Resin structure
By maintaining specific depth and surface area ratios of grooves on both surfaces of a resin structure, warpage and rigidity issues are addressed, ensuring a stable and rigid structure.
Patent Information
- Application Number
- JP2023057476
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing resin structures face issues with warpage and reduced rigidity due to volume reduction in thinned portions, particularly when mechanical strength is required.
A resin structure with grooves on both surfaces, where the depth and surface area ratios of the grooves on the front and back surfaces are maintained within specific ranges to prevent warpage and maintain rigidity.
The solution effectively suppresses warpage and maintains excellent rigidity in the resin structure.
Smart Images

Figure 2024145218000005 
Figure 2024145218000006 
Figure 2024145218000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin structure. [Background technology]
[0002] Patent Document 1 discloses a plate-shaped plastic plate with multiple recesses formed on the front side. Such plastic plates warp because the front side and back side have different shapes. Patent Document 1 states that warping can be suppressed by forming a recessed portion on the back side and making the total volume of the multiple recesses and the volume of the recessed portion approximately the same. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-61919 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as a result of the inventors' investigations, it was found that the method disclosed in Patent Document 1 has a problem in that the rigidity of the resin structure is impaired because the volume of the resin structure is reduced by the volume of the recessed portion on the back side of the resin structure. This is particularly problematic when the resin structure is required to have a certain level of mechanical strength.
[0005] The present invention has been made to solve the above problems, and an object of the present invention is to provide a resin structure having a groove portion on at least one surface, which suppresses the occurrence of warping and has excellent rigidity. [Means for solving the problem]
[0006] As a result of intensive research to solve the above-mentioned problems, the inventors have found that for a resin structure having grooves on both its front and back surfaces, the above-mentioned problems can be solved by setting the ratio of the surface area of the groove on the front surface to the surface area of the groove on the back surface of the resin structure, and the ratio of the volume of the groove on the front surface to the volume of the groove on the back surface, each within a predetermined range. Based on these findings, the present inventors have completed the present invention.
[0007] That is, the present invention provides the following [1] to [8]. [1] A resin structure having a flat plate structure having a first surface and a second surface opposite to the first surface, the flat plate structure having grooves on both the first surface and the second surface, the depth (h1) of the grooves on the first surface and the depth (h2) of the grooves on the second surface are both at least 1 / 2 of a thickness T of the flat plate structure, the grooves on the first surface and the grooves on the second surface are arranged such that the grooves on the first surface and the grooves on the second surface do not overlap when the flat plate structure is viewed in a vertical projection from the first surface side, a ratio (S2 / S1) of a total surface area (S2) of the grooves on the second surface to a total surface area (S1) of the grooves on the first surface is 0.5 to 1.4, and a ratio (V2 / V1) of a total volume (V2) of the grooves on the second surface to a total volume (V1) of the grooves on the first surface is 0.3 to 0.9. [2] The resin structure according to the above [1], wherein the first surface has at least one groove portion having a length of 90% or more of the shortest side length of the flat structure, and the second surface does not have a groove portion having a length of 90% or more of the shortest side length of the flat structure. [3] The resin structure according to the above [1] or [2], wherein the first surface has a groove portion having a curved portion and a straight portion. [4] The resin structure according to any one of the above [1] to [3], wherein the resin structure comprises a resin composition, and the resin composition comprises a thermoplastic resin. [5] The resin structure according to any one of the above [1] to [4], wherein the resin structure comprises a resin composition, and the resin composition comprises a fibrous material. [6] The resin structure according to any one of the above [1] to [5], wherein the resin structure comprises a resin composition, and the resin composition comprises an intumescent flame retardant. [7] The resin structure according to the above [6], wherein the intumescent flame retardant contains a compound having a melamine structure or a piperazine structure. [8] The resin structure according to any one of the above [4] to [7], wherein the resin structure is a mat made of inorganic fibers impregnated with the resin composition. Effect of the Invention
[0008] According to the present invention, it is possible to provide a resin structure which is suppressed from warping and has excellent rigidity. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing an example of a resin structure according to an embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the periphery of a groove in an example of a resin structure according to an embodiment. [Diagram 3] FIG. 3 is a perspective view illustrating an example of a resin structure according to an embodiment. [Figure 4] FIG. 4 is a perspective view showing an example of the resin structure according to Calculation Example 1-1 and Calculation Example 1-2. [Diagram 5] FIG. 5 is a perspective view showing an example of the resin structure according to Calculation Example 2-1 and Calculation Example 2-2.
[0010] Hereinafter, the embodiments of the present invention will be described in detail. However, the following description is merely an example of an embodiment of the present invention, and the present invention is not limited to the contents thereof.
[0011] [Resin structure] The resin structure of the present invention comprises a flat plate structure having a first surface and a second surface opposite to the first surface, and has grooves on both the first surface and the second surface of the flat plate structure, the depth (h1) of the grooves on the first surface and the depth (h2) of the grooves on the second surface are both at least half the thickness T of the flat plate structure, the grooves on the first surface and the grooves on the second surface are arranged such that the grooves on the first surface and the grooves on the second surface do not overlap when the flat plate structure is viewed as a vertical projection from the first surface side, a ratio (S2 / S1) of a total surface area (S2) of the grooves on the second surface to a total surface area (S1) of the grooves on the first surface is 0.5 to 1.4, and a ratio (V2 / V1) of a total volume (V2) of the grooves on the second surface to a total volume (V1) of the grooves on the first surface is 0.3 to 0.9.
[0012] Description will be given below with reference to the appropriate drawings. Fig. 1 shows an example of a resin structure 10 according to an embodiment of the present invention. Fig. 2 is an enlarged cross-sectional view of the periphery of a groove portion in the example of the resin structure 10 according to the embodiment of the present invention. The resin structure 10 includes a flat plate structure 100 having a first surface 110 and a second surface 120 opposite to the first surface 110. The flat plate structure 100 has grooves on both the first surface 110 and the second surface 120 (groove 111 on the first surface 110 and groove 121 on the second surface 120).
[0013] The depth (h 1 ) of the groove 111 in the first surface 110 and the depth (h 2 ) of the groove 121 in the second surface 120 are both equal to or greater than ½ of the thickness T of the flat plate structure 100 . The depth (h1) of the groove 111 on the first surface 110 is preferably 5 / 6 or less, and more preferably 2 / 3 or less, of the thickness T of the flat plate structure 100. In this case, sufficient rigidity can be imparted to the resin structure. The depth (h2) of the groove 121 of the second surface 120 is preferably 5 / 6 or less, and more preferably 2 / 3 or less, of the thickness T of the flat plate structure 100. In this case, sufficient rigidity can be imparted to the resin structure. The depth (h1) of the groove 111 and the depth (h2) of the groove 121 may be the same value or may be different values.
