Zeolite membrane composite and method for producing the same, and method for producing methanol using the same
The zeolite membrane composite with a sodium/aluminum molar ratio exceeding 1 and an amorphous layer addresses thermal expansion issues, enhancing methanol production efficiency by improving permeance ratios and reducing energy consumption.
Patent Information
- Application Number
- JP2023057143
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methanol production processes face challenges in achieving a high permeance ratio for methanol gas to hydrogen gas separation due to thermal expansion differences between porous alumina and zeolite membranes, leading to peeling and reduced permeability.
A zeolite membrane composite is developed with a portion of the sodium/aluminum molar ratio exceeding 1, primarily located near the porous support, incorporating an amorphous layer to alleviate thermal expansion stress and prevent peeling, using a method that includes seeding with a higher amount of seed crystals on the porous support.
The composite achieves a significantly improved methanol gas to hydrogen gas permeance ratio, enabling efficient methanol production at higher temperatures and pressures with reduced energy consumption and equipment constraints.
Smart Images

Figure 2024144949000003 
Figure 2024144949000004 
Figure 2024144949000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a zeolite membrane composite and a method for producing methanol using the same for methanol separation. [Background technology]
[0002] Methods for producing methanol from a gas containing hydrogen and carbon monoxide (hereinafter sometimes referred to as "synthetic gas") have been known for a long time, and examples of such methods include a method using a copper-based catalyst (copper-zinc-based catalyst, copper-chromium-based catalyst). The reaction for producing methanol from synthesis gas is an equilibrium reaction, and the lower the temperature and the higher the pressure, the more favorable it is. However, because the reaction rate decreases at lower temperatures, the general methanol production process is carried out under harsh conditions of 200-300°C and 5-10MPaG (or higher pressure), which consumes a large amount of energy during methanol production and has many equipment restrictions.
[0003] As a method for efficiently producing methanol, several methods have been proposed in which the gas composition in the reactor is shifted from the equilibrium composition by removing methanol from the reaction system, and the reaction is carried out at a conversion rate exceeding the equilibrium conversion rate.
[0004] Furthermore, Patent Documents 1 to 4 propose a method of increasing the conversion rate above the equilibrium conversion rate by installing a separation membrane in a methanol synthesis reactor and removing methanol and water from within the reaction system using the separation membrane. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 9-511509 [Patent Document 2] JP 2016-117726 A [Patent Document 3] JP 2016-174996 A [Patent Document 4] JP 2007-55970 A Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Document 1 describes a perfluorinated polysulfonic acid membrane doped with lithium ions, using methanol as a separation membrane. Patent Document 2 describes a porous graphite membrane, and Patent Document 3 describes a zeolite separation membrane made of MFI type zeolite with a Si / Al ratio of 50 or more. Patent Document 4 describes the prevention of catalyst deterioration by selectively removing water. However, while these methods were sufficient for separating carbon dioxide and methanol, separating hydrogen and methanol was difficult, and the permeance ratio of methanol gas to hydrogen gas was low, making further improvement a challenge. The present inventors have attempted to solve this problem by forming a dense, gap-free film, but have found that even when a sufficiently dense film is created, the permeance ratio is insufficient. Under these circumstances, the inventors of the present invention conducted further research and found that the thermal expansion coefficient of porous alumina at up to 400°C is approximately 7×10 -6 / ℃, whereas MFI zeolite is about 2.4 × 10 -6 / ℃, the difference in thermal expansion coefficients means that separation, which is usually carried out at high temperatures of 200 to 300℃, sometimes causes peeling between the porous alumina support and the zeolite membrane due to the difference in thermal expansion coefficients, making it easier for gases other than methanol gas to permeate, and reducing the permeance ratio. Therefore, an object of the present invention is to provide a zeolite membrane composite having a high methanol gas / hydrogen gas permeance ratio, a method for producing the zeolite membrane composite, and a method for producing methanol using the zeolite membrane composite. [Means for solving the problem]
[0007] As described above, for example, in a composite of porous alumina and MFI type zeolite, the difference in thermal expansion coefficient may occur, which may cause peeling. Since such a difference in thermal expansion cannot be alleviated by a material having an ordered structure such as zeolite, it was found that an amorphous material having an irregular structure should be intentionally introduced, and such a portion can be confirmed by the sodium aluminum ratio. This makes it possible to prevent peeling and improve the permeance ratio of methanol gas / hydrogen gas. A method for obtaining such a zeolite membrane was also found, and the present invention was completed.
