Flame retardant processing agent such as polyester, and method for producing fiber-dyed material
A flame retardant processing agent for polyester fibers uses bromine and phosphorus compounds with surfactants to adsorb flame retardants, addressing dye aggregation and ensuring uniform dyeing while reducing environmental impact.
Patent Information
- Application Number
- JP2023056254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Polyester fibers are prone to fire spread and require high amounts of halogen-containing flame retardants, leading to dye aggregation, contamination, and non-uniform dyeing, which increases energy consumption and waste, and non-halogen alternatives need improvement for environmental protection.
A flame retardant processing agent combining bromine-containing and phosphorus-containing flame retardants with anionic surfactants and optional ethylene oxide adducts is used to adsorb flame retardants into fibers, preventing dye aggregation and ensuring uniform dyeing.
The agent suppresses dye and flame retardant aggregation, providing uniform dyeing and improved environmental performance by reducing waste and energy consumption.
Smart Images

Figure 2024143526000001 
Figure 2024143526000002 
Figure 2024143526000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame retardant for fibers such as polyester. More specifically, the present invention relates to a flame retardant for fibers such as polyester, which imparts flame retardancy to polyester fibers and gives a uniform dyed product without agglomerating dyes and flame retardants when the polyester fibers are dyed at high temperatures. [Background technology]
[0002] Polyester fibers are prone to flame spread when exposed to flame, and for interior fabrics and fabrics for automobile interiors, flame retardancy is imparted during dyeing or in a post-process using flame retardant processing agents. These flame retardant processing agents include halogen-containing flame retardant processing agents and non-halogen flame retardant processing agents, such as phosphorus-containing compounds, and from the perspective of environmental protection, much research has been conducted on phosphorus-containing flame retardants (Patent Documents 1 and 2). However, since phosphorus-containing flame retardants require a large amount of additives to obtain the required flame retardant performance, the current situation is that from the perspective of performance, flame retardants that use halogen-containing flame retardants as the main component are often used.
[0003] Typically, polyester fibers are dyed using disperse dyes in an aqueous solution system at 110 to 140°C under high temperature and pressure in a weakly acidic pH range, and flame retardants are added during the dyeing process to be imparted to the fibers.
[0004] Regarding the application of flame retardants during dyeing, with typical flame retardant agents, 50-60% of the flame retardant structure contained in the agent is absorbed into the fiber, and the remaining flame retardant structure is discarded as waste liquid, so improvements are required from the standpoint of environmental protection and cost.
[0005] Furthermore, in the dyeing process where flame retardants are used in combination, the flame retardant components in the flame retardant agent cause coagulation with the dye, resulting in contamination of the dyed item and the dyeing machine, or in the case of flame retardant components with a crystallization temperature, crystallization occurs on the fiber surface, deteriorating the texture of the dyed item and even worsening the flame retardant performance of the dyed item itself. Re-dyeing of the dyed item due to defective dyeing or insufficient flame retardant performance leads to a decrease in energy efficiency and an increase in running costs due to increased wastewater.
[0006] In order to solve such problems, flame retardants having a uniformly dispersed state, as disclosed in Patent Documents 3, 4 and 5, have been developed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-006992 A [Patent Document 2] Patent Application No. 2005-506799 [Patent Document 3] JP 2011-12352 A [Patent Document 4] JP 2019-94577 A [Patent Document 5] JP 2012-167411 A Summary of the Invention [Problem to be solved by the invention]
[0008] The object of the present invention is to provide a flame retardant agent which, when dyeing fibers such as polyester using a combination of a dye and a functional agent such as a flame retardant agent under high temperature and pressure, can efficiently adsorb a flame retardant component in the flame retardant agent into the interior of the fiber, prevent dye aggregation and aggregation between the dye and the functional agent, and provide a uniformly dyed product. [Means for solving the problem]
[0009] As a result of extensive research into solving the above problems, the inventors have discovered a flame retardant that has good emulsification and dispersibility of flame retardant components, suppresses dye aggregation and crystallization on the fiber surface when used in combination with a flame retardant during dyeing of fibers such as polyester under high temperature and pressure, adsorbs the flame retardant components into the interior of the fiber, and can provide a uniformly dyed product.
