Cement composition, method for manufacturing the same, and cement milk

By using light calcium carbonate and a controlled thickener content in cement compositions, the manufacturing process emits less carbon dioxide and produces suitable cement milk for semi-flexible pavements, addressing emission reduction and workability challenges.

JP2024145396AInactive Publication Date: 2024-10-15MU MATEX CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023057721
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge is to reduce carbon dioxide emissions during the manufacturing of cement compositions used for forming semi-flexible pavements while maintaining the physical properties and workability of the cement milk.

Method used

Incorporating light calcium carbonate and adjusting the content of a thickener in the cement composition, along with other admixtures, to create a cement milk with reduced emissions and suitable viscosity for semi-flexible pavement formation.

Benefits of technology

The solution results in a cement composition with lower carbon dioxide emissions and produces cement milk that maintains workability and physical properties, facilitating the construction of semi-flexible pavements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145396000001
    Figure 2024145396000001
  • Figure 2024145396000002
    Figure 2024145396000002
  • Figure 2024145396000003
    Figure 2024145396000003
Patent Text Reader

Abstract

To provide a cement component which is designed to decrease an amount of emission of CO2 during manufacturing and by which it is possible to obtain cement milk suitable for forming a semi-flexible pavement.SOLUTION: One aspect of the present disclosure provides a cement composition containing cement, a fine aggregate, and an admixture material. The admixture material includes light calcium carbonate, a thickener, and a polymer. Density of the light calcium carbonate is 2.65 g / cm3 or less. A content of the thickener is 0.03 pt.mass or less with respect to a total of 100 pts.mass of the cement, the fine aggregate, and light calcium carbonate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a cement composition and a method for producing the same, and a cement milk. [Background technology]

[0002] Semi-flexible pavements are pavements that combine the "flexibility" of asphalt pavements with the "rigidity" of concrete pavements, and can be formed by infiltrating a special cement milk into the voids of an open-graded asphalt mix.

[0003] In cement compositions for forming semi-flexible pavement, calcium carbonate is sometimes used as an admixture material with the aim of controlling the physical properties of the hardened body. For example, Patent Document 1 discloses a semi-flexible pavement injection material characterized by containing cement, calcium carbonate powder, re-emulsified powdered resin, and a water-reducing agent, and describes that the semi-flexible pavement injection material solves the problem of providing a semi-flexible pavement injection material that is easy to work with, does not cause settlement of the material during injection, and provides good physical properties of the semi-flexible pavement after injection. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-278901 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand to reduce carbon dioxide (CO2) emissions during the production of cement products.

[0006] The present disclosure aims to provide a cement composition that reduces CO2 emissions during production and that can produce cement milk suitable for forming semi-flexible pavement. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by using precipitated calcium carbonate in a cement composition and adjusting the content of a thickener.

[0008] This disclosure provides the following [1] to [9]. [1] Contains cement, fine aggregate and admixtures, The admixture comprises precipitated calcium carbonate, a thickener and a polymer; The density of light calcium carbonate is 2.65g / cm 3 is as follows: A cement composition comprising a thickener in an amount of 0.03 parts by mass or less per 100 parts by mass of the total of cement, fine aggregate, and precipitated calcium carbonate. [2] The cement composition according to [1], wherein the content of the precipitated calcium carbonate is 5 to 80 parts by mass per 100 parts by mass of the cement. [3] The cement composition according to [1] or [2], which is mixed with water and used as cement milk for semi-flexible pavement. [4] The cement composition according to any one of [1] to [3], wherein when 50 parts by mass of water are mixed with 100 parts by mass of the cement composition to prepare cement milk, the viscosity of the cement milk at 20°C is 150 to 500 mPa s. [5] The cement composition according to any one of [1] to [4], wherein a bleeding rate is 3.50 volume % or less when 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk and the cement milk is allowed to stand for 3 hours. [6] A cement milk comprising the cement composition according to any one of [1] to [5] and water. [7] The cement milk according to [6], wherein the water content is 40 to 60 parts by mass per 100 parts by mass of the cement composition. [8] A step of preparing light calcium carbonate by contacting CO2 with milk of lime in which at least one of quicklime and slaked lime is dispersed in water; A method for producing a cement composition, comprising: mixing an admixture containing light calcium carbonate, a thickener and a polymer, cement, and a fine aggregate, The CO2 balance in the process of preparing light calcium carbonate is -300 kg CO2 / t or less, A method for producing a cement composition, wherein the amount of a thickener is 0.03 parts by mass or less per 100 parts by mass of the total amount of the precipitated calcium carbonate, cement, and fine aggregate. [9] The method according to [8], wherein the CO2 contacted with the milk of lime contains CO2 derived from exhaust gas from a cement factory. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a cement composition that reduces CO2 emissions during production and that can produce cement milk suitable for forming semi-flexible pavement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the following description, when it is written "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified.