[0008] The present invention resides in the following. [1] A zeolite membrane composite having a zeolite membrane on a porous support, the zeolite membrane comprising a site having a sodium / aluminum (molar ratio) of more than 1. [2] The zeolite membrane composite according to the above [1], wherein the site where the sodium / aluminum (molar ratio) exceeds 1 is present within 80% of the zeolite membrane thickness from the upper end of the porous support. [3] The zeolite membrane composite according to the above [1] or [2], wherein the difference between the sodium / aluminum (molar ratio) at 0 to 30% of the zeolite membrane thickness from the upper end of the porous support and the sodium / aluminum (molar ratio) at 50 to 80% of the zeolite membrane thickness from the upper end of the porous support is 0.5 or more. [4] The zeolite membrane composite according to any one of the above [1] to [3], wherein the zeolite is any one of a CHA type, an FAU type, an MFI type, an LTA type, and an RHO type. [5] The zeolite membrane composite according to any one of [1] to [4] above, wherein the sodium / aluminum (molar ratio) is 1.2 or more. [6] The zeolite composite membrane according to any one of [1] to [5] above, wherein the zeolite membrane has a thickness of 0.5 μm or more and 30 μm or less. [7] A method for producing a zeolite membrane composite on a porous support, comprising the steps of: applying seed crystals to the surface of the porous support at a concentration of 0.011 g / cm 2 A method for producing the above-mentioned zeolite membrane composite. [8] A method for producing methanol, comprising reacting a raw material gas containing at least hydrogen, and carbon monoxide and / or carbon dioxide in a reactor in the presence of a catalyst to obtain methanol, wherein the methanol produced by the reaction permeates through the zeolite membrane composite described in any one of [1] to [6] above and is extracted. Effect of the Invention
[0009] According to the present invention, there are provided a zeolite membrane composite having a high methanol gas / hydrogen gas permeance ratio, a method for producing the zeolite membrane composite, and a method for producing methanol using the zeolite membrane composite. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram for explaining a method for measuring the sodium / aluminum (molar ratio) and the membrane thickness of zeolite. [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a method for producing methanol using the zeolite membrane composite of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Representative embodiments for carrying out the present invention will be described in detail below. However, the present invention is not limited to the following embodiments and can be carried out in various modified forms without departing from the gist of the present invention.
[0012] An embodiment of the present invention is a zeolite membrane composite having a zeolite membrane on a porous support, characterized in that the zeolite membrane has a site where the sodium / aluminum (molar ratio) exceeds 1. Normally, zeolites are electrically neutral if all of the T atoms constituting the framework are Si, but for example, zeolites used for ammonia separation have some of the Si substituted with Al. As a result, they are negatively charged, and Na ions are adsorbed for charge compensation. At this time, the ratio of Al in the framework to the adsorbed Na is 1:1 in the case of zeolite, and the sodium / aluminum (molar ratio) does not theoretically exceed 1. However, if there is an amorphous portion that has not been crystallized, the sodium / aluminum (molar ratio) at that portion will be greater than 1. This can be confirmed by SEM-EDS and is characteristic of non-crystallized amorphous regions.
