Aqueous ink, ink cartridge, and inkjet recording method

The aqueous ink formulation with silica-coated titanium oxide, a specific water-soluble organic solvent, and a low HLB surfactant addresses the issues of ink fixation and water scratch resistance, providing enhanced durability and stability in inkjet recording.

JP2024144322APending Publication Date: 2024-10-11CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024050579
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-28
Filing Date
2024-03-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing aqueous inks for inkjet recording fail to provide sufficient ink fixation recovery properties and water scratch resistance, especially when used in outdoor or wet environments, due to issues with pigment dispersion stability and surfactant solubility in water.

Method used

An aqueous ink formulation containing titanium oxide particles coated with silica, a specific water-soluble organic solvent with a boiling point of 120°C to 230°C and SP value of 11.0 to 13.5, and a surfactant with an HLB value of 3 to 8, balanced at specific content percentages to enhance dispersion stability and reduce surfactant solubility in water.

Benefits of technology

The ink achieves improved ink fixation recovery and water scratch resistance, ensuring stable ejection and durable image quality even under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144322000016
    Figure 2024144322000016
  • Figure 2024144322000017
    Figure 2024144322000017
  • Figure 2024144322000001
    Figure 2024144322000001
Patent Text Reader

Abstract

To provide aqueous ink for inkjet or the like by which an image having excellent fixation recovering properties of ink and excellent water scratch resistance can be recorded.SOLUTION: Aqueous ink for inkjet contains titanium oxide particles, resin particles, water-soluble organic solvent, and surfactant. The water-soluble organic solvent includes a first water-soluble organic solvent having a boiling point of 120°C or higher and 230°C or lower and an SP value of 11.0 or more and 13.5 or less. The content (mass%) of the water-soluble organic solvent is 5.00 mass% or more and 30.00 mass% or less on the basis of the entire ink mass, and the ratio of the first water-soluble organic solvent (mass%) occupied in the water-soluble organic solvent is 0.70 times or more. The surfactant includes first surfactant having an HLB value of 3 or more and 8 or less. The content (mass%) of the surfactant is 0.10 mass% or more and 0.40 mass% or less on the basis of the entire ink mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based ink, an ink cartridge, and an ink-jet recording method. [Background technology]

[0002] In recent years, inkjet recording devices have come to be widely used when outputting advertisements or exhibits using recording media such as paper or resin film. In such cases, images that are required to be eye-catching are required to be recorded, and therefore images that exhibit high color development are required. From the viewpoints of environmental impact and safety, there is an increasing need for a recording method that can record images for the above-mentioned applications using aqueous inks containing pigments. Titanium oxide is widely used as a pigment for aqueous white inks for inkjet printing.

[0003] When an image is recorded on a recording medium using an aqueous ink containing a pigment, the resulting image is in a state where the pigment is fixed on the surface of the recording medium, so abrasion resistance is important. Furthermore, images recorded for the above-mentioned purposes may be used outdoors or in places where they are expected to get wet, such as labels, so abrasion resistance in a state where water is attached (hereinafter referred to as water abrasion resistance) is likely to be an issue. In order to improve the water abrasion resistance of aqueous ink, for example, a highly hydrophobic component that is not washed away by water can be added, but this makes the dispersion state of the pigment more unstable, making the ink more likely to stick. If the above-mentioned sticking occurs near the ejection port of the recording head, it is likely to lead to a decrease in ejection performance.

[0004] To date, in order to improve the water abrasion resistance of images and the fixation recovery of ink by ink components, for example, inks containing a surfactant with a low HLB value and a water-soluble organic solvent with a high boiling point have been proposed (see Patent Document 1). Also, inks containing a surfactant with a low HLB value, a specific resin, and a water-soluble organic solvent have been proposed (see Patent Document 2). Furthermore, an inkjet recording method using inks containing an organic pigment, a surfactant with a low HLB value, and a water-soluble organic solvent has been proposed (see Patent Document 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2022-131612 A [Patent Document 2] JP 2023-008056 A [Patent Document 3] JP 2013-230638 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors prepared an aqueous ink with reference to the inks proposed in Patent Document 1 and Patent Document 2, and investigated the ink adhesion recovery and water abrasion resistance of the image. In addition, an aqueous ink was prepared with reference to the ink proposed in Patent Document 3, and this aqueous ink was applied to the inkjet recording method described in Patent Document 3 to perform recording, and similarly investigated. As a result, it was found that the water abrasion resistance of the image and the ink adhesion recovery are insufficient and there is room for improvement in performance, given the current situation in which performance is required even under more severe environmental changes.

[0007] Therefore, an object of the present invention is to provide an aqueous ink for inkjet recording that is excellent in ink adhesion recovery and water abrasion resistance, an ink cartridge using said aqueous ink, and an inkjet recording method. [Means for solving the problem]

[0008] The above object is achieved by the present invention as described below. That is, the aqueous ink according to the present invention is an aqueous ink for inkjet containing titanium oxide particles, resin particles, a water-soluble organic solvent, and a surfactant, the titanium oxide particles are titanium oxide having at least a part of their surface covered with silica and are dispersed at least by the action of the silica, the water-soluble organic solvent includes a first water-soluble organic solvent having a boiling point of 120°C or more and 230°C or less and an SP value of 11.0 or more and 13.5 or less, the content (mass%) of the water-soluble organic solvent is 5.00% by mass or more and 30.00% by mass or less based on the total mass of the ink, the ratio (mass%) of the first water-soluble organic solvent to the water-soluble organic solvent is 0.70 times or more, the surfactant includes a first surfactant having an HLB value of 3 or more and 8 or less, and the content (mass%) of the surfactant is 0.10% by mass or more and 0.40% by mass or less based on the total mass of the ink. Effect of the Invention

[0009] According to the present invention, it is possible to provide a water-based ink for inkjet use that is excellent in ink adhesion recovery properties and is capable of recording images that are excellent in water abrasion resistance, an ink cartridge using the water-based ink, and an inkjet recording method. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view illustrating an embodiment of an ink cartridge of the present invention. [Diagram 2] 1A and 1B are diagrams illustrating an example of an inkjet recording apparatus used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording apparatus, and (b) is a perspective view of a head cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt." Titanium oxide and titanium oxide particles may be simply referred to as "pigment." Furthermore, water-based ink for inkjet printing may be simply referred to as "ink." Physical property values ​​are values ​​at room temperature (25°C) and normal pressure (1 atm) unless otherwise specified.

[0012] Inorganic oxides such as titanium oxide used as a pigment in white ink react with water molecules constituting the aqueous medium in the aqueous ink to generate hydroxyl groups (hereinafter, sometimes referred to as "surface hydroxyl groups") on the surface. For this reason, in the case of aqueous inkjet inks, in order to utilize the generated surface hydroxyl groups while further improving the storage stability of the ink, they are generally used in a state where they have been surface-treated with inorganic oxides such as alumina and silica. The surface hydroxyl groups of titanium oxide particles have properties specific to the inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the isoelectric point, which is an indicator of the strength of the acid, differs depending on the type of inorganic compound. Therefore, although titanium oxide itself is an inorganic oxide, the surface of titanium oxide particles shows the properties of an inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the surface charge of titanium oxide particles is strongly dependent on the pH of the aqueous medium, the type of surface treatment agent, and the amount of the surface treatment agent used. In other words, "titanium oxide is dispersed at least by the action of silica" means that at least a part of the surface of the titanium oxide particles is covered with silica and dispersed by the action of its surface hydroxyl groups. However, if the water-soluble resin serving as a dispersant for titanium oxide particles is contained in excess (for example, 0.01 times or more in terms of mass ratio relative to the titanium oxide content), it is believed that this will destabilize the dispersion caused by the action of silica. Of course, this does not exclude the addition of materials that aid dispersion. Simply put, if a water-soluble resin is used when dispersing titanium oxide (when preparing the dispersion), it can be determined that the titanium oxide is dispersed by the water-soluble resin serving as a dispersant.

