Ground improvement body and manufacturing method of the ground improvement body

By incorporating carbon dioxide fixation powder from recycled concrete and ground improvement materials into the ground improvement body, the method effectively immobilizes carbon dioxide, reducing emissions and enhancing structural strength through calcium carbonate formation.

JP2024143666APending Publication Date: 2024-10-11TAKENAKA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023056447
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for recycling concrete waste in ground improvement bodies do not effectively immobilize carbon dioxide, and methods that use carbon dioxide in ground improvement processes release it back into the atmosphere, failing to achieve significant carbon dioxide reduction.

Method used

A ground improvement body and method that incorporates carbon dioxide fixation powder derived from recycled concrete and ground improvement material powders, which are pulverized and reacted with carbon dioxide to form calcium carbonate, immobilizing carbon dioxide within the structure.

Benefits of technology

The method efficiently fixes carbon dioxide, reducing emissions and enhancing the strength of the ground improvement body by forming calcium carbonate, thereby addressing carbon dioxide reduction and improving structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143666000001
    Figure 2024143666000001
  • Figure 2024143666000002
    Figure 2024143666000002
  • Figure 2024143666000003
    Figure 2024143666000003
Patent Text Reader

Abstract

To provide a ground improvement body in which carbon dioxide is fixated, and a manufacturing method thereof.SOLUTION: The disclosure relates to a ground improvement body that includes carbon dioxide fixation powders derived from at least one of recycled concrete powders and recycled ground improvement body powders, a binder material, soil, and water, and a manufacturing method thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a ground improvement body and a method for manufacturing a ground improvement body. [Background technology]

[0002] Cement, a binding material used in structures, emits a large amount of carbon dioxide due to the raw materials and firing process used to manufacture cement, so there is a demand for reducing carbon dioxide emissions. One method is to use recycled concrete, which is generated during the demolition of structures, as a concrete raw material. In Japan, where cities have developed in areas with weak ground such as river mouths and coastal areas, various ground improvement methods are used to improve the bearing capacity and deformation performance of soft ground, with cement-based ground improvement bodies being the most commonly used. The amount of cement used for ground improvement is about 6 million tons per year, and a huge amount of cement, about 1 / 6 of the total cement consumed domestically, is used to manufacture ground improvement bodies. The soil improvement body obtained using cement exerts a certain strength by appropriately mixing and stirring the cement and soil during production and hardening over time. Therefore, reducing the amount of cement used and improving carbon dioxide fixation are important issues in reducing carbon dioxide emissions. In recent years, various uses of recycled concrete for the construction of buildings have been investigated, but the application of recycled concrete to ground improvement bodies has not been sufficiently investigated.

[0003] Patent Document 1 proposes a method for recycling fine powder, which is generated as a by-product when producing recycled aggregate from waste concrete, as part of the cement raw material. The method described in Patent Document 1 describes a method for adding a small amount of fine waste concrete powder that contains almost no calcium hydroxide and has progressed carbonation to cement clinker, which is a cement raw material, and claims that this method can expand the recycling of fine waste concrete powder.

[0004] Patent Document 2 describes a ground improvement method in which water, cellulose nanofibers, carbon dioxide, and calcium carbonate are mixed to prepare a cellulose nanofiber-containing liquid, the calcium carbonate is converted to water-soluble calcium bicarbonate, and the liquid is infiltrated into the ground to be improved. The method disclosed herein improves the strength of the ground by recrystallizing the calcium bicarbonate through the release of water or carbon dioxide from the cellulose nanofiber-containing liquid that has infiltrated into the ground over time. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-193679 A [Patent Document 2] JP 2010-254503 A Summary of the Invention [Problem to be solved by the invention]

[0006] Reusing concrete waste generated by the demolition of concrete structures and the like into cement is useful for reducing carbon dioxide emissions, but the method of Patent Document 1 only results in a small amount of recycling. In addition, in Patent Document 2, the carbon dioxide once used in the preparation of the mixed liquid is released back into the atmosphere when calcium carbonate recrystallizes, so the carbon dioxide is not fixed in the ground improvement body.

[0007] An object of one embodiment of the present disclosure is to provide a ground improvement body in which carbon dioxide is immobilized. Another object of the present disclosure is to provide a method for producing a ground improvement body in which carbon dioxide is immobilized. [Means for solving the problem]

[0008] Means for solving the above problem include the following aspects.

[0009] <1> A ground improvement body comprising a carbon dioxide fixation powder derived from at least one of recycled concrete powder and recycled ground improvement body powder, a binder, soil and water. In the first aspect, the carbon dioxide fixation powder is derived from at least one of recycled concrete powder and recycled ground improvement body. Therefore, the carbon dioxide fixation powder used in the ground improvement body is effective for recycling waste concrete and waste ground improvement body, and can reduce carbon dioxide emissions during production. Furthermore, the obtained ground improvement body has better strength because it contains the carbon dioxide fixation powder, compared to a ground improvement body containing only a binder.

[0010] <2> A method for manufacturing a ground improvement body with fixed carbon dioxide, comprising: a crushing step of crushing at least one of recycled concrete debris and ground improvement body debris to obtain a powder that passes through a 1.7 mm sieve; a carbon dioxide fixation step of contacting the obtained powder with carbon dioxide to obtain a carbon dioxide fixation powder; and a mixing step of mixing the carbon dioxide fixation powder, a binder, water, and soil to obtain a mixture.

[0011] In the second aspect, the carbon dioxide fixation powder is prepared by crushing at least one of recycled concrete debris and ground improvement body debris to obtain a powder that has passed through a 1.7 mm sieve, and contacting the obtained powder with carbon dioxide, which causes the calcium oxide, calcium hydroxide, etc. contained in the recycled concrete debris to react with the carbon dioxide to become calcium carbonate. The carbon dioxide fixation process described above makes it possible to obtain a powder that fixes a large amount of carbon dioxide. Furthermore, by mixing water, a binder, and the carbon dioxide fixation powder with soil and hardening it, in addition to the hardening properties of the binder, the carbon dioxide fixation powder penetrates into the gaps between the binder particles, making the structure denser, and thus improving the strength of the ground improvement body.

