Metal-containing photoresist developer composition, and method of forming patterns including development stage using the same
The developer composition for metal-containing photoresists addresses sensitivity and LER issues by using a pH-balanced buffer system, improving CD uniformity and LER in photolithography processes.
Patent Information
- Application Number
- JP2024000157
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-01-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional chemically amplified photoresists face challenges with reduced sensitivity and increased line edge roughness (LER) at small feature sizes, leading to difficulties in achieving excellent etching resistance, resolution, and critical dimension (CD) uniformity during photolithography processes.
A developer composition for metal-containing photoresists is formulated with an organic solvent, an acid compound, and a counterbase, maintaining a balanced pH through a buffer system to stabilize pH fluctuations during exposure and development, thereby improving CD uniformity and reducing LER.
The developer composition stabilizes pH imbalances, enhancing CD uniformity and reducing LER, ensuring stable and precise pattern formation in semiconductor manufacturing.
Smart Images

Figure 2024144101000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a developer composition for a metal-containing photoresist and a pattern forming method including a development step using the same. [Background technology]
[0002] In recent years, the semiconductor industry has been continuously shrinking its critical dimensions, which has required new types of high performance photoresist materials and patterning methods to meet the demands of fabricating and patterning smaller features.
[0003] Traditional chemically amplified (CA) photoresists are designed to have high sensitivity, but when they are composed of typical elements (mainly C with lesser amounts of O, F, S), the absorbance of the photoresist at 13.5 nm wavelength is reduced, resulting in reduced sensitivity and, in part, more difficulty under EUV exposure. CA photoresists also suffer from roughness issues at small feature sizes, and experiments have revealed that line edge roughness (LER) increases as the photospeed decreases, in part due to the nature of the acid-catalyzed reaction process. Due to the shortcomings and problems of CA photoresists, there has been a demand for new types of high-performance photoresists in the semiconductor industry.
[0004] In particular, there is currently a need to develop a photoresist that can ensure excellent etching resistance and resolution in the photolithography process, while at the same time improving sensitivity and CD (critical dimension) uniformity and improving LER characteristics. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Korean Patent Publication No. 2021-0053232 [Patent Document 2] Korean Patent Publication No. 2001-0013818 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to provide a developer composition for metal-containing photoresist that can improve CD uniformity by preventing and stabilizing momentary pH imbalances induced by acids consumed or released from photoresists during exposure or development processes.
[0007] A further object of the present invention is to provide a pattern forming method which comprises a development step using the above composition. [Means for solving the problem]
[0008] The developer composition for a metal-containing photoresist according to the present invention comprises an organic solvent, an acid compound, and a counter base of the acid compound.
[0009] The acid compound is contained in an amount of 0.01% by mass to 10% by mass.
[0010] The counter base is contained in an amount of 0.001% by mass to 1% by mass.
[0011] The acid compound and the counter base are contained in a mass ratio of 1:0.01 to 1:1.
[0012] The counter base may be derived from an ammonium salt, an alkali metal salt, an alkaline earth metal salt, or a combination thereof.
[0013] The metal-containing photoresist can include a metal compound that includes at least one of an organotin oxo group and an organotin carboxyl group.
[0014] The metal-containing photoresist may include a metal compound represented by the following Chemical Formula 1:
[0015] [ka]
[0016] In the above Chemical Formula 1, R 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 30 carbon atoms, and -R a -OR b (where R a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 30 carbon atoms, -OR c and -OC(=O)R d is selected from among R 2 ~R 4 At least one of the is -OR c and -OC(=O)R d is selected from among In this case, R cis a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R d is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.
[0017] R in the above Chemical Formula 1 2 ~R 4 R in c and R d may each independently be a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.
[0018] A method for forming a pattern according to another embodiment of the present invention includes the steps of applying a metal-containing photoresist composition onto a substrate, drying and heating the composition to form a metal-containing photoresist film on the substrate, exposing the metal-containing photoresist film to light, and developing the metal-containing photoresist film using the above-mentioned metal-containing photoresist developer composition. Effect of the Invention
[0019] The developer composition for metal-containing photoresist according to the present invention can improve CD uniformity by preventing and stabilizing momentary pH imbalances induced by acids consumed or released from the photoresist during the exposure or development process. [Brief description of the drawings]
[0020] [Figure 1] 1A to 1C are schematic cross-sectional views showing the order of steps for explaining a pattern formation method. [Diagram 2] 1A to 1C are schematic cross-sectional views showing the order of steps for explaining a pattern formation method. [Diagram 3] 1A to 1C are schematic cross-sectional views showing the order of steps for explaining a pattern formation method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, in describing the present invention, descriptions of already known functions or configurations will be omitted in order to clarify the gist of the present invention.