[0014] The thickness T of the flat structure 100 is not particularly limited, but from the viewpoint of ease of molding, it is preferably 0.1 cm or more, more preferably 0.2 cm or more, even more preferably 0.3 cm or more, preferably 1 cm or less, more preferably 0.9 cm or less, and even more preferably 0.8 cm or less.
[0015] The groove portion 111 of the first surface 110 and the groove portion 121 of the second surface 120 are arranged so that the groove portion 111 of the first surface 110 and the groove portion 121 of the second surface 120 do not overlap when the flat plate structure 100 is viewed in vertical projection from the first surface 110 side. This is a requirement required because the depth (h1) of the groove portion 111 of the first surface 110 and the depth (h2) of the groove portion 121 of the second surface 120 are both ½ or more of the thickness T of the flat plate structure 100. That is, when the depth (h1) of the groove portion 111 and the depth (h2) of the groove portion 121 are both equal to or greater than ½ of the thickness T of the flat plate structure 100, the groove portion 111 of the first surface 110 and the groove portion 121 of the second surface 120 cannot be arranged to overlap when the flat plate structure 100 is viewed as a vertical projection from the first surface 110 side. Therefore, the resin structure 10 is arranged so that the groove portion 111 of the first surface 110 and the groove portion 121 of the second surface 120 do not overlap each other. As described later, as a result of the inventors' studies, it has been confirmed that when the groove portions 111 of the first surface 110 and the groove portions 121 of the second surface 120 are arranged so that they do not overlap when the flat plate structure 100 is viewed as a vertical projection from the first surface 110 side, if the ratio (S2 / S1) of the total surface area (S2) of the groove portions 121 of the second surface 120 to the total surface area (S1) of the groove portions 111 of the first surface 110 and the ratio (V2 / V1) of the total volume (V2) of the groove portions 121 of the second surface 120 to the total volume (V1) of the groove portions 111 of the first surface 110 are both within a specified range, it is possible to both suppress the occurrence of warping and suppress the decrease in rigidity. The surface area of the grooves herein refers to the combined surface area of the bottom and sides of the grooves.
[0016] In resin structure 10, the ratio (S2 / S1) of the sum (S2) of the surface area of grooves 121 on second surface 120 to the sum (S1) of the surface area of grooves 111 on first surface 110 is 0.5 or more and 2.5 or less. When the ratio (S2 / S1) of the sum of the surface areas of the grooves is within the above range, the occurrence of warping of the resin structure can be suppressed. The present inventors consider the reason for this as follows. When the surface areas of the front and back surfaces of a resin structure are different, a difference occurs in the cooling rate of the resin during molding between the front and back surfaces, which is thought to cause a difference in the amount of shrinkage and thus warping. For this reason, by setting the ratio of the total surface area of the groove portions on the front and back surfaces of the resin structure to a predetermined range, the occurrence of warping of the resin structure is suppressed. From the same viewpoint as above, the ratio (S2 / S1) of the total surface area (S2) of the grooves 121 of the second surface 120 to the total surface area (S1) of the grooves 111 of the first surface 110 is preferably 0.6 or more, more preferably 0.7 or more, and even more preferably 0.8 or more. Also, it is preferably 1.3 or less, more preferably 1.2 or less, and even more preferably 1.1 or less.
[0017] In resin structure 10, a ratio (V2 / V1) of a total volume (V2) of groove portions 121 on second surface 120 to a total volume (V1) of groove portions 111 on first surface 110 is 0.3 or more and 0.9 or less. When the ratio (V2 / V1) of the total volumes of groove portions is within the above range, a decrease in rigidity of the resin structure can be suppressed. As described above, the present inventors have considered that one of the causes of warping of the resin structure is that the difference in surface area between the front and back surfaces of the resin structure causes a difference in the cooling rate of the resin during molding between the front and back surfaces. Based on this, the present inventors thought that, for example, if exactly the same grooves are formed on the front and back surfaces of the resin structure, the surface areas of both surfaces will be equal, and the occurrence of warping can be suppressed. However, after further investigation, it was found that if the same grooves are formed on both the front and back surfaces of the resin structure, the volume of the resin structure is reduced by the volume of the grooves, which causes the rigidity of the entire resin structure to be impaired. In addition, the rigidity of the resin structure is also a factor that affects the magnitude of warping. Therefore, in order to obtain a resin structure that suppresses warping and does not impair rigidity, it is important to pay attention not only to the ratio of the surface area of the front and back surfaces of the resin structure, but also to the volume ratio at the same time. As described later, as a result of the inventors' studies, it has been confirmed that when the ratio (S2 / S1) of the sum of the surface areas (S2) of the groove portions 121 of the second surface 120 to the sum of the surface areas (S1) of the groove portions 111 of the first surface 110 is within the aforementioned specified range, when the ratio (V2 / V1) of the sum of the volumes (V2) of the groove portions 121 of the second surface 120 to the sum of the volumes (V1) of the groove portions 111 of the first surface 110 is 0.2 or more and 0.8 or less, it is possible to achieve both suppression of the occurrence of warping and suppression of a decrease in rigidity. From the same viewpoint as above, the ratio (V2 / V1) of the total volume (V2) of the grooves 121 of the second surface 120 to the total volume (V1) of the grooves 111 of the first surface 110 is preferably 0.4 or more, more preferably 0.5 or more, and is preferably 0.8 or less, more preferably 0.7 or less.
[0018] The resin structure 10 of the present invention will be described in further detail below.
[0019] The resin structure 10 has a flat plate structure 100. It is sufficient that the resin structure 10 has the flat plate structure 100 in at least a part thereof, and the entire resin structure 10 does not need to be the flat plate structure 100. For example, as shown in FIG. 3, the resin structure 10 may be in a box shape with one flat plate structure as the bottom. FIG. 3(a) is a perspective image seen from the first surface side, and FIG. 3(b) is a perspective image seen from the second surface side. The resin structure 10 may also have a box shape in which a plurality of flat plate structures are three-dimensionally combined. On the other hand, the entire resin structure 10 may be the flat plate structure 100. In this case, the resin structure 10 has a flat plate shape. The flat plate structure 100 has a first surface 110 and a second surface 120 opposite to the first surface. The areas of the first surface 110 and the second surface 120 are generally approximately equal. In addition, it is preferable that the first surface 110 and the second surface 120 are arranged approximately parallel to each other. The "flat plate structure" is a structure in which the area of the surface other than the first surface 110 and the second surface 120 is smaller than the area of the first surface 110 or the second surface 120. For example, the area of the surface other than the first surface 110 and the second surface 120 may be 50% or less, 40% or less, or 30% or less of the area of the first surface 110 or the second surface 120. The shape of the flat plate structure 100 is not particularly limited, and may be a square, a rectangle, a trapezoid, an ellipse, a circle, or the like.
