Insolubilization material

Magnesium oxide particles with controlled elution and hydration properties address the rapid elution issue in acidic soil, ensuring effective long-term insolubilization of heavy metals by precise manufacturing processes.

JP2024143103AActive Publication Date: 2024-10-11UBE CHEM IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023055604
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Magnesium oxide used in existing methods for insolubilizing heavy metals in acidic soil elutes rapidly, limiting its long-term effectiveness.

Method used

Development of magnesium oxide particles with controlled elution rate and hydration properties, characterized by specific dissolution rate test value (50%) X ≤ 0.00150, crystallite diameter of 50 to 300 nm, BET specific surface area ≤ 1.8 m²/g, and controlled impurity content, achieved through precise calcination, pulverization, and classification.

Benefits of technology

Ensures long-term insolubilization of heavy metals in acidic soil by suppressing elution and maintaining stability, even in environments with moisture exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143103000001
    Figure 2024143103000001
  • Figure 2024143103000002
    Figure 2024143103000002
Patent Text Reader

Abstract

To provide an insolubilization material having appropriate leachability capable of exerting effect for a long term while insolubilizing heavy metals contained in earth.SOLUTION: An insolubilization material of the present invention is an insolubilization material for insolubilizing heavy metals, where the insolubilization material contains a magnesium oxide particle having 0.00150 or lower of an elution rate test value (50%) X expressed by the following formula (1). X=(m1 / 2) / (t1 / 2) (1). In the formula (1), m1 / 2 is a half amount of a sulfuric acid consumption amount (sulfuric acid mol / MgO mol) at an end point by a magnesium oxide particle in an elution test for maintaining pH at 3 of a magnesium oxide suspension, and t1 / 2 is a titration time (s) until reaching m1 / 2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an insolubilizing material. [Background technology]

[0002] In order to improve soil contaminated with heavy metals, etc., a method of insolubilizing heavy metals using an insolubilizing agent has been proposed (for example, Patent Document 1). In this method, magnesium oxide having specific physical properties and a powdered chelating agent are used as insolubilizing agents to insolubilize soil contaminated with heavy metals, etc. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-114291 A Summary of the Invention [Problem to be solved by the invention]

[0004] The magnesium oxide used in the technology described in Patent Document 1 is said to be highly active and capable of rapid reaction. However, when used in a low pH environment known as acidic soil, the majority of the highly active magnesium oxide is dissolved early on, which may hinder the long-term expression of its effects. To realize an insolubilizing material suitable for environments such as acidic soil, it is necessary to achieve both reactivity that enables insolubilization and the suppression of dissolution so that the material will remain in the environment for a long period of time. An object of the present invention is to provide an insolubilizing material that can insolubilize heavy metals contained in soil and the like while exhibiting a long-term effect and has an appropriate elution property. [Means for solving the problem]

[0005] The insolubilizing material of the present invention is an insolubilizing material that insolubilizes heavy metals, and is characterized by containing magnesium oxide particles having a dissolution rate test value (50%) X represented by the following formula (1) of 0.00150 or less. X=(m 1 / 2 ) / (t 1 / 2 ) (1) (In the above formula (1), m 1 / 2 is half the amount of sulfuric acid consumed by magnesium oxide particles at the end of the dissolution test in which the pH of the magnesium oxide suspension is maintained at 3 (mol of sulfuric acid / mol of MgO), and t 1 / 2 is m 1 / 2 is the titration time (s) until Effect of the Invention

[0006] According to the present invention, it is possible to provide an insolubilizing material that can insolubilize heavy metals contained in soil and the like while exhibiting a long-term effect and has an appropriate elution property. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] As a result of extensive research, the present inventors focused on the action of magnesium oxide as an alkaline agent and discovered new magnesium oxide particles having properties suitable for this application, thereby completing the present invention. Hereinafter, an embodiment of the present invention will be described in detail.

