Coating composition for surface protective layer formation and coated body

The coating composition with enhanced weather resistance and chemiluminescence-based prediction addresses the inadequacies of existing protective layers, ensuring long-term protection and efficient prediction of weather resistance for building materials.

JP2024146381APending Publication Date: 2024-10-15DAI NIPPON TORYO CO LTD

Patent Information

Application Number
JP2023059243
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing surface protective layers for building materials fail to provide sufficient weather resistance, especially when used with active energy ray-curable inks or photocatalyst layers, and there is a lack of a reliable method to predict weather resistance without lengthy testing.

Method used

A coating composition that forms a surface protective layer with an apparent activation energy of 35 kJ/mol or more, determined through chemiluminescence measurement, and includes ultraviolet absorbers and radical scavengers to enhance weather resistance, along with a method to predict weather resistance using chemiluminescence analysis.

Benefits of technology

The coating composition achieves high weather resistance, protecting the design layer for an extended period and providing a reliable method to predict weather resistance in a short time, even with active energy ray-curable inks or photocatalyst layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146381000001_ABST
    Figure 2024146381000001_ABST
Patent Text Reader

Abstract

To provide a coating composition capable of forming a surface protective layer which may achieve high level weathering resistance, and can protect design thereof for a long term, even when a design layer is formed of active energy ray-curable ink or a photocatalyst layer exists in an outermost layer.SOLUTION: There is provided a coating composition for surface protective layer formation configured so that: in a coated film formed on an aluminum plate, a chemical light emission amount in a specific condition is measured from a coated film which is exposed for a short term or promoted, and from a coated film which is continuously further exposed for a short term or promoted, and apparent activation energy acquired on the basis of the Arrhenius rule, on the basis of the chemical light emission amount of the coated film, is 35 kJ / mol or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating composition for forming a surface protective layer and a coated body, and in particular to a coating composition capable of forming a surface protective layer that can achieve excellent weather resistance. [Background technology]

[0002] As exterior building materials for houses and the like, building boards with a design layer on the surface, such as ceramic siding boards, metal siding boards, and ALC panels, are used. After construction, these building boards are required to withstand environmental factors such as sunlight, ultraviolet rays, rain, snow, and wind, and to maintain the surface design for a long time, so a surface protective layer is often formed to protect the design layer. In particular, in recent years, with the development of printing technology such as inkjet ink and the diversification of design-forming materials such as coral, shells, beads, and metallic pigments, the design layers have become more diverse and often have uneven surfaces, and the functions required of the surface protective layer are becoming increasingly high.

[0003] JP 2011-93306 A (Patent Document 1) describes an invention related to an architectural decorative board having a receiving layer, a printed layer, and a top clear layer on the surface of a substrate. Patent Document 1 describes that by adding a curing agent such as a silane coupling agent, an oxazoline group-containing compound, or a carbodiimide group-containing compound to a water-based clear paint for forming the top clear layer, ink bleeding and interlayer peeling in the printed layer are improved as much as possible, and an architectural decorative board can be provided in which the durability (water resistance, light resistance, and weather resistance) of the entire decorative coating film is significantly improved.

[0004] In addition, Patent Document 1 describes, as a background, that when a top clear layer is formed with a conventional water-based clear paint, the ink forming a pattern in the printed layer is redissolved (ink redissolved) in the aqueous solvent of the water-based clear paint applied thereon, causing ink bleeding in the printed layer, and in some cases peeling (interlayer peeling) occurs between the ink receiving layer and the top clear layer, and sufficient protection performance is not necessarily obtained in terms of water resistance and ink bleeding in the printed layer, so that in terms of product quality stability, it has been the reality that a solvent-based clear paint must be used for the clear paint forming the top clear layer. This problem of ink redissolution is recognized to be more prominent when the ink is water-based ink. Patent Document 1 examines the case where water-based ink is used, and therefore, in the invention described in Patent Document 1, the top clear layer is recognized to be a surface protective layer that can be applied without problems to the printed layer formed from water-based ink.

[0005] International Publication No. 2012 / 133667 (Patent Document 2) describes an invention relating to a method for producing a multi-layer coating film, which includes the steps of forming an undercoat coating layer on a substrate, then applying and curing an active energy ray curable ink by an inkjet method, and then applying a topcoat paint to form a topcoat coating layer. Patent Document 2 describes that since the ink is an active energy ray curable ink, there is no problem with ink redissolution, but since the adhesion between layers is low, the problem of adhesion is solved by adjusting the surface free energy of the undercoat coating film layer, the surface tension of the active energy ray curable ink, and the surface tension of the topcoat paint.

[0006] JP 2016-55249 A (Patent Document 3) describes an invention relating to a method for manufacturing a building board in which a cured coating film is formed from an active energy ray curable ink on a substrate that has been coated with an undercoat, and then a topcoat paint is applied. Here too, the problem of reduced interlayer adhesion caused by the use of active energy ray curable ink is cited as an issue, and the invention described in Patent Document 3 describes how the adhesion issue is resolved by controlling the reaction rate during the curing reaction of the cured coating film formed from the active energy ray curable ink and the surface temperature during the application of the topcoat paint.

[0007] JP 2019-217680 A (Patent Document 4) describes an invention related to a printed matter having an ink layer made of active energy ray curable ink and a surface protective layer on a substrate. In Patent Document 4, the problem of odor of the ink layer made of active energy ray curable ink is focused on that the cause is the emission of unreacted monomer remaining in the ink layer, and it is described that a surface protective layer is laminated on the ink layer to suppress the amount of emission of unreacted monomer.

[0008] Since it takes many years to evaluate the weather resistance of coating films, including such surface protective layers, methods for predicting the weather resistance of coating films are also being studied. Patent No. 6188625 (Patent Document 5) describes an invention of a coating film weather resistance prediction method for predicting the weather resistance of coating films made of organic paint, which is composed of a calibration curve creation process and a weather resistance prediction process. This patent describes that for organic coating film samples, the apparent activation energy of each sample can be calculated from the data on the amount of chemiluminescence after the start of deterioration, and that a calibration curve that can be generally used for weather resistance prediction processes for coating films made of organic paints in general can be obtained from the correlation between this apparent activation energy and the standard deterioration time until each organic coating film reaches its deterioration limit, and that by using this calibration curve, it is possible to quantitatively predict coating deterioration in a short time, which could not actually be achieved without a long test using conventional test methods. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2011-93306 A [Patent Document 2] International Publication No. 2012 / 133667 [Patent Document 3] JP 2016-55249 A [Patent Document 4] JP 2019-217680 A [Patent Document 5] Patent No. 6188625 [Non-patent literature]

[0010] [Non-Patent Document 1] "Chemiluminescence of Polymer Materials" Sumitomo Chemical 1993-II, P.86-P.98 Summary of the Invention [Problem to be solved by the invention]

[0011] According to the inventions described in Patent Documents 1 to 4, it is possible to form a design layer having excellent design, and by forming a surface protective layer capable of protecting the design layer, it is possible to provide a printed matter that can withstand outdoor use. On the other hand, since repainting a building requires a great deal of labor, such as assembling scaffolding, painting, curing, and dismantling the scaffolding, it is required to ensure weather resistance for a long period of time in order to delay the repainting time. In particular, the design layer formed by the active energy ray curable ink has a lower molecular weight and a thinner film thickness than conventional enamel paints, and is more susceptible to the effects of ultraviolet rays, so it is important how the surface protective layer blocks ultraviolet rays and protects the design layer from environmental factors such as wind and rain. In addition, when a photocatalyst layer is present on the outermost layer, the coating film is easily deteriorated by radicals generated by ultraviolet rays, so the surface protective layer is required to have a protective function that is resistant to deterioration by radicals. However, it cannot be said that there is a common index for obtaining a highly weather-resistant coating film, and it is often difficult to predict the weather resistance of the coating film from the paint formulation. For this reason, in order to confirm the weather resistance of a coating film, it is necessary to actually form a coating film and conduct weather resistance tests to judge the coating film performance. However, because weather resistance tests take an enormous amount of time, there was a need for a method that could predict the weather resistance of a coating film in a short period of time and judge the coating film performance.

[0012] Therefore, an object of the present invention is to provide a coating composition capable of forming a surface protective layer that can realize a high level of weather resistance and can protect the design for a long period of time even when the design layer is an active energy ray-curable ink or when a photocatalyst layer is present on the outermost layer. Another object of the present invention is to provide a coated body using such a coating composition. [Means for solving the problem]

[0013] The present inventors have conducted research into coating film deterioration prediction methods in order to achieve a high level of weather resistance. As a method for predicting coating film deterioration, they have focused on the "ease of oxidation of a coating film" and devised a method for evaluating the weather resistance of a coating film by evaluating this. This "ease of oxidation" was evaluated by measuring the amount of chemiluminescence, which can be evaluated by the coating film shape, as used in Patent Document 5. Patent Document 5 describes an invention in which the apparent activation energy of a specimen to be evaluated is calculated from the amount of chemiluminescence measured at an arbitrary temperature, and the weather resistance of the coating film is predicted. However, for specimens in which coating film changes such as volatilization or decomposition of components occur within the temperature range to be measured, it is difficult to calculate the activation energy, and it is difficult to predict the weather resistance.

[0014] As a result of further investigation, the amount of chemiluminescence was measured using coating films that had been exposed for a short period of time or accelerated exposure, and coating films that had been continuously exposed for a short period of time or accelerated exposure. It was found that there is a correlation between the apparent activation energy obtained from the amount of chemiluminescence of these coating films based on the Arrhenius law and the weather resistance of the coating film.

[0015] As a result of further investigations, the inventors measured the chemiluminescence amounts under specific conditions of coating films formed on aluminum plates that had been exposed or accelerated for a short period of time, and those that had been continuously exposed or accelerated for a short period of time.They confirmed that if the apparent activation energy obtained from the chemiluminescence amounts of these coating films, based on the Arrhenius law, was 35 kJ / mol or more, the coating film could be used as a surface protective layer with excellent weather resistance, thereby completing the present invention.

[0016] Accordingly, the coating composition of the present invention is a coating composition for forming a surface protective layer, which is obtained by forming a coating composition for forming a surface protective layer on an aluminum plate, and is prepared by subjecting a coating film (A) to an accelerated weather resistance test using a sunshine carbon arc lamp based on JIS K7350-4 for 60 hours and a coating film (B) to such a test for 180 hours. Heating of the coating film (A) and the coating film (B) in an oxygen atmosphere at 110°C, 130°C, and 150°C is started, and the amount of chemiluminescence of the coating film (A) and the coating film (B) at each heating temperature 1200 seconds after the start of heating are measured under the following conditions, and the difference in the amount of chemiluminescence between the coating film (B) and the coating film (A) at each heating temperature is determined, and a semi-logarithmic graph is created with the natural logarithmic value of the difference on the ordinate and the reciprocal of the absolute temperature of each heating temperature on the abscissa. The coating composition has an apparent activation energy of 35 kJ / mol or more, as determined from the slope of a regression equation created from points plotted on the semi-logarithmic graph based on the Arrhenius law. < Chemiluminescence measurement conditions > Test piece size: 3cm x 3cm Dry film thickness: 30μm Oxygen flow rate: 50ml / min Exposure time: 10 seconds Detection wavelength: 300~850nm

[0017] In addition, the first coated body of the present invention is a coated body having at least a substrate and a surface protective layer, characterized in that the surface protective layer includes a coating film formed by the above-mentioned paint composition of the present invention.

[0018] In addition, a second coated body of the present invention is a coated body having at least a substrate, a surface protective layer, and a photocatalyst layer formed on the surface protective layer, characterized in that the surface protective layer includes a coating film formed by the above-mentioned paint composition of the present invention. Effect of the Invention

[0019] According to the coating composition of the present invention, it is possible to provide a coating composition capable of forming a surface protective layer that can realize a high level of weather resistance and can protect the design for a long period of time even when the design layer is an active energy ray-curable ink or when a photocatalyst layer is present on the outermost surface. Furthermore, according to the coated body of the present invention, it is possible to provide a coated body using such a coating composition. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a flow chart showing an example of a method for calculating activation energy according to the present invention. [Diagram 2] 1 is a graph in which the ordinate indicates the amount of chemiluminescence (count per 10 seconds) of a coating film after an exposure time of 10 seconds, and the abscissa indicates the time (seconds) from the start of heating of the coating film that underwent an accelerated weather resistance test until measurement, and shows the measurement results of the amount of chemiluminescence of a coating film that underwent an accelerated weather resistance test for the topcoat paint (paint for forming a surface protective layer) of Example 11. [Diagram 3] 1 is a semi-logarithmic graph in which the ordinate represents the natural logarithm of the difference between the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 180 hours and the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 60 hours, and the abscissa represents the reciprocal of the absolute temperature of the heating temperature of the coating film subjected to the accelerated weathering test. The graph was created based on the measurement results of the amount of chemiluminescence for the topcoat paint (paint for forming a surface protective layer) of Example 11, and the regression equation created from the graph is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention relates to a coating composition, a method for forming a surface protective layer, and a coated body.

[0022] One embodiment of the present invention is a coating composition for forming a surface protective layer. Here, the surface protective layer is a layer for protecting a substrate or an undercoat layer or a design layer formed on the substrate. The surface protective layer often contains organic matter, and there is a method for detecting weak luminescence derived from peroxides generated by the oxidation of these organic matter as chemiluminescence. Chemiluminescence is used as an index for measuring the susceptibility of a coating film to oxidative deterioration.

[0023] The chemiluminescence of paint films is explained as follows. When a paint film is exposed to deterioration factors such as ultraviolet light or heat, the substances that make up the film decompose, generating radicals, which are then added to by oxygen, accelerating oxidation through the autoxidation mechanism. Oxidation causes the main chains of the polymers that make up the film to break, crosslink, and undergo structural changes, resulting in a decrease in physical properties and a change in appearance. Chemiluminescence is a phenomenon in which energy produced by a chemical reaction is released as light. Most chemiluminescence is related to oxidation reactions, in which excited carbonyls and singlet oxygen are generated by oxidation reactions in coating films, and light is emitted when these return to their ground state. (See Non-Patent Document 1) As the oxidation reaction of the coating progresses, luminescent species such as peroxides are generated and accumulate in the coating. The lower the weather resistance of the coating, the more likely it is that the oxidation reaction will progress and luminescent species will accumulate. In Patent Document 5, the oxidation of the coating is considered as a first-order chemical reaction, and the amount of chemiluminescence in the initial state and the state after short-term deterioration of the coating of various types of paint is measured, the activation energy is calculated based on the Arrhenius law, and a calibration curve is created based on these results to predict the weather resistance of the specimen to be evaluated. However, for coating films in which the coating state changes due to factors other than oxidation or hydrolysis after short-term deterioration from the initial stage of coating film formation, the above method may not correlate with the activation energy and weather resistance. The present inventors focused on the fact that the difference between the initial state of the coating film and the state after short-term deterioration may result in a lack of correlation between the activation energy and weather resistance, and investigated what factors change the coating state other than oxidation or hydrolysis deterioration. As a result, it was confirmed that the method described in Patent Document 5 makes it difficult to obtain a correlation between the activation energy and weather resistance for coating films containing high-boiling point solvents and coating films in which the curing reaction has not yet completed in the initial stage. This is thought to be because the exposure to light or heat during short-term deterioration causes the volatilization of high-boiling point solvents and the progress of the curing reaction, which changes the ease of oxygen penetration into the coating film.

[0024] When the value of the activation energy changes due to factors other than the deterioration of the coating film, it is difficult to identify the factors that change the coating film state for an unknown coating film, and the weather resistance of the coating film cannot be evaluated. Therefore, the present inventors further investigated a method for reliably evaluating the weather resistance of a coating film, accelerated the deterioration of the coating film in an extremely short period of time, prepared a coating film in which changes in the coating film other than deterioration due to oxidation or hydrolysis were suppressed, and determined the apparent activation energy based on the Arrhenius law from the difference in the amount of chemiluminescence between the coating film and a coating film further accelerated in deterioration, thereby confirming that the activation energy correlates with weather resistance, and thus completing the present invention.

[0025] That is, the coating composition of the present invention is a coating composition for forming a surface protective layer, in which a coating film obtained by forming a coating composition on an aluminum plate is subjected to an accelerated weather resistance test using a sunshine carbon arc lamp based on JIS K7350-4 for 60 hours (coating film (A)) and a coating film (B) are subjected to the test for 180 hours, and the coating films (A) and (B) are heated in an oxygen atmosphere at 110°C, 130°C, and 150°C for 1200 seconds, and the amounts of chemiluminescence of the coating films (A) and (B) at each heating temperature are measured under the following conditions, the difference in the amounts of chemiluminescence between the coating films (B) and (A) at each heating temperature is determined, and a semi-logarithmic graph is created with the natural logarithmic value of the difference on the ordinate and the reciprocal of the absolute temperature of each heating temperature on the abscissa, and the apparent activation energy calculated from the slope of a regression equation prepared from the semi-logarithmic graph based on the Arrhenius law is 35 kJ / mol or more. < Chemiluminescence measurement conditions > Test piece size: 3cm x 3cm Dry film thickness: 30μm Oxygen flow rate: 50ml / min Exposure time: 10 seconds Detection wavelength: 300~850nm

[0026] In this specification, the apparent activation energy thus determined is referred to as the "activation energy according to the present invention." In addition, the coating film subjected to the accelerated weathering test using a sunshine carbon arc lamp for 60 hours based on JISK7350-4 is referred to as "coating film (A)," and the coating film subjected to the accelerated weathering test using a sunshine carbon arc lamp for 180 hours based on JISK7350-4 is referred to as "coating film (B)."

[0027] The amount of chemiluminescence is the number of photons emitted per unit time during chemiluminescence (cps; counts per second), and can be measured by a weak luminescence detector. An example of a weak luminescence detector is a chemiluminescence analyzer manufactured by Tohoku Electronics Industries Co., Ltd. In addition, the detection wavelength of the amount of chemiluminescence can be set to a range including wavelengths of 420 to 530 nm, since the chemiluminescence of the coating film is presumed to be mainly derived from excited carbonyl, but since other excited substances such as singlet oxygen may also be present, it is preferable to measure the amount of chemiluminescence over a wide wavelength range, for example, 300 to 850 nm. The amount of chemiluminescence is an index of deterioration of the coating film, and the smaller the apparent activation energy value obtained, the more likely the coating film is to deteriorate, and the lower the weather resistance of the coating film. Furthermore, the measurement of the amount of chemiluminescence does not require pulverizing the coating film, and the weather resistance of the coating film can be evaluated while maintaining its shape.

[0028] The chemiluminescence measurement atmosphere can be oxygen or air, but it is preferable to perform the measurement in an oxygen atmosphere. The gas flow rate is 50 mL / min. A metal plate with a thickness of 2 mm or less can be used as the substrate when measuring the coating. Substrates with low thermal conductivity such as slate may affect the measurement results, and since the substrate condition is not constant, it is difficult to make a consistent evaluation of the chemiluminescence derived from the coating. The coating thickness is preferably 10 μm or more.