[0013] Generally, a surfactant is added to an aqueous ink to reduce image unevenness, and a water-soluble organic solvent is added to suppress adhesion of pigments to the recording head and realize stable ejection. In particular, from the viewpoint of solubility in the aqueous medium that constitutes the ink, it is common to use a surfactant that is highly hydrophilic, that is, one with a large HLB value.

[0014] The present inventors have investigated the reason why the ink fixing recovery of the ink is not obtained and the water abrasion resistance of the image is poor in the ink prepared with reference to the inks described in Patent Documents 1 and 2, and in the inkjet recording method described in Patent Document 3. As a result, it was found that the water abrasion resistance is reduced because the surfactant and the water-soluble organic solvent remain inside the recorded image. It is presumed that the water abrasion resistance is reduced because the liquid component remains inside the image, not only the strength of the image layer is reduced, but also the surfactant with high hydrophilicity is dissolved in the water attached to the image, and the water abrasion resistance is reduced. The same tendency was observed when resin particles that can improve the robustness by forming a resin film on the surface of the image were added to this ink and evaluated.

[0015] As a result of the study by the present inventors, it was found that some inks containing inorganic pigments tend to have improved adhesion recovery properties compared to inks containing organic pigments. This is thought to be because, as mentioned above, some inorganic pigments, such as inorganic oxides, have hydrophilic surfaces, and therefore tend to have high redispersibility even if they are fixed. On the other hand, it was also found that inorganic pigments with hydrophilic surfaces have good affinity with water, so that water abrasion resistance of the image cannot be obtained.

[0016] Therefore, the present inventors have re-examined the possibility of improving the adhesion recovery of ink and the water-resistant abrasion resistance of images by combining a surfactant and a water-soluble organic solvent, even when the inorganic pigment is hydrophilic. As a result, they have found that the adhesion recovery of ink and the water-resistant abrasion resistance of images can be improved by using a surfactant with a relatively low HLB value and a water-soluble organic solvent.

[0017] That is, the ink of the present invention has the following characteristics. First, the aqueous ink contains, in addition to titanium oxide particles and resin particles, a water-soluble organic solvent and a surfactant. The titanium oxide particles are titanium oxide having at least a portion of their surface covered with silica, and are dispersed at least by the action of the silica. The water-soluble organic solvent contains a first water-soluble organic solvent having a boiling point of 120°C or more and 230°C or less and an SP value of 11.0 or more and 13.5°C or less, and the ratio of the first water-soluble organic solvent is 0.70 or more. The SP value is a value calculated by the Fedors method, and although the unit may be omitted, it is generally expressed as "(cal / cm 3 ) 1 / 2 " The content of the water-soluble organic solvent is 5.00% by mass or more and 30.00% by mass or less, based on the total mass of the ink. The surfactant includes a first surfactant having an HLB value of 3 or more and 8 or less. The content (mass %) of the surfactant is 0.10% by mass or more and 0.40% by mass or less, based on the total mass of the ink. The inventors speculate that the mechanism by which the above configuration improves the adhesion recovery of the ink and the water abrasion resistance of the image is as follows.

[0018] The titanium oxide particles are titanium oxide particles at least partly coated with silica on the surface thereof, and are dispersed at least by the action of the silica. As described above, the titanium oxide particles have a hydrophilic surface due to the influence of the surface hydroxyl groups, and therefore have high redispersibility and excellent fixation recovery. In addition, the surface charge state of the titanium oxide particles, which are titanium oxide particles coated with silica, changes depending on the pH of the ink. In the pH range normally used for ink, the surface hydroxyl groups derived from silica are negatively charged. Therefore, even if the titanium oxide particles approach each other, aggregation can be suppressed by electrostatic repulsion, and they can be stably dispersed. The surfactant contains a first surfactant having an HLB value of 3 or more and 8 or less. The first surfactant is a compound with a relatively low HLB value, that is, a relatively high hydrophobicity. Therefore, when the liquid component in the ink dries and the image is fixed, it is considered that the surfactant and water are not easily mixed, and the surfactant is quickly oriented on the surface of the image. As a result, even if water adheres to the surface of the image, the surfactant is not easily dissolved, and therefore the water abrasion resistance is improved.

[0019] However, the first surfactant is difficult to mix with water. Therefore, the ink contains a first water-soluble organic solvent whose SP value is 11.0 or more and 13.5 or less. This allows the first surfactant to be stably dissolved or compatible in the ink. If the HLB value of the first surfactant is less than 3, the surfactant cannot be stably dissolved even in the presence of the first water-soluble organic solvent, and it is difficult to obtain a uniform image with reduced unevenness. Therefore, the strength of the image layer varies, and scraping or the like is likely to occur from the part with low strength, and water abrasion resistance is not obtained. In addition, if the HLB value of the first surfactant is more than 8, the hydrophilicity of the surfactant increases too much, which increases the solubility in water, leading to a decrease in the strength of the image layer. As a result, water abrasion resistance is not obtained.

[0020] As described above, if the surfactant added to obtain a uniform image remains inside the image, it is likely to reduce the strength of the image layer. By setting the content of the surfactant to a relatively small amount of 0.10% by mass or more and 0.40% by mass or less, the amount of surfactant remaining in the image layer can be reduced while maintaining the wettability of the ink to the recording medium, and the strength of the image layer can be improved. If the content of the surfactant is less than 0.10% by mass, the wettability of the ink to the recording medium cannot be obtained, and a uniform image cannot be obtained. As a result, water abrasion resistance cannot be obtained. If the content of the surfactant is more than 0.40% by mass, the amount of surfactant remaining in the image is too large, so the strength of the image layer is reduced and water abrasion resistance cannot be obtained.

[0021] The first water-soluble organic solvent has an SP value of 11.0 or more and 13.5 or less, and a boiling point of 120°C or more and 230°C or less. When the ink contains a water-soluble organic solvent having a boiling point in the above range, the ink is appropriately suppressed from evaporating, is less likely to stick, and even if sticking occurs in the recording head, the stuck matter can be dissolved when the ink comes into contact with newly supplied ink. If the boiling point of the first water-soluble organic solvent in the ink is less than 120°C, the ink is more likely to evaporate and sticking progresses near the ejection port of the recording head. As a result, the ink cannot recover from sticking. If the boiling point of the first water-soluble organic solvent in the ink is more than 230°C, the ink is less likely to evaporate and more water-soluble organic solvent remains in the image. As a result, the strength of the image layer is reduced, and water abrasion resistance is not obtained.

