Dope-dyed liquid crystal polyester filament
A liquid crystal polyester filament with controlled pigment concentration and specific structural units addresses the dyeability issue, providing high strength and modulus while ensuring good design visibility in acoustic filters.
Patent Information
- Application Number
- JP2023057260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Liquid crystal polyester fibers are difficult to dye or color, limiting their use in applications requiring both high mechanical properties and design visibility, such as acoustic filters, due to restrictions on fineness, strength, and elongation caused by composite spinning methods.
A liquid crystal polyester filament with a pigment concentration of 0.1 to 5.0% by weight, composed of three or more structural units, including components that maintain appropriate crystallinity and linearity, allowing for high strength, elastic modulus, and effective coloring without compromising fluidity and orientation.
The filament achieves high mechanical properties with sufficient coloration, enabling its use in visible acoustic filters that require both durability and aesthetic appeal.
Smart Images

Figure 2024145033000001 
Figure 2024145033000002 
Figure 2024145033000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a liquid crystal polyester filament having high strength and high elastic modulus. [Background technology]
[0002] Electrical and electronic products such as mobile phones, smartphones, cordless phones, portable media players, portable game devices, digital cameras, and digital video cameras (hereinafter referred to simply as "electrical products", but the concept is used to include electronic products as well) have sound receiving and producing units such as microphones and speakers in their housing structures, with openings provided in the corresponding positions and sound being transmitted through these openings.
[0003] As typified by the spread of smartphones, these electrical appliances are increasingly being used not only indoors but also outdoors, making it desirable for them to have a dust-proof structure. On the other hand, as electrical appliances become more compact and more powerful, openings in the appliances also become smaller, and there is a demand to ensure sound permeability (breathability).
[0004] Conventionally, an acoustic filter made of mesh is attached to the openings of the sound generating section and the sound receiving section in order to ensure dust protection and sound permeability. Acoustic filters are required to have both high dust protection and sound permeability as electrical products become more sophisticated and compact, and the mesh is becoming thinner and finer while maintaining the uniformity of the openings. For this reason, the filaments that make up the filters are required to be finer, stronger, and have a higher elasticity.
[0005] Generally, these acoustic filters use polyester fibers, polyamide fibers, metal fibers, etc. Among polyesters, liquid crystal polyester is a polymer consisting of rigid molecular chains, and it is known that the molecular chains are highly oriented in the fiber axis direction during melt spinning, and by further performing heat treatment (solid-state polymerization), the highest strength and elastic modulus can be obtained among fibers obtained by melt spinning, making it a polymer that is truly suitable for acoustic filters.
[0006] On the other hand, since the acoustic filters used in electrical appliances are directly visible to the consumer, they need to be colored from a design perspective, and there is a growing demand for colored filters that use liquid crystal polyester.
[0007] As a colored liquid crystal polyester, Patent Document 1 proposes a composite fiber having a core-sheath structure in which the sheath component is colored. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 3-127225 [Non-patent literature]
[0009] [Non-Patent Document 1] "Modification of Liquid Crystal Polymers and the Latest Application Technology" edited by the Technical Information Association (2006) (pages 235-256) Summary of the Invention [Problem to be solved by the invention]
[0010] Although the liquid crystal polyester fiber has high mechanical properties such as high strength, high elastic modulus, and fineness, its use in applications requiring design and visibility that are directly visible to the consumer has been limited because it is difficult to dye or color it. In recent years, there has been a demand for the development of colored high strength and high elastic modulus fibers for applications such as acoustic filters that require design and advanced features. In Patent Document 1, a fiber is made to have a core-sheath structure, with the core component being liquid crystal polyester and the sheath component being aromatic polyester containing a pigment, thereby obtaining a colored fiber that has high strength and high elastic modulus. However, this method requires composite spinning of the liquid crystal polyester, and there are significant restrictions on physical properties such as fineness, strength, and elongation for cross-sectional formation and color development. In addition, since only the sheath component contains a pigment, the fluidity, orientation, and crystallinity of the polymer of only the sheath component deteriorates, resulting in differences in fluidity, orientation, and crystallinity with the core component, liquid crystal polyester, which undergoes significant orientation and crystallization the moment it comes out of the nozzle during spinning, is likely to cause deterioration in operability. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention has the following configuration: That is, the present invention is a liquid crystal polyester filament characterized in that the pigment concentration is 0.1 to 5.0% by weight.
[0012] Furthermore, the present invention preferably relates to a single-component liquid crystal polyester filament having a pigment concentration of 0.1 to 5.0% by weight.
[0013] Furthermore, the present invention preferably relates to a liquid crystal polyester filament made of a liquid crystal polyester having a pigment concentration of 0.1 to 5.0% by weight and having three or more structural units.
[0014] Furthermore, the present invention is preferably a single-component liquid crystal polyester filament made of a liquid crystal polyester having a pigment concentration of 0.1 to 5.0% by weight and having three or more component structural units.
[0015] Furthermore, the present invention preferably relates to a liquid crystal polyester filament having a color tone L value of 40 or less, a strength of 5.0 to 20.0 cN / dtex, an elongation of 1.5 to 4.5%, and an elastic modulus of 600 to 900 cN / dtex.
[0016] Furthermore, the present invention preferably relates to a liquid crystal polyester filament characterized in that the pigment is carbon black. Effect of the Invention
[0017] The liquid crystal polyester filament of the present invention has high mechanical properties such as high strength and high elastic modulus, and is also colored, so it can be suitably used in applications such as acoustic filters that are visible to consumers and require design and visibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The method for producing the liquid crystal polyester filament of the present invention will be described in detail below.
[0019] The liquid crystal polyester used in the present invention is a polyester that can form an anisotropic molten phase, i.e., liquid crystallinity, when melted. This property can be confirmed, for example, by placing a sample made of liquid crystal polyester on a hot stage, heating it under a nitrogen atmosphere, and observing the transmitted light of the sample under polarized light.
[0020] Examples of the liquid crystal polyesters used in the present invention include (1) polymers of aromatic oxycarboxylic acids, (2) polymers of aromatic dicarboxylic acids and aromatic diols or aliphatic diols, and (3) copolymers of the above (1) and (2). For high strength, high elastic modulus, and high heat resistance, fully aromatic polyesters that do not use aliphatic diols are preferred. Examples of the aromatic oxycarboxylic acids include hydroxybenzoic acid, hydroxynaphthoic acid, and the like, and alkyl, alkoxy, and halogen-substituted products of the above aromatic oxycarboxylic acids.
[0021] Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, diphenyldicarboxylic acid, naphthalenedicarboxylic acid, diphenyletherdicarboxylic acid, diphenoxyethanedicarboxylic acid, diphenylethanedicarboxylic acid, and the like, as well as alkyl, alkoxy, and halogen-substituted derivatives of the above aromatic dicarboxylic acids.
[0022] Further, examples of the aromatic diol include hydroquinone, resorcinol, dioxydiphenyl, naphthalenediol, etc., and alkyl, alkoxy, and halogen-substituted derivatives of the above aromatic diols, and examples of the aliphatic diol include ethylene glycol, propylene glycol, butanediol, and neopentyl glycol.
[0023] As the liquid crystal polyester used in the present invention, copolymers of p-hydroxybenzoic acid component, 4,4'-dihydroxybiphenyl component, hydroquinone component, terephthalic acid component and / or isophthalic acid component, copolymers of p-hydroxybenzoic acid component and 6-hydroxy 2-naphthoic acid component, copolymers of p-hydroxybenzoic acid component, 6-hydroxy 2-naphthoic acid component, hydroquinone component and terephthalic acid component, etc. are mentioned as preferred examples because they have excellent spinnability, can achieve high strength and high elastic modulus, and can improve abrasion resistance by performing high temperature heat treatment after solid phase polymerization.