[0012] <3> The carbon dioxide fixation process is a wet process in which carbon dioxide gas is supplied to a slurry in which the powder and water are mixed, or a dry process in which the powder is placed in a closed space with a carbon dioxide concentration of 5% or more. <2> A method for producing a ground improvement body in which carbon dioxide is fixed as described above. In the third embodiment, by contacting the crushed bodies with carbon dioxide by a wet process or a dry process, a large amount of carbon dioxide can be efficiently fixed in the powder. Effect of the Invention

[0013] According to one embodiment of the present disclosure, a ground improvement body in which carbon dioxide is immobilized can be provided. According to another embodiment of the present disclosure, a method for producing a ground improvement body in which carbon dioxide is immobilized can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <Ground improvement body> The ground improvement body of the present disclosure includes carbon dioxide fixation powder derived from at least one of recycled concrete powder and recycled ground improvement body powder, a binder, soil and water.

[0015] In this disclosure, the term "ground improvement body" refers to a body obtained by mixing and hardening a cement-based solidification material such as cement slurry and soil. The ground improvement body does not contain aggregates such as stones, as in concrete, or contains very little of them.

[0016] Since the ground improvement body of the present disclosure contains carbon dioxide fixation powder derived from at least one of recycled concrete powder and recycled ground improvement body powder, it is possible to reduce the amount of powder derived from new concrete used as the fine powder used in the manufacture of the ground improvement body, and further, it is believed that the use of the carbon dioxide fixation powder can reduce carbon dioxide emissions. In the following, at least one of the recycled concrete powder and the recycled ground improvement body powder may be collectively referred to as "recycled concrete powder, etc."

[0017] Generally, recycled concrete powder generated during the demolition and crushing of concrete contains crushed powder of hardened cement, powder of ground aggregate, and powder of crushed sand.Recycled ground improvement powder obtained by crushing ground improvement body also contains powder derived from cement components such as cement solidification material, as well as soil particles.

[0018] (Carbon dioxide fixation powder) Recycled concrete powder contains calcium derived from cement components in the form of calcium oxide (CaO), calcium hydroxide (Ca(OH)2), etc. Recycled concrete powder containing calcium derived from cement components adsorbs a certain amount of carbon dioxide even when left in the air, for example, but the amount of adsorption is not sufficient. There are no particular limitations on the carbon dioxide fixation powder used in the ground improvement body of the present disclosure, but from the standpoint of carbon dioxide fixation efficiency, it is preferable to use carbon dioxide fixation powder obtained by efficiently adsorbing carbon dioxide to calcium derived from cement components using various methods other than by leaving it to stand, that is, carbon dioxide fixation powder that adsorbs more carbon dioxide than when left to stand to stand. By performing an operation to adsorb carbon dioxide onto recycled concrete powder, etc., it is possible to bind a large amount of carbon dioxide to calcium, resulting in the production of more calcium carbonate (CaCO3) and the fixation of more carbon dioxide.

[0019] The carbon dioxide fixation powder contained in the ground improvement body of the present disclosure preferably has a carbon dioxide fixation amount of 50 kg or more per 1000 kg of the powder, more preferably 70 kg or more, and even more preferably 90 kg or more. By making the carbon dioxide fixation powder contained in the ground improvement body a carbon dioxide fixation amount of 50 kg or more per 1,000 kg of powder, the ground improvement body of the present disclosure can fix a large amount of carbon dioxide within the structure, thereby further reducing the burden on the environment.

[0020] The amount of carbon dioxide fixed in the carbon dioxide fixation powder can be determined from the mass loss at 600° C. to 800° C. in a TG-DTA test (Thermogrammetry-Differential Thermal Analysis). As a TG-DTA measuring device, for example, Thermoplus EVO2 TG-DTA8122 manufactured by Rigaku Corporation can be used. Here, the amount of calcium carbonate in the carbon dioxide fixation powder is measured, and the amount of carbon dioxide is calculated from the amount of calcium carbonate contained in the powder, which is defined as the amount of carbon dioxide fixed in the carbon dioxide fixation powder (carbon dioxide content).

[0021] There are no particular limitations on the size of the carbon dioxide fixation powder, so long as it can pass through a sieve with 1.7 mm openings. For example, if the powder is obtained by pulverizing hardened recycled concrete and can pass through a 1.7 mm sieve, that is, the maximum particle size is 1.7 mm or less, there are no particular limitations on the particle size distribution due to differences in pulverization method, etc. From the viewpoint of the balance between the amount of carbon dioxide fixed and the strength of the obtained ground improvement body, the average particle size of the carbon dioxide fixation powder is preferably 1000 μm or less, and more preferably 100 μm or less.

[0022] The content of carbon dioxide fixation powder in the ground improvement body can be selected appropriately in the range of 10% by mass to 110% by mass, relative to the total mass of the binder described below, taking into consideration the manner in which the ground improvement body is used and the required strength, and it is preferably in the range of 30% by mass to 60% by mass.

[0023] (Binding material) The ground improvement body of the present disclosure includes a binder. Any known hydraulic component can be used as the binder without any restrictions. Examples of the binder include cement, specifically, blast furnace cement type B, blast furnace cement type C, and cement-based solidification materials that are used in normal ground improvement. When the ground improvement material is mixed with the soil as a fluid slurry such as cement slurry, the content of the binder is 3The content can be appropriately selected taking into consideration the manner of use of the ground improvement body and the required strength. The amount of binder contained in the ground improvement body is determined according to the required strength. For example, 3 For this, the binder content can be in the range of 100 kg to 500 kg.