[0010] The present invention provides a flame retardant processing agent obtained by dispersing (A) a bromine-containing flame retardant and (B) a phosphorus-containing flame retardant using (C) an anionic surfactant represented by the following general formula (1) and (D) a nonionic surfactant represented by the following general formula (2), and optionally (E) an aromatic ring-containing polyoxyethylene alkyl ether, by a general emulsification dispersion method, thereby uniformly emulsifying and dispersing (A) the bromine-containing flame retardant and (B) the phosphorus-containing flame retardant.
[0011] That is, the present invention provides a flame retardant comprising the following components (A) to (D), (A) Bromine-containing flame retardant 10 to 50 parts by mass (B) Phosphorus-containing flame retardant: 2 to 15 parts by mass (C) an oxyalkylene group (A 3 O) having an average added mole number of 5 to 60 0.3 to 8 parts by mass [ka] (In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms, M' is a hydrogen atom, NH4 + , or a monovalent metal ion), and (D) an oxyalkylene group (A 3 O) having an average added mole number of 6 to 25, 3 to 15 parts by mass [ka] (In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms. Contains The present invention provides the flame retardant, wherein the component (D) is a combination of a compound (D1) represented by the above formula (2) having an average number of moles of oxyalkylene groups added of 6 to 13 and a compound (D2) represented by the above formula (2) having an average number of moles of oxyalkylene groups added of 14 to 25, and the mass ratio of compound (D1) / compound (D2) is 8 / 1 to 2 / 1.
[0012] The present invention further provides the flame retardant as described above, further comprising at least one component selected from the following [1] to [6]: [1] The composition further contains (E) an ethylene oxide adduct of chlorophenol or an ethylene oxide adduct of benzoic acid in an amount of 1 to 15 parts by mass per 100 parts by mass of the flame retardant. [2] The average number of moles of ethylene oxide added in the component (E) is 0.3 to 30 moles. [3] In the above formula (1), M' is an ammonium ion, an organic ammonium ion, a sodium ion, or a potassium ion. [4] In the formula (1), M' is an ammonium ion, and A 3 is ethylene. [5] Also contains a solvent. [6] The flame retardant processing agent, which is for polyester-based fibers.
[0013] The present invention also provides a method for producing a dyed fiber, comprising the steps of adding the flame retardant to a dyebath and dyeing a fiber with the dyebath to obtain a dyed product, the method further comprising at least one component selected from the following [1] and [2]: [1] The above-mentioned production method, wherein the amount of the flame retardant added is 3 to 30% by weight based on the item to be dyed. [2] The above-mentioned method, wherein the fiber is polyester.
[0014] Furthermore, the present invention provides a flame retardant processing agent for use with fibers such as polyester, which, when dyeing with a flame retardant processing agent under high temperature and pressure, effectively adsorbs a flame retardant component to fibers such as polyester, suppresses aggregation with the dye and crystallization on the fiber surface, and can provide a uniformly dyed product. Effect of the Invention
[0015] The flame retardant of the present invention can suppress the generation of aggregates of dyes and flame retardants during high-temperature dyeing treatment of fibers such as polyester, and can provide uniformly dyed, high-quality dyed products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Each component will be described in more detail below.
[0017] The component (A) is a bromine-containing flame retardant. Examples of the bromine-containing flame retardant include hexabromocyclododecane, decabromodiphenyl ether, tetrabromobisphenol A, bis(pentabromophenyl)ethane, tribromophenol, ethylenebistetrabromophthalimide, and brominated polystyrene. The bromine-containing flame retardant may be a commercially available bromine-containing flame retardant. More specifically, tris(2,3-dibromopropyl)isocyanurate, which is often used for polyester fibers, is suitable.
[0018] The amount of component (A) contained in the flame retardant of the present invention is 10 to 50% by mass, preferably 12 to 45% by mass, and more preferably 15 to 40% by mass, based on the total mass of the flame retardant.