[0024] In the present invention, the liquid crystal polyester is particularly preferably composed of the following structural units (I), (II), (III), (IV) and (V). In the present invention, the structural unit refers to a unit that can constitute a repeating structure in the main chain of the polymer.
[0025] [ka]
[0026] This combination gives the molecular chains suitable crystallinity and nonlinearity, i.e., a melting point suitable for melt spinning. Therefore, at a spinning temperature set between the melting point and the thermal decomposition temperature of the polymer, the polymer has good spinnability, and a uniform fiber can be obtained in the longitudinal direction. In addition, the fiber has suitable crystallinity, which increases the strength and elastic modulus of the fiber.
[0027] Furthermore, it is important to combine components consisting of diols with high linearity and no bulkiness, such as structural units (II) and (III). By combining these components, the molecular chains in the fiber have an orderly structure with little disorder, and the crystallinity is not excessively increased, and the interaction perpendicular to the fiber axis can be maintained. This not only results in high strength and elastic modulus, but also provides particularly excellent abrasion resistance by performing high-temperature heat treatment after solid-state polymerization. Furthermore, if the polymer does not have components such as structural units (II) and (III) and is too expensive, the crystal structure will be disturbed by the inclusion of pigments, etc., and the interaction perpendicular to the fiber axis will not be maintained, and the strength and elastic modulus will tend to decrease. On the other hand, by having components such as structural units (II) and (III), pigments can be included in the non-crystalline part without disturbing the polymer structure, and in addition to obtaining high strength and elastic modulus, a polymer with excellent colorability in the original dye can be obtained.
[0028] The above structural unit (I) is preferably 40 to 85 mol %, more preferably 65 to 80 mol %, and even more preferably 68 to 75 mol % of the total of the structural units (I), (II) and (III). By setting it in such a range, the crystallinity can be set in an appropriate range, high strength and elastic modulus can be obtained, and the melting point can be in a range that allows melt spinning.
[0029] The structural unit (II) is preferably 60 to 90 mol % based on the total of the structural units (II) and (III), more preferably 60 to 80 mol %, and further preferably 65 to 75 mol %. By setting it in such a range, the crystallinity is not excessively increased and the interaction in the direction perpendicular to the fiber axis can be maintained, so that the wear resistance can be improved by performing a high-temperature heat treatment after solid-state polymerization.
[0030] The structural unit (IV) is preferably 40 to 95 mol % based on the total of the structural units (IV) and (V), more preferably 50 to 90 mol %, and even more preferably 60 to 85 mol %. By setting it in such a range, the melting point of the polymer is in an appropriate range, and since it has good spinnability at a spinning temperature set between the melting point of the polymer and the thermal decomposition temperature, a uniform fiber in the longitudinal direction can be obtained. In addition, since the linearity of the polymer is moderately disturbed, the fibril structure is easily disturbed by high-temperature heat treatment after solid-state polymerization, and the interaction in the direction perpendicular to the fiber axis is enhanced, and the abrasion resistance can be improved. Furthermore, by setting the structural units (IV) and (V) in such a range, a pigment enters the part where the linearity of the polymer is disturbed, and a polymer excellent in spinnability, abrasion resistance, and colorability can be obtained.
[0031] As described above, by using structural units of three or more components, it is possible to obtain a polymer with appropriate crystallinity and polymer linearity, and to obtain a dyed fiber with excellent strength and elastic modulus.
[0032] The preferred ranges of each structural unit of the liquid crystal polyester used in the present invention are as follows: The total of the following structural units (I) to (V) is 100 mol %. By adjusting the composition within this range, the liquid crystal polyester fiber of the present invention can be suitably obtained. Structural unit (I) 45 to 65 mol% Structural unit (II) 12 to 18 mol% Structural unit (III) 3 to 10 mol% Structural unit (IV) 5 to 20 mol% Structural unit (V) 2 to 15 mol% Furthermore, the total amount of the structural units (IV) and (V) and the total amount of the structural units (II) and (III) are preferably substantially equimolar.
[0033] In addition to the above-mentioned monomers, the liquid crystal polyester used in the present invention may further be copolymerized with other monomers within a range that does not impair the liquid crystallinity.
[0034] In addition, other polymers can be added or used in combination with the liquid crystal polyester used in the present invention within a range that does not impair the effects of the present invention. Addition or use in combination refers to the case where polymers are mixed together, or in the case of conjugate spinning of two or more components, other polymers are mixed partially or entirely with one or more components. When a polymer is added or used in combination, it is preferable that the melting point of the polymer is within ±30°C of the melting point of the liquid crystal polyester in order not to impair spinnability. In order to improve the strength and elastic modulus of the obtained fiber and to suppress the generation of fluff and thread breakage due to peeling at the polymer interface, the amount of the polymer added or used in combination is preferably 50% by weight or less, more preferably 5% by weight or less, and most preferably, no other polymer is substantially added or used in combination.
[0035] The liquid crystal polyester used in the present invention may contain small amounts of various additives such as inorganic substances such as various metal oxides, kaolin, and silica, colorants, matting agents, flame retardants, antioxidants, ultraviolet absorbers, infrared absorbers, crystal nucleating agents, fluorescent brighteners, end group capping agents, and compatibilizers, within the range in which the effects of the present invention are not impaired.
[0036] The polystyrene-equivalent weight average molecular weight (hereinafter referred to as molecular weight) of the liquid crystal polyester used in the present invention is preferably 30,000 or more. By setting the molecular weight to 30,000 or more, it is possible to have an appropriate viscosity at the spinning temperature and improve spinnability. The higher the molecular weight, the higher the strength, elongation, and elastic modulus of the obtained fiber. However, if the molecular weight is too high, the viscosity increases and the fluidity deteriorates, and finally the fiber does not flow at all, so the molecular weight is preferably less than 250,000, and more preferably less than 200,000. The polystyrene-equivalent weight average molecular weight referred to here refers to a value measured by the method described in the Examples.
[0037] The melting point of the liquid crystal polyester used in the present invention is preferably 200 to 380° C. in order to broaden the melt-spinnable temperature range, and more preferably 250 to 360° C. in order to improve spinnability. The melting point of the liquid crystal polyester polymer refers to a value measured by the method described in the examples.
[0038] The method for obtaining the liquid crystal polyester filament of the present invention having a pigment concentration of 0.1 to 5.0% by weight is not limited in any way, but the important point is that in the production of the liquid crystal polyester filament, a liquid crystal polyester containing a pigment is used during melt spinning.
[0039] The pigment concentration of the liquid crystal polyester filament of the present invention is preferably 0.1 to 5.0% by weight. When the pigment concentration is 0.5% by weight or more, sufficient coloring is obtained, and when it is 5.0% by weight or less, sufficient strength and elastic modulus for use as a filter or the like are obtained. More preferably, it is 0.5 to 3.0% by weight. As the pigment to be used, either an organic compound pigment or an inorganic compound pigment can be used. Specifically, as the organic colorant, azo colorant, anthraquinone-based, or isoindoline-based condensed polycyclic colorant can be mentioned, and as the inorganic colorant, carbon black (hereinafter, CB), cadmium-based, titanium-based, or lead-based colorant can be mentioned. Conventionally known pigments that disperse well in molten liquid crystal polyester, can be colored at the melt spinning stage, and have excellent heat resistance can be used, and may be selected according to the desired color. Generally, black is preferred as an acoustic filter, so carbon black (hereinafter, CB) is preferred as the pigment to be used in the present invention. When CB is used as a pigment, the preferred particle size is 10 to 200 nm from the viewpoint of dispersibility and colorability.
