Inorganic binder and inorganic fiber composition
An inorganic binder with alkaline substances, water, SiO2, and carbon dioxide suppresses needle-like crystal formation in inorganic fiber compositions, enhancing process stability and reducing carbon emissions.
Patent Information
- Application Number
- JP2023059460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing inorganic binders used in inorganic fiber compositions, such as those containing cement, result in the formation of needle-like crystals during the curing process, which is visually observable and undesirable.
An inorganic binder comprising alkaline substances, water, and SiO2 with a specific amount of carbon dioxide relative to the volume of water, along with an inorganic powder, is used to suppress the formation of needle-like crystals.
The proposed binder effectively prevents the precipitation of needle-like crystals during the curing process, while reducing carbon dioxide emissions by avoiding the use of cement as a main component.
Smart Images

Figure 2024146510000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an inorganic binder. More specifically, the present invention relates to an inorganic binder capable of suppressing the formation of needle-like crystals during the curing process of an inorganic fiber composition formed with inorganic fibers. The present invention also relates to an inorganic fiber composition. More specifically, the present invention relates to an inorganic fiber composition formed with inorganic fibers and an inorganic binder capable of suppressing the formation of needle-like crystals during the curing process. [Background technology]
[0002] In order to impart fire resistance, fire prevention, sound absorption, or heat insulation to structural members, spray materials such as rock wool spray material, which is made of fibers such as rock wool and a binder such as cement paste, are sprayed. Rock wool spray material, which is a representative spray material, is made of rock wool, cement, and water, and is widely used because of its excellent fire resistance, workability, and the like (see, for example, Patent Document 1). Cement is an inexpensive and excellent inorganic binder, but since it is produced by decomposing the raw material limestone at high temperature and reacting it with silicon dioxide raw material, aluminum oxide raw material, iron oxide raw material, and the like at high temperature, it generates a large amount of carbon dioxide, which is a representative greenhouse gas, during production. For this reason, a spray material (inorganic fiber composition) using an inorganic binder that does not contain cement as a main component, and an inorganic binder for this purpose are desired.
[0003] It has been disclosed that phosphosilicates, alkali silicates (e.g., water glass), geopolymers, colloidal silica, or colloidal alumina can be used as binders for rock wool fibers of a specific composition (see, for example, Patent Document 2).
[0004] Incidentally, there is a technique for spraying a binder together with pressurized air when spraying the binder onto fibers and joining them to form a sprayed material layer (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-348978 A [Patent Document 2] Special Publication No. 2012-532830 [Patent Document 3] Jpn. Jpn. Published No. 55-054755 Summary of the Invention [Problem to be solved by the invention]
[0006] As a result of various investigations into forming an inorganic fiber composition layer (spraying material layer, coating material layer) made of a rock wool composition by spraying an inorganic binder containing an alkali silicate as an inorganic binder other than cement and an SiO2-containing inorganic powder other than cement and an alkali silicate together with rock wool, it was found that needle-shaped crystals made of an alkali carbonate hydrate may be precipitated on the surface of the inorganic fiber composition layer in the process of curing the inorganic fiber composition layer to a degree that can be confirmed by the naked eye. The present invention aims to provide a technology capable of suppressing the precipitation of needle-shaped crystals occurring during the curing process, that is, an inorganic binder and an inorganic fiber composition capable of suppressing the precipitation of needle-shaped crystals occurring during the curing process. [Means for solving the problem]
[0007] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by containing an alkaline substance, water, and an SiO2-containing inorganic powder, and by containing a specific amount of carbon dioxide relative to the volume of the water contained therein, and have completed the present invention. That is, the present invention is an inorganic binder represented by the following (1) or (2), and an inorganic fiber composition represented by the following (3) or (4). (1) An inorganic binder containing an alkaline substance, water, and SiO2-containing inorganic powder, and containing 0.2 gas volumes (GV) or more of carbon dioxide per volume of water contained. (2) The inorganic binder of (1) above, wherein the alkaline substance is one or more selected from alkali silicates, alkali hydroxides and alkali oxides, and the SiO2-containing inorganic powder is an SiO2-containing inorganic powder other than cement and alkali silicates. (3) An inorganic fiber composition comprising the inorganic binder of (1) or (2) above and inorganic fibers as main components. (4) The inorganic fiber composition according to (3), wherein the inorganic fiber is rock wool. Effect of the Invention
[0008] According to the present invention, an inorganic binder containing an alkaline substance, for example, an inorganic fiber composition layer (spraying material layer, coating material layer) mainly composed of an inorganic binder containing an alkali silicate and not mainly composed of cement and inorganic fibers, is obtained which can suppress the formation and precipitation of needle-like crystals on the surface of the inorganic fiber composition layer to a degree that can be confirmed with the naked eye during the curing process of the inorganic fiber composition layer.