[0020] The area of the first surface 110 or the second surface 120 is not particularly limited, but from the viewpoint of ease of molding, it is preferable that the area is 100 cm 2 More than 400cm is preferable. 2 More preferably, 900 cm 2 More preferably, 9m 2 Less than 6m is preferable 2 Less than 4m is preferable. 2 The following is even more preferred:
[0021] The plate structure 100 has grooves on both the first surface 110 and the second surface 120 . The width of the groove is not particularly limited, but from the viewpoint of ease of molding, it is preferably 0.3 cm or more, more preferably 0.5 cm or more, even more preferably 1 cm or more, and is preferably 10 cm or less, more preferably 7 cm or less, and even more preferably 5 cm or less.
[0022] The shape of the groove is not particularly limited and may be linear, annular, or the like, but from a practical standpoint, it is preferable for the groove to have both curved and linear portions.
[0023] It is preferable that the first surface 110 of the flat plate structure 100 has at least one groove portion having a length of 90% or more of the shortest side length L of the flat plate structure, and the second surface 120 has no groove portion having a length of 90% or more of the shortest side length of the flat plate structure. The "length L of the shortest side of the flat plate structure" refers to the shortest side of the outer periphery in the shape of the flat plate structure 100. When the flat plate structure 100 is an ellipse or a circle, the short diameter or diameter is the length L of the shortest side of the flat plate structure. It is more preferable that the first surface 110 has a groove portion having a length of 100% or more of the length L of the shortest side of the flat structure, and the length of the groove portion may be 120% or more, 150% or more, or 200% or more of the length L of the shortest side of the flat structure. It is more preferable that the second surface 120 does not have a groove portion having a length of 80% or more of the length L of the shortest side of the flat structure, and it is even more preferable that the second surface 120 does not have a groove portion having a length of 70% or more of the length L of the shortest side of the flat structure.
[0024] In the resin structure 10 of the present invention, the first surface 110 and the second surface 120 of the flat plate structure 100 have grooves of the same shape pattern on both sides, and the grooves on the second surface 120 are preferably formed with a plurality of partitions in addition to the shape pattern of the grooves on the first surface. By providing the partitions, the total volume of the grooves on the second surface is reduced by the volume of the partitions, and the rigidity of the resin structure 10 is not impaired. When the partitions are formed, the total surface area of the grooves on the second surface after the partitions are formed may not match the total surface area of the grooves on the first surface, but the ratio of the total surface area of the grooves on the second surface (S2) to the total surface area of the grooves on the first surface (S1) can be adjusted within the above-mentioned predetermined range by adjusting the length of the partitions.
[0025] The resin structure 10 of the present invention can include a resin composition.
[0026] [Resin composition] The composition according to the present invention preferably contains a thermoplastic resin (hereinafter referred to as thermoplastic resin (a)).
[0027] <Thermoplastic resin (a)> The thermoplastic resin (a) is not particularly limited, and examples thereof include polyolefin resin, polycarbonate resin, polyester resin, acrylonitrile styrene resin, ABS resin, polyamide resin, modified polyphenylene oxide, etc. Among these, polyolefin resin is preferred in the present invention. These may be used alone or in combination of two or more. For example, the thermoplastic resin (a) may be a composite resin of two or more of the above thermoplastic resins.
[0028] The polyolefin resin is not particularly limited, and may be any of the resins described below. The polyester resin is not particularly limited, and may be, for example, polybutylene terephthalate. The polyamide resin is not particularly limited, and may be, for example, nylon 66 or nylon 6. Among them, the present invention is particularly useful when the thermoplastic resin (a) contains at least a polyolefin resin. In the present invention, the term "polyolefin resin" refers to a resin in which the proportion of olefin units or cycloolefin units is 90 mol % or more relative to 100 mol % of all structural units constituting the resin. The proportion of olefin units or cycloolefin units relative to 100 mol % of all structural units constituting the polyolefin resin is preferably 95 mol % or more, and particularly preferably 98 mol % or more.
[0029] Examples of polyolefin resins include α-olefin polymers such as polyethylene, polypropylene, polybutene, poly(3-methyl-1-butene), poly(3-methyl-1-pentene), and poly(4-methyl-1-pentene); α-olefin copolymers such as ethylene-propylene block or random copolymers, α-olefin-propylene block or random copolymers having 4 or more carbon atoms, ethylene-methyl methacrylate copolymers, and ethylene-vinyl acetate copolymers; and cycloolefin polymers such as polycyclohexene and polycyclopentene. Examples of polyethylene include low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. Examples of polypropylene include isotactic polypropylene, syndiotactic polypropylene, hemiisotactic polypropylene, and stereoblock polypropylene. In the α-olefin-propylene block or random copolymers having 4 or more carbon atoms, examples of the α-olefins having 4 or more carbon atoms include butene, 3-methyl-1-butene, 3-methyl-1-pentene, and 4-methyl-1-pentene. These polyolefin resins may be used alone or in combination of two or more kinds. Among the above olefin resins, polypropylene-based resins (hereinafter sometimes referred to as "PP resins") are particularly preferred.
[0030] (Melt Flow Rate (MFR)) The melt flow rate (hereinafter sometimes abbreviated as MFR) (230°C, 2.16 kg load) of the thermoplastic resin (a) used in the present invention is preferably 40 to 500 g / 10 min. When the MFR is 40 g / 10 min or more, no chipping occurs when the resin structure is molded, and the processability does not decrease. When the MFR is 500 g / 10 min or less, no flash occurs during the production of the resin structure. From the above viewpoints, the MFR is preferably 50 to 400 g / 10 min, more preferably 60 to 400 g / 10 min, and more preferably 70 to 300 g / 10 min. The MFR of the thermoplastic resin (a) can be adjusted, for example, by controlling the hydrogen concentration during polymerization. The MFR is a value measured in accordance with JIS K7210.
[0031] (Thermoplastic resin (a) content) The content of the thermoplastic resin (a) in the resin structure of the present invention is not particularly limited, but is preferably 15 to 80% by mass. When the content of the thermoplastic resin is 15% by mass or more, the molding processability is particularly good, and molding of the resin structure is easy. On the other hand, when the content of the thermoplastic resin is 80% by mass or less, a sufficient amount of a copolymer of an α-olefin and an unsaturated carboxylic acid having functions as a flame retardant and a dispersant, and inorganic fibers, which will be described later, can be contained, and good flame resistance can be obtained. From the above viewpoints, the content of the thermoplastic resin in the resin structure is preferably 35 to 70% by mass, and more preferably 40 to 60% by mass.