[0022] Moreover, the ratio (mass%) of the first water-soluble organic solvent in the water-soluble organic solvent is 0.70 times or more. By making the water-soluble organic solvent composition as described above, the effect of appropriately suppressing the evaporation of the ink is fully exhibited. As a result, the ink adhesion recovery is improved. If the ratio is less than 0.70 times and the boiling point of the water-soluble organic solvent other than the first water-soluble organic solvent is less than 120°C, the ink evaporation is not suppressed by the high boiling point of the first water-soluble organic solvent. As a result, the ink adhesion recovery is not obtained because the ink adhesion progresses near the ejection port of the recording head. On the other hand, if the ratio is less than 0.70 times and the boiling point of the water-soluble organic solvent other than the first water-soluble organic solvent is more than 230°C, the ink evaporation is difficult to progress, and the water-soluble organic solvent remaining in the image layer increases. As a result, the strength of the image layer is reduced and water abrasion resistance is not obtained.

[0023] The content of the water-soluble organic solvent including the first water-soluble organic solvent in the ink is 5.00% by mass or more and 30.00% by mass or less based on the total mass of the ink. By setting the content of the water-soluble organic solvent in the above range, the amount of the water-soluble organic solvent remaining in the image is reduced, and the adhesion near the ejection port of the recording head can be suppressed. If the content of the water-soluble organic solvent is less than 5.00% by mass, the high boiling point of the first water-soluble organic solvent does not suppress the evaporation of the ink, and the adhesion progresses near the ejection port of the recording head. As a result, the adhesion recovery of the ink cannot be obtained. In addition, the amount of the water-soluble organic solvent is too small, and the first surfactant, which is difficult to mix with water, cannot be stably dissolved or mixed in the ink, and as a result, water abrasion resistance cannot be obtained. If the content of the water-soluble organic solvent is more than 30.00% by mass, the amount of the water-soluble organic solvent remaining inside the image becomes too large, the strength of the image layer decreases, and water abrasion resistance cannot be obtained.

[0024] <Water-based ink> The ink of the present invention is a water-based ink for inkjet use, which contains titanium oxide particles, resin particles, a specific water-soluble organic solvent, and a specific surfactant. The components constituting the ink of the present invention and the physical properties of the ink will be described in detail below.

[0025] (Colorant) The ink contains titanium oxide particles that have been surface-treated with silica as a coloring material (pigment). That is, the ink contains titanium oxide particles that are titanium oxide with at least a portion of their surface covered with silica. The content (mass%) of titanium oxide particles in the ink is preferably 0.10% by mass or more and 20.00% by mass or less based on the total mass of the ink. In particular, it is more preferably 1.00% by mass or more and 20.00% by mass or less, and particularly preferably 1.00% by mass or more and 15.00% by mass or less.

[0026] Titanium oxide is a white pigment, and has three crystal forms: rutile, anatase, and brookite. Among them, rutile titanium oxide is preferred. Titanium oxide can be industrially produced by the sulfuric acid method and the chlorine method, and the titanium oxide used in the present invention may be produced by either method.

[0027] The volume-based cumulative 50% particle diameter (hereinafter also referred to as the average particle diameter) of the titanium oxide particles is preferably 200 nm or more and 500 nm or less. In particular, the volume-based cumulative 50% particle diameter of the titanium oxide particles is more preferably 200 nm or more and 400 nm or less. The volume-based cumulative 50% particle diameter of the titanium oxide particles (D 50 ) is the diameter of the particle that is 50% of the total volume of the measured particles in the particle size accumulation curve, calculated from the small particle size side. 50 can be measured under the following conditions: SetZero: 30 seconds, number of measurements: 3, measurement time: 180 seconds, shape: aspheric, refractive index: 2.60. A particle size analyzer using a dynamic light scattering method can be used as the particle size distribution measuring device. Of course, the measurement conditions are not limited to those described above.

[0028] Titanium oxide that has been surface-treated with silica is used. In particular, titanium oxide that has been surface-treated with alumina and silica is preferably used. The surface treatment is expected to suppress photocatalytic activity and improve dispersibility. In this specification, "alumina" is a general term for oxides of aluminum such as aluminum oxide. In this specification, "silica" is a general term for silicon dioxide or a substance composed of silicon dioxide. Most of the alumina and silica that coat titanium oxide are present in the form of silicon dioxide and aluminum oxide.

[0029] The proportion (mass%) of titanium oxide in the titanium oxide particles is preferably 90.00 mass% or more based on the total mass of the titanium oxide particles, and the proportion (mass%) of titanium oxide in the titanium oxide particles is preferably 98.50 mass% or less based on the total mass of the titanium oxide particles.

[0030] The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.50 to 1.00 times the ratio (mass%) of silica in terms of mass ratio. The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.50 to 4.00 mass% based on the total mass of the titanium oxide particles. In particular, the ratio (mass%) of alumina in the titanium oxide particles is more preferably 1.00 to 4.00 mass% based on the total mass of the titanium oxide particles. The ratio (mass%) of silica in the titanium oxide particles is preferably 1.00 to 4.00 mass% based on the total mass of the titanium oxide particles. By setting the ratio of silica in the above range, not only can electrostatic repulsion of negative charges due to surface hydroxyl groups derived from silica be obtained, but also when a silane compound described later is used, the reactivity with the silane compound is appropriately adjusted, and the aggregation of the titanium oxide particles can be suppressed. As a result, the fixation recovery property of the ink can be further improved.

[0031] The ratio of alumina and silica in titanium oxide particles, i.e., the amount of alumina and silica coating, can be measured by, for example, quantitative analysis of aluminum and silicon elements by inductively coupled plasma (ICP) emission spectrometry. In this case, it is assumed that all atoms coated on the surface are oxides, and the obtained values ​​of aluminum and silicon can be calculated by converting them to their oxides, i.e., alumina and silica. The ratio (mass%) of aluminum element in titanium oxide particles obtained by inductively coupled plasma emission spectrometry is preferably 0.57 times or more and 1.13 times or less in mass ratio to the ratio (mass%) of silicon element. When this value is converted to its oxides, i.e., alumina and silica, the ratio (mass%) of alumina in titanium oxide particles is 0.50 times or more and 1.00 times or less in mass ratio to the ratio (mass%) of silica.

[0032] Surface treatment methods for titanium oxide include wet treatment and dry treatment. For example, titanium oxide can be dispersed in a liquid medium, and then reacted with a surface treatment agent such as sodium aluminate or sodium silicate to perform surface treatment. The ratio of these surface treatment agents can be appropriately changed to adjust the properties to the desired level. In addition to silica, inorganic oxides such as alumina, zinc oxide, and zirconia, and organic substances such as polyols can be used for surface treatment, as long as the effects of the present invention are not impaired.

[0033] As long as the effect of the present invention is not impaired, the ink may contain other pigments besides titanium oxide. In this case, the ink may be of a color other than white ink. The content (mass %) of the other pigments in the ink is preferably 0.10 mass % or more and 5.00 mass % or less, and more preferably 0.10 mass % or more and 1.00 mass % or less, based on the total mass of the ink.

[0034] (Resin particles) The ink contains resin particles. The resin particles are a component that can be fixed on a recording medium to form a film, increase the adhesion between the recording medium and the image, and impart physical strength such as abrasion resistance to the image. The resin particles do not need to contain a coloring material. The content (mass%) of the resin particles in the ink is preferably 0.10% by mass or more and 15.00% by mass or less, based on the total mass of the ink, and more preferably 1.00% by mass or more and 10.00% by mass or less. The content (mass%) of the resin particles in the ink is preferably 0.50 times or more, more preferably 1.50 times or more, and particularly preferably 1.70 times or more, in terms of mass ratio to the content (mass%) of the pigment. Also, it is preferably 10.00 times or less. The resin particles are present in the ink in a dispersed state, that is, in the form of a resin emulsion.

