Coating device, method, and electrode
The coating device and method address solvent-related adhesion issues in multilayer electrodes by using a roll-based system for solvent-free bilayer application, enhancing conductivity and energy density while minimizing defects.
Patent Information
- Application Number
- JP2024055817
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing electrode manufacturing methods for multilayer coatings often require solvents, leading to adhesion issues and reduced performance due to incomplete coating, resulting in increased rejects and lower power output.
A coating device and method that applies bilayer powder layers directly to a substrate using a roll-based system with controlled metering and crimping, ensuring solvent-free production and improved adhesion without mixing layers, enhancing electrical conductivity and energy density.
The solution achieves uniform, solvent-free bilayer electrode coatings with improved conductivity and energy density by sequential application of powder layers with controlled adhesion forces and temperatures, reducing defects and optimizing material usage.
Smart Images

Figure 2024144390000001_ABST
Abstract
Description
[Technical field]
[0001] The invention relates to a coating device for producing an electrode having at least one bilayer powder layer on a substrate having the features of independent claim 1, to a method for producing an electrode having at least one bilayer powder layer, in particular a bilayer cathode layer and / or anode layer, on a substrate having the features of independent claim 6, as well as to an electrode having the features of independent claim 13.
[0002] In an attempt to fabricate solvent-free or dry electrodes, electrodes have traditionally been fabricated with a single layer coating. To improve battery cell performance, traditional electrode fabrication has pursued the approach of fabricating electrodes with multiple layer coatings (different compositions of individual layers) because such electrodes have enhanced energy density and electrical conductivity.
[0003] Currently, electrodes with solvent-free, multilayer coatings are often produced as free-standing films, where two powders are pressed against a current collector in a calendar gap.
[0004] However, it is still typical for electrodes to be wet processed and therefore contain solvents.
[0005] Another way is the sequential application of the individual layers as free-standing films on the side of the substrate provided for this purpose, for example, the application and pressing of the individual layers in each case can take place in two successively arranged calender gaps.
[0006] However, in this case, a certain amount of moisture in the adhesion promoter or powder is often necessary, since otherwise the adhesion of the layers cannot be guaranteed. This can result in a substrate or current collector that is not completely covered. This, in turn, can result in an increase in rejects or a decrease in power of the electrodes thus produced.
[0007] It is therefore an object of the present invention to at least partially overcome at least one of the above-mentioned disadvantages. In particular, it is an object of the present invention to provide a coating device which allows for dry electrode production, whereby the electrical conductivity or energy density of the electrode is increased. Furthermore, it is an object of the present invention to provide a method for dry electrode production and the electrodes thus produced.
[0008] The above-mentioned problem is solved by a coating device having the features of independent claim 1, a method having the features of independent claim 6 and an electrode having the features of independent claim 13. Further features and details of the invention emerge from the dependent claims, the description and the drawings. In this specification, the disclosures to the individual aspects of the invention are always or can be linked to one another, since features and details explained in connection with the coating device according to the invention are naturally also valid in connection with the method according to the invention and / or in connection with the electrode according to the invention and respectively vice versa.
[0009] According to the invention, in a first aspect of the invention, a coating apparatus for producing an electrode having at least one bilayer powder layer, in particular a bilayer cathode layer and / or a bilayer anode layer, on a substrate, in particular a current collector, is envisaged, which comprises a feed unit for feeding the substrate into a first crimping gap, a first roll arrangement for transferring a first powder as a first layer to a first side of the substrate, and a second roll arrangement for transferring a second powder as a second layer to the first layer on the first side of the substrate.
[0010] Here, the first roll arrangement has a first metering unit that receives the first powder and fills the first metering gap with the first powder. Additionally, the first roll arrangement has a first application roll, a first pressure roll unit and a second pressure roll unit, where the first metering gap is provided between the first application roll and the first pressure roll unit and the first pressure roll unit and the second pressure roll unit. The first metering gap is provided here for applying the first powder as a first layer to the first pressure roll unit with a first application force and the first pressure gap is provided for transferring the first layer from the first pressure roll unit to a first side of the substrate with a first pressure force.
[0011] The second roll arrangement is disposed after the first roll arrangement, and the first roll arrangement is configured to feed the substrate coated on a first side into a second crimping gap of the second roll arrangement.
[0012] The second roll arrangement has a second metering unit that receives the second powder and fills the second metering gap with the second powder. The second roll arrangement has a second application roll, a third pressure roll unit and a fourth pressure roll unit, the second metering gap is provided between the second application roll and the third pressure roll unit, and the second pressure gap is provided between the third pressure roll unit and the fourth pressure roll unit. The second metering gap is provided for applying the second powder as a second layer to the third pressure roll unit with a second application force, and the second pressure gap is provided for transferring the second layer from the third pressure roll unit to the first layer on the first side of the supplied substrate with a second pressure force.
[0013] The coating device is based on a roll-borne coating, in which a first powder is first applied as a first layer to a roll of a first pressure roll unit and then transferred or pressed onto the substrate from one roll or from this roll. This is followed by a further roll-borne coating, in which a second powder is applied as a second layer to a roll of a third pressure roll unit and then transferred onto the first layer from this roll or from another roll. This is particularly advantageous for the coating of the substrate with a solvent-free, dry powder material, and therefore the coating device is highly suitable for dry electrode production.
[0014] Furthermore, the first application roll of the first roll arrangement and the second application roll of the second roll arrangement can have a lower rotation speed than the application roll of the first or third pressure roll unit, respectively, with which they form the metering gap. This ensures that the first powder continues to adhere to the first pressure roll unit as a first layer, and the second powder continues to adhere to the third pressure roll unit as a second layer. In this case, when applying the powder to the respective application roll, the respective powder is sheared in the metering gap. The application force can therefore be a shear force, and the application rolls can also be called shear rolls.