[0009] According to the present invention, an inorganic fiber composition is obtained that is primarily composed of inorganic fibers and an alkali-containing inorganic binder that can suppress the formation and precipitation of needle-like crystals to a degree that can be visually confirmed on the surface of an inorganic fiber composition layer (spraying material layer, coating material layer) during the curing process. In addition, since the binder and inorganic fibers used in the present invention do not contain cement as a main component, the amount of carbon dioxide emitted during the production of the raw materials can be reduced compared to the case where cement is used as a raw material for the binder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The inorganic binder of the present invention contains an alkaline substance, water, and SiO2-containing inorganic powder, and is characterized by containing 0.2 gas volumes (GV) or more of carbon dioxide relative to the volume of the water contained. In other words, the inorganic binder of the present invention contains 0.2 gas volumes (GV) or more of carbon dioxide (carbonic acid gas) in the water contained therein. Here, the gas volume (GV) refers to the volume ratio of the carbon dioxide (carbonic acid gas) dissolved in the water contained in the inorganic binder of the present invention at 1 atmosphere and 20°C to the volume of the water (the ratio of the volume of the carbonic acid gas to the volume (volume) of the water).
[0011] The alkaline substance in the present invention is preferably one or more selected from silicates, hydroxides and oxides of alkali metals, that is, one or more selected from alkali silicates, alkali hydroxides and alkali oxides, and preferably one or more selected from sodium silicate, potassium silicate, sodium hydroxide, potassium hydroxide, sodium oxide and potassium oxide. The alkaline substance in the present invention may be in the form of a powder or granule, but in the case of alkali silicates or alkali hydroxides, an aqueous solution may be used. Commercially available water glass may be used as the aqueous solution of sodium silicate.
[0012] The content of the alkaline substance in the inorganic binder of the present invention is preferably 1 to 70 mass % of the solid content in the inorganic binder in terms of solid content. If it is less than 1 mass %, the strength, especially the initial strength, of the inorganic fiber composition is insufficient (small), and if it exceeds 70 mass %, the strength of the inorganic fiber composition is also insufficient (small).
[0013] The SiO2-containing inorganic powder in the present invention includes cements whose main component is calcium silicate, such as Portland cement and ecocement, alkali silicate, blast furnace slag powder, copper slag powder, ferro-nickel slag powder, and other slag powders used in metal refining, powder of sewage sludge slag burned product, powder of molten slag from urban waste, fly ash, pulp sludge incineration ash, biomass boiler incineration ash, sewage sludge incineration ash, rice husk ash, silica fume, crushed waste glass, crushed waste ceramics, tile ceramics, and other powders from various industries. Preferred examples of the main by-product chemical compositions include inorganic powders containing SiO2, powders of clay minerals such as silica powder, diatomaceous earth powder, talc powder, kaolin, bentonite, etc., powders of minerals containing SiO2 (SiO2-containing minerals) such as volcanic ash and igneous rock powder, powders of fired igneous rocks and powders of fired SiO2-containing minerals such as metakaolin, powders of inorganic industrial products containing SiO2 (SiO2-containing industrial products) such as colloidal silica, synthetic silica glass, white carbon, silica gel, and precipitated silica. Since no carbon dioxide (carbon dioxide gas) is generated from the raw materials during production, the SiO2-containing inorganic powder in the present invention is preferably an inorganic powder containing SiO2 other than cement, which is mainly composed of calcium silicate, that is, inorganic powders containing SiO2 as the main chemical composition and by-produced from various industries, such as alkali silicate, slag powder in metal refining such as blast furnace slag powder, fly ash and silica fume, powders of igneous rock burnt products and powders of SiO2-containing minerals such as metakaolin, powders of SiO2-containing minerals such as volcanic ash and igneous rock powder, and powders of SiO2-containing industrial products such as colloidal silica and white carbon. Examples of the SiO2-containing inorganic powder include those having a Blaine specific surface area of 2000 cm 2 / g or more is preferable because the binder hardens quickly, and more preferably 2500 cm 2 / g or higher.