[0029] The exposure time for measuring the amount of chemiluminescence can be in the range of 1 to 10 seconds. However, since the amount of chemiluminescence is small at low temperatures, the exposure time for measuring the amount of chemiluminescence in the examples of this specification was set to 10 seconds.

[0030] The coating composition of the present invention has an activation energy according to the present invention of 35 kJ / mol or more, preferably 40 kJ / mol or more, and more preferably 45 kJ / mol or more. When the activation energy according to the present invention is 35 kJ / mol or more, the coating film has excellent weather resistance. The upper limit of the activation energy is not particularly limited, but is, for example, 120 kJ / mol or less.

[0031] FIG. 1 is a flow chart showing an example of a method for calculating activation energy according to the present invention. In the "coating film preparation" block in Figure 1, the surface temperature of the aluminum plate is adjusted to 50°C, and paint is applied to the aluminum plate to prepare a coating film with a dry thickness of 30 μm. In the block "Accelerated weathering test 60 hours later / Chemiluminescence measurement (110℃, 130℃, 150℃)", the coating film is subjected to accelerated weathering test using sunshine carbon arc lamp for 60 hours based on JISK7350-4:2008 (Plastics - Exposure test method using laboratory light source - Part 4: Open-flame carbon arc lamp), and the coating film that has been subjected to the accelerated weathering test is heated at temperatures of 110℃, 130℃, and 150℃, and the amount of chemiluminescence of the coating film at each temperature 1200 seconds after the start of heating is measured with an exposure time of 10 seconds. The amount of chemiluminescence obtained is the integrated value for the exposure time of 10 seconds. In this way, by preparing a coating film that has been subjected to an accelerated weathering test for a short period of time, it is possible to prepare a coating film that suppresses changes in the coating film other than deterioration of the coating film due to oxidation and hydrolysis. In the block "Accelerated weathering test after 180 hours / chemiluminescence measurement (110℃, 130℃, 150℃)", the coating is subjected to accelerated weathering test using sunshine carbon arc lamp for 180 hours based on JISK7350-4:2008 (Plastics - Exposure test method using laboratory light source - Part 4: Open-flame carbon arc lamp), and the coating that has been subjected to the accelerated weathering test is heated at temperatures of 110℃, 130℃, and 150℃, and the chemiluminescence amount of the coating at each temperature 1200 seconds after the start of heating is measured with an exposure time of 10 seconds. The amount of chemiluminescence obtained is the integrated value for an exposure time of 10 seconds. In the "calculation of apparent activation energy" block, a semi-logarithmic graph is created with the natural logarithmic value of the difference between the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 180 hours and the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 60 hours as the ordinate and the reciprocal of the absolute temperature of the heating temperature of the coating film subjected to the accelerated weathering test as the abscissa, and the apparent activation energy is calculated from the slope of the regression equation created from the semi-logarithmic graph based on the Arrhenius law. In the block "Comparison with the results of accelerated deterioration test", in order to investigate the relationship between the activation energy and weather resistance according to the present invention, a coating film was formed using a commercially available paint, and the activation energy was calculated and a long-term accelerated weather resistance test known so far was performed at the same time, and the results were compared. As a result, it was confirmed that the higher the activation energy value according to the present invention, the smaller the change in gloss value, the smaller the change in color difference, or the less likely the coating film to crack or other damage occurs, especially for the coating film after 7500 hours of accelerated weather resistance test using a sunshine carbon arc lamp, and further for the coating film after 1000 hours of test using an Iwasaki Electric Eye Super UV Tester. Next, a coating composition with a higher activation energy value was examined, and it was confirmed that when the activation energy according to the present invention is 35 kJ / mol or more, both the coating film after 7500 hours of accelerated weather resistance test using a sunshine carbon arc lamp, and the coating film after 1000 hours of test using an Iwasaki Electric Eye Super UV Tester have a high gloss retention rate and are capable of forming a surface protective layer with little apparent change in the coating film.

[0032] The correlation between the activation energy and the weather resistance of the coating film according to the present invention applies to all coating films containing organic components. The main organic components constituting the coating film are organic binder components, and examples thereof include acrylic resins, urethane resins, fluororesins, acrylic silicone resins, alkyd resins, epoxy resins, and polyester resins, but are not limited thereto. The organic binder components may be used alone or in combination of two or more. The coating film includes various coating films formed from transparent paints, enamel paints, glitter paints, and the like. As the coating film, any coating film can be used, such as water-based paints, organic solvent-based paints, active energy ray curing paints, powder-based paints, and solventless paints.

[0033] Possible methods for making the activation energy of the present invention 35 kJ / mol or more include selecting a resin that is resistant to photodegradation, optimizing the film formation conditions, appropriately blending an ultraviolet absorber or a radical scavenger, adjusting the type and amount of pigments, additives, and media, and combinations of these.

[0034] The coating composition of the present invention preferably contains an ultraviolet absorber and / or a radical scavenger, and it is more preferable that a portion of the ultraviolet absorber and the radical scavenger are copolymerized in the resin.

[0035] Here, "a part of the ultraviolet absorber and the radical scavenger" means a part of the entire ultraviolet absorber and the radical scavenger used in the coating composition of the present invention. Since "a part of the ultraviolet absorber and the radical scavenger" is a part of the entire ultraviolet absorber and the radical scavenger, it may be the case of only the ultraviolet absorber, the case of only the radical scavenger, or the case of both the ultraviolet absorber and the radical scavenger. Also, since "a part of the ultraviolet absorber and the radical scavenger" is a part of the entire ultraviolet absorber and the radical scavenger, it may be the case of the entire ultraviolet absorber used in the coating composition of the present invention, or the case of the entire radical scavenger used in the coating composition of the present invention.

[0036] In particular, when the coating composition of the present invention is an aqueous coating composition, it is preferable to include a water-dispersible resin, and since the resin particles of the water-dispersible resin are fused together during film formation to form a film, it is more preferable to include a resin in which a part of the ultraviolet absorber and / or radical scavenger is copolymerized with the water-dispersible resin. "Copolymerized with the water-dispersible resin" means that "a part of the ultraviolet absorber and radical scavenger" is copolymerized with other monomers as a constituent unit of the water-dispersible resin. In other words, the water-dispersible resin means that "a part of the ultraviolet absorber and radical scavenger" is included as a constituent element (repeating unit, etc.).

[0037] In the coating composition of the present invention, when a portion of the ultraviolet absorber and the radical scavenger are copolymerized with the resin, the remaining portions of the ultraviolet absorber and the radical scavenger are not copolymerized with the resin.

[0038] Here, "the remaining portion of the ultraviolet absorber and radical scavenger" means the portion of the ultraviolet absorber and radical scavenger used in the coating composition of the present invention excluding "a part of the ultraviolet absorber and radical scavenger" copolymerized in the resin. "The remaining portion of the ultraviolet absorber and radical scavenger" may be the ultraviolet absorber alone, the radical scavenger alone, or both the ultraviolet absorber and the radical scavenger. Also, "the remaining portion of the ultraviolet absorber and radical scavenger" may be the entire ultraviolet absorber used in the coating composition of the present invention, or the entire radical scavenger used in the coating composition of the present invention.

[0039] Moreover, "not copolymerized in the resin" means that it is not present as a structural unit of the resin. Therefore, in the coating composition of the present invention, "the remaining portions of the ultraviolet absorber and the radical scavenger" are present in the coating composition in a dispersed or dissolved state.

[0040] In the coating composition of the present invention, it is preferred that a part of the ultraviolet absorber and the radical scavenger are copolymerized with the resin, and the remaining parts of the ultraviolet absorber and the radical scavenger are not copolymerized with the resin, thereby improving weather resistance without reducing water resistance and preventing deterioration of the surface protective layer.

[0041] Furthermore, a preferred embodiment of the coating composition of the present invention contains a resin and (A) an ultraviolet absorber and / or a radical scavenger dispersed or dissolved in the coating composition, where the resin contains (B) a resin containing an ultraviolet absorber and / or a radical scavenger as a constituent element, and one of component (A) and component (B) is at least an ultraviolet absorber, and the other of component (A) and component (B) is at least a radical scavenger.

[0042] In the coating composition of the present invention, the amount of ultraviolet absorber and radical scavenger in the coating film-forming components is preferably 2.0 to 15.0 mass%, more preferably 4.0 to 13.0 mass%, and even more preferably 6.0 to 11.0 mass%. Here, the "amount of ultraviolet absorber and radical scavenger" refers to the total amount of ultraviolet absorber and radical scavenger used in the coating composition of the present invention, and is the sum of "a part of the ultraviolet absorber and radical scavenger" that is copolymerized in the resin and "the remaining part of the ultraviolet absorber and radical scavenger" that is not copolymerized in the resin.

[0043] In this specification, the film-forming components refer to the components excluding volatile components such as water, organic solvents, and film-forming aids, and are the components that will ultimately form a coating film. In this specification, the components remaining when the coating composition is dried at 130°C for 60 minutes are treated as the film-forming components. The amount of the film-forming components in the coating composition of the present invention is, for example, 20 to 80 mass%, preferably 30 to 70 mass%, and particularly preferably 35 to 60 mass%.

[0044] In the coating composition of the present invention, when the resin contains a water-dispersible resin, the mass ratio (A:B) of the amount (A) of "a part of the ultraviolet absorber and radical scavenger" copolymerized in the water-dispersible resin to the amount (B) of "the remaining part of the ultraviolet absorber and radical scavenger" not copolymerized in the water-dispersible resin is preferably 5:95 to 95:5, and more preferably 15:85 to 85:15.

[0045] The ultraviolet absorber has the effect of absorbing ultraviolet rays and preventing deterioration caused by ultraviolet rays. Examples of the ultraviolet absorber include benzophenone-based ultraviolet absorbers, benzoate-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers (particularly hydroxyphenyltriazine-based ultraviolet absorbers), and benzylidene camphor-based ultraviolet absorbers. The ultraviolet absorber may be used alone or in combination of two or more types, but it is preferable that the ultraviolet absorber contains two or more ultraviolet absorbers with different absorption peaks. The ultraviolet absorber preferably contains a triazine-based ultraviolet absorber, and particularly preferably contains a triazine-based ultraviolet absorber and a benzotriazole-based ultraviolet absorber.

[0046] Examples of the ultraviolet absorber include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone-2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4, 4'-Dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α-(dimethylbenzyl)phenyl]benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzo Triazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], methyl-3-[3-t-butyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]phenol, 2-(2-hydroxyphenyl)propionate and polyethylene glycol condensation products, 2-(2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,6-di-t-butylphenyl-3',5'-di-t-butyl-4'-hydroxybenzoate, hexadecyl-3,5-di-t-butyl-4-hydroxybenzoate, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, hydroxyphenyl triazine, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, and the like.

[0047] Among the ultraviolet absorbents, examples of polymerizable ultraviolet absorbents include ultraviolet absorbing monomers such as benzotriazole-based ultraviolet absorbing monomers and benzophenone-based ultraviolet absorbing monomers.

[0048] Examples of the benzotriazole-based ultraviolet absorbing monomer include 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole, and 2-[2'-hydroxy-5'-(meth)acryloylaminomethyl-5'-tert-octylphenyl]-2H-benzotriazole. 2-[2'-hydroxy-5'-(meth)acryloyloxypropylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyhexylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy- 5'-tert-butyl-3'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-cyano-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-tert-butyl-2H-benzotriazole, 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethylphenyl] 2-[2'-hydroxy-5'-(meth)acryloyloxyethoxy]-3'-tert-butylphenyl]-4-tert-butyl-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-methoxy-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-nitro-2H-benzotriazole, 3-(meth)acryloyl-2-hydroxypropyl-3-[3-(2-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenylpropionate, and the like.

[0049] Examples of benzophenone-based ultraviolet absorbing monomers include 2-hydroxy-4-(meth)acryloyloxybenzophenone, 2-hydroxy-4-[2-hydroxy-3-(meth)acryloyloxy]propoxybenzophenone, 2-hydroxy-4-[2-(meth)acryloyloxy]ethoxybenzophenone, 2-hydroxy-4-[3-(meth)acryloyloxy-2-hydroxypropoxy]benzophenone, 2-hydroxy-3-tert-butyl-4-[2-(meth)acryloyloxy]butoxybenzophenone, and 2,2'-dihydroxy-4-[3-(meth)acryloyloxy-2-hydroxypropoxy]benzophenone.

[0050] As used herein, the term (meth)acryloyl means methacryloyl or acryloyl. For example, 2-hydroxy-4-(meth)acryloyloxybenzophenone is 2-hydroxy-4-methacryloyloxybenzophenone or 2-hydroxy-4-acryloyloxybenzophenone.

[0051] In the coating composition of the present invention, the amount of the ultraviolet absorber in the coating film-forming components is preferably 1.5 to 9.0 mass%, more preferably 2.5 to 7.5 mass%, and even more preferably 3.0 to 6.0 mass%. Here, when the ultraviolet absorber is composed of an ultraviolet absorber copolymerized in the resin and an ultraviolet absorber not copolymerized in the resin, the "amount of ultraviolet absorber" means the total amount thereof.

[0052] The radical scavenger can capture free radicals and improve light stability. In the present invention, the radical scavenger also includes a substance (so-called polymerization inhibitor) that reacts with free radicals and has a function of preventing polymerization reaction from occurring. The radical scavenger may be used alone or in combination of two or more kinds.

[0053] Examples of the radical scavenger include hindered amine compounds, hydroquinone compounds, phenol compounds, phenothiazine compounds, nitroso compounds, and N-oxyl compounds, and hindered amine light stabilizers (HALS) are particularly preferred.

[0054] Examples of the radical scavenger include hindered amine compounds such as bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, 1-{2-(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy)ethyl}-2,2,6,6-tetramethylpiperidine, and 8-acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro{4.5}decane-2,4-dione; phenols; and o-, m-, or p-cresols. phenolic compounds such as 2-t-butyl-4-methylphenol, 6-t-butyl-2,4-dimethylphenol, 2,6-di-t-butyl-4-methylphenol, 2-t-butylphenol, 4-t-butylphenol, 2,4-di-t-butylphenol, 2-methyl-4-t-butylphenol, 4-t-butyl-2,6-dimethylphenol, hydroquinone, hydroquinone monomethyl ether, methylhydroquinone, 2,5-di-t-butyl Hydroquinone compounds such as 4-methylbenzcatechin, t-butylhydroquinone, 3-methylbenzcatechin, 2-methyl-p-hydroquinone, 2,3-dimethylhydroquinone, trimethylhydroquinone, t-butylhydroquinone, benzoquinone, t-butyl-p-benzoquinone, and 2,5-diphenyl-p-benzoquinone; phenothiazine compounds; nitroso-based compounds such as N-nitroso-N-phenylhydroxylamine ammonium and N-nitroso-N-phenylhydroxylamine aluminum salt; and N-oxyl-based compounds such as 4-hydroxy-2,2,6,6-tetramethyl-piperidine-N-oxyl, 4-oxo-2,2,6,6-tetramethyl-piperidine-N-oxyl, and 4-methoxy-2,2,6,6-tetramethyl-piperidine-N-oxyl.

[0055] Among the radical scavengers, examples of the polymerizable radical scavengers include polymerizable photostable monomers. The polymerizable photostable monomers are compounds having a polymerizable group and a functional group having a photostabilizing effect. Examples of the polymerizable group include polymerizable unsaturated groups such as alkenyl groups (vinyl groups, allyl groups, etc.) and alkenylcarbonyl groups (e.g., (meth)acryloyl groups, crotonoyl groups, etc.).

[0056] Examples of the polymerizable light-stable monomer include, in addition to the hindered amine-based polymerizable light-stable monomers described below, a reaction product of decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester, 1,1-dimethylethyl hydroperoxide, and octane, bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, and a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate.

[0057] Examples of the hindered amine polymerizable light-stable monomer include polymerizable compounds having a piperazine skeleton (particularly, a 2,2,6,6-tetramethylpiperidine skeleton) (compounds having a piperazine skeleton and a polymerizable group).

[0058] Representative examples of the hindered amine-based polymerizable light-stable monomer include compounds represented by the following structural formula (1). [ka] In structural formula (1), R 1 and R 2 is a hydrogen atom or an alkyl group, and R 3 , R 4 , R 5 and R 6is an alkyl group, X is an oxygen atom (-O-) or an imino group (-NH-), and Y and Z are hydrogen atoms or substituents.

[0059] R in structural formula (1) 1 ~R 6 In the above, examples of the alkyl group include C methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, s-butyl group, and t-butyl group. 1-20 Alkyl groups, preferably C 1-10 Alkyl groups, more preferably C 1-4 An alkyl group is preferable, and a methyl group is particularly preferable. Representative R 1 and R 2 is a hydrogen atom or a methyl group, and in particular R 1 is a hydrogen atom, R 2 is preferably a hydrogen atom or a methyl group. 3 ~R 6 is a methyl group.

[0060] The substituents in Y and Z in the structural formula (1) include hydrocarbon groups [e.g., alkyl groups {e.g., the above-mentioned alkyl groups such as methyl groups (e.g., C 1-20 Alkyl groups, preferably C 1-4 alkyl group)}], alkoxy group (e.g., methoxy group, ethoxy group, etc. 1-20 Alkoxy groups, preferably C 1-10 Alkoxy groups, more preferably C 1-4 alkoxy groups, particularly preferably methoxy groups), acyl groups (e.g., C 1-10 acyl group), halogen atoms (for example, fluorine atom, chlorine atom, bromine atom, iodine atom), cyano group, hydroxyl group, polymerizable groups (for example, (meth)acryloyl group, crotonoyl group), etc.

[0061] In the structural formula (1), representative Y is a hydrogen atom, an alkyl group (e.g., a C group such as a methyl group), 1-4 alkyl group), alkoxy group (e.g., methoxy group, etc. 1-4 Alkoxy groups), acyl groups (e.g., acetyl groups, etc.1-4 Examples of Z include an acyl group, a (meth)acryloyl group, a crotonoyl group, etc., and in particular, a hydrogen atom or a methyl group is preferable. Representative examples of Z include a hydrogen atom or a cyano group, and in particular, a hydrogen atom is preferable.

