Cement admixture and producing method thereof, cement composition, cement-cured material and producing method thereof

A cement admixture using treated calcium aluminate slag and gypsum with balanced CaO/Al2O3 ratio addresses the issues of carbon emissions and slow strength development in cement production, ensuring adequate construction time and promoting rapid carbonation for enhanced strength and carbon dioxide absorption.

JP2024144178APending Publication Date: 2024-10-11TAIHEIYO MATERIALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024031253
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing cement production methods emit significant amounts of carbon dioxide and result in slow strength development and large drying shrinkage, while using calcium aluminate-based materials for rapid hardening accelerates setting, reducing construction time and initial strength development.

Method used

A cement admixture using calcium aluminate slag, treated with water to form a hydrate coating, is combined with gypsum and metal salts to achieve a balanced molar ratio of CaO to Al2O3, ensuring a sufficient pot life and good strength development, while incorporating carbonation curing to enhance carbon dioxide absorption.

Benefits of technology

The solution provides a cement admixture that balances pot life and strength development, reduces carbon emissions, and promotes rapid carbonation, achieving high compressive strength and efficient carbon dioxide absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144178000001
    Figure 2024144178000001
  • Figure 2024144178000002
    Figure 2024144178000002
  • Figure 2024144178000003
    Figure 2024144178000003
Patent Text Reader

Abstract

To provide a cement admixture that secures a sufficient usable time and has excellent strength developability, and to realize energy saving and CO2 reduction in the production of the cement admixture.SOLUTION: A cement admixture containing a calcium aluminate powder. Here, the powder contains a calcium aluminate slag having an inclusion molar ratio (CaO / Al2O3) of 0.9-1.5 between CaO and Al2O3 as a chemical component generated as a by-product during metal refining, and at least a part of the powder is subjected to a hydration treatment.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a cement admixture and a method for producing the same. The present invention also relates to a cement composition containing the cement admixture, a hardened cement product using the cement admixture, and a method for producing the same. [Background technology]

[0002] In recent years, the issue of global warming has become a major global concern, and various fields are seeking ways to reduce carbon dioxide emissions. It is known that the cement used in mortar concrete emits large amounts of carbon dioxide during its production. For this reason, the use of blended cement, in which part of the cement is replaced with blast furnace slag powder or fly ash, has been considered as one solution. However, it has been pointed out that mortar concrete using blended cement has problems such as slow strength development and large drying shrinkage. Furthermore, fly ash is produced as a by-product of coal-fired power generation, and coal-fired power generation itself emits large amounts of carbon dioxide, which is a problem. Therefore, it is expected that the number of coal-fired power plants will decrease in the future.

[0003] On the other hand, it is known that hardened mortar concrete gradually absorbs carbon dioxide from the air, resulting in so-called neutralization. Therefore, methods have been investigated to actively absorb carbon dioxide during the curing process of hardened mortar concrete, thereby reducing the total amount of carbon dioxide emitted during the production of mortar concrete. For example, Patent Document 1 proposes CO2-absorbing precast concrete, which incorporates γ-CS, a powder component with carbon dioxide absorption properties, and performs carbonation curing to form a carbonated region at a depth of 20 mm or more from the surface. Patent Document 2 also proposes a technology related to a cementitious hardened concrete that uses a cement mixing powder containing either mullite or anorthite, or both, and performs carbonation curing after demolding, thereby significantly reducing carbon dioxide emissions even when cured at approximately 20°C.

[0004] On the other hand, calcium aluminate-based slag is known to be generated as a by-product during metal refining. For example, calcium aluminate slag is known to be generated when aluminum is used as a deoxidizer in the steel slag produced as a by-product in the stainless steelmaking process. It has also been disclosed that calcium aluminate is generated as the primary slag in a metal chromium production process that includes a step of charging chromium oxide, aluminum, and lime (Patent Document 3). Furthermore, Patent Document 4 proposes a simple and inexpensive method for producing valuable metals such as V, Ni, and Mo and calcium aluminate from spent catalysts, such as spent desulfurization catalysts. Such calcium aluminate slag generated as a by-product is widely used in the refining process of steel manufacturers and other companies as a roasting solvent to replace fluorite or to adjust the composition of refining slag. Another effective utilization method has been proposed: using calcium aluminate as a raw material for CaO and Al2O3 in the production of alumina cement (Patent Document 5). Effective utilization of calcium aluminate as a by-product is an important technology currently in demand from the perspectives of energy conservation and CO2 reduction.

[0005] The present invention has investigated a new method for utilizing such calcium aluminate slag and discovered its effective use in hardened cement pastes. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2011-168436 [Patent Document 2] Japanese Patent Application Laid-Open No. 2016-153357 [Patent Document 3] International Publication WO2013 / 187348 [Patent Document 4] Japanese Patent Application Laid-Open No. 2004-35995 [Patent Document 5] Japanese Patent Application Laid-Open No. 2006-282486 Summary of the Invention [Problem to be solved by the invention]