[0015] The first and second pressing roll units may each have one pressing roll. The pressing rolls of the first and second pressing roll units, which form a pressing gap for applying a pressing force for transferring the first layer, rotate at the same rotational speed facing each other, which can provide an optimal coating result. The first application roll may have a lower rotational speed than the pressing roll of the first pressing roll unit, which forms a metering gap with the first application roll, which ensures that the first powder and the second powder remain attached to the first pressing unit as the first layer and are carried by the first pressing unit. The same applies for the third and fourth pressing roll units of the second roll arrangement. These may each also have one pressing roll, which rotate at the same rotational speed facing each other, which form a pressing force for transferring the second layer to the first layer.
[0016] In this case, the rotational speeds of the first and second pressure roll units are matched to the rotational speeds of the third and fourth pressure roll units so that the shear forces on the first layer already applied in the second pressure gap are as small as possible so as not to destroy the coating.
[0017] By depositing the individual layers of the bi-layer powder layer sequentially, the boundary layer between the first powder and the second powder, i.e., the first layer and the second layer, of the first bi-layer powder layer is reduced because no intermixing of the first powder and the second powder occurs.
[0018] It may be advantageous within the scope of the invention if the first roll arrangement has a third metering unit which receives a third powder and fills the third metering gap with the third powder, the first roll arrangement has a third application roll, the third metering gap is provided between the third application roll and the second pressure roll unit, and the third metering gap is provided for applying the third powder as a third layer to the third pressure roll unit with a third application force. The first pressure gap is provided for transferring the third layer from the second pressure roll unit to the second side of the substrate with a first application force.
[0019] This allows for the deposition of a first layer onto a first side of the substrate and, in parallel, the deposition of a third layer onto a second side of the substrate, with a first compression force in the first compression gap.
[0020] Within the scope of the present invention, it is conceivable that the second roll arrangement has a fourth metering unit which receives a fourth powder and fills the fourth metering gap with the fourth powder, that the second roll arrangement has a fourth application roll, that the fourth metering gap is provided between the fourth application roll and the fourth pressing roll unit, that the fourth metering gap is provided for applying the fourth powder as a fourth layer to the fourth pressing roll unit with a fourth application force, and that the second pressing gap is provided for transferring the fourth layer from the fourth pressing roll unit to the third layer on the second side of the substrate with a second pressing force.
[0021] This allows the deposition of a second layer onto a first layer of the substrate and, in parallel, the deposition of a fourth layer onto a third layer of the substrate, by a second compression force in the second compression gap.
[0022] In this case, the properties and characteristics of the coating device mentioned in relation to the first and second coating rolls apply analogously to the properties and characteristics related to the third and fourth coating rolls.
[0023] Furthermore, the third application roll of the first roll arrangement and the fourth application roll of the second roll arrangement can have a lower rotation speed than the application roll of the second or fourth pressure roll unit, respectively, with which they form the metering gap, which ensures that the third powder continues to adhere to the second pressure roll unit as a third layer and the fourth powder continues to adhere to the fourth pressure roll unit as a fourth layer.
[0024] Within the scope of the present invention, it may be assumed that the first pressing roll unit of the first roll arrangement has at least one first pressing roll and at least one second pressing roll, and at least one first pressing gap is provided between the at least one first pressing roll and the at least one second pressing roll. Additionally or alternatively, the second pressing roll unit of the first roll arrangement has at least one third pressing roll and at least one fourth pressing roll, and at least one second pressing gap is provided between the at least one third pressing roll and the at least one fourth pressing roll. Additionally or alternatively, the third pressing roll unit of the second roll arrangement has at least one fifth pressing roll and at least one sixth pressing roll, and at least one third pressing gap is provided between the at least one fifth pressing roll and the at least one sixth pressing roll. Additionally or alternatively, the fourth pressing roll unit of the second roll equipment has at least one seventh pressing roll and at least one eighth pressing roll, and at least one fourth press gap is provided between the at least one seventh pressing roll and the at least one eighth pressing roll.
[0025] The first and / or second and / or third and / or fourth press gaps press the first or second or third or fourth layer, which are then transferred to the substrate. This allows a denser packing of the first bilayer powder layer, which has a first and a second layer. At the same time, a denser packing of the second bilayer powder layer, which has a third and a fourth layer, can also be produced. This also allows the electrical conductivity to be further improved. Furthermore, the press gaps have the additional effect that the shear forces acting in both the metering gap and the pressing gap can be reduced, since less force is required for the application or transfer in these gaps. This leads to a uniform application and transfer, and reduces the number of defects during application or transfer.
[0026] It is further conceivable that in the region of the first metering gap a first shielding lamella is provided in the region of the first put-on roll and / or a second shielding lamella is provided in the region of the first pressure roll unit. Additionally or alternatively, it is conceivable that in the region of the second metering gap a third shielding lamella is provided in the region of the second put-on roll and / or a fourth shielding lamella is provided in the region of the third pressure roll unit. Additionally or alternatively, it is conceivable that in the region of the third metering gap a fifth shielding lamella is provided in the region of the third put-on roll and / or a sixth shielding lamella is provided in the region of the second pressure roll unit. Additionally or alternatively, it is conceivable that in the region of the fourth metering gap a seventh shielding lamella is provided in the region of the fourth application roll and / or an eighth shielding lamella is provided in the region of the fourth pressure roll unit.
[0027] The shielding lamellae are used to prevent the powder from coming into contact with the respective pressure roll unit before the metering gap or from adhering to the application roll assigned to the respective pressure roll unit. At the same time, such shielding lamellae can easily control the drawing of the powder into the first and / or second metering gap. At the same time, it is conceivable for the shielding lamellae to have structures for cleaning the respective application roll and / or respective pressure roll unit or for removing adhering material. This allows the cleanest possible application of the new first and / or second and / or third and / or fourth layer or a clean transfer of the first and / or second layer to the substrate or a clean transfer of the third layer to the first layer and / or the fourth layer to the second layer.
