] In the calcined inorganic mineral, the framework of tetracoordinated Al and pentacoordinated Al is unstable, which is considered to contribute to an increase in reactivity with an alkaline irritant. When the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 30% or more, the effect of this action can be fully enjoyed. On the other hand, if the ratio of tetracoordinated Al and pentacoordinated Al is too high, there is a risk that the reaction with the alkaline irritant will proceed rapidly. When the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 50% or less, such a phenomenon can be easily suppressed. From these viewpoints, the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is preferably 30 to 45%, more preferably 35 to 45%. From the viewpoint of easily obtaining the above-mentioned effects, the peak area ratios of both 4-coordinate Al and 5-coordinate Al may be 30 to 50%, preferably 30 to 45%, and more preferably 35 to 45%.

[0025] The sum of the peak areas of tetracoordinated Al and pentacoordinated Al is preferably 50% or more from the viewpoint of reactivity with an alkaline irritant, and is preferably 90% or less from the viewpoint of the reaction rate with an alkaline irritant. From these viewpoints, the sum of the peak areas of tetracoordinated Al and pentacoordinated Al is more preferably 60 to 90%, and further preferably 70 to 80%. In view of the above, the peak area of ​​6-coordinated Al is preferably from 10 to 50%, more preferably from 10 to 40%, and further preferably from 20 to 30%.

[0026] In order for the inorganic mineral to have the desired peak areas for tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al, the inorganic mineral may be calcined at a predetermined temperature, more specifically, calcined according to the calcination process described below.

[0027] The above peak area ratio is measured as follows. Nuclides of calcined inorganic minerals 27 The chemical shift and coordination state of Al-NMR are analyzed using an NMR apparatus JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method is the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube is used. The analysis conditions are magnetic field strength: 18.79 T, frequency: 20 kHz, number of integrations: 256, and pulse width: 90° (0.6 μs). Obtained 27 For the Al-NMR spectrum, the waveform of each peak is separated using a Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function.The area of ​​each peak is then calculated using the integral value of each separated peak. In addition, calcined inorganic minerals 27 In the Al-NMR spectrum, peak P1 is observed in the chemical shift range of -10 ppm to 15 ppm, peak P2 in the chemical shift range of 50 ppm to 80 ppm, and peak P3 in the chemical shift range of 30 ppm to 40 ppm. Peak P1 corresponds to 6-coordinated Al, which originates from the inorganic mineral framework. Peaks P2 and P3 originate from 4-coordinated Al and 5-coordinated Al, respectively, which are thought to be generated by partial collapse of the inorganic mineral framework (e.g., decomposition and dehydroxylation of the 6-coordinated Al structure by heat treatment at high temperature). From the obtained areas of the peaks P1 to P3, the sum of the area of ​​P1+P2+P3 and the ratios of the areas of P2 and P3 based on this sum are calculated.

[0028] (Alkaline stimulant) Alkaline stimulants include Portland cement clinker, Portland cement, tricalcium silicate (3CaO·SiO2, represented as C3S), and hydrated lime.

[0029] Portland cement clinker can use Portland cement clinker used for preparing various Portland cements specified in JIS R 5210:2003 "Portland Cement". Examples of the various Portland cements include ordinary Portland cement, early-strength Portland cement, medium-heat Portland cement, and low-heat Portland cement. The Portland cement clinker may be a Portland cement clinker used for preparing ordinary Portland cement and early-strength Portland cement.

[0030] The mineral composition of Portland cement clinker can be calculated by the Bogue formula. Here, the Bogue formula is a widely used formula for calculating the content ratio of main minerals in Portland cement clinker from the content ratio of chemical composition. By using the Bogue formula shown below, the contents of tricalcium silicate (3CaO·SiO2, denoted as C3S), dicalcium silicate (2CaO·SiO2, denoted as C2S), and tricalcium aluminate (3CaO·Al2O3, denoted as C3A) in Portland cement clinker can be calculated. In the following formulas, "%" means "mass%". The chemical formula represents the content ratio (mass%) of each compound shown by the chemical analysis values according to JIS R 5204:2019 "Fluorescent X-ray Analysis Method for Cement".

[0031] <Bogue formula> C3S [%]=(4.07×CaO [%])-(7.60×SiO2 [%])-(6.72×Al2O3 [%])-(1.43×Fe2O3 [%])-(2.85×SO3 [%]) C2S [%]=(2.87×SiO2 [%])-(0.754×C3S [%]) C3A [%]=(2.65×Al2O3 [%])-(1.69×Fe2O3 [%]) C4AF [%]=3.04×Fe2O3 [%]

[0032] The Portland cement may be normal Portland cement, high early strength Portland cement, extra high early strength Portland cement, moderate heat Portland cement, low heat Portland cement, sulfate resistant Portland cement.