[0007] Calcium aluminate is commonly used as the main component of rapid-hardening materials for cement. Therefore, the present inventors prepared an admixture using calcium aluminate slag instead of calcium aluminate and added it to mortar concrete for further investigation. However, when an admixture using calcium aluminate slag is used, the setting of mortar concrete becomes rapid. It was found that adding a large amount of set adjuster reduces the early strength development even when sufficient construction time (working time) is ensured. The objective of the present invention is to provide a cement admixture that effectively utilizes calcium aluminate slag to achieve sufficient working time and good strength development while saving energy and reducing CO2 emissions, as well as a cement composition and hardened cement product using the admixture. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems and have found that a cement admixture with sufficient pot life and good strength development can be obtained by hydrating a powder of a calcium aluminate-based material containing calcium aluminate slag having an appropriate molar ratio of CaO to Al2O3, thereby completing the present invention. That is, the present invention is as shown in [1] to

[12] . [1] A cement admixture comprising a powder of a calcium aluminate-based material, The powder contains calcium aluminate slag, which is generated as a by-product during metal refining and has a molar ratio of CaO to Al2O3 (CaO / Al2O3) of 0.9 to 1.5 as chemical components, and A cement admixture, wherein at least a portion of the powder has been subjected to a hydration treatment. [2] The content of calcium aluminate slag in the powder is 30 to 100 mass%, The cement admixture according to [1], wherein the proportion of the hydrated powder in the powder is 50 to 100 mass %. [3] The cement admixture according to [1] or [2], further comprising gypsum, wherein the content of the powder in the cement admixture is 20 to 80 mass %, and the content of the gypsum in the cement admixture is 80 to 20 mass %. [4] The cement admixture according to any one of [1] to [3], further comprising one or more metal salts selected from the group consisting of aluminum sulfates, alkali metal sulfates, and alkali metal carbonates. [5] The cement admixture according to any one of [1] to [4], further comprising one or more retarders selected from organic acids or salts thereof. [6] A cement composition comprising the cement admixture according to any one of [1] to [5] and cement. [7] The cement composition according to [6], wherein the cement is Portland cement. [8] The cement composition according to [6] or [7], wherein the content of the cement admixture is 10 to 30 parts by mass per 100 parts by mass of the total of the cement and the cement admixture. [9] The cement composition according to any one of [6] to [8], further comprising a set retarder.

[10] A hardened cement product obtained by hardening the cement composition according to any one of [6] to [9].

[11]

[10] The hardened cement body according to

[10] , wherein the carbonation rate of the hardened cement body is 0.3 mm / day or more.

[12] A cement admixture preparation step of kneading the cement admixture according to any one of [1] to [5], cement, water, and aggregate to prepare a cement admixture; A casting step of casting the cement mixture into a formwork; a demolding step of demolding the hardened cement mixture from the formwork after the cement mixture cast in the formwork has hardened; a carbonation curing step of curing the hardened body of the cement kneaded material released from the formwork in an atmosphere containing carbon dioxide; A method for producing a hardened cement product, comprising:

[13] A method for producing a cement admixture containing a powder of a calcium aluminate-based material, comprising: (A) a calcium aluminate slag content adjusting step in which the powder is prepared so that calcium aluminate slag, which is generated as a by-product during metal refining and has a molar ratio of CaO to Al2O3 (CaO / Al2O3) of 0.9 to 1.5 as chemical components, is contained in the powder at 30 to 100 mass%; (B) a hydration treatment step of hydrating the powder; (C) a water content adjusting step of adjusting the proportion of the water-treated powder in the cement admixture to 50 to 100 mass %; A method for producing a cement admixture, comprising: [Effects of the Invention]

[0009] According to the present invention, a cement admixture can be obtained that has sufficient pot life and good strength development. This effectively utilizes calcium aluminate slag, a by-product of metal refining, and can achieve energy savings and CO2 reduction in the production of the cement admixture. Furthermore, by using this cement admixture, a hardened cement product with good strength development and a fast carbonation rate can be obtained. DETAILED DESCRIPTION OF THE INVENTION

[0010] <Cement admixture> The cement admixture of the present invention contains a powder of a calcium aluminate-based material obtained by hydration, and the calcium aluminate-based material includes calcium aluminate slag generated as a by-product during metal refining. This cement admixture will be described in detail below.

[0011] (Calcium aluminate powder) The calcium aluminate powder of the present invention is a substance whose main component is a calcium aluminate compound composed of CaO and Al2O3, such as CaO·2Al2O3, CaO·Al2O3, 12CaO·7Al2O3, and 3CaO·Al2O3. Calcium aluminate compounds containing small amounts of components other than CaO and Al2O3 include calcium aluminoferrites such as 4CaO·Al2O3·Fe2O3 and 2CaO·Al2O3·Fe2O3, which are compounds consisting of CaO, Al2O3, and Fe2O3; calcium fluoroaluminates such as 3CaO·3Al2O3·CaF2 and 11CaO·7Al2O3·CaF2, in which halogens are dissolved or substituted in calcium aluminate; calcium sodium aluminates such as 8CaO·Na2O·3Al2O3, in which sodium is partially substituted; and calcium aluminosilicates in which SiO2 is partially dissolved or substituted. Additionally, calcium aluminate-based materials include industrially produced alumina cement and calcium aluminate slag, which is generated as a by-product.

[0012] The calcium aluminate-based material may be crystalline, amorphous, or a mixture of amorphous and crystalline materials. The calcium aluminate-based material may also contain impurities such as K2O, TiO2, MgO, SrO, and MnO. These impurities are derived from natural raw materials, such as limestone and bauxite, used in the production of the calcium aluminate-based material.

