Unshaped refractory spraying construction method
The described method addresses the issues of uniformity and score line formation in refractory layer construction by using anchors and controlled spraying techniques, resulting in a stable and uniformly thick refractory layer with ease of application.
Patent Information
- Application Number
- JP2023059646
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional spraying construction methods for refractory layers in furnaces face challenges in achieving uniform thickness and forming score lines without relying on worker skill, and often result in uneven surfaces.
A method involving the use of anchors, nuts, and battledore bolts to secure a plate-shaped body, followed by controlled spraying of monolithic refractory material, ensuring uniform thickness and score line formation.
Enables the formation of a refractory layer with uniform thickness and depth, facilitating easy score line creation, and enhances stability and ease of application, independent of worker skill.
Smart Images

Figure 2024146625000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a spraying method for forming a refractory layer (refractory wall) by spraying a moldable refractory onto a target surface such as the inner or outer peripheral surface of the steel shell of a furnace such as a combustion furnace. [Background technology]
[0002] As a construction method for forming a refractory layer (refractory wall) of an iron-making furnace, a steel-making furnace, a non-ferrous metal industrial furnace, an oil industrial furnace, a combustion furnace, etc., a spraying construction method is known in which an unshaped refractory is sprayed onto the construction target surface, such as the inner or outer peripheral surface of the steel shell that covers the furnace. The spraying construction method has the advantage that construction can be performed in a short time and no joints are formed, compared to a construction method in which shaped refractories such as firebricks are assembled. In addition, the spraying construction method has the advantage that the work is easier and can be performed with a small amount of water, compared to a pouring construction in which an unshaped refractory is poured into a mold that has been assembled in advance, and therefore a refractory layer with high strength can be formed.
[0003] On the other hand, the spraying method makes it difficult to obtain a uniform thickness for the refractory layer, and the surface of the refractory layer is prone to unevenness, so that it may be necessary to trim the surface with a tool such as a scraper to make it uniform in thickness. Therefore, the thickness and smoothness of the refractory layer may vary depending on the skill of the worker. In addition, in the case of a refractory layer formed from an amorphous refractory, a lattice-shaped long groove (so-called score line) must generally be formed on the surface of the refractory layer using a blade such as an electric cutter in order to absorb (alleviate) the stress associated with thermal expansion and thermal contraction, so that the conventional spraying method is not necessarily simple.
[0004] In order to eliminate the drawbacks of such spraying construction methods, the applicants have proposed a construction method for making the thickness of a refractory layer made of amorphous refractory uniform and easily forming score lines on the surface of the refractory layer, in which a construction tool having a component that will burn when the furnace is in use fixed to the top of an anchor is fixed to the inner or outer surface of the steel shell, and then the amorphous refractory is sprayed (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-145506 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, although the spraying method as disclosed in Patent Document 1 is easier to make the thickness of the refractory layer uniform and easier to form score lines on the surface of the refractory layer than the conventional spraying methods, its effects are still not sufficient.The object of the present invention is to provide a spraying method which eliminates the problems of the conventional spraying methods, is inexpensive, and can easily form a refractory layer of uniform thickness without depending on the skill of the worker, and can easily form score lines of uniform width and depth on the surface of the refractory layer. [Means for solving the problem]
[0007] The invention described in claim 1 of the present invention is a spraying construction method for spraying a shaped refractory material onto the inner or outer peripheral surface of a steel shell covering a furnace to form a wall body made of a refractory material, the method comprising an anchor erecting step of erecting a plurality of anchors in a predetermined regular arrangement on the inner peripheral surface of the steel shell covering the furnace, a nut fixing step of fixing a cylindrical nut having a female thread on its inner peripheral surface to the inner peripheral surface of the steel shell so as to be located between two adjacent anchors erected on the inner peripheral surface of the steel shell, a bolt screwing step of screwing a shuttlecock bolt into the nut fixed to the inner peripheral surface of the steel shell, and a bolt screwed into the nut. The method is characterized by comprising a plate fixing process for fixing a wide rectangular plate to the shuttlecock bolt so that its longitudinal direction is perpendicular to the axial direction of the bolt; a plywood box forming process for forming a blocking portion made of plywood by erecting a number of plywood panels on the inner surface of the steel shell so as to sandwich the plate so as to cover the sides of the two adjacent anchors and the nut located between them; an outside box spraying process for spraying amorphous refractory material on the outside of the blocking portion; and an inside box spraying process for spraying amorphous refractory material on the inside of the blocking portion.
[0008] In addition, as the amorphous refractory to be sprayed in the spray application method of the present invention, refractory materials such as alumina, spinel, alumina-silica, alumina-spinel, and alumina-magnesia can be suitably used.
[0009] The invention recited in claim 2 is the invention recited in claim 1, characterized in that the anchor installation step comprises arranging Y-shaped anchors on the inner circumferential surface of the shell so that the front directions of adjacent anchors are perpendicular to each other.