[0013] Such sites where the sodium / aluminum (molar ratio) exceeds 1 relieve stress due to thermal expansion and prevent peeling between the porous substrate and the zeolite membrane, and therefore are preferably located on the porous support side rather than the surface of the zeolite membrane, and are preferably located within 80% of the zeolite membrane thickness from the upper end of the porous support, more preferably within 50%. In the portion where the sodium / aluminum (molar ratio) exceeds 1, the sodium / aluminum (molar ratio) is preferably 1.2 or more, more preferably 1.5 or more, and further preferably 2 or more.
[0014] In addition, as an index showing that a sufficient amorphous layer is present, the area on the porous support side, specifically, 0 to 30% of the zeolite film thickness from the top end of the porous support (hereinafter referred to as "T 0~30 The sodium / aluminum (molar ratio) at the interface between the zeolite membrane and the porous support is 50 to 80% of the zeolite membrane thickness (hereinafter referred to as "T 50~80" represents the surface side from the center of the zeolite membrane.) is preferably 0.5 or more, and more preferably 0.7 or more. That is, T 0~30 T 50~80 This also indicates that an amorphous layer is present on the surface side of the support.
[0015] The sodium / aluminum (molar ratio) can be measured using SEM-EDS. The measurement is carried out at at least five measurement points. It is preferable that all five measurement points do not exceed 1. If all five measurement points are amorphous, this may indicate either a bias in the measurement points or the material is unsuitable as a separation membrane, so it is advisable to change the measurement points and measure again or to confirm the structure by XRD.
[0016] The analysis of such composition is carried out by the standard measuring method used in the analysis of the examples, as described below. (Pretreatment) The zeolite membrane composite was trimmed and polished to make flakes, and then the cross section was processed by ion milling from the porous support side to make it smooth, and Pt was evaporated to give electrical conductivity. (Device) SEM-EDS analysis was carried out using the following equipment: Field emission scanning electron microscope: JSM-7900F (manufactured by JEOL Ltd.) Detector: Secondary electron detector EDS:Ultim Max 170 (manufactured by Oxford) (Measurement conditions) Acceleration voltage: 6 kV Magnification: About 5000x CPS: About 3000 or more Accumulation: 100 seconds Acquisition range: 2~5μm×0.5~2μm
[0017] [Zeolite membrane composite] The zeolite membrane composite of the present invention has a zeolite membrane on a porous support.
[0018] <Porous support> The porous support used in the present invention may be made of various materials, but is preferably an inorganic porous body. Specific examples of the material that can be used include alumina, titania, zirconia, and silica, but is preferably alumina. The pores of the porous support are not particularly limited, so long as macropores are present and do not prevent successful formation of the zeolite membrane, and any commonly used pores may be used.
[0019] <Zeolite membrane> The zeolite constituting the zeolite membrane used in the present invention is not particularly limited as long as it contains aluminum, but it is preferable that the main zeolite constituting the zeolite membrane contains a zeolite having a pore structure with 12 or less oxygen rings and 6 or more oxygen rings. The value of n in the zeolite having n-membered oxygen rings refers to the zeolite with the largest number of oxygen atoms among the pores composed of oxygen and T elements (elements other than oxygen that compose the framework) that form the zeolite framework. For example, when pores with 12-membered oxygen rings and 8-membered oxygen rings exist, such as in MOR-type zeolites, the zeolite is considered to have 12-membered oxygen rings.
[0020] Zeolites having a pore structure with 12 or less oxygen rings and 6 or more oxygen rings include codes defined by the International Zeolite Association (IZA), such as AEI, AEL, AFI, AFG, ANA, ATO, BEA, BRE, CAS, CDO, CHA, CON, DDR, DOH, EAB, EPI, ERI, ESV, EUO, FAR, FAU, FER, FRA, HEU, GIS, GIU, GME, GOO, ITE, KFI, LEV, LIO, LOS, LTA, LTL, LTN, MAR, MEP, MER, MEL, MFI, MON, MOR, MSO, MTF, MTN, MTW, MWW, NON, NES, OFF, PAU, PHI, RHO, RTE, RTH, RUT, SGT, OD, STI, STT, TOL, TON, TSC, UFI, VNI, WEI, and YUG. It is preferable to select one of these. More preferably, it is any of the CHA type, FAU type, MFI type, LTA type, or RHO type, even more preferably, it is the CHA type, MFI type, LTA type, or RHO type, even more preferably, it is the MFI type or RHO type, and most preferably, it is the MFI type.