[0013] The calcium aluminate-based substance in the present invention includes calcium aluminate slag (details will be described later) generated as a by-product during metal refining, but may also include other calcium aluminate-based substances. Alumina cement is preferred as a calcium aluminate-based substance other than calcium aluminate slag. Alumina cement is a cement containing calcium aluminates primarily composed of CaO·2Al2O3 and CaO·Al2O3, and is widely used in monolithic refractories. The cement admixture used in the present invention is preferably manufactured and sold as Alumina Cement No. 1, which falls under the former JIS Classification Type 3.

[0014] In the calcium aluminate-based material of the present invention, the molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) as chemical components is preferably 0.9 to 1.7, more preferably 0.95 to 1.4, and particularly preferably 1.0 to 1.3, from the viewpoints of ensuring usable time and developing strength. In addition, the fineness of the material is preferably 3000 to 8000 cm2 in terms of Blaine specific surface area. 2 / g, and 3500 to 7000 cm 2 / g is more preferred.

[0015] Calcium aluminate-based materials can be produced by mixing raw materials for CaO sources such as quicklime and limestone, Al2O3 sources such as bauxite and band shale, and other raw materials in a predetermined ratio, and firing or melting the mixture at a temperature of 1400 to 2000°C in an electric furnace, rotary kiln, melting furnace, etc. The fired or melted material is cooled and then pulverized to obtain powder of the calcium aluminate-based material.

[0016] (Calcium aluminate slag) The calcium aluminate-based material of the present invention is characterized by containing calcium aluminate slag, which is generated as a by-product during metal refining. The content of this calcium aluminate slag in the calcium aluminate-based material is preferably 30 to 100 mass%, more preferably 40 to 95 mass%, and particularly preferably 50 to 90 mass%. If the content is less than 30 mass%, there is a risk that the initial strength development will be reduced.

[0017] Specific examples of calcium aluminate slag in the present invention include calcium aluminate slag produced during the refining of nickel, molybdenum, vanadium, etc., or alloys with iron such as ferronickel and ferrovanadium. Regarding chemical components, the CaO / Al2O3 molar ratio is preferably 0.9 to 1.5, more preferably 0.95 to 1.4, and particularly preferably 1.0 to 1.3. If the CaO / Al2O3 molar ratio is less than 0.9, there is a risk that initial strength development will be insufficient. On the other hand, if the CaO / Al2O3 molar ratio exceeds 1.5, there is a risk that it will be difficult to ensure a sufficient working life.

[0018] The calcium aluminate slag of the present invention may contain, as its mineral phase, krotite (CaO Al2O3), mayenite (12CaO 7Al2O3), gehlenite (2CaO Al2O3 SiO2), calcium aluminoferrite (4CaO Al2O3 Fe2O3), periclase (MgO), akermanite (2CaO MgO 2SiO2), etc. Among these, those containing krotite as the main component (50 mass% or more) are preferred.

[0019] Furthermore, from the viewpoint of early strength development, it is preferable to contain mayenite. Mayenite has high initial hydration activity and contributes to early strength development. However, if it is contained in a large amount, it may accelerate the setting of mortar concrete, making it difficult to ensure the usable time. For this reason, the content is preferably 1 to 20 mass%, more preferably 2 to 10 mass%, and even more preferably 3 to 8 mass%. The content of mayenite can be measured using an X-ray diffractometer by a calibration curve method, the Rietveld method, or the like.

[0020] In addition, calcium aluminate slag may contain small amounts of metals and metal oxides, such as iron, nickel, molybdenum, vanadium, chromium, and cobalt. The metal and metal oxide content is preferably 5% by mass or less in terms of metal oxide.

[0021] The ignition loss of calcium aluminate slag usually increases (indicated by a + sign). Here, ignition loss refers to the weight loss when heated in air at 950°C for one hour. The increase in ignition loss is thought to be due to the transition metals contained in the slag remaining in the metallic state or in the form of low-valence compounds.

[0022] Furthermore, calcium aluminate slag is usually cooled naturally, resulting in a crystalline product with almost no amorphous calcium aluminate. The vitrification rate is not particularly limited, but is typically less than 20%. The vitrification rate can be measured using an X-ray diffractometer, either by the calibration curve method or the Rietveld method.

[0023] Calcium aluminate slag is usually obtained as a mass of several mm to several tens of cm, which is then crushed to produce calcium aluminate slag powder. The fineness of calcium aluminate slag powder is 3000 to 8000 cm in terms of Blaine specific surface area. 2 / g, and 3500 to 7000 cm 2 / g is more preferred.

[0024] (Water treatment) The calcium aluminate-based substance used in the cement admixture of the present invention contains a powder of a calcium aluminate-based substance obtained by hydration treatment. This forms a coating layer of calcium aluminate hydrate on the surface of the powder particles, suppressing hydration reactions upon contact with water and ensuring a sufficient usable time (e.g., 40 minutes or more) even when used in mortar or concrete. The proportion of the powder of calcium aluminate-based substance obtained by hydration treatment in the calcium aluminate-based substance is preferably 50 to 100 mass%, more preferably 60 to 95 mass%, and particularly preferably 70 to 90 mass%. If it is less than 50 mass%, there is a risk that a sufficient usable time cannot be ensured.