[0010] The invention described in claim 3 is the invention described in claim 1 or 2, characterized in that the nut is a tall nut that is long in the axial direction. Effect of the Invention
[0011] According to the spraying construction method of amorphous refractory material described in claim 1 (hereinafter simply referred to as the spraying construction method), it is possible to stably stand the plate material (plate-shaped body) for forming score lines in an upright position without using anchors attached to the surface of the furnace shell, so that an amorphous refractory layer with uniform score line width and depth can be easily formed on the inner or outer surface of the furnace shell, regardless of the skill of the worker, etc.
[0012] According to the spraying method of claim 2, the monolithic refractory layer formed on the inner or outer peripheral surface of the steel shell of the furnace is unlikely to peel off from the inner or outer peripheral surface of the steel shell.
[0013] According to the spraying construction method described in claim 3, the work of screwing the shuttlecock bolt into the nut in the bolt screwing step becomes easier, so that the amorphous refractory layer can be formed very easily and efficiently. [Brief description of the drawings]
[0014] [Figure 1] 1 is a flowchart showing each step of a spraying construction method. [Diagram 2] FIG. 1 is an explanatory diagram showing the steps of a spraying construction method (a is a perspective view, and b is a plan view). [Diagram 3] FIG. 2 is an explanatory diagram (front view) showing an anchor. [Figure 4] FIG. 1 is an explanatory diagram showing the steps of a spraying construction method (a is a perspective view, and b is a plan view). [Diagram 5] FIG. 13 is an explanatory diagram (front view) showing a shuttlecock bolt. [Figure 6] FIG. 1 is an explanatory diagram showing the steps of a spraying construction method (a is a perspective view, and b is a plan view). [Figure 7] FIG. 1 is an explanatory diagram showing the steps of a spraying construction method (a is a perspective view, and b is a plan view). [Figure 8] FIG. 1 is an explanatory diagram showing the steps of a spraying construction method (a is a perspective view, and b is a plan view). [Figure 9]It is an explanatory drawing (plan view) showing the steps of the spraying construction method. [Figure 10] It is an explanatory drawing (plan view) showing the steps of the spraying construction method. [Figure 11] It is an explanatory drawing (plan view) showing the steps of the spraying construction method. [Figure 12] It is an explanatory drawing showing the refractory layer formed by the spraying construction method (a is a plan view, and b is a cross-sectional view taken along line A-A in a). [Figure 13] It is an explanatory drawing (plan view) showing a modified example of the panel joint body used in the spraying construction method.
Embodiments for Carrying out the Invention
[0015] Hereinafter, a detailed description will be given with reference to the drawings of an embodiment of the work of forming a refractory layer (refractory wall) made of unshaped refractory on the inner peripheral surface of a furnace (such as a combustion furnace) using the spraying construction method according to the present invention.
[0016] <Steps of the Spraying Construction Method> FIG. 1 shows the steps of the spraying construction method, and the spraying construction method S sequentially performs the following steps (a) to (g). a. Anchor erection step, and b. Nut fixing step c. Bolt screwing step d. Plate-like body fixing step e. Panel box forming step f. Outer spraying of the box step g. Inner spraying of the box step Hereinafter, each step will be described in order.
[0017] <a. Anchor erection step> In the spraying construction method S, first, an anchor erection step is carried out in which a plurality of anchors are erected on the inner peripheral surface of an iron sheet covering a furnace (combustion furnace) (covering the outer periphery) in a predetermined regular arrangement. FIG. 2 shows a state in which the anchors 2, 2... are erected on the inner peripheral surface (substantially horizontal surface) of the iron sheet 1 in the anchor erection step, and FIG. 3 shows the anchor 2. The anchor 2 erected on the iron sheet 1 has its lower end bent at a right angle with respect to the shaft portion (central portion in the vertical direction), and the upper portion is bent on the opposite side of the lower end so as to form an angle of about 120° in the same plane with respect to the shaft portion. It is composed of a long member 2a made of metal (iron) and a short member 2b made of metal (iron) whose upper portion is bent so as to form an angle of about 120° with respect to the lower portion. And the anchor 2 is arranged such that the lower end and the upper bent portions of the long member 2a and the upper bent portion of the short member 2b are in the same plane, and the short member 2b is welded to the long member 2a so as to form a V-shaped angle of 120° with the upper bent portion of the long member 2a and the upper bent portion of the short member 2b, and is integrally formed.