[0014] The content of the SiO2-containing inorganic powder in the inorganic binder of the present invention is preferably 30 to 99 mass% of the solid content in the inorganic binder in terms of solid content. If it is less than 30 mass%, the strength when made into an inorganic fiber composition is insufficient (small), and even if it exceeds 99 mass%, the strength, especially the initial strength, when made into an inorganic fiber composition is insufficient (small).
[0015] As described above, since the alkali silicate is also an alkaline substance in the present invention, when the alkali silicate is contained, it is preferable to contain other SiO2-containing inorganic powders (SiO2-containing inorganic powders other than alkali silicates), particularly "SiO2-containing inorganic powders other than cement and alkali silicates". As the alkali silicate, it is preferable to use one or more selected from sodium silicate or sodium silicate aqueous solution such as sodium metasilicate, sodium orthosilicate, water glass, lithium silicate or lithium silicate aqueous solution, potassium silicate or potassium silicate aqueous solution. Furthermore, as the alkali silicate used in the present invention, it is more preferable to use one or more selected from sodium silicate or sodium silicate aqueous solution such as sodium metasilicate, sodium orthosilicate, water glass, etc., because they are easily available and the reactivity of the binder is high.
[0016] In the inorganic binder of the present invention, if the alkaline substance is one or more selected from alkali silicate, alkali hydroxide, and alkali oxide, and the SiO2-containing inorganic powder is mainly composed of "SiO2-containing inorganic powder other than cement and alkali silicate", the amount of carbon dioxide (carbon dioxide gas) generated from the raw material during the production of the SiO2-containing inorganic powder is small, and the amount of carbon dioxide (carbon dioxide gas) generated including the production of the raw material can be suppressed, which is preferable. Here, "SiO2-containing inorganic powder other than cement and alkali silicate" as the main component means that it does not contain alkali silicate and the content of cement in the SiO2-containing inorganic powder is 10% by mass or less, and it is more preferable that the content of cement in the SiO2-containing inorganic powder is 5% by mass or less.
[0017] In the present invention, since the carbon dioxide is contained in an amount of 0.2 gas volumes (GV) or more relative to the volume of the water contained, it is believed that the contained alkaline substance is quickly converted to carbonate or carbonate hydrate, making it difficult for carbonate hydrate crystals to grow. If the carbon dioxide content is less than 0.2 gas volumes (GV) relative to the volume of the water contained, there will be many alkaline ions that are not bonded to carbonate ions, and these will react with carbon dioxide gas in the air and the water molecules in the inorganic binder of the present invention, causing the growth of alkali carbonate hydrate crystals, which will precipitate to an extent that can be confirmed by the naked eye.
[0018] In order to obtain the inorganic binder of the present invention, carbon dioxide (carbonic acid gas) can be blown into the inorganic binder or the water or aqueous solution of the raw material of the inorganic binder to contain 0.2 gas volumes (GV) or more of carbon dioxide relative to the volume of water contained. In addition, the inorganic binder of the present invention can be manufactured using carbonated water containing 0.2 gas volumes (GV) or more of carbon dioxide (carbonic acid gas). The content of carbon dioxide relative to the volume of water contained in the inorganic binder of the present invention is preferably 10 gas volumes (GV) or less, more preferably 6 gas volumes (GV) or less, and even more preferably 5 gas volumes (GV) or less. If the carbon dioxide content is high, the mixer, hoses, containers, etc. used in the production must be stronger, which makes them heavy and expensive. In addition, when using carbonated water, it is easy to obtain if it is 6 gas volumes (GV) or less, and it is even easier to obtain and preferable if it is 5 gas volumes (GV) or less.