[0011] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0012] <Cement composition> One embodiment of the cement composition according to the present disclosure includes cement, fine aggregate, and admixture, the admixture including precipitated calcium carbonate, a thickener, and a polymer. The cement composition may also be referred to as a hydraulic composition.

[0013] Cement means fine powder of mineral matter that reacts with water and hardens. The cement may be Portland cement as specified in JIS R 5210:2009 "Portland cement". The Portland cement may be, for example, ordinary Portland cement, early strength Portland cement, moderate heat Portland cement, low heat Portland cement, etc. In addition, as another cement, for example, it is preferable to use at least one of blast furnace cement as specified in JIS R 5211:2009 "Blast furnace cement" and fly ash cement as specified in JIS R 5213:2019 "Fly ash cement" because it is possible to reduce carbon dioxide emissions during cement production. The cement preferably contains at least one of ordinary Portland cement and early strength Portland cement.

[0014] In the above cement composition, the content of cement may be 30 parts by mass or more, 40 parts by mass or more, 50 parts by mass or more, 55 parts by mass or more, or 60 parts by mass or more, and may be 90 parts by mass or less, 80 parts by mass or less, or 70 parts by mass or less, per 100 parts by mass in total of the cement, fine aggregate, and light calcium carbonate.

[0015] The fine aggregate may be one that passes entirely through a mesh sieve with 10 mm openings and 85% or more by mass through a mesh sieve with 5 mm openings. Examples of fine aggregate include silica sand, river sand, land sand, sea sand, crushed sand, etc.

[0016] In the above cement composition, the content of the fine aggregate may be 5 parts by mass or more, or 10 parts by mass or more, and may be 30 parts by mass or less, or 20 parts by mass or less, per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate.

[0017] Light calcium carbonate is chemically produced using limestone as a raw material, and is different from heavy calcium carbonate, which is produced by crushing and classifying limestone. Light calcium carbonate can be prepared by reacting milk of lime with carbon dioxide.

[0018] In the above cement composition, the density of the precipitated calcium carbonate is 2.65 g / cm 3 Heavy calcium carbonate is mainly made up of calcite (density: approx. 2.71 g / cm3), which has the most stable crystal structure. 3 ), so the density is about 2.7g / cm 3 In the present specification, density means true density unless otherwise specified. In the present specification, the density of the precipitated calcium carbonate is preferably determined by a pycnometer method using a pycnometer. The density of the precipitated calcium carbonate may be determined, for example, by a gas phase displacement method or a method using a Le Chatelier flask according to "Physical Testing Methods for Cement" and "7 Density Test" defined by JIS R 5201.