[0021] The thickness of the zeolite membrane is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more. By making the thickness equal to or greater than the lower limit, the performance as a separation membrane is easily exhibited. The upper limit of the membrane thickness is preferably 30 μm or less, more preferably 20 μm or less, and most preferably 10 μm or less. By making the thickness equal to or greater than the upper limit, damage to the zeolite membrane due to thermal expansion or the like can be prevented, and at the same time, sufficient transmittance can be obtained. The membrane thickness can be easily distinguished by the difference in density between the zeolite part and the support part by SEM, so it can be measured by measuring several average parts by SEM observation. It is sufficient to measure five average places and take the average value, and preferably all five places are within the above range.
[0022] <Method of manufacturing zeolite membrane composite> Next, a method for producing the zeolite membrane composite of the present invention will be described. The method for producing the zeolite membrane composite of the present invention may be a method for producing a zeolite membrane on a commonly used porous body, except that a part of the zeolite membrane is made amorphous, and the method for supporting the zeolite membrane may be a dipping method, a rubbing method, a suction method, an impregnation method, or the like. In this case, it is preferable to use fine crystals called seed crystals. These seed crystals play the role of nuclei when growing the crystals that constitute the zeolite membrane.
[0023] A typical method for providing a site on the porous support of the present invention where the sodium / aluminum (molar ratio) exceeds 1 is to use a larger amount of seed crystals during membrane formation than the range normally used. Specifically, 0.011 g / cm per surface area of the porous support is used. 2 More than 0.013 g / cm 2 More preferably, 0.015 g / cm 2 This allows the seed crystals to be densely packed near the surface of the porous support, resulting in the formation of amorphous portions that absorb sodium from the raw material mixture. The presence of these portions can be confirmed by the sodium / aluminum (molar ratio) exceeding 1.
[0024] The zeolite membrane composite of the present invention relieves stress due to thermal expansion and suppresses peeling and cracking of the zeolite membrane, and therefore exhibits its effects without limiting its applications. However, it is particularly effective when used at temperatures higher than room temperature, and is preferably applied to those used at 70°C or higher. The following description will be given taking as an example the case where the method is applied to a production method of methanol, but the method can also be suitably used for separating ammonia and other substances.
[0025] <Methanol production method> Methanol is produced by reacting synthesis gas as a raw material in the presence of a catalyst. The raw gas is H 2 and CO xIt may contain gases other than H. 2 and CO x Other gases include CH 4 , C 2 H 4 , C 2 H 6 , C 3 H 6 , C 3 H 8 , C 4 H 8 , C 4 H 10 , H 2 O, etc., but H 2 and CO x The content of other gases is usually 50% by volume or less.
[0026] The catalyst used in producing methanol from the raw material gas may be a known catalyst, such as a copper-based catalyst (copper-zinc-based catalyst, copper-chromium-based catalyst), a zinc-based catalyst, a chromium-based catalyst, an aluminum-based catalyst, etc.
[0027] FIG. 2 is a schematic cross-sectional view showing one embodiment of a reactor in which the present invention is carried out. The reactor 10 has a raw material feed inlet a, a permeate gas outlet b, and a non-permeate gas outlet c, and is made of a material that can withstand the high temperature and pressure conditions in which the methanol production reaction takes place. Although there is only one inlet a, outlet b, and outlet c in the figure, there may be multiple inlets a, b, and c. For example, a zeolite membrane composite 1, which is a methanol permselective membrane of the present invention, is placed in a reactor 10.