[0025] The hydrate that is coated on the surface of powder particles of a calcium aluminate-based substance is not particularly limited, and examples thereof include CaO·Al2O3·10H2O, 2CaO·Al2O3·8H2O, 3CaO·Al2O3·6H2O, 3CaO·Al2O3·8H2O, 4CaO·Al2O3·13H2O, 4CaO·Al2O3·19H2O, CaO·H2O, Al2O3·H2O, Al2O3·3H2O, 3CaO·Al2O3·CaSO4·12H2O, 3CaO·Al2O3·3CaSO4·32H2O, 3CaO·Al2O3·CaCO3·12H2O, and 3CaO·Al2O3·3CaCO3·30H2O.

[0026] The cement admixture of the present invention can contain gypsum in addition to the powder of calcium aluminate-based material obtained by the above-mentioned hydration treatment.

[0027] The gypsum is not particularly limited as long as it is anhydrous gypsum, dihydrate gypsum, or hemihydrate gypsum, but anhydrous gypsum is preferred from the viewpoint of the strength-enhancing effect. In addition, both natural and chemical gypsum produced as by-products can be used. The Blaine specific surface area of ​​the gypsum is 3000 to 12000 cm 2 / g is preferred, and 4000 to 10000 cm 2 / g is more preferable. When the cement admixture according to the present invention contains gypsum, the content of the powder in the cement admixture is preferably 20 to 80 mass% and the content of the gypsum is preferably 80 to 20 mass%. The amount of gypsum blended is preferably 20 to 150 parts by mass, more preferably 30 to 100 parts by mass, per 100 parts by mass of the calcium aluminate-based substance.

[0028] Furthermore, the cement admixture according to the present invention preferably further contains one or more metal salts selected from the group consisting of aluminum sulfate, alkali metal sulfate, and alkali metal carbonate. As the aluminum sulfate, aluminum sulfate and its hydrate can be used. For example, commercially available aluminum sulfate (aluminum sulfate 14-17 hydrate) can be used. When used, the amount of aluminum sulfate is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, per 100 parts by mass of the calcium aluminate-based material.

[0029] Examples of the alkali metal sulfate include lithium sulfate, potassium sulfate, sodium sulfate, etc. When the alkali metal sulfate is added, the amount of the alkali metal sulfate added is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, per 100 parts by mass of the calcium aluminate-based substance.

[0030] Examples of the alkali metal carbonate include lithium carbonate, potassium carbonate, sodium carbonate, etc. When the alkali metal carbonate is added, the amount of the alkali metal carbonate is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, per 100 parts by mass of the calcium aluminate-based substance. The cement admixture of the present invention can contain both the above-mentioned gypsum and metal salt at the same time.

[0031] The cement admixture of the present invention may further contain one or more retarders selected from organic acids or their salts. Examples of organic acids include citric acid, gluconic acid, malic acid, and tartaric acid, and examples of their salts include sodium citrate, potassium citrate, sodium gluconate, and Rochelle salt. Citric acid, tartaric acid, and alkali metal salts thereof are particularly preferred in terms of their retarding effect on calcium aluminate-based materials (calcium aluminate slag) and compatibility with strength development. The amount of retarder blended in the cement admixture is preferably 0.5 to 5 mass %, more preferably 1 to 3 mass %.

[0032] <Cement composition> The cement composition of the present invention is a composition containing cement and the above-mentioned cement admixture. Examples of cement include various Portland cements, such as normal, early-strength, ultra-early-strength, low-heat, and moderate-heat cements, as well as various blended cements and ecocements obtained by mixing these Portland cements with fly ash, blast furnace slag, silica fume, or limestone powder. These can be used alone or in combination of two or more. From the viewpoints of strength development and the fresh properties of the kneaded product, the amount of cement admixture is preferably 20 to 100 parts by mass, more preferably 30 to 80 parts by mass, per 100 parts by mass of cement. In one embodiment, the content of the cement admixture is preferably 10 to 30 parts by mass per 100 parts by mass of the total of cement and cement admixture. If the content of the cement admixture is excessively low, early strength development may be poor and carbonation may be difficult to proceed. On the other hand, if the viscosity is too high, it may be difficult to ensure the fluidity of the cement mixture, and the strength elongation after the initial strength development may be poor. Furthermore, aggregate and water are appropriately added to the cement composition. The cement mixture is obtained by adding aggregate and water appropriately to the cement composition and kneading them.

[0033] (cement) The cement used in the present invention is not particularly limited, and examples thereof include various Portland cements such as ordinary, early strength, ultra-early strength, moderate heat, and low heat, mixed cements such as blast furnace cement and fly ash cement, ecocement, etc. Among these, ordinary Portland cement or early strength Portland cement is preferred from the viewpoint of strength development and cost.

[0034] (aggregate) The aggregates used in the present invention include fine aggregates and coarse aggregates. These aggregates are not particularly limited, and aggregates generally used in mortar concrete can be used. Examples of fine aggregates that can be used include river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, and mixtures thereof. Examples of coarse aggregates that can be used include river gravel, mountain gravel, land gravel, crushed stone, and mixtures thereof.

[0035] The amount of aggregate to be mixed (the total amount when fine aggregate and coarse aggregate are used in combination) is preferably 200 to 700 parts by mass, more preferably 200 to 600 parts by mass, per 100 parts by mass of cement and cement admixture, from the viewpoints of fluidity, crack prevention, and material separation prevention. When fine aggregate and coarse aggregate are used in combination, the fine aggregate ratio is preferably 5 to 60%.