[0019] The Blaine specific surface area of ​​light calcium carbonate is 1000 cm 2 / g or more, 1500cm 2 / g or more, 2000cm 2 / g or more, 2300cm 2 / g or more, 2500cm 2 / g or more, or 2700 cm 2 / g or more. The Blaine specific surface area of ​​the precipitated calcium carbonate is 7000 cm 2 / g or less, 6000cm 2 / g or less, 5000cm 2 / g or less, 4000cm 2 / g or less, 3500cm 2 / g or less, or 3000cm 2 In this specification, the Blaine specific surface area refers to a value measured in accordance with the method described in JIS R 5201:2015 "Physical testing methods for cement."

[0020] The content of the light calcium carbonate may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, 20 parts by mass or more, or 30 parts by mass or more, relative to 100 parts by mass of the cement content. The content of the light calcium carbonate may be 100 parts by mass or less, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of the cement content. The content of the light calcium carbonate may be, for example, 1 to 100 parts by mass, or 5 to 80 parts by mass, relative to 100 parts by mass of the cement content.

[0021] The content of the light calcium carbonate may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 20 parts by mass or more per 100 parts by mass of the total of the cement, fine aggregate, and light calcium carbonate. The content of the light calcium carbonate may be 50 parts by mass or less, 40 parts by mass or less, or 30 parts by mass or less per 100 parts by mass of the total of the cement, fine aggregate, and light calcium carbonate.

[0022] Examples of thickeners include organic thickeners such as cellulose-based thickeners, starch-based thickeners, guar gum-based thickeners, and vinyl-based thickeners, and inorganic thickeners such as bentonite, kaolinite, talc, etc. One of these may be used alone, or two or more may be used in combination.

[0023] The content of the thickener is 0.03 parts by mass or less per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate. The content of the thickener may be less than 0.03 parts by mass or 0.02 parts by mass or less per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate. When the content of the thickener is equal to or less than the upper limit, the viscosity of the obtained cement milk is lowered, the injectability of the cement milk into the pavement is improved, and the cement milk is more suitable for forming a semi-flexible pavement. The content of the thickener may be 0.001 parts by mass or more, or 0.005 parts by mass or more per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate. When the content of the thickener is equal to or more than the lower limit, the viscosity of the obtained cement milk is higher, the material separation of the cement milk is less likely to occur, the bleeding rate is smaller, and the strength is easily maintained.

[0024] The polymer may be a known polymer for cement, a polymer for cement admixture, or the like. The polymer may be, for example, at least one selected from the group consisting of a re-emulsified powder polymer, a water-soluble polymer, and a liquid polymer. Examples of the re-emulsified powder polymer include vinyl acetate-based polymers and acrylic acid ester-based polymers. Examples of the vinyl acetate-based polymer include ethylene vinyl acetate and vinyl acetate vinyl versatate (VAVeoVa). Examples of the acrylic acid ester-based polymer include styrene acrylic acid ester and polyacrylic acid ester. Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, and polyacrylates. Examples of the cellulose derivatives include methyl cellulose and hydroxypropyl methyl cellulose. Examples of the polyacrylates include calcium polyacrylate and magnesium polyacrylate. Examples of the liquid polymer include unsaturated polyester resins and epoxy resins.

[0025] In the above cement composition, the polymer content may be 0.1 parts by mass or more, 0.5 parts by mass or more, or 0.7 parts by mass or more per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate, and may be 5 parts by mass or less, 3 parts by mass or less, or 2 parts by mass or less per 100 parts by mass of the total of the cement, the fine aggregate, and the light calcium carbonate.

[0026] In the cement composition, the content of the polymer relative to 100 parts by mass of the cement may be 0.5 parts by mass or more, 0.8 parts by mass or more, 1.0 parts by mass or more, or 1.3 parts by mass or more. The mass ratio may be 5.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, or 2.0 parts by mass or less.

[0027] The admixture may include a rapid-setting admixture. Rapid-setting properties can be imparted to the cement milk by replacing a portion of the cement with the rapid-setting admixture. The rapid-setting admixture may be a mixture of calcium aluminate and gypsum. The content of the rapid-setting admixture may be 10 parts by mass or more, or 15 parts by mass or more, per 100 parts by mass of the cement and the rapid-setting admixture in total. The content of the rapid-setting admixture may be 40 parts by mass or less, or 35 parts by mass or less, per 100 parts by mass of the cement and the rapid-setting admixture in total.