[0019] The (B) component is a phosphorus-containing flame retardant. Examples of the phosphorus-containing flame retardant include resorcinol bisdiphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, tris(chloropropyl) phosphate, tris(dichloropropyl) phosphate, bisphenol A bis(diphenyl phosphate), biphenyl diphenyl phosphate, and trixylenyl phosphate. The phosphorus-containing flame retardant may be a commercially available product.
[0020] The amount of component (B) contained in the flame retardant of the present invention is 2 to 20 mass %, preferably 3 to 18 mass %, and more preferably 4 to 15 mass %, based on the mass of the entire flame retardant.
[0021] The component (C) is a compound represented by the following general formula (1), and has an average added mole number of oxyalkylene groups of 5 to 60. The average added mole number of oxyalkylene groups is more preferably 8 to 50, and further preferably 10 to 40. [ka] In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms, and M' is a hydrogen atom or NH4 + and a monovalent metal ion. The monovalent metal ion is preferably a sodium ion or a potassium ion. Preferably, M' is NH4 + It is.
[0022] The compound represented by the above general formula (1) is important in that it enhances the stability of the flame retardant and enhances the dispersibility of the flame retardant component in the dyeing solution during dyeing. In the present invention, the group represented by C6H5-CH(CH3)- is called a styryl group. A structure in which the styryl group is bonded to a phenyl ether is called a styrenated phenyl ether, and a phenol having a styryl group is called a styrenated phenol.
[0023] In the above formula (1), m represents the average number of moles of styryl groups added, and does not necessarily have to be an integer. m is 1 to 3, and more preferably 2 to 3.
[0024] A 3is an alkylene group having 2 to 4 carbon atoms, preferably 2 or 3 carbon atoms, and more preferably an ethylene group having 2 carbon atoms. n is the number of oxyalkylene groups, and may be any number that results in the above average number of moles added, and is, for example, a number from 1 to 70, more preferably a number from 3 to 60, and even more preferably a number from 5 to 50. The above component (C) may contain a compound having n outside the above range, so long as the average number of moles added of oxyalkylene groups falls within the above range.
[0025] The above component (C) preferably includes ammonium salts and metal (Na, K) salts of polyoxyethylene tristyrenated phenyl ether sulfate.
[0026] The preparation of component (C) may be performed according to a conventional method. For example, polyoxyethylene styrenated phenyl ether sulfate ammonium salt and metal (Na, K) salt can be produced by reacting phenol with styrene monomer under normal conditions, followed by addition of ethylene oxide. Then, sulfonic acid can be introduced into polyoxyalkylene glycol by a general sulfonation or sulfation method, and neutralization can be performed as necessary.
[0027] The amount of component (C) contained in the flame retardant of the present invention is 0.3 to 8 mass %, preferably 0.4 to 5 mass %, and more preferably 0.5 to 3 mass %, based on the mass of the entire flame retardant.
[0028] The component (D) is a compound represented by the following general formula (2) and has an average number of moles of oxyalkylene groups added of 6 to 25. The average number of moles of oxyalkylene groups added is more preferably 8 to 23, and even more preferably 9 to 21. The present invention ensures the stability of the flame retardant by combining a compound represented by the following general formula (2) having a high average number of moles added (high oxyalkylene adduct) with a compound having a low average number of moles added (low oxyalkylene adduct). In the present invention, the high oxyalkylene adduct is a compound having an average number of moles of oxyalkylene groups added of 14 to 25 moles, preferably 16 to 23 moles, and more preferably 18 to 21 moles. The low oxyalkylene adduct is a compound having an average number of moles of oxyalkylene groups added of 6 to 13 moles, preferably 8 to 11 moles, and more preferably 9 to 10 moles. [ka] (In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms.