[0008] The insolubilizing material of the present invention can be used to insolubilize heavy metals contained in soil, etc. Examples of materials to be treated that contain heavy metals include soil, construction waste soil, rocks and crushed stone, incineration ash, sludge, etc. Specific examples of heavy metals include arsenic, selenium, lead, etc. The insolubilizing material of the present invention contains magnesium oxide particles having a dissolution rate test value (50%) X defined within a predetermined range. The dissolution rate test value (50%) X can be determined according to a dissolution rate test based on the measurement of the alkali dissolution rate.

[0009] To measure the alkaline dissolution rate, a magnesium oxide suspension in which 50 mg of magnesium oxide particles are dispersed in 100 mL of ion-exchanged water and 0.05 mol / L sulfuric acid are used. Using an automatic potentiometric titrator, the pH of the MgO suspension is maintained at 3 by dripping sulfuric acid, and the amount of sulfuric acid consumed to maintain the pH is calculated. From the measurement results, the dissolution rate test value (50%) X can be calculated using the method represented by the following formula (1). X=(m 1 / 2 ) / (t 1 / 2 ) (1) (In the above formula (1), m 1 / 2 is half the amount of sulfuric acid consumed by magnesium oxide particles at the end of the dissolution test in which the pH of the magnesium oxide suspension is maintained at 3 (mol of sulfuric acid / mol of MgO), and t 1 / 2 is m 1 / 2 is the titration time (s) until

[0010] In order to ensure appropriate dissolution, the magnesium oxide particles of the present invention have a dissolution rate test value (50%) X of 0.00150 or less. The dissolution rate test value (50%) X is preferably 0.00005 to 0.00120, and more preferably 0.00010 to 0.00090.

[0011] Moreover, the magnesium oxide particles preferably have a 7d hydration weight gain of 20% by mass or less. By using magnesium oxide particles exhibiting the above-mentioned 7d hydration weight gain, stable effects can be exhibited for a long period of time. The 7d hydration weight gain is the weight gain rate after the magnesium oxide particles are hydrated for 7 days. The measurement method will be described in detail later. The 7d hydration weight gain of the magnesium oxide particles is more preferably 16% by mass or less, and further preferably 12% by mass or less.

[0012] The 7d hydration weight gain of the magnesium oxide particles can be calculated from the results of the hydration test described below using the following formula (2). 7d Hydration weight increase rate (mass%) = (W1-W0) / W0×100 (2) W0: Magnesium oxide particle weight (g) W1···7d Weight of magnesium particles after hydration (g)

[0013] The crystallite diameter of the magnesium oxide particles in the present invention is preferably 50 to 300 nm. This can ensure more favorable elution properties. The smaller the crystallite diameter of magnesium oxide particles, the faster the elution tends to be. The crystallite diameter of the magnesium oxide particles is more preferably 60 to 250 nm, and further preferably 70 to 200 nm. The crystallite diameter is a value obtained by processing the MgO (002) plane peak in the XRD pattern with analysis software. In general, one particle is a polycrystalline body composed of multiple single crystals, and the crystallite diameter indicates the average size of the single crystals in the polycrystalline body.

[0014] As described later, the magnesium oxide particles of the present invention are obtained from a magnesia sintered body obtained by firing a magnesium compound, and the crystallite size can be controlled by the firing temperature. Magnesia is often produced by thermal decomposition of the magnesium compound used as the raw material, and after fine crystals are generated, crystal growth progresses according to the firing temperature. The crystallite size of the magnesium oxide particles can also be adjusted by the impurity content. Si and the like tend to promote crystal growth, and crystal growth is particularly likely to be promoted in magnesia sintered bodies with an MgO content of 99 mass% or less. Furthermore, it is also possible to reduce the crystallite size of the magnesium oxide particles by pulverizing the magnesia sintered body.

[0015] In addition, magnesium oxide particles have a BET specific surface area of ​​1.8 m 2 / g or less. This ensures more favorable elution properties. The BET specific surface area of ​​the magnesium oxide particles is more preferably 0.05 to 1.8 m 2 / g, more preferably 0.1 to 1.5 m 2 / g.