[0028] The zeolite membrane composite 1 is formed by forming a zeolite membrane on a porous support. The shape of the porous support is not limited to a tubular shape, and may be a columnar shape, a hollow columnar shape, or a hollow honeycomb shape. One end of the zeolite membrane composite 1 is sealed by a cap 2. The other end is connected to a pipe 3. The pipe 3 and the zeolite membrane composite 1, and the cap 2 and the zeolite membrane composite 1 are connected by a bonding material. The method of connecting the zeolite membrane composite is not limited to the above, and for example, both ends may be connected to pipes to allow gas to flow inside.
[0029] A catalyst 13 is arranged around the tubular zeolite membrane composite 1. The raw material gas fed from the feed inlet a comes into contact with the catalyst 13, promoting the production of methanol. The produced methanol then permeates the zeolite membrane of the zeolite membrane composite 1, thereby producing methanol with a higher purity. Furthermore, the selective permeation of methanol through the zeolite composite 1 reduces the methanol concentration in the gas in contact with the catalyst 13, promoting the production of methanol.
[0030] The other end of the pipe 3 is connected to a permeation gas outlet b of the reactor, and transfers methanol that has permeated through the zeolite membrane of the zeolite membrane composite 1 to the permeation gas outlet b. The zeolite membrane composite 1 may be directly connected to the permeation gas outlet b of the reactor without passing through the pipe 3.
[0031] In this embodiment, a zeolite membrane composite formed on a support can be used as the zeolite membrane. The zeolite membrane composite is prepared by, for example, preparing a cylindrical support, and first supporting zeolite microcrystals in the pores. The zeolite can be grown by hydrothermal synthesis, as in the case of zeolite synthesis.
[0032] In this embodiment, a raw material gas containing at least hydrogen and carbon monoxide and / or carbon dioxide is reacted in a reactor in the presence of a catalyst to obtain methanol. The reaction conditions are not particularly limited, but the reaction temperature is preferably 200°C or higher and 300°C or lower. The reaction temperature means the temperature inside the reactor. By setting the reaction temperature at 200°C or higher, the reaction rate increases and the productivity increases. By setting the reaction temperature at 300°C or lower, the chemical equilibrium of the reaction becomes favorable for obtaining methanol, so that the conversion rate can be increased even if the performance of the membrane is somewhat inferior. In addition, the allowable range of heat resistance required for the bonding material is expanded.
[0033] The methanol obtained by the above reaction permeates through a methanol selective permeable membrane in the reactor, and the methanol is recovered from a permeated gas outlet of the reactor. The pressure in the reactor when the produced methanol is permeated through the methanol selective permeable membrane, i.e., the pressure (gauge pressure) on the gas supply side of the methanol selective permeable membrane in the reactor, is preferably 1 MPaG or more, more preferably 2 MPaG or more, and preferably 8 MPaG or less, and more preferably 5 MPaG or less. By setting the pressure within an appropriate range, the equilibrium constraints of the reaction are reduced, and the reaction rate is improved, making it easier to achieve higher productivity. In addition, the increase in the manufacturing cost of the reactor and the cost of pressurizing the raw material gas due to excessive pressure can be suppressed. In addition, in the reaction vessel, the methanol partial pressure (absolute pressure) on the gas supply side of the methanol selective permeable membrane is preferably 0.1 MPaA or more, more preferably 0.2 MPaA or more, and preferably 6 MPaA or less, and more preferably 5 MPaA or less. By setting the methanol partial pressure within this range, a sufficient amount of methanol can be obtained to permeate the membrane, and the effect of the membrane can be fully exerted. On the other hand, within this range, the durability and sealing property required for the joint do not become higher than necessary, and jointing can be easily performed in large quantities. The gauge pressure in the reactor can be measured by a pressure gauge installed in the reactor. The absolute pressure of methanol in the reactor changes from the upstream to the downstream of the reactor, but here, the absolute pressure of methanol in the reactor is calculated from the analysis result of the gas composition at the reactor outlet by gas chromatography and the gauge pressure. EXAMPLES
[0034] The present invention will be described in more detail below with reference to examples. However, it goes without saying that the scope of the present invention is not limited to the embodiments shown in the following examples.