[0062] Examples of the hindered amine-based polymerizable light-stable monomer include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine having a substituent {e.g., 4-(meth)acryloyloxy-2,2,6,6-tetramethyl-1-alkylpiperidine [e.g., 4-(meth)acryloyloxy-1-C such as 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 1-4 alkyl-2,2,6,6-tetramethylpiperidine], 4-(meth)acryloyloxy-2,2,6,6-tetramethyl-1-alkoxypiperidine [e.g., 4-(meth)acryloyloxy-1-C alkyl-2,2,6,6-tetramethylpiperidine, etc. 1-4 N-substituted (meth)acryloyloxy-2,2,6,6-tetramethylpiperidines such as alkoxy-2,2,6,6-tetramethylpiperidine, 4-substituted-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidines such as 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, etc., 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidines such as 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, etc. 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidines having a substituent {e.g., 4-(meth)acryloylamino-2,2,6,6-tetramethyl-1-alkylpiperidines [e.g., 4-(meth)acryloylamino-2,2,6,6-tetramethyl-1-alkylpiperidines such as 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, etc. 1-4N-substituted (meth)acryloylamino-2,2,6,6-tetramethylpiperidines such as alkylpiperidines, 4-substituted-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidines such as 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, etc.} 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidines; 4-crotonoylamino-2,2,6,6-tetramethylpiperidine; 1-( Examples of the 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine include 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine and 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine; and 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine and other 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine.

[0063] In the coating composition of the present invention, the amount of radical scavenger in the coating film-forming components is preferably 0.5 to 6.0 mass%, more preferably 1.5 to 5.5 mass%, and even more preferably 2.5 to 5.0 mass%. Here, when the radical scavenger is composed of a radical scavenger copolymerized with the resin and a radical scavenger not copolymerized with the resin, the "amount of radical scavenger" means the total amount thereof.

[0064] The coating composition of the present invention preferably contains a water-dispersible resin. In this specification, the term "water-dispersible resin" refers to a resin capable of distributing in water to form a heterogeneous system (e.g., an emulsion or suspension). The water-dispersible resin preferably contains an emulsion resin. The emulsion resin is a water-dispersible resin that can have a large molecular weight and also has excellent dispersion stability. In the coating composition of the present invention, the amount of the water-dispersible resin in the coating film-forming components is preferably 30 to 95% by mass, more preferably 35 to 90% by mass, and even more preferably 40 to 80% by mass. The water-dispersible resin may be used alone or in combination of two or more types.

[0065] The water-dispersible resin preferably contains a water-dispersible resin containing an acrylic component as a constituent element (repeating unit, etc.). In this specification, the term "acrylic component" refers to acrylic acid, methacrylic acid and derivatives thereof (for example, compounds having a (meth)acryloyl group such as esters and amides of acrylic acid and methacrylic acid, acrylic acid nitrile, methacrylic acid nitrile, etc.). The above-mentioned polymerizable ultraviolet absorbers and polymerizable radical scavengers having a (meth)acryloyl group are also included in the "acrylic component". The acrylic components may be used alone or in combination of two or more.

[0066] The water-dispersible resin containing an acrylic component as a constituent element includes, in addition to acrylic resin, various modified resins such as acrylic styrene resin, acrylic silicone resin, fluorine-modified acrylic resin, fatty acid-modified acrylic resin, urethane-modified acrylic resin, and epoxy-modified acrylic resin.

[0067] The amount of the acrylic component in the water-dispersible resin is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more.

[0068] In this specification, the expression "the amount of component X in the water-dispersible resin" refers to the amount of component X relative to the total mass of the water-dispersible resin contained in the coating composition. For example, when the water-dispersible resin in the coating composition is composed of a water-dispersible resin (A) containing an acrylic component as a constituent element and a water-dispersible resin (B) not containing an acrylic component, the "amount of the acrylic component in the water-dispersible resin" refers to the amount of the acrylic component relative to the total mass of the water-dispersible resin (A) and the water-dispersible resin (B).

[0069] The water-dispersible resin may contain a non-acrylic component as a constituent element (repeating unit, etc.). The non-acrylic component is a component other than the acrylic component, and examples thereof include, in addition to styrene, carboxyl group-containing monomers such as fumaric acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, crotonic acid, and vinyl versatic acid; aromatic monomers such as methylstyrene, chlorostyrene, methoxystyrene, and vinyltoluene; olefin monomers such as ethylene and propylene; vinyl monomers such as vinyl acetate and vinyl chloride; amide monomers such as maleic acid amide; alkoxysilyl group-containing monomers such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane; dialkyl fumarate, allyl alcohol, vinylpyridine, and butadiene.

[0070] The water-dispersible resin preferably contains at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent (repeating unit, etc.). The water-dispersible resin containing an ultraviolet absorber and / or a radical scavenger as a constituent may be a water-dispersible resin containing an acrylic component as a constituent. Here, the ultraviolet absorber and the radical scavenger may be either an acrylic component or a non-acrylic component, but are preferably acrylic components.

[0071] In one embodiment of the coating composition of the present invention, the water-dispersible resin may include a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent derived from an acrylic component and / or a non-acrylic component.

[0072] The amount of the ultraviolet absorber and / or radical scavenger in the water-dispersible resin is preferably 0.5 to 15.0% by mass, more preferably 1.0 to 13.0% by mass, and further preferably 1.5 to 11.0% by mass. Here, the "amount of ultraviolet absorber and / or radical scavenger" means the amount of the ultraviolet absorber or the radical scavenger when the water-dispersible resin contains only one of the ultraviolet absorber and the radical scavenger, and means the total amount of the ultraviolet absorber and the radical scavenger when the water-dispersible resin contains both the ultraviolet absorber and the radical scavenger. If the amount of ultraviolet absorber and / or radical scavenger is less than 0.5% by mass, the coating film is likely to deteriorate when exposed to rain, sunlight, etc. outdoors for a long period of time. If the amount of ultraviolet absorber and / or radical scavenger is more than 15.0% by mass, the coating film is likely to suffer from defects such as yellowing.

[0073] The water-dispersible resin preferably includes a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent element (repeating unit, etc.). The water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent element may be a water-dispersible resin containing an acrylic component as a constituent element, or may be a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent element.

[0074] By using a monomer having an SP value of 9.4 or less, the water resistance of the resin can be improved and bleeding of the ultraviolet absorber and the radical scavenger can be suppressed. The SP value of the monomer is preferably 8.50 to 9.40. The monomer having an SP value of 9.4 or less may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. Examples of the monomer having an SP value of 9.4 or less include n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isobornyl (meth)acrylate. The monomer having an SP value of 9.4 or less may be used alone or in combination of two or more.

[0075] In this specification, the term (meth)acrylate means methacrylate or acrylate. For example, 2-ethylhexyl (meth)acrylate is 2-ethylhexyl acrylate or 2-ethylhexyl methacrylate. In addition, a prefix indicating a plurality of (meth)acrylates may be added to (meth)acrylates, such as di(meth)acrylate, tri(meth)acrylate, etc., in which case each (meth)acrylate may be the same or different.

[0076] In one embodiment of the coating composition of the present invention, the water-dispersible resin may include a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less as a constituent derived from an acrylic component and / or a non-acrylic component.

[0077] The amount of monomers having an SP value of 9.4 or less in the water-dispersible resin is preferably 1.0 to 60.0 mass %, more preferably 3.0 to 45.0 mass %, and even more preferably 5.0 to 30.0 mass %.

[0078] The SP value (solubility parameter) is a guideline for determining compatibility, and there are various calculation and measurement methods. In this specification, the SP value of a monomer means the solubility parameter calculated by the Hoy method based on the structure.

[0079] The water-dispersible resin preferably includes a water-dispersible resin containing a cyclic aliphatic monomer as a constituent (repeating unit, etc.). The water-dispersible resin containing a cyclic aliphatic monomer as a constituent may be a water-dispersible resin containing an acrylic component as a constituent, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent, or a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent.

[0080] The cyclic aliphatic monomer is an alicyclic monomer (a saturated or unsaturated carbon ring having no aromaticity, such as a cycloalkyl group, preferably C 4-20 Cycloalkyl groups, more preferably C 4-10 A cyclic aliphatic monomer is a monomer having a cycloalkyl group, and the use of a cyclic aliphatic monomer can improve the water resistance of the resin. The cyclic aliphatic monomer may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. Examples of cyclic aliphatic monomers include alicyclic (meth)acrylates [e.g., cycloalkyl (meth)acrylates (e.g., cyclohexyl (meth)acrylate, etc. C 4-20 Cycloalkyl(meth)acrylates, preferably C 4-10 Cycloalkyl (meth)acrylates), alkylcycloalkyl (meth)acrylates (e.g., 4-methylcyclohexyl (meth)acrylate, etc. 1-4 Alkyl C 4-10 Cycloalkyl (meth)acrylate), cycloalkyl alkyl (meth)acrylate (e.g., cyclohexyl methyl (meth)acrylate, cyclohexyl ethyl (meth)acrylate, cyclohexyl propyl (meth)acrylate, 4-methylcyclohexyl methyl (meth)acrylate, etc. 4-10Cycloalkyl C 1-4 alkyl(meth)acrylate), crosslinked cyclic (meth)acrylate (e.g., isobornyl(meth)acrylate, adamantyl(meth)acrylate, etc.) etc. The cyclic aliphatic monomer may be used alone or in combination of two or more kinds.

[0081] In one embodiment of the coating composition of the present invention, the water-dispersible resin may comprise at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer as a constituent derived from an acrylic component and / or a non-acrylic component.

[0082] The amount of the cyclic aliphatic monomer in the water-dispersible resin is preferably from 1.0 to 90.0% by mass, more preferably from 10.0 to 80.0% by mass, and further preferably from 30.0 to 70.0% by mass.

[0083] The water-dispersible resin preferably contains a water-dispersible resin containing as a constituent (repeating unit, etc.) a monomer that gives a homopolymer with a glass transition temperature (Tg) of less than 50° C. The water-dispersible resin containing as a constituent a monomer that gives a homopolymer with a Tg of less than 50° C. may be a water-dispersible resin containing as a constituent an acrylic component, a water-dispersible resin containing as a constituent at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, a water-dispersible resin containing as a constituent a monomer having an SP value of 9.4 or less, or a water-dispersible resin containing as a constituent a cyclic aliphatic monomer.

[0084] By using a monomer that gives a homopolymer Tg of less than 50°C, the flexibility of the resin can be improved. The homopolymer Tg here is preferably -90°C or more and less than 15°C. The monomer that gives a homopolymer Tg of less than 50°C may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. Examples of monomers that give a homopolymer Tg of less than 50°C include methyl acrylate, ethyl acrylate, n-butyl acrylate, isopropyl acrylate, n-butyl methacrylate, n-hexyl methacrylate, lauryl methacrylate, hydroxypropyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, and glycidyl methacrylate. The monomer that gives a homopolymer Tg of less than 50°C may be used alone or in combination of two or more.

[0085] In one embodiment of the coating composition of the present invention, the water-dispersible resin may comprise at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer having a homopolymer Tg of less than 50°C, as constituents derived from an acrylic component and / or a non-acrylic component.

[0086] The amount of monomers in the water-dispersible resin that give a homopolymer Tg of less than 50° C. is preferably 10.0 to 70.0 mass %, more preferably 10.0 to 50.0 mass %, and even more preferably 10.0 to 30.0 mass %.

[0087] The water-dispersible resin preferably contains a water-dispersible resin containing as a constituent element (repeating unit, etc.) a monomer that gives a homopolymer glass transition temperature (Tg) of 50° C. or higher. The water-dispersible resin containing as a constituent element (repeating unit, etc.) a monomer that gives a homopolymer Tg of 50° C. or higher may be a water-dispersible resin containing an acrylic component as a constituent element, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent element, a water-dispersible resin containing as a constituent element a monomer having an SP value of 9.4 or less, a water-dispersible resin containing as a constituent element a cyclic aliphatic monomer, or a water-dispersible resin containing as a constituent element a monomer that gives a homopolymer Tg of less than 50° C.

[0088] By using a monomer that gives a homopolymer Tg of 50° C. or more, the rigidity of the resin can be improved. The homopolymer Tg here is preferably 50 to 130° C. The monomer that gives a homopolymer Tg of 50° C. or more may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. Examples of the monomer that gives a homopolymer Tg of 50° C. or more include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, acrylic acid, methacrylic acid, 2-hydroxyethyl methacrylate, acrylamide, N-methylol acrylamide, diacetone acrylamide, styrene, acrylonitrile, and cyclohexyl methacrylate. The monomer that gives a homopolymer Tg of 50° C. or more may be used alone or in combination.

[0089] In one embodiment of the coating composition of the present invention, the water-dispersible resin may comprise a water-dispersible resin containing, as constituents derived from an acrylic component and / or a non-acrylic component, at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer whose homopolymer Tg is less than 50°C, and / or a monomer whose homopolymer Tg is 50°C or higher.

[0090] The amount of monomers in the water-dispersible resin that give a homopolymer Tg of 50° C. or higher is preferably 40.0 to 95.0 mass %, more preferably 50.0 to 90.0 mass %, and even more preferably 60.0 to 90.0 mass %.

[0091] The water-dispersible resin preferably contains a water-dispersible resin containing as a constituent element a monomer that gives a homopolymer Tg of less than 50° C. and a water-dispersible resin containing as a constituent element a monomer that gives a homopolymer Tg of 50° C. or more, or contains a water-dispersible resin containing as constituent elements a monomer that gives a homopolymer Tg of less than 50° C. and a monomer that gives a homopolymer Tg of 50° C. or more. This makes it possible to obtain a resin that has a good balance between flexibility and rigidity, and improves the durability of the coating film.

[0092] The glass transition temperature of a homopolymer is common technical knowledge. When a monomer with an unknown glass transition temperature is used, the glass transition temperature of the monomer can be determined by differential scanning calorimetry (DSC), differential thermal analysis (DTA), thermomechanical analysis (TMA), etc.

[0093] The water-dispersible resin preferably contains a water-dispersible resin containing a crosslinking component as a constituent (repeating unit, etc.). The water-dispersible resin containing a crosslinking component as a constituent may be a water-dispersible resin containing an acrylic component as a constituent, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent, a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent, a water-dispersible resin containing a cyclic aliphatic monomer as a constituent, a water-dispersible resin containing a monomer having a homopolymer Tg of less than 50°C as a constituent, or a water-dispersible resin containing a monomer having a homopolymer Tg of 50°C or more as a constituent.

[0094] By using the crosslinking component, a crosslinked structure can be formed in the resin. This can prevent the ultraviolet absorber and the radical scavenger from flowing out of the coating film. The crosslinking may be, for example, crosslinking by polymerization, or crosslinking by chemical reaction (for example, reaction with isocyanate, reaction with epoxy, hydrolysis silylation reaction, reaction with hydrazine, reaction with aziridine, etc.). The form of crosslinking is not particularly limited and can be appropriately selected depending on the type of crosslinking component, etc., and may be either intramolecular crosslinking or intermolecular crosslinking, or may be crosslinked in both of these forms.

[0095] The crosslinking component may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. The crosslinking component may be used alone or in combination of two or more kinds.

[0096] Examples of the crosslinking component by polymerization include compounds having two or more polymerizable groups. Examples of the polymerizable group include polymerizable unsaturated groups such as alkenyl groups (vinyl groups, allyl groups, etc.) and alkenylcarbonyl groups (e.g., (meth)acryloyl groups, crotonoyl groups, etc.).

[0097] Examples of the compound having two or more polymerizable groups include diol di(meth)acrylates {e.g., alkanediol di(meth)acrylates [e.g., ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, etc. 2-10alkanediol di(meth)acrylate], polyalkylene glycol di(meth)acrylate [e.g., diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate], alkylene oxide modified alkylene glycol di(meth)acrylate [e.g., ethylene oxide modified 1,6-hexanediol di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate], di(meth)acrylate of aromatic diol or its alkylene oxide adduct [e.g., bisphenol A di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate]}, poly(meth)acrylate of polyol having three or more hydroxy groups {e.g., pentaerythritol di- or tetra(meth)acrylate [e.g., pentaerythritol monohydroxytri(meth)acrylate, acrylate, pentaerythritol tetra(meth)acrylate], dipentaerythritol di- to hexa(meth)acrylate [e.g., dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol (monohydroxy)penta(meth)acrylate], trimethylolpropane di- to tri(meth)acrylate [e.g., trimethylolpropane tri(meth)acrylate, trimethylolpropane triethoxytri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate], ditrimethylolpropane di- to tetra(meth)acrylate [e.g., ditrimethylolpropane tetra(meth)acrylate], glycerin di- to tri(meth)acrylate [e.g., ethoxylated glycerin tri(meth)acrylate, propylene oxide-modified glycerol tri(meth)acrylate], etc. 3-10 poly(meth)acrylates of polyols}; unsaturated hydrocarbons [e.g., alkadienes (e.g., butadiene, isoprene, chloroprene, and other C 4-10alkadienes); aromatic hydrocarbons (for example, divinylbenzene); diallyl dicarboxylates (for example, diallyl phthalate), triallyl isocyanurate, and other compounds having multiple allyl groups.

[0098] The chemically crosslinkable component is a compound having a polymerizable group and a group having crosslinkability by chemical reaction, such as an epoxy group-containing monomer, a carbonyl group-containing monomer, an aziridinyl group-containing monomer, an isocyanato group-containing monomer, a silane group-containing monomer, etc. Examples of the polymerizable group include polymerizable unsaturated groups such as an alkenyl group (vinyl group, allyl group, etc.) and an alkenylcarbonyl group (e.g., (meth)acryloyl group, crotonoyl group, etc.).

[0099] Examples of the epoxy group-containing monomer include epoxy group-containing (meth)acrylates [e.g., glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, glycidyloxyalkyl (meth)acrylates (e.g., glycidyloxy C such as 2-glycidyloxyethyl (meth)acrylate, etc.] 2-4 alkyl (meth)acrylate)], allyl glycidyl ether, and the like.

[0100] Examples of the carbonyl group-containing monomer include aldehydes having a polymerizable double bond (e.g., acrolein, formylstyrol, (meth)acryloxyalkylpropenal), ketones having a polymerizable double bond (e.g., vinyl ethyl ketone), and carbonyl group-containing (meth)acrylates (e.g., acetonyl (meth)acrylate, diacetone (meth)acrylate, 2-hydroxypropyl (meth)acrylate acetylacetate, butanediol-1,4-acrylate acetylacetate, 2-(acetoacetoxy)ethyl (meth)acrylate).

[0101] Examples of the aziridinyl group-containing monomer include (meth)acryloylaziridine and aziridinyl group-containing (meth)acrylates (for example, 2-aziridinylethyl (meth)acrylate).

[0102] Examples of the isocyanato group-containing monomer include isocyanato group-containing (meth)acrylates, etc. Examples of the isocyanato group-containing (meth)acrylates include 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, 5-methacryloyloxy-3-oxypentyl isocyanate, etc.

[0103] Examples of the silane group-containing monomer include a monomer having a silyl group to which a hydrolyzable (condensable) group (e.g., an alkoxy group or a halogen atom) is bonded, and examples thereof include compounds represented by the following structural formula (2). (R1) n -Si-(R2) 4-n (2) In the structural formula (2), R1 represents a group having a polymerizable unsaturated bond group. R2 represents a hydrogen atom, a hydrolytically condensable group, a hydrocarbon group, or an epoxy group (an epoxy group-containing group), and at least one R2 represents a hydrolytically condensable group. n represents an integer of 1 to 3.