[0028] Furthermore, in the case of the coating device, it is conceivable that the first coating roll and / or the second coating roll and / or the third coating roll and / or the fourth coating roll and / or the first pressure roll unit and / or the second pressure roll unit and / or the third pressure roll unit and / or the fourth pressure roll unit are temperature adjustable.
[0029] This can significantly simplify the application and delivery of various powders or layers to a roll or substrate, since the adhesion at the surface can be adapted to the material to be applied.
[0030] The above-mentioned object is furthermore achieved in a second aspect of the invention by a method according to the invention for producing an electrode having at least one bilayer powder layer, in particular a bilayer cathode layer and / or a bilayer anode layer, on a substrate, in particular a current collector, in a coating device according to any of the preceding claims, which method comprises: - feeding the substrate by a feeding unit into a first crimping gap of a first roll arrangement; filling the first metering gap with a first powder by a first metering unit; - applying a first powder as a first layer to a first pressure roll unit in a first metering gap with a first application force; - transferring the first layer to a first side of the substrate in a first crimping gap by a crimping force; feeding the substrate with the delivered first layer into a second crimping gap of a second roll arrangement, filling the second metering gap with a second powder by a second metering unit; - applying a second powder as a second layer to a third pressure roll unit in a second metering gap with a second application force; transferring the second layer to the first layer on the first side of the substrate in a second crimping gap by a second crimping force; It has.
[0031] By depositing the first and second layers in succession, the first layer is additionally compressed, which advantageously affects the electrical conductivity and energy density of the electrode that can be produced using this first layer.
[0032] It is also conceivable in this method that a third metering unit fills the third metering gap with a third powder, which is applied to the second pressing roll unit in the third metering gap as a third layer by a third application force, and that the third layer is transferred to the second side of the substrate in the first pressing gap by a first pressing force.
[0033] The third metering unit and third application roll allow the first layer to be delivered to the first side of the substrate and the third layer to be delivered to the second side of the substrate at the same time, which is time-saving and efficient.
[0034] Within the scope of the present invention, optionally, the fourth metering unit can fill the fourth metering gap with a fourth powder, which is applied to the fourth pressing roll unit as a fourth layer in the fourth metering gap by a fourth application force, and the fourth layer is delivered to the third layer on the second side of the substrate in the second pressing gap by a second pressing force.
[0035] The fourth metering unit and fourth application roll allow the second layer to be applied to the first layer on the first side of the substrate at the same time that the fourth layer is applied to the third layer on the second side of the substrate, which is time-saving and efficient.
[0036] It may further be conceivable within the scope of the present invention that the first metering unit continuously fills the first metering gap and / or the second metering unit continuously fills the second metering gap and / or the third metering unit continuously fills the third metering gap and / or the fourth metering unit continuously fills the fourth metering gap.
[0037] This allows particularly uniform results to be achieved when producing the individual layers at the pressure roll unit, which is then passed onto the substrate or onto a layer that has already been applied to the substrate.
[0038] In the context of the present invention, it is conceivable to press the first layer in at least one first press gap of a first pressing roll unit of the first roll arrangement. Additionally or alternatively, it is conceivable to press the third layer in at least one second press gap of a second pressing roll unit of the first roll arrangement. Additionally or alternatively, it is conceivable to press the second layer in at least one third press gap of a third pressing roll unit of the second roll arrangement. Additionally or alternatively, it is conceivable to press the fourth layer in at least one fourth press gap of a fourth pressing roll unit of the second roll arrangement.
[0039] Pressing in each press gap causes a compression of the first layer and / or the second layer and / or the third layer and / or the fourth layer, thereby producing a closer packing of the respective at least bi-layered powder layers on the first side and / or the second side of the substrate, which allows a reduction in the first adhesion force and / or the second adhesion force and / or the third adhesion force and / or the fourth adhesion force and / or the first compression force and / or the second compression force.
[0040] Furthermore, it is considered that the temperature of the first coating roll and / or the second coating roll and / or the third coating roll and / or the fourth coating roll and / or the first pressure roll unit and / or the second pressure roll unit and / or the third pressure roll unit and / or the fourth pressure roll unit may be adjusted to a temperature of 80°C to 150°C, particularly 100°C to 120°C.
[0041] This allows for improved application of the first and second powders as a first layer to the first compression roll unit and / or improved application of the third and fourth powders as a second layer to the second compression roll unit. Furthermore, temperature adjustment of the individual rolls can improve the delivery of the first layer to the first side of the substrate and / or the third layer to the second side of the substrate and / or the second layer to the first layer on the first side of the substrate and / or the fourth layer to the third layer on the second side of the substrate, since the individual bonding of the individual powders of each layer is enhanced by heat.
[0042] In this case, it is also conceivable to temperature-regulate the supply unit in order to pre-warm the substrate for delivery, i.e. for pressing a first layer onto the first side of the substrate and / or for pressing a third layer onto the second side of the substrate.
[0043] Within the scope of the present invention, it may be advantageous for the first pressure roll unit and the second pressure roll unit of the first roll arrangement to rotate opposite each other at the same first rotation speed, wherein the ratio of the first rotation speed of the first pressure roll unit to the second rotation speed of the first covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3 and / or the ratio of the first rotation speed of the second pressure roll unit to the fifth rotation speed of the third covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3. Additionally or alternatively, the third pressure roll unit and the fourth pressure roll unit of the second roll facility rotate facing each other at the same third rotational speed, and the ratio of the third rotational speed of the third pressure roll unit to the fourth rotational speed of the second covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3, and / or the ratio of the third rotational speed of the fourth pressure roll unit to the sixth rotational speed of the fourth covering roll is 10:1 to 10:4, preferably 10:1.5 to 10:3, more preferably 10:2 to 10:3.