[0032] <Polypropylene resin (a-1)> The thermoplastic resin (a) used in the resin structure of the present invention preferably contains a polypropylene-based resin. Examples of the polypropylene-based resin include a propylene homopolymer and a propylene-α-olefin copolymer. Here, the propylene-α-olefin copolymer may be either a random copolymer or a block copolymer.
[0033] (Polypropylene resin (a-1) content) The content of the polypropylene resin (a-1) in the resin structure of the present invention is not particularly limited, but is preferably 15 to 80% by mass. When the content of the polypropylene resin is 15% by mass or more, the molding processability is sufficient, and molding of the resin structure is easy. On the other hand, when the content is 80% by mass or less, the contents of the flame retardant, dispersant, and inorganic fiber become insufficient, and sufficient flame shielding properties are obtained. From the above viewpoints, the content of the polypropylene resin in the resin structure is more preferably 35 to 70% by mass, and even more preferably 40 to 60% by mass.
[0034] <Intumescent flame retardants (b1)> The resin composition according to the present invention preferably contains an intumescent flame retardant (b1). Intumescent flame retardants are flame retardants that suppress the combustion of materials by forming an intumescent surface layer that prevents the diffusion of radiant heat from the combustion source and combustion gases and smoke from the burning material to the outside. Among the intumescent flame retardants, phosphorus-based flame retardants are preferred, and examples thereof include salts of (poly)phosphoric acid and nitrogen compounds, specifically ammonium salts and amine salts of (poly)phosphoric acid, such as ammonium polyphosphate, melamine polyphosphate, piperazine polyphosphate, ammonium pyrophosphate, melamine pyrophosphate, and piperazine pyrophosphate. Among these, it is particularly preferable to contain a compound having a melamine structure or a piperazine structure. Examples of the nitrogen compounds include ammonia, melamine, piperazine, and other nitrogen compounds. Examples of the other nitrogen compounds include, for example, N,N,N',N'-tetramethyldiaminomethane, ethylenediamine, N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-diethylethylenediamine, amine, 1,2-propanediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, trans-2,5-dimethylpiperazine, 1,4-bis(2-aminoethyl)piperazine, 1,4-bis(3-aminopropyl)piperazine, acetoguanamine, benzoguanamine, acrylguanamine, 2 ,4-diamino-6-nonyl-1,3,5-triazine, 2,4-diamino-6-hydroxy-1,3,5-triazine, 2-amino-4,6-dihydroxy-1,3,5-triazine, 2,4-diamino-6-methoxy-1,3,5-triazine, 2,4-diamino-6-ethoxy-1,3,5-triazine, 2,4-diamino-6-propoxy-1,3,5-triazine, 2,4-diamino-6-isopropoxy-1,3,5-triazine, 2,4-diamino -6-mercapto-1,3,5-triazine, 2-amino-4,6-dimercapto-1,3,5-triazine, ammeline, benzguanamine, acetoguanamine, phthalodiguanamine, melamine cyanurate, melamine pyrophosphate, butylenediguanamine, norbornenediguanamine, methylenediguanamine, ethylenedimelamine, trimethylenedimelamine, tetramethylenedimelamine, hexamethylenedimelamine, 1,3-hexylenedimelamine, and the like.
[0035] (Content of intumescent flame retardant (b1)) The content of the intumescent flame retardant (b1) in the resin structure of the present invention is not particularly limited, but is preferably in the range of 1 to 30% by mass as the content in the resin composition. When it is 1% by mass or more, good flame retardancy can be imparted to the resin structure, and good flame shielding properties can be obtained. On the other hand, when the flame retardant is 30% by mass or less, the thermoplastic resin can be contained in a sufficient content ratio, so that the molding processability becomes better. From the above viewpoints, the content of the flame retardant in the resin composition is more preferably in the range of 1 to 25% by mass, and further preferably in the range of 3 to 20% by mass.
[0036] The resin composition according to the present invention preferably contains a metal oxide. The metal oxide serves as a flame retardant assistant. Specific examples of the metal oxide include cadmium oxide, zinc oxide, cuprous oxide, cupric oxide, ferrous oxide, ferric oxide, cobalt oxide, manganese oxide, molybdenum oxide, tin oxide, and titanium oxide. Among these, zinc oxide, which is highly effective, is particularly preferred. The content of the metal oxide is preferably in the range of 0.01 to 20 parts by mass, more preferably in the range of 0.5 to 10 parts by mass, and even more preferably in the range of 1 to 5 parts by mass, relative to 100 parts by mass of the flame retardant including the intumescent flame retardant (b1). When in the above range, the effect as a flame retardant auxiliary can be sufficiently exhibited.
[0037] <Copolymer of α-olefin and unsaturated carboxylic acid> The resin composition according to the present invention preferably contains a copolymer of an α-olefin and an unsaturated carboxylic acid. By using the copolymer, the dispersibility of the flame retardant including the intumescent flame retardant (b1) can be improved, and the content of the intumescent flame retardant and the like can be reduced.
[0038] In the "copolymer of α-olefin and unsaturated carboxylic acid" according to the present invention (hereinafter referred to as "copolymer (c1)"), it is preferable that the proportion of α-olefin units in the total of 100 mol% of α-olefin units and unsaturated carboxylic acid units is 20 mol% or more and 80 mol% or less. In the copolymer (c1), the ratio of the α-olefin units to the total amount of the α-olefin units and the unsaturated carboxylic acid units is preferably 30 mol% or more, and more preferably 70 mol% or less. If the ratio of the α-olefins is equal to or more than the lower limit, the compatibility with the thermoplastic resin (a) such as a polyolefin resin is improved, and if it is equal to or less than the upper limit, the compatibility with the intumescent flame retardant (b1) is improved.
[0039] In the copolymer (c1), the α-olefin is more preferably an α-olefin having 5 to 80 carbon atoms. If the α-olefin has 5 or more carbon atoms, compatibility with the thermoplastic resin (a) tends to be better, and if it has 80 or less carbon atoms, it is advantageous in terms of raw material costs. From the above viewpoints, the number of carbon atoms in the α-olefin is more preferably 10 to 80, even more preferably 12 to 70, and particularly preferably 18 to 60.