[0040] It is preferable to use a known method for incorporating the pigment into the liquid crystal polyester. A method can be used in which the desired content is kneaded in advance in a previous process (melt-kneading process), then chipped and melt-spun, but the entire liquid crystal polyester is subjected to excessive heat history, and a decrease in strength is inevitable. Therefore, a method can be preferably used in which chips containing pigment far exceeding the desired content and chips containing no pigment at all are weighed by a gravimetric or volumetric method, and a certain amount is mixed uniformly using a mixing layer equipped with a stirrer to be melt-spun.
[0041] In the melt spinning, the liquid crystal polyester can be melt extruded by a known method, but it is preferable to use an extruder-type extruder in order to eliminate the ordered structure generated during polymerization. The extruded polymer is metered by a known metering device such as a gear pump through a pipe, and is led to a spinneret after passing through a filter to remove foreign matter. At this time, the temperature (spinning temperature) from the polymer pipe to the spinneret is preferably set to the melting point of the liquid crystal polyester or higher in order to increase the fluidity, and more preferably to the melting point of the liquid crystal polyester + 10°C or higher. However, if the spinning temperature is excessively high, the viscosity of the liquid crystal polyester increases, leading to deterioration of the fluidity and deterioration of the spinnability, so it is preferably set to 500°C or lower, and more preferably to 400°C or lower. It is also possible to independently adjust the temperatures from the polymer pipe to the spinneret. In this case, the discharge is stabilized by making the temperature of the part close to the spinneret higher than the temperature on the upstream side.
[0042] In the present invention, depending on the spinneret used during spinning, it is possible to make either monofilament or multifilament, and it is sufficient to use a spinneret that corresponds to the desired filament shape. In addition, in the present invention, depending on the spinneret used during spinning, it is possible to make either single-component fiber or composite fiber, and it is sufficient to use a spinneret that can obtain a cross section according to the desired filament shape. On the other hand, by using a polymer having three or more structural units, the filament of the present invention achieves sufficient mechanical properties (strength, elastic modulus) and coloring with a pigment without forming a composite fiber, and unless there is a special reason, it is desirable to use a spinneret that can obtain a single component with stable cross-sectional formation. On the other hand, the present invention does not prohibit the formation of a composite fiber according to the characteristics required depending on the application, such as using a composite fiber consisting of a sheath component that does not contain a pigment and a core component that contains a pigment for applications where abrasion resistance is important.
[0043] The polymer discharged from the nozzle hole is passed through a heat-retaining and cooling region to solidify, and then taken up by a roller (godet roller) rotating at a constant speed. If the heat-retaining region is too long, spinnability deteriorates, so it is preferably up to 200 mm from the nozzle surface, and more preferably up to 100 mm. The heat-retaining region can also be heated using a heating means, and the temperature range is preferably 100°C to 500°C, and more preferably 200°C to 400°C. Inert gas, air, steam, etc. can be used for cooling, but it is preferable to use a parallel or annular air flow in order to reduce the environmental load.
[0044] The take-up speed is preferably 50 m / min or more, more preferably 500 m / min or more, from the viewpoint of productivity and reduction of single fiber fineness. The liquid crystal polyester given as a preferred example in the present invention has suitable spinnability at the spinning temperature, so that the take-up speed can be made high, and although there is no particular upper limit, it is about 2000 m / min from the viewpoint of spinnability.
[0045] In melt spinning, it is preferable to apply an oil during the period from cooling and solidifying the polymer to winding in order to improve the handleability of the fiber. Any known oil can be used, but it is preferable to use a general spinning oil or a solid-state polymerization oil described below in order to improve the unwinding property when unwinding the fiber obtained by melt spinning (hereinafter referred to as the raw spun yarn) in the rewinding step before solid-state polymerization.
[0046] The winding can be performed using a known winding machine to produce packages in the form of pirns, cheeses, cones, etc., but winding into pirns, in which the rollers do not come into contact with the package surface during winding, is preferred in that it does not apply frictional forces to the fibers and cause them to fibrillate.
[0047] In the present invention, it is preferable to apply a solid-phase polymerization oil agent to the liquid crystal polyester fiber and then perform solid-phase polymerization. The solid-phase polymerization oil agent referred to in the present invention is an oil agent that suppresses fusion between fibers when the oil agent is attached to the liquid crystal polyester fiber and solid-phase polymerized, and a known one can be used, but from the viewpoint of suppressing fusion and easy cleaning, it is preferable to use a mixture of inorganic particles (A) and a phosphoric acid compound (B). In the present invention, even if it does not contain oil, such as a mixture of inorganic particles (A) and a phosphoric acid compound (B), it is also referred to as a solid-phase polymerization oil agent.
[0048] The inorganic particles (A) in the present invention are known inorganic particles, examples of which include minerals, metal hydroxides such as magnesium hydroxide, metal oxides such as silica and alumina, carbonate compounds such as calcium carbonate and barium carbonate, sulfate compounds such as calcium sulfate and barium sulfate, and CB, etc. By applying such highly heat-resistant inorganic particles onto fibers, the contact area between single fibers can be reduced, making it possible to prevent fusion that occurs during solid-state polymerization.
[0049] The inorganic particles (A) are preferably easy to handle in consideration of the coating process, are easily dispersed in water in consideration of reducing the environmental load, and are desirably inactive under solid-phase polymerization conditions. From these viewpoints, it is preferable to use silica or silicate. In the case of silicate, phyllosilicates having a layered structure are particularly preferable. Examples of phyllosilicates include kaolinite, halloyite, serpentine, garnierite, smectite, pyrophyllite, talc, and mica. Among these, it is most preferable to use talc and mica in consideration of ease of availability.
[0050] The phosphoric acid compound (B) in the present invention may be any of the compounds represented by the following chemical formulas (1) to (3).
[0051] [ka]
[0052] Here, R1 and R2 are hydrocarbons, M1 is an alkali metal, and M2 is an alkali metal, hydrogen, a hydrocarbon, or an oxygen-containing hydrocarbon.
[0053] Here, n represents an integer of 1 or more. From the viewpoint of suppressing thermal decomposition, the upper limit of n is preferably 100 or less, and more preferably 10 or less.
[0054] Considering the gas generated by thermal decomposition during solid-state polymerization, and from the viewpoint of reducing the environmental load, R1 preferably does not contain a phenyl group in the structure, and is more preferably composed of an alkyl group. The carbon number of R1 is preferably 2 or more from the viewpoint of affinity with the fiber surface, and is preferably 20 or less from the viewpoint of suppressing the weight loss rate due to the decomposition of organic components accompanying solid-state polymerization and preventing carbon generated by decomposition during solid-state polymerization from remaining on the fiber surface.
[0055] From the viewpoint of solubility in water, R2 is preferably a hydrocarbon having 5 or less carbon atoms, more preferably 2 or 3 carbon atoms. From the viewpoint of production costs, M1 is preferably sodium or potassium.
[0056] In order to apply the inorganic particles (A) and the phosphoric acid compound (B) uniformly while optimizing the amount of adhesion, it is preferable to use a mixed oil agent in which the inorganic particles (A) are added to a dilution of the phosphoric acid compound (B), and it is preferable to use water as the dilution agent from the viewpoint of safety. From the viewpoint of suppressing fusion, the concentration of the inorganic particles (A) in the dilution agent is desirably high, 0.01% by weight or more, more preferably 0.1% by weight or more, and the upper limit is preferably 10% by weight or less, more preferably 5% by weight or less, from the viewpoint of uniform dispersion. From the viewpoint of uniform dispersion of the inorganic particles (A), the concentration of the phosphoric acid compound (B) is desirably high, 0.1% by weight or more, more preferably 1.0% by weight or more. There is no particular restriction on the upper limit of the concentration of the phosphoric acid compound (B), but in order to avoid excessive adhesion due to an increase in the viscosity of the mixed oil agent and uneven adhesion due to an increase in the temperature dependency of the viscosity, it is preferably 50% by weight or less, more preferably 30% by weight or less.