[0028] The admixture may contain other components (hereinafter, simply referred to as "other components") other than the light calcium carbonate, thickener, polymer, and fast-hardening admixture. Examples of the other components include defoamers, water-reducing agents, air-enhancing agents, water retention agents, hardening accelerators, setting regulators (setting retarders, etc.), rebar rust inhibitors, expanders, silica fume, etc. The content of the other components may be 0.01 parts by mass or more and 0.3 parts by mass or less relative to 100 parts by mass of the total of the cement, fine aggregate, and light calcium carbonate.

[0029] The cement composition can be mixed with water to prepare cement milk. The cement milk obtained by mixing the cement composition with water is suitable for semi-flexible pavement. Therefore, the cement composition may be mixed with water and used as cement milk for semi-flexible pavement.

[0030] When 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk, the viscosity of the cement milk at 20°C may be 150 to 500 mPa·s. The viscosity may be 200 to 400 mPa·s, or may be 300 to 400 mPa·s. When the viscosity is equal to or greater than the lower limit, the occurrence of bleeding is more easily suppressed. When the viscosity is equal to or less than the upper limit, the filling property of the cement milk tends to be improved. The viscosity of the cement milk at 20°C means a value measured by a B-type viscometer. More specifically, the viscosity of the cement milk at 20°C is measured by the method described in the Examples.

[0031] When 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk and the cement milk is left for 3 hours, the bleeding rate may be 3.50% by volume or less. The bleeding rate may be 3.30% by volume or less, 3.00% by volume or less, or 2.70% by volume or less.

[0032] The bleeding rate means a value obtained by the following method. In an environment of 20±3°C, 1000 mL of cement milk is poured into a watertight and strong container, the container is covered, and the container is left on a horizontal table for 3 hours from the time of pouring water during the production of the cement milk. The amount of water that seeps out onto the surface (bleeding water amount) is measured in 1 mL units. Based on the measured value, the bleeding rate is calculated by the following formula. More specifically, the bleeding rate is measured by the method described in the Examples. The bleeding rate value is rounded off to two decimal places to obtain a value to two decimal places. Bleeding rate (volume%) = (Bleeding water volume (mL) / 1000mL) x 100

[0033] <Cement milk> One embodiment of the cement milk according to the present disclosure includes the above-mentioned cement composition and water. The content of water may be 20 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more, relative to 100 parts by mass of the cement composition. The content of water may be 80 parts by mass or less, 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, relative to 100 parts by mass of the cement composition. The content of water may be 30 to 70 parts by mass, or 40 to 60 parts by mass.

[0034] As described above, the cement milk obtained by mixing the cement composition with water is suitable for semi-flexible pavement. The present disclosure can also be said to provide a method for constructing semi-flexible pavement, which includes filling voids in an asphalt mixture with the cement milk. The asphalt mixture may be, for example, a mixture of aggregate (crushed stone, sand, etc.), filler (stone powder, etc.), and asphalt. The construction method may include spreading the asphalt mixture evenly. In the spread asphalt mixture, voids exist between particles of aggregate, etc. A semi-flexible pavement can be constructed by filling voids in the asphalt mixture with cement milk and then hardening the cement milk.

[0035] <Method of manufacturing cement composition> One embodiment of a method for producing a cement composition according to the present disclosure includes a step of preparing light calcium carbonate by contacting CO with milk of lime in which at least one of quicklime and slaked lime is dispersed in water (hereinafter also referred to as a "light calcium carbonate preparation step"), and a step of mixing light calcium carbonate, an admixture containing a thickener and a polymer, cement, and fine aggregate (hereinafter also referred to as a "mixing step").