[0040] In the copolymer (c1), examples of the unsaturated carboxylic acid include (meth)acrylic acid, maleic acid, methylmaleic acid, fumaric acid, methylfumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, glutaconic acid, norbornane-5-ene-2,3-dicarboxylic acid, and esters, anhydrides, imides, etc. of these unsaturated carboxylic acids. Note that "(meth)acrylic acid" refers to acrylic acid or methacrylic acid. Specific examples of the ester, anhydride or imide of an unsaturated carboxylic acid include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and glycidyl (meth)acrylate; dicarboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride; and maleimide compounds such as maleimide, N-ethylmaleimide, and N-phenylmaleimide. These may be used alone or in combination of two or more. Among the above, esters and dicarboxylic anhydrides are preferred from the viewpoint of copolymerization reactivity, and among these, dicarboxylic anhydrides are preferred, and maleic anhydride is particularly preferred, from the viewpoint of compatibility with phosphorus-based flame retardants that are suitable as flame retardants.
[0041] The weight average molecular weight of the copolymer (c1) is preferably 2,000 or more, more preferably 3,000 or more, and is preferably 50,000 or less, more preferably 30,000 or less. When the weight average molecular weight of the copolymer (c1) is within the above range, the dispersibility of the intumescent flame retardant (b1) is more excellent. The weight average molecular weight of the copolymer (c1) is a value calculated as standard polystyrene by dissolving the copolymer (c1) in tetrahydrofuran (THF) and measuring the result by gel permeation chromatography.
[0042] Commercially available products of the copolymer (c1) include Lycorb CE2 (manufactured by Clariant Japan KK) and Diacalna 30M (manufactured by Mitsubishi Chemical Corporation).
[0043] The content of the (c1) copolymer in this resin structure relative to 100 parts by mass of the flame retardant containing the intumescent flame retardant (b1) is in the range of more than 0 and not more than 25 parts by mass, and preferably in the range of 0.01 to 10 parts by mass. If the content of the (c1) copolymer exceeds 0, the dispersibility of the intumescent flame retardant (b1) becomes insufficient, and the resin structure cannot be provided with sufficient flame-shielding properties. On the other hand, if the content is 25 parts by mass or less, the physical properties of the resin structure become insufficient. From the same viewpoint, the content of the (c1) copolymer is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more. On the other hand, the upper limit is more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less.
[0044] In addition, for the (Y) inorganic fibers described in detail below, the ratio of the (c1) copolymer to 100 parts by mass of the (Y) inorganic fibers is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. On the other hand, it is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 2.0 parts by mass or less. If the ratio of the (c1) copolymer is equal to or more than the lower limit, the flame-resistant properties and physical properties of the resin structure obtained and the appearance of the molded product obtained are improved. If the ratio of the (c1) copolymer is equal to or less than the upper limit, the effect of the (c1) copolymer on the flame-resistant properties of the resin structure can be further suppressed.
[0045] <Fibrous material> The resin composition according to the present invention preferably contains a fibrous material. As the fibrous material, various fibers can be used, and a suitable fibrous material is an inorganic fiber. As the inorganic fiber, there are glass fiber, rock wool, alumina fiber, silica alumina fiber, and other metal oxide fibers, potassium titanate fiber, calcium silicate (wollastonite) fiber, ceramic fiber, such as ceramic fiber, carbon fiber, metal fiber, and the like. These inorganic fibers may be used alone or in combination of two or more. Of the above inorganic fibers, at least one selected from glass fibers and alumina fibers is preferred from the viewpoints of flame resistance and processability.
[0046] The inorganic fibers preferably have an average fiber diameter of 3 to 25 μm, and an average fiber length of 0.1 mm or more, more preferably 1 mm or more, and even more preferably 5 mm or more. As for the average fiber diameter and the average fiber length, the preferred ranges vary depending on the type of inorganic material constituting the inorganic fibers, and specific preferred ranges will be described later. The fiber diameter can be measured using a scanning electron microscope or the like, and the average fiber diameter can be obtained by, for example, measuring the fiber diameters of 10 randomly selected fibers and calculating the average value. The fiber length can be measured using a ruler, calipers, or the like from an image enlarged by a microscope or the like as necessary, and the average fiber length can be obtained by, for example, measuring the fiber lengths of 10 randomly selected fibers and calculating the average value. As for the average fiber diameter and the average fiber length, the preferred ranges vary depending on the type of inorganic material constituting the inorganic fibers, and specific preferred ranges will be described later.
[0047] The content of inorganic fibers in the resin composition of the present invention is preferably 1 to 80% by mass. If the content of inorganic fibers is less than 1% by mass, the strength, rigidity, and impact resistance of the resin structure may decrease, and if it exceeds 80% by mass, the production and processing of the resin structure may become extremely difficult. In addition, if the content of inorganic fibers exceeds 80% by mass, the specific gravity of the resin structure increases, and the weight reduction effect as a metal substitute decreases, which is not preferable. From the above viewpoints, the content of the inorganic fibers in the resin composition of the present invention is more preferably 3 to 60 mass %, further preferably 10 to 50 mass %, and particularly preferably 30 to 45 mass %.
[0048] (Glass fiber) One of the inorganic fibers suitable for the resin composition of the present invention is glass fiber. The glass fiber may be, for example, a long fiber having an average fiber length of 30 mm or more, or a fiber (chopped strand) having a short average fiber length, but it is preferable to use a glass fiber having a long average fiber length from the viewpoints of flame retardancy, rigidity, impact resistance, etc. More specifically, the average fiber length is preferably 5 mm or more. When the average fiber length is 5 mm or more, the strength and impact resistance of the resin structure become good. From the above viewpoints, the average fiber length of the glass fiber is preferably 5 mm or more, and more preferably 30 mm or more. For example, when using pellets produced by the pultrusion method using glass fibers, the length of the pellets is the fiber length of the glass fibers, which is a maximum of about 20 mm. In addition, in a swirl mat system using long glass fibers, the length of the glass fibers in the roving used for production is the maximum fiber length, which can be as long as 17,000 m (17 km), but when cut to fit the size of the resin structure, the cut length is the maximum fiber length.
[0049] The average fiber diameter of the glass fibers is preferably in the range of 9 to 25 μm. When the average fiber diameter is 9 μm or more, the resin structure has sufficient rigidity and impact resistance, while when the average fiber diameter is 25 μm or less, the resin structure has good strength. From the above viewpoints, the average fiber diameter of the glass fibers is more preferably in the range of 10 to 15 μm. The average fiber diameter and average fiber length of the glass fibers can be measured by the above-mentioned method.
[0050] The material of the glass fiber used in the present invention is not particularly limited, and may be any of alkali-free glass, low-alkali glass, and alkali-containing glass, and various compositions that have conventionally been used as glass fibers can be used.
[0051] (Carbon Fiber) One of the inorganic fibers suitable for the resin composition of the present invention is carbon fiber. The suitable range of the carbon fiber is the same as that of the glass fiber.