[0057] The inorganic particles (A) and the phosphoric acid compound (B) may be applied to the fibers between melt spinning and winding. In order to increase the efficiency of application, however, it is preferable to apply the inorganic particles (A) and the phosphoric acid compound (B) to the yarn while rewinding the yarn that has been melt spun and wound, or to apply a small amount of the inorganic particles (A) and the phosphoric acid compound (B) to the yarn while rewinding the wound yarn.
[0058] The application method may be a guide oiling method, but in order to apply the oil evenly to fibers with a fine total fineness, it is preferable to apply the oil using a metal or ceramic kiss roll (oiling roll).If the fibers are in a reel or tow shape, they can be applied by immersing them in the mixed oil.
[0059] The adhesion rates of the inorganic particles (A) and the phosphoric acid compound (B) to the fibers are not particularly limited as long as they can prevent fusion between fibers during solid-phase polymerization. When the adhesion rate of the inorganic particles (A) is (a) weight % and the adhesion rate of the phosphoric acid compound (B) is (b) weight %, the adhesion rate (a) of the inorganic particles (A) is preferably 0.01 weight % or more to obtain the effect of suppressing fusion by the inorganic particles. The upper limit of the adhesion rate (a) is preferably 10 weight % or less from the viewpoint of uniform adhesion. The adhesion rate (b) of the phosphoric acid compound (B) is preferably 10 weight % or more, more preferably 15 weight % or more, and even more preferably 20 weight % or more. The upper limit is preferably less than 40 weight % from the viewpoint of uneven adhesion in the fiber longitudinal direction and handling.
[0060] The oil adhesion rate (a+b) of the solid-phase polymerization oil exceeds 10% by weight, but by carrying out solid-phase polymerization with a large amount of oil that exceeds 10% by weight, a high suppression effect against fiber fusion during solid-phase polymerization can be obtained. The higher the oil adhesion rate (a+b) of the solid-phase polymerization oil, the higher the effect of suppressing fusion, so the oil adhesion rate is preferably more than 15% by weight, and more preferably more than 20% by weight. On the other hand, the upper limit is preferably 40% by weight or less from the viewpoint of suppressing adhesion unevenness in the longitudinal direction. The oil adhesion rate (a+b) of the solid-phase polymerization oil to the fiber refers to the value of the oil adhesion rate obtained by the method described in the examples for the fiber after the solid-phase polymerization oil is applied. The adhesion rate (a) of the inorganic particles (A) and the adhesion rate (b) of the phosphoric acid compound (B) referred to here refer to the values calculated by the following formula.
[0061] (Deposition rate (a) of inorganic particles (A)) = (a + b) × Ca / (Ca + Cb) (Deposition rate (b) of phosphoric acid compound (B)) = (a + b) × Cb / (Ca + Cb) Here, Ca denotes the concentration of inorganic particles (A) in the solid-phase polymerization oil solution, and Cb denotes the concentration of phosphoric acid compound (B) in the solid-phase polymerization oil solution.
[0062] Furthermore, it is preferable that the adhesion rate (a) by weight of the inorganic particles (A) and the adhesion rate (b) by weight of the phosphoric acid compound (B) satisfy b / a ≧ 1. By making the adhesion rate (b) of the phosphoric acid compound (B) equal to or greater than the adhesion rate (a) of the inorganic particles (A), the excellent cleaning properties resulting from the formation of a condensation salt during solid-phase polymerization of the phosphoric acid compound (B) are more significantly exhibited, and this is also preferable from the viewpoint of suppressing adhesion or falling off between the inorganic particles (A) and the fibers.
[0063] In the present invention, solid-state polymerization is carried out after applying a solid-state polymerization oil, which increases the molecular weight and also increases the strength, elastic modulus, and elongation. The solid-state polymerization can be carried out in the form of a reel or a tow (for example, placed on a metal net, etc.), or it can be carried out continuously as a thread between rollers, but it is preferable to carry out the solid-state polymerization in the form of a package in which the fibers are wound around a core material, from the viewpoints of simplifying the equipment and improving productivity.
[0064] The solid-state polymerization can be carried out in an inert gas atmosphere such as nitrogen, in an oxygen-containing active gas atmosphere such as air, or under reduced pressure, but it is preferable to carry out the polymerization in a nitrogen atmosphere in order to simplify the equipment and to prevent oxidation of the fibers or core material. In this case, the atmosphere for the solid-state polymerization is preferably a low-humidity atmosphere with a dew point of -40°C or lower.
[0065] The solid-state polymerization temperature is preferably Tm1-60°C or higher, assuming that the endothermic peak temperature of the liquid crystal polyester filament subjected to solid-state polymerization is Tm1 (°C). By setting the temperature at such a high temperature near the melting point, the solid-state polymerization proceeds quickly, and the strength of the fiber can be improved. Note that Tm1 here generally refers to the melting point of the liquid crystal polyester filament, and in the present invention, refers to the value obtained by the measurement method described in the Examples. Note that it is preferable to set the maximum temperature to less than Tm1 (°C) in order to prevent fusion. In addition, it is more preferable to increase the solid-state polymerization temperature stepwise or continuously with respect to time, since it is possible to prevent fusion and increase the time efficiency of solid-state polymerization. In this case, since the melting point of the liquid crystal polyester filament increases with the progress of solid-state polymerization, the solid-state polymerization temperature can be increased to about Tm1+100°C of the liquid crystal polyester filament before solid-state polymerization. However, even in this case, it is preferable that the maximum temperature in solid-state polymerization is Tm1-60 (°C) or higher but less than Tm1 (°C) of the fiber after solid-state polymerization, in order to increase the solid-state polymerization rate and prevent fusion.
[0066] The solid-state polymerization time is preferably 5 hours or more, more preferably 10 hours or more, at the maximum temperature in order to sufficiently increase the molecular weight of the fiber, i.e., strength, elastic modulus, and elongation. On the other hand, since the effects of increasing strength, elastic modulus, and elongation are saturated with time, it is preferable to set the time to 50 hours or less in order to increase productivity.
[0067] In the present invention, it is preferable to remove the solid-state polymerization oil while running the fiber after solid-state polymerization. A known method can be used to remove the solid-state polymerization oil, but it is preferable to use a nozzle spraying a mixed fluid of liquid and gas after immersing the fiber in a liquid to cause it to swell.
[0068] The solid-state polymerization oil remaining on the fiber surface after solid-state polymerization accumulates on guides, reeds, and the fiber itself during the weaving process, which is a post-processing step of the fiber, generating debris called scum. If this scum gets mixed into the product, it can cause product defects or can hinder the shedding motion of the yarn, leading to yarn breakage. Therefore, in the production of liquid crystalline polyester fibers, it is important to wash off the solid-state polymerization oil after solid-state polymerization.
[0069] In particular, there is a growing demand for higher density weaving (higher mesh) and reduced gauze thickness to improve the performance of acoustic filters made of filaments, as well as an increased demand for higher opening ratios, and in order to achieve this, finer filament fineness is being required. In addition, as the density increases, the load and number of beatings on the filaments increases during weaving, and scum from solid-phase polymerization oil remaining on the fiber surface increases, resulting in more broken weave yarns and more product defects (scum), and so there is a demand for stronger washing than ever before.
[0070] The solid-state polymerized yarn in the package after the washing step is unwound, and in order to prevent fibrillation when peeling off slight fusion caused by solid-state polymerization, it is preferable to unwind the yarn in a direction perpendicular to the axis of rotation (fiber circumferential direction) while rotating the solid-state polymerization package, i.e., by so-called side unwinding. Examples of such unwinding methods include a method of actively driving the yarn at a constant rotation speed using a motor or the like, a method of controlling the rotation speed using a dancer roller to unwind at a controlled speed, and a method of hanging the solid-state polymerization package on a free roll and unwinding the fiber while pulling it with a controlled speed roller.