[0022] In order to clearly explain the present invention, parts unnecessary for the explanation are omitted, and the same or similar components are given the same reference numerals throughout the specification. In addition, the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, so the present invention is not necessarily limited to those shown in the drawings.
[0023] In the drawings, the thicknesses of various layers and regions are exaggerated to clearly show the layers and regions. Also, in the drawings, the thicknesses of some layers and regions are exaggerated for the convenience of explanation. When a layer, film, region, plate, or other part is described as being "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part therebetween.
[0024] In this specification, "substituted" means that a hydrogen atom is substituted with a deuterium atom, a halogen atom, a hydroxy group, an amino group, a substituted or unsubstituted amino group having 1 to 30 carbon atoms, a nitro group, a substituted or unsubstituted silyl group having 1 to 40 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, an alkylsilyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a cyano group. "Unsubstituted" means that a hydrogen atom is not substituted with another substituent and remains as a hydrogen atom.
[0025] As used herein, unless otherwise defined, an "alkyl group" refers to a straight or branched chain aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" that does not contain any double or triple bonds.
[0026] The alkyl group may be an alkyl group having 1 to 20 carbon atoms. More specifically, the alkyl group may be an alkyl group having 1 to 10 carbon atoms or an alkyl group having 1 to 6 carbon atoms. For example, an alkyl group having 1 to 4 carbon atoms means an alkyl group containing 1 to 4 carbon atoms in the alkyl chain, and indicates one selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl and t-butyl.
[0027] Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, a pentyl group, a hexyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group.
[0028] In this specification, unless otherwise defined, a "cycloalkyl group" means a monovalent cyclic aliphatic hydrocarbon group.
[0029] As used herein, unless otherwise defined, an "alkenyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group and an aliphatic unsaturated alkenyl group containing one or more double bonds.
[0030] As used herein, unless otherwise defined, an "alkynyl group" refers to a straight-chain or branched-chain aliphatic hydrocarbon group and an aliphatic unsaturated alkynyl group containing one or more triple bonds.
[0031] As used herein, an "aryl group" refers to a substituent in which all elements of the cyclic substituent have p-orbitals and these p-orbitals form conjugation, including monocyclic or fused polycyclic (i.e., rings which share adjacent pairs of carbon atoms) functional groups.
[0032] The developer composition for metal-containing photoresist according to the present invention will now be described.
[0033] A developer composition for a metal-containing photoresist according to one embodiment of the present invention comprises an organic solvent, an acid compound, and a counter base of the acid compound.
[0034] The acid compound may be either an inorganic acid or an organic acid. Specific examples of inorganic acids include sulfuric acid, phosphonic acid, hydrochloric acid, nitric acid, carbonic acid, and phosphoric acid. Specific examples of organic acids include acetic acid, glycolic acid, methylphosphonic acid, vinylphosphonic acid, formic acid, propionic acid, succinic acid, malic acid, butyric acid, tartaric acid, and fumaric acid. These acid compounds may be used alone or in combination of two or more. The acid compound is preferably acetic acid, glycolic acid, sulfuric acid, phosphonic acid, methylphosphonic acid, vinylphosphonic acid, formic acid, propionic acid, and / or succinic acid.
[0035] The acid compound is contained in an amount of 0.01% by mass to 10% by mass based on the total mass of the composition.
[0036] The acid compound may be contained within the above range of 0.01% by mass to 5% by mass, specifically 0.05% by mass to 5% by mass, and more specifically 0.1% by mass to 5% by mass. When two or more types of acid compounds are contained, the above content means the total amount thereof.
[0037] The counter base of the acid compound is a salt of the acid compound. That is, the counter base of the acid compound may be a salt consisting of the conjugate base of the acid compound and its counter ion. In the composition of the present invention, an instantaneous imbalance in pH value may occur during the development process due to the acid consumed during development or released from the photoresist. However, by adding a counter base to create a similar pH buffer system, the instability caused by the imbalance in pH value can be reduced. Therefore, the reduction in instability caused by the imbalance in pH value can solve the problem of CD deviation, and as a result, the CD variation and LER can be reduced.
[0038] The counter base is contained in an amount of 0.001% by mass to 1% by mass based on the total mass of the composition.