[0035] In this specification, the term "resin particles" refers to a resin that does not dissolve in the aqueous medium constituting the ink, specifically, a resin that can exist in the aqueous medium in a state in which particles whose particle diameter can be measured by dynamic light scattering are formed. On the other hand, the term "water-soluble resin" refers to a resin that can dissolve in the aqueous medium constituting the ink, specifically, a resin that can exist in the aqueous medium in a state in which particles whose particle diameter can be measured by dynamic light scattering are not formed. The term "resin particles" can also be referred to as "water-dispersible resin (water-insoluble resin)". The determination of whether a resin is a water-soluble resin or a resin particle using dynamic light scattering will be described in detail below.

[0036] The constituent units of the resin constituting the resin particles can be appropriately selected from the same as the units constituting the water-soluble resin described later. In particular, the resin constituting the resin particles is preferably an acrylic resin. The acid value of the resin constituting the resin particles is preferably 5 mgKOH / g or more and 100 mgKOH / g or less. The weight average molecular weight of the resin constituting the resin particles is preferably 1,000 or more and 3,000,000 or less, and more preferably 100,000 or more and 3,000,000 or less. The volume-based cumulative 50% particle diameter (D 50) is preferably 50 nm or more and 500 nm or less. The volume-based cumulative 50% particle diameter of the resin particles is the diameter of the particle that is 50% of the total volume of the measured particles when integrated from the small particle diameter side in a particle diameter integration curve. The volume-based cumulative 50% particle diameter of the resin particles can be measured under the same measurement conditions using a particle size analyzer by the dynamic light scattering method described later. In addition, whether or not a certain resin is a resin particle can be determined by whether or not the particle diameter is measured when measured under the same measurement conditions using a particle size analyzer by the dynamic light scattering method.

[0037] (Water-soluble resin) The ink may further contain a water-soluble resin. However, the water-soluble resin may hinder the dispersion caused by the action of the silica. Therefore, as described above, when a water-soluble resin is added to the ink, it is preferable to keep its content small.

[0038] Examples of the water-soluble resin include acrylic resins, urethane resins, olefin resins, etc. Among them, acrylic resins and urethane resins are preferred, and acrylic resins composed of units derived from (meth)acrylic acid or (meth)acrylate are more preferred.

[0039] The form of the water-soluble resin may be a block copolymer, a random copolymer, a graft copolymer, or a combination thereof. Among them, a block copolymer is preferred, and a copolymer having a hydrophobic block composed of units having no acid groups, i.e., hydrophobic units, is preferred. In particular, the water-soluble resin is more preferably a copolymer including an A block having no acid groups and a B block having an acid group. The A block is a hydrophobic block composed of units having no acid groups. If the B block includes a unit having an acid group, it may further include a unit having no acid groups, i.e., a hydrophilic unit. In addition, when the B block is formed of a plurality of units, it is preferred to be a random copolymer. By having a hydrophobic block in which units having no acid groups are polymerized continuously, as in the above-mentioned A block, it is easier to interact with resin particles compared to a random portion in which a plurality of types of monomers are polymerized discontinuously. Therefore, it is considered that the movement of the particulate components of the ink can be more effectively suppressed, and the color development of the image can be improved.

[0040] The acrylic resin preferably has a hydrophilic unit and a hydrophobic unit as constituent units. Among them, a water-soluble resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of a monomer having an aromatic ring and a (meth)acrylic acid ester monomer is preferred. In particular, a water-soluble resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of styrene and α-methylstyrene is preferred.

[0041] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group. The hydrophilic unit can be formed, for example, by polymerizing a hydrophilic monomer having a hydrophilic group. Specific examples of the hydrophilic monomer having a hydrophilic group include acidic monomers having a carboxylic acid group such as (meth)acrylic acid, itaconic acid, maleic acid, and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. Examples of cations constituting the salts of acidic monomers include ions of lithium, sodium, potassium, ammonium, and organic ammonium.

[0042] The hydrophobic unit is a unit that does not have a hydrophilic group such as an anionic group. The hydrophobic unit can be formed, for example, by polymerizing a hydrophobic monomer that does not have a hydrophilic group such as an anionic group. Specific examples of the hydrophobic monomer include monomers having an aromatic ring such as styrene, α-methylstyrene, and benzyl (meth)acrylate; and (meth)acrylic acid ester monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0043] The urethane resin can be obtained by reacting, for example, polyisocyanate with a polyol. In addition, a chain extender may be further reacted with the urethane resin. Examples of the olefin resin include polyethylene and polypropylene.

[0044] In this specification, "a resin is water-soluble" means that when the resin is neutralized with an alkali equivalent to the acid value, the resin is present in an aqueous medium in a state in which it does not form particles whose particle size can be measured by a dynamic light scattering method. Whether or not a resin is water-soluble can be determined according to the following method. First, a liquid (resin solid content: 10 mass%) containing a resin neutralized with an alkali (sodium hydroxide, potassium hydroxide, etc.) equivalent to the acid value is prepared. Next, the prepared liquid is diluted 10 times (volume basis) with pure water to prepare a sample solution. Then, when the particle size of the resin in the sample solution is measured by a dynamic light scattering method, if no particles having a particle size are measured, the resin can be determined to be water-soluble. The measurement conditions at this time can be, for example, SetZero: 30 seconds, number of measurements: 3 times, and measurement time: 180 seconds. In addition, a particle size analyzer using a dynamic light scattering method (for example, the product name "UPA-EX150", manufactured by Nikkiso) can be used as a particle size distribution measuring device. Of course, the particle size distribution measuring device and the measurement conditions are not limited to those described above.

[0045] The acid value of the water-soluble resin is preferably 100 mgKOH / g or more and 250 mgKOH / g or less, and the weight average molecular weight of the water-soluble resin is preferably 3,000 or more and 15,000 or less.

[0046] (Surfactant) The ink contains a surfactant including a first surfactant having an HLB value of 3 or more and 8 or less. The surfactant contained in the ink of the present invention is a substance composed of a hydrophobic portion (hydrocarbon chain, perfluoroalkyl group, siloxane structure, etc.) and a hydrophilic portion (ethylene oxide group, etc.). In particular, the HLB value of the first surfactant is more preferably 3 or more and 6 or less. The "HLB value" of the surfactant in this specification is a value determined by the Griffin method, and is calculated based on the formula HLB value = 20 x (formula weight of hydrophilic group of surfactant) / (molecular weight of surfactant). The HLB value determined by the Griffin method is a physical property value that indicates the degree of hydrophilicity or lipophilicity of the surfactant, and takes a value of 0 to 20. The smaller the HLB value, the higher the lipophilicity, and the larger the HLB value, the higher the hydrophilicity. The HLB value of the surfactant is preferably 4 or more.

[0047] The content (mass %) of the surfactant in the ink must be 0.10% by mass or more and 0.40% by mass or less based on the total mass of the ink. The content (mass %) of the surfactant in the ink is preferably 0.10% by mass or more and 0.30% by mass or less based on the total mass of the ink. Of these, the content (mass %) of the surfactant in the ink is particularly preferably 0.20% by mass or more and 0.30% by mass or less based on the total mass of the ink.