[0036] (water) The water used in the present invention is not particularly limited, and may be tap water, etc. In the above cement mixture, the blending ratio of water to a total of 100 parts by mass of cement and cement admixture is preferably 30 to 100 parts by mass, more preferably 40 to 70 parts by mass.

[0037] The cement composition of the present invention preferably contains a set retarder to adjust the working life. Examples of set retarders include organic acids such as citric acid, gluconic acid, malic acid, and tartaric acid, or their salts, boric acid, borates such as sodium borate, phosphates, and sugars. The amount of set retarder added is appropriately adjusted within the range of 0.1 to 5.0 parts by mass per 100 parts by mass of the total of the cement and cement admixture.

[0038] In addition to the cement and the above-mentioned cement admixture, the cement composition of the present invention can contain additives and aggregates in combination to the extent that the features of the present invention are not impaired. Examples of such additives include cement dispersants such as water reducing agents, air-entraining water reducing agents, high-performance water reducing agents, superplasticizers, strength promoters, polymers for cement admixtures, foaming agents, foaming agents, waterproofing agents, rust inhibitors, shrinkage reducing agents, thickeners, water retention agents, pigments, water repellents, anti-efflorescence agents, defoamers, fibers, silica fume, and calcium carbonate fine powder.

[0039] <Hardened cement> The hardened cement product of the present invention is a hardened cement product obtained by hardening the above-mentioned cement composition. Examples of hardened cement products include mortar and concrete. The hardened cement product of the present invention exhibits good strength development at an early age and also at an age of 14 days. There is almost no decrease in compressive strength compared to when only cement is used without using a cement admixture. The compressive strength at an age of 14 days is 90% or more compared to when only cement is used.

[0040] The hardened cement product of the present invention is characterized by a fast carbonation rate. Specifically, when carbonation cured at a carbon dioxide gas concentration of 5%, the rate of progression of carbonation depth (carbonation rate) is 0.3 mm / day or more. In a particularly preferred blend, it is 0.5 mm / day or more.

[0041] As described above, the hardened cement product of the present invention uses calcium aluminate slag generated as a by-product, and has good strength development, rapidly absorbs carbon dioxide, and rapidly promotes carbonation. Furthermore, the total amount of carbon dioxide emitted during the production of the hardened cement product can be significantly reduced, taking into account the amount of carbon dioxide absorbed after hardening.

[0042] <Method of manufacturing hardened cement> The method for producing a hardened cement product of the present invention includes a cement mixture preparation step of preparing a cement mixture by mixing the above-mentioned cement admixture with cement, water, and aggregate; a casting step of casting the cement mixture into a formwork; a demolding step of releasing the hardened cement mixture from the formwork after the cement mixture in the formwork has hardened; and a carbonation curing step of curing the hardened cement mixture released from the formwork in an atmosphere containing carbon dioxide.

[0043] The cement mixture preparation step is a step of preparing a cement mixture by mixing the cement admixture, cement, water, and aggregate materials of the present invention. The method of mixing the materials is not particularly limited. The equipment used for mixing is also not particularly limited, but conventional mixers such as pan mixers, twin-screw mixers, and tilting mixers used for mixing general mortar concrete can be used.

[0044] The casting process is a process of casting the cement mixture into a formwork. The casting method is not particularly limited, and casting is performed by a conventional method used in the production of general mortar concrete. The curing method from casting the cement mixture into the formwork until demolding is not particularly limited, and general curing methods such as air curing, underwater curing, sealed curing, and steam curing can be used.

[0045] The demolding step is a step of demolding the hardened cement mixture from the formwork after the cement mixture in the formwork has hardened. 2 It is preferable that this is equal to or greater than this.

[0046] The carbonation curing process is a process of curing the hardened cement body in an atmosphere containing carbon dioxide. The carbon dioxide-containing atmosphere is not particularly limited as long as it contains carbon dioxide that promotes carbonation (synonymous with neutralization) of the hardened cement body, but a carbon dioxide gas concentration of 1% or more can increase the amount of carbon dioxide absorbed by the hardened cement body. It is preferably 2% or more, more preferably 3% or more, and particularly preferably 5% or more. There is no particular upper limit to the carbon dioxide gas concentration, and the higher the carbon dioxide gas concentration, the greater the amount of carbon dioxide absorbed. However, from the viewpoint of reducing the cost of curing equipment, etc., it is preferably 90% or less, more preferably 70% or less, and particularly preferably 50% or less.

[0047] The temperature in the carbonation curing step is not particularly limited, but is preferably 5 to 80° C. The relative humidity in the carbonation curing step is not particularly limited, but is preferably 30 to 90%.

[0048] <Manufacturing method of cement admixture> The method for producing a cement admixture of the present invention is a method for producing a cement admixture containing a powder of a calcium aluminate-based material obtained by a hydration treatment, the calcium aluminate-based material including calcium aluminate slag generated as a by-product during metal refining, and includes steps (A) to (C). Each step will be described in detail below.

[0049] (A) Calcium aluminate slag content preparation process This process adjusts the calcium aluminate slag content in the calcium aluminate-based substance. Powder of calcium aluminate slag and powder of a calcium aluminate-based substance other than calcium aluminate slag are mixed in a predetermined ratio to prepare the calcium aluminate-based substance. The mixing method is not particularly limited, and mixing can be performed using a powder mixer. Examples of powder mixers that can be used include a Lödige mixer, a Henschel mixer, a Nauta mixer, and a VH powder mixer. The mixing time is adjusted appropriately depending on the amount of material to be mixed and the equipment used, but is preferably 2 to 30 minutes. When using a lumpy calcium aluminate-based substance, the calcium aluminate slag content can be adjusted by mixing and grinding it with calcium aluminate slag. The grinding method is also not particularly limited, and grinding can be performed using a grinding device such as a ball mill or a vibration mill.