[0044] When the first pressing roll unit of the first roll facility has a first pressing roll and a second pressing roll, and / or the second pressing roll unit of the first roll facility has a third pressing roll and a fourth pressing roll, the first rotation speed is effective as the rotation speed of the first pressing roll of the first pressing roll unit and the third pressing roll of the second pressing roll unit. This is because they form a first pressing gap. In this case, the second pressing roll and the fourth pressing roll may each have a rotation speed different from the first rotation speed. For example, the ratio of the first rotation speed of the first pressing roll and the third pressing roll to the rotation speed of the second pressing roll and / or the fourth pressing roll may be 10:5 to 10:8, preferably 10:6 to 10:8, more preferably 10:7 to 10:8.
[0045] If the third pressing roll unit of the second roll facility has a fifth pressing roll and a sixth pressing roll, and / or the fourth pressing roll unit of the second roll facility has a seventh pressing roll unit and an eighth pressing roll unit, the third rotation speed is effective as the rotation speed of the fifth pressing roll and the seventh pressing roll, since they form the second pressing gap. Here too, the sixth pressing roll and the eighth pressing roll may have a rotation speed different from the third rotation speed. For example, the ratio of the third rotation speed of the fifth pressing roll and the seventh pressing roll to the rotation speed of the sixth pressing roll and / or the eighth pressing roll may be 10:5 to 10:8, preferably 10:6 to 10:8, more preferably 10:7 to 10:8.
[0046] Here, it has been found to be advantageous that the ratio of rotation speeds results in an increased stability of the first layer or the first at least bilayered powder layer on the current collector of the electrode and / or the second layer or the second at least bilayered powder layer on the current collector of the electrode.
[0047] The above-mentioned object is further achieved in a third aspect of the present invention by an electrode according to the invention having a two-layered powder layer produced by the above-mentioned coating device and / or the above-mentioned method, wherein the substrate is a current collector having a first side and a second side, the first layer of the two-layered powder layer consisting of a first powder and the second layer of the two-layered powder layer consisting of a second powder.
[0048] Within the scope of the present invention it is conceivable that the third layer of the double-layered powder layer consists of a third powder and the fourth layer of the double-layered powder layer consists of a fourth powder.
[0049] Here, the electrode can be used as both an anode and a cathode, in which case the cathode bilayer powder layer can be different from the anode bilayer powder layer, and the anode current collector and the cathode current collector can be different.
[0050] Such electrodes have an optimally compacted bilayer powder layer, which is solvent-free, and at the same time, the electrodes thus produced have high electrical conductivity and energy density.
[0051] A particularly good ratio of material usage of the first, second, third and fourth powders to the existing electrical conductivity of the two-layer powder layer is obtained when the two-layer powder layer has a layer thickness of 40-150 μm, where the first powder of the first layer and the third powder of the third layer have a layer thickness of 10-70 μm, which also allows for a cost-effective use of materials.
[0052] The advantages detailed with respect to the coating apparatus of the first aspect of the invention apply equally to the method of the second aspect of the invention as well as to the electrode of the third aspect of the invention.
[0053] Further advantages, features and details of the invention will become apparent from the following description, in which several embodiments of the invention are described in detail with reference to the drawings. In this application, the features described in the claims and in the specification may each individually or in any combination form the essence of the invention. The invention is illustrated in the following drawings. [Brief description of the drawings]
[0054] [Figure 1] FIG. 1 shows a schematic of a coating apparatus for application and delivery of a first bilayer powder layer. [Diagram 2] FIG. 1 shows a schematic of a coating apparatus for application and delivery of a first bi-layer powder layer and a second bi-layer powder layer. [Diagram 3] FIG. 2 is a diagram showing a portion of the first metering gap of FIG. 1; [Figure 4] FIG. 2 is a schematic diagram showing a method using the coating apparatus shown in FIG. 1. [Diagram 5] FIG. 3 is a schematic diagram showing a method using the coating apparatus shown in FIG. 2. [Figure 6]FIG. 2 is a schematic diagram of an electrode.
[0055] 1 and 2 each show a coating device 10 for producing an electrode 11 having at least one bilayer powder layer 12, in particular a bilayer cathode layer 13 and / or a bilayer anode layer 14, on a substrate 15, in particular a current collector 16. Here, FIG. 1 shows a coating device 10 for coating on one side of a substrate 15 by deposition 130 and delivery 140 of at least one first bilayer powder layer 12, and FIG. 2 shows a coating device 10 for coating on both sides of a substrate 15 by deposition 130, 180 and delivery 140, 190 of at least one first bilayer powder layer 12, i.e. first layer 26 and second layer 34, and at least one second bilayer powder layer 12, i.e. third layer 41 and fourth layer 47.
[0056] Both the coating apparatus 10 of FIG. 1 and the coating apparatus 10 of FIG. 2 have a feeding unit 17 for feeding 110 the substrate 15 into the first crimping gap 18, a first roll arrangement 19 for delivering 140 a first powder 21 to a first side 27 of the substrate 15 as a first layer 26, and a second roll arrangement 28 for delivering 140 a second powder 29 to the first layer 26 on the first side 27 of the substrate 15.
[0057] The first roll arrangement 19 here has a first metering unit 20 which receives a first powder 21 and fills a first metering gap 22 with the first powder 21. The first roll arrangement 19 further comprises a first cover roll 23, a first pressure roll unit 24 and a second pressure roll unit 25. Here, the first metering gap 22 is arranged between the first cover roll 23 and the first pressure roll unit 24, and the first pressure gap 18 is arranged between the first pressure roll unit 24 and the second pressure roll unit 25.
[0058] The first metering gap 22 is provided here for applying 130 the first powder 21 as a first layer 26 to the first compression roll unit 24 with a first application force FA1, and the first compression gap 18 is provided for transferring 140 the first layer 26 from the first compression roll unit 24 to the first side 27 of the substrate 15 with a first application force FP1.
[0059] The second roll arrangement 28 is arranged after the first roll arrangement 19, where the first roll arrangement 19 is configured to feed the substrate 15 coated on a first side 27 to a second crimping gap 30 of the second roll arrangement 28.