[0035] (SEM-EDX measurement position) The measurement conditions for SEM-EDX are as described above, but the method for determining the film thickness and measurement position will be explained using Figure 1. Figure 1 is a 5000x SEM image, and since large particles (alumina particles in this case) are visible in the porous support, the bottom end of the zeolite membrane can be easily identified. The thickness up to the top end is the film thickness. The film thickness can be obtained by measuring about five locations with an average film thickness. In addition, the sodium to aluminum ratio can be measured at about five arbitrary locations to check whether there are any locations where this ratio exceeds 1. It is advisable to measure about five locations in the same manner to see whether or not the area where the sodium / aluminum (molar ratio) exceeds 1 is present within 80% of the zeolite membrane thickness from the upper end of the porous support. The method for determining the measurement locations is explained below.
[0036] The measurement site is, for example, the area indicated by the white square in Figure 1, and the relative position can be determined by taking an SEM photograph. The distance between the top and bottom ends of the zeolite in the white square in Figure 1 was measured to be 3.6 μm. Meanwhile, the distance from the bottom end to the top end of the white square was 2.3 μm, and the distance to the bottom end was 1.8 μm. Top: (2.3 / 3.6)*100=63% Bottom: (1.8 / 3.6)*100=50% Therefore, the measurement was performed at 50-63% of the membrane. Similar measurements were performed at 5 locations, and the difference between the sodium / aluminum (molar ratio) at 0-30% from the top of the porous support and the sodium / aluminum (molar ratio) at 50-80% from the top of the porous support could be calculated using the location with the highest sodium / aluminum ratio.
[0037] <Example 1> (Raw material mixture for hydrothermal synthesis) 2.8 g of 97% by mass sodium hydroxide (granular, manufactured by Hayashi Pure Chemical Industries, Ltd.) and 154.3 g of demineralized water were mixed and added to sodium aluminate (Al 2 O 3 0.17 g of colloidal silica (Nissan Chemical Industries, Ltd., Snowtex 40) was added and stirred at 50° C. for 30 minutes. 19.4 g of colloidal silica was added and stirred at 50° C. for 4 hours to obtain a raw material mixture for hydrothermal synthesis. The composition (molar ratio) of this raw material mixture for hydrothermal synthesis was SiO 2 / Al 2 O 3 / NaOH / H 2 O=1 / 0.008 / 0.54 / 70.
[0038] (Porous support) The porous support used was an 8 cm alumina tube (outer diameter 12 mm, inner diameter 9 mm) manufactured by Iwao Porcelain Industry Co., Ltd., which had been washed by flowing desalted water and then dried.
[0039] (Seed crystal dispersion) MFI type zeolite was ground in a mortar, and seed crystals were dispersed in the ground zeolite so that the seed crystal concentration was 0.15% by mass, to prepare a seed crystal dispersion.