[0029] That is, the present invention is characterized in that the component (D) is a combination of a compound (D1) having an average number of moles of oxyalkylene groups added of 6 to 13 in the above formula (2) and a compound (D2) having an average number of moles of oxyalkylene groups added of 14 to 25, and the mass ratio of compound (D1) / compound (D2) is 8 / 1 to 2 / 1, more preferably 7 / 1 to 3 / 1, and further preferably 6 / 1 to 5 / 1. A combination in which the mass ratio of compound (D2) to the mass of compound (D1) is high is preferred.
[0030] The compound represented by the above formula (2) is, in detail, a polyoxyalkylene-containing styrenated phenyl ether, and is important in that it exerts the effect of emulsifying and dispersing the flame retardant components in the flame retardant processing agent in the solution. In the present invention, the group represented by C6H5-CH(CH3)- is called a styryl group. Also, a structure in which the styryl group is bonded to a phenyl ether is called a styrenated phenyl ether, and a phenol having a styryl group is called a styrenated phenol.
[0031] In the above formula (2), m represents the average number of moles of styryl groups added, and does not necessarily have to be an integer. m is 1 to 3, and more preferably 2 to 3.
[0032] A 3 is an alkylene group having 2 to 4 carbon atoms, preferably 2 or 3 carbon atoms, and more preferably an ethylene group having 2 carbon atoms. n is the number of oxyalkylene groups in the compound represented by formula (2) above, and may be any number that results in the above average number of moles added, and is, for example, a number from 1 to 35, more preferably 3 to 33, and even more preferably 4 to 31. Compound (D1) and compound (D2) may contain a compound having n outside the above range, as long as the average number of moles added of oxyalkylene groups falls within the above range.
[0033] Component (D) may be prepared by a conventional method, for example, by reacting phenol with a styrene monomer under normal conditions, followed by addition of ethylene oxide.
[0034] The amount of component (D) contained in the flame retardant of the present invention is 3 to 15 mass %, preferably 4 to 13 mass %, more preferably 5 to 10 mass % based on the total mass of the flame retardant. A combination of multiple types having different numbers of moles of oxyalkylene added can be used.
[0035] The flame retardant of the present invention preferably further contains (E) an ethylene oxide adduct of chlorophenol or an ethylene oxide adduct of benzoic acid, which improves the stability of the flame retardant and enhances the absorption of the flame retardant component into the fiber during dyeing.
[0036] The average number of moles of ethylene oxide (EO) added in the component (E) is from 0.3 to 30 moles, more preferably from 0.5 to 20 moles, and even more preferably from 0.8 to 10 moles. The average number of moles added does not have to be an integer.
[0037] The amount of component (E) contained in the flame retardant of the present invention is 1 to 15 mass %, preferably 2 to 13 mass %, and more preferably 3 to 10 mass %, based on the mass of the entire flame retardant.
[0038] The flame retardant of the present invention may contain water and / or a solvent for the purpose of improving the appearance stability of the agent and the solubility when added to a dye solution.
[0039] The flame retardant of the present invention is used in combination with dyeing of polyester fibers and in a treatment step in a functionality imparting step. Examples of polyester fibers include polyester fibers, cationic dyeable polyester fibers, regenerated polyester fibers, and polyester fibers made of two or more of these. Other fibers include textile products made of blends of the polyester fibers with natural fibers (cotton, hemp, silk, wool, etc.), semi-synthetic fibers (rayon, acetates, etc.), and other synthetic fibers (nylon, acrylic, polyamide, polyurethane, polyethylene, polypropylene, etc.). The fiber treatment aid of the present invention is preferably a fiber treatment aid for polyester fibers.
[0040] The form of the fiber product is not particularly limited, and may be short fiber, long fiber, thread, woven fabric, knitted fabric, nonwoven fabric, or the like.
[0041] In the dyeing and functionality imparting processing using the flame retardant of the present invention, additives such as dyeing assistants, deodorants, antibacterial agents, softeners, water absorbents, water and oil repellents, smoothing agents, penetrants, antistatic agents, chelating agents, antioxidants, defoamers, carrier agents, fixing agents, light stabilizers, UV absorbers, thickeners, and yellowing inhibitors can be used as necessary within the range that does not impair the effects of the present invention. These additives can be used simultaneously with the dyeing process of fibers such as polyester using the flame retardant of the present invention and / or in the pretreatment process and / or posttreatment process.