[0024] (soil) The ground improvement body of the present disclosure includes soil. The soil may be soil at the site where the ground improvement body is to be constructed. The soil may be used in the form of soil cement in which the on-site soil is mixed with a cement component as a binder. Increasing the content of the binder in the ground improvement body will improve the strength of the resulting ground improvement body, but it may result in a decrease in workability because the fluidity of the composition used to form the ground improvement body will decrease. When using the ground improvement body in a surface soil improvement method, the binder such as cement is often added in powder form directly to the ground and mixed and stirred, so that more binder can be used for the soil.

[0025] (water) The ground improvement material of the present disclosure contains water. There are no particular restrictions on the water contained in the ground improvement material. When mixing with soil to form a ground improvement body, as long as it meets conditions such as not containing harmful substances and not impairing the hardening properties of the binder, tap water, reclaimed water, stored rainwater, etc. can be selected as appropriate and added. The water content is appropriately selected depending on the strength required for the ground improvement body and the purpose, such as whether the ground improvement body is to be formed in a shallow layer such as the surface layer of the ground or in a deep layer. The total content of solids contained in the ground improvement body, such as binder and carbon dioxide fixation powder, relative to the mass of water, i.e., the water / solid ratio, can be 50% to 300%. Note that when the water / solid ratio is set to, for example, 60% or less for the purpose of improving the strength of the ground improvement body, a known chemical admixture may be further included for the purpose of improving fluidity.

[0026] The ground improvement body of the present disclosure can be used by applying the binder and the carbon dioxide fixation powder as powder to the ground for surface layer improvement. In addition, when applied to the mixed improvement of shallow, middle, and deep layers of the ground, and to the soil cement wall method for use in retaining walls, it can be used as a so-called cement slurry containing the binder, the carbon dioxide fixation powder, and water, and can be injected into the ground and mixed for use. The ground improvement body of the present disclosure is useful for ground improvement for various purposes. The ground improvement body of the present disclosure contains carbon dioxide fixation powder derived from recycled concrete powder or the like, thereby becoming a ground improvement body in which carbon dioxide is fixed. There are no particular limitations on the manufacturing method of the ground improvement body of the present disclosure, but from the standpoint of effectiveness it is preferable to manufacture it using the manufacturing method of the ground improvement body of the present disclosure described below.

[0027] <Method of manufacturing ground improvement body> The manufacturing method of the ground improvement body of the present disclosure (hereinafter also referred to as the manufacturing method of the present disclosure) includes a crushing step (step A) of crushing at least one of recycled concrete debris and ground improvement body debris to obtain a powder that passes through a 1.7 mm sieve, a carbon dioxide fixation step (step B) of contacting the obtained powder with carbon dioxide to obtain a carbon dioxide fixation powder, and a mixing step (step C) of mixing the carbon dioxide fixation powder, a binder, water, and soil to obtain a mixture.

[0028] (Process A: Crushing process) Step A is a crushing step in which at least one of recycled concrete debris and ground improvement body debris is crushed to obtain powder that has passed through a 1.7 mm sieve. When crushing recycled concrete rubble, it is first pre-crushed to a size that can be fed into a crusher, for example, to a particle size of about 40 mm, and then fed into the crusher for crushing. Examples of the crushing equipment used for crushing include a blasting machine that crushes pre-crushed concrete debris by using collisions between the concrete debris without using media, a planetary mill that crushes the concrete debris by rubbing between the concrete debris without using media, and a ball mill that crushes the sample using media. In addition, a crusher run production machine can be used to crush the demolished concrete, to obtain crushed material of a predetermined size range, which can then be subjected to the process B described below.

[0029] The pulverized material obtained using the pulverizing device exemplified above is sieved through a sieve with 1.7 mm openings to obtain a pulverized material that has passed through the sieve with 1.7 mm openings. The performance of recycled concrete debris is affected by the compressive strength of the hardened concrete before demolition, the type of cement used in production, the amount of cement added, etc., so the crushed material used in the production method of the ground improvement body disclosed in the present invention has a compressive strength of 18 N / mm 2 It is desirable to use the above recycled concrete as a raw material.

[0030] When using ground improvement body debris as a raw material for carbon dioxide fixation powder, the ground improvement body existing underground is first excavated and pre-crushed until the maximum particle size is approximately 40 mm. It is then crushed using the crusher exemplified above in the same manner as the recycled concrete debris described above, and sieved through a sieve with 1.7 mm openings to obtain a crushed material that has passed through a sieve with 1.7 mm openings. In addition, since the compressive strength of the ground improvement body is relatively low compared to the hardened concrete body, the material scraped from the ground improvement body with the drilling bit of a mechanical ground improvement construction machine may be used. Unlike the hardened concrete body, the ground improvement body contains almost no aggregate, so the powder derived from the ground improvement body may be one with an average particle size of 50 mm or less, which may be crushed by the above-mentioned method to prepare a 1.7 mm sieve-passing powder.

[0031] When obtaining carbon dioxide fixation powder using recycled concrete debris, it is preferable to include a step of separating the aggregate contained in the concrete from the recycled concrete powder after the crushing step. By carrying out the subsequent step B using the recycled concrete powder from which the aggregate has been removed after the separation step and obtaining a carbon dioxide fixation powder, the efficiency of carbon dioxide fixation in the powder can be improved.

[0032] On the other hand, when carbon dioxide fixation powder is obtained using ground improvement body rubble, unlike concrete waste such as recycled concrete rubble, it contains no or very little aggregate, so there is an advantage that carbon dioxide fixation powder can be easily obtained by fixing carbon dioxide in the powder as is without separating the aggregate from the crushed ground improvement body.