[0039] The counter base may be contained within the above range of 0.001% by mass to 0.5% by mass, specifically 0.01% by mass to 0.5% by mass, and more specifically 0.05% by mass to 0.5% by mass. The counter base may be used alone or in combination of two or more. When two or more types of counter bases are contained, the above content means the total amount.
[0040] The acid compound and the counter base may be contained in a mass ratio of 1:0.01 to 1:1.
[0041] The acid compound and the counter base are contained in a mass ratio of 1:0.03 to 1:1 within the above range, and specifically may be contained in a mass ratio of 1:0.05 to 1:1.
[0042] When the mixture ratio of the acid compound and the counter base is within the above range, a buffer system is formed in the developer, and hydrogen ions (H + Even if the pH value increases or decreases, no sudden changes in pH occur, and the composition is stabilized, ensuring stable results in terms of CD variation and LER.
[0043] The counter base of the acid compound according to one embodiment may be derived from an ammonium salt, an alkali metal salt, an alkaline earth metal salt, or a combination thereof. The alkali metal salt includes, for example, a sodium salt, a potassium salt, and a lithium salt. The alkaline earth metal salt includes, for example, a calcium salt, a strontium salt, and a barium salt.
[0044] Specific examples of the counter base of the acid compound include ammonium acetate, ammonium glycolate, ammonium sulfate, ammonium phosphonate, ammonium methylphosphonate, ammonium vinylphosphonate, ammonium formate, ammonium propionate, ammonium succinate, sodium acetate, sodium glycolate, sodium sulfate, sodium phosphonate, sodium vinylphosphonate, sodium formate, sodium propionate, sodium succinate, potassium acetate, potassium glycolate, potassium sulfate, potassium phosphonate, potassium vinylphosphonate, potassium formate, potassium propionate, potassium succinate, calcium acetate, calcium sulfate, calcium phosphonate, calcium vinylphosphonate, calcium formate, and calcium succinate. The counter base is preferably ammonium acetate, ammonium glycolate, ammonium sulfate, ammonium phosphonate, ammonium methylphosphonate, ammonium vinylphosphonate, sodium formate, sodium propionate, sodium succinate, sodium vinylphosphonate, potassium acetate, potassium propionate, or potassium succinate.
[0045] Examples of the organic solvent contained in the metal-containing photoresist developer composition according to an embodiment include, but are not limited to, at least one of ethers, alcohols, glycol ethers, aromatic hydrocarbon compounds, ketones, and esters. For example, the organic solvent may be ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol methyl ether, diethylene glycol ethyl ether, propylene glycol, propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol ethyl ether, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentanol (or methyl isobutyl carbinol ( ... carbinol, MIBC), hexanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3- These include, but are not limited to, methyl methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, gamma-butyrolactone, methyl-2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate, or combinations thereof.
[0046] When other additives described later are contained, the organic solvent is contained in the amount remaining excluding the contained components.
[0047] The developer composition for metal-containing photoresist according to the present invention may further include at least one other additive selected from a surfactant, a dispersant, a moisture absorbent, and a coupling agent.
[0048] The metal-containing photoresist may include a metal compound containing at least one of an organotin oxo group and an organotin carboxyl group. The organotin oxo group may, for example, be an alkyl tin oxo group (also called an alkoxystannyl group). The organotin carboxyl group may, for example, be an alkyl tin carboxyl group (also called an acyloxystannyl group).
[0049] For example, the metal-containing photoresist may include a metal compound represented by the following Chemical Formula 1:
[0050] [ka]
[0051] In the above Chemical Formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 6 to 30 carbon atoms, and -R a -OR b (where R a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 30 carbon atoms, -OR c and -OC(=O)R d is selected from among R 2 ~R 4 At least one of the is -OR c and -OC(=O)R d is selected from among In this case, R c is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R d is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.
[0052] R in the above Chemical Formula 1 2 ~R 4 R in c and R d may each independently be a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.
[0053] Meanwhile, according to another embodiment, there is provided a method for forming a pattern, comprising the step of developing using the above-mentioned metal-containing photoresist developer composition. For example, the pattern produced may be a negative type photoresist pattern.
[0054] A method for forming a pattern according to one embodiment includes the steps of applying a metal-containing photoresist composition onto a substrate, drying and heating the composition to form a metal-containing photoresist film on the substrate, exposing the metal-containing photoresist film to light, and developing the metal-containing photoresist film using the above-mentioned metal-containing photoresist developer composition.