[0060] The second roll arrangement 28 comprises a second metering unit 31 which receives a second powder 29 and fills a second metering gap 32 with the second powder 29. The second roll arrangement 28 further comprises a second application roll 33, a third pressure roll unit 34 and a fourth pressure roll unit 35. The second metering gap 32 is arranged between the second application roll 33 and the third pressure roll unit 34. The second pressure gap 30 is likewise arranged between the third pressure roll unit 34 and the fourth pressure roll unit 35. Here, the second metering gap 32 is provided for depositing 130 the second powder 29 as a second layer 36 onto the third pressing roll unit 34 with a second deposition force FA2, and the second pressing gap 30 is provided for transferring 140 the second layer 36 from the third pressing roll unit 34 to the first layer 26 on the first side 27 of the supplied substrate 15 with a second deposition force FP2.
[0061] In order to be able to apply the two-layer powder layer 12 to the substrate 15 on both sides, the first roll arrangement 19 of the coating device 10 of FIG. 2 has a third metering unit 37 which receives a third powder 38 and fills a third metering gap 39 with the third powder 38. Furthermore, a third application roll 40 is provided, the third metering gap 39 being provided between the third application roll 40 and the second pressure roll unit 25. The third metering gap 39 is used to apply 130 the third powder 38 as a third layer 41 to the third pressure roll unit 34 with a third application force FA3. In this situation too, the first pressure gap 18 is provided to transfer 140 the third layer 41 from the second pressure roll unit 25 to the second side 42 of the substrate 15 with a first application force FP1.
[0062] Additionally, the second roll arrangement 28 has a fourth metering unit 43 which receives a fourth powder 44 and fills a fourth metering gap 45 with the fourth powder 44. For this purpose, a fourth application roll 46 is provided, the fourth metering gap 45 being provided between the fourth application roll 46 and the fourth pressure roll unit 35. The fourth metering gap 45 is provided for applying 130 the fourth powder 44 as a fourth layer 47 to the fourth pressure roll unit 35 with a fourth application force FA4. The second pressure gap 30 is provided for transferring 140 the fourth layer 47 from the fourth pressure roll unit 35 to the third layer 41 on the second side 42 of the substrate 15 with a second application force FP2.
[0063] Further, in the coating apparatus 10 shown in FIG. 2, the first pressure roll unit 24 of the first roll facility 19 is shown to have at least one first pressure roll 48 and at least one second pressure roll 49, with at least one first press gap 50 being provided between the at least one first pressure roll 48 and the at least one second pressure roll 49, and the second pressure roll unit 25 of the first roll facility 19 is shown to have at least one third pressure roll 51 and at least one fourth pressure roll 52, with at least one second press gap 53 being provided between the at least one third pressure roll 51 and the at least one fourth pressure roll 52. Additionally, the third pressing roll unit 34 of the second roll facility 28 has at least one fifth pressing roll 54 and at least one sixth pressing roll 55, and at least one third pressing gap 56 is provided between the at least one fifth pressing roll 54 and the at least one sixth pressing roll 55. Additionally, the fourth pressing roll unit 35 of the second roll facility 28 has at least one seventh pressing roll 57 and at least one eighth pressing roll 58, and at least one fourth pressing gap 59 is provided between the at least one seventh pressing roll 57 and the at least one eighth pressing roll 58.
[0064] Figure 3 shows an enlarged portion of the first metering gap 22 with the first metering unit 20, which can be designed both in the coating apparatus 10 of Figure 1 and in the coating apparatus 10 of Figure 2. In the region of the first metering gap 22, a first shielding lamella 60 is provided in the region of the first application roll 23 and / or a second shielding lamella 61 is provided in the region of the first pressure roll unit 24.
[0065] It is conceivable here that in the region of the second metering gap 32 a third shielding lamella 62 is provided in the region of the second put-on roll 33 and / or a fourth shielding lamella 63 is provided in the region of the third pressure roll unit 34, and / or in the region of the third metering gap 39 a fifth shielding lamella 64 is provided in the region of the third put-on roll 40 and / or a sixth shielding lamella 65 is provided in the region of the second pressure roll unit 25, and / or in the region of the fourth metering gap 45 a seventh shielding lamella 66 is provided in the region of the fourth put-on roll 46 and / or an eighth shielding lamella 67 is provided in the region of the fourth pressure roll unit 35.
[0066] 4 and 5 respectively show a method 100 for producing an electrode 11 having at least one bilayer powder layer 12, in particular a bilayer cathode layer 13 and / or a bilayer anode layer 14, on a substrate 15, in particular a current collector 16, in a coating apparatus 10 according to FIG. 1 or 2. These methods comprise the steps of: A step 110 of feeding the substrate 15 by a feeding unit 17 into a first crimping gap 18 of a first roll arrangement 19; filling 120 the first metering gap 22 with a first powder 21 by means of a first metering unit 20; A step 130 of depositing the first powder 21 as a first layer 26 on the first pressure roll unit 24 in the first metering gap 22 with a first deposition force FA1; a step 140 of transferring the first layer 26 to the first side 27 of the substrate 15 in the first crimping gap 18 with a first crimping force FP1; feeding 160 the substrate 15 with the delivered 140 first layer 26 into a second crimping gap 30 of a second roll fixture 28; filling 170 the second metering gap 32 with a second powder 29 by means of a second metering unit 31; a step 180 of depositing the second powder 29 as a second layer 36 on the third pressure roll unit 34 in the second metering gap 32 with a second deposition force FA2; a step 190 of transferring the second layer 36 to the first layer 26 of the first side 27 of the substrate 15 in the second crimping gap 30 with a second crimping force FP2; It has.
[0067] The coating apparatus 10 of Figure 2 has a third metering unit 37, and therefore in the method of Figure 5, the third metering unit 37 fills 120 the third metering gap 39 with a third powder 38, which is applied 130 to the second pressing roll unit 25 in the third metering gap 39 as a third layer 41 by a third application force FA3, and the third layer 41 is delivered 140 to the second side 42 of the substrate 15 in the first pressing gap 18 by a first pressing force FP1.