[0036] Milk of lime is a suspension of slaked lime (Ca(OH)2) and is prepared by dispersing at least one of quick lime (CaO) and slaked lime in water. When quick lime is dispersed in water, the quick lime reacts with the water to produce slaked lime.

[0037] Light calcium carbonate is prepared by contacting milk of lime with CO2. Contacting milk of lime with CO2 may be, for example, blowing CO2 into milk of lime. CO2 to be contacted with milk of lime may include CO2 derived from exhaust gas. CO2 derived from exhaust gas may be, for example, CO2 derived from exhaust gas of a cement factory. By using CO2 derived from exhaust gas of a cement factory as CO2 to be contacted with milk of lime, it is possible to further reduce the apparent CO2 emission amount during the production of a cement composition. The apparent CO2 emission amount during the production of a cement composition means a value obtained by subtracting the amount of CO2 consumed during the production of a cement composition from the amount of CO2 emitted during the production of the cement composition (including the production of raw materials for the cement composition. The same applies below).

[0038] The CO2 balance in the light calcium carbonate preparation process may be 0 kgCO2 / t or less, -150 kgCO2 / t or less, or -300 kgCO2 / t or less. The CO2 balance in the light calcium carbonate preparation process can be obtained by subtracting the mass (kg) of CO2 adsorbed and fixed in calcium carbonate by producing 1 ton of light calcium carbonate from the mass (kg) of CO2 emitted by producing 1 ton of light calcium carbonate. In addition, the CO2 balance in the light calcium carbonate preparation process may be, for example, -1000 kgCO2 / t or more, or -500 kgCO2 / t or more.

[0039] The CO balance due to the effect of the light calcium carbonate of the cement composition (CO balance due to the effect of the light calcium carbonate when producing 1 t of the cement composition) may be, for example, -50 kg CO / t or less, or -80 kg CO / t or less. In addition, the CO balance due to the effect of the light calcium carbonate of the cement composition may be, for example, -500 kg CO / t or more, or -250 kg CO / t or more.

[0040] The admixture used in the mixing step includes light calcium carbonate, a thickener, and a polymer. As the light calcium carbonate, the light calcium carbonate described above as the light calcium carbonate in the cement composition can be used.

[0041] The amount of the precipitated calcium carbonate per 100 parts by mass of the cement may be within the above-mentioned numerical range as the content of the precipitated calcium carbonate per 100 parts by mass of the cement in the cement composition.

[0042] The amount of light calcium carbonate per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate may be within the above-mentioned numerical range as the content of light calcium carbonate per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate in the cement composition.

[0043] As the thickener, the thickeners mentioned above as the thickener for the cement composition can be used.

[0044] The amount of the thickener is 0.03 parts by mass or less per 100 parts by mass of the total amount of the precipitated calcium carbonate, cement and fine aggregate.

[0045] The amount of the thickener to be mixed per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate may be within the above-mentioned numerical range as the content of the thickener per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate in the cement composition.

[0046] As the polymer, the polymers described above as the polymer in the cement composition can be used.

[0047] The amount of the polymer to be mixed per 100 parts by mass of the total of the amounts of the light calcium carbonate, the cement, and the fine aggregate may be within the above-mentioned numerical range as the content of the polymer per 100 parts by mass of the total of the light calcium carbonate, the cement, and the fine aggregate in the cement composition.

[0048] The amount of the polymer to be blended per 100 parts by mass of cement may be within the above-mentioned numerical range as the content of the polymer per 100 parts by mass of cement in the cement composition.

[0049] The admixture may include a fast-setting admixture and may include other components. As the fast-setting admixture and other components, the fast-setting admixture and other components described above as the fast-setting admixture and other components in the cement composition can be used, respectively.

[0050] The amount of the rapid-hardening admixture per 100 parts by mass of the total amount of the cement and the rapid-hardening admixture in the cement composition may be within the above-mentioned numerical range as the content of the rapid-hardening admixture per 100 parts by mass of the total amount of the cement and the rapid-hardening admixture.