[0104] In the structural formula (2), examples of the polymerizable unsaturated bond group in R1 include a vinyl group, an allyl group, and a (meth)acryloyl group. Examples of the hydrocarbon group in R2 include an alkyl group and an aryl group (e.g., a phenyl group). Examples of the alkyl group include C groups such as a methyl group and an ethyl group. 1-4 In R2, examples of the hydrolytic condensable group include a hydroxyl group, a halogen atom (e.g., a chlorine atom), an alkoxy group, an acyloxy group, an aryloxy group (e.g., a phenoxy group), and a mercapto group. In R2, examples of the alkoxy group include C groups such as a methoxy group and an ethoxy group. 1-4 In R2, examples of the acyloxy group include an acetyloxy group, a propionyloxy group, and the like. 2-4 Examples include an acyloxy group.

[0105] Examples of the silane group-containing monomer include vinyl group-containing silanes {e.g., halosilanes having a vinyl group (e.g., vinyl mono- to trihalosilanes such as vinyltrichlorosilane), alkoxysilanes having a vinyl group (e.g., vinyl alkoxysilanes (e.g., vinyl mono- to trialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane, preferably vinyl mono- to trialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane), 1-4 Alkoxysilane), vinyl alkoxyalkoxysilane (for example, vinyl mono- to tri-(C alkoxysilane) such as vinyl tri(methoxyethoxy)silane and vinyl tris(β-methoxyethoxy)silane) 1-4 Alkoxy C 1-4 alkoxy)silane), styryl group-containing silane (for example, styryl mono- to trialkoxysilane such as p-styryltrimethoxysilane, preferably styryl mono- to tri-C 1-4 alkoxysilanes)]}, (meth)acryloyl group-containing silanes {for example, alkoxysilanes having a (meth)acryloyl group [for example, (meth)acryloxyalkyl mono- to trialkoxysilanes such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane, preferably (meth)acryloxyC 2-4 Alkyl mono to tri C 1-4 Alkoxysilane], hydroxysilane having a (meth)acryloyl group [for example, (meth)acryloxyalkylhydroxysilane such as 3-(meth)acryloxypropylhydroxysilane and 3-(meth)acryloxypropylmethylhydroxysilane, preferably (meth)acryloxyC 2-4 alkylhydroxysilanes}.

[0106] In one embodiment of the coating composition of the present invention, the water-dispersible resin can comprise at least one selected from the group consisting of ultraviolet absorbers and radical scavengers, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer whose homopolymer Tg is less than 50°C, and / or a monomer whose homopolymer Tg is 50°C or higher, and / or a water-dispersible resin containing a cross-linking component as a constituent derived from an acrylic component and / or a non-acrylic component.

[0107] The amount of the crosslinkable monomer in the water-dispersible resin is preferably from 1.0 to 30.0% by mass, more preferably from 1.5 to 25.0% by mass, and further preferably from 2.0 to 20.0% by mass.

[0108] The water-dispersible resin preferably includes a water-dispersible resin containing a reactive emulsifier as a constituent (repeating unit, etc.). The water-dispersible resin containing a reactive emulsifier as a constituent may be a water-dispersible resin containing an acrylic component as a constituent, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent, a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent, a water-dispersible resin containing a cyclic aliphatic monomer as a constituent, a water-dispersible resin containing a monomer having a homopolymer Tg of less than 50°C as a constituent, a water-dispersible resin containing a monomer having a homopolymer Tg of 50°C or more as a constituent, or a water-dispersible resin containing a crosslinking component as a constituent.

[0109] The reactive emulsifier is an emulsifier having a polymerizable group. Examples of the polymerizable group include polymerizable unsaturated groups such as alkenyl groups (vinyl groups, allyl groups, etc.) and alkenylcarbonyl groups (e.g., (meth)acryloyl groups, crotonoyl groups, etc.). The reactive emulsifier may be either an acrylic component or a non-acrylic component, but is preferably an acrylic component. The reactive emulsifier may be used alone or in combination of two or more types.

[0110] Examples of reactive emulsifiers include propenyl-alkyl sulfosuccinate salts, (meth)acrylic acid polyoxyethylene sulfonate salts, polyoxyethylene alkylpropenyl phenyl ether ammonium sulfate, sulfonate salts of allyloxymethyl alkyloxy polyoxyethylene, sulfonate salts of allyloxymethyl nonylphenoxyethyl hydroxypolyoxyethylene, allyloxymethyl alkoxyethyl hydroxypolyoxyethylene sulfate salts, bis(polyoxyethylene polycyclic phenyl ether) methacrylated sulfonate salts, allyloxymethyl alkoxyethyl hydroxypolyoxyethylene, polyoxyethylene alkylpropenyl phenyl ether, allyloxymethyl nonylphenoxyethyl hydroxypolyoxyethylene, and the like.

[0111] In one embodiment of the coating composition of the present invention, the water-dispersible resin may comprise at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer whose homopolymer has a Tg of less than 50°C, and / or a monomer whose homopolymer has a Tg of 50°C or more, and / or a cross-linking component, and / or a reactive emulsifier, as components derived from an acrylic component and / or a non-acrylic component.

[0112] The amount of the reactive emulsifier in the water-dispersible resin is preferably from 0.1 to 15.0% by mass, more preferably from 0.3 to 12.0% by mass, and even more preferably from 0.5 to 10.0% by mass.

[0113] Water-dispersible resins have a Martens hardness of 5 to 90 N / mm 2 It is preferable that the water-dispersible resin contains a water-dispersible resin having a Martens hardness of 5 to 90 N / mm 2 By using a water-dispersible resin, it is possible to prevent the occurrence of fine cracks in the coating film. 2The water-dispersible resin may be a water-dispersible resin containing an acrylic component as a constituent element, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a constituent element, a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a constituent element, a water-dispersible resin containing a cyclic aliphatic monomer as a constituent element, a water-dispersible resin containing a monomer having a homopolymer Tg of less than 50°C as a constituent element, a water-dispersible resin containing a monomer having a homopolymer Tg of 50°C or more as a constituent element, a water-dispersible resin containing a crosslinking component as a constituent element, or a water-dispersible resin containing a reactive emulsifier as a constituent element.

[0114] In one embodiment of the coating composition of the present invention, the water-dispersible resin contains at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer having a homopolymer Tg of less than 50°C, and / or a monomer having a homopolymer Tg of 50°C or more, and / or a crosslinking component, and / or a reactive emulsifier as constituents derived from an acrylic component and / or a non-acrylic component, and has a Martens hardness of 5 to 90 N / mm 2 The resin may include

[0115] The water-dispersible resin can be obtained by polymerization of monomer components as constituent elements, and is preferably obtained by emulsion polymerization of the monomer components as constituent elements. The monomer components may be used alone or in combination of two or more.

[0116] Examples of the monomer component include the above-mentioned polymerizable ultraviolet absorber, polymerizable radical scavenger, monomer with SP value of 9.4 or less, cyclic aliphatic monomer, monomer with homopolymer Tg of less than 50° C., monomer with homopolymer Tg of 50° C. or more, polymerizable cross-linking component (also called cross-linking monomer) and reactive emulsifier, as well as alkyl (meth)acrylate, alkoxy alkyl (meth)acrylate, hydroxyl group-containing monomer, aromatic monomer, acid group-containing monomer, nitrogen atom-containing monomer, oxo group-containing monomer, fluorine atom-containing monomer, etc. The monomer component may be either an acrylic component or a non-acrylic component.

[0117] Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, amyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, n-lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate. 1-20 Examples thereof include alkyl (meth)acrylates.

[0118] Examples of alkoxyalkyl (meth)acrylates include C 2-methoxyethyl (meth)acrylate. 1-12 Alkoxy C 1-12 Examples thereof include alkyl (meth)acrylates.

[0119] Examples of the hydroxyl group-containing monomer include hydroxyl group-containing (meth)acrylates, such as hydroxyalkyl (meth)acrylates [e.g., hydroxy C such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate]. 2-10 Alkyl (meth)acrylate, preferably hydroxy C 2-6 Alkyl (meth)acrylate, more preferably hydroxy C 2-4 alkyl (meth)acrylates], (meth)acrylates of polyols having three or more hydroxyl groups [e.g., tri- to hexahydroxy C such as glycerin mono(meth)acrylate, 3-10 (Meth)acrylate of polyol], and the like.

[0120] Examples of aromatic monomers include styrene monomers [e.g., styrene, α-alkylstyrene (e.g., α-C such as α-methylstyrene, etc.] 1-4 C alkylstyrenes, alkylstyrenes (e.g., vinyltoluene, etc. 1-4 alkylstyrenes), halostyrenes (e.g., chlorostyrenes), etc.], aromatic (meth)acrylates [e.g., aryl (meth)acrylates (e.g., phenyl (meth)acrylates, etc. 6-10 Aryl (meth)acrylate), aralkyl (meth)acrylate (e.g., benzyl (meth)acrylate, phenethyl (meth)acrylate, etc. 6-10 Aryl C 1-4 alkyl (meth)acrylate), aryloxyalkyl methacrylate (e.g., phenoxyethyl methacrylate, etc. 6-10 Aryloxy C 1-4 alkyl methacrylates).

[0121] Examples of the acid group-containing monomer include carboxylic acid group-containing monomers and sulfonic acid group-containing monomers. Examples of the carboxylic acid group-containing monomer include unsaturated monocarboxylic acids (e.g., aliphatic unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid), and unsaturated dicarboxylic acids (e.g., aliphatic unsaturated monocarboxylic acids such as maleic acid and fumaric acid). Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid. The acid group-containing monomer may be anionized (or may form a salt).

[0122] Examples of the nitrogen atom-containing monomer include (meth)acrylamide-based compounds, nitrogen atom-containing (meth)acrylate compounds, N-vinylpyrrolidone, (meth)acrylonitrile, etc. Examples of the (meth)acrylamide-based compounds include N-substituted (meth)acrylamides such as (meth)acrylamide, diacetone (meth)acrylamide, N-monomethyl (meth)acrylamide, N-monoethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, Nn-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, methylene bis (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, and diacetone (meth)acrylamide [e.g., N-alkyl (meth)acrylamides (e.g., N,N-diC 1-4 Examples of the nitrogen atom-containing (meth)acrylate compound include N-substituted aminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate (for example, N,N-diC alkyl (meth)acrylamide). 1-4 Alkylamino C 2-4 Alkyl (meth)acrylates, etc.

[0123] Examples of the oxo group-containing monomer include (di)ethylene glycol (methoxy)(meth)acrylates such as ethylene glycol (meth)acrylate, ethylene glycol methoxy(meth)acrylate, diethylene glycol (meth)acrylate, and diethylene glycol methoxy(meth)acrylate.

[0124] Examples of the fluorine atom-containing monomer include fluorine atom-containing acrylic monomers [e.g., fluoroalkyl(meth)acrylates (e.g., trifluoroethyl(meth)acrylate, tetrafluoropropyl(meth)acrylate, octafluoropentyl(meth)acrylate, etc. fluoro C 1-10 Alkyl (meth)acrylate, preferably fluoro C 2-6 alkyl (meth)acrylates).

[0125] The water-dispersible resin may be a resin having a single phase structure or a resin having a heterogeneous phase structure. In this specification, the term "heterogeneous phase structure resin" refers to a resin in which different monomer compositions constitute multiple sites and exist in a domain or layer form. Among these, a resin in which multiple sites constituted by one or more monomer compositions exist in a layer form is also called a "multilayer structure resin". In addition, the inner layer of the water-dispersible resin particles having this multilayer structure is called the "core" and the outer layer is called the "shell", and this may be called a resin having a core-shell structure. On the other hand, a resin having a single phase structure is a resin in which the monomer composition is not divided into domains or layers, preferably a resin in which the monomer composition is uniformly distributed. The single layer structure can be prepared by one-stage emulsion polymerization, and the heterogeneous phase structure can be prepared by multiple-stage emulsion polymerization. The heterogeneous phase structure has, for example, 2 to 5 layers or domains, preferably 2 to 3 layers or domains.

[0126] The heterogeneous phase structure can be used, for example, to prepare a water-dispersible resin having two or more glass transition temperatures. This allows the heterogeneous phase structure to be composed of a hard layer or domain (hard layer or domain) and a soft layer or domain (soft layer or domain). For example, in the case of a water-dispersible resin particle having a multi-layer structure, the outer layer (the outermost layer in the case of three or more layers) may be a hard layer and the inner layer (a layer other than the outermost layer in the case of three or more layers) may be a soft layer, or the outer layer (the outermost layer in the case of three or more layers) may be a soft layer and the inner layer (a layer other than the outermost layer in the case of three or more layers) may be a hard layer. In addition, when there are multiple inner layers, there may be a hard layer and a soft layer between the inner layers.

[0127] The method of emulsion polymerizing the monomer components may be emulsion polymerized in the presence of an emulsifier. For example, a method of mixing (dropping, etc.) the monomer components into a solvent (solution) containing an emulsifier and polymerizing the monomer components, a method of mixing (dropping, etc.) the previously emulsified monomer components into a solvent and polymerizing the monomer components, etc. can be mentioned. As the solvent, an aqueous solvent such as water or a mixed solvent of water and a water-soluble organic solvent can usually be used. As the water-soluble organic solvent, alcohol, for example, C such as methanol, ethanol, etc. can be used. 1-4 Alcohols and the like can be mentioned. The water-soluble organic solvent can be used alone or in combination of two or more. As a method for producing a heterogeneous phase structure, for example, a multi-stage emulsion polymerization method in which the above-mentioned emulsion polymerization is repeatedly performed can be mentioned.

[0128] Examples of the emulsifier include the above-mentioned reactive emulsifiers, as well as anionic emulsifiers, nonionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, polymeric emulsifiers, etc. The emulsifiers may be used alone or in combination of two or more.

[0129] Examples of the anionic emulsifier include alkyl sulfate salts such as ammonium dodecyl sulfate and sodium dodecyl sulfate; alkyl sulfonate salts such as ammonium dodecyl sulfonate and sodium dodecyl sulfonate; alkyl aryl sulfonate salts such as ammonium dodecyl benzene sulfonate and sodium dodecyl naphthalene sulfonate; polyoxyethylene alkyl sulfate salts; polyoxyethylene alkyl aryl sulfate salts; dialkyl sulfosuccinates; aryl sulfonic acid-formalin condensates; and fatty acid salts such as ammonium laurate and sodium stearylate.

[0130] Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, condensates of polyethylene glycol and polypropylene glycol, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, and condensates of ethylene oxide and aliphatic amines.

[0131] Examples of the cationic emulsifier include alkyl ammonium salts such as dodecyl ammonium chloride.

[0132] Examples of amphoteric emulsifiers include betaine ester emulsifiers.

[0133] Examples of polymeric emulsifiers include poly(meth)acrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; polyhydroxyalkyl(meth)acrylates such as polyhydroxyethyl acrylate; and polymers containing one or more of the monomers constituting these polymers as copolymerization components.

[0134] When polymerizing the monomer components, a polymerization initiator can be used. As the polymerization initiator, those generally used in conventional radical polymerization can be used, and among them, water-soluble ones are preferable. For example, persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-aminodipropane) hydrochloride, 4,4'-azobis-cyanovaleric acid, 2,2'-azobis(2-methylpropionamidine), and 2,2'-azobis(2-methylbutanamideoxime) dihydrochloride tetrahydrate; and peroxides such as hydrogen peroxide, t-butyl hydroperoxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide. The polymerization initiator may be used alone or in combination of two or more. The amount of the polymerization initiator per 100 parts by mass of the monomer component is, for example, 0.01 to 3 parts by mass.

[0135] In order to promote the decomposition of the polymerization initiator, for example, a reducing agent such as L-ascorbic acid, sodium thiosulfate, sodium hydrogen sulfite, or a decomposing agent for the polymerization initiator such as a transition metal salt such as ferrous sulfate may be added in an appropriate amount to the reaction system. In addition, if necessary, for example, an additive such as a chain transfer agent, a pH buffer, or a chelating agent may be added in an appropriate amount to the reaction system. Examples of the chain transfer agent include alkyl mercaptans, aromatic mercaptans, and halogenated hydrocarbons, and among these, lauryl mercaptan, n-butyl mercaptan, t-butyl mercaptan, octyl mercaptan, n-dodecyl mercaptan, 2-ethylhexyl thioglycolate, 2-methyl-t-butylthiophenol, carbon tetrabromide, and α-methylstyrene dimer are preferred.

[0136] The atmosphere in which the monomer components are emulsion-polymerized is not particularly limited, but is preferably an inert gas such as nitrogen gas. The polymerization temperature in which the monomer components are emulsion-polymerized is not particularly limited, but is usually preferably 50 to 100°C. The polymerization temperature may be constant or may be changed during the polymerization reaction. The polymerization time for emulsion-polymerizing the monomer components is not particularly limited and may be appropriately set depending on the progress of the polymerization reaction, but is usually about 2 to 9 hours.

[0137] The water-dispersible resin has a weight-average molecular weight of preferably 100,000 or more, more preferably 300,000 or more, even more preferably 550,000 or more, and particularly preferably 600,000 or more. The upper limit of the weight-average molecular weight of the water-dispersible resin is not particularly limited when it has a crosslinked structure, since it is difficult to measure the weight-average molecular weight, but when it does not have a crosslinked structure, it is preferably 5,000,000 or less from the viewpoint of improving film-forming properties.

[0138] In this specification, the weight average molecular weight of the water-dispersible resin is a value measured by gel permeation chromatography (GPC), using polystyrene as the standard substance and tetrahydrofuran as the mobile phase.

[0139] The water-dispersible resin preferably has at least two glass transition temperatures. The water-dispersible resin may be a resin having at least two glass transition temperatures (particularly a resin having a heterophase structure), or may be two or more types of resin having different glass transition temperatures. The water-dispersible resin preferably has at least a glass transition temperature (Tg1) of 15°C to 35°C and a glass transition temperature (Tg2) of 55 to 150°C. This makes it possible to form a coating film that has hardness and elasticity, is resistant to cracking and scratches, and has excellent blocking resistance and durability.