[0040] (Production of Zeolite Membrane Composite) The porous support was immersed in the above-mentioned seed crystal dispersion for 60 seconds, and then dried at room temperature for 30 minutes and at 70° C. for 30 minutes to attach the seed crystals to the porous support. The mass of the attached seed crystals was about 0.0045 g, and the ratio of the surface area of the porous support to the seed crystals was 0.015 g / cm. 2By this method, three porous supports with seed crystals attached were prepared. The three porous supports with the seed crystals attached were immersed vertically in the Teflon (registered trademark) inner cylinder containing the above-mentioned hydrothermal synthesis raw material mixture, the autoclave was sealed, and the temperature was raised to 180°C in a thermostatic chamber over 5 hours, and then the mixture was heated under autogenous pressure for 15 hours in a stationary state. After a predetermined time had passed, the porous support-zeolite membrane composite was taken out of the reaction mixture after cooling, washed, and desalted water was added again, and the mixture was heated in an autoclave at 120°C for 20 hours. After a predetermined time had passed, the porous support-zeolite membrane composite was taken out of the desalted water after cooling, and dried at 100°C for 3 hours to obtain an MFI type zeolite membrane composite 1. The mass of the zeolite membrane on the porous support was 0.11 g. The air permeability of the zeolite membrane composite 1 at 50 Torr was 0 cm 3 The results are shown in Table 1. The results of SEM-EDX analysis of this zeolite membrane composite are shown in Table 2.
[0041] <Comparative Example 1> (Raw material mixture for hydrothermal synthesis) 2.8 g of 97% by mass sodium hydroxide (granular, manufactured by Hayashi Pure Chemical Industries, Ltd.) and 154.3 g of demineralized water were mixed and added to sodium aluminate (Al 2 O 3 0.17 g of colloidal silica (Nissan Chemical Industries, Ltd., Snowtex 40) was added and stirred at 50° C. for 30 minutes. 19.4 g of colloidal silica was added and stirred at 50° C. for 4 hours to obtain a raw material mixture for hydrothermal synthesis. The composition (molar ratio) of this raw material mixture for hydrothermal synthesis was SiO 2 / Al 2 O 3 / NaOH / H 2 O=1 / 0.008 / 0.54 / 70.
[0042] (Porous support) The porous support used was an 8 cm alumina tube (outer diameter 12 mm, inner diameter 9 mm) manufactured by Iwao Porcelain Industry Co., Ltd., which had been washed by flowing desalted water and then dried.
[0043] (Seed crystal dispersion) MFI type zeolite was ground in a mortar, and seed crystals were dispersed in the ground zeolite so that the seed crystal concentration was 0.15% by mass, to prepare a seed crystal dispersion.
[0044] (Production of Zeolite Membrane Composite) The porous support was immersed in the above-mentioned seed crystal dispersion for 10 seconds, and then dried at room temperature for 30 minutes and at 70° C. for 30 minutes to attach the seed crystals to the porous support. The mass of the attached seed crystals was about 0.0030 g, and the ratio of the surface area of the porous support to the seed crystals was 0.010 g / cm. 2 By this method, three porous supports with seed crystals attached were prepared. The three porous supports with the seed crystals attached were immersed vertically in the Teflon (registered trademark) inner cylinder containing the above-mentioned hydrothermal synthesis raw material mixture, the autoclave was sealed, and the temperature was raised to 180°C in a thermostatic chamber over 5 hours, and then the mixture was left to stand for 15 hours and heated under autogenous pressure. After a predetermined time had passed, the porous support-zeolite membrane composite was taken out of the reaction mixture after cooling, washed, and desalted water was added again, and the mixture was heated in an autoclave at 120°C for 20 hours. After a predetermined time had passed, the porous support-zeolite membrane composite was taken out of the desalted water after cooling, and dried at 100°C for 3 hours to obtain an MFI type zeolite membrane composite 2. The mass of the zeolite membrane on the porous support was 0.12 g. The air permeability of the zeolite membrane composite 2 at 50 Torr was 0 cm 3 The results are shown in Table 1. The results of SEM-EDX analysis of this zeolite membrane composite are shown in Table 2.