[0033] (Process B) Step B is a carbon dioxide fixation step in which the powder obtained by pulverization in step A is contacted with carbon dioxide to obtain a carbon dioxide fixation powder. There are no particular limitations on the method for contacting the powder obtained in step A with carbon dioxide. Methods for contacting the powder with carbon dioxide include, for example, a wet process in which carbon dioxide gas is supplied to a slurry in which the powder is mixed with water, and a dry process in which the powder is placed in a closed space with a carbon dioxide concentration of 5% or more. Either method can be used.

[0034] -Wet process- An example of the wet process is a method in which the obtained powder is mixed with water to prepare a slurry, and carbon dioxide gas is supplied to the slurry. The powder and water are mixed to prepare a slurry, which is then left to stand for 30 to 90 minutes to allow for mixing, and carbon dioxide gas is supplied to the slurry. The supply of carbon dioxide gas is preferably stopped when the pH of the slurry reaches about 6.8 to 8.0, and more preferably when the pH reaches about 6.8 to 7.0.

[0035] As a specific method in the wet process, a container containing powder is filled with water to immerse the powder in water to prepare a slurry, and carbon dioxide gas is blown into the slurry to create bubbles. There are no particular limitations on the water used for immersion. From the viewpoint of treatment efficiency, it is preferable that the water used contains a small amount of impurities that form salts upon contact with carbon dioxide gas, and examples of the water that can be used include ion-exchanged water and tap water.

[0036] In the carbon dioxide fixation step, when a wet process is applied, the carbon dioxide gas concentration supplied to the water can be 5%, preferably 10% or more, and more preferably 20% or more. There is no particular upper limit to the carbon dioxide gas concentration, and the carbon dioxide gas concentration may be 100%. The higher the carbon dioxide concentration, the better the production efficiency of the carbon dioxide fixation powder tends to be. The carbon dioxide gas to be supplied may be exhaust gas containing carbon dioxide gas, as in the dry process described below. When exhaust gas is used as a carbon dioxide gas supply source, the carbon dioxide gas concentration depends on the amount of carbon dioxide gas contained in the exhaust gas. Even when exhaust gas is used, the carbon dioxide gas concentration in the exhaust gas is preferably 5% or more.

[0037] The amount of carbon dioxide gas supplied to the slurry and the supply rate of carbon dioxide gas at the above concentration can be appropriately selected depending on the purpose. By blowing carbon dioxide gas with the supply amount (total amount) and supply rate of carbon dioxide gas optimized, the powder immersed in water can be efficiently contacted with the carbon dioxide gas, and carbon dioxide fixation powder can be obtained. The solubility of carbon dioxide in water increases as the water temperature decreases, so there is no need to specifically control the temperature of the slurry. When exhaust gas is used as a source of carbon dioxide, the temperature of the water may rise depending on the temperature of the exhaust gas. However, since the water temperature never reaches 100°C, it is not expected to affect the progress of the carbonation process of the recycled aggregate.

[0038] There is no particular limitation on the temperature of the slurry, and the wet process can be carried out at room temperature. When exhaust gas is used to supply carbon dioxide, the temperature of the slurry may rise to, for example, about 90° C. depending on the temperature and supply amount of the exhaust gas, but a carbon dioxide fixation powder can be obtained even under such temperature conditions.

[0039] The treatment time in the wet process is not particularly limited, and may be, for example, 5 minutes to 10 hours, and preferably 30 minutes to 6 hours. Since the pH of the slurry tends to decrease as the carbonation of the cement-derived components progresses due to contact between the powder and carbon dioxide gas, the end point of the carbonation treatment may be the time when the pH of the water reaches 6 to 8. It is preferable to carry out the wet treatment until the pH of the water reaches 6.5 to 7.0, and more preferably until the pH reaches 6.5 to 6.8. It is even more preferable to continue the wet treatment for an additional 30 to 90 minutes after the pH of the water reaches a target value, for example, the pH of the water reaches 6.5 to 7.0. The pH of the slurry can be measured with a known pH meter. In this disclosure, the pH is measured with a glass electrode type hydrogen ion concentration indicator (TPX-999Si) manufactured by Toko Chemical Laboratory Co., Ltd., assuming a liquid temperature of 20° C.

[0040] After the pH reaches a predetermined value, the water contained in the slurry is removed to recover the powder. Since the recovered powder is a wet material containing water, it is preferable to dehydrate it to a water content of about 30% using a filter press device or the like from the viewpoints of transportability of the powder and workability when manufacturing the ground improvement body.

[0041] -Dry process- The dry process can be a process in which the powder is placed in a closed space with a carbon dioxide concentration of 5% or more. For example, the powder obtained in the process A is placed in a tank (closed space) in which the carbon dioxide concentration, humidity, and temperature are adjusted, and the powder is collected when the change in mass reaches a predetermined value. In the dry process, the recycled aggregate can be placed in a closed space and the closed space can be filled with carbon dioxide gas to bring the aggregate into contact with the carbon dioxide gas.

[0042] The temperature in the closed space is preferably 5° C. to 200° C., and more preferably 20° C. to 100° C. For example, the carbonation treatment can be carried out in a closed space without temperature control in an atmosphere having a temperature of 0° C. to 40° C. From the viewpoint of further improving carbonation efficiency, the humidity in the closed space can be set to 30% RH to 90% RH, and preferably 50% RH to 80% RH.

[0043] The carbon dioxide gas concentration in the gas to be contacted is 5% or more, preferably 10% or more, and more preferably 50% or more. The carbon dioxide gas to be contacted may be 100% carbon dioxide gas. The carbon dioxide gas used in the carbonation treatment may be exhaust gas containing carbon dioxide. Examples of the exhaust gas include exhaust gas discharged from a heating furnace and exhaust gas discharged from a power engine, and there is no particular limitation as long as it contains carbon dioxide at a concentration of 5% or more. By using exhaust gas containing carbon dioxide for the carbonation treatment, it is possible to simultaneously reduce the amount of carbon dioxide in the exhaust gas and adsorb the carbon dioxide to the powder. When the temperature of the exhaust gas is high and exceeds 100°C, efficient contact with carbon dioxide can be achieved without the need to heat the closed space, which has the advantage of simultaneously reducing energy consumption and reducing the amount of carbon dioxide in the exhaust gas. For the purpose of efficiently obtaining carbon dioxide fixation powder, the closed space may be pressurized and carbon dioxide gas may be supplied to contact the powder.