[0140] In this specification, the glass transition temperature (Tg) of a resin refers to a value measured by DSC in accordance with JIS K7121: 2012. Specifically, about 10 mg of a resin piece is placed in an aluminum pan for measurement, and DSC measurement is performed under the following measurement conditions to determine the glass transition temperature. (Measurement temperature conditions) 1st temperature rise: -80℃~220℃(20℃ / min) Temperature drop condition: 220℃~-80℃(50℃ / min) 2nd temperature rise: -80℃~220℃(10℃ / min)

[0141] The coating composition of the present invention preferably further contains a crosslinking component. By using the crosslinking component, a crosslinked structure can be imparted to the resin when forming a coating film. The crosslinking by the crosslinking component may be intramolecular crosslinking (particularly intraparticle crosslinking) or intermolecular crosslinking (particularly interparticle crosslinking), but intermolecular crosslinking is preferred because it has a greater effect of suppressing the outflow of the ultraviolet absorber and radical scavenger from the coating film. In addition, by using the crosslinking component, the adhesion to the layer (particularly the design layer) to which the coating composition of the present invention is applied can also be improved. In a preferred embodiment of the coating composition of the present invention, the water-dispersible resin comprises a resin that includes a crosslinking component as a component, and / or the coating composition further comprises a crosslinking component (apart from the water-dispersible resin).

[0142] Examples of the crosslinking component include, in addition to the crosslinking component that is a constituent element of the water-dispersible resin described above, silane coupling agents and crosslinking agents. Examples of the crosslinking agent include melamine-based crosslinking agents, oxazoline-based crosslinking agents, acrylamide-based crosslinking agents, polyamide-based crosslinking agents, epoxy-based crosslinking agents, isocyanate-based crosslinking agents, aziridine-based crosslinking agents, titanate-based crosslinking agents, urea-based crosslinking agents, alkyl alcohol-modified urea-based crosslinking agents, hydrazide-based crosslinking agents, carbodiimide-based crosslinking agents, zirconium compounds, zinc compounds, titanium compounds, aluminum compounds, and other polyvalent metal compounds. Among these, silane coupling agents, oxazoline-based crosslinking agents, and carbodiimide-based crosslinking agents are preferred. The crosslinking component may be used alone or in combination of two or more.

[0143] As the silane coupling agent, for example, the above-mentioned silane group-containing monomers can be used, and an epoxy group-containing silane coupling agent is preferred.

[0144] Examples of oxazoline crosslinking agents include 2,2'-bis(2-oxazoline), 1,2-bis(2-oxazoline-2-yl)ethane, 1,4-bis(2-oxazoline-2-yl)butane, 1,8-bis(2-oxazoline-2-yl)butane, 1,4-bis(2-oxazoline-2-yl)cyclohexane, 1,2-bis(2-oxazoline-2-yl)benzene, 1,3-bis(2-oxazoline-2-yl)benzene, 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline.

[0145] Examples of the carbodiimide crosslinking agent include carbodiimide compounds such as N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimide, N-[3-(dimethylamino)propyl]-N'-ethylcarbodiimide methiodide, N-tert-butyl-N'-ethylcarbodiimide, N-cyclohexyl-N'-(2-morpholinoethyl)carbodiimide meso-p-toluenesulfonate, N,N'-di-tert-butylcarbodiimide, and N,N'-di-p-tolylcarbodiimide; carbodiimide compounds obtained by a known condensation reaction of polyisocyanate in the presence of a carbodiimidization catalyst; and carbodiimide compounds made from polyisocyanate and polyalkylene oxide as raw materials.

[0146] In the coating composition of the present invention, the amount of the crosslinking component in the coating film-forming components is preferably 0.5 to 20.0 mass%, more preferably 2.0 to 17.0 mass%, and even more preferably 3.0 to 15.0 mass%. Here, when the crosslinking component is composed of a crosslinking component contained as a constituent element in the resin and a crosslinking component contained separately in the coating composition, the "amount of the crosslinking component" means the total amount of the crosslinking components.

[0147] The coating composition of the present invention has a Martens hardness of 5 to 90 N / mm 2 A coating film exposed to the elements and the sun for a long period of time outdoors will develop fine cracks, causing a problem of reduced weather resistance. 2 By using a flexible resin, it is possible to prevent the occurrence of cracks in the coating film for a long period of time. 2 It is preferable that:

[0148] Martens hardness: 5 to 90N / mm 2 As described above, the resin may be a water-dispersible resin or a resin other than a water-dispersible resin. In one embodiment of the coating composition of the present invention, the water-dispersible resin has a Martens hardness of 5 to 90 N / mm 2 and / or the coating composition of the present invention has a Martens hardness of 5 to 90 N / mm 2 The resin further contains another resin having a Martens hardness of 5 to 90 N / mm 2 The resins may be used alone or in combination of two or more.

[0149] In this specification, Martens hardness refers to a value measured using a microhardness tester (e.g., Shimadzu DUH-211 microhardness tester) with a 115° triangular pyramid indenter under conditions of a temperature of 20°C, a relative humidity of 50%, a test force of 5 mN, a loading rate of 1 mN / sec, and a loading and unloading holding time of 5 sec. The Martens hardness (HMs) can be determined from the slope of the test force vs. indentation depth curve.

[0150] For the sample for measuring Martens hardness, a resin solution with a solid content of 38% by mass is prepared by mixing a film-forming assistant with the resin so that the minimum film-forming temperature is 40°C, and adding an antifoaming agent and thickener as appropriate. The resin solution is applied to a tinplate using a 10-mil applicator, dried in a drying oven at 100°C for 5 minutes, and then cured at room temperature for 1 week to prepare a sample for measurement. The applicator gap can be changed so that the sample for measurement has a film thickness of 40 μm.

[0151] The Martens hardness of a resin is affected by both the composition of the monomers that make up the resin and the particle structure of the water-dispersible resin, so the Martens hardness is set to 5 to 90 N / mm 2 In order to keep the hardness within this range, it is necessary to consider the monomer composition and the polymerization method. As a result of the inventors' investigation, it was found that the Martens hardness is affected to a certain extent by the Tg of the monomer, and that a resin with a homogeneous layer structure whose Tg is higher than 55°C has a Martens hardness of 90 N / mm 2 However, this cannot be determined solely from Tg. For example, when the amount of a monomer having an aromatic ring skeleton such as styrene increases, the Martens hardness becomes 90 N / mm 2 It was found that the Martens hardness tends to be larger than the Tg, and conversely, in monomers with an alicyclic skeleton such as cyclohexyl methacrylate, the Martens hardness tends to be lower than the Tg. It was also confirmed that resins with a heterophase structure and containing soft parts tend to have a low Martens hardness, and that increasing the crosslink density tends to increase the Martens hardness. From these findings, it was found that the Martens hardness of a resin is 5N / mm 2 When the Martens hardness is less than 90 N / mm, the Martens hardness can be increased by increasing the blending ratio of a monomer that has a high Tg when formed into a film by itself, increasing the blending ratio of a monomer having an alicyclic skeleton or an aromatic skeleton, or increasing the crosslink density of the coating film. 2 If the Martens hardness exceeds this value, the Martens hardness can be reduced by increasing the proportion of a monomer that has a low Tg when formed into a film alone, by adding a monomer with four or more alkyl chains, or by reducing the crosslink density of the coating film.

[0152] In the coating composition of the present invention, the Martens hardness of the coating film forming component is 5 to 90 N / mm 2 The amount of the resin is preferably 5.0 to 99.0% by mass, more preferably 10.0 to 75.0% by mass, and further preferably 20.0 to 60.0% by mass. 2 The amount of resin is determined by the Martens hardness of 5 to 90N / mm 2 When the resin is composed of a water-dispersible resin and other resins, the total amount means the total amount of the resins.

[0153] The coating composition of the present invention preferably contains an adhesion improver. As described above, the crosslinking component can improve the adhesion of the coating composition of the present invention to the layer (particularly the design layer) to which it is applied, and therefore can also be expressed as an adhesion improver. In addition to the crosslinking component, the adhesion improver preferably includes silane group-containing monomers, hydroxyl group-containing monomers, and nitrogen atom-containing monomers (preferably amino group-containing monomers and amide group-containing monomers) among the monomer components used in the water-dispersible resin described above, and among these, the crosslinking component is particularly preferred. In addition, a silane coupling agent is also suitable as an adhesion improver. The adhesion improver may be used alone or in combination of two or more types.

[0154] Examples of the silane coupling agent include an amino group-containing silane coupling agent, an epoxy group-containing silane coupling agent, and an isocyanate group-containing silane coupling agent.

[0155] Specific examples of amino group-containing silane coupling agents include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriisopropoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane. silane, N-β-(aminoethyl)-γ-aminopropyltriisopropoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-8-aminooctyltrimethoxysilane, γ-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and the like.

[0156] Specific examples of epoxy group-containing silane coupling agents include glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyldimethylmethoxysilane, γ-glycidoxypropyl(ethyl)dimethoxysilane, β-3,4-epoxycyclohexylethyltrimethoxysilane, β-3,4-epoxycyclohexylethyltriethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 8-glycidoxyoctylmethyldimethoxysilane, and 8-glycidoxyoctylmethyldiethoxysilane.

[0157] A specific example of the isocyanate group-containing silane coupling agent is 3-isocyanatepropyltriethoxysilane.

[0158] In the coating composition of the present invention, the amount of adhesion improver in the coating film-forming components is preferably 1.0 to 40.0 mass%, more preferably 3.0 to 34.0 mass%, and even more preferably 4.5 to 30.0 mass%. Here, when the adhesion improver consists of an adhesion improver dispersed or dissolved in the coating composition and an adhesion improver contained as a constituent element in the resin, the "amount of adhesion improver" means the total amount thereof.

[0159] In the coating composition of the present invention, the water-dispersible resin preferably contains a water-dispersible resin containing an adhesion improver as a component. The water-dispersible resin containing an adhesion improver as a component may be a water-dispersible resin containing an acrylic component as a component, a water-dispersible resin containing at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger as a component, a water-dispersible resin containing a monomer having an SP value of 9.4 or less as a component, a water-dispersible resin containing a cyclic aliphatic monomer as a component, a water-dispersible resin containing a monomer having a homopolymer Tg of less than 50°C as a component, a water-dispersible resin containing a monomer having a homopolymer Tg of 50°C or more as a component, a water-dispersible resin containing a crosslinking component as a component, a water-dispersible resin containing a reactive emulsifier as a component, or a water-dispersible resin having a Martens hardness of 5 to 90 N / mm 2 The resin may be a water-dispersible resin.

[0160] In one embodiment of the coating composition of the present invention, the water-dispersible resin contains at least one selected from the group consisting of an ultraviolet absorber and a radical scavenger, and / or a monomer having an SP value of 9.4 or less, and / or a cyclic aliphatic monomer, and / or a monomer having a homopolymer Tg of less than 50°C, and / or a monomer having a homopolymer Tg of 50°C or more, and / or a crosslinking component, and / or a reactive emulsifier, and / or an adhesion improver other than the crosslinking component, as constituents derived from an acrylic component and / or a non-acrylic component, and has a Martens hardness of 5 to 90 N / mm 2 The resin may include

[0161] The amount of the adhesion improver in the water-dispersible resin is preferably from 1.5 to 60.0 mass %, more preferably from 4.5 to 50.0 mass %, and even more preferably from 7.0 to 40.0 mass %.

[0162] The coating composition of the present invention preferably contains 10% by weight or more, more preferably 10.0 to 70.0% by mass, and even more preferably 10.0 to 35.0% by mass, of a monomer that gives a homopolymer Tg of less than 50°C in the resin component. The flexibility of the resin can be improved by using a monomer that gives a homopolymer Tg of less than 50°C. The homopolymer Tg here is preferably -90°C or more and less than 15°C.

[0163] Here, the "resin components contained in the coating composition" refer to components that become part of the resin after the coating film is formed, in addition to the resin, and include resins and cross-linking components, etc. In addition, components contained as constituent elements in the resin (ultraviolet absorbers, radical scavengers, etc.) are also included in the resin components because they are part of the resin.

[0164] The coating composition of the present invention contains a resin component in the coating composition, which preferably contains 40% by weight or more, more preferably 40.0 to 95.0% by mass, of a monomer having a homopolymer Tg of 50° C. or higher. By using a monomer having a homopolymer Tg of 50° C. or higher, the rigidity of the resin can be improved. The homopolymer Tg here is preferably 50 to 130° C.

[0165] The coating composition of the present invention may contain a surfactant. Surfactants are classified into anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. The amount of the surfactant in the coating composition of the present invention is preferably 15.0 mass% or less, and more preferably 1.0 to 12.0 mass%.

[0166] The coating composition of the present invention is preferably an aqueous coating composition. In this specification, the term "aqueous coating composition" refers to a coating composition containing water as a main solvent. The water is not particularly limited, but preferred examples include pure water such as ion-exchanged water and distilled water. In addition, when the coating composition is to be stored for a long period of time, water that has been sterilized by ultraviolet irradiation or the like may be used to prevent the growth of mold and bacteria. In the coating composition of the present invention, the amount of water is preferably 20 to 80% by mass, more preferably 30 to 70% by mass.

[0167] The coating composition of the present invention is suitable for forming a surface protective layer for protecting a design layer. Since the coating composition of the present invention can achieve a high level of weather resistance, it is suitable as a coating composition for a surface protective layer because it can protect the design for a long period of time even when the design layer is an active energy ray-curable ink or when a photocatalyst layer is present on the outermost layer. In particular, the coating composition of the present invention has a Martens hardness of 5 to 90 N / mm 2 When the surface protective layer contains this resin, the resistance to swelling and shrinkage of the layers below the surface protective layer and the substrate and to changes in outdoor environmental temperature is improved, and the occurrence of cracks in the surface protective layer can be prevented, thereby ensuring a high level of weather resistance for a long period of time.

[0168] The coating composition of the present invention may be a clear coating or an enamel coating, but is preferably a clear coating. In this specification, the clear coating refers to a clear coating having a visible light transmittance of 60% or more when a film having a thickness of 10 μm is formed, and the light transmittance is preferably 70% or more, and particularly preferably 80% or more. When the coating composition of the present invention is applied onto a design layer as a clear coating, the design layer can be protected without impairing the design of the design layer, and when the coating composition of the present invention protects a substrate as a clear coating, the design of the substrate can be protected without impairing the design.

[0169] The visible light transmittance means the total light transmittance in the visible region (360 nm to 750 nm), and can be measured in accordance with JIS K 7375:2008.

[0170] The coating composition of the present invention preferably has an ultraviolet ray transmittance of less than 30%, more preferably less than 20%, and even more preferably less than 10%, when a film having a thickness of 10 μm is formed.

[0171] In this specification, ultraviolet transmittance means the transmittance of light in the wavelength range from 280 nm to 400 nm, and can be measured using a spectrophotometer. Specifically, the coating composition of the present invention is applied to quartz glass so that the dry film thickness is 10 μm, and then dried in a drying oven at 80° C. for 10 minutes to prepare a sample for measurement. The ultraviolet transmittance of the sample can then be measured using a UV-visible spectrophotometer (e.g., Shimadzu UV-2450).

[0172] The coating composition of the present invention can contain other components, such as other resins, solvents, pigments, matte beads, color beads, mica, surface conditioners, wetting agents, dispersants, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, color separation inhibitors, viscosity adjusters, rheology control agents, leveling agents, defoamers, drying agents, plasticizers, preservatives, anti-fungal agents, antibacterial agents, insecticides, antiviral agents, antistatic agents, and conductivity imparting agents, as appropriate depending on the purpose.

[0173] The coating composition of the present invention can be prepared by mixing various components appropriately selected as necessary. The coating composition of the present invention may be a one-component type or a two-component type, but in the case of a two-component type coating composition, the base agent and the curing agent are prepared in advance and mixed at the time of painting, so that the coating composition can be prepared. Usually, the base agent contains a resin, and the curing agent contains a crosslinking agent. When mixing the base agent and the curing agent, additives such as water and a diluent may be further added for the purpose of adjusting the viscosity, etc.

[0174] The coating composition of the present invention has a viscosity of 1 to 1000 (Pa s, 23°C) at a shear rate of 0.1 (1 / s), and preferably has a viscosity of 0.05 to 10 (Pa s, 23°C) at a shear rate of 1000 (1 / s). In this specification, the viscosity is measured using a rheometer (e.g., ARES rheometer manufactured by TA Instruments) after adjusting the liquid temperature to 23°C.

[0175] The means for applying the coating composition of the present invention is not particularly limited, and known coating means such as brush coating, roller coating, trowel coating, spatula coating, flow coater coating, and spray coating (e.g., air spray coating, airless spray coating), can be used.

[0176] The drying means for the coating composition of the present invention is not particularly limited, and may be either natural drying at ambient temperature or forced drying using a dryer or the like, but forced drying is preferred when the coating composition of the present invention contains a resin with a high glass transition temperature.When the coating composition of the present invention contains a resin containing, as a constituent element, a monomer whose homopolymer Tg is 50°C or higher, it is preferred to apply the coating composition and then heat-dry it at 80 to 150°C.

[0177] Another aspect of the present invention is a method for forming a surface protective layer, which includes applying a coating composition to a design layer to form a surface protective layer. In this specification, this method for forming a surface protective layer is also referred to as the "method for forming a surface protective layer of the present invention." In the method for forming a surface protective layer of the present invention, the coating composition is the coating composition of the present invention described above. The design layer is a layer on which a design is applied. Here, the design is a shape, pattern, or color, or a combination of these. The design layer may also include a monochromatic colored layer, or may consist of only a monochromatic colored layer. Details of the design layer will be described in the description of the coated body of the present invention below.

[0178] In the method for forming a surface protective layer of the present invention, a surface protective layer can be formed by applying a coating composition. Here, the coating means and drying means of the coating composition are as described in the coating composition of the present invention.

[0179] In the method for forming a surface protective layer of the present invention, when the resin component contained in the coating composition contains 40% by weight or more of a monomer having a homopolymer Tg of 50° C. or higher, it is preferable to apply the coating composition and then heat-dry it at 80 to 150° C. By carrying out such a heat treatment, a uniform surface protective layer without unevenness can be formed even when a large amount of a monomer having a high homopolymer Tg is contained.

[0180] In the method for forming a surface protective layer of the present invention, the surface protective layer preferably has a visible light transmittance of 60% or more, more preferably 70% or more, and even more preferably 80% or more. A surface protective layer with a high visible light transmittance can protect the design layer without impairing the design of the design layer.

[0181] In the method for forming a surface protective layer of the present invention, the surface protective layer preferably has an ultraviolet ray transmittance of less than 30%, more preferably less than 20%, and even more preferably less than 10%.

[0182] In the method for forming a surface protective layer of the present invention, the thickness of the surface protective layer is, for example, 3.0 to 100.0 μm, and preferably 5.0 to 70.0 μm.

[0183] In one embodiment of the method for forming a surface protective layer of the present invention, the design layer is an active energy ray-cured layer. The active energy ray-cured layer is a layer obtained by curing an active energy ray-curable ink with active energy rays.

[0184] In one embodiment of the surface protection layer forming method of the present invention, the design layer includes an active energy ray cured layer. Since a design may be expressed using a plurality of materials, the design layer may not be formed only from the active energy ray cured layer, and may include other materials. In this case, it is preferable that the surface protection layer is a layer in contact with the active energy ray cured layer.