[0048] The content (mass%) of the first surfactant is preferably 0.05% by mass or more and 0.50% by mass or less, and more preferably 0.10% by mass or more and 0.40% by mass or less. The ratio (mass%) of the first surfactant in the surfactant is preferably 0.50 times or more. If the ratio is less than 0.50 times, the first surfactant that is easily oriented on the image surface may be insufficient, and water abrasion resistance may not be sufficiently obtained. The first surfactant is not particularly limited as long as it is within the above HLB value range, but from the viewpoint of compatibility with water-soluble organic solvents and suppression of adsorption to pigments, an acetylene glycol-based nonionic surfactant is preferable. The acetylene glycol-based surfactant is a general term for a symmetrical compound having an acetylene group in the center of the structure, and is, for example, a compound represented by the following formula (1). That is, examples include ethylene oxide adducts of acetylene glycol. By using the above surfactant, a more uniform image is obtained and water abrasion resistance is further improved.

[0049] [ka] (In formula (1), m and n each independently represent an integer of 0 or more.)

[0050] The ink can contain one or more types of surfactants. As the first surfactant, two or more types of surfactants can be used. Examples of surfactants that can be used in combination with the first surfactant include anionic surfactants, cationic surfactants, and other nonionic surfactants. Among these, nonionic surfactants that have low affinity with colorants and are effective in small amounts are preferred.

[0051] From the viewpoint of solubility, the SP value of the surfactant is preferably 11.0 or more and 13.5 or less. In this specification, the SP value (δ) is a value calculated by the Fedors method based on the following formula. Although units are omitted in this specification, the unit of the SP value (δ) is ((cal / cm 3 ) 1 / 2 ). δ = (ΔE vap / V)1 / 2 (In the formula, ΔE vap represents the molar heat of vaporization (cal / mol), and V represents the molar volume at 25°C (cc / mol).

[0052] (Water-soluble organic solvent) The ink contains a water-soluble organic solvent including a first water-soluble organic solvent having a boiling point of 120° C. or more and 230° C. or less and an SP value of 11.0 or more and 13.5 or less. The ratio (mass%) of the first water-soluble organic solvent in the water-soluble organic solvent is 0.70 times or more. In particular, the ratio (mass%) of the first water-soluble organic solvent in the water-soluble organic solvent is preferably 0.90 times or more. By setting the ratio within the above range, most of the water-soluble organic solvent is the first water-soluble organic solvent whose evaporation is appropriately suppressed, and the water-soluble organic solvent remaining in the image is effectively suppressed, and the strength of the image film can be improved. As a result, the water abrasion resistance can be further improved. The ratio (mass%) of the first water-soluble organic solvent in the water-soluble organic solvent is more preferably 0.95 times or more. Furthermore, the ratio (mass%) of the first water-soluble organic solvent in the water-soluble organic solvent may be 1.00 times. In other words, all of the water-soluble organic solvent may be the first water-soluble organic solvent.

[0053] The content (mass%) of the water-soluble organic solvent must be 5.00% by mass or more and 30.00% by mass or less based on the total mass of the ink. The content (mass%) of the water-soluble organic solvent including the first water-soluble organic solvent is preferably 5.00% by mass or more and 20.00% by mass or less, more preferably 10.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. The content (mass%) of the first water-soluble organic solvent is preferably 3.50% by mass or more and 30.0% by mass or less, more preferably 7.00% by mass or more and 20.00% by mass or less.

[0054] The first water-soluble organic solvent has a boiling point of 120°C or more and 230°C or less, and an SP value of 11.0 or more and 13.5 or less. Examples of such water-soluble organic solvents include propylene glycol (188°C, 13.5), 1,2-butanediol (193°C, 12.8), 1,2-pentanediol (230°C, 12.2), 1,2-hexanediol (224°C, 11.8), diethylene glycol monomethyl ether (194°C, 11.2), propylene glycol (188°C, 13.5), and 1,3-dimethyl-2-imidazolidinone (222°C, 11.4). Here, the numbers in parentheses are the boiling points and SP values ​​of each water-soluble organic solvent at 1 atmosphere. The boiling points of major water-soluble organic solvents were referenced to the values ​​listed in Chemical Handbook Basics I, 5th Revised Edition, 2004, edited by the Chemical Society of Japan. As the first water-soluble organic solvent, one or more kinds can be used. The boiling point of the first water-soluble organic solvent is preferably 120°C or more and 210°C or less.

[0055] From the viewpoint of volatility, the first water-soluble organic solvent preferably contains an alkanediol. Among them, an alkanediol that is liquid at 25°C is preferable, 1,2-alkanediol is more preferable, and 1,2-butanediol and 1,2-hexanediol are particularly preferable. All of the water-soluble organic solvents in the ink may be alkanediols. It is preferable not to use lactams.

[0056] The ink may contain other water-soluble organic solvents other than the first water-soluble organic solvent, as long as the effect of the present invention is not impaired. There is no particular limitation on the other water-soluble organic solvents as long as they are water-soluble (preferably, soluble in water at any ratio at 25°C). Specifically, monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds, sulfur-containing polar compounds, etc. can be used.

[0057] Usually, "water-soluble organic solvent" means a liquid, but in the present invention, compounds that are solid at 25°C (room temperature) are also included in water-soluble organic solvents. Examples of water-soluble organic solvents that are generally used in water-based inks and are solid at 25°C include 1,6-hexanediol, trimethylolpropane, ethylene urea, urea, and polyethylene glycol with a number average molecular weight of 1,000. Water-soluble organic solvents do not include "surfactants."

[0058] (Compound represented by general formula (2)) As described above, titanium oxide has a surface hydroxy group, which is a hydrophilic group. However, titanium oxide, which is a metal oxide, has a larger specific gravity than other pigments commonly used in aqueous inks for inkjet printing. Therefore, in order to efficiently stabilize the dispersion state, the ink may contain a component that assists dispersion, for example, a compound represented by the following general formula (2). Some of the compounds represented by general formula (2) are known as silane coupling agents. The content (mass%) of the compound represented by general formula (2) in the ink is preferably 0.01 mass% or more and 1.00 mass% or less, and more preferably 0.02 mass% or more and 0.50 mass% or less, based on the total mass of the ink. In addition, the content (mass%) of the compound represented by general formula (2) in the ink is preferably 0.002 times or more and 0.10 times or less in terms of mass ratio to the content (mass%) of titanium oxide particles.

[0059] A part of OR1 bonded to silicon atoms in the compound represented by general formula (2) is hydrolyzed in an aqueous medium to form a silanol group. Therefore, it has affinity with the surface hydroxyl groups derived from silica on the titanium oxide particle surface. In addition to the structure capable of forming a silanol group as described above, the compound represented by general formula (2) also has a structure having n alkylene oxide groups having 2 to 4 carbon atoms as repeating units ((OR4) in general formula (2)) via X, which serves as a linking group. n) below. Hereinafter, the above structure is also referred to as an alkylene oxide chain. Since the alkylene oxide chain is hydrophilic, it extends appropriately in an aqueous medium and exhibits a repulsive force due to steric hindrance. Therefore, the compound represented by general formula (2) has the effect of assisting the dispersion of titanium oxide particles. As a result of the inventors' investigation, it was found that the fixation recovery property of the ink is further improved by adding the compound represented by general formula (2) to the ink.

[0060] [ka] (In the general formula (2), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Each R4 is independently an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)

[0061] In the general formula (2), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, and an n-butyl group. Among these, a methyl group is preferable from the viewpoint of ease of hydrolysis. a representing the number of R1O is 1 to 3, and b representing the number of R2 is 0 to 2, and a+b=3. Among these, it is preferable that a is 3 and b is 0, that is, all three substituents of the silicon atom are R1O.