[0052] <Optional addition ingredients> In addition to the above-mentioned components, any additive components may be blended into the resin composition of the present invention for the purpose of further improving the effects of the present invention or imparting other effects, within a range that does not significantly impair the effects of the present invention. Specific examples of such additives include colorants such as pigments, light stabilizers such as hindered amines, ultraviolet absorbers such as benzotriazoles, nucleating agents such as sorbitol, antioxidants such as phenols and phosphorus, antistatic agents such as nonionic surfactants, neutralizing agents such as inorganic compounds, antibacterial and antifungal agents such as thiazoles, flame retardants and flame retardant assistants such as halogen compounds and lignophenols, plasticizers, dispersants such as organic metal salts, lubricants such as fatty acid amides, metal deactivators such as nitrogen compounds, polyolefin resins other than the polypropylene resins, thermoplastic resins such as polyamide resins and polyester resins, and elastomers (rubber components) such as olefin elastomers and styrene elastomers. These optional components may be used in combination of two or more kinds.
[0053] Light stabilizers and ultraviolet absorbers, for example, hindered amine compounds, benzotriazoles, benzophenones, and salicylates, are effective in imparting or improving the weather resistance, durability, and the like of polypropylene resin compositions and molded articles thereof, and are effective in further improving weather discoloration resistance. Here, the method of using the light stabilizer and the ultraviolet absorber in combination is preferable because it has a large effect of improving weather resistance, durability, weather discoloration resistance, and the like.
[0054] As the antioxidant, for example, a phenol-based, phosphorus-based or sulfur-based antioxidant is effective in imparting or improving heat resistance, processing stability, heat aging resistance, etc. to a polypropylene resin composition and a molded article thereof. Furthermore, antistatic agents such as nonionic and cationic antistatic agents are effective in imparting and improving antistatic properties to resin compositions such as polypropylene-based resin compositions and resin structures formed from the resin compositions.
[0055] <Method of producing thermoplastic resin composition> As described above, the resin composition according to the present invention contains (a) a thermoplastic resin, a modified polyolefin resin added as needed, a flame retardant including an intumescent flame retardant (b1), and (c1) a copolymer added as needed. In addition, optional additives may be further blended. In the above-mentioned resin composition, when the thermoplastic resin (a) is a polypropylene resin (a-1), it may be particularly called a polypropylene resin composition (hereinafter sometimes referred to as a "PP composition"). The resin composition or PP composition can be produced by a conventional method, for example, by blending the above components, mixing, and melt-kneading. The mixing is carried out using a mixer such as a tumbler, a V blender, or a ribbon blender, and the melt kneading is carried out using equipment such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, a roll mixer, a Brabender plastograph, or a kneader, and the materials are melt kneaded and granulated.
[0056] <Method of Manufacturing Resin Structure> The resin structure of the present invention is preferably produced by impregnating a mat made of a fibrous material (hereinafter sometimes referred to as a "fiber mat") with the above-mentioned resin composition or PP composition. Examples of the impregnation method include a method of applying the resin composition or PP composition to a fiber mat, and a method of preparing a sheet of the resin composition or PP composition (hereinafter sometimes referred to as a "resin sheet" or "PP sheet"), laminating the resin sheet or PP sheet on the fiber mat, and heating and melting the resin sheet or PP sheet to impregnate the fiber mat. In the present invention, from the viewpoint of the impregnation of the resin of the resin structure into the fibers, a method of laminating a resin sheet or a PP sheet on a fiber mat and heating and melting it is preferred. In particular, the fiber mat is laminated between two resin sheets or PP sheets, and then the laminate is heated and pressurized, and then cooled and solidified to obtain the laminate. The thickness of the resin sheet or PP sheet is not particularly limited as long as it allows good impregnation into the fiber mat.
[0057] (fiber mat) The form of the fibers used in the method for producing a resin structure is not particularly limited, and various forms can be used, but a mat-like or sheet-like form is preferred. More specifically, an inorganic fiber mat is preferred, and more specifically, a mat formed from glass fibers (hereinafter referred to as a "glass fiber mat") and a mat formed from metal oxide fibers such as alumina fibers (hereinafter referred to as a "metal oxide mat") are more preferred.
[0058] The basis weight (mass per unit area) of the fiber mat is not particularly limited and is determined appropriately depending on the application, but is preferably 300 g / m 2 More preferably, 800 g / m 2 More preferably, 1500 g / m 2 The basis weight of the fiber mat is not particularly limited, but is preferably 5000 g / m 2 Less than 4500g / m 2 Less than 4000g / m 2 Less than 3500 g / m 2 The following is the result.
[0059] The basis weight per unit area of the fiber mat can be set within the above range by adjusting the amount of fibers per unit area when stacking the fiber aggregates constituting the fiber mat with a folding device. The fiber mat of the present invention may be a structure in which multiple fiber mats are bonded together, or a single structure, but a single structure is preferable in terms of handling properties and peel strength at the adhesive interface.
[0060] (fiberglass mat) Examples of the form of the glass fiber mat used in the present invention include felt and blanket processed with short fiber glass wool, chopped strand mat processed with continuous glass fiber, swirl (spiral) mat of continuous glass fiber, unidirectionally aligned mat, etc. Among these, the use of a glass fiber mat obtained by needle punching a swirl (spiral) mat of continuous glass fiber is particularly preferable because the strength and impact resistance of the resin structure are excellent.
[0061] In the method of laminating a resin sheet or a PP sheet on a fiber mat and heating and melting the same, the heating temperature is preferably 170 to 300° C. If the heating temperature is 170° C. or higher, the polypropylene resin has sufficient fluidity, and the fiber mat can be sufficiently impregnated with the PP composition, resulting in a suitable resin structure. On the other hand, if the heating temperature is 300° C. or lower, the resin composition or the PP composition does not deteriorate. Furthermore, the pressure applied is preferably 0.1 to 1 MPa. When the pressure applied is 0.1 MPa or more, the fiber mat can be sufficiently impregnated with the resin composition or PP composition, and a suitable resin structure can be obtained. On the other hand, when the pressure is 1 MPa or less, the resin composition or PP composition flows, and no burrs are generated. The cooling temperature is not particularly limited as long as it is equal to or lower than the solidification point of the thermoplastic resin in the resin composition or PP composition, but if the cooling temperature is equal to or lower than 80° C., the obtained resin structure will not be deformed when taken out. From the above viewpoints, the cooling temperature is preferably room temperature to 80° C.
[0062] Methods for obtaining a resin structure by heating and pressurizing the above-mentioned laminate and cooling the laminate include a method of press-molding the laminate in a mold equipped with a heating device, and a lamination process in which the laminate is heated and pressurized by passing it between two pairs of rollers equipped with a heating device. In particular, the lamination process is preferable because it allows continuous production and has good productivity.