[0185] In one embodiment of the method for forming a surface protective layer of the present invention, the design layer may be a monochromatic colored layer. Even in this case, it is preferable that the surface protective layer is a layer in contact with the colored layer.

[0186] The surface protective layer forming method of the present invention may include forming a photocatalyst layer on the surface protective layer. In the surface protective layer forming method of the present invention, the surface protective layer is a layer for protecting the design layer and is a layer located on the surface of the coated body, but is not limited to being located on the outermost surface of the coated body, and an additional layer may be formed on the surface protective layer.

[0187] The photocatalyst layer is a layer containing in its composition a material that exhibits photocatalytic activity when irradiated with light such as sunlight. On the other hand, when a photocatalyst layer is present on the outermost layer, ultraviolet rays may generate radicals that may deteriorate coating films such as the design layer and the surface protection layer. However, in the present invention, the surface protection layer is a layer that is not easily deteriorated by radicals, and therefore the surface protection layer itself and the design layer can exhibit a protective function against such radicals.

[0188] Another aspect of the present invention is a coated body including at least a substrate and a surface protective layer, or a coated body including at least a substrate, a surface protective layer, and a photocatalyst layer. In this specification, this coated body is also referred to as the "coated body of the present invention." In the coated body of the present invention, the surface protective layer is a surface protective layer formed by the coating composition of the present invention described above.

[0189] In the coated body of the present invention, the Martens hardness of the coated body or the surface protective layer is 10 to 200 N / mm 2 It is preferable that the Martens hardness of the coating or surface protective layer is 10 N / mm 2 If it is less than 200N / mm, the coating film becomes too soft and the surface is easily scratched, damaging the appearance. 2 If it is larger, the coating film becomes hard, and it is undesirable that the coating film is likely to crack when exposed to rain, wind, and sunlight for a long period of time. Here, the Martens hardness of the coated body or the surface protective layer can be measured by the same method as the Martens hardness of the resin described in this specification. The Martens hardness of the coated body is the Martens hardness measured for the entire layer formed on the surface of the coated body.

[0190] In the coated body of the present invention, the surface protective layer preferably has at least a glass transition temperature (Tg1) of 15°C to 35°C and a glass transition temperature (Tg2) of 55 to 150°C.

[0191] In this specification, the glass transition temperature of the surface protective layer can be measured using a DSC (differential scanning calorimeter) in accordance with JIS K 7121:2012 (Method for measuring the glass transition temperature of plastics). Specifically, about 10 mg of a film piece of the surface protective layer is collected in an aluminum pan for measurement, and DSC measurement is performed under the following measurement conditions to determine the glass transition temperature. (Measurement temperature conditions) 1st temperature rise: -80℃~220℃(20℃ / min) Temperature drop condition: 220℃~-80℃(50℃ / min) 2nd temperature rise: -80℃~220℃(10℃ / min)

[0192] In the coated body of the present invention, the surface protective layer has a visible light transmittance of preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. Also, in the coated body of the present invention, the surface protective layer has an ultraviolet light transmittance of preferably less than 30%, more preferably less than 20%, and even more preferably less than 10%.

[0193] In the coated body of the present invention, the film thickness of the surface protective layer is, for example, 3.0 to 100.0 μm, and preferably 5.0 to 70.0 μm.

[0194] In the coated body of the present invention, the surface protective layer may be one layer or two or more layers. In one embodiment of the coated body of the present invention, the surface protective layer is composed of at least two layers, a first protective layer containing an adhesion improver and a second protective layer not containing an adhesion improver. Since the crosslinking component contained in the coating composition of the present invention corresponds to an adhesion improver, it is preferable that the first protective layer is a surface protective layer formed by the coating composition of the present invention, and the first protective layer is in contact with the design layer.

[0195] When the surface protective layer in the coated body of the present invention consists of two or more layers, the Martens hardness, glass transition temperature, visible light transmittance, ultraviolet light transmittance and film thickness values ​​of the surface protective layer described above are values ​​for the surface protective layer as a whole.

[0196] The coated body of the present invention may have a design layer on the substrate. In this case, the surface protective layer is preferably a layer for protecting the design layer. In the coated body of the present invention, the design layer preferably includes an active energy ray cured layer. Since a design may be expressed using a plurality of materials, the design layer may not be formed only from the active energy ray cured layer, and may include other materials. In this case, the surface protective layer, particularly the surface protective layer formed by the coating composition of the present invention, is preferably a layer in contact with the active energy ray cured layer.

[0197] The active energy ray curable layer is a layer obtained by curing an active energy ray curable ink with active energy rays. For example, the active energy ray curable ink can be printed on a substrate by a printing means such as printing with an inkjet printer (i.e., inkjet method), and then cured to form the active energy ray curable layer. The thickness of the active energy ray curable layer is, for example, 0.1 to 30.0 μm.

[0198] The active energy ray-curable ink contains a photopolymerizable compound and a photopolymerization initiator.

[0199] A photopolymerizable compound is a compound that undergoes a polymerization reaction via a radically polymerizable functional group (e.g., a photopolymerizable unsaturated group such as a carbon-carbon double bond constituting an acryloyl group, a methacryloyl group, a vinyl group, or an allyl group). A radically polymerizable carbon-carbon double bond is also called an "ethylenically unsaturated double bond."

[0200] Photopolymerizable compounds are classified into monofunctional polymerizable compounds and polyfunctional polymerizable compounds. Here, examples of monofunctional polymerizable compounds include monofunctional polymerizable monomers having one functional group exhibiting radical polymerizability (for example, monofunctional polymerizable monomers having one polymerizable unsaturated group) and monofunctional polymerizable oligomers having one functional group exhibiting radical polymerizability (for example, monofunctional polymerizable oligomers having one polymerizable unsaturated group). Examples of polyfunctional polymerizable compounds include polyfunctional polymerizable monomers having two or more functional groups exhibiting radical polymerizability (for example, polyfunctional polymerizable monomers having two or more polymerizable unsaturated groups) and polyfunctional polymerizable oligomers having two or more functional groups exhibiting radical polymerizability (for example, polyfunctional polymerizable oligomers having two or more polymerizable unsaturated groups).

[0201] Specific examples of monofunctional polymerizable monomers include isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, 2-ethylhexyl-diglycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, ethyl carbitol (meth)acrylate, 2-(2'-vinyl (oxyethoxy)ethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, cyclohexyl (meth)acrylate, N-(meth)acryloylmorpholine, tetrahydrofurfuryl (meth)acrylate, (2-methyl-2-ethyl-1,3-Dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, gamma-butyrolactone (meth)acrylate, N-vinylcaprolactam, N-(meth)acryloyloxyethylhexahydrophthalimide, 1-(meth)acryloylpyrrolidin-2-one, 1-(meth)acryloylpiperidin-2-one, N-vinyl-2-pyrrolidone, N-vinylimidazole, dimethylacrylamide, hydroxyethyl (meth)acrylamide , diethylacrylamide, isopropylacrylamide, dimethylaminopropyl (meth)acrylamide, diacetone acrylamide, Nn-butoxymethylacrylamide, N-isobutoxymethylacrylamide, N-methoxymethylacrylamide, N-methylol acrylamide, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, benzyl (meth)acrylate, neopentyl glycol (meth)acrylic acid benzoate, iso Bornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, γ-(meth)acryloxypropylmethyldimethoxysilane, γ-(meth)acryloxypropylmethyldiethoxysilane, γ-(meth)acryloxypropylmethyldipropoxysilane, γ-(meth)acryloxypropylmethyldipropoxysilane, Examples of the silane include acryloxybutylphenyl dimethoxysilane, γ-(meth)acryloxypropyl dimethyl methoxysilane, γ-(meth)acryloxypropyl diethyl methoxysilane, β-(meth)acryloxyethyl trimethoxysilane, β-(meth)acryloxyethyl triethoxysilane, polyoxyethylene mono(meth)acrylate, polyoxypropylene mono(meth)acrylate, polyoxybutylene mono(meth)acrylate, and the like, and those modified with alkylene glycol.

[0202] Among the polyfunctional polymerizable monomers, specific examples of polyfunctional polymerizable monomers (bifunctional polymerizable monomers) having two functional groups exhibiting radical polymerization include 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, and the like. All di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 2-methyl-1,8-octanediol di(meth)acrylate, diethylene glycol Di(meth)acrylate, dipropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, PO (propylene oxide) modified neopentyl glycol di(meth)acrylate, cyclohexane dimethanol diacrylate, tricyclodecane dimethanol diacrylate, dimethylol-tricyclodecane di(meth)acrylate, dicyclopentanyl diacrylate, bisphenol A di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and the like.

[0203] Specific examples of polyfunctional polymerizable monomers having three or more functional groups exhibiting radical polymerization (polyfunctional polymerizable monomers having three or more functions) include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, EO-modified diglycerin tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, EO-modified dipentaerythritol hexa(meth)acrylate, and glycerin tri(meth)acrylate.

[0204] The polymerizable oligomer is preferably an acrylic oligomer. The acrylic oligomer is an oligomer having an acryloyl group or a methacryloyl group as a functional group exhibiting radical polymerizability. Specific examples of the acrylic oligomer include polyurethane acrylic oligomer [acrylic oligomer having multiple urethane bonds (-NHCOO-)], polyester acrylic oligomer [acrylic oligomer having multiple ester bonds (-COO-)], polyamino acrylic oligomer [acrylic oligomer having multiple amino groups (-NH2)], polyepoxy acrylic oligomer [acrylic oligomer having multiple epoxy groups], silicone acrylic oligomer [acrylic oligomer having multiple siloxane bonds (-SiO-)], polybutadiene acrylic oligomer [acrylic oligomer having multiple butadiene units], etc.

[0205] The amount of the photopolymerizable compound in the active energy ray-curable ink is, for example, 20.0 to 90.0% by mass. The photopolymerizable compound may be used alone or in combination of two or more kinds.

[0206] In the active energy ray curable ink, the average number of functional groups of the photopolymerizable compound is preferably less than 1.5, and more preferably 1.05 to 1.2. When the average number of functional groups of the photopolymerizable compound contained in the ink is less than 1.5, and particularly 1.05 to 1.2, the effect of suppressing the cure shrinkage of the film is high, the adhesion of the film itself can be significantly improved, and the film strength can be maintained. This makes it possible to ensure the adhesion to various substrates and films and the film strength of the active energy ray curable layer itself.

[0207] In this specification, the average number of functional groups of the photopolymerizable compound contained in the ink can be calculated as follows. Average number of functional groups = [total number of ethylenically unsaturated double bonds contained in photopolymerizable compound] / [total number of molecules of photopolymerizable compound] Formula (1) Here, the "total number of ethylenically unsaturated double bonds contained in the photopolymerizable compound" in formula (1) is calculated by multiplying the number of ethylenically unsaturated double bonds per molecule of the photopolymerizable compound by the total number of molecules of the photopolymerizable compound. When multiple types of photopolymerizable compounds are blended in the ink, the number of ethylenically unsaturated double bonds is calculated for each type, and the total number of ethylenically unsaturated double bonds is the total number of ethylenically unsaturated double bonds. (Example of how to determine the average number of functional groups of a photopolymerizable compound) The total amount of the photopolymerizable compounds is 100 parts by mass. Photopolymerizable compound A: Number of ethylenically unsaturated double bonds = 1, molecular weight X A , 30 parts by mass Photopolymerizable compound B: Number of ethylenically unsaturated double bonds = 2, molecular weight X B , 70 parts by mass Average number of functional groups={(1×30 / X A )+(2×70 / X B )} / {(30 / X A )+(70 / X B )}

[0208] The photopolymerization initiator has the effect of initiating polymerization of the above-mentioned photopolymerizable compound by irradiation with active energy rays. Examples of the photopolymerization initiator include benzophenone-based compounds, acetophenone-based compounds, thioxanthone-based compounds, and acylphosphine oxide-based compounds. Furthermore, in order to promote the initiation reaction of the photopolymerization initiator, it is also possible to use an auxiliary such as a photosensitizer in combination.

[0209] The amount of the photopolymerization initiator in the active energy ray-curable ink is, for example, 1 to 15% by mass. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0210] The active energy ray curable ink may contain coloring materials such as dyes and pigments. Known materials may be used as coloring materials, and examples of such materials include inorganic pigments and dyes such as carbon black, yellow iron oxide, red iron oxide, composite oxides (nickel-titanium, chromium-titanium, bismuth-vanadium, cobalt-aluminum, cobalt-aluminum-chromium, ultramarine blue), and titanium oxide, as well as organic pigments and dyes such as quinacridone, diketopyrol, benzimidazolone, isoindolinone, anthrapyrimidine, phthalocyanine, threne, dioxazine, and azo. From the viewpoint of weather resistance, it is preferable to use inorganic pigments.

[0211] The amount of the coloring material in the active energy ray-curable ink is preferably 1 to 20% by mass. The coloring materials may be used alone or in combination of two or more.

[0212] The active energy ray curable ink preferably contains an adhesion improver. By using the adhesion improver, the adhesion of the design layer can be improved. Suitable examples of the adhesion improver for the active energy ray curable ink include hydroxyl group-containing monomers, nitrogen atom-containing monomers (preferably amino group-containing monomers and amide group-containing monomers), silane group-containing monomers, and silane coupling agents.

[0213] Examples of the hydroxyl group-containing monomer include hydroxyl group-containing (meth)acrylates, such as hydroxyalkyl (meth)acrylates [e.g., hydroxy C such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate]. 2-10 Alkyl (meth)acrylate, preferably hydroxy C 2-6 Alkyl (meth)acrylate, more preferably hydroxy C 2-4 alkyl (meth)acrylates], (meth)acrylates of polyols having three or more hydroxyl groups [e.g., tri- to hexahydroxy C such as glycerin mono(meth)acrylate, 3-10 (Meth)acrylate of polyol], and the like.

[0214] Examples of the nitrogen atom-containing monomer include (meth)acrylamide-based compounds, nitrogen atom-containing (meth)acrylate compounds, N-vinylpyrrolidone, (meth)acrylonitrile, etc. Examples of the (meth)acrylamide-based compounds include N-substituted (meth)acrylamides such as (meth)acrylamide, diacetone (meth)acrylamide, N-monomethyl (meth)acrylamide, N-monoethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, Nn-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, methylene bis (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, and diacetone (meth)acrylamide [e.g., N-alkyl (meth)acrylamides (e.g., N,N-diC 1-4 Examples of the nitrogen atom-containing (meth)acrylate compound include N-substituted aminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate (for example, N,N-diC alkyl (meth)acrylamide). 1-4 Alkylamino C2-4 Alkyl (meth)acrylates, etc.

[0215] Examples of the silane group-containing monomer are monomers having a silyl group bonded to a hydrolyzable (condensable) group (eg, an alkoxy group, a halogen atom), and include compounds represented by the following structural formula (3). (R1) n -Si-(R2) 4-n (3) In the structural formula (3), R1 represents a group having a polymerizable unsaturated bond group. R2 represents a hydrogen atom, a hydrolytically condensable group, a hydrocarbon group, or an epoxy group (an epoxy group-containing group), and at least one R2 represents a hydrolytically condensable group. n represents an integer of 1 to 3.

[0216] In the structural formula (3), examples of the polymerizable unsaturated bond group in R1 include a vinyl group, an allyl group, and a (meth)acryloyl group. Examples of the hydrocarbon group in R2 include an alkyl group and an aryl group (e.g., a phenyl group). Examples of the alkyl group include C groups such as a methyl group and an ethyl group. 1-4 In R2, examples of the hydrolytic condensable group include a hydroxyl group, a halogen atom (e.g., a chlorine atom), an alkoxy group, an acyloxy group, an aryloxy group (e.g., a phenoxy group), and a mercapto group. In R2, examples of the alkoxy group include C groups such as a methoxy group and an ethoxy group. 1-4 In R2, examples of the acyloxy group include an acetyloxy group, a propionyloxy group, and the like. 2-4 Examples include an acyloxy group.

[0217] Examples of the silane group-containing monomer include vinyl group-containing silanes {e.g., halosilanes having a vinyl group (e.g., vinyl mono- to trihalosilanes such as vinyltrichlorosilane), alkoxysilanes having a vinyl group (e.g., vinyl alkoxysilanes (e.g., vinyl mono- to trialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane, preferably vinyl mono- to trialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane),1-4 Alkoxysilane), vinyl alkoxyalkoxysilane (for example, vinyl mono- to tri-(C alkoxysilane) such as vinyl tri(methoxyethoxy)silane and vinyl tris(β-methoxyethoxy)silane) 1-4 Alkoxy C 1-4 alkoxy)silane), styryl group-containing silane (for example, styryl mono- to trialkoxysilane such as p-styryltrimethoxysilane, preferably styryl mono- to tri-C 1-4 alkoxysilanes)]}, (meth)acryloyl group-containing silanes {for example, alkoxysilanes having a (meth)acryloyl group [for example, (meth)acryloxyalkyl mono- to trialkoxysilanes such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane, preferably (meth)acryloxyC 2-4 Alkyl mono to tri C 1-4 Alkoxysilane], hydroxysilane having a (meth)acryloyl group [for example, (meth)acryloxyalkylhydroxysilane such as 3-(meth)acryloxypropylhydroxysilane and 3-(meth)acryloxypropylmethylhydroxysilane, preferably (meth)acryloxyC 2-4 alkylhydroxysilanes}.

[0218] Examples of the silane coupling agent include an amino group-containing silane coupling agent, an epoxy group-containing silane coupling agent, and an isocyanate group-containing silane coupling agent.

[0219] Specific examples of amino group-containing silane coupling agents include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriisopropoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane. silane, N-β-(aminoethyl)-γ-aminopropyltriisopropoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-8-aminooctyltrimethoxysilane, γ-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and the like.

[0220] Specific examples of epoxy group-containing silane coupling agents include glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyldimethylmethoxysilane, γ-glycidoxypropyl(ethyl)dimethoxysilane, β-3,4-epoxycyclohexylethyltrimethoxysilane, β-3,4-epoxycyclohexylethyltriethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 8-glycidoxyoctylmethyldimethoxysilane, and 8-glycidoxyoctylmethyldiethoxysilane.

[0221] A specific example of the isocyanate group-containing silane coupling agent is 3-isocyanatepropyltriethoxysilane.

[0222] The amount of the adhesion improver in the active energy ray-curable ink is, for example, 0.1 to 30.0% by mass. The adhesion improver may be used alone or in combination of two or more kinds.

[0223] The active energy ray-curable ink may contain, as other components, additives such as a solvent, a dispersant, a surface conditioner, an antioxidant, a plasticizer, an anti-rust agent, a solvent, an antibacterial agent, an antiviral agent, a viscosity adjuster, a filler, an antifoaming agent, a charge control agent, a stress relaxation agent, a penetrating agent, a light guiding material, a glittering material, a magnetic material, a phosphor, an ultraviolet absorbing agent, and a radical scavenger, as necessary.