[0019] The inorganic binder of the present invention preferably has a water content of 20 to 96 mass%, more preferably 23 to 95 mass%. Here, the water content (C W ) is the mass of water contained in the inorganic binder of the present invention (M W ) to the mass of inorganic binder (M B ) is expressed as a percentage, and the mass of water contained in the inorganic binder (M W) does not need to be taken into consideration when the influence of moisture in the air is so small that it can be ignored, such as the mass of water contained in SiO2-containing inorganic powder. C W (%)=M W ÷M B ×100 (1) In the present invention, if the water content is less than 20 mass%, there is a risk of poor mixing with the inorganic fibers when forming the inorganic fiber composition, and if it exceeds 96 mass%, the inorganic fiber composition formed will lack strength and will be prone to crumbling.
[0020] The inorganic binder of the present invention is preferably used as a binder for inorganic fiber compositions, and more preferably used as a binder for rock wool compositions. Suitable examples of inorganic fibers include rock wool (including slag wool), glass wool, and ceramic wool. Cotton-like fibers made of these fibers are more preferred, and granular fibers in granular form are even more preferred. Examples of such granular fibers include rock wool granular cotton, which is particularly preferred.
[0021] The inorganic binder of the present invention may contain one or more other components in addition to the alkaline substance, water, and SiO2-containing inorganic powder, as long as the effects of the present invention are not impaired. Examples of the other components include chemical additives such as viscosity adjusters, reaction accelerators, and reaction inhibitors, extenders such as fillers and aggregates, and organic fibers such as polypropylene fibers. Examples of the chemical additives include admixtures for cement, mortar, or concrete other than those mentioned above.
[0022] The inorganic fiber composition of the present invention is characterized by comprising the above-mentioned inorganic binder and inorganic fibers as main components. The inorganic fibers are the same as those described above, and suitable examples thereof include rock wool (including slag wool), glass wool, and ceramic wool. Cotton-like fibers made of these fibers are more preferable, and granular fibers made of granules are even more preferable.
[0023] The inorganic fiber composition of the present invention may contain one or more other components in addition to the above-mentioned inorganic binder and inorganic fibers, as long as the effects of the present invention are not impaired. Examples of the other components include chemical additives such as viscosity adjusters, reaction accelerators, and reaction inhibitors, extenders such as fillers and aggregates, and organic fibers such as polypropylene fibers. Examples of the chemical additives include admixtures for cement, mortar, or concrete other than inorganic fibers.
[0024] In the present invention, the inorganic binder solid content is preferably 5 to 80 parts by mass relative to 100 parts by mass of the total of the inorganic binder solid content and the inorganic fiber solid content. If it is less than 5 parts by mass, the strength of the formed inorganic fiber composition may be low and it may crumble. If it exceeds 80 parts by mass, the density of the inorganic fiber composition may be high, and the performance required for the inorganic fiber composition, such as fire resistance, fire prevention, heat insulation, sound absorption, and sound insulation, may be low.
[0025] In the present invention, the amount of moisture in the inorganic binder is preferably 25 to 300 parts by mass per 100 parts by mass of the inorganic fibers contained. If the amount is less than 25 parts by mass, the strength of the formed inorganic fiber composition may be low and it may crumble, and the formed inorganic fiber composition may peel off when it is applied to a ceiling, wall, etc. If the amount is more than 300 parts by mass, the formed inorganic fiber composition may peel off when it is applied to a ceiling, wall, etc., and moisture may seep out from the inorganic fiber composition.
[0026] The inorganic fiber composition of the present invention may be produced by mixing the inorganic binder and inorganic fibers, or by mixing the components of the inorganic binder and inorganic fibers together. The mixing here includes confluence mixing. That is, for example, similar to the semi-dry method in the rock wool spraying method, the inorganic fibers (e.g., rock wool granular cotton) pressurized in the pressure hose are discharged from the outlet of the spray nozzle connected to the pressure hose, and the inorganic binder is sprayed onto the inorganic fibers to confluence mix, thereby producing the inorganic fiber composition of the present invention. The inorganic fiber composition of the present invention can also be produced by confluence mixing the inorganic binder and inorganic fibers in a pressure hose or pipe. The inorganic fiber composition of the present invention can also be produced by mixing the inorganic binder and inorganic fibers or each material with a mixer.