[0055] More specifically, the step of forming a pattern using the metal-containing photoresist composition can include a step of applying the metal-containing photoresist composition onto a substrate on which a thin film has been formed by spin coating, slit coating, inkjet printing, or the like, and a step of drying the applied metal-containing photoresist composition to form a photoresist film. The metal-containing photoresist composition can include a tin-based compound, and for example, the tin-based compound can include at least one of an alkyltin oxo group (also referred to as an alkoxystannyl group), an alkyltin carboxyl group (also referred to as an acyloxystannyl group), and an alkyltin hydroxyl group.
[0056] Next, a composition for removing edge bead of metal-containing photoresist may be applied along the edge of the substrate.
[0057] Next, a first heat treatment step can be performed to heat the substrate on which the metal-containing photoresist film is formed. The first heat treatment step can be performed at a temperature of 80° C. to 120° C. During this process, the solvent evaporates and the metal-containing photoresist film can be more firmly attached to the substrate.
[0058] Next, the photoresist film is exposed to light.
[0059] As an example, examples of light that can be used in the above exposure process include light having short wavelengths such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), and ArF excimer laser (wavelength 193 nm), as well as light having high energy wavelengths such as EUV (wavelength 13.5 nm) and E-Beam (electron beam).
[0060] More specifically, the exposure light in one embodiment may be short-wavelength light having a wavelength range of 5 nm to 150 nm, or may be light having a high-energy wavelength such as EUV (wavelength 13.5 nm) or E-Beam (electron beam).
[0061] In the step of forming the photoresist pattern, a negative type pattern may be formed.
[0062] The exposed areas of the photoresist film have a different solubility than the unexposed areas of the photoresist film by forming a polymer through a crosslinking reaction, such as condensation between organometallic compounds.
[0063] Next, the substrate is subjected to a second heat treatment step. The second heat treatment step can be performed at a temperature of 90° C. to 200° C. By performing the second heat treatment step, the exposed area of the photoresist film becomes less soluble in a developer.
[0064] Specifically, the photoresist film corresponding to the unexposed region is dissolved using the above-mentioned photoresist developer and then removed, thereby completing a photoresist pattern corresponding to the negative tone image.
[0065] As described above, the photoresist pattern can be formed by exposure to light having a wavelength such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and high-energy light such as EUV (wavelength 13.5 nm) and E-Beam (electron beam). The photoresist pattern can have a thickness of 5 nm to 100 nm. As an example, the photoresist pattern is formed to a thickness of 5 nm to 90 nm, 5 nm to 80 nm, 5 nm to 70 nm, 5 nm to 60 nm, 5 nm to 50 nm, 5 nm to 40 nm, 5 nm to 30 nm, or 5 nm to 20 nm.
[0066] Meanwhile, the photoresist pattern can have a half-pitch of 50 nm or less, such as 40 nm or less, for example 30 nm or less, such as 20 nm or less, for example 15 nm or less, and a line width roughness of 10 nm or less, 5 nm or less, 3 nm or less, 2 nm or less.
[0067] The method for forming a pattern will be specifically described below as an example with reference to the drawings.
[0068] 1 to 3 are schematic cross-sectional views showing the order of steps for explaining a pattern formation method.
[0069] Referring to FIG. 1, the exposed photoresist film is developed to form a photoresist pattern 130P.
[0070] In an exemplary embodiment, the exposed photoresist film may be developed to remove the unexposed areas of the photoresist film to form a photoresist pattern 130P consisting of the exposed areas of the photoresist film. The photoresist pattern 130P may include a plurality of openings OP.
[0071] In an exemplary embodiment, the photoresist film is developed by a negative-tone development (NTD) process, in which a developer composition for a metal-containing photoresist according to an embodiment can be used as the developer composition.
[0072] 2, the feature layer 110 is processed using the photoresist pattern 130P in the result of FIG.
[0073] For example, in order to process the feature layer 110, various processes can be performed, such as a process of etching the feature layer 110 exposed through the opening OP of the photoresist pattern 130P, a process of implanting impurity ions into the feature layer 110, a process of forming an additional film on the feature layer 110 through the opening OP, a process of deforming a part of the feature layer 110 through the opening OP, etc. Fig. 2 illustrates, as an example process of processing the feature layer 110, etching the feature layer 110 exposed through the opening OP to form a feature pattern 110P.