[0033] Based on the total amount of the calcined inorganic mineral and the alkaline irritant, the content of the alkaline irritant is equal to or more than the lower limit, so that good compressive strength can be obtained, and the content is equal to or less than the upper limit, so that CO2 emissions can be reduced. From these viewpoints, the content is 10% by mass or more, preferably 20% by mass or more, and more preferably 30% by mass or more. In addition, the content is 90% by mass or less, preferably 80% by mass or less, and more preferably 70% by mass or less.

[0034] From the viewpoint of compressive strength, the total amount (content) of the calcined inorganic mineral and the alkaline irritant in the hydraulic composition is preferably 75 mass% or more, more preferably 80 mass% or more, and more preferably 85 mass% or more, based on the total amount of the hydraulic composition, and may be 100 mass% (hydraulic composition substantially consisting of the calcined inorganic mineral and the alkaline irritant).

[0035] (Carbonates) The hydraulic composition may contain a carbonate. The carbonates include alkaline earth metal carbonates, which are added to the hydraulic composition for the purpose of promoting the hydration reaction between the alkaline irritant and the calcined inorganic mineral, and examples of such carbonates include calcium carbonate (limestone) and magnesium carbonate. In addition, carbonates of alkali metals such as sodium carbonate decahydrate (Na2CO3·10H2O), sodium carbonate (Na2CO3), potassium carbonate (K2CO3), and sodium sesquicarbonate dihydrate (Na3H(CO3)2·NaHCO3·2H2O), which react with inorganic minerals as alkaline irritants, can also be used.

[0036] As the limestone, for example, powders mainly composed of calcium carbonate, such as limestone powder that is generally available on the market, and kansui stone powder, can be used. The limestone preferably includes those conforming to the minor mixing components described in JIS R 5210:2009 "Portland cement".

[0037] The content of carbonate in the hydraulic composition is, from the viewpoint of fluidity, 0% by mass or more, and preferably more than 0% by mass, and may be 10% by mass or more, based on the total amount of the hydraulic composition; on the other hand, from the viewpoint of compressive strength, it is preferably 25% by mass or less, and may be 20% by mass or less, or may be 15% by mass or less. In addition, the mass ratio of the carbonate to the mass of the calcined inorganic mineral in the hydraulic composition (carbonate / calcined inorganic mineral) is preferably 2.0 or less, more preferably 1.0 or less, from the viewpoint of compressive strength. The lower limit of the mass ratio is not particularly limited, but may be 0.

[0038] (Other ingredients) The hydraulic composition may contain inorganic fine powder, gypsum, etc., in addition to the calcined inorganic mineral, the alkaline irritant, and the carbonate. When the hydraulic composition contains these other components in addition to the carbonate, the total amount (content) of the carbonate and the other components can be 25 mass% or less, may be 20 mass% or less, or may be 15 mass% or less, based on the total amount of the hydraulic composition.

[0039] The inorganic fine powder is added to the hydraulic composition for the purpose of improving the compressive strength. Examples of the inorganic fine powder include powdered materials such as silica stone and crushed stone. The content of the inorganic fine powder in the hydraulic composition is 0 mass% or more, and preferably more than 0 mass%, based on the total amount of the hydraulic composition from the viewpoint of fluidity, while it is preferably 15 mass% or less from the viewpoint of compressive strength.

[0040] Gypsum is added to the hydraulic composition for the purpose of adjusting the hydration reaction rate. Examples of gypsum include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. The gypsum content in the hydraulic composition can be equivalent to the amount of gypsum in general Portland cement, and is 0 mass% or more, based on the total amount of the hydraulic composition, and is preferably more than 0 mass%, while it is preferably 5 mass% or less from the viewpoint of easily maintaining a good hydration reaction rate.

[0041] <Cured body> The hardened body is obtained by hardening the paste containing the hydraulic composition and water. The hardening conditions are not particularly limited. The hardened body can be prepared according to the method described in JIS R 5201:2015 "Physical test method for cement".

[0042] The amount of water in the paste is preferably 35 parts by mass or more relative to 100 parts by mass of the total amount of the hydraulic composition from the viewpoint of fluidity, and is preferably 80 parts by mass or less from the viewpoint of easily making the pore structure of the hardened body dense. From these viewpoints, the amount of water is preferably 35 to 80 parts by mass, and more preferably 50 to 70 parts by mass.