[0062] In the general formula (2), R4 is independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include an ethylene group, an n-propylene group, an i-propylene group, and an n-butylene group. Among them, an ethylene group is preferable. The number of OR4, that is, n (average value) representing the number of alkylene oxide groups, is 6 to 24.

[0063] In the general formula (2), X is a single bond or an alkylene group having 1 to 6 carbon atoms. When X is a single bond, it means that the silicon atom and OR4 are directly bonded. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an i-propylene group, an n-butylene group, an n-pentylene group, and an n-hexylene group. Among them, an n-propylene group is preferable.

[0064] (aqueous medium) The ink is an aqueous ink containing water as an aqueous medium. The ink contains an aqueous medium that is a mixed solvent of water and a water-soluble organic solvent containing a first water-soluble organic solvent. As the water, deionized water (ion-exchanged water) is preferably used. The content (mass %) of water in the ink is preferably 50.00 mass % or more and 95.00 mass % or less based on the total mass of the ink. As the water-soluble organic solvent, the above-mentioned ones can be used.

[0065] (Other additives) In addition to the additives described above, the ink may contain various additives, such as other surfactants, pH adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters, and chelating agents, as necessary.

[0066] (Ink properties) Since the ink is applied to the inkjet method, it is preferable to appropriately control the physical properties of the ink. The surface tension of the ink at 25°C is preferably 10 mN / m or more and 60 mN / m or less, and more preferably 20 mN / m or more and 40 mN / m or less. The surface tension of the ink can be adjusted by appropriately determining the type and content of the surfactant in the ink. In addition, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.0 or less. The pH of the ink can be measured with a general pH meter equipped with a glass electrode or the like.

[0067] <Ink cartridges> The ink cartridge of the present invention includes ink and an ink storage section that stores the ink. The ink stored in the ink storage section is the water-based ink of the present invention described above. FIG. 1 is a cross-sectional view that shows a schematic diagram of an embodiment of the ink cartridge of the present invention. As shown in FIG. 1, an ink supply port 12 for supplying ink to a recording head is provided on the bottom surface of the ink cartridge. The inside of the ink cartridge is an ink storage section for storing ink. The ink storage section is composed of an ink storage chamber 14 and an absorber storage chamber 16, which are communicated with each other via a communication port 18. The absorber storage chamber 16 is also communicated with the ink supply port 12. The ink storage chamber 14 stores liquid ink 20, and the absorber storage chamber 16 stores absorbers 22 and 24 that hold the ink in an impregnated state. The ink storage section may not have an ink storage chamber that stores liquid ink, and may be in a form in which the entire amount of ink stored is held by the absorber. The ink storage section may also be in a form in which the entire amount of ink stored is stored in a liquid state, without having an absorber. Furthermore, the ink cartridge may be configured to have an ink container and a recording head.

[0068] <Inkjet recording method> The inkjet recording method of the present invention is a method of ejecting the above-described aqueous ink of the present invention from an inkjet recording head to record an image on a recording medium. Methods for ejecting the ink include a method of imparting mechanical energy to the ink and a method of imparting thermal energy to the ink. In the present invention, it is particularly preferable to adopt a method of ejecting the ink by imparting thermal energy to the ink. Other than using the ink of the present invention, the steps of the inkjet recording method may be known.

[0069] FIG. 2 is a diagram showing an example of an inkjet recording device used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording device, and (b) is a perspective view of a head cartridge. The inkjet recording device is provided with a conveying means (not shown) for conveying a recording medium 32, and a carriage shaft 34. A head cartridge 36 can be mounted on the carriage shaft 34. The head cartridge 36 includes recording heads 38 and 40, and is configured so that an ink cartridge 42 is set thereon. While the head cartridge 36 is conveyed in the main scanning direction along the carriage shaft 34, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, an image is recorded on the recording medium 32 by conveying the recording medium 32 in the sub-scanning direction by a conveying means (not shown).

[0070] (Recording medium) In the inkjet recording method of the present invention, it is preferable to use a non-absorbent recording medium (a low to non-absorbent recording medium). The low to non-absorbent recording medium is a recording medium that is capable of being held in contact with the ink for 30 msec in the Bristow method described in JAPAN TAPPI Paper and Pulp Test Method No. 51 "Liquid Absorbency Test Method for Paper and Paperboard". 1 / 2 Water absorption up to 0mL / m 2 More than 10mL / m 2 In the present invention, a recording medium that satisfies the above-mentioned condition of water absorption amount is defined as a "low to non-absorbent recording medium". A recording medium for inkjet recording having a coating layer (ink receiving layer) formed of inorganic particles (glossy paper, matte paper, etc.) and plain paper having no coating layer have a water absorption amount of 10 mL / m 2 It is an "absorbent recording medium" that exceeds this.

[0071] Examples of low to non-absorbent recording media that can be used include plastic films, recording media in which a plastic film is bonded to the recording surface of a substrate, and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp. Among these, plastic films are preferred, and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp are also preferred. EXAMPLES

[0072] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples without departing from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified.

[0073] <Preparation of titanium oxide particles> Commercially available titanium oxide particles that had been surface-treated in advance and titanium oxide particles prepared by surface-treating untreated titanium oxide were used. The cumulative 50% particle diameter (D 50 ) was measured using a particle size analyzer using dynamic light scattering (trade name "Nanotrac WaveII-EX150", manufactured by Microtrack Bell). The properties of titanium dioxide particles are shown in Table 1. In Table 1, TITANIX: JR and JR-403 are the trade names of rutile-type titanium dioxide manufactured by Teika.

[0074] (Measurement of the amount of alumina and silica coating) The ratio of alumina and silica in the titanium oxide particles, i.e., the amount of alumina and silica coating, was measured as follows. The prepared titanium oxide particles were added to nitric acid to prepare a liquid, and quantitative analysis of aluminum and silicon elements was performed using an inductively coupled plasma (ICP) emission spectrometer. In this case, it was assumed that all atoms coating the surface were in the form of oxides, and the obtained values ​​of aluminum and silicon were converted to the oxides, i.e., alumina and silica, to calculate the mass ratio.

[0075] (Titanium oxide particles 1, 3) Titanium oxide particles were produced by surface treatment of the titanium oxide using a wet method. Surface treatment using the wet method involves contacting untreated titanium oxide with a surface treatment agent (sodium aluminate, sodium silicate, etc.), and the amount and ratio of the surface treatment agent used were appropriately adjusted to provide a surface treatment at any ratio.

[0076] Specifically, 300 parts of rutile-type titanium oxide (trade name "TITANIX JR", manufactured by Teika Co., Ltd.) that had not been subjected to surface treatment and 700 parts of pure water were mixed with a homogenizer. Then, the temperature was raised to 90°C while stirring, and potassium hydroxide (pH adjuster) was added to adjust the pH to 10.5. Next, sodium silicate was added, and dilute sulfuric acid (pH adjuster) was added over about 1 hour to adjust the pH to 5.0. The reaction was continued for about 1 hour. Thereafter, sodium aluminate was added little by little at 90°C. At this time, in order to maintain the pH, dilute sulfuric acid was used in combination to maintain the pH at 6.0 to 8.0. After the addition of sodium aluminate, the reaction was continued for about 1 hour to obtain a dispersion. The dispersion was cooled to 25°C, and then purified by repeatedly sedimenting with a centrifuge and redispersing in ion-exchanged water, and dried at 120°C to obtain titanium oxide particles that had been subjected to surface treatment with at least one of alumina and silica. Table 1 shows the characteristics of each titanium oxide particle.