[0051] The amount of other components to be mixed per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate may be within the above-mentioned numerical range as the content of other components per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate in the cement composition.

[0052] As the cement and the fine aggregate, the cement and the fine aggregate described above as the cement and the fine aggregate in the cement composition can be used, respectively.

[0053] The amounts of cement and fine aggregate per 100 parts by mass of the total of the amounts of light calcium carbonate, cement, and fine aggregate may be within the numerical ranges described above as the contents of cement and fine aggregate per 100 parts by mass of the total of the light calcium carbonate, cement, and fine aggregate in the cement composition. EXAMPLES

[0054] The present disclosure will be described in more detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the following examples.

[0055] In the following Examples and Comparative Examples, the components shown in Table 1 below were used as raw materials.

[0056] [Table 1]

[0057] [Analysis of heavy calcium carbonate and light calcium carbonate] The chemical compositions of the heavy calcium carbonate (LSP) and light calcium carbonate (ET) were determined in accordance with JIS R 5202:2010 "Methods for chemical analysis of cement". The results are shown in Table 2. Table 2 also shows the values ​​of loss on ignition (sometimes written as ig. loss). The loss on ignition was measured in accordance with the method described in "5.2 Cases other than blast furnace cement and blast furnace slag" in "5. Methods for determining loss on ignition" of JIS R 5202:2010. In addition, the true density of LSP and ET was determined using a fully automatic pycnometer (manufactured by Anton Paar Japan Co., Ltd., product name "Fully automatic pycnometer Pentapyc5200e"). The results are shown in Table 3. The Blaine specific surface area of ​​ET was determined in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement", and was 2840 cm 2 / g.

[0058] [Table 2]

[0059] [Table 3]

[0060] [Manufacture of Cement Composition and Cement Milk] By mixing each component at the mixing ratio shown in Table 4, the cement compositions according to Comparative Examples 1 and 2 and Example 1 were manufactured. Further, 50 parts by mass of water was added to 100 parts by mass of each cement composition, and using a Three One Motor BL1200 (with turbine blades), the cement milk according to Comparative Examples 1 and 2 and Example 1 was prepared by kneading at a rotation speed of 800 rpm for 2 minutes.

[0061] [Evaluation] For the manufactured cement milk and cement composition, the following tests were conducted to obtain the evaluation values in each test. The results are shown in Table 4. Also, the suitable ranges of each evaluation value are shown in Table 5. When the evaluation value is within the suitable range shown in Table 5, it can be said that it is a cement milk suitable for forming a semi-flexible pavement.

[0062] [CO2 Balance] The CO2 balance during the manufacture of the light calcium carbonate used as the admixture was -390 kg / t. This is because the mass of CO2 adsorbed and immobilized on calcium carbonate by manufacturing 1 t of light calcium carbonate is 440 kg, and the mass of CO2 emitted by manufacturing 1 t of light calcium carbonate is 50 kg. In the cement compositions of Example 1 and Comparative Example 2, 22 parts by mass of light calcium carbonate is blended with respect to a total of 101.14 parts by mass of cement, fine aggregate, and admixture. Therefore, the CO2 balance due to the effect of light calcium carbonate was calculated to be -84.8 kg per 1 t of the cement composition. For Comparative Example 1 using heavy calcium carbonate instead of light calcium carbonate, for the sake of convenience, the CO2 balance was described as 0.

[0063] [Viscosity] The viscosity of the cement milk immediately after production (within 60 seconds after production) was measured using a B-type rotational viscometer (manufactured by BROOK FIELD, product name "LVDV-A"). The measurement was carried out in an environment at room temperature of 20°C.