[0063] (Application) Applications of the resin structure of the present invention include, for example, plastic plates which may be used as reactors for the polymerase chain reaction (PCR method) for amplifying DNA, and housings for home appliances.
[0064] (Warpage deformation of resin structure) The amount of warpage of a resin structure having a given shape was calculated and estimated based on the following method. The amount of warpage was calculated by computer simulation using commercially available molding analysis software. In the computer simulation, 3D data of the target shape and the following molding conditions were used. The molding conditions used for the calculation were a compression speed of 78 mm / sec, a compression time of 60 sec, a clamping force of 200 tons, and a mold temperature of 25°C.
[0065] (Calculation example 1-1) As shown in Fig. 4, the amount of warpage was calculated for a flat resin structure having a first surface with a plurality of grooves in a linear shape pattern, and a second surface opposite the first surface with grooves in which a plurality of partitions are periodically formed in the same linear shape pattern as the first surface. Fig. 4(a) is a perspective image seen from the first surface side, and Fig. 4(b) is a perspective image seen from the second surface side. The grooves on the second surface were positioned so as not to overlap with the grooves on the first surface when the flat resin structure was viewed as a vertical projection from the first surface. The conditions used in the groove calculation were as follows. The physical properties of the resin were density 1202 kg / m 3 The used values were a specific heat of 1395 J / (kg·°C) and a thermal conductivity of 0.27 W / (m·°C). The dimensions of the molded body were 100 mm square, 2 mm thick, and the width and depth of the grooves on the first and second surfaces were 3 mm and 1 mm, respectively. For a flat resin structure, the length and number of the partitions formed in the grooves on the second surface were changed to change the ratio (S2 / S1) of the total surface area of the grooves on the second surface to the total surface area of the grooves on the first surface, S2. The amount of warpage was calculated for each case. As a reference example, the amount of warpage was calculated in the same manner for a resin structure modified to have a plurality of grooves in a linear pattern only on the first surface and no grooves on the second surface, and a resin structure modified to have a plurality of grooves in a linear pattern on both the first and second surfaces and no partitions on the grooves on the second surface. The results are shown in Table 1.
[0066] [Table 1]
[0067] From Table 1, it can be seen that when the ratio (S2 / S1) of the sum of the surface areas of the second surfaces (S2) to the sum of the surface areas of the first surfaces (S1) is 0.5 or more and 1.4 or less, the amount of warping deformation is small and good.
[0068] (Calculation example 1-2) As in Calculation Example 1-1, the amount of warpage was calculated for a flat resin structure having a first surface with a plurality of grooves in a linear shape pattern, and a second surface opposite the first surface with grooves in which a plurality of partitions are periodically formed in the same linear shape pattern as the first surface. The grooves on the second surface were positioned so as not to overlap with the grooves on the first surface when the flat resin structure was viewed as a vertical projection from the first surface. The conditions used in the calculation were as follows. The physical properties of the resin were density 1202 kg / m 3 The specifications used were a specific heat of 1395 J / (kg·°C) and a thermal conductivity of 0.27 W / (m·°C). The dimensions of the molded body were a resin structure 100 mm square, 2 mm thick, with the width and depth of the grooves on the first and second surfaces being 3 mm and 1 mm, respectively. However, unlike the case of Calculation Example 1-1, for the flat resin structure, the ratio (S2 / S1) of the total surface area of the grooves on the second surface (S2) to the total surface area of the grooves on the first surface (S1) was fixed at 1, while the length and number of the partitions formed in the grooves on the second surface were changed to change the ratio (V2 / V1) of the total volume of the grooves on the second surface (V2) to the total volume of the grooves on the first surface (V1), and the amount of warpage was calculated for each case. The results are shown in Table 2.
[0069] [Table 2]
[0070] From Table 1, it can be seen that, when the ratio (S2 / S1) of the total surface area of the second surface (S2) to the total surface area of the first surface (S1) is fixed at 1, if the ratio (V2 / V1) of the total volume of the grooves of the second surface (V2) to the total volume of the grooves of the first surface (V1) is 0.4 to 0.9, the increase in the amount of warpage deformation is suppressed. In addition, the volume of the grooves is reduced, and the decrease in rigidity is also suppressed.
[0071] (Calculation example 2-1) As shown in Figure 5, the amount of warpage was calculated for a flat resin structure having grooves in a perfect circular pattern on a first surface, and a groove in which a plurality of partitions are periodically formed in the same perfect circular pattern as on the first surface on a second surface opposite the first surface. Figure 5(a) is a perspective image seen from the first surface side, and Figure 5(b) is a perspective image seen from the second surface side. The grooves on the second surface were positioned so as not to overlap with the grooves on the first surface when the flat resin structure was viewed as a perpendicular projection from the first surface. The conditions used in the calculation were as follows. The physical properties of the resin were density 1202 kg / m 3 The used values were a specific heat of 1395 J / (kg·°C) and a thermal conductivity of 0.27 W / (m·°C). The dimensions of the molded body were: resin structure 10 was 100 mm square, 2 mm thick, the groove portion on the first surface had a diameter of 60 mm, a width of 5 mm and a depth of 1 mm, and the groove portion on the second surface had a diameter of 73.7 mm, a width of 3.7 mm and a depth of 1 mm. For a flat resin structure, the length and number of the partitions formed in the grooves on the second surface were changed to change the ratio (S2 / S1) of the total surface area of the grooves on the second surface to the total surface area of the grooves on the first surface, S2. The amount of warpage was calculated for each case. As a reference example, the amount of warpage was calculated in the same manner for a resin structure modified to have a groove with a perfect circular pattern only on the first surface and no groove on the second surface, and a resin structure modified to have grooves with a perfect circular pattern on both the first and second surfaces and no partitions formed in the grooves on the second surface. The results are shown in Table 3.
[0072] [Table 3]
[0073] From Table 3, it can be seen that when the ratio (S2 / S1) of the sum of the surface areas of the second faces (S2) to the sum of the surface areas of the first faces (S1) is 0.5 or more and 1.4 or less, the amount of warpage deformation is good.