[0016] The BET specific surface area of ​​magnesium oxide particles can be controlled by the firing temperature of the magnesia sintered body. The higher the firing temperature, the smaller the BET specific surface area tends to be. It is also possible to increase the BET specific surface area by pulverizing the fired magnesia sintered body. In addition, it is also possible to select magnesium oxide particles mainly composed of particles having a desired BET specific surface area by classifying the fired and / or pulverized magnesia sintered body.

[0017] The MgO content of the magnesium oxide particles in the present invention is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 97% by mass or more. The magnesium oxide particles may contain impurities such as Ca, Si, Fe, and Al.

[0018] Impurities can be evaluated using the S / M ratio represented by the following formula (3). S / M=(SiO2 content) / (MgO content) (3) The SiO2 content and MgO content are values ​​calculated by converting the five elements Mg, Ca, Si, Fe, and Al detected by X-ray fluorescence measurement into MgO, CaO, SiO2, Fe2O3, and Al2O3, respectively, and setting the total content (mass%) to 100.

[0019] When the (S / M ratio) is 0.001 to 0.040, the stability is improved, and moisture resistance tends to be maintained even if a large load is applied to the surface during pulverization and classification. It is presumed that the heterophase (Si-Mg compound) formed during firing of the magnesia sintered body retards the internal penetration of deterioration due to moisture absorption, etc. The (S / M ratio) is preferably 0.002 to 0.035, and more preferably 0.002 to 0.030.

[0020] The magnesium oxide particles in the present invention can be obtained by pulverizing a magnesia sintered body and, if necessary, classifying the pulverized material. The magnesia sintered body can be obtained by firing magnesium compounds such as magnesium hydroxide, magnesium carbonate, magnesium chloride, magnesium nitrate, and magnesium sulfate. As the magnesium hydroxide, a product precipitated by the reaction of magnesium salt in seawater with calcium hydroxide can be used. As the magnesium carbonate, magnesite ore can be used.

[0021] The magnesium compound is preferably calcined in air at 1300 to 2800°C. If the temperature is less than 1300°C, the crystallite size tends to be smaller than the specified range and the BET specific surface area tends to be larger than the specified range, and the material is likely to have an excessive dissolution rate. On the other hand, if the temperature exceeds 2800°C, the crystallite size tends to be larger than the specified range and the BET specific surface area tends to be smaller than the specified range, and the material is likely to have an insufficient function as an insolubilizer. The calcination temperature is more preferably 1400 to 2400°C. The calcination time is preferably 10 minutes to 10 hours.

[0022] The content of components in the magnesium oxide particles, including the MgO content, can be adjusted when the magnesia sintered body is fired. Specifically, it can be controlled by selecting the magnesium compound that is the firing raw material and using additives that correspond to impurities such as Si. Considering the production efficiency, it is preferable to adjust the content by selecting and combining the magnesium compound with reference to the amount of impurities in the magnesium compound that is the raw material.

[0023] The SiO2 content can be adjusted by any additive. The additive is not particularly limited, but examples thereof include silica fume, silica sand, sodium silicate, etc. As the magnesium compound, a commercially available product can be used, but a magnesium compound with adjusted components can also be prepared using a known method. In addition, if a magnesia sintered body that meets the specified conditions is available, it can also be used.

[0024] When the magnesia sintered body contains a large amount of coarse particles, it can be crushed to a particle size that is easy to handle. Examples of crushing devices include crushing devices such as hammer crushers, roll crushers, jaw crushers, and impact crushers, and crushing devices such as disk mills, rolling ball mills, vibration ball mills, pin mills, bead mills, jet mills, and cyclone mills. These devices can be used alone or in combination of two or more.

[0025] After pulverization, the mixture can be classified to remove coarse powder and / or fine powder and obtain a desired particle size distribution. The classification method is not particularly limited, and a vibrating sieve, an air classifier, a cyclone classifier, or the like can be used alone or in combination of two or more kinds.