[0042] Method for producing dyed textiles The present invention provides a method for producing a dyed fiber, which comprises the steps of adding the flame retardant to a dye bath and dyeing a fiber in the dye bath to obtain a dyed product imparted with flame retardancy. The dyeing method for fibers such as polyester may be performed according to a conventional method. For example, a fabric to be dyed, a dye, a dyeing assistant, other additives for imparting functionality, and the flame retardant of the present invention may be added to a dye bath liquid adjusted to pH 4.5 to 6.0, and dyeing may be performed at any dyeing temperature using a dyeing machine. The dyeing temperature may be 80°C to 150°C, preferably 100°C to 140°C, and the pressure may be 0.00MPa to 0.80MPa, preferably 0.05MPa to 0.60MPa.
[0043] The composition of the dye bath may be in accordance with a conventional dyeing method. The amount of the flame retardant added to the dye bath may be appropriately adjusted, but is preferably 3 to 30% by weight, and more preferably 5 to 20% by weight, based on the material to be dyed. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0045] [Performance evaluation test method] (Preparation of test solution 1) Test solution 1 was prepared by adding 10 g / L of a flame retardant prepared by the method described below, 0.3 g / L of acetic acid, and 0.4 g / L of Toho Salt UF-350C (a mixture of nonionic and anionic surfactants, manufactured by Toho Chemical Industry Co., Ltd.) as a dyeing assistant to 1 L of water as a solvent and mixing them. (Preparation of test solution 2) Test solution 2 was prepared by adding 0.5 g / L of NaOH, 2.0 g / L of sodium dithionite, and 0.2 g / L of Neoscore SD-110A (nonionic surfactant) (manufactured by Toho Chemical Industry Co., Ltd.) as a soaping agent to 1 L of water as a solvent and mixing them. (Flame retardant treatment) A test cloth (weight M1) of unprocessed polyester fabric adjusted to a constant weight with an error of 0-1% and the above test liquid 1 in an amount 10 times the weight of the test cloth were placed in the pot of the dyeing tester, and processing was carried out for 30 minutes at 0.30 MPa and 130°C. After processing, the test cloth was rinsed, and the above test liquid 2 in an amount 10 times the weight of the test cloth was placed in the dyeing pot, and a soaping treatment was carried out for 20 minutes at 80°C. After dyeing, the test cloth was removed from the pot, washed with water, and dried to obtain a test cloth for evaluation. (weight M2)
[0046] (1) Measurement of flame retardant exhaustion rate in flame retardant processing agents (Calculation of exhaustion rate) The weight of the test cloth obtained by carrying out the above flame retardant treatment up to the soaping treatment without using a flame retardant was designated as M0, and the flame retardant exhaustion rate was calculated by the following formula. Exhaustion rate (%) = 100 × {(M2-M0) / weight of flame retardant component contained in the amount of test liquid 1 used (g)}
[0047] (2) Flame retardancy evaluation The test cloth obtained by the above flame retardant treatment was subjected to the following measurements according to JIS L 1091A-1 (45° microburner method): flame remaining time (seconds), dust remaining time (seconds), and charred area (cm 2 In the 3-second flame heating test, the residual flame was within 3 seconds, the residual dust was within 5 seconds, and the charred area was 30 cm 2 If the test results were within the range, the test was deemed to have passed. If the test results were not within the range, the test was deemed to have failed. Each test was performed three times, and the average value was calculated.
[0048] (3) Evaluation of texture A panel of 10 experts compared the feel of the evaluation test cloth obtained by the above-mentioned flame retardant processing with that of a test cloth treated without using a flame retardant (untreated cloth) using a score in increments of 1 within the range of 4 (maximum value) to 1 (minimum value) based on the following scoring criteria, and the average score of the 10 expert panelists was calculated. 4: The fabric has a soft feel 3: The texture is the same as that of untreated fabric. 2: Feels harder than untreated fabric 1: There is a clear sense of roughness and stiffness
[0049] (4) Stability of formulation 100 ml of the flame retardant prepared as described below was placed in a 100 ml glass container and stored for one month at 25° C. After one month, the volume ratios of the separated upper and lower layers were compared, and those with less than 5% separation were marked with an ◯, and those with 5% or more separation were marked with an ×.