[0050] (B) Hydration process This process involves hydrating a powder of a calcium aluminate-based material containing calcium aluminate slag. This results in the formation of a hydrate coating layer on the surface of the powder particles. While the hydration method is not particularly limited, it is preferable to use a powder mixer in which a predetermined amount of water is gradually sprayed with a sprayer to mix, as this results in a relatively uniform hydrate phase coating. Examples of powder mixers that can be used include a Lödige mixer, a Henschel mixer, a Nauta mixer, and a VH powder mixer. The mixing time is adjusted appropriately depending on the amount of material to be mixed and the equipment used, but is preferably 2 to 30 minutes. The amount of water sprayed is preferably 0.2 to 3.5 mass% based on the weight of the calcium aluminate-based material. Instead of spraying water, other liquids (e.g., aqueous organic solvents, carbonated water) can be used as long as they react with calcium aluminate to form hydrates.

[0051] (C) Water content adjustment process This step is a step of adjusting the proportion of calcium aluminate-based material powder obtained by hydration treatment (hydration ratio) in the calcium aluminate-based material. Specifically, the hydration ratio is adjusted by blending and mixing a powder of a hydrated calcium aluminate-based material with a powder of an unhydrated calcium aluminate-based material that has not been hydrated, so that the hydration ratio is 50 to 100% by mass. The mixing method is not particularly limited, and mixing can be performed using a powder mixer. Examples of powder mixers that can be used include a Lödige mixer, a Henschel mixer, a Nauta mixer, and a VH powder mixer. The mixing time can be adjusted appropriately depending on the amount of material to be mixed and the equipment used, but is preferably 2 to 30 minutes.

[0052] Furthermore, if necessary, the gypsum is mixed with one or more selected from the group consisting of aluminum sulfate, alkali metal sulfate, and alkali metal carbonate to prepare a cement admixture. The mixing method is not particularly limited, and mixing can be performed using a powder mixer. Examples of powder mixers that can be used include a Loedige mixer, a Henschel mixer, a Nauta mixer, and a VH powder mixer. The mixing time is adjusted appropriately depending on the amount of material to be mixed and the equipment used, but is preferably 2 to 30 minutes. [Example]

[0053] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following examples.

[0054] Example 1 (1) Calcium aluminate slag (code: CAS) Calcium aluminate slag generated during metal refining was used. Calcium aluminate slag generated as slag after refining ferrovanadium was used. The chemical composition of the calcium aluminate slag is shown in Table 1. This calcium aluminate slag contained 0.66 mass% vanadium in oxide equivalent. The CaO / Al2O3 molar ratio was 1.1, and the ignition loss was +0.25 mass% (gain). The mineral composition included 80 mass% krotite, 5 mass% mayenite, 10 mass% gehlenite, and 2 mass% periclase. The vitrification rate was 2%. The mineral content and vitrification rate were calculated by the Rietveld method using an X-ray diffractometer. This calcium aluminate slag was coarsely crushed and then pulverized in a ball mill to obtain a slag with a Blaine specific surface area of ​​5020 cm2. 2 / g of powder.

[0055] [Table 1]

[0056] (2) Preparation of calcium aluminate-based materials As a calcium aluminate-based material other than calcium aluminate slag, commercially available alumina cement No. 1 was used. This alumina cement had a CaO / Al2O3 molar ratio of 1.2 and a mineral composition consisting mainly of chlorite. The mayenite content was measured using X-ray diffraction and found to be 0.3 mass%. The fineness was measured by a Blaine specific surface area of ​​4100 cm 2 The calcium aluminate slag powder and alumina cement were mixed in a Lödige mixer to adjust the calcium aluminate slag content in the calcium aluminate-based material.

[0057] (3) Hydration 50 kg of the prepared calcium aluminate powder was placed in a Lödige mixer, and 250 g of water was added by spraying using a sprayer while the mixer was rotating. After mixing for 10 minutes, a hydrated calcium aluminate powder was obtained.

[0058] (4) Preparation of cement admixture The powder of the calcium aluminate-based material that had been hydrated and the powder of the calcium aluminate-based material that had not been hydrated were mixed in a predetermined ratio (hydration ratio) and mixed for 10 minutes in a Lödige mixer. Various inorganic salts were then added and mixed for 10 minutes to prepare cement admixtures. The inorganic salts were 100 parts by mass of calcium aluminate-based material, and 100 parts by mass of anhydrous gypsum (commercially available; Blaine specific surface area 7100 cm) was used. 2 The mixture was mixed with 100 parts by mass of sodium sulfate (reagent; manufactured by Kanto Chemical Co., Ltd.), 6 parts by mass of sodium sulfate (reagent; manufactured by Kanto Chemical Co., Ltd.), and 6 parts by mass of lithium carbonate (reagent; manufactured by Kanto Chemical Co., Ltd.).

[0059] (5) Preparation of mortar specimens Mortar specimens were prepared using the prepared cement admixture (symbol: AD). The materials used are shown below. The mortar mix is ​​shown in Table 2. The mortar specimens were prepared and cured in a 20°C environment. 0.6% by mass of the retarder was added to the total amount of cement and cement admixture.