[0026] The magnesia sintered body can be subjected to the above-mentioned pulverization and / or classification process as necessary to adjust the particle size to a predetermined value. The pulverization process and the classification process can be combined appropriately depending on the magnesia sintered body, and the order and number of times are not particularly limited. Either the classification process or the pulverization process can be performed first, and the magnesia sintered body that has been subjected to the pulverization process can be further subjected to the pulverization process after the classification process.

[0027] The magnesium oxide particles satisfying the above-mentioned requirements can be suitably used as an insolubilizing material for insolubilizing heavy metals in soil. The insolubilizing material of the present invention can be used to suppress the elution of heavy metals into the surrounding environment, for example, by mixing with the object to be insolubilized, using in an adsorption layer method, or incorporating into a sheet-like structure or other structure that comes into contact with the object to be insolubilized. EXAMPLES

[0028] The present invention will be described in detail below with reference to examples. However, the object of the present invention is not limited to these examples, and the present invention is not limited to these examples.

[0029] <Production of Magnesium Oxide Particles> As the magnesium compound of the raw material, magnesium hydroxide obtained by the reaction of seawater and slaked lime was prepared. The component content in magnesium hydroxide is determined by the impurities from slaked lime, the presence or absence of the impurity removal process, and additives. Magnesium hydroxide was calcined to produce a magnesia sintered body, and magnesium oxide particles serving as examples and comparative examples were manufactured by combining pulverization and classification. In the production of the magnesium oxide particles, the firing temperature, pulverization, and classification were controlled so that the crystallite diameter and BET specific surface area of the magnesium oxide particles would be the values shown in Table 1. The firing temperature and the presence or absence of pulverization and classification are as shown in Table 1. For pulverization, an impact crusher and a cyclone mill were used, and for classification, screening and air classification were used.

[0030] Regarding the magnesium oxide particles of the examples and comparative examples, the BET specific surface area, crystallite diameter, and contained components were determined. The respective evaluation methods are as follows.

[0031] <BET Specific Surface Area> Using a fully automatic BET specific surface area measuring device (manufactured by Mountech Co., Ltd., Macsorb Model-1210), after degassing at 180 °C for 10 minutes as a pretreatment, measurement was performed by the BET one-point method.

[0032] <Crystallite Diameter> First, using an X-ray diffractometer (NEW D8 ADVANCE manufactured by Bruker AXS), an XRD pattern was obtained under the following conditions. X-ray source: CuKα (Ni filter) Tube voltage: 40 kV Tube current: 40 mA Detector: 1-dimensional semiconductor high-speed detector LynxEye Divergence slit: 0.30 degrees Step size: 0.020 degrees Counting time: 0.50 seconds / step The crystallite size was calculated from the obtained XRD pattern using analysis software (DIFFRAC.EVA V.3.2 manufactured by Bruker AXS). The MgO (002) plane peak in the XRD pattern was specified, and the value calculated as the crystallite size based on the half-width was used.

[0033] <Measurement of ingredients> The components of magnesium oxide particles were measured by the glass bead method using lithium tetraborate as a fusible material, using an X-ray fluorescence analyzer (Rigaku Supermini 200). A calibration curve prepared from the Refractories Association standard material, magnesia refractories for X-ray fluorescence analysis (JRRM401-410), was used for quantitative analysis of the detected characteristic X-rays.

[0034] The five elements Mg, Ca, Si, Fe, and Al detected by X-ray fluorescence measurement were converted to MgO, CaO, SiO2, Fe2O3, and Al2O3, respectively. The S / M ratio was calculated by the following formula (3) using the SiO2 content and MgO content when the total content (mass%) was set to 100. S / M=(SiO2 content) / (MgO content) (3) The results obtained are summarized in Table 1 below together with the production conditions.

[0035] [Table 1]

[0036] The magnesium oxide particles of the examples and comparative examples were evaluated for dissolution, hydration weight gain, and As insolubilization ability by the following methods.