[0077] (Titanium oxide particles 2, 4) Commercially available titanium oxide particles were used as titanium oxide particles 2 and 4, respectively. Table 1 shows the properties of titanium oxide particles 2 and 4. In addition to alumina and silica, titanium oxide particles 2 contained inorganic oxides such as zirconia and zinc oxide, and organic compounds such as polyols, but the proportion of these was at most about 1.00%. Therefore, for convenience, these were included in the proportion T (%) of titanium oxide in the titanium oxide particles ("Titanium oxide T (%)" in Table 1).

[0078] [Table 1]

[0079] <Preparation of compound represented by general formula (2)> The compound represented by general formula (2) was synthesized by the following procedure. The synthesis conditions and structures of the compound synthesized as the compound represented by general formula (2) are shown in Tables 2 and 3, respectively. The compound represented by general formula (2) can be synthesized by allylation and hydrosilylation of a raw material (such as a polyalkylene glycol monoalkyl ether).

[0080] The raw materials, base, and solvent shown in Table 2 were placed in a three-neck flask equipped with a stirrer and a nitrogen inlet tube, and stirred at 25°C for 30 minutes. As the "sodium hydride", a paraffin dispersion of 60% sodium hydride was used, and the dispersion was used so that the amount of sodium hydride used was as shown in Table 2. Then, the bromide shown in Table 2 was added dropwise while stirring at 25°C, and stirring was continued for 12 hours after the end of the dropwise addition to obtain a solution containing the reactants. After filtering out the unreacted sodium hydride and neutralized product (sodium bromide) from the solution containing the reactants, THF was removed under reduced pressure to obtain a concentrate. The concentrate was dissolved in 500 parts of pure water, and this aqueous solution was extracted three times with 200 mL of hexane, and then extracted with 200 mL of dichloromethane. The solvent containing the product was dried by adding magnesium sulfate, and concentrated under reduced pressure to obtain each of the allylated compounds (allylation process).

[0081] The allylated raw materials and silane compounds shown in Table 2 were placed in a dry, passivated round-bottom flask equipped with a stirrer and an argon inlet tube, and stirred at 85°C. Then, 0.54 parts of an aqueous solution of 65 mmol / L chloroplatinic acid monohydrate in isopropyl alcohol was added, and the mixture was heated at 85°C for 5 hours. After the reaction was completed, the mixture was allowed to cool to 25°C, and the excess silane compounds were removed under reduced pressure. The residue was purified by column chromatography using silica gel passivated with triethoxysilane as a carrier to obtain each compound (hydrosilylation step). The eluent used for purification by column chromatography was ethyl acetate / hexane / ethanol = 85 / 15 / 5 (by volume).

[0082] [Table 2]

[0083] [Table 3]

[0084] <Preparation of pigment dispersion> The pigment dispersion was prepared according to the following procedure. The preparation conditions for the pigment dispersion are shown in Table 4.

[0085] (Pigment Dispersion 1-8) 40.00 parts of titanium oxide particles, a dispersant, a neutralizer, and ion-exchanged water with a total of 100.00 parts of the components shown in Table 4 were mixed, and preliminary dispersion was performed using a homogenizer. Then, dispersion treatment (main dispersion) was performed for 12 hours at 25°C using a paint shaker using 0.5 mm zirconia beads. When a neutralizer was used, potassium hydroxide was used. The amount used was appropriately adjusted so that the pH of the main dispersion was 10.5. The pH of the main dispersion was measured using a pH meter (trade name "Portable pH Meter D-74", manufactured by Horiba, Ltd.) at the time of starting the main dispersion. The zirconia beads were filtered out, and an appropriate amount of ion-exchanged water was added as necessary to prepare each pigment dispersion containing 40.00% titanium oxide particles. In Table 4, the aqueous solution of resin 1 was the same as that used in the preparation of pigment dispersion 9, and details will be described later.

[0086] (Pigment Dispersion 9) A styrene-ethyl acrylate-acrylic acid copolymer (resin 1) with an acid value of 150 mgKOH / g and a weight average molecular weight of 8,000 was prepared. 20.00 parts of resin 1 were neutralized with potassium hydroxide in an amount equimolar to the acid value, and an appropriate amount of pure water was added to prepare an aqueous solution of resin 1 with a resin (solid content) content of 20.00%. A mixture was obtained by mixing 20.00 parts of a pigment (CI Pigment Blue 15:3), 30.00 parts of the aqueous solution of resin 1, and 50.00 parts of pure water. The obtained mixture and 200 parts of zirconia beads with a diameter of 0.3 mm were placed in a batch-type vertical sand mill (manufactured by Imex) and dispersed for 5 hours while cooling with water. After centrifuging to remove coarse particles, the mixture was filtered under pressure using a cellulose acetate filter (Advantec) with a pore size of 3.0 μm to prepare Pigment Dispersion 9 with a pigment content of 20.00% and a resin dispersant (Resin 1) content of 6.00%.

[0087] (Pigment Dispersion 10, 11) Pigment dispersions 10 and 11 were prepared with a pigment content of 20.00% and a resin dispersant (resin 1) content of 6.00% in the same manner as in the preparation of pigment dispersion 9, except that the pigment (CI Pigment Blue 15:3) was changed to CI Pigment Red 122 and CI Pigment Yellow 74, respectively.

[0088] (Pigment Dispersion 12) A commercially available pigment dispersion (product name "Cab-O-Jet 400", manufactured by Cabot) was used as the pigment dispersion 12. The pigment dispersion 12 is a dispersion in water of a self-dispersing pigment in which an atomic group containing an anionic group is bonded to the surface of a pigment (carbon black) particle, and the pigment content is 15.00%.

[0089] [Table 4]

[0090] <Synthesis of resin particles> In a four-neck flask equipped with a stirrer, a reflux condenser, and a nitrogen gas inlet tube, 0.2 parts of potassium persulfate and 74.0 parts of ion-exchanged water were placed, and nitrogen gas was introduced. The monomers shown in Table 6 and 0.3 parts of an emulsifier (trade name "NIKKOL BC15", manufactured by Nikko Chemicals) were mixed to obtain a mixture. The obtained mixture was dropped into the four-neck flask over 1 hour under stirring, and then reacted at a temperature of 80 ° C. for 2 hours. After that, the contents were cooled to 25 ° C., and a neutralizing agent in an amount equimolar to the acid value of the resin and an appropriate amount of ion-exchanged water were added to prepare an aqueous dispersion of each resin particle having a resin particle content of 40.00% and a cumulative 50% particle size based on volume of 100 nm. The acid value of the resin particles is shown in Table 5. Details of each component in Table 5 are shown below. ·BMA: Butyl methacrylate ·MAA: Methacrylic acid

[0091] [Table 5]

[0092] <Ink Preparation> (Preparation of surfactant) The properties of the surfactants used in preparing the ink are shown in Table 6. In Table 6, surfactant 3, oxyethylene behenyl ether, was synthesized by forming an ether bond between behenyl alcohol and ethylene oxide by a conventional method.

[0093] [Table 6]

[0094] (Preparation of water-soluble organic solvent) The properties of the water-soluble organic solvents used in preparing the inks are shown in Table 7. In Table 7, whether or not the solvent was the first water-soluble organic solvent is indicated by ○ or ×.