[0050] (5) Confirmation of agglomerates when heated at high temperatures (Preparation of test solution) Test liquid 3 was prepared by adding 10 g / L of a flame retardant prepared by the method described below, 1 g / L of a disperse dye (red, CI60), 0.3 g / L of acetic acid, and 0.4 g of a dyeing assistant, Toho Salt UF-350C, to 1 L of water as a solvent. The test liquid 3 was heated in a glass container while being mixed, and heated for 10 minutes under boiling temperature conditions of 95°C to 105°C. After heating, the mixture was filtered using a funnel and a test cloth, and the amount of aggregates remaining on the filter cloth that were generated during boiling and evaporation of the test liquid was confirmed. The smaller the number of aggregates that were generated, the better the dispersion ability. The presence or absence and amount of aggregates were visually confirmed, and evaluation was performed according to the following criteria. (evaluation) ◎ No dirt is visible on the filter cloth. ○One or two small aggregates are observed on the filter cloth. △ Many small aggregates are observed on the filter cloth. ×: Many large aggregates are observed on the filter cloth.
[0051] (6) Surface observation The fiber surface of the evaluation test cloth obtained by the above flame retardant processing was observed at a magnification of 200 times using a scanning electron microscope with EDX (energy dispersive X-ray analysis) function (Hitachi tabletop microscope TM3030Plus, manufactured by Hitachi High-Tech Corporation). Furthermore, elemental analysis was performed on the surface deposits to identify the crystallized bromine-containing flame retardant that had crystallized on the fiber surface. Observations were performed at random 5 x 5 points, and the number of places where crystals of the bromine-containing flame retardant had precipitated was counted. ◎ Observed at less than five measurement points. ○: Observed at measurement points with 5 or more but less than 10 points. △: Observed at measurement points with 10 or more but less than 20 points. ×: Observed at 20 or more measurement points.
[0052] [Examples and Comparative Examples] Flame retardant adjustment Each component was charged into a vertical bead mill (AIMEX Easy Nano RMB2 wet grinder) according to the formulation shown in Table 1 or 2, and zirconia beads with a diameter of 0.5 mm of the same volume as the charged amount were added, and emulsification and dispersion processing was carried out for 4 hours at a peripheral speed of 4 to 8 m / s. It was confirmed that the d50 of the volume average particle diameter of the flame retardant after emulsification and dispersion processing was 0.5 to 1.0 μm, and the zirconia beads were removed by filter filtration to recover the target flame retardant.
[0053] The components used in the following examples and comparative examples are as follows. (A) Bromine-containing flame retardant: Tris(2,3-dibromopropyl)isocyanurate (manufactured by Manac Corporation, product name EB-70) (B1) Phosphorus-containing flame retardant 1: Biphenyl diphenyl phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name BDP) (B2) Phosphorus-containing flame retardant 2: Bisphenol A bis(diphenyl phosphate) (manufactured by ADEKA Corporation, product name Adeka STAB FP-600) (B3) Phosphorus-containing flame retardant 3: Tricresyl phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name TCP) (B4) Phosphorus-containing flame retardant 4: Resorcinol polyphenyl phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., product name CR-733S) (C1) Polyoxyethylene tristyrenated phenol sulfate ammonium salt (average EO addition mole number: 18) (C2) Polyoxyethylene tristyrenated phenol sulfate ammonium salt (average EO addition mole number: 30) (D1) Polyoxyethylene tristyrenated phenol (average EO addition mole number: 9) (D2) Polyoxyethylene tristyrenated phenol (average EO addition mole number: 18) (D3) Polyoxyethylene tristyrenated phenol (average EO addition mole number: 30) (E1) Polyoxyethylene chlorophenol (average EO addition mole number: 1.2) (E2) Polyoxyethylene chlorophenol (average EO addition mole number: 6) (E3) Polyoxyethylene benzoic acid (average EO addition mole number: 1.5) (E4) Polyoxyethylene benzoic acid (average EO addition mole number: 3)