[0071] The method for washing the solid-state polymerized fibers is to first run the fibers after solid-state polymerization while immersing them in a liquid in which the solid-state polymerized oil agent can dissolve or disperse. The method for immersing the fibers in the liquid may be a method of contacting the fibers with the liquid using a kiss roll, but the method of running the fibers in a bath filled with the liquid is preferred in that it can reduce the amount of liquid used, prevents the liquid from scattering around, and allows the contact time with the liquid to be extended.
[0072] The liquid used for cleaning by immersion is preferably water to reduce the environmental load. The higher the temperature of the liquid, the higher the removal efficiency, and a temperature of 30°C or higher is preferable, and 40°C or higher is more preferable. However, if the temperature is too high, the liquid will evaporate significantly, so a temperature of -20°C or lower than the boiling point of the liquid is preferable, and -30°C or lower is more preferable.
[0073] It is preferable to add a surfactant to the liquid used for cleaning in order to improve the cleaning efficiency. The amount of surfactant added is preferably 0.01 to 1 wt %, more preferably 0.1 to 0.5 wt %, in order to increase the removal efficiency and reduce the environmental load.
[0074] Furthermore, in order to improve the cleaning efficiency, it is preferable to apply vibration or liquid flow to the liquid used for cleaning by immersion. In this case, although there is a method such as ultrasonically vibrating the liquid, it is preferable to apply a liquid flow from the viewpoint of simplifying the equipment and saving energy. Methods for applying a liquid flow include stirring in the liquid bath and applying a liquid flow with a nozzle, but applying a liquid flow with a nozzle is preferable because it can be easily performed by supplying the liquid bath with a nozzle when circulating it. In addition, the method of immersing the fiber in the liquid may be a method of guiding the fiber into the bath using a guide or the like, but in order to suppress fibrillation of the solid-phase polymerized fiber due to contact resistance with the guide, it is preferable to provide slits at both ends of the bath so that the fiber can pass through the bath through the slits and to not provide a yarn guide in the bath.
[0075] Next, washing is performed using a liquid / gas mixed fluid spray nozzle, which allows fine liquid particles to collide with the remaining solid-state polymerized oil agent on the fiber surface, effectively removing the remaining solid-state polymerized oil agent without applying excessive load to the running yarn.
[0076] The running tension of the running yarn immediately after washing with the liquid and gas mixture spray nozzle is preferably 1.0 cN or more and 20.0 cN or less. A running tension of 1.0 cN or more is preferable because it stabilizes the running state. If it exceeds 20.0 cN, it is not preferable because fibril and fluff are likely to occur due to friction with guides, etc. during the process. More preferably, it is 5.0 cN or more and 15.0 cN or less.
[0077] The amount of solid-phase polymerized oil adhering to the liquid crystal polyester fiber after washing is preferably 0.20% by weight or less, more preferably 0.10% by weight or less, and most preferably 0.07% by weight or less, from the viewpoint of improving the processability of the fiber in the advanced processing step and the weaving step and improving the quality of the fabric. The amount of solid-phase polymerized oil adhering to the liquid crystal polyester fiber after washing refers to a value measured by the method for measuring the oil adhesion rate described in the Examples for the fiber wound immediately after the washing step.
[0078] In addition, when the use of the liquid crystal polyester filament requires improvement in the abrasion resistance of the fiber, it is preferable to perform a high-temperature heat treatment at a temperature of Tm1+10°C or higher after washing. Note that Tm1 here refers to a value obtained by the measurement method described in the Examples. Tm1 is the melting point of the fiber, and by performing a heat treatment at a high temperature of melting point+10°C or higher on the liquid crystal polyester filament, the peak half-width at Tm1 becomes 15°C or higher, and the degree of crystallization and perfection of the crystals of the entire fiber are reduced, thereby greatly improving the abrasion resistance.
[0079] In terms of heat treatment, there is solid-phase polymerization of liquid crystal polyester filaments, but in this case, the treatment temperature must be below the melting point of the fiber, otherwise the fiber will fuse and melt. In the case of solid-phase polymerization, the melting point of the fiber increases with the treatment, so the final solid-phase polymerization temperature may be above the melting point of the fiber before treatment, but even in that case, the treatment temperature is lower than the melting point of the treated fiber, that is, the melting point of the fiber after heat treatment. In other words, the high-temperature heat treatment here does not mean performing solid-phase polymerization, but rather reducing the structural difference between the dense crystalline part and the amorphous part formed by solid-phase polymerization, that is, reducing the degree of crystallization and the perfection of the crystal to increase the wear resistance. Therefore, even if Tm1 changes due to heat treatment, the treatment temperature is preferably Tm1+10°C or more of the treated fiber, and from this point of view, the treatment temperature is preferably Tm1+10°C or more of the treated fiber, more preferably Tm1+40°C or more, even more preferably Tm1+60°C or more, and particularly preferably Tm1+80°C or more. The upper limit of the treatment temperature is the temperature at which the fibers melt and varies depending on the tension, speed, single fiber fineness, and treatment length, but is generally Tm1 + 300°C.
[0080] Another heat treatment is the hot drawing of liquid crystal polyester filaments, but hot drawing tensions the fibers at high temperatures, and the fiber structure has a high molecular chain orientation, increasing strength and elastic modulus, while maintaining the crystallinity and crystalline perfection, i.e., ΔHm1 remains high and the peak half-width of Tm1 remains small. Therefore, the fiber structure has poor abrasion resistance, which is different from the heat treatment of the present invention, which aims to improve abrasion resistance by reducing the crystallinity (ΔHm1 decrease) and reducing the crystalline perfection (peak half-width increase). Note that the high-temperature heat treatment referred to in the present invention reduces the crystallinity, so the strength and elastic modulus do not increase.
[0081] It is preferable to carry out the high-temperature heat treatment while continuously running the fibers, since this prevents fusion between the fibers and improves the uniformity of the treatment. At this time, it is preferable to carry out a non-contact heat treatment in order to prevent the generation of fibrils and to carry out a uniform treatment. Heating means include atmospheric heating and radiation heating using a laser or infrared rays, but heating with a slit heater using a block or plate heater is preferable because it has the effects of both atmospheric heating and radiation heating and improves the stability of the treatment.
[0082] The treatment time is preferably longer in order to reduce the degree of crystallinity and the perfection of the crystals, and is preferably 0.01 seconds or more, more preferably 0.05 seconds or more, and even more preferably 0.1 seconds or more. The upper limit of the treatment time is preferably 5.0 seconds or less, more preferably 3.0 seconds or less, and even more preferably 2.0 seconds or less in order to reduce the load on the equipment and because a long treatment time relaxes the orientation of the molecular chains and reduces the strength and elastic modulus.
[0083] The treatment speed depends on the treatment length, but the faster the treatment speed, the faster the treatment becomes possible at high temperature in a short time, the greater the effect of improving abrasion resistance, and the greater the productivity, so that the treatment speed is preferably 100 m / min or more, more preferably 200 m / min or more, and even more preferably 300 m / min or more. The upper limit of the treatment speed is about 1000 m / min from the viewpoint of the running stability of the fiber.
[0084] The treatment length depends on the heating method, but in the case of non-contact heating, in order to perform uniform treatment, it is preferably 100 mm or more, more preferably 200 mm or more, and even more preferably 500 mm or more. Also, if the treatment length is too long, uneven treatment and fiber melting may occur due to yarn shaking inside the heater, so it is preferably 3000 mm or less, more preferably 2000 mm or less, and even more preferably 1000 mm or less.