[0068] Furthermore, the coating apparatus 10 of FIG. 2 is also provided with a fourth metering unit 43, so that in the method of FIG. 5, the fourth metering unit 43 fills 170 the fourth metering gap 45 with a fourth powder 44, which is applied 180 to the fourth pressing roll unit 35 in the fourth metering gap 45 as a fourth layer 47 by a fourth application force FA4, and the fourth layer 47 is delivered 140 to the third layer 41 on the second side 42 of the substrate 15 in the second pressing gap 30 by a second pressing force FP2.
[0069] In order to achieve good results in the deposition of layers on the substrate 15, the coating apparatus 10 and method 100 are configured such that the first metering unit 20 continuously fills 120 the first metering gap 22, the second metering unit 31 continuously fills 170 the second metering gap 32, the third metering unit 37 continuously fills 120 the third metering gap 39, and the fourth metering unit 43 continuously fills 170 the fourth metering gap 45.
[0070] In the method 100 of Figure 5, the first layer 26 is pressed 150 in at least one first press nip 50 of a first compression roll unit 24 of the first roll installation 19, and the third layer 41 is pressed 150 in at least one second press nip 53 of a second compression roll unit 25 of the first roll installation 19. Additionally, the second layer 36 is pressed 200 in at least one third press nip 56 of a third compression roll unit 34 of the second roll installation 28, and the fourth layer 47 is pressed 200 in at least one fourth press nip 59 of a fourth compression roll unit 35 of the second roll installation 28.
[0071] For better application 130 of the layer and delivery 140 of the layer, the first application roll 23 and the second application roll 33 as shown in Figures 1 and 2, the third application roll 40 and the fourth application roll 46 as shown in Figure 2, and the first pressure roll unit 24 and the second pressure roll unit 25 and the third pressure roll unit 34 and the fourth pressure roll unit 35 of Figures 1 and 2 as shown in Figures 4 and 5 are temperature-adjusted 210 to a temperature of 80°C to 150°C.
[0072] When performing the method 100 shown in FIG. 4 by the coating apparatus 10 shown in FIG. 1 or the method 100 of FIG. 5 by the coating apparatus 10 of FIG. 2, the first pressure roll unit 24 and the second pressure roll unit 25 of the first roll facility 19 rotate opposite each other at the same first rotation speed v1, and the ratio of the first rotation speed v1 of the first pressure roll unit 24 to the second rotation speed v2 of the first covering roll 23 is 10:1 to 10:4. At the same time, the third pressure roll unit 34 and the fourth pressure roll unit 35 of the second roll facility 28 rotate opposite each other at the same third rotation speed v3, and the ratio of the third rotation speed v3 of the third pressure roll unit 34 to the fourth rotation speed v4 of the second covering roll 33 is 10:1 to 10:4.
[0073] In the method 100 shown in FIG. 5, the ratio between the first rotational speed v1 of the second pressing roll unit 25 and the fifth rotational speed v5 of the third pressing roll 40 is 10:1 to 10:4, and the ratio between the third rotational speed v3 of the fourth pressing roll unit 35 and the sixth rotational speed v6 of the fourth coating roll 46 is 10:1 to 10:4.
[0074] 6 shows an electrode 11 having a bilayer powder layer 12 produced by a method 100 according to the coating apparatus 10 shown in FIG 1 or 2 and / or the method shown in FIG 3 or 4, where the substrate 15 is a current collector 16 having a first side 27 and a second side 42, a first layer 26 of the bilayer powder layer 12 consisting of a first powder 21, and a second layer 36 of the bilayer powder layer 12 consisting of a second powder 29.
[0075] Additionally, a third layer 41 of the bi-layer powder layer 12 is made of the third powder 38 and a fourth layer 47 of the bi-layer powder layer 12 is made of the fourth powder 44 .
[0076] Here, the bi-layer powder layer 12 on the first side 27 of the substrate 15 has a first layer thickness SD1 and the bi-layer powder layer 12 on the second side 42 of the substrate 15 has a second layer thickness SD2 of 40-150 μm, the first powder 21 of the first layer 26 has a first layer thickness SP1 of 10-70 μm, and the third powder 38 of the third layer 41 has a second layer thickness SP2 of 10-70 μm. This allows for cost-efficient material usage. [Explanation of symbols]
[0077] 10 Coating device 11 electrodes 12 Two-layered powder layer 13 Cathode layer 14 Anode layer 15 Base material 16 Current collector 17 Supply Unit 18 First crimp gap 19 First Roller Equipment 20 First metering unit 21 First Powder 22 First metering gap 23 First application roll 24 First pressure roller unit 25 Second Compression Roll Unit 26 First Layer 27 First Side 28 Second Rolling Equipment 29 Second Powder 30 Second crimp gap 31 Second metering unit 32 Second metering gap 33 Second application roll 34 3rd Compression Roll Unit 35 4th compression roll unit 36 Second Layer 37 Third metering unit 38 The Third Powder 39 Third metering gap 40 Third application roll 41 The Third Layer 42 Second Side 43 4th metering unit 44 Fourth Powder 45 Fourth metering gap 46 Fourth application roll 47 Fourth Layer 48 First crimping roll 49 Second crimping roll 50 First press gap 51 Third bonding roll 52 4th compression roll 53 Second press gap 54 5th compression roll 55 6th compression roll 56 Third press gap 57 7th compression roll 58 No. 8 crimping roll 59 Fourth press gap 60 First shielding sheet 61 Second shielding sheet 62 Third shielding sheet 63 Fourth Shielding Sheet 64 Fifth Shielding Sheet 65 6th shielding sheet 66 Seventh Shielding Sheet 67 8th shielding sheet 100 ways Generation of the first and third layers 110 supply 120 Parallel filling 130 Adherence 140 Delivery 150 Press Creating the second and fourth layers 160 supply 170 Parallel filling 180 Adhesion 190 Delivery 200 Press 210 Temperature adjustment FA1 First adhesion FA2 Second Adhesion FA3 Third Adhesion FA4 4th adhesion force FP1 First crimp force FP2 Secondary Crimping Force SD1: First layer thickness of the first bilayer powder layer SD1 Second layer thickness of the second bilayer powder layer SP1: First layer thickness of the first powder of the first two-layer powder layer SP2: the second layer thickness of the third powder in the second bilayer powder layer v1 First rotation speed v2 Second rotation speed v3 Third rotation speed v4 Fourth rotation speed v5 Fifth rotation speed v6 6th rotation speed