[0224] The active energy ray curable ink can be prepared by mixing various components appropriately selected as necessary. In addition, it is preferable to filter the ink using a filter in order to prevent clogging of the nozzles of the head due to impurities, etc.

[0225] The active energy ray curable ink preferably has a surface tension in the range of 20 to 30 mN / m at 25° C. When the ink surface tension at 25° C. is within the above specified range, good ejection stability can be obtained. The surface tension of the ink can be measured by a plate method.

[0226] The printing of the active energy ray curable ink is preferably performed by an inkjet printing method. Inkjet printing can be performed using various inkjet printers. Examples of inkjet printers include inkjet printers that eject the ink composition by a charge control method or a piezoelectric method. Large inkjet printers, specifically inkjet printers intended for printing on articles produced on industrial lines, can also be suitably used.

[0227] The layer formed from the active energy ray curable ink is cured by irradiation with active energy rays such as ultraviolet rays. A high pressure mercury lamp, a metal halide lamp, an LED lamp, etc. can be used as a light source of the active energy rays. In addition, the wavelength of the active energy rays irradiated to cure this layer preferably overlaps with the absorption wavelength of the photopolymerization initiator, and the main wavelength of the active energy rays is preferably 350 to 400 nm. The integrated light amount of the active energy rays is 100 to 2000 mJ / cm. 2 It is preferable that the range is .

[0228] Printing using active energy ray-curable ink can achieve surface finishing such as glossy or matte finishes by appropriately selecting the ejection conditions and subsequent curing conditions. For example, if the ink spreads and then hardens over time, it will have a glossy finish, and if the ink droplets harden while remaining in a lens shape, it will have a matte finish.

[0229] In the coated body of the present invention, when the design layer includes a layer other than the active energy ray-cured layer, the layer other than the active energy ray-cured layer may include layers formed from various paints and inks, such as organic solvent-based paints and inks that use an organic solvent as the main solvent, water-based paints and inks that use water as the main solvent, photocurable paints that use a photopolymerizable compound, and powder paints.

[0230] In the coated body of the present invention, the decorative layer preferably has a glass transition temperature of -10°C to 90°C. When the decorative layer includes an active energy ray-cured layer, the active energy ray-cured layer preferably has a glass transition temperature of -30°C to 60°C.

[0231] The glass transition temperatures of the design layer and the active energy ray-curable layer can be measured by the same method as for the glass transition temperature of the surface protective layer.

[0232] In the coated body of the present invention, the design layer, particularly the active energy ray cured layer, is preferably a layer that can relieve internal stress generated in the laminate structure in order to ensure adhesion to the substrate and other layers (particularly layers formed from water-based paints and inks) and prevent interlayer delamination, and is preferably soft. On the other hand, the surface protective layer is preferably hard from the viewpoint of protecting the design layer from external factors.

[0233] In the coated body of the present invention, the glass transition temperature of the design layer, particularly the active energy ray-cured layer, is preferably lower than that of the surface protective layer. Here, when each layer has a plurality of glass transition temperatures, the "glass transition temperature of the design layer, particularly the active energy ray-cured layer" refers to the highest glass transition temperature among the glass transition temperatures of the design layer, particularly the active energy ray-cured layer, and the "glass transition temperature of the surface protective layer" refers to the lowest glass transition temperature among the glass transition temperatures of the surface protective layer.

[0234] In the coated body of the present invention, the thickness of the decorative layer is, for example, 0.1 to 150.0 μm, and preferably 0.1 to 100.0 μm.

[0235] The coated body of the present invention may further include a photocatalyst layer on the surface protective layer. The photocatalyst layer is a layer containing a material in a composition that exhibits photocatalytic action when irradiated with light such as sunlight. On the other hand, when a photocatalyst layer is present on the outermost layer, radicals may be generated by ultraviolet light, which may deteriorate coating films such as the design layer and the surface protective layer. However, in the present invention, the surface protective layer is a layer that is not easily deteriorated by radicals, so that the surface protective layer itself and the design layer can exhibit a protective function against such radicals.

[0236] Examples of materials that exhibit photocatalytic activity include metal oxides such as anatase type titanium oxide, rutile type titanium oxide, tin oxide, zinc oxide, and cerium oxide, but are not limited to these materials.

[0237] The photocatalyst layer may contain, as other components, additives such as resins, dispersants, surface conditioners, antioxidants, plasticizers, rust inhibitors, solvents, antibacterial agents, antiviral agents, viscosity adjusters, fillers, defoamers, charge control agents, stress relaxation agents, penetrating agents, light-guiding materials, glittering materials, magnetic materials, phosphors, ultraviolet absorbing agents, and radical scavengers, as necessary.

[0238] The photocatalyst layer can be formed from various types of paints and inks, such as organic solvent-based paints and inks that use an organic solvent as the main solvent, water-based paints and inks that use water as the main solvent, photocurable paints and inks that use a photopolymerizable compound, and powder paints.

[0239] In the coated body of the present invention, examples of the substrate include plastic substrates such as epoxy resin, ABS resin, polycarbonate, polyvinyl chloride, polystyrene, acrylic resin, particularly polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), polypropylene (PP), etc.; metal substrates such as iron, stainless steel, aluminum, copper, titanium, and alloys thereof; inorganic substrates other than metals such as cement, concrete, gypsum, calcium silicate, calcium carbonate, marble, artificial marble, glass, ceramic, etc.; paper-based substrates, wood substrates, composite substrates combining two or more of these substrates, etc.

[0240] The shape of the substrate may be, for example, a film, a sheet, a plate, etc. The surface of the substrate may be smooth or may have irregularities.

[0241] Specific examples of the substrate include wood building materials such as veneer, plywood, particle board, and medium density fiberboard (MDF); ceramic building materials such as ceramic siding board, flexible board, calcium silicate board, gypsum slag barite board, wood chip cement board, asbestos cement board, pulp cement board, precast concrete board, lightweight aerated concrete (ALC) board or ALC panel, and gypsum board; various building materials (particularly building boards) such as metal siding board, and metal building materials such as aluminum, iron, and stainless steel. Specific examples of the substrate include plastic substrates such as PVC sheet, tarpaulin, plastic cardboard, and acrylic board, coated paper (specifically resin-coated paper), art paper, cast paper, lightly coated paper, fine paper, synthetic paper, and inkjet paper; tiles, glass plates, and the like.

[0242] The surface of the substrate may be subjected to pretreatment such as degreasing, chemical conversion treatment, and polishing, or may be coated with a sealer or primer. For example, when the substrate is a substrate (particularly a porous substrate) that may excessively absorb paint or ink, such as a ceramic building material, the surface of the substrate may be coated with a sealer and a sealer layer may be formed on the substrate. Also, when the substrate is a metal building material, the surface of the substrate may be coated with a primer and a primer layer may be formed on the substrate.

[0243] In one embodiment of the coated body of the present invention, the coated body can include a substrate, a design layer, and a surface protective layer, where the design layer is located on the substrate or on an undercoat film such as a sealer, and the surface protective layer is located on the design layer and covers the design layer. In addition, the outermost surface layer of the coated body may include a photocatalyst layer, or an overcoat layer containing a water repellent, a hydrophilic agent, etc.

[0244] When the coated body of the present invention includes an ink layer as a design layer, it is preferable to include a receiving layer. The receiving layer is a layer for absorbing ink and fixing a coloring material. By forming a receiving layer on a substrate, the color development of the design layer can be improved, and the adhesion between the design layer and the substrate can be improved via the receiving layer.

[0245] The receiving layer preferably contains a resin, and examples thereof include acrylic resin, silicone resin, acrylic silicone resin, styrene acrylic copolymer resin, polyester resin, fluororesin, rosin resin, petroleum resin, coumarone resin, phenol resin, urethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, vinyl resin, amine resin, ketimine resin, and resins obtained by modifying these resins (modified resins). The amount of the resin in the receiving layer is, for example, 20.0 to 85.0% by mass. The resin may be used alone or in combination of two or more.

[0246] The receiving layer preferably contains a pigment. As the pigment, for example, a pigment commonly used in the paint industry, such as an anti-rust pigment, an extender pigment, a color pigment, or a luster pigment, can be used. The amount of the pigment in the receiving layer is, for example, 0.1 to 80.0% by mass. The pigment may be used alone or in combination of two or more kinds.

[0247] The receiving layer may contain, as other components, additives such as dispersants, surface conditioners, antioxidants, plasticizers, rust inhibitors, solvents, antibacterial agents, antiviral agents, viscosity adjusters, fillers, defoamers, charge control agents, stress relaxation agents, penetrating agents, light-guiding materials, glittering materials, magnetic materials, phosphors, ultraviolet absorbers, and radical scavengers, as necessary.

[0248] The receiving layer can be formed from various types of paints and inks, such as organic solvent-based paints and inks that use an organic solvent as the main solvent, water-based paints and inks that use water as the main solvent, photocurable paints and inks that use a photopolymerizable compound, and powder paints.

[0249] The receiving layer is preferably hard from the viewpoints of protecting the substrate and ensuring adhesion when the substrate is a hard substrate, for example.

[0250] In the coated body of the present invention, the glass transition temperature of the receiving layer is preferably from 10° C. to 80° C. The glass transition temperature of the receiving layer can be measured by the same method as for the glass transition temperature of the surface protective layer.

[0251] In the coated body of the present invention, the glass transition temperatures (Tg) of the receptive layer, the decorative layer and the surface protective layer preferably satisfy the following relationship. Tg of design layer ≦ Tg of receiving layer ≦ Tg of surface protective layer Here, when each layer has multiple glass transition temperatures, "Tg of design layer" refers to the highest glass transition temperature among the glass transition temperatures of the design layers, particularly the active energy ray-cured layer, "Tg of surface protective layer" refers to the lowest glass transition temperature among the glass transition temperatures of the surface protective layers, and "Tg of receiving layer" refers to each Tg of the receiving layer (i.e., each Tg satisfies the above relationship).

[0252] In the coated body of the present invention, the thickness of the receptive layer is, for example, 1.0 to 100.0 μm, and preferably 5.0 to 70.0 μm.

[0253] In one embodiment of the coated body of the present invention, the coated body can include a substrate, a receiving layer, a design layer, and a surface protective layer, where the receiving layer is located on the substrate, the design layer is located on the receiving layer, and the surface protective layer is located on the design layer and covers the design layer. In addition, the coated body may have an overcoat layer containing a photocatalyst layer, a water repellent, a hydrophilic agent, etc., on the outermost surface layer. EXAMPLES

[0254] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0255] <Water dispersible resin> The following were prepared as emulsions for water-dispersible resins 1 to 14. Water-dispersible resins 10 to 12 are resins containing γ-methacryloyloxypropyltrimethoxysilane (KBM503), a crosslinking component, as a constituent element. The Martens hardness of each resin was measured by the following method.

[0256] <Martens hardness of water-dispersible resin> A resin solution with a solid content of 38% by mass was prepared by mixing the water-dispersible resins 1 to 14 with a film-forming assistant so that the minimum film-forming temperature was 40°C. The obtained resin solution was applied to a tin plate using a 6-mil applicator so that the dry film thickness was 40 μm, and then dried in a drying oven at 100°C for 5 minutes, and then aged at room temperature for 1 week to prepare a measurement sample. The Martens hardness of each test plate was measured using a microhardness tester (SHIMADZU microhardness tester DUH-211) with a 115° triangular pyramid indenter under the conditions of a temperature of 20°C, a relative humidity of 50%, a test force of 5 mN, and a loading speed of 3 sec, and the Martens hardness (HMs) was calculated from the slope of the test force vs. indentation depth curve.

[0257] <Details of Water-dispersible Resins 1 to 14> Water-dispersible resin 1: Emulsion polymer of [MMA / CHMA / EHA / HEMA / AA / LA82 (mass ratio 33.5 / 25 / 34 / 3 / 1.5 / 3)], solid content 45% by mass, Martens hardness 28.0N / mm 2 Water-dispersible resin 2: Emulsion polymer of [MMA / CHMA / EHA / BA / HEMA / AA / LA82 (mass ratio 23.5 / 20 / 20 / 29 / 3 / 1.5 / 3)], solid content 45% by mass, Martens hardness 11.0N / mm 2 Water-dispersible resin 3: Emulsion polymer of [MMA / CHMA / EHA / HEMA / AA / TN400 / LA82 (mass ratio 48.5 / 30 / 14 / 2 / 1.5 / 1 / 3)], solid content 45% by mass, Martens hardness 52.0N / mm 2 · Aqueous dispersible resin 4: Emulsion polymer of [MMA / CHMA / EHA / BA / HEMA / AA / TN400 / LA82 (mass ratio 16.5 / 16 / 25 / 35 / 2 / 1.5 / 1 / 3)], solid content 45% by mass, Martens hardness 3.5 N / mm 2 · Aqueous dispersible resin 5: Emulsion polymer of [MMA / CHMA / BMA / EHA / BA / HEMA / AA / TN400 / LA82 (mass ratio 53.5 / 2 / 20 / 10 / 7 / 2 / 1.5 / 1 / 3)], solid content 45% by mass, Martens hardness 72.0 N / mm 2 · Aqueous dispersible resin 6: Emulsion polymer of [First stage: MMA / CHMA / HEMA / AA / LA82 / TN400 (mass ratio 26 / 20 / 2 / 1 / 0.5 / 1), Second stage: CHMA / EHA / HEMA / LA82 / TN400 (mass ratio 21 / 26 / 1 / 0.5 / 1)], solid content 45% by mass, Martens hardness 55.0 N / mm 2 · Aqueous dispersible resin 7: Emulsion polymer of [First stage: MMA / CHMA / EHA / HEMA / AA (mass ratio 10 / 15 / 20 / 3 / 1), Second stage: MMA / CHMA / EHA / HEMA / LA82 (mass ratio 12 / 30 / 4 / 1 / 4)], solid content 45% by mass, Martens hardness 33.0 N / mm 2 · Aqueous dispersible resin 8: Emulsion polymer of [First stage: MMA / CHMA / AA (mass ratio 26 / 23 / 1), Second stage: CHMA / EHA / AA (mass ratio 23 / 26 / 1)], solid content 45% by mass, Martens hardness 56.0 N / mm 2 · Aqueous dispersible resin 9: Emulsion polymer of [First stage: MMA / EHA / BA / AA (mass ratio 24 / 15 / 10 / 1), Second stage: MMA / BA / AA (mass ratio 42 / 7 / 1)], solid content 45% by mass, Martens hardness 43.0 N / mm 2 Water-dispersible resin 10: [1st stage: MMA / CHMA / AA / TN400 (mass ratio 18 / 14 / 1 / 1), 2nd stage: CHMA / EHA / KBM503 / TN400 (mass ratio 8 / 23 / 1 / 1, 3rd stage: emulsion polymer of MMA / CHMA / EHA / KBM503 / LA82 / TN400 (mass ratio 5 / 15 / 10 / 1 / 1 / 1), solid content 45% by mass, Martens hardness 28.0N / mm 2 Water-dispersible resin 11: [1st stage: MMA / CHMA / HEMA / AA / LA82 / TN400 (mass ratio 18 / 12 / 3 / 1 / 0.5 / 0.5), 2nd stage: CHMA / EHA / KBM503 / LA82 / TN400 (mass ratio 1 3 / 18 / 1 / 1 / 1), 3rd stage: CHMA / BMA / EHA / KBM503 / LA82 / TN400 (mass ratio 13 / 13 / 3 / 1 / 0.5 / 0.5)] emulsion polymer, solid content 45% by mass, Martens hardness 39.0N / mm 2 Water-dispersible resin 12: [1st stage: MMA / CHMA / HEMA / AA / RUVA-93 (mass ratio 25 / 21 / 2 / 1 / 1), 2nd stage: CHMA / EHA / HEMA / KBM503 (mass ratio 22 / 26 / 1 / 1)] emulsion polymer, solid content 45% by mass, Martens hardness 21.0N / mm 2 ·Water dispersible resin 13: [MMA / EHA / HEMA / AA / LA82 (mass ratio 78.5 / 14 / 3 / 1.5 / 1.5 / 3) solid content 45% by mass, Martens hardness 102.0N / mm 2 Water-dispersible resin 14: Emulsion polymer of [1st stage: MMA / ST / EHA / BA / AA (mass ratio 12 / 12 / 15 / 10 / 1), 2nd stage: MMA / ST / EHA / BA / AA (mass ratio 30 / 12 / 7 / 1)], solid content 45 mass%, Martens hardness 45.0 N / mm 2

[0258] The abbreviations for the monomers constituting the emulsion polymer have the following meanings. MMA: Methyl methacrylate, homopolymer Tg 105℃, SP value 9.53 CHMA: Cyclohexyl methacrylate, homopolymer Tg 66℃, SP value 9.48 BMA: n-Butyl methacrylate, homopolymer Tg 20℃, SP value 9.27 EHA: 2-Ethylhexyl acrylate, homopolymer Tg-50℃, SP value 9.2 BA: n-Butyl acrylate, homopolymer Tg-55℃, SP value 9.67 HEMA: 2-hydroxyethyl methacrylate, homopolymer Tg 55°C, SP value 11.87 ·KBM503: γ-methacryloyloxypropyltrimethoxysilane, homopolymer Tg 30℃ AA: Acrylic acid, homopolymer Tg 106℃, SP value 10.01 Radical Scavenger LA82: 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (ADEKA Corporation) RUVA-93: 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole (Otsuka Chemical Co., Ltd.) TN400: TINUVIN400, triazine-based UV absorber (BASF Ltd.)

[0259] Details of the materials used in making the building boards are given below. <Base material> Slate board (150mm x 70mm x 5mm, manufactured by TP Giken Co., Ltd.) <Sealer> Water-based Mighty Sealer Multi (cationic water-based paint, product name manufactured by Dai Nippon Toryo Co., Ltd.) <Undercoat paint> DNT Viewacrylic (water-based acrylic emulsion paint, product name manufactured by Dai Nippon Toryo Co., Ltd.) <Ink receiving layer coating 1> The raw materials and titania beads were mixed according to the formulation shown in Table 1, and then dispersed in a bead mill. After dispersion, the titania beads were removed to prepare coating material 1 for ink-receiving layer. The resin particle water dispersion 1 shown in Table 1 is a resin particle water dispersion 1 prepared according to <Preparation of resin particle water dispersion 1 (Synthesis Example 1)> described in paragraphs

[0074] to

[0076] of JP2019-217680A.

[0260] [Table 1]

[0261] Notes for Table 1 are as follows: 1) Titanium dioxide, density 3.8g / cm 3 (TITONE R-62N, Sakai Chemical Industry Co., Ltd.) 2) Ground calcium carbonate, density 2.7g / cm 3 , average particle size 2μm (Maruo Calcium) 3) SN Deformer 1316 (San Nopco) 4) ASE-60 (Rohm and Haas) 5) Proxel AM (Arch Chemicals) 6) TINUVIN 1130 (BASF) 7) Sanol LS-292 (manufactured by Sankyo Kasei Co., Ltd.)