[0085] The above-mentioned washing and heat treatment are preferably carried out in one continuous process without winding in between. In particular, when winding the liquid crystal polyester filament after solid-state polymerization, fibrillation of the fiber occurs due to rubbing with the winder, etc., so that it is preferable to carry out heat treatment after washing to improve abrasion resistance.
[0086] It is also preferable to apply a finishing oil from the viewpoint of improving processability in subsequent steps such as washing, heat treatment, etc. As the finishing oil, a finishing oil generally used for polyester fibers can be preferably applied.
[0087] The adhesion rate of the finishing oil is preferably 0.1% by weight or more based on the fiber weight in order to improve the abrasion resistance and processability by improving the surface smoothness. The higher the oil content, the greater the effect, so 0.3% by weight or more is more preferable. However, if the oil content is too high, the adhesive strength between the fibers increases, hindering processability and causing process stains, so 2.0% by weight or less, 1.5% by weight or less is preferable. The adhesion rate of the finishing oil here refers to the value obtained by subtracting the adhesion rate of the remaining solid-phase polymerized oil on the same fiber from the oil adhesion rate value determined for the fiber after the finishing oil has been applied by the method described in the Examples.
[0088] In this manner, the liquid crystal polyester filament of the present invention can be obtained.
[0089] The liquid crystal polyester filament preferably used in the acoustic filter obtained by the present invention has a strength of 5.0 to 20.0 cN / dtex. More preferably, the strength is 10.0 cN / dtex or more. The liquid crystal polyester filament preferably used in the acoustic filter obtained by the present invention has an elongation of 1.5 to 4.5%. More preferably, it is 3.5% or less. The liquid crystal polyester filament preferably used in the acoustic filter obtained by the present invention has an elastic modulus of 600 to 900 cN / dtex. More preferably, it is 800 cN / dtex or less. In addition, the liquid crystal polyester filament preferably used in the filter having excellent design preferably has a color tone L value of 40 or less. In addition, the liquid crystal polyester filament of the present invention preferably used in the acoustic filter is preferably a monofilament in order to make it into a filter, but it can also be a multifilament depending on the application, and is not limited to a monofilament. The liquid crystal polyester filaments of the present invention, which are suitable for use in acoustic filters, desirably have a fineness of 10 T or less, preferably 8 T or less, and more preferably 6 T or less in order to achieve both dust resistance and sound permeability, but may have a fineness of 10 T or more depending on the application, and the fineness is not limited. The liquid crystal polyester filaments obtained in the present invention can be woven at a desired density using the warp and weft to form a colored filter. EXAMPLES
[0090] The liquid crystal polyester filament of the present invention will be specifically described below with reference to examples. The measured values in the examples were measured by the following methods.
[0091] A. Fineness A 300 m reel of fiber was taken using a measuring machine, its weight (g) was multiplied by 100 / 3, 10 measurements were taken per level, and the average value was taken as the fineness (dtex).
[0092] B. Strength, elongation, elastic modulus According to the method described in JIS L1013:1999, 20 measurements per level were taken continuously in the longitudinal direction of the fiber using a Tensilon UTM-100 manufactured by Orientec Co., Ltd., under the conditions of a sample length of 500 mm and a tensile speed of 50 mm / min, and the average values were taken as strength (cN / dtex), elongation (%), and modulus of elasticity (cN / dtex). The modulus of elasticity refers to the initial tensile resistance.
[0093] C. Oil adhesion rate 1.0±0.1 g of fiber was collected and dried at 60°C for 10 minutes, after which its weight was measured (W0). The fiber was then immersed in a solution of sodium dodecylbenzenesulfonate at 2.0% by weight relative to the fiber weight in water at least 100 times the weight of the fiber, and ultrasonically cleaned at room temperature for 20 minutes. After cleaning, the fiber was washed with water and dried at 60°C for 10 minutes, after which its weight (W1) was measured, and the weight was calculated using the following formula: (Oil adhesion rate (weight%)) = (W0-W1) x 100 / W1 The oil adhesion rate was calculated by the following.
[0094] D. Color Tone L Value A sample for color measurement was created by wrapping the filaments around a plate in three layers with a pitch of 0.5 cm and a width of 4.5 cm, and measuring the color using a Konica Minolta CR-400 color difference meter. The L value represents the brightness (luminosity) of the color and ranges from 0 to 100 (closer to 0 is black, closer to 100 is white), with the higher the number, the brighter the color.
[0095] E. Tm1 of liquid crystal polyester fiber, peak half-width at Tm1, heat of fusion ΔHm1, melting point of liquid crystal polyester polymer (Tm2) Differential calorimetry was performed using a TA instruments DSC2920. The temperature of the endothermic peak observed when measuring under temperature rising conditions of 20°C / min from 50°C was designated as Tm1 (°C). The peak half-width (°C) and heat of fusion (ΔHm1) (J / g) at Tm1 were measured.
[0096] For the liquid crystal polyester polymer shown in the reference example, after observing Tm1, the polymer was held at a temperature of Tm1+20°C for 5 minutes, then cooled to 50°C at a temperature drop rate of 20°C / min, and then measured again at a temperature rise rate of 20°C / min. The endothermic peak observed when the temperature was raised was taken as Tm2, and Tm2 was taken as the melting point of the polymer.
[0097] F. Weight average molecular weight (molecular weight) converted into polystyrene A mixed solvent of pentafluorophenol / chloroform = 35 / 65 (weight ratio) was used as the solvent, and the liquid crystal polyester was dissolved so that the concentration was 0.04 to 0.08 weight / volume % to prepare a sample for GPC measurement. If insoluble matter was found even after leaving it at room temperature for 24 hours, it was left to stand for another 24 hours, and the supernatant was used as a sample. This was measured using a GPC measuring device manufactured by Waters, and the weight average molecular weight (Mw) was calculated in terms of polystyrene. Columns: Shodex K-806M x 2, K-802 x 1 Detector: Differential refractive index detector RI Temperature: 23±2℃ Flow rate: 0.8mL / min Injection volume: 200μL.
[0098] G. Filter opening and aperture ratio The gaps (μm) between the warp threads of the filter and the gaps (μm) between the weft threads were measured using an optical microscope, and their average value was taken as the mesh size (μm) of the filter.
[0099] From the average value of the gap L1 (μm) between the warp threads of the filter, the average value of the gap L2 (μm) between the weft threads, and the number of meshes M (pieces / 2.54 cm) of the filter, from the following formula (I): K = L1 × L2 × M 2 / (2.54×10000) 2 (I) The aperture ratio K (%) of the filter was calculated.
[0100] H. Filter performance evaluation (breathability, dust resistance, dimensional stability, design) The filters obtained in the Examples and Comparative Examples were evaluated for performance in terms of breathability, dust resistance, dimensional stability, and design according to the following evaluation criteria. Each evaluation of breathability, dust resistance, and dimensional stability was performed by an evaluator familiar with the subject evaluation. <Breathability> A filter with 27 μm mesh size obtained from the liquid crystal filaments of the examples and comparative examples was attached to a sound generating device that emits a sound of 50 dB, and the way the sound was heard was compared between sound that passed through the filter and sound that did not pass through the filter. A: The sound that has passed through the filter can be heard clearly. B: Filtered sound is attenuated but still audible. C: No sound can be heard through the filter. <Dustproof> The mesh size of the filters obtained from the liquid crystal filaments of the examples and comparative examples was evaluated, and it was determined that filters with a mesh size of 50 μm or less were less permeable to dust and had high dust-proofing properties. A: Small mesh size and high dust resistance C: Large mesh size and poor dust resistance <Dimensional stability> The filters obtained from the liquid crystal filaments of the examples and comparative examples were pressed by hand in a direction perpendicular to the filter surface, and the degree of deformation after pressing was evaluated. A: The mesh does not deform even when pressed by hand. B: The mesh deforms slightly when pressed by hand, but quickly returns to its original shape. C: The mesh is significantly deformed when pressed by hand. <Design> For the liquid crystal filaments of the Examples and Comparative Examples, when the color tone L value measured in the above item D was 40 or more, it was evaluated as not being sufficiently colored and having poor design. When the color tone L value was 30 or more and less than 40, it was evaluated as being colored but light in color. When the color tone L value was less than 30, it was evaluated as being sufficiently colored and having excellent design. A: It is well colored and has an excellent design. B: It is colored, but the color is pale. C: Not sufficiently colored, poor design.