[0044] The preferred treatment time in the dry treatment is appropriately selected in relation to the carbon dioxide gas concentration and supply amount. For example, when carbon dioxide gas with a concentration of 10% to 50% is used, the treatment time can be 1 hour or more, preferably 24 hours or more, more preferably 2 days or more, even more preferably 5 days or more, and even more preferably 10 days or more. There is no particular upper limit to the treatment time, but from the viewpoint of production efficiency, it can be 20 days or less. The preferred treatment time can be appropriately selected depending on the state of the recycled concrete powder, etc. If the processing time for the dry process is 5 days or more, it is preferable to stir the powder left in the closed space about once every several hours to 3 days in order to make the carbonation proceed more efficiently. Stirring allows the powder to come into contact with carbon dioxide gas more uniformly.

[0045] The amount of carbon dioxide adsorption in the carbon dioxide fixation powder obtained in step B can be determined by a TG-DTA test in the same manner as in the measurement of the amount of carbon dioxide fixation in the carbon dioxide fixation powder described above. For example, in a wet process, carbon dioxide gas was supplied to a slurry containing 125 g / L (liter) of powder, and after the pH of the slurry reached 6.8, carbon dioxide gas was supplied for 60 minutes to obtain a powder, which contained 22.9% calcium carbonate, while in a dry process, carbon dioxide gas with a concentration of 10% was supplied to an apparatus at a temperature of 20°C and 60% RH for 9 days to obtain a powder, which contained 22.5% calcium carbonate. When untreated powder was similarly measured, the calcium carbonate content was 15.5%, and it was confirmed that the calcium carbonate content increased by about 7% due to the carbonation treatment.

[0046] The carbon dioxide fixation powder obtained through step B preferably has a carbon dioxide fixation amount of 50 kg or more per 1000 kg of the powder, more preferably 70 kg or more, and even more preferably 90 kg or more.

[0047] Step C is a mixing step in which the carbon dioxide fixation powder obtained in step B, a binder, water, and soil are mixed to obtain a mixture. There are no particular limitations on the binder, and blast furnace cement type B, blast furnace cement type C, cement-based solidification materials, etc., which are normally used for ground improvement bodies, can be used.

[0048] In step C, when the carbon dioxide fixation powder is mixed into the cement slurry containing the binder and water to form a mixture, and the mixture is mixed with soil while maintaining its fluidity, the content of the binder such as cement is 100% per 1 m of the soil to be improved. 3 It is preferable that the range is 100 kg to 500 kg. The content of the carbon dioxide fixation powder can be 10% by mass to 110% by mass with respect to the total mass of the binder. The total content of the binder and the carbon dioxide fixation powder relative to the water content, that is, the water / solid ratio, can be set to 50% to 300%. In addition, when the water / solid ratio is set to 60% or less, preferably in the range of 47% to 55%, for the purpose of improving strength, etc., it is preferable to use a chemical admixture from the viewpoint of improving fluidity. That is, the mixture in step C can further contain a chemical admixture.

[0049] The chemical admixture may be selected from known chemical admixtures capable of improving the fluidity of the cement slurry, and examples of the chemical admixture include chemical admixtures containing a water-soluble vinyl copolymer. The content of the chemical admixture is appropriately selected depending on the purpose, and is generally, but not limited to, 0.3 mass % to 1.0 mass % based on the total mass of the binder.

[0050] (Construction method of ground improvement body) Next, a method for constructing a ground improvement body using the mixture obtained by the manufacturing method of the present disclosure will be described below, taking an example in which cement is used as a binder. To prepare the ground improvement body, first, cement and water are mixed to prepare a cement slurry, and the resulting cement slurry is mixed and stirred with the soil in the ground to form a mixture. The resulting mixture is allowed to harden as is to form a ground improvement body. This method is generally called the mechanical cement mixing method, and can be applied to both deep layer mixing method and shallow layer mixing method. Moreover, a high-pressure injection method in which the obtained cement slurry is injected into the ground under high pressure and mixed with the soil in the ground can also be used as a construction method. In addition, when forming a ground improvement body at a shallow layer, such as for reinforcing the ground surface, the ground improvement body can be constructed using a powder shallow layer improvement method, in which a binder, carbon dioxide fixation powder, and soil in the ground are mixed and stirred in powder form.

[0051] Below, as examples of construction methods, the construction procedures for the deep layer mixing method using cement slurry and the powder shallow layer mixing method using powder are shown. In the deep layer mixing method using cement slurry and the shallow layer mixing method using powder, it is important and preferable to conduct a preliminary strength test indoors using the local ground and the cement to be used before construction in order to confirm the strength development of the ground improvement body. When using carbon dioxide fixation powder, it is preferable to conduct a test using the carbon dioxide fixation powder to be used in the preliminary strength test indoors.