[0060] (Materials used) (1) Cement (C): Ordinary Portland cement (manufactured by Taiheiyo Cement Corporation, density: 3.16 g / cm 3 ) (2) Fine aggregate (S): JIS standard sand (3) Water (W): Tap water (4) Settling retarder: Citric acid (commercially available first-grade reagent)

[0061] [Table 2]

[0062] (Test Method) The test method is shown below. (1) Pot life The initial setting time was measured in accordance with JIS A 1147 "Test method for concrete setting time," and this initial setting time was taken as the working time. (2) Compressive strength The compressive strength of each age was measured in accordance with the Japan Society of Civil Engineers standard JSCE-G541 "Test method for compressive strength of filling mortar."

[0063] (Test results) The test results are shown in Table 3. In a 20°C environment, it was confirmed that when the hydration rate was 100% by mass and 50% by mass, the pot life could be secured and the initial strength development was good from the age of 4 hours. However, when the CAS content was 15% by mass, the compressive strength at the age of 4 hours decreased. When the hydration rate was 0% by mass, the pot life was less than 30 minutes, and it was confirmed that the time required for the construction process could not be secured.

[0064] [Table 3]

[0065] Example 2 Mortar specimens were prepared and cured in a 5°C environment. The amount of retarder added was 0.16% by mass relative to the total amount of cement and cement admixture when the water content was 100% by mass, and 0.25% by mass when the water content was 50% by mass. Otherwise, the test was carried out in the same manner as in Example 1.

[0066] The test results are shown in Table 4. In a 5°C environment, it was confirmed that when the hydration rate was 100% and 50% by mass, the pot life could be secured and that good initial strength development was achieved from an age of 4 hours. However, when the CAS content was 100% and 15% by mass, the compressive strength at an age of 4 hours decreased. Furthermore, when the hydration rate was 100% and the CAS content was 100%, the strength at an age of 6 hours also decreased. With a hydration rate of 0% by mass, the pot life was less than 30 minutes, confirming that the time required for the construction process could not be secured.

[0067] [Table 4]

[0068] Example 3 (1) Preparation of calcium aluminate-based materials In this example, the calcium aluminate-based substance used was the calcium aluminate slag powder prepared in Example 1. 50 kg of this powder was placed in a Lödige mixer, and while the mixer was rotating, 250 g of water was sprayed in using a sprayer to perform a hydration treatment, yielding calcium aluminate slag powder whose surface was coated with hydrate.

[0069] (2) Preparation of cement admixture Hydrated hydrate-coated calcium aluminate slag powder and anhydrous gypsum (commercial product, Blaine specific surface area 7100 cm) 2 / g) were mixed to prepare cement admixtures. The formulations of each cement admixture are shown in Table 5. As comparative examples, test samples were also tested: test sample (B) using unhydrated calcium aluminate slag powder; and test sample (C) using alumina cement (commercially available) instead of calcium aluminate slag.

[0070] [Table 5]

[0071] (3) Preparation of mortar The cement admixtures in Table 5 and ordinary cement (manufactured by Taiheiyo Cement Corporation, density: 3.16 g / cm 3 A cement mixture (mortar) was prepared using 100% slag, fine aggregate (JIS standard sand), and water (tap water). Table 6 shows the mortar mix prepared according to the cement admixture content. The mixture was mixed using a mortar mixer for 3 minutes and then subjected to various tests. The test methods are as follows:

[0072] [Table 6]

[0073] (Test Method) (1) Mortar flow The test was conducted in accordance with JIS R 5201 "Physical Tests for Mortar." (2) Compression strength test The compressive strength was tested at ages of 1 and 14 days in accordance with the Japan Society of Civil Engineers standard JSCE-G541 "Test method for compressive strength of filling mortar." The curing temperature was kept at 20°C until just before the test. (3) Compressive strength (4) Neutralization depth The test was conducted in accordance with JIS A 1152 "Method for measuring the depth of neutralization of concrete." The materials were sealed and cured for up to three days, after which they were demolded and tested in a neutralization tank at a temperature of 20°C, humidity of 60%, and CO2 concentration of 5% for 28 days.

[0074] (Test results) The test results are shown in Table 7. It can be seen that the cement hardened body of the present invention has good fluidity (mortar flow) of the cement mixture and also good strength development (compressive strength at 1 day and 4 day ages). The compressive strength ratio (at 14 days age) in the table indicates the strength ratio relative to the compressive strength of mortar without any cement admixture (Test No. 18). The test levels of the examples are all 0.90 or higher. Furthermore, the carbonation rate calculated from the carbonation depth at 28 days age is 0.3 mm / day or higher in all examples.

[0075] [Table 7]

[0076] Example 4 (1) Preparation of calcium aluminate-based materials As in Example 3, the calcium aluminate slag powder prepared in Example 1 was used as the calcium aluminate-based substance. The calcium aluminate slag powder that had been hydrated in the same manner as in Example 3 and the unhydrated calcium aluminate slag powder were mixed in the proportions shown in Table 8 to prepare a calcium aluminate slag powder mixture.

[0077] (2) Preparation of cement admixture The prepared powder mixture of calcium aluminate slag and anhydrous gypsum (commercial product, specific surface area 7100 cm) was used. 2 / g) were mixed to prepare cement admixtures. The formulations of each cement admixture are shown in Table 8.