[0018] In the anchor erection step, the Y-shaped anchors 2, 2... formed as described above are welded to the inner peripheral surface of the iron sheet 1 at the lower end portion of the long member 2a such that the shaft portion (central portion in the vertical direction) of the long member 2a is perpendicular to the surface of the iron sheet 1. Also, as shown in FIG. 2, the shaft portions of the long members 2a of the respective anchors 2, 2... are located at lattice points having equal lengths in the front, rear, left, and right directions, and the front directions of adjacent anchors 2, 2 are perpendicular to each other. The anchors 2, 2... are arranged on the inner peripheral surface of the iron sheet 1 (note that the broken lines in FIG. 2 and the like are virtual lines for making the arrangement state of the anchors 2, 2... easier to understand). Further, when welding the anchors 2, 2... to the inner peripheral surface of the iron sheet 1 in this way, it is preferable to adjust the distance between the shaft portions of the long members 2a of adjacent anchors 2, 2 to 200 mm to 250 mm.
[0019] <b. Nut Fixing Step> As described above, in the anchor installation step, after the anchors 2, 2... are regularly arranged (installed) on the inner peripheral surface of the iron sheet 1, as shown in FIG. 4, cylindrical nuts 3, 3... having female threads formed on their inner peripheral surfaces are fixed (welded) at predetermined positions on the inner peripheral surface of the iron sheet 1. As the nut 3, a tall nut that is long in the axial direction (longer than the radial direction) can be preferably used. Further, the nut 3 is located at the midpoint of the axial portions (central portions of the long portions 2a) of the adjacent anchors 2, 2, and the outer periphery of the lower end is welded to the inner peripheral surface of the iron sheet 1 so that the axial direction (height direction of the nut 3) is orthogonal to the inner peripheral surface of the iron sheet 1. When welding the nut 3 to the inner peripheral surface of the iron sheet 1 in this way, it is preferable to use spot welding so that it can be easily removed later. Then, the nuts 3, 3... are welded to the inner peripheral surface of the iron sheet 1 in a scattered manner so that there is one nut for approximately 6 to 8 anchors 2, 2...
[0020] <c. Bolt Screwing Step> And, as described above, after the nuts 3, 3... are installed in a scattered manner at predetermined positions on the inner peripheral surface of the iron sheet 1, wing nuts 4, 4... are screwed onto those nuts 3, 3... FIG. 5 shows the wing nut 4. The wing nut 4 is integrally formed of metal (iron), and a substantially cylindrical bolt body 4b is connected to the lower end of a long (vertically long) rectangular plate-like portion 4a. And on the right side of the plate-like portion 4a, three screw insertion holes 4c, 4c... are bored at equal intervals on the same upper and lower line, and on the left side of the plate-like portion 4a, three screw insertion holes 4c, 4c... are staggered from the screw insertion holes 4c, 4c... on the right side (so that the screw insertion holes 4c, 4c... on the right side are located in the middle of the two adjacent screw insertion holes 4c, 4c... on the left side), and are bored at equal intervals on the same upper and lower line. Further, on the outer periphery of the lower side of the bolt body 4b, a male thread that engages with the female thread engraved on the inner peripheral surface of the nut 3 is formed. When screwing the wing nuts 4, 4... onto the nuts 3, 3..., the plate surface of the plate-like body 4a of the wing nut 4 is arranged to be orthogonal to the virtual line connecting the axial portions of the adjacent Y-shaped anchors 2, 2.
[0021] <d. Plate-Like Body Fixing Step> After screwing the battens bolts 4, 4,... to the nuts 3, 3,... as described above, as shown in FIG. 6, a wide rectangular plate-like body 5 is fixed to the plate-like portions 4a of those battens bolts 4, 4,... so that the longitudinal direction is orthogonal to the axial direction of the battens bolt 4 (screwed with a wood screw or the like using the screw insertion holes 4c, 4c,...). By the wide rectangular plate-like bodies 5 screwed to the plate-like portions 4a of the respective battens bolts 4, 4,..., a score line will be formed after construction. In this case, a wooden plate can be preferably used as the plate-like body 5. Further, when screwing the plate-like body 5 to the plate-like portion 4a of the battens bolt 4, it is preferable to screw it so that the upper end edge of the plate-like body 5 and the upper end edge of the plate-like portion 4a of the battens bolt 4 are aligned (matched) (see FIG. 6(a)).
[0022] <e. Compane box forming step> After screwing the plate-like bodies 5 to the plate-like portions 4a of the respective battens bolts 4, 4,... as described above, one battens bolt 4 (and nut 3), and the surroundings on the sides of two adjacent anchors 2, 2 sandwiching the battens bolt 4 are covered, and six companes (plate bodies made of wood, synthetic resin, etc.) are erected so as to sandwich the plate-like body 5, thereby forming a compane box (closed portion).
[0023] FIG. 7 shows a state in which a compane box is formed. When forming the compane box B, first, three rectangular companes 6, 6,... are joined in a U-shape (U-shaped in plan view) to form a compane assembly C. Thereafter, the compane assembly C is arranged so that the upper portions of the outer end edges on the left and right sides of the open side are joined to the surface of the plate-like body 5, and is erected by welding to the inner peripheral surface of the iron sheet 1.
[0024] Also, when standing the panel assembly C upright on the inner peripheral surface of the iron sheet