[0262] <Active energy ray curable ink> Cyan ink, magenta ink, and yellow ink were prepared according to the formulations shown in Table 2 below (the amount of each component in the formulations shown in the table is shown in parts by mass). Specifically, all of the raw materials in Table 2 were mixed together, kneaded and dissolved in a bead mill for 5 hours, and then filtered through a glass fiber filter with a pore size of 1 μm to remove impurities.

[0263] [Table 2]

[0264] Details of the materials used in preparing the inks are given below. DAIPYROXIDE Blue #9410 [Blue pigment, CI Pigment Blue 28, product name manufactured by Dainichi Seika Color & Chemicals Co., Ltd.] BAYFERROX 130M [Magenta pigment, CI Pigment Red 101, LANXESS product name] TAROX Synthetic Iron Oxide HY-100 [Yellow pigment, CI Pigment Yellow 42, Titan Kogyo Co., Ltd. product name] TEGO-Dispers 685 [Pigment dispersant, product name manufactured by Evonic]

[0265] <Paint for forming surface protective layer> Topcoat paints were prepared as paints for forming surface protective layers according to the formulations shown in the following Tables 3 to 8. The amount of each component in the formulations shown in the tables is shown in parts by mass. Specifically, all the raw materials in Tables 3 to 8 were mixed and stirred with a high-speed disperser (Homodisper 2.5, manufactured by Primix Corporation), and then filtered through a 100-mesh metal screen to remove impurities. The raw materials used are as follows: TINUVIN 1130 [UV absorber, product name manufactured by BASF Japan Ltd.] TINUVIN 384 [UV absorber, product name manufactured by BASF Japan Ltd.] TINUVIN 400DW [UV absorber, product name manufactured by BASF Japan Ltd.] TINUVIN 477DW [UV absorber, product name manufactured by BASF Japan Ltd.] TINUVIN 479DW [UV absorber, product name manufactured by BASF Japan Ltd.] TINUVIN LS-292 [radical scavenger, product name manufactured by BASF Japan Ltd.] · TINUVIN 123DW [radical scavenger, product name manufactured by BASF Japan Ltd.] ·Diethylene glycol monobutyl ether (film-forming agent) Viscalex VG2 [Thickener, product name manufactured by Hoechst Chemical Co., Ltd.] BYK-028 [Antifoaming agent, product name manufactured by BYK] BYK-349 [Leveling agent, BYK product name] ACEMATT TS100 [Matte agent, product name manufactured by Evonik] Kanebinol KD12 [acrylic silicone resin, product name manufactured by Henkel Japan Ltd.] Lumiflon FE4300 [Fluoropolymer, product name manufactured by Asahi Glass Co., Ltd.] KBM403 [3-glycidoxypropyltrimethoxysilane, product name manufactured by Shin-Etsu Chemical Co., Ltd.] · KBE9007 [3-isocyanatepropyltriethoxysilane, product name manufactured by Shin-Etsu Chemical Co., Ltd.] EPOCROS WS500 [Oxazoline-containing resin, product name manufactured by Nippon Shokubai Co., Ltd.] Carbodilite E-02 [water-dispersible polycarbodiimide compound, product name manufactured by Nisshinbo Co., Ltd.]

[0266] <Photocatalytic coating agent> Photocatalytic coating agent A: Teika Co., Ltd. TKC-304 Photocatalytic coating agent B: PEARLEX Technologies Purecoat

[0267] <How to prepare test panels for coating film evaluation> An aluminum plate was used as the substrate, and the surface temperature of the substrate was adjusted to 50°C. The above-mentioned topcoat paint (paint for forming a surface protective layer) was then applied with an air spray at a rate of 100 g / m. 2 After coating to a thickness equivalent to a dry film thickness of 30 μm, the aluminum plate was dried at 120° C. for 15 minutes to form a coating film with a dry film thickness of 30 μm on the aluminum plate, forming a coating film for evaluation.

[0268] < Coating film evaluation method > For the coating film applied to the aluminum plate, a coating film was prepared that had been subjected to an accelerated weathering test using a sunshine carbon arc lamp for 60 hours and another for 180 hours, based on JISK7350-4:2008 (Plastics - Exposure test methods using laboratory light sources - Part 4: Open-flame carbon arc lamp). The coating film subjected to the accelerated weathering test for 60 hours was designated as coating film (A), and the coating film subjected to the accelerated weathering test for 180 hours was designated as coating film (B). Each coating (film thickness 30 μm) was cut to 3 cm × 3 cm to prepare a test piece (substrate with coating) for measuring the amount of chemiluminescence. The test piece for measurement was placed in the sample chamber of a weak luminescence detection device (Tohoku Electronics Industry Co., Ltd. CLA-FS4). Oxygen was flowed into the sample chamber at 50 ml / min to create an oxygen atmosphere, heating was started at each temperature (110 ° C, 130 ° C, 150 ° C), and the amount of chemiluminescence of the coating at each temperature 1200 seconds after the start of heating was measured with an exposure time of 10 seconds. The amount of chemiluminescence obtained is the integrated value for the exposure time of 10 seconds. The detection wavelength was 300 to 850 nm.

[0269] FIG. 2 is a graph in which the ordinate indicates the amount of chemiluminescence of the coating film after an exposure time of 10 seconds (count per 10 seconds) and the abscissa indicates the time (seconds) from the start of heating of the coating film that underwent an accelerated weather resistance test to measurement, and shows the measurement results of the amount of chemiluminescence of the coating film that underwent an accelerated weather resistance test for the topcoat paint (paint for forming a surface protective layer) of Example 11. In Figure 2, the chemiluminescence amounts (integrated values) of the coating films subjected to accelerated weathering tests with an exposure time of 10 seconds 1,200 seconds after the start of heating are shown, from the bottom, as follows: the value when the coating film subjected to 60 hours of accelerated weathering tests was heated at 110°C, the value when the coating film subjected to 180 hours of accelerated weathering tests was heated at 110°C, the value when the coating film subjected to 60 hours of accelerated weathering tests was heated at 130°C, the value when the coating film subjected to 180 hours of accelerated weathering tests was heated at 130°C, the value when the coating film subjected to 60 hours of accelerated weathering tests was heated at 150°C, and the value when the coating film subjected to 180 hours of accelerated weathering tests was heated at 150°C.

[0270] Calculation of apparent activation energy The difference between the amount of chemiluminescence of the coating film (B) and the amount of chemiluminescence of the coating film (A) at each measurement temperature was calculated, and a semi-logarithmic graph was created with the natural logarithm of the difference on the vertical axis and the reciprocal of the absolute temperature of each temperature on the horizontal axis. The apparent activation energy was calculated from the slope of the regression equation created from the points plotted on the graph. The above regression equation can be set based on the Arrhenius law, which makes it possible to predict the rate of chemical reactions at a specified temperature.

[0271] Figure 3 is a semi-logarithmic graph with the natural logarithm of the difference between the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 180 hours and the amount of chemiluminescence of a coating film subjected to an accelerated weathering test for 60 hours on the ordinate and the reciprocal of the absolute temperature of the heating temperature of the coating film subjected to the accelerated weathering test on the abscissa, and shows a graph created based on the measurement results of the amount of chemiluminescence for the topcoat paint (paint for forming a surface protective layer) of Example 11, and a regression equation created from the graph. The graph shown in Figure 3 is an Arrhenius plot, and the apparent activation energy (53 kJ / mol) can be obtained from the slope of the regression equation (-6382.6) based on the Arrhenius law.

[0272] <Making of building boards> 1. Preparation of Sealer Plate Apply 100g / m of water-based Mighty Sealer Multi to the base material. 2 The paint was applied with an air spray so that the surface was coated with the desired color, and the paint was dried at room temperature for 2 hours to prepare a sealer plate. 2. Preparation of the primed substrate The sealer plate prepared in the above step 1 was heated to 60°C, and the above-mentioned ink-receiving layer coating material 1 was applied by air spray in an amount of 130 g / m 2 After coating so that the thickness of the dried film was approximately 30 μm, it was dried at 100°C for 3 minutes to prepare an ink-receiving layer substrate for ink decoration as an undercoat substrate. 3. Preparation of substrate with colored layer Substrates with colored layers were prepared by carrying out the same procedure as in "2. Preparation of primed substrate", except that each color of DNT View Acrylic was applied under the same conditions instead of the paint for the ink-receiving layer. For the examples in which "water-based paint" is entered in the "design layer" column in Tables 3 to 8, this substrate with a colored layer was produced. 4. Preparation of substrate with ink layer The ink receiving layer substrate prepared in 2 above was adjusted to a substrate temperature of 50 to 60°C, and the above-mentioned active energy ray curable inks (cyan ink, magenta ink, and yellow ink) were used to form gradation patterns of each color (solid images in which the recording density was recorded in 20% increments from 10% to 100%) using an inkjet printer [EB100 (control device), XY100 (transport stage), both manufactured by Konica Minolta IJ Co., Ltd.]. The ink receiving layer substrate was then printed using a metal halide lamp with a peak illuminance of 300 mW / cm. 2 Accumulated light intensity of 200mJ / cm 2 The ink was cured by irradiation with ultraviolet light of 1000 ohms to prepare a substrate with an ink layer. For the examples in which "UV ink" is entered in the "design layer" column in Tables 3 to 8, a substrate with this ink layer was produced. 5.Surface protection layer With the surface temperature of the substrate on which the ink layer and colored layer were formed adjusted to 50°C, the above-mentioned topcoat paint (paint for forming the surface protective layer) was applied with an air spray at a coating amount of 100 g / m 2 After coating on the ink layer and colored layer so as to have a dry film thickness of 30 μm, the coating was dried at 120° C. for 15 minutes to form a surface protective layer. 6.Photocatalyst layer With the surface temperature of the substrate adjusted to 60°C, a photocatalytic coating agent was applied to the surface protection layer formed in step 5 above using an air spray at a rate of 20 g / m. 2 After coating to a thickness equivalent to 400 nm on a dry basis, the coating was dried at 60°C for 3 minutes to form a photocatalyst layer. In the examples marked with "A" in the "Photocatalytic coating agent" column of Tables 3 to 8, the photocatalytic layer was formed using photocatalytic coating agent A, and in the examples marked with "B", the photocatalytic layer was formed using photocatalytic coating agent B. In these examples, the photocatalytic layer exists on the outermost surface layer. No photocatalyst layer was formed for the examples marked with "-" in the "Photocatalyst coating agent" column in Tables 3 to 8. In these examples, the outermost layer was a surface protection layer.

[0273] A building board was prepared according to the description in <Preparation of Building Board> above. * The substrate temperature described in 1. to 6. of <Preparation of building board> was measured using an infrared radiation non-contact thermometer (ISK-8700II, AS ONE Corporation).

[0274] <Martens hardness of coated body> After the building boards prepared above were cured at room temperature for one week, the Martens hardness of the coating film formed on the building board was measured using a microhardness tester (Shimadzu microhardness tester DUH-211) with a 115° triangular pyramid indenter under the following conditions: temperature 20°C, relative humidity 50%, test force 5mN, load speed 1mN / sec, and load and unload hold time 5sec. The Martens hardness (HMs) was calculated from the slope of the test force vs. indentation depth curve and evaluated based on the following criteria. The results are shown in Tables 3 to 8. In addition, when the coating film contains aggregate components such as matte beads, color beads, mica, etc., the measurement shall be made on the part excluding these. (Evaluation Criteria) ○: Martens hardness is 10 to 200 N / mm 2 △: Martens hardness is 10N / mm 2 Less than or equal to 200N / mm 2 Greater than.

[0275] <Water resistance (compliant with JIS K 5600-6-2:1999)> The prepared building board was immersed in a thermostatic water tank maintained at 40°C, and after 240 hours, it was taken out and dried. Thereafter, the appearance such as blistering and whitening was observed, and the adhesion was evaluated. The results are shown in Tables 3 to 8. The evaluation criteria are as follows. ⊚: No abnormal appearance such as swelling or whitening, and adhesion is classified as 0. ◯: No abnormal appearance such as blistering or whitening, and adhesion is in category 1 or 2. △: No abnormal appearance such as blistering or whitening, and adhesion is in the category of 3 to 5. ×: Abnormal appearance such as swelling or whitening is observed. The classifications 0 to 5 described in 8.3 of JIS K 5600-5-6:1999 are as follows: Category 0: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. Class 1: Remaining rate of laminated coating is 95-99%. Class 2: Remaining rate of laminated coating is 85% or more but less than 95%. Category 3: Remaining rate of laminated coating is between 65% and 85%. Category 4: Remaining rate of laminated coating is between 0% and 65%. Category 5: Any degree of peeling that cannot be classified as Category 4.

[0276] <Accelerated Weathering 1 (Sunshine)> Based on JISK7350-4:2008 (Plastics - Exposure test methods using laboratory light sources - Part 4: Open-flame carbon arc lamp), the architectural boards were subjected to accelerated weathering tests using sunshine carbon arc lamps for 7500 hours, and then the color difference, gloss retention and coating appearance were evaluated by comparing with the initial boards using the following methods. The results are shown in Tables 3 to 8. ⊚: The coating film is free of defects such as cracks, the gloss retention is 90% or more, and the color difference is ΔE<1.0. ◯: The coating film is free of defects such as cracks, the gloss retention is 80% or more, and the color difference is ΔE<2.0. △: The coating film has no defects such as cracks, the gloss retention is 70% or more, and the color difference is ΔE<3.0. ×: Cracks are generated in the coating film, and the gloss retention is less than 70%, or the color difference is ΔE>3.0.

[0277] <Accelerated weather resistance 2 (Super UV test)> The building boards were subjected to a test using an Iwasaki Electric Eye Super UV Tester for 1000 hours, after which the color difference, gloss retention and coating appearance were evaluated in comparison with the initial boards using the following methods. ⊚: The coating film is free of defects such as cracks, the gloss retention is 90% or more, and the color difference is ΔE<1.0. The results are shown in Tables 3 to 8. ◯: There is no significant change in appearance, the gloss retention is 80% or more, and the color difference is ΔE<2.0. △: There is no significant change in appearance, the gloss retention is 70% or more, and the color difference is ΔE<3.0. ×: Cracks are generated in the coating film, and the gloss retention is less than 70%, or the color difference is ΔE>3.0.

[0278] The gloss retention and color difference used in the accelerated weather resistance evaluation can be calculated by the following formulas. Gloss retention (%) = (60° gloss value after test) / (60° gloss value of initial plate) x 100 Color difference (ΔE)=((ΔL) 2 +(Δa) 2 +(Δb) 2 ) 1 / 2 (ΔL = L value after test - L value of initial plate) (Δa = a value after test - a value of initial plate) (Δb = b value after test - b value of initial plate) The gloss value was measured using BYK's micro-TRI-gloss, and the color measurement value was measured using Konica Minolta's CR-400.

[0279] Regarding weather resistance, accelerated weather resistance 1 (Sunshine test) and accelerated weather resistance 2 (Super UV test) were evaluated, and if the evaluation results were ◎, ○, or △, the coating composition is capable of forming a surface protective layer that can achieve a high level of weather resistance. Such a coating composition can form a surface protective layer that can protect the design for a long period of time even when the design layer is an active energy ray-curable ink or when a photocatalyst layer is present on the outermost layer.

[0280] <Blocking resistance> The painted surface of the building board was left at 40°C for 24 hours at 1t / m 2 A load of 10 ... 〇: No cracks in the coating, no visible pressure marks △: There are no cracks in the coating, but pressure marks are visible ×: The coating film cracks

[0281] [Table 3]

[0282] [Table 4]

[0283] [Table 5]

[0284] [Table 6]

[0285] [Table 7]

[0286] [Table 8]

[0287] In the table, "Amount of UV absorber in resin" and "Amount of UV absorber other than resin" both indicate the amount (mass%) of UV absorber in the paint composition, and the "UV absorber" in "Amount of UV absorber in resin" refers to an UV absorber contained as a component of the water-dispersible resin, while the "UV absorber" in "Amount of UV absorber other than resin" refers to an UV absorber that is dispersed or dissolved in the paint composition, rather than as a component of the water-dispersible resin. Similarly, "amount of radical scavenger in resin" and "amount of radical scavenger other than resin" both indicate the amount (mass%) of radical scavenger in the paint composition, and the "radical scavenger" in "amount of radical scavenger in resin" refers to a radical scavenger contained as a component of the water-dispersible resin, while the "radical scavenger" in "amount of radical scavenger other than resin" refers to a radical scavenger that is dispersed or dissolved in the paint composition, rather than as a component of the water-dispersible resin.

Claims

1. Regarding the coating film obtained by forming a coating composition for forming a surface protective layer on an aluminum plate, a coating film (A) that was subjected to an accelerated weather resistance test using a sunshine carbon arc lamp based on JIS K7350-4 for 60 hours and a coating film (B) that was subjected to the test for 180 hours were prepared. Heating of the coating film (A) and the coating film (B) in an oxygen atmosphere at 110°C, 130°C, and 150°C was started, and the amount of chemiluminescence of the coating film (A) and the coating film (B) at each heating temperature 1200 seconds after the start of heating were measured under the following conditions, and the difference in the amount of chemiluminescence between the coating film (B) and the coating film (A) at each heating temperature was determined. A semi-logarithmic graph was created with the natural logarithmic value of the difference on the ordinate and the reciprocal of the absolute temperature of each heating temperature on the abscissa, and a coating composition for forming a surface protective layer having an apparent activation energy of 35 kJ / mol or more, as determined from the slope of a regression equation prepared from the semi-logarithmic graph based on the Arrhenius law. <Conditions for measuring chemiluminescence intensity> Test piece size: 3cm x 3cm Dry film thickness: 30μm Oxygen flow rate: 50 ml / min Exposure time: 10 seconds Detection wavelength: 300 to 850 nm

2. A coated body having at least a substrate and a surface protective layer, characterized in that the surface protective layer comprises a coating film formed by the coating composition for forming a surface protective layer according to claim 1.

3. A coated body having at least a substrate, a surface protective layer, and a photocatalyst layer formed on the surface protective layer, characterized in that the surface protective layer comprises a coating film formed by the coating composition for forming a surface protective layer according to claim 1.

Citation Information

Patent Citations

  • Monitor circuit for semiconductor laser

    JP1986088625A

  • Building decorative board, water-based clear coating used for manufacturing the same, and coating for forming water-based printing object surface

    JP2011093306A

  • Manufacturing method for building board

    JP2016055249A

  • Printed matter

    JP2019217680A

  • Multiple layer coating and manufacturing method for same

    WO2012133667A1

Cited By

  • Method for manufacturing high-elasticity acrylic syrup and acrylic syrup composition thereof

    KR102918219B1