[0064] <P-funnel flow time> In accordance with JSCE-F521-1999 "Test Method for Fluidity of Injection Mortar for Prepacked Concrete (Method Using P-Funnel)", the P-funnel flow time of the cement milk was measured. The measurement was carried out in an environment at room temperature of 20°C.

[0065] <Bleeding rate> A container with a capacity of 1000 mL, which is watertight and strong (manufactured by AS ONE Corporation, product name "Disposable Cup (Blow Molded) 1000 mL") was prepared. The following tests were conducted in an environment of 20 ± 3°C. The prepared container was filled with cement milk up to the 1000 mL line, and the container was gently tapped so that the surface of the sample became smooth. Next, the container containing the sample was placed on a horizontal table so as not to vibrate, and covered with a plastic plate. During the test, the lid was always kept on except when water was being absorbed. Three hours after the water injection time during the production of the cement milk, the water that had oozed out on the surface of the sample was absorbed. Using a graduated cylinder, the amount of water absorbed (bleeding water volume) was measured in 1 mL units. Based on the results of the above tests, the bleeding rate was calculated using the following formula. The third decimal place was rounded off to obtain a value up to two decimal places. Bleeding rate (volume %) =(Bleeding water volume (mL) / 1000 mL)×100

[0066] <Setting time> In accordance with JIS R 5201:2015 9.4.3 "Measurement of Initial and Final Setting", the setting time (initial and final) was determined. However, the measurement interval was in 10-minute units.

[0067] <Compressive strength and flexural strength of hardened body> The above cement milk was used instead of the specified mortar for the preparation of the test specimens, and 4cm x 4cm x 16cm test specimens were prepared in accordance with JIS R 5201:2015. However, the test specimens were prepared by pouring the cement milk, demolded the next day, and cured in water for 7 days, and the compressive strength and flexural strength of the test specimens (hardened bodies) were measured at 7 days. The tests were conducted in an environment at room temperature of 20℃.

[0068] [Table 4]

[0069] [Table 5]

Claims

1. Contains cement, fine aggregate and admixtures, The admixture comprises precipitated calcium carbonate, a thickener and a polymer; The density of the precipitated calcium carbonate is 2.65 g / cm 3 is as follows: A cement composition comprising the thickener in an amount of 0.03 parts by mass or less per 100 parts by mass of the cement, the fine aggregate, and the light calcium carbonate combined.

2. The cement composition according to claim 1, wherein the content of the light calcium carbonate is 5 to 80 parts by mass per 100 parts by mass of the cement.

3. 3. The cement composition according to claim 1 or 2, which is mixed with water and used as a cement milk for semi-flexible paving.

4. The cement composition according to claim 1 or 2, wherein the viscosity of the cement milk at 20°C when 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare the cement milk is 150 to 500 mPa·s.

5. 3. The cement composition according to claim 1 or 2, wherein the bleeding rate is 3.50 vol% or less when 50 mass parts of water are mixed with 100 mass parts of the cement composition to prepare cement milk and the cement milk is allowed to stand for 3 hours.

6. A cement milk comprising the cement composition according to claim 1 or 2 and water.

7. The cement milk according to claim 6, wherein the water content is 40 to 60 parts by mass per 100 parts by mass of the cement composition.

8. At least one of quicklime and slaked lime is dispersed in water, and then CO 2 preparing precipitated calcium carbonate by contacting A method for producing a cement composition, comprising: mixing the light calcium carbonate, a thickener, and a polymer-containing admixture, cement, and fine aggregate, In the step of preparing the light calcium carbonate, 2 Balance is -300kgCO 2 / t or less, A method for producing a cement composition, wherein the thickener is mixed in an amount of 0.03 parts by mass or less per 100 parts by mass of the total amount of the precipitated calcium carbonate, the cement, and the fine aggregate.

9. The CO 2 However, CO from exhaust gases from cement factories 2 The method of claim 8, comprising:

Citation Information

Patent Citations

  • Half-flexible grouting material and pavement construction using the same

    JP1999278901A