[0095] [Table 7]

[0096] (Ink Preparation) The components of the types and amounts shown in the upper rows of Tables 8 to 11 were mixed and stirred. Proxel GXL(S) (trade name) is a preservative manufactured by LONZA. Then, pressure filtration was performed using a membrane filter (manufactured by Sartorius) with a pore size of 5.0 μm to prepare each ink. The properties of each ink prepared are shown in the lower rows of Tables 8 to 11. In Tables 8 to 11, the ratio of the first water-soluble organic solvent to the water-soluble organic solvent is shown in the column "Ratio (times) of the first water-soluble organic solvent". Also, the ratio of the first surfactant to the surfactant is shown in the column "Ratio (times) of the first surfactant". In the case of ink prepared from a pigment dispersion using titanium oxide particles at least a part of whose surface is at least partially covered with silica, "○" is shown in the column "Contribution of silica to dispersion of titanium oxide particles". However, when the ink contains a water-soluble resin at a mass ratio of 0.01 times or more to the content of titanium oxide particles, it is considered that the dispersion due to the action of silica is destabilized. Therefore, in the case of the ink described above, the column "Contribution of silica to dispersion of titanium oxide particles" was marked "X."

[0097] [Table 8]

[0098] [Table 9]

[0099] [Table 10]

[0100] [Table 11]

[0101] <Evaluation> The inks obtained above were evaluated for the following items. In the present invention, for each of the evaluation criteria for the following items, "AA", "A" and "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown in Table 12.

[0102] Each ink obtained above was filled into an ink cartridge, and the ink cartridge was set in an inkjet recording device (product name "PIXUS PRO-10S", manufactured by Canon) equipped with a recording head that ejects ink by thermal energy. In this embodiment, the recording duty of a solid image recorded under the condition that four ink droplets of about 3.8 ng are applied to a unit area of ​​1 / 600 inch x 1 / 600 inch is defined as 100%. In order to prevent bias in the application position of the ink droplets, the ink droplets were applied under the condition that one ink droplet was applied to each of the four areas obtained by dividing the unit area of ​​1 / 600 inch x 1 / 600 inch into four, for a total of four droplets.

[0103] Using the above-mentioned inkjet recording device (serial method), ink was applied to a transparent label paper (product name "MZ0021E", manufactured by Avery), which is a non-absorbent recording medium, as follows to record a solid image. First, ink was applied so that the recording duty was 300%, and a solid image of 32.0 mm x 200.0 mm was recorded. At this time, the moving speed in the sub-scanning direction of the carriage carrying the recording head was 12.7 cm / s. After applying the ink, without transporting the recording medium in the sub-scanning direction, hot air at 80°C was blown from a position 10 mm above the recording medium for 10 seconds, and then the paper was discharged, and a solid image was recorded. The hot air was generated by a hot air dryer (product name "TSK hot air dryer TSK-18", manufactured by Kansai Electric Heat Co., Ltd.) and blown from a nozzle with a diameter of 4 mm. The wind speed was 30.0 m / s.

[0104] The above-mentioned hot air drying is not intended to dry all of the liquid components of the recorded image. This is a preliminary drying to suppress transfer or loss due to contact with the image, such as a paper presser of the recording medium, when handling the recording medium in the next process after recording. Preliminary drying makes the recording medium easier to handle. After that, the obtained solid image was placed in an oven at 80°C for 6 minutes to thoroughly dry the liquid components on the surface of the recording medium, and an evaluation image was obtained.

[0105] (Water abrasion resistance) Using a friction fastness tester (product name "JIS L 0849 Gakushin type II type", manufactured by DJK), a test load of 500g was applied to the evaluation image and a maximum of 30 strokes of the cloth cut to 50 x 50 mm from product name "attached white cotton cloth (Kanakin No. 3)" (manufactured by JSA GROUP) were rubbed. The cloth was moistened beforehand by dripping 100 μL of pure water onto it. The friction speed was 10 strokes / minute. After every 10 strokes, the state of scraping of the image was visually confirmed, and the water rub resistance of the image was evaluated according to the evaluation criteria shown below. AA: No image scraping occurred after 30 round trips. A: After 30 round trips, the image was scratched off, but after 20 round trips, the image was not scratched off. B: After 20 strokes, the image was scraped off, but after 10 strokes, the image was not scraped off. C: After 10 reciprocating passes, the image was scraped off.

[0106] (Adhesion recovery) After recording the above evaluation image, the power was turned off with the recording head in the home position (with the nozzle surface of the recording head covered with a cap). After leaving this state for three days in an environment of 25°C, the inkjet recording device was turned on and the same evaluation image as above was recorded again, and the degree of smearing of the recorded image was visually confirmed, and the adhesion recovery property was evaluated according to the evaluation criteria shown below. A: The area where blurring was observed was 10% or less. B: The area where blurring was confirmed was more than 10% but not more than 50%. C: The area where blur was confirmed exceeded 50%.

[0107] [Table 12]

Claims

1. A water-based inkjet ink containing titanium oxide particles, resin particles, a water-soluble organic solvent, and a surfactant, the titanium oxide particles are titanium oxide having at least a part of their surface covered with silica, and are dispersed at least by the action of the silica; the water-soluble organic solvent includes a first water-soluble organic solvent having a boiling point of 120° C. or more and 230° C. or less and an SP value of 11.0 or more and 13.5 or less, the content (mass %) of the water-soluble organic solvent is 5.00 mass % or more and 30.00 mass % or less based on the total mass of the ink, The ratio (mass%) of the first water-soluble organic solvent to the water-soluble organic solvent is 0.70 times or more; the surfactant comprises a first surfactant having an HLB value of 3 or more and 8 or less, The content (mass %) of the surfactant is 0.10 mass % or more and 0.40 mass % or less based on the total mass of the ink.

2. 2. The aqueous ink according to claim 1, wherein the HLB value of the first surfactant is 3 or more and 6 or less.

3. The aqueous ink according to claim 1 , wherein a ratio (mass %) of the first surfactant to the total surfactant is 0.50 times or more.

4. 2. The aqueous ink according to claim 1, wherein the first surfactant is an acetylene glycol-based nonionic surfactant.

5. The aqueous ink according to claim 1 , wherein a ratio (mass %) of the first water-soluble organic solvent to the water-soluble organic solvent is 0.90 times or more.

6. The aqueous ink according to claim 1 , wherein a ratio (mass %) of the first water-soluble organic solvent to the water-soluble organic solvent is 0.95 times or more.

7. The aqueous ink of claim 1 , wherein the first water-soluble organic solvent comprises an alkanediol.

8. The water-based ink according to claim 1 , further comprising a compound represented by the following general formula (2): 【Chemistry 1】 (In general formula (2), R 1 , R 2 , and R 3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 4 is an alkylene group having 2 to 4 carbon atoms; X is a single bond or an alkylene group having 1 to 6 carbon atoms; n is 6 to 24; a is 1 to 3, b is 0 to 2, and a+b=3.

9. An ink cartridge including an ink and an ink storage section for storing the ink, 9. An ink cartridge, comprising the ink according to claim 1.

10. An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, comprising: An ink-jet recording method, comprising the ink according to claim 1 .

Citation Information

Patent Citations

  • Inkjet recording method, inkjet recording apparatus, and recorded matter

    JP2013230638A

  • Ink jet ink composition and recording method

    JP2022131612A

  • Ink jet ink composition and recording method

    JP2023008056A