[0052] In the mechanical deep mixing method, a kneading mixer is used to mix cement and water to create a cement slurry, which is then transported into the ground using a pressure pump and pressure hose, where it is sprayed from the tip of the mixing blade and mixed with the ground using the mixing blade. When constructing a ground improvement body using carbon dioxide fixation powder, a predetermined amount of carbon dioxide fixation powder is added when mixing the cement slurry with the kneading mixer to create a cement slurry containing the carbon dioxide fixation powder. Depending on the amount of carbon dioxide fixation powder added, an optional chemical admixture may be added as necessary. By using the chemical admixture, the agitation property of the cement slurry containing the carbon dioxide fixation powder and the pumpability by a pressure pump are improved. The compressive strength of the ground improvement body is affected by the water / solids ratio of the cement slurry (water and cement, etc.). For example, the carbon dioxide fixation powder obtained through a wet process may contain approximately 30% moisture. When using such a powder, the moisture content of the carbon dioxide fixation powder is measured in advance, and the amount of water added when preparing the cement slurry is reduced, thereby making it possible to achieve a planned ratio of water to cement in the cement slurry. On the other hand, the carbon dioxide fixation powder obtained through the dry process contains almost no moisture, so there is no need to adjust the amount of water added when preparing the cement slurry.

[0053] In the powder shallow layer mixing treatment method, at least a specified amount of cement and carbon dioxide fixation powder are spread on the surface of the ground to be improved, and then an excavation machine (backhoe) is used to mix the cement, carbon dioxide fixation powder, and ground (soil) to create a ground improvement body. At this time, a specified carbon dioxide fixation powder is spread at the same time as the cement is spread, and the cement, carbon dioxide fixation powder, and ground are mixed with an excavation machine (backhoe) to create a ground improvement body. As in the above-mentioned Mechanical Deep Mixing Treatment Publication, when using carbon dioxide fixation powder obtained by a wet process, it is preferable to ensure a predetermined strength by, for example, adding a slightly larger amount of cement, taking into consideration that the carbon dioxide fixation powder contains about 30% moisture. On the other hand, when using carbon dioxide fixation powder obtained through a dry process, there is no particular need to adjust the amount of cement, even in the powder shallow layer mixing treatment method.

[0054] In either construction method, according to the manufacturing method of the ground improvement body disclosed herein, in addition to a binder such as cement, carbon dioxide fixation powder is used to manufacture the ground improvement body, so that carbon dioxide is fixed in the ground improvement body formed by hardening the mixture with soil. Also, by adjusting the contents of the binder, the carbon dioxide fixation powder, and the water, a ground improvement body that maintains strength according to the construction area is manufactured. One of the advantages of the manufacturing method disclosed herein is that conventional manufacturing methods for ground improvement bodies can be applied as is, and by using only a binder and carbon dioxide fixation powder, a ground improvement body in which carbon dioxide is fixed can be easily obtained without the need for any additional special equipment, etc. In addition, the use of carbon dioxide fixation powder derived from at least one of recycled concrete debris and ground improvement body debris leads to effective utilization of waste materials including concrete.

[0055] (Performance of ground improvement body) -Compressive strength- The ground improvement body of the present disclosure preferably has sufficient compressive strength for ground improvement. The strength development of the ground improvement body is judged by the uniaxial compressive strength of the ground improvement body made by mixing a binder, carbon dioxide fixation powder, water, and soil. Unconfined compressive strength is measured based on JIS A 1216:2020 "Unconfined compression test method for soil". The target value of the compressive strength of the ground improvement body disclosed in the present disclosure is appropriately selected depending on the purpose of construction, but generally, the uniaxial compressive strength is 1N / mm 2 Above this level, it is considered to be at a practical level with no problems, and 2N / mm 2 It is preferable that the resistance is 3N / mm or more. 2 More preferably, it is equal to or greater than this.

[0056] -Physical properties of cement slurry- In the manufacturing method of the ground improvement body disclosed herein, when a so-called cement slurry manufactured by mixing a binder, a carbon dioxide fixation powder, and water is used, the cement slurry preferably has good fluidity from the viewpoint of workability. The fluidity of the cement slurry is evaluated by the P funnel flow time in accordance with the Japan Society of Civil Engineers' standard "Test method for fluidity of mortar for injection of prepacked concrete (method using P funnel) (JSCE-F 521-1999)." In general, it is believed that if the flow time of the slurry through the P funnel is 25 seconds or less, the slurry can be pumped using a pump, and if it is 20 seconds or less, no major problems will arise with pumping the slurry. Therefore, in the present disclosure, the fluidity of the cement slurry is preferably such that the flow time is 25 seconds or less, more preferably 20 seconds or less. Note that, when the ground improvement body is produced near the surface layer for the purpose of improving a shallow layer of the ground, there is no problem if the above fluidity is not satisfied. The separation resistance of the cement slurry is evaluated by visually checking whether or not the prepared cement slurry separates.

[0057] -Prevention of hexavalent chromium leaching- It is preferable that the leaching of hexavalent chromium from the ground be suppressed by producing a ground improvement body. Prevention of hexavalent chromium leaching can be evaluated based on the results of leaching tests of hexavalent chromium from ground improvement bodies. The leaching of hexavalent chromium from ground improvement bodies can be carried out in accordance with the method set out in Environment Agency Notification No. 46 (dated August 23, 1991). For example, a model ground improvement body can be prepared, and soil lumps and aggregates from the obtained ground improvement body are roughly crushed to obtain soil of 2 mm or less, which is then dispersed in water and the dispersion liquid is continuously shaken for 6 hours to perform an elution test. After the elution test, the dispersion liquid is sampled and the amount of eluted hexavalent chromium is measured. If the amount of eluted hexavalent chromium in the elution test is 0.05 mg / L or less, it is evaluated that the elution of hexavalent chromium has been suppressed, and is at a level that is not problematic in practical use. EXAMPLES

[0058] The following describes the ground improvement body and the manufacturing method thereof according to the present disclosure by way of examples. It goes without saying that the ground improvement body and the manufacturing method thereof according to the present disclosure are not limited to the following examples, and include various modified examples within the scope of the present disclosure. In the following examples, "%" means "% by mass" unless otherwise specified.