Claims
1. A coating device (10) for producing an electrode (11) having at least one bilayer powder layer (12), in particular a bilayer cathode layer (13) and / or a bilayer anode layer (14), on a substrate (15), in particular a current collector (16), comprising: The coating device (10) comprises: a supply unit (17) for supplying (110) a substrate (15) into a first crimping gap (18); a first roll facility (19) for delivering (140) a first powder (21) as a first layer (26) to a first side (27) of the substrate (15); The first roll arrangement (19) has a first metering unit (20) that receives a first powder (21) and fills a first metering gap (22) with the first powder (21), and The first roll facility (19) comprises a first application roll (23), a first pressure roll unit (24) and a second pressure roll unit (25); the first metering gap (22) is provided between the first applied roll (23) and the first pressure roll unit (24), and the first pressure gap (18) is provided between the first pressure roll unit (24) and the second pressure roll unit (25); The first metering gap (22) is provided for applying (130) the first powder (21) as a first layer (26) to the first pressure roll unit (24) with a first application force (FA1); and the first pressing gap (18) is provided for transferring (140) the first layer (26) from the first pressing roll unit (24) to a first side (27) of the substrate (15) with a first pressing force (FP1); The coating device (10) comprises: a second roll facility (28) for delivering (140) a second powder (29) to the first layer (26) on the first side (27) of the substrate (15); the second roll arrangement (28) is arranged after the first roll arrangement (19), the first roll arrangement (19) being configured to feed the substrate (15) coated on the first side (27) to a second crimping gap (30) of the second roll arrangement (28); the second roll arrangement (28) has a second metering unit (31) which receives a second powder (29) and fills a second metering gap (32) with the second powder (29); The second roll facility (28) comprises a second application roll (33), a third pressure roll unit (34) and a fourth pressure roll unit (35); The second metering gap (32) is provided between the second application roll (33) and the third pressure roll unit (34); and The second pressing gap (30) is provided between the third pressing roll unit (34) and the fourth pressing roll unit (35), the second metering gap (32) is provided for depositing (130) the second powder (29) as a second layer (36) onto the third pressure roll unit (34) with a second deposition force (FA2); and the second pressing gap (30) is provided for transferring (140) the second layer (36) from the third pressing roll unit (34) to the first layer (26) of the first side (27) of the supplied substrate (15) with a second pressing force (FP2); A coating device (10).
2. The first roll arrangement (19) has a third metering unit (37) that receives a third powder (38) and fills a third metering gap (39) with the third powder (38), and the first roll arrangement (19) has a third application roll (40), the third metering gap (39) is provided between the third application roll (40) and the second pressure roll unit (25), and the third metering gap (39) is filled with the third powder (38). is provided for depositing (130) the third powder (38) as a third layer (41) onto the third pressing roll unit (34) with a third deposition force (FA3), and the first pressing gap (18) is provided for transferring (140) the third layer (41) from the second pressing roll unit (25) to a second side (42) of the substrate (15) with the first pressing force (FP1). The coating device (10) of claim 1.
3. The second roll arrangement (28) has a fourth metering unit (43) that receives a fourth powder (44) and fills a fourth metering gap (45) with the fourth powder (44), and the second roll arrangement (28) has a fourth application roll (46), the fourth metering gap (45) is provided between the fourth application roll (46) and the fourth pressure roll unit (35), and ... the fourth powder (44) is provided for depositing (130) as a fourth layer (47) onto the fourth pressure roll unit (35) with a fourth deposition force (FA4), and the second pressure gap (30) is provided for transferring (140) the fourth layer (47) from the fourth pressure roll unit (35) to the third layer (41) on the second side (42) of the substrate (15) with the second pressure force (FP2). The coating device (10) according to claim 1 or 2.
4. the first pressing roll unit (24) of the first roll facility (19) comprises at least one first pressing roll (48) and at least one second pressing roll (49), with at least one first pressing gap (50) between the at least one first pressing roll (48) and the at least one second pressing roll (49); and / or the second pressing roll unit (25) of the first roll facility (19) has at least one third pressing roll (51) and at least one fourth pressing roll (52), with at least one second pressing gap (53) between the at least one third pressing roll (51) and the at least one fourth pressing roll (52); and / or the third pressing roll unit (34) of the second roll facility (28) has at least one fifth pressing roll (54) and at least one sixth pressing roll (55), and at least one third pressing gap (56) is provided between the at least one fifth pressing roll (54) and the at least one sixth pressing roll (55); and / or the fourth pressing roll unit (35) of the second roll facility (28) has at least one seventh pressing roll (57) and at least one eighth pressing roll (58), and at least one fourth pressing gap (59) is provided between the at least one seventh pressing roll (57) and the at least one eighth pressing roll (58). The coating device (10) according to any one of claims 1 to 3.