[0101] Example 1 A 5L reaction vessel equipped with a stirring blade and a distillation tube was charged with 870 parts by weight of p-hydroxybenzoic acid, 327 parts by weight of 4,4'-dihydroxybiphenyl, 89 parts by weight of hydroquinone, 292 parts by weight of terephthalic acid, 157 parts by weight of isophthalic acid, and 1460 parts by weight of acetic anhydride (1.10 equivalents of phenolic hydroxyl groups in total), and the mixture was heated from room temperature to 145°C in 30 minutes while stirring under a nitrogen gas atmosphere, and then reacted at 145°C for 2 hours. The mixture was then heated to 335°C in 4 hours.
[0102] The polymerization temperature was maintained at 335°C, the pressure was reduced to 133 Pa in 1.5 hours, and the reaction was continued for another 40 minutes, completing the polycondensation when the torque reached 28 kgcm. Next, the pressure in the reaction vessel was increased to 0.1 MPa, and the polymer was extruded into strands through a die with a circular outlet of 10 mm in diameter, and pelletized by a cutter. The composition, melting point, and molecular weight of the liquid crystal polyester obtained are as shown in Table 1.
[0103] [Table 1]
[0104] 30 parts by mass of CB having an average particle size of 50 μm was added to 70 parts by mass of the above liquid crystal polyester, and the mixture was fed into a twin-screw kneading device while being stirred with a Henschel mixer and melt-kneaded. The mixture was then extruded from a die into a strand shape, cooled with water, and cut to prepare a master chip containing CB.
[0105] The chips were blended so that the weight ratio of the liquid crystal polyester to the master chip was 39:1, and the mixture was vacuum dried at 160 ° C for 12 hours. The mixture was then melted at 330 ° C in a φ15 mm single-screw extruder manufactured by Osaka Seiki Kogyo Co., Ltd., and passed through a pipe at a spinning temperature of 340 ° C. The polymer was supplied to a spinning pack while being metered with a gear pump so that the spinning rate was 1.7 g / min per nozzle. In the spinning pack, the polymer was filtered using a metal nonwoven fabric filter, and four threads of the polymer were discharged from a nozzle with an L / D of 2.0. The discharged polymer was passed through a 40 mm heat retention area, and then cooled and solidified from the outside of the threads by a circular cooling wind of an air flow at 25 ° C., and then a spinning oil mainly composed of a fatty acid ester compound was applied, and all filaments were taken up by a first godet roll at 1000 m / min. This was passed through a second godet roll at the same speed, and then wound into a pirn shape using a spindle traverse type pirn winder (without a contact roll that comes into contact with the package) with a dancer arm. The spinning draft was 25, and no yarn breakage occurred during winding, resulting in good spinnability. The single fiber fineness of the obtained fiber was 7.0 dtex, the strength was 5.2 cN / dtex, the elongation was 1.3%, and the elastic modulus was 561 cN / dtex. The filtration pressure at the start of spinning was 6.7 MPa, the filtration pressure increase was 0.09 MPa / hr, and it took more than 8 days until the filtration pressure reached the upper limit of 25 MPa, without any yarn breakage or the like, and spinning was possible with good operability.
[0106] The spun fiber package was rewound using a winding device (without touch roll, wind number 8.7, taper angle 45°) in which an electric cylinder RCP-SAC3 manufactured by IAI was connected to the cam box part (traverse device) of a precision winder SSP-MV manufactured by Kozu Seisakusho Co., Ltd. via a link mechanism. At this time, the outer diameter of the package was detected by a displacement sensor IL-065 manufactured by Keyence, and the electric cylinder was driven to move the cam box part so that the free length was constant based on the detected package diameter. The spun fiber was unwound in the vertical direction (perpendicular to the fiber circumferential direction), and an oiling roller (stainless steel roll with matte finish) was used to oil the solid-phase polymerization oil agent, which was prepared by dispersing 1.0 wt% of talc as inorganic particles (A) in an aqueous solution containing 10.0 wt% of a phosphoric acid compound (B1) represented by the following chemical formula (4) as a phosphoric acid compound (B). The oil adhesion rate (a+b) of the solid-phase polymerized oil agent on the fiber after rewinding was 21.8% by weight.
[0107] [ka]
[0108] Next, the rewound package was subjected to solid-state polymerization. The solid-state polymerization was carried out using a closed oven, where the temperature was raised from room temperature to 240°C in about 30 minutes, and then held at 240°C for 3 hours, after which the temperature was raised at 4°C / hour to 290°C, and held for 15 hours. The atmosphere was dehumidified nitrogen, supplied at a flow rate of 20NL / min, and exhausted from the exhaust port to prevent the inside of the oven from becoming pressurized.
[0109] The fiber obtained after solid-state polymerization had a fineness of 6.3 dtex, a strength of 16.9 cN / dtex, an elongation of 1.8%, and an elastic modulus of 1115 cN / dtex, which confirmed that the strength, elongation, and elastic modulus were improved compared to the fiber before solid-state polymerization, and that solid-state polymerization had progressed.The fiber obtained after solid-state polymerization had a Tm1 of 344°C, a ΔHm1 of 8.6 J / g, and a peak half-width at Tm1 of 6.5°C.
[0110] Next, the fiber was unwound from the package after solid-state polymerization and washed to remove the solid-state polymerization oil. The package after solid-state polymerization was fitted to a free roll creel (having an axis and bearings, the outer layer can rotate freely. No brake or drive source), from which the yarn was pulled out horizontally (in the direction of fiber rotation), and the fiber was continuously passed through a bathtub (without a guide inside that comes into contact with the fiber) with a bath length of 150 cm (contact length of 150 cm) and slits on both ends to wash and remove the solid-state polymerization oil. The washing liquid was 50°C hot water containing nonionic and anionic surfactants. After that, washing was performed with a spray nozzle of a mixed fluid of water and air using a two-fluid air atomizing nozzle manufactured by Spraying Systems Co., Ltd. Two spray nozzles with a hole diameter of 1.5 mm were used, the water pressure was 0.20 MPa, the compressed air pressure was 0.20 MPa, and the distance between the spray nozzle nozzle and the running yarn was 15.0 mm. The amount of water used was 100mL / min·pieces, and the amount of compressed air used was 35L / min·pieces. After washing, the fiber was passed through a bearing roller guide, and then passed through the first roller with a separate roller at 400m / min. Since the creel is a free roll, tension is applied to the fiber by this roller, which unwinds it from the solid-state polymerization package and allows the fiber to run.
[0111] The fiber that passed through the roller was passed between 1m long slit heaters heated to 510℃, and high-temperature non-contact heat treatment was performed. No guides were provided inside the slit heater, and the heater and fiber were not in contact with each other. After passing through the heater, the fiber was passed through a second roller with a separate roller. The first and second rollers were set at the same speed. The fiber that passed through the second roller was given a finishing oil mainly composed of fatty acid ester compounds by a ceramic oiling roller, and was wound up by a spindle traverse type pirn winder with a dancer arm. The physical properties of the obtained fiber were as shown in Table 2, with a strength of 12.2cN / dtex, elongation of 2.0%, elastic modulus of 716cN / dtex, and color tone L value of 20.6. There was no yarn breakage during heat treatment, and the operability was good.