[0078] [Table 8]

[0079] (3) Preparation of mortar The cement admixtures in Table 8 and ordinary cement (manufactured by Taiheiyo Cement Corporation, density: 3.16 g / cm 3 Mortar was prepared using 100% slag, fine aggregate (JIS standard sand), and water (tap water). Table 9 shows the mortar mixes prepared according to the cement admixture content. The mixture was mixed using a mortar mixer for 3 minutes and then subjected to various tests. The test methods are as follows:

[0080] (Test Method) (1) Mortar flow The test was conducted in accordance with JIS R 5201 "Physical Tests for Mortar." (2) Compression strength test The compressive strength was tested at 18 hours and 14 days in accordance with the Soil Science Society standard JSCE-G541 "Test method for compressive strength of filling mortar." The curing temperature was kept at 20°C until just before the test.

[0081] [Table 9]

[0082] (Test results) The mortar flow and compressive strength of each mortar were tested. The test results are shown in Table 10. It can be seen that the mortar using the cement admixture of the present invention has good fluidity (mortar flow immediately after preparation and after 60 minutes) and good strength development (compressive strength at 18 hours and 14 days).

[0083] [Table 10]

[0084] Example 5 (1) Preparation of cement admixture A powder mixture of calcium aluminate slag prepared in the same manner as in Example 4 and anhydrous gypsum (commercially available, Blaine specific surface area 7100 cm) was used. 2 / g), and citric acid (commercially available first-grade reagent) was mixed as a retarder to prepare a cement admixture. The formulation of each cement admixture is shown in Table 11.

[0085] [Table 11]

[0086] (2) Preparation of mortar The cement admixtures in Table 11 and ordinary cement (manufactured by Taiheiyo Cement Corporation, density: 3.16 g / cm 3 ), fine aggregate (JIS standard sand), and water (tap water) were used to prepare mortar in the same manner as in Example 4, and the mortar was subjected to various tests.

[0087] (Test results) The mortar flow and compressive strength of each mortar were tested. The test results are shown in Table 12. It can be seen that the fluidity of the mortar using the cement admixture containing the retarder was good, especially after 60 minutes, and that the strength development after 18 hours was also good.

[0088] [Table 12]

Claims

1. A cement admixture comprising a powder of a calcium aluminate-based material, The powder is a by-product of metal refining and contains CaO and Al as chemical components. 2 O 3 The molar ratio of CaO to Al 2 O 3 ) is 0.9 to 1.5, and A cement admixture, wherein at least a portion of the powder has been subjected to a hydration treatment.

2. The content of calcium aluminate slag in the powder is 30 to 100% by mass, The cement admixture according to claim 1, wherein the proportion of the hydrated powder in the powder is 50 to 100 mass%.

3. The cement admixture according to claim 1 or 2, further comprising gypsum, the content of the powder in the cement admixture being 20 to 80% by mass, and the content of the gypsum being 80 to 20% by mass.

4. 3. The cement admixture according to claim 1 or 2, further comprising one or more metal salts selected from the group consisting of aluminum sulfate, alkali metal sulfate and alkali metal carbonate.

5. 3. The cement admixture according to claim 1 or 2, further comprising one or more retarders selected from organic acids or salts thereof.

6. A cement composition comprising the cement admixture according to claim 1 or 2 and cement.

7. 7. The cement composition of claim 6, wherein the cement is Portland cement.

8. The cement composition according to claim 6, wherein the content of the cement admixture is 10 to 30 parts by mass per 100 parts by mass of the total of the cement and the cement admixture.

9. 7. The cement composition of claim 6 further comprising a set retarder.

10. A hardened cement product obtained by hardening the cement composition according to claim 6.

11. The hardened cement body according to claim 10, wherein a carbonation rate of the hardened cement body is 0.3 mm / day or more.

12. A cement admixture preparation step of kneading the cement admixture according to claim 1 or 2, cement, water, and aggregate to prepare a cement kneaded product; A casting step of casting the cement mixture into a formwork; a demolding step of demolding the hardened body of the cement kneaded material from the formwork after the cement kneaded material cast in the formwork has hardened; a carbonation curing step of curing the hardened body of the cement kneaded material removed from the formwork in an atmosphere containing carbon dioxide; A method for producing a hardened cement body, comprising:

13. A method for producing a cement admixture containing a powder of a calcium aluminate-based material, comprising: (A) The powder is a by-product of metal refining and contains CaO and Al as chemical components. 2 O 3 The molar ratio of CaO to Al 2 O 3 A calcium aluminate slag content adjustment step of adjusting calcium aluminate slag having a calcium aluminate content of 0.9 to 1.5 in the powder so that the calcium aluminate slag content is 30 to 100 mass %; (B) a hydration treatment step of hydrating the powder; (C) a water content adjustment step of adjusting the proportion of the water-treated powder in the cement admixture to 50 to 100 mass%; A method for producing a cement admixture, comprising:

Citation Information

Patent Citations

  • Method for manufacturing ferroalloy from spent catalyst

    JP2004035995A

  • Alumina cement, alumina cement composition, and monolithic refractory

    JP2006282486A

  • Concrete kneading material, co2 absorption precast concrete and method of producing the same

    JP2011168436A

  • Cement curing body and manufacturing method therefor

    JP2016153357A

  • Metal chrome fabrication method

    WO2013187348A1