[0043] <Method for producing hydraulic composition> The method for producing the hydraulic composition is to determine the mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ The method includes a preparation step of mixing a calcined inorganic mineral having a SiO2 to Al2O3 mass ratio (SiO2 / Al2O3) of 2.0 to 6.0 and a SiO2 to Al2O3 mass ratio of 0.5 to 3.0 with an alkaline irritant to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of the alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.

[0044] The method for producing a hydraulic composition may further include a calcination step of calcining an inorganic mineral at 500 to 950° C. to obtain a calcined inorganic mineral, prior to the preparation step. In this case, the inorganic mineral may be a clay mineral, as described above.

[0045] (Preparation process) In the preparation step, the calcined inorganic mineral and the alkaline irritant are mixed. When mixing the two, the carbonate and the other components described above may be mixed together. The amounts of each raw material are as described above.

[0046] In the preparation process, each raw material may be crushed. When crushing is performed, the order of mixing and crushing is not particularly limited. That is, each raw material may be mixed and then crushed, each raw material may be crushed individually and then mixed, or each raw material may be mixed and crushed simultaneously. Mixing may be performed using a mixer such as a pan mixer, a tilting mixer, or a ribbon mixer, or may be mixed and crushed using a crusher such as a ball mill, a vertical roller mill, or a roller press, or each raw material may be crushed and then mixed using a mixer such as a mechanical mixer.

[0047] (calcination process) The calcination temperature in the calcination step is preferably 500° C. or higher from the viewpoint of increasing the compressive strength of the inorganic mineral, and is preferably 950° C. or lower from the viewpoint of suppressing the formation of other minerals (for example, the formation of mullite in the case of allophane). From these viewpoints, the calcination temperature is more preferably 600 to 900° C. The calcination time is not particularly limited, but may be 0.5 to 5 hours, or may be 1 to 4 hours, in view of the effect on the crystal structure.

[0048] The calcination process is 27 It can be said that the calcination process is a process in which an inorganic mineral is calcined so that the ratio of the peak area of ​​at least one of tetracoordinated Al and pentacoordinated Al is 30-50% when the sum of the peak areas of tetracoordinated Al, pentacoordinated Al, and hexacoordinated Al analyzed by Al-NMR is 100%. If the area of ​​the peak P1 of hexacoordinated Al derived from the inorganic mineral skeleton is too large, sufficient compressive strength cannot be obtained. It can be said that the calcination process is a process in which the skeleton of the inorganic mineral is partially collapsed, and peaks P2 and P3 derived from tetracoordinated Al and pentacoordinated Al, which contribute to improving the compressive strength, are generated. EXAMPLES

[0049] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.

[0050] <Raw materials for hydraulic composition> (Inorganic Minerals) The types of inorganic mineral (clay mineral) samples used are shown in Table 1. When the inorganic mineral was metakaolin or halloysite, the inorganic mineral content was measured by Rietveld analysis using XRD, and when the inorganic mineral was allophane, the inorganic mineral content was measured by the acid-alkali alternating dissolution method. Fe in inorganic minerals 2+ Amount, Fe 3+ Amount and mass ratio of Fe 3+ / Fe 2+ was measured and calculated by the phenanthroline absorptiometry method in accordance with JIS K0120:2016 "Testing method for industrial wastewater" using an ultraviolet-visible spectrophotometer (Hitachi High-Tech Science Corporation, product name: U-2900 type).

[0051] [Table 1]

[0052] (Alkaline stimulant) Ordinary Portland cement (OPC, manufactured by UBE Mitsubishi Cement Co., Ltd.) was used as the alkaline activator.

[0053] (Carbonates) Calcium carbonate (Ube Material Industries, Ltd. (fine limestone powder, 325 mesh product)) was used as the carbonate.

[0054] <Preparation of hydraulic composition> Various inorganic minerals were calcined at 900℃ for 1 hour to obtain calcined inorganic minerals. Next, according to the formulation shown in Table 2, the calcined inorganic mineral, the alkaline irritant, and optionally the carbonate were mixed to prepare a hydraulic composition.

[0055] (Measurement of chemical composition) The chemical composition of the calcined inorganic minerals was measured using an X-ray fluorescence analyzer (Rigaku: ZSX100e). The results are shown in Table 1.