[0037] <Dissolution rate test> First, 50 mg of magnesium oxide particles were dispersed in 100 mL of ion-exchanged water to prepare a magnesium oxide suspension. Using an automatic potentiometric titrator (Kyoto Electronics Manufacturing, AT-510), 0.05 mol / L of sulfuric acid was added dropwise while stirring the magnesium oxide suspension to maintain the pH of the magnesium oxide suspension at 3, and the amount of sulfuric acid consumed (CS(1)) (mol sulfuric acid / mol MgO) required to maintain the pH was determined. The end point of the measurement was determined to be 1 hour after the start of the measurement or the time when it was determined from the amount of sulfuric acid consumed that all of the MgO in the magnesium oxide suspension had been consumed, and the time from the start of the measurement to the end point was defined as the titration time (s).

[0038] The same measurement was performed on 100 mL of ion-exchanged water to determine the blank sulfuric acid consumption (CS(0)) (mol sulfuric acid / mol MgO). The sulfuric acid consumption (mol sulfuric acid / mol MgO) at the end point by the magnesium oxide suspension was calculated by subtracting the sulfuric acid consumption (CS(0)) (mol sulfuric acid / mol MgO) at the end point by the blank from the sulfuric acid consumption (CS(1)) (mol sulfuric acid / mol MgO) at the end point by the magnesium oxide particles.

[0039] The amount of sulfuric acid consumed by the magnesium oxide particles at the end point (mol of sulfuric acid / mol of MgO) was calculated as m 1 / 2 is half the amount of sulfuric acid consumed by magnesium oxide particles at the end point (mol of sulfuric acid / mol of MgO), and t 1 / 2 is m 1 / 2 The titration time (s) required to reach the value is the time required for titration to reach the value. The dissolution rate test value (50%) X corresponds to the dissolution test slope (50%). If the dissolution rate test value (50%) X represented by the following formula (1) is 0.00150 or less, the drug has an appropriate dissolution rate. X=(m 1 / 2 ) / (t 1 / 2 ) (1)

[0040] <Hydration test> 10 g of magnesium oxide particles were mixed with 500 mL of ion-exchanged water and allowed to stand at room temperature for 7 days. The dispersion after standing was subjected to solid-liquid separation by suction filtration (5C filter paper), and the solid content was vacuum dried at room temperature to obtain hydrated magnesium particles. The weight of the hydrated magnesium particles was measured, and the 7-day hydration weight increase rate (mass %) was determined from the following formula (2). 7-day hydration weight increase rate (mass %) = (W1 - W0) / W0 × 100 (2) W0 ··· Weight of magnesium oxide particles (g) W1 ··· Weight of magnesium particles after 7-day hydration (g) The smaller the 7-day hydration weight increase rate, the more it can be expected to exhibit a long-term retention effect in the use environment. On the other hand, the larger the 7-day hydration weight increase rate, the higher the possibility that the rate of outflow to the outside of the system through digestion and elution in the use environment will increase.

[0041] <As insolubilization test> The As insolubilizing ability can be evaluated by an As insolubilization test. First, an As standard solution (100 ppm, commercially available product) was diluted with ion-exchanged water, and the pH was adjusted to 3 using sulfuric acid to prepare an adjusted As solution (1 ppm). 250 ml of the obtained adjusted As solution was placed in a plastic container together with 1.0 g of MgO particles and shaken using a shaker. Specifically, it was shaken horizontally 200 times per minute with an amplitude of 4 - 5 cm for 24 hours. The dispersion after shaking was subjected to solid-liquid separation by suction filtration using a 45 μm filter. The As concentration in the separated liquid was measured by ICP-MS, and the As insolubilization rate was calculated according to the following formula (4). As insolubilization rate = (C0 - C) / C0 × 100 (4) C0 ··· Concentration of adjusted As solution (ppm) C ··· As solution concentration after the test (ppm)

[0042] The obtained results are summarized in Table 2 below.