[0059] <Production Examples 1 and 2 of Carbon Dioxide Fixation Powder> Carbon dioxide fixation powder was prepared using recycled concrete rubble. Concrete chunks generated during the demolition of buildings were crushed to obtain coarsely crushed material of less than 40 mm in size, which was then crushed and sieved to obtain powder that passed through a sieve with 1.7 mm openings, and used as recycled concrete powder. In this manufacturing example, the recycled concrete powder was obtained by crushing the concrete by collision between samples without using media using a blasting machine. In addition, when strength tests were conducted on concrete cores taken from the floors of each floor of the building before demolition, which is the raw material for recycled concrete debris, the average compressive strength of the cores was 27.4 N / mm 2 It was.

[0060] The obtained recycled concrete powder was contacted with carbon dioxide gas to obtain a carbon dioxide fixation powder. First, a wet carbonation device equipped with a 20 L container was prepared, and water and recycled concrete powder were put into the container and stirred to prepare a slurry with a solid concentration of 125 g / L. After leaving the slurry to stand for 60 minutes, carbon dioxide gas was supplied at 20 L / min, and after the pH of the slurry reached 6.8, the supply of carbon dioxide gas was continued for another 60 minutes, and then the slurry was left to stand, the water was separated, and a carbon dioxide fixation powder was obtained. Since the carbon dioxide fixation powder contains water, the water was further removed by pressing to make the water content about 30%. (Step B-1) The powder obtained by step B-1 (wet step) may be referred to as "powder (I)" below.

[0061] The same recycled concrete powder was also placed in a tank at 20°C, 60% RH, and 10% carbon dioxide concentration for 9 days. During this time, the recycled concrete powder was stirred every day so that the carbon dioxide would come into contact with the entire recycled concrete powder, and a carbon dioxide fixation powder was obtained. (Step B-2) The powder obtained by step B-2 (dry step) may be referred to as "powder (II)" below.

[0062] (Evaluation of carbon dioxide fixation powder) The physical properties of the carbon dioxide fixation powder obtained through step B-1 (powder (I)) and the carbon dioxide fixation powder obtained through step B-2 (powder (II)) were evaluated by the following methods.

[0063] The 50% particle size of each powder was determined from the particle size distribution using a laser diffraction / scattering particle size distribution analyzer (Microtrac MT3300EXII, manufactured by Microtrac Bell Co., Ltd.). The density of each powder was measured using a gas phase substitution test device (automatic true density measurement device BELPycno, manufactured by Microtrack BEL Co., Ltd.). In the TG-DTA test, the amount of calcium carbonate in each powder was calculated from the mass loss at 600℃ to 800℃ using Thermo plus Evo2 TG-DTA8122 (manufactured by Rigaku Corporation). Furthermore, the amount of carbon dioxide fixed in the powder was calculated from the amount of calcium carbonate. The results are shown in Table 1 below. As a reference example, the results for the recycled concrete powder (powder (0)) obtained in step A are also shown.

[0064] [Table 1]

[0065] Furthermore, each powder was analyzed using an X-ray diffractometer (D8 ADVANCE, manufactured by Bruker).

[0066] As a result of the analysis, peaks of hydrates such as ettringite (Ett) and calcium hydroxide (CH) were confirmed in the untreated powder (powder (0)) that had only been subjected to step A, but no hydrate peaks were observed in powder (I) and powder (II). It is considered that the hydrates contained in the powder disappeared as a result of step B. In addition, the amount of calcium carbonate contained in the powder was increased by about 7% in Powder (I) and Powder (II) compared to Powder (0), and the measurement of the amount of fixed carbon dioxide confirmed that by carrying out Process B, the amount of fixed carbon dioxide in the recycled concrete powder increased by about 30 kg per ton compared to untreated Powder (0).

[0067] From the above results, it can be seen that in the manufacturing method of the ground improvement body disclosed herein, carrying out step B does not significantly affect the particle size and density of the powder, and more carbon dioxide is fixed.

[0068] <Examples 1 to 6> The obtained carbon dioxide fixation powder was used to manufacture a ground improvement body. Tap water was used for the manufacture of the ground improvement body. (Materials used) -Binding material- Blast-furnace cement type B (manufactured by Nippon Steel Blast-furnace Cement Co., Ltd., density 3.02 g / cm 3 ) Blast-furnace cement type C (manufactured by Nippon Steel Blast-furnace Cement Co., Ltd., density 2.96 g / cm 3 ) Cement-based solidification material (Nippon Steel Blast Furnace Cement, Solstar (registered trademark) R100, density 3.00 g / cm 3 ) - Carbon dioxide fixation powder - Powder (I) and Powder (II) obtained in the above manufacturing example -Chemical admixtures- Chupole (registered trademark) HP-11, manufactured by Takemoto Oil Co., Ltd.

[0069] -soil- (Materials used) · Silica sand (dried silica sand No. 6: from Tohoku Silica Sand) ·Frog-eye clay (original special grade frog-eye 200m / s) 1. Artificial sandy ground (model soil 1) The artificial sandy ground is made of silica sand and frog-eye clay in a mass ratio of 9:1 (set moisture content: 18%). 2. Artificial clay ground (model soil 2) The artificial clay ground is made of silica sand and frog-eye clay in a mass ratio of 1:9 (set moisture content: 55%).

[0070] Model soil 1m 3 Cement, water and powder (I) were added to the mixture in the amounts shown in Table 2 below to produce a mixture. (Step C) The mixture was thoroughly mixed and stirred as a slurry for forming a ground improvement body, and a P funnel test was performed and the presence or absence of separation of the slurry was evaluated according to the method described below. The produced slurry for forming the ground improvement body was poured into a formwork (size: diameter 50 mm, height 100 mm) and allowed to harden to obtain a ground improvement body for uniaxial compression tests, and the compressive strength was evaluated. Additionally, the amount of hexavalent chromium eluted was evaluated.