[0054] The components (C1) to (C2), (D1) to (D3), and (E1) to (E4) were produced by the following methods. Ingredient (C1): A 5L autoclave was charged with 400g of styrenated phenol (main component: tristyrenated phenol) and 2.5g of potassium hydroxide, and the inside of the vessel was thoroughly replaced with nitrogen. The temperature was raised to 150°C, and 790g of ethylene oxide was gradually added to obtain polyoxyethylene (18 moles) tristyrenated phenyl ether. Next, 500g of the obtained polyoxyethylene (18 moles) tristyrenated phenyl ether, 35.2g of sulfamic acid, and 21.7g of urea were charged into a 1L glass flask, and the temperature was gradually raised to 120°C to react, obtaining polyoxyethylene (18 moles) tristyrenated phenyl ether sulfate ammonium salt. The anion purity of the product synthesized by combined sulfuric acid was 85% or more. The average number of moles of styryl groups added was 2.8 moles.
[0055] Component (C2): A 5L autoclave was charged with 400g of styrenated phenol (main component: tristyrenated phenol) and 3.0g of potassium hydroxide, and the inside of the vessel was thoroughly replaced with nitrogen. The temperature was raised to 150°C, and 1320g of ethylene oxide was gradually added to obtain polyoxyethylene (30 moles) tristyrenated phenyl ether. Next, 500g of the obtained polyoxyethylene (30 moles) tristyrenated phenyl ether, 37.0g of sulfamic acid, and 22.9g of urea were charged into a 1L glass flask, and the temperature was gradually raised to 120°C to react, obtaining polyoxyethylene (30 moles) tristyrenated phenyl ether sulfate ammonium salt. The anion purity of the product synthesized by combined sulfuric acid was 85% or more. The average number of moles of styryl groups added was 2.8 moles.
[0056] Ingredient (D1): A 5L autoclave was charged with 400g of styrenated phenol (main component: tristyrenated phenol) and 2.5g of potassium hydroxide, and the inside of the vessel was thoroughly replaced with nitrogen. The temperature was raised to 150°C, and 395g of ethylene oxide was gradually added to obtain polyoxyethylene (9 moles) tristyrenated phenyl ether. The average number of moles of styryl groups added was 2.8 moles.
[0057] Ingredients (D2): A 5L autoclave was charged with 400g of styrenated phenol (main component: tristyrenated phenol) and 2.5g of potassium hydroxide, and the inside of the vessel was thoroughly replaced with nitrogen. The temperature was raised to 150°C, and 790g of ethylene oxide was gradually added to obtain polyoxyethylene (18 moles) tristyrenated phenyl ether. The average number of moles of styryl groups added was 2.8 moles.
[0058] Ingredient (D3): A 5L autoclave was charged with 400g of styrenated phenol (main component: tristyrenated phenol) and 5.3g of potassium hydroxide, and the inside of the vessel was thoroughly replaced with nitrogen. The temperature was raised to 150°C, and 1316g of ethylene oxide was gradually added to obtain polyoxyethylene (30 moles) tristyrenated phenyl ether. The average number of moles of styryl groups added was 2.8 moles.
[0059] Ingredient (E1): A 5L autoclave was charged with 400g of o-chlorophenol and 0.3g of potassium hydroxide, and the inside of the autoclave was thoroughly replaced with nitrogen. The temperature was then raised to 160°C, and 164g of ethylene oxide was gradually added to obtain polyoxyethylene (1.2 mol) chlorophenol.
[0060] Ingredient (E2): A 5L autoclave was charged with 400g of o-chlorophenol and 0.5g of potassium hydroxide, and the inside of the autoclave was thoroughly replaced with nitrogen. The temperature was then raised to 160°C, and 821g of ethylene oxide was gradually added to obtain polyoxyethylene (6 mol) chlorophenol.