[0112] The liquid crystal polyester thus obtained was woven to a mesh number of 500 / 2.54 cm to produce a filter with an opening size of 27 μm and an opening rate of 28%. The performance of the filter was evaluated, and as shown in Table 2, it was found to have good breathability, dust resistance, dimensional stability, and design.
[0113] Example 2 A liquid crystal polyester fiber was obtained in the same manner as in Example 1, except that the weight ratio of liquid crystal polyester to master chip was changed to 59:1, and the chips were blended. The fiber obtained by spinning had a single fiber fineness of 7.2 dtex, a strength of 5.7 cN / dtex, an elongation of 1.3%, and an elastic modulus of 558 cN / dtex. The filtration pressure at the start of spinning was 6.6 MPa, the filtration pressure increase was 0.09 MPa / hr, and it took more than 8 days to reach the upper limit of the filtration pressure of 25 MPa without any thread breakage, and spinning was performed with good operability. The physical properties of the fiber obtained by heat treatment were as shown in Table 2, with a strength of 12.8 cN / dtex, an elongation of 2.1%, an elastic modulus of 710 cN / dtex, and a color tone L value of 24.2. The heat treatment also had good operability without any thread breakage. The obtained liquid crystal polyester was woven to a mesh number of 500 / 2.54 cm to produce a filter with an opening of 27 μm and an opening rate of 28%. The performance of the filter was evaluated, and as shown in Table 2, it was found to have good breathability, dust resistance, dimensional stability, and design.
[0114] Example 3 A liquid crystal polyester fiber was obtained in the same manner as in Example 1, except that the weight ratio of liquid crystal polyester to master chip was changed to 99:1, and the chips were blended. The fiber obtained by spinning had a single fiber fineness of 7.2 dtex, a strength of 6.1 cN / dtex, an elongation of 1.4%, and an elastic modulus of 572 cN / dtex. The filtration pressure at the start of spinning was 6.2 MPa, the filtration pressure increase was 0.08 MPa / hr, and it took more than 8 days to reach the upper limit of the filtration pressure of 25.0 MPa without any thread breakage, and the spinning could be performed with good operability. The physical properties of the fiber obtained by heat treatment were as shown in Table 2, with a strength of 13.9 cN / dtex, an elongation of 2.3%, an elastic modulus of 719 cN / dtex, and a color tone L value of 33.2. The heat treatment also had no thread breakage, and the operability was good. The liquid crystal polyester obtained was woven to a mesh number of 500 / 2.54 cm to produce a filter with an opening size of 27 μm and an opening rate of 28%. The performance of the filter was evaluated, and as shown in Table 2, it had good breathability, dust resistance, and dimensional stability, and in terms of design, although the filter was colored, the color was light.
[0115] Example 4 A liquid crystal polyester fiber was obtained in the same manner as in Example 1, except that the weight ratio of liquid crystal polyester to master chip was changed to 29:1, and the chips were blended. The fiber obtained by spinning had a single fiber fineness of 6.9 dtex, a strength of 4.6 cN / dtex, an elongation of 1.2%, and an elastic modulus of 570 cN / dtex. The filtration pressure at the start of spinning was 6.9 MPa, the filtration pressure increase was 0.11 MPa / hr, and there was no thread breakage or the like for 7 days until the upper limit of the filtration pressure of 25 MPa was reached, and spinning was performed with good operability. The physical properties of the fiber obtained by heat treatment were as shown in Table 2, with a strength of 10.9 cN / dtex, an elongation of 1.8%, an elastic modulus of 702 cN / dtex, and a color tone L value of 19.8. There was no thread breakage during heat treatment, and the operability was good. The obtained liquid crystal polyester was woven to a mesh number of 500 / 2.54 cm to produce a filter with an opening of 27 μm and an opening rate of 28%. The performance of the filter was evaluated, and as shown in Table 2, it was found to have good breathability, dust resistance, dimensional stability, and design.
[0116] Example 5 A liquid crystal polyester fiber was obtained in the same manner as in Example 1, except that the weight ratio of liquid crystal polyester to master chip was changed to 9:1, and the chips were blended. The fiber obtained by spinning had a single fiber fineness of 7.0 dtex, a strength of 4.0 cN / dtex, an elongation of 1.1%, and an elastic modulus of 582 cN / dtex. The filtration pressure at the start of spinning was 7.8 MPa, the filtration pressure increase was 0.2 MPa / hr, and it took only about 4 days to reach the upper limit of the filtration pressure of 25 MPa. There were many thread breaks, and the operability was poor. The physical properties of the fiber obtained by heat treatment were as shown in Table 2, with a strength of 8.9 cN / dtex, an elongation of 1.7%, an elastic modulus of 685 cN / dtex, and a color tone L value of 18.4. In the heat treatment, many thread breaks occurred, and the operability was poor. The obtained liquid crystal polyester was woven to a mesh number of 500 / 2.54 cm to produce a filter with an opening of 27 μm and an opening rate of 28%. The performance of the filter was evaluated, and as shown in Table 2, it was found to have good breathability, dust resistance, dimensional stability, and design.
[0117] Comparative Example 1 Spinning was performed in the same manner as in Example 1, except that the chips were blended so that the weight ratio of liquid crystal polyester to master chips was 4:1.The filtration pressure at the start of spinning was 8.5 MPa, and the filtration pressure increase was 0.5 MPa / hr. It took only about one day for the filtration pressure to reach the upper limit of 25 MPa. In addition, there were many thread breaks, and it was impossible to collect spun samples.
[0118] Comparative Example 2 A liquid crystal polyester fiber was obtained in the same manner as in Example 1, except that the master chip was not used and only the liquid crystal polyester was used. The fiber obtained by spinning had a single fiber fineness of 7.1 dtex, a strength of 6.9 cN / dtex, an elongation of 1.4%, and an elastic modulus of 603 cN / dtex. The filtration pressure at the start of spinning was 5.8 MPa, the filtration pressure increase was 0.06 MPa / hr, and it took more than 8 days to reach the upper limit of the filtration pressure of 25 MPa, without any thread breakage, and spinning was performed with good operability. The physical properties of the fiber obtained by heat treatment were as shown in Table 2, with a strength of 17.2 cN / dtex, an elongation of 2.9%, an elastic modulus of 725 cN / dtex, and a color tone L value of 53.5. There was no thread breakage during heat treatment, and the operability was good. The obtained liquid crystal polyester was woven to a mesh number of 500 / 2.54 cm to form a filter, and a filter with an opening of 27 μm and an opening rate of 28% was obtained. When the filter performance was evaluated, it was found to have good breathability, dust resistance, and dimensional stability, as shown in Table 2, but it was not colored and had poor design.
[0119] Comparative Example 3 A filter was made by weaving a mesh count of 500 fibers / 2.54 cm using ordinary polyethylene terephthalate fibers with the physical properties shown in Table 2, and the resulting filter had an opening size of 21 μm and an aperture ratio of 17%. When the performance of the filter was evaluated, as shown in Table 2, it had good dust resistance, but poor breathability and dimensional stability. On the other hand, it had excellent design potential, as it could be dyed after being made into a mesh.
[0120]
Table 2
Claims
1. A liquid crystal polyester filament having a pigment concentration of 0.1 to 5.0% by weight.
2. The liquid crystal polyester filament according to claim 1, characterized in that the color tone L value is 40 or less, the strength is 5.0 to 20.0 cN / dtex, the elongation is 1.5 to 4.5%, and the elastic modulus is 600 to 900 cN / dtex.
3. 3. The liquid crystal polyester filament according to claim 1, wherein the pigment is carbon black.
Citation Information
Patent Citations
Fully aromatic thermotropic polyester
JP1988057635A
Method for preparing high strength dope-colored fiber