[0027] The produced inorganic fiber composition of the present invention is applied to a desired location or in a desired form by spraying, coating, filling, driving, plastering, spreading and then rolling, filling in a breathable container, etc. By covering the surfaces of members such as pillars, beams, floors, ceilings, and walls with the inorganic fiber composition of the present invention or filling the interior of a member, or by forming a member from the inorganic fiber composition of the present invention, the performance of the member, such as fire resistance, fire prevention, sound absorption (soundproofing), or heat insulation, can be improved. EXAMPLES
[0028] [Example 1] An inorganic binder was prepared using alkali silicate, "SiO2-containing inorganic powder other than cement and alkali silicate," and water in the mixing ratio shown in Table 1. The materials used are shown below. Table 1 also shows the method of incorporating carbon dioxide (carbonic acid gas) and the carbon dioxide (carbonic acid gas) content relative to the volume of water included. <Materials used> (1) Alkaline silicate: No. 3 water glass (solid content: 39.2% by mass, SiO2: 29.4% by mass, Na2O: 9.7% by mass, H2O: 60.8% by mass), symbol: WG3 (2) SiO2-containing inorganic powder other than cement and alkali silicate: Blast furnace slag powder (ground blast furnace slag powder 4000, Blaine specific surface area: 4130 cm 2 / g), symbol;BSF (3) Water 1: Commercially available carbonated water, symbol: W1 (4) Water 2: Water supply in Sakura City, Chiba Prefecture, symbol; W2
[0029] [Table 1]
[0030] The prepared inorganic binder and rock wool granular cotton (inorganic fiber) were sprayed on the inside of a container (inner dimensions 20 (cm) × 20 (cm) × 5 (cm)) by the same spraying method as the semi-dry method in the rock wool spraying method to prepare a rock wool composition (inorganic fiber composition). At this time, the amount of rock wool granular cotton was adjusted to 600 parts by mass per 100 parts by mass of blast furnace slag powder. The prepared rock wool composition was aged for one month in a constant temperature room at room temperature of 20 ° C and relative humidity of 60%. Thereafter, the surface of the rock wool composition was visually observed to confirm the presence or absence of precipitation of needle-shaped crystals. When no needle-shaped crystals were precipitated, it was evaluated as "good" (symbol: ○), and when needle-shaped crystals were precipitated, it was evaluated as "poor" (symbol: ×). The results are shown in Table 1 together with the mixing ratio of the inorganic binder.
[0031] In the inorganic binders of Mixture No. 2 to Mixture No. 6 and the rock wool compositions (inorganic fiber compositions) prepared using these inorganic binders, precipitation of needle-like crystals was not observed in the Examples. On the other hand, in the inorganic binders of Mixture No. 1 and Mixture No. 7, which have low carbon dioxide gas contents, and the rock wool compositions (inorganic fiber compositions) prepared using these inorganic binders, precipitation of needle-like crystals was observed in the Comparative Examples. [Industrial Applicability]
[0032] The present invention can be suitably used in inorganic fiber compositions that impart, for example, fire resistance, fire prevention, sound absorption (soundproofing), heat insulation, or the like, and can be suitably used in civil engineering structures, architectural structures, constructions, and articles that require performance such as fire resistance, fire prevention, sound absorption (soundproofing), or heat insulation.
Claims
1. Alkaline substance, water and SiO 2 An inorganic binder containing an inorganic powder and containing 0.2 gas volumes (GV) or more of carbon dioxide relative to the volume of the water contained therein.
2. The alkaline substance is one or more selected from an alkali silicate, an alkali hydroxide, and an alkali oxide, and the SiO 2 The inorganic powder contained is SiO other than cement and alkali silicate. 2 2. The inorganic binder of claim 1 which is a containing inorganic powder.
3. 3. An inorganic fiber composition comprising as main components the inorganic binder according to claim 1 or 2 and inorganic fibers.
4. 4. The inorganic fiber composition according to claim 3, wherein said inorganic fiber is rock wool.
Citation Information
Patent Citations
JP1980054755U
Rock wool spraying construction method and spraying device
JP2002348978A
Mineral fibers and their use
JP2012532830A