[0074] (Calculation example 2-2) As in Calculation Example 2-1, the amount of warpage was calculated for a flat resin structure having a first surface with a groove portion in a perfect circular pattern, and a second surface opposite the first surface with a groove portion in which a plurality of partitions are periodically formed in the same perfect circular pattern as the first surface. The groove portion on the second surface was positioned so as not to overlap with the groove portion on the first surface when the flat resin structure was viewed as a perpendicular projection from the first surface. The conditions used in the calculation were as follows. The physical properties of the resin were density 1202 kg / m 3 The used values were a specific heat of 1395 J / (kg·°C) and a thermal conductivity of 0.27 W / (m·°C). The dimensions of the molded body were: resin structure 10 was 100 mm square, 2 mm thick, the groove portion on the first surface had a diameter of 60 mm, a width of 5 mm and a depth of 1 mm, and the groove portion on the second surface had a diameter of 73.7 mm, a width of 3.7 mm and a depth of 1 mm. However, unlike the case of Calculation Example 2-1, for the flat resin structure, the ratio (S2 / S1) of the total surface area of the grooves on the second surface (S2) to the total surface area of the grooves on the first surface (S1) was fixed at 1, while the length and number of the partitions formed in the grooves on the second surface were changed to change the ratio (V2 / V1) of the total volume of the grooves on the second surface (V2) to the total volume of the grooves on the first surface (V1), and the amount of warpage was calculated for each case. The results are shown in Table 4.
[0075] [Table 4]
[0076] From Table 4, it can be seen that, when the ratio (S2 / S1) of the total surface area of the second surface (S2) to the total surface area of the first surface (S1) is fixed at 1, if the ratio (V2 / V1) of the total volume of the grooves of the second surface (V2) to the total volume of the grooves of the first surface (V1) is 0.2 or more and 0.9 or less, the increase in the amount of warpage deformation is suppressed. In addition, the volume of the grooves is reduced, and the decrease in rigidity is also suppressed.
[0077] (Consideration) In the above Calculation Examples 1-1 and 1-2, the amount of warpage was calculated for a resin structure having grooves in a linear shape pattern, and in the above Calculation Examples 2-1 and 2-2, the amount of warpage was calculated for a resin structure having grooves in a circular shape pattern. In a resin structure having grooves in a linear shape pattern, when the ratio (S2 / S1) of the total surface area (S2) of the second surface to the total surface area (S1) of the first surface is 0.5 to 1.4, and the ratio (V2 / V1) of the total volume (V2) of the grooves in the second surface to the total volume (V1) of the grooves in the first surface is 0.4 to 0.9, the amount of warpage of the resin structure is good and the decrease in rigidity is also suppressed. On the other hand, in a resin structure having grooves with a circular shape pattern, when the ratio (S2 / S1) of the sum of the surface areas of the second surfaces (S2) to the sum of the surface areas of the first surfaces (S1) is 0.5 or more and 1.4 or less, and the ratio (V2 / V1) of the sum of the volumes of the grooves of the second surfaces (V2) to the sum of the volumes of the grooves of the first surfaces (V1) is 0.2 or more and 0.9 or less, the amount of warping deformation of the resin structure is good and a decrease in rigidity is also suppressed. Regarding the shape pattern of the groove portions of the resin structure, any shape pattern can be specified by combining curved portions (circular) and straight portions (straight line). Therefore, it is presumed that a resin structure having groove portions of any shape pattern, in which the depth (h1) of the groove portion on the first surface and the depth (h2) of the groove portion on the second surface are both equal to or greater than 1 / 2 of the thickness T of the flat plate structure, will have a good amount of warping deformation of the resin structure and suppress a decrease in rigidity within a numerical range obtained by averaging the numerical ranges shown by the respective calculation results for the case having groove portions of a straight-line shape pattern and the case having groove portions of a perfect circular shape pattern. That is, in a resin structure having grooves of any shape pattern, the depth (h1) of the grooves on the first surface and the depth (h2) of the grooves on the second surface are both equal to or greater than 1 / 2 of the thickness T of the flat plate structure, and when the ratio (S2 / S1) of the total surface area (S2) of the second surface to the total surface area (S1) of the first surface is 0.5 or more and 1.4 or less, and the ratio (V2 / V1) of the total volume (V2) of the grooves on the second surface to the total volume (V1) of the grooves on the first surface is 0.3 or more and 0.9 or less, it is considered that the amount of warping deformation of the resin structure is good and a decrease in rigidity is also suppressed. [Industrial Applicability]
[0078] The resin structure of the present invention is suppressed in warping and has excellent rigidity, and therefore can be suitably used for plastic plates that are sometimes used as reactors in the PCR method for amplifying DNA, housings of home appliances, and the like. [Explanation of symbols]
[0079] 10 Resin structure 100 flat plate structure 110 First Side 111 Groove portion of the first surface 120 Second Side 121 Groove portion of second surface h1: Depth of the groove on the first surface h2: Depth of the groove on the second surface T Thickness of the plate structure
Claims
1. A resin structure having a flat plate structure having a first surface and a second surface opposite to the first surface, The flat plate structure has a groove on both the first surface and the second surface, The depth (h 1 ) and the depth (h 2 ) are each equal to or greater than 1 / 2 of the thickness T of the flat plate structure, the grooves on the first surface and the grooves on the second surface are arranged such that the grooves on the first surface and the grooves on the second surface do not overlap with each other when the flat plate structure is viewed in vertical projection from the first surface side; a ratio (S2 / S1) of the sum of the surface areas of the groove portions of the second surface (S2) to the sum of the surface areas of the groove portions of the first surface (S1) is 0.5 or more and 1.4 or less; A resin structure, wherein a ratio (V2 / V1) of a total volume (V2) of the groove portions of the second surface to a total volume (V1) of the groove portions of the first surface is 0.3 or more and 0.9 or less.
2. The first surface has at least one groove having a length of 90% or more of the shortest side of the flat plate structure, The resin structure according to claim 1 , wherein the second surface does not have a groove having a length of 90% or more of the length of the shortest side of the flat plate structure.
3. The resin structure according to claim 1 , wherein the first surface has a groove portion having a curved portion and a straight portion.
4. The resin structure includes a resin composition, The resin structure according to claim 1 or 2, wherein the resin composition comprises a thermoplastic resin.
5. The resin structure includes a resin composition. The resin structure according to claim 1 or 2, wherein the resin composition contains a fibrous material.
6. The resin structure includes a resin composition, The resin structure according to claim 1 or 2, wherein the resin composition contains an intumescent flame retardant.
7. The resin structure according to claim 6 , wherein the intumescent flame retardant comprises a compound having a melamine structure or a piperazine structure.
8. 5. The resin structure according to claim 4, wherein the resin structure is a mat made of inorganic fibers impregnated with the resin composition.
Citation Information
Patent Citations
Manufacture of diaphragm having uneven multi-grooved structure
JP1991000377A
Flame-retardant polyamide resin composition
JP2012214559A
Film having exceptional embossability, and film having convex parts and concave parts
WO2017146051A1
Stampable sheet and molded body using same
WO2022220303A1
Plastic plate and plate
JP2005061919A