[0056] (Peak area ratio calculation) Nuclides of calcined inorganic minerals 27 The chemical shifts and coordination states of Al-NMR were analyzed using an NMR system JNM-ECZ800R (manufactured by JEOL Ltd.). The analysis method was the MAS (Magic Angle Spinning) method, and a 3.2 mm sample tube was used. The analysis conditions were magnetic field strength: 18.79 T, frequency: 20 kHz, number of integrations: 256, and pulse width: 90° (0.6 μs). Obtained 27 For the Al-NMR spectrum, the peaks were separated using the Voigt function, which is a convolution function of a Gaussian function and a Lorentzian function. 27 In the Al-NMR spectrum, peak P1 in the chemical shift range of −10 ppm to 15 ppm corresponds to 6-coordinate Al, peak P2 in the chemical shift range of 50 ppm to 80 ppm corresponds to 4-coordinate Al, and peak P3 in the chemical shift range of 30 ppm to 40 ppm corresponds to 5-coordinate Al. The area of ​​each peak was calculated using the integral value of each separated peak. From the obtained areas of each peak, the sum of the areas of P1+P2+P3 and the ratio (%) of the areas of P1 to P3 based on the sum were calculated. The results are shown in Table 1.

[0057] <Preparation of hardened body> The prepared hydraulic composition was mixed with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate, and water, to prepare a hardened body in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement." The prepared hardened body was cured underwater in a thermostatic chamber at 20°C until ages of 7 and 28 days.

[0058] <Activity index measurement> The compressive strength of the above-mentioned hardened body was measured at ages of 7 and 28 days in accordance with the description in JIS R 5201:2015 "Physical Testing Methods for Cement". The activity index is the ratio of the compressive strength of the hardened body to the compressive strength of the reference hardened body, expressed as a percentage. The reference hardened body was prepared by mixing ordinary Portland cement with standard sand for cement strength testing provided by the Japan Cement Association as fine aggregate and water in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement".

[0059] [Table 2]

Claims

1. The mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ ) is 2.0 to 6.0, and Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 The hydraulic composition comprises a calcined inorganic mineral having a sintering ratio of 0.5 to 3.0 in an amount of 10 to 90 mass% based on the total amount of the calcined inorganic mineral and the alkaline irritant, and an alkaline irritant in an amount of 90 to 10 mass% based on the total amount of the calcined inorganic mineral and the alkaline irritant.

2. 2. The hydraulic composition according to claim 1, wherein the hydraulic composition further comprises a carbonate, and the mass ratio of the carbonate to the mass of the calcined inorganic mineral (carbonate / calcined inorganic mineral) is 2.0 or less.

3. 3. The hydraulic composition according to claim 1, wherein the calcined inorganic mineral is a clay mineral calcined at 500 to 950°C.

4. The hydraulic composition according to claim 1 or 2, wherein the alkaline activator comprises Portland cement.

5. 3. The hydraulic composition according to claim 1 or 2, wherein the calcined inorganic mineral comprises calcined allophane or calcined halloysite.

6. The hydraulic composition according to claim 5 , wherein the content of the calcined allophane or the calcined halloysite in the calcined inorganic mineral is 60 mass % or more.

7. A hardened body obtained by hardening a paste containing the hydraulic composition according to claim 1 or 2 and water.

8. The mass ratio of trivalent iron ions to divalent iron ions (Fe 3+ / Fe 2+ ) is 2.0 to 6.0, and Al 2 O 3 SiO 2 Mass ratio (SiO 2 / Al 2 O 3 The method for producing a hydraulic composition includes a preparation step of mixing a calcined inorganic mineral having a calcination ratio of 0.5 to 3.0 with an alkaline irritant to prepare a hydraulic composition containing 10 to 90 mass% of the calcined inorganic mineral based on the total amount of the calcined inorganic mineral and the alkaline irritant, and 90 to 10 mass% of the alkaline irritant based on the total amount of the calcined inorganic mineral and the alkaline irritant.

9. The method according to claim 8, further comprising a calcination step of calcining the inorganic mineral at 500 to 950° C. to obtain the calcined inorganic mineral prior to the preparation step.

10. The method according to claim 9, wherein the inorganic mineral is a clay mineral.

Citation Information

Patent Citations

  • Cement admixture and cement composition using the same

    JP1991265549A

  • Admixture for cement and cement composition containing the same

    JP2001302296A

  • Fire-proof composition

    JP2003128450A

  • Hydraulic composition, cured product, and method for producing hydraulic composition

    JP2023127724A

  • Cement composition

    JP2023131119A