[0071] -Compressive strength- The unconfined compressive strength was measured based on JIS A 1216:2020 "Unconfined compression test method for soil". -Physical properties of cement slurry- The evaluation was based on the P funnel flow time in accordance with the Japan Society of Civil Engineers standard "Method of fluidity test for injection mortar for prepacked concrete (method using P funnel) (JSCE-F 521-1999)." The separation resistance of the cement slurry was evaluated by visually checking whether the prepared cement slurry separated or not.

[0072] -Prevention of elution of hexavalent chromium- The elution of hexavalent chromium from the manufactured ground improvement body was carried out based on the method set out in the Environment Agency Notification No. 46 (dated August 23, 1991). That is, soil of 2 mm or less obtained by crushing the soil lumps and aggregates in the obtained ground improvement body was collected, dispersed in water, and the dispersion was continuously shaken for 6 hours to perform an elution test. After the elution test, the dispersion was collected and the amount of eluted hexavalent chromium was measured. The results are shown in Table 2.

[0073] -Carbon dioxide emissions- Carbon dioxide emissions were calculated by subtracting the amount of carbon dioxide fixed in the ground improvement bodies from the amount of carbon dioxide generated during the production of cement used in constructing each ground improvement body. Carbon dioxide emissions resulting from the energy used in transporting materials and constructing the ground improvement bodies were not taken into account. The carbon dioxide generated during cement production was calculated using the value of 451.8 kg-CO2 / t for blast-furnace cement type B in the appendix on page 8 of the Cement Association: Summary of Cement LCI Data (February 2023). (See https: / / www.jcassoc.or.jp / cement / 4pdf / jg1i_01.pdf) The amount of carbon dioxide fixed in the ground improvement material was calculated assuming that the amount of CO2 fixed by the CO2 fixing fine powder per 1,000 kg is 90 kg-CO2 / t.

[0074] [Table 2]

[0075] The compressive strength increased by adding powder (I) compared to the control sample that did not contain powder. This is thought to be because the addition of the carbon dioxide fixation powder reduced voids in the ground improvement body through the generation of hydrates, which contributed to the improvement of strength. The soil improvement bodies of the examples were all found to have an effect of inhibiting the elution of hexavalent chromium. Furthermore, from the results of Examples 1 to 4, it was found that the compressive strength of the ground improvement body improved as the water-binder ratio increased, but on the other hand, the fluidity of the cement slurry tended to decrease. In Examples 5 and 6, in which chemical admixtures were added to improve fluidity, there was a tendency for both compressive strength and fluidity to improve further, indicating that the use of chemical admixtures is effective in preventing a decrease in fluidity when producing high-strength ground improvement bodies.

[0076] <Examples 7 to 14> The recycled concrete powder obtained through step A was sieved through a sieve with different mesh sizes to obtain powder with a maximum particle size of 335 μm to 1700 μm (1.7 mm), and step B-2 was carried out to obtain powder (II) with a different particle size. In process A, powder obtained by a blast processing machine, which crushes samples by collision without using media, and powder obtained by a crusher run production machine were used to carry out process B-2 to produce powder (II), and the differences due to the crushing method were also examined. For Examples 7 to 14, the properties of the mixture, the strength of the obtained ground improvement body, and other items were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0077] [Table 3]

[0078] The results in Table 3 show that the compressive strength increased slightly by adding powder (II) compared to the control example not containing powder. Both the fluidity of the cement slurry and the inhibition of elution of hexavalent chromium were at a level that would pose no practical problems. Comparison of Examples 7 to 14 shows that, when the water-binder ratio is the same, differences in the grinding method and the maximum particle size of the powder (II) do not have a significant effect on the compressive strength, fluidity, and hexavalent chromium elution inhibition effect.

[0079] <Examples 15 to 19, Comparative Examples 1 to 5> Next, the type of cement used was changed to the type shown in Table 4, and mixtures were prepared. The obtained mixture was used as a model ground to manufacture ground improvement bodies using an artificial sandy ground (model soil 1) and an artificial clayey ground (model soil 2). The compressive strength, hexavalent chromium elution amount, and carbon dioxide emission amount of the obtained ground improvement body were evaluated in the same manner as in Example 1. The results are shown in Table 4. In Table 4, artificial sandy ground is abbreviated as "sand" and artificial clayey ground is abbreviated as "clay."

[0080] [Table 4]

[0081] The results in Table 4 show that when the model soil is clayey soil, as in the case of sandy soil, the compressive strength of each example containing powder (I) is slightly increased compared to each comparative example not containing powder. Moreover, the examples had lower carbon dioxide emissions than the comparative examples, and the inhibition of elution of hexavalent chromium was at a level that would not pose a problem in practical use.

Claims

1. A ground improvement body comprising a carbon dioxide fixation powder derived from at least one of recycled concrete powder and recycled ground improvement body powder, a binder, soil and water.

2. A crushing step of crushing at least one of the recycled concrete rubble and the ground improvement body rubble to obtain a powder that has passed through a 1.7 mm sieve; a carbon dioxide fixation step of contacting the obtained powder with carbon dioxide to obtain a carbon dioxide fixation powder; A mixing step of mixing the carbon dioxide fixation powder, a binder, water, and soil to obtain a mixture. A method for manufacturing ground improvement bodies that fix carbon dioxide.

3. The method for producing a ground improvement body with fixed carbon dioxide according to claim 2, wherein the mixture further contains a chemical admixture.

4. The carbon dioxide fixation process is a wet process in which carbon dioxide gas is supplied to a slurry in which the powder and water are mixed, or a dry process in which the powder is placed in a closed space having a carbon dioxide concentration of 5% or more. A method for producing a ground improvement body with fixed carbon dioxide according to claim 2 or 3.

Citation Information

Patent Citations

  • Foundation improvement material and production method thereof

    JP2021134285A

  • Fine powder cement

    JP2010254503A

  • Ground improvement method

    JP2018193679A