5. In the region of the first metering gap (22), a first shielding lamella (60) is provided in the region of the first application roll (23) and / or a second shielding lamella (61) is provided in the region of the first pressure roll unit (24), and / or in the region of the second metering gap (32), a third shielding lamella (62) is provided in the region of the second application roll (33) and / or a fourth shielding lamella (63) is provided in the region of the third pressure roll unit (34), and / or in the region of the third metering gap (39), a fifth shielding lamella (64) is provided in the region of the third application roll (40) and / or a sixth shielding lamella (65) is provided in the region of the second pressure roll unit (25), and / or in the region of the fourth metering gap (45), a seventh shielding lamella (66) is provided in the region of the fourth application roll (46) and / or an eighth shielding lamella (67) is provided in the region of the fourth pressure roll unit (35), The coating device (10) according to any one of claims 1 to 4.
6. A method (100) for producing an electrode (11) having at least one bilayer powder layer (12), in particular a bilayer cathode layer (13) and / or a bilayer anode layer (14), on a substrate (15), in particular a current collector (16), in a coating device (10) according to any one of claims 1 to 5, comprising the steps of: - feeding (110) the substrate (15) by a feeding unit (17) into a first crimping gap (18) of a first roll facility (19); - filling (120) the first metering gap (22) with a first powder (21) by means of a first metering unit (20); - depositing (130) the first powder (21) as a first layer (26) on a first pressure roll unit (24) in the first metering gap (22) with a first deposition force (FA1); - transferring (140) the first layer (26) to a first side (27) of the substrate (15) in the first crimping gap (18) with a first crimping force (FP1); feeding (160) said substrate (15) with said first layer (26) delivered (140) to a second crimping gap (30) of a second roll fixture (28); - filling (170) the second metering gap (32) with a second powder (29) by means of a second metering unit (31); - depositing (180) the second powder (29) as a second layer (36) on a third pressure roll unit (34) in the second metering gap (32) with a second deposition force (FA2); - transferring (190) the second layer (36) to the first layer (26) of the first side (27) of the substrate (15) in the second crimping gap (30) with a second crimping force (FP2); It has Method (100).
7. a third metering unit (37) fills (120) a third metering gap (39) with a third powder (38), the third powder (38) is applied (130) in the third metering gap (39) to a second pressing roll unit (25) by a third application force (FA3) as a third layer (41), and the third layer (41) is delivered (140) to a second side (42) of the substrate (15) by the first pressing force (FP1) in the first pressing gap (18); The method (100) of claim 6.
8. a fourth metering unit (43) fills (170) a fourth metering gap (45) with a fourth powder (44), the fourth powder (44) is applied (180) in the fourth metering gap (45) as a fourth layer (47) to a fourth pressing roll unit (35) by a fourth application force (FA4), and the fourth layer (47) is transferred (140) to the third layer (41) on the second side (42) of the substrate (15) by the second pressing force (FP2) in the second pressing gap (30); The method (100) of claim 6 or 7.
9. the first metering unit (20) continuously fills the first metering gap (22) (120), and / or the second metering unit (31) continuously fills the second metering gap (32) (170), and / or the third metering unit (37) continuously fills the third metering gap (39) (120), and / or the fourth metering unit (43) continuously fills the fourth metering gap (45) (170), The method (100) of any one of claims 6 to 8.
10. pressing (150) the first layer (26) in at least one first pressing nip (50) of the first compression roll unit (24) of the first roll facility (19); and / or pressing (150) the third layer (41) in at least one second pressing nip (53) of the second pressing roll unit (25) of the first roll facility (19); and / or pressing (200) the second layer (36) in at least one third press nip (56) of the third compression roll unit (34) of the second roll facility (28); and / or pressing (200) the fourth layer (47) in at least one fourth press nip (59) of the fourth compression roll unit (35) of the second roll facility (28); The method (100) of any one of claims 6 to 9.
11. adjusting (210) the temperature of the first applying roll (23) and / or the second applying roll (33) and / or the third applying roll (40) and / or the fourth applying roll (46) and / or the first pressure roll unit (24) and / or the second pressure roll unit (25) and / or the third pressure roll unit (34) and / or the fourth pressure roll unit (35) to a temperature of 80° C. to 150° C., The method (100) of any one of claims 6 to 10.
12. the first pressure roll unit (24) and the second pressure roll unit (25) of the first roll facility (19) rotate opposite each other at the same first rotation speed (v1), the ratio between the first rotation speed (v1) of the first pressure roll unit (24) and the second rotation speed (v2) of the first applied roll (23) being between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:3, and / or the ratio between the first rotation speed (v1) of the second pressure roll unit (25) and the fifth rotation speed (v5) of the third applied roll (40) being between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:3, and / or the first pressing roll unit (34) and the fourth pressing roll unit (35) of the second roll facility (28) rotate opposite each other at the same third rotation speed (v3), the ratio of the third rotation speed (v3) of the third pressing roll unit (34) to the fourth rotation speed (v4) of the second applying roll (33) being between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:3, and / or the ratio of the third rotation speed (v3) of the fourth pressing roll unit (35) to the sixth rotation speed (v6) of the fourth applying roll (46) being between 10:1 and 10:4, preferably between 10:1.5 and 10:3, more preferably between 10:2 and 10:3, The method (100) of any one of claims 6 to 11.
13. Electrode (11) having a two-layer powder layer (12) produced by the coating device (10) according to any one of claims 1 to 5 and / or the method (100) according to any one of claims 6 to 12, The substrate (15) is a current collector (16) having a first side (27) and a second side (42); a first layer (26) of the two-layered powder layer (12) made of a first powder (21), and a second layer (36) of the two-layered powder layer (12) made of a second powder (29); Electrode (11).
14. a third layer (41) of the two-layered powder layer (12) made of a third powder (38), and a fourth layer (47) of the two-layered powder layer (12) made of a fourth powder (44); The electrode (11) according to claim 13.
Citation Information
Patent Citations
Dry-method electrode production equipment
CN217334143U
Method for manufacturing electrode for electrochemical element
JP2013077561A
Manufacturing method of film-coated object, manufacturing device of film-coated object, film-coated object, non-aqueous secondary battery electrode plate, and movable body
JP2016059870A
Manufacturing method of electrode plate
JP2018101518A
Method for manufacturing electrode
JP2018125201A