[0061] Component (E3): A 5 L autoclave was charged with 400 g of benzoic acid and 0.6 g of potassium hydroxide, and the inside of the autoclave was thoroughly replaced with nitrogen. The temperature was then raised to 160° C., and 230 g of ethylene oxide was gradually added to obtain polyoxyethylene (1.5 mol) benzoic acid.
[0062] Ingredient (E4): A 5 L autoclave was charged with 400 g of benzoic acid and 0.85 g of potassium hydroxide, and the inside of the autoclave was thoroughly replaced with nitrogen. The temperature was then raised to 160° C., and 460 g of ethylene oxide was gradually added to obtain polyoxyethylene (3.0 mol) benzoic acid.
[0063] [Table 1]
[0064] [Table 2]
[0065] As shown in the table above, when fibers such as polyester are dyed using a combination of a dye and a flame retardant processing agent under high temperature and pressure conditions, the flame retardant components in the flame retardant processing agent of the present invention are efficiently adsorbed into the interior of the fiber, preventing dye aggregation and aggregation between the dye and functional agents, thereby enabling the production of a uniformly dyed product.
Claims
1. A flame retardant processing agent comprising the following components (A) to (D): (A) Bromine-containing flame retardant: 10 to 50 parts by mass (B) Phosphorus-containing flame retardant: 2 to 15 parts by mass (C) an oxyalkylene group (A 3 O) having an average added mole number of 5 to 60: 0.3 to 8 parts by mass 【Chemistry 1】 (In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms, M' is a hydrogen atom, NH 4 + or a monovalent metal ion), and (D) an oxyalkylene group (A 3 O) having an average added mole number of 6 to 25: 3 to 15 parts by mass 【Chemistry 2】 (In the formula, m is a number from 1 to 3, n is a number that is the average number of moles added, and A 3 is an alkylene group having 2 to 4 carbon atoms. Contains The flame retardant processing agent, wherein the component (D) is a combination of a compound (D1) represented by the above formula (2) having an average number of moles of oxyalkylene groups added of 6 to 13 and a compound (D2) represented by the above formula (2) having an average number of moles of oxyalkylene groups added of 14 to 25, and the mass ratio of compound (D1) / compound (D2) is 8 / 1 to 2 / 1.
2. The flame retardant according to claim 1, further comprising (E) an ethylene oxide adduct of chlorophenol or an ethylene oxide adduct of benzoic acid in an amount of 1 to 15 parts by mass per 100 parts by mass of the flame retardant.
3. 3. The flame retardant according to claim 2, wherein the average number of moles of ethylene oxide added in the component (E) is 0.3 to 30 moles.
4. 2. The flame retardant according to claim 1, wherein in formula (1), M' is an ammonium ion, an organic ammonium ion, a sodium ion, or a potassium ion.
5. In the formula (1), M' is an ammonium ion, 3 The flame retardant according to claim 1, wherein is ethylene.
6. The flame retardant according to claim 1 , further comprising a solvent.
7. The flame retardant according to any one of claims 1 to 6, which is for use with polyester fibers.
8. A method for producing a dyed fiber product, comprising the steps of: adding the flame retardant according to any one of claims 1 to 6 to a dyebath; and dyeing a fiber with the dyebath to obtain a dyed product.
9. The method according to claim 8, wherein the amount of the flame retardant added is 3 to 30% by weight based on the material to be dyed.
10. The method of claim 8 wherein the fibers are polyester.
Citation Information
Patent Citations
Apparatus and method for using training sequences to estimate timing errors in digital signal receivers
JP2005506799A
Flame retardant for polyester fiber, method for producing flame-retardant polyester fiber product using the same, and flame-retardant polyester fiber product obtained from the same
JP2011012352A
Frame retardant agent and frame retardant method for polyester fiber product
JP2012167411A
Flame retardant processing of polyester synthetic fiber structure
JP2019006992A
Flame-retardant finishing agent for polyester-based fiber
JP2019094577A