[0045] [Table 1]
[0046] [Table 2]
[0047] As described above, the zeolite composite of Example 1 having a portion where Na / Al exceeds 1 was able to obtain a remarkable effect of improving the permeance ratio of methanol to hydrogen by about three times. It can be seen that the portion where the sodium / aluminum (molar ratio) exceeds 1 is in the range of 50% from the bottom end. It can also be confirmed that the difference between the sodium / aluminum (molar ratio) at 0-30% from the top end of the porous support and the sodium / aluminum (molar ratio) at 50-80% is 0.5 or more. The difference between the sodium / aluminum (molar ratio) at 0-30% and the sodium / aluminum (molar ratio) at 50-80% can be obtained by measuring five points for each and subtracting the minimum value of the sodium / aluminum (molar ratio) at 50-80% from the maximum value of the sodium / aluminum (molar ratio) at 0-30%, but this may be omitted when it is not necessary to measure five points as in this embodiment. The fact that there are areas where the difference in the sodium / aluminum ratio is large indicates the presence of amorphous buffer areas against thermal expansion, and the areas of spectra 3 to 5 in Example 1 also indicate the presence of parts of a regular zeolite membrane. [Industrial Applicability]
[0048] It has been clarified that the use of the zeolite membrane composite of the present invention can provide a high methanol gas / hydrogen gas permeance ratio at high temperature and pressure in the presence of methanol vapor during methanol production. The principle by which such high permeance is obtained is also applicable to other reactions, so that the present invention can be applied to various reactions requiring separation. As a zeolite separation membrane capable of providing high permeance, this technology is of great industrial value. [Explanation of symbols]
[0049] 1 Zeolite membrane composite 2 Cap 3 Piping 10. Reactor 13. Catalyst
Claims
1. A zeolite membrane composite having a zeolite membrane on a porous support, the zeolite membrane comprising a site having a sodium / aluminum (molar ratio) of more than 1.
2. 2. The zeolite composite membrane according to claim 1, wherein the site where the sodium / aluminum (molar ratio) exceeds 1 is present within 80% of the zeolite membrane thickness from the upper end of the porous support.
3. 3. The zeolite membrane composite according to claim 1, wherein a difference between a sodium / aluminum (molar ratio) at 0 to 30% of the zeolite membrane thickness from the upper end of the porous support and a sodium / aluminum (molar ratio) at 50 to 80% of the zeolite membrane thickness from the upper end of the porous support is 0.5 or more.
4. 3. The zeolite composite membrane according to claim 1, wherein the zeolite is any one of a CHA type, a FAU type, a MFI type, a LTA type, and a RHO type.
5. 3. The zeolite membrane composite according to claim 1, wherein the sodium / aluminum (molar ratio) is 1.2 or more.
6. 3. The zeolite composite membrane according to claim 1, wherein the thickness of the zeolite membrane is from 0.5 μm to 30 μm.
7. A method for producing a zeolite membrane composite by forming a zeolite membrane on a porous support, the method comprising the steps of: applying seed crystals to the surface of the porous support at a concentration of 0.011 g / cm 2 A method for producing the above-mentioned zeolite membrane composite.
8. A method for producing methanol, comprising reacting a raw material gas containing at least hydrogen and carbon monoxide and / or carbon dioxide in a reactor in the presence of a catalyst to obtain methanol, comprising the steps of:
3. A method for producing methanol, comprising the steps of: permeating methanol produced by a reaction through the zeolite membrane composite according to claim 1 or 2 and extracting the methanol.
Citation Information
Patent Citations
Catalytic device for methanol synthesis and method for synthesizing methanol
JP2001009265A
Method and apparatus for synthesizing zeolite membrane
JP2004099338A
Manufacturing method of zeolite membrane
JP2006159031A
Manufacturing method of p-xylene
JP2016098205A
Zeolite separation membrane and separation module
JP2016174996A
Cited By
To provide a method for synthesizing a methanol aqueous solution and an apparatus for producing a methanol aqueous solution.
JP2026091052A
A method for synthesizing an aqueous methanol solution, and an apparatus for producing an aqueous methanol solution.
JP7954909B2
Method for synthesizing aqueous methanol solution and apparatus for producing aqueous methanol solution
WO2026110661A1