[0043]

Table 2

[0044] The magnesium oxide particles of the Examples all had a dissolution rate test value (50%) X of 0.00150 or less, indicating that they had appropriate dissolution properties. Moreover, the magnesium oxide particles of the Examples had a 7d hydration weight gain rate of 20% by mass or less. In contrast, the magnesium oxide particles of the Comparative Examples had a dissolution rate test value (50%) X of more than 0.00150, indicating that they had excessively fast dissolution.

[0045] The magnesium oxide particles of Comparative Example, which had a fast dissolution rate, had a large hydration weight gain rate of 23% or more, while the magnesium oxide particles of Examples 1 to 3, which had a slow dissolution rate, had an extremely small weight gain. The weight gain in the hydration test indicates the amount of magnesium hydroxide produced by the reaction of magnesium oxide with water. Since magnesium hydroxide is water-soluble, when rainwater or the like passes through a system in which highly reactive magnesium oxide is blended as an insolubilizer as in the Comparative Example, there is a high possibility that Mg will be eluted out of the system as magnesium hydroxide. On the other hand, by using magnesium oxide as in the Examples, it is expected that it will remain in the system as an insolubilizer for a long period of time and be effective, even in an environment where rainwater or the like passes through the system.

[0046] Furthermore, from the results of the As removal test, in a test simulating the insolubilization of heavy metals in an acidic soil environment over a short period of time, the magnesium oxide particles of Examples 1 to 3 showed insolubilization ability at the same level as the lightly fired products of Comparative Examples 1 and 2. Conventionally, heavily fired products fired at high temperatures have been considered to have low reactivity and inferior insolubilization ability, but the magnesium oxide particles of the Examples can provide good results even in insolubilization over a short period of time.

[0047] The magnesium oxide particles of the comparative example have a BET specific surface area of ​​1.8 m 2 / g, whereas the magnesium oxide particles of the examples all have a BET specific surface area of ​​1.8 m 2 / g or less and a crystallite size in the range of 50 to 300 nm. These physical properties are presumed to also contribute to the appropriate dissolution properties of the magnesium oxide particles of the examples.

Claims

1. An insolubilizing material that insolubilizes heavy metals, An insolubilizing material comprising magnesium oxide particles having a dissolution rate test value (50%) X represented by the following formula (1) of 0.00150 or less. X=(m 1/2 ) / (t 1/2 ) (1) (In the above formula (1), m 1/2 is half the amount of sulfuric acid consumed (mol sulfuric acid / mol MgO) by magnesium oxide particles at the end point of the dissolution test in which the pH of the magnesium oxide suspension is maintained at 3, and t 1/2 is m 1/2 is the titration time (s) until

2. 2. The insolubilizing material according to claim 1, wherein the magnesium oxide particles have a 7d hydration weight increase rate, represented by the following formula (2), of 20 mass % or less. 7-day water absorption weight gain rate (mass %) = (W 1 − W 0 ) / W 0 × 100 (2) W 0 ...Magnesium oxide particle weight (g) W 1 ...7d Magnesium particle weight after hydration (g)

3. The magnesium oxide particles have a crystallite diameter of 50 to 300 nm and a BET specific surface area of ​​1.8 m 2 The insolubilizing material according to claim 1, wherein the molecular weight of the insolubilizing material is 1 / g or less.

4. 2. The insolubilizing material according to claim 1, wherein the magnesium oxide particles have an MgO content of 90 mass % or more and an S / M ratio represented by the following formula (3) of 0.001 to 0.040: S / M = (SiO 2 Content rate) / (MgO content rate) (3) (SiO 2 The content and MgO content are the five elements Mg, Ca, Si, Fe, and Al detected by fluorescent X-ray measurement, respectively, as MgO, CaO, SiO 2 , Fe 2 O 3 , Al 2 O 3 The total content (mass%) of the converted components is taken as 100.)

Citation Information

Patent Citations

  • Magnesium oxide powder for soil hardening material

    JP2007084360A

  • Soil solidifier

    JP2007161838A

  • Soil solidifier

    JP2007161839A

  • Heavy metal insolubilizer and heavy metal contaminated soil treatment agent