[0074] 3, the photoresist pattern 130P remaining on the feature pattern 110P in the resultant structure of FIG. 2 is removed. An ashing and stripping process can be used to remove the photoresist pattern 130P. EXAMPLES
[0075] The present invention will be described in more detail with reference to the following examples of the preparation of the above-mentioned metal-containing photoresist developer composition, but the technical features of the present invention are not limited to the following examples.
[0076] [Production of metal-containing photoresist developer composition] The organic solvent (PGMEA) and additives were mixed in the compositions shown in Table 1 below in a polypropylene bottle (PP bottle), and then completely dissolved by shaking at room temperature (25°C).Then, the mixture was passed through a PTFE filter having a pore size of 1 μm to obtain a developer composition.
[0077] [Table 1]
[0078] [Preparation of metal-containing photoresist composition] An organometallic compound having a structural unit represented by the following chemical formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1% by weight, and then filtered through a 0.1 μm PTFE syringe filter to prepare a metal-containing photoresist composition.
[0079] [ka]
[0080] (Rating 1: CD measurement) The developer is injected during the development process of the coating-exposure-development process for producing patterned wafers, and is evaluated. After the process is completed, the patterned wafer has a line / space CD pattern formed, and is then transferred to a CD-SEM measurement device to measure the CD (Critical Dimension) size. The CD size is measured at 10 points using a CD-SEM image, and the average value and standard deviation (std) are calculated, and the standard deviation (std) is listed in Table 1.
[0081] Referring to Table 1, it can be seen that when the metal-containing photoresist developer compositions of Examples 1 to 15 are used, the CD size variation is smaller and superior properties are exhibited compared to when the metal-containing photoresist developer compositions of Comparative Examples 1 to 6 are used.
[0082] Although specific embodiments of the present invention have been described and illustrated above, the present invention is not limited to the described embodiments, and it is obvious to those skilled in the art that various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, such modifications or variations should not be understood individually from the technical spirit and perspective of the present invention, and the modified embodiments belong to the scope of the claims of the present invention. [Explanation of symbols]
[0083] 100 Substrates OP Opening 110 Feature Layer 110P Feature Pattern 130P Photoresist pattern
Claims
1. Organic solvents, Acid compounds, and The counter base of the acid compound 1. A developer composition for a metal-containing photoresist comprising:
2. 2. The developer composition for metal-containing photoresist according to claim 1, wherein the acid compound is contained in an amount of 0.01% by mass to 10% by mass based on the total mass of the composition.
3. 2. The developer composition for metal-containing photoresist according to claim 1, wherein the counter base is contained in an amount of 0.001% by mass to 1% by mass based on the total mass of the composition.
4. 2. The developer composition for metal-containing photoresist according to claim 1, wherein the acid compound and the counter base are contained in a mass ratio of 1:0.01 to 1:
1.
5. 2. The metal-containing photoresist developer composition of claim 1, wherein the counter base is derived from an ammonium salt, an alkali metal salt, an alkaline earth metal salt, or a combination thereof.
6. 2. The developer composition for metal-containing photoresist of claim 1, wherein the metal-containing photoresist comprises a metal compound containing at least one of an organotin oxo group and an organotin carboxyl group.
7. The metal-containing photoresist developer composition according to claim 6, wherein the metal compound is a compound represented by the following formula 1: [Formula 1] In the above Chemical Formula 1, R 1 is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 30 carbon atoms, and -R a -O-R b (Here, R a is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms; R b is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms; R 2 ~R 4 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 30 carbon atoms, -OR c and -OC(=O)R d is selected from among R 2 ~R 4 At least one of the groups is -OR c and -OC(=O)R d is selected from among At this time, R c is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof; R d is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a combination thereof.
8. R in the above Chemical Formula 1 2 ~R 4 R in c and R dThe developer composition for metal-containing photoresist according to claim 7, wherein each of the groups is independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms.
9. applying a metal-containing photoresist composition onto a substrate; a heat treatment step of drying and heating to form a metal-containing photoresist film on the substrate; exposing the metal-containing photoresist film to light; developing the photoresist using the developer composition for metal-containing photoresist according to any one of claims 1 to 8; A pattern forming method comprising the steps of:
Citation Information
Patent Citations
Method of forming resist mask
JP1982069743A
Composition and method for removing residue and patterning process
JP2006307158A
Organometallic photoresist developer compositions and processing methods
JP2022526031A
Locking device for sliding windows
KR1020240020064A
Method of manufacturing a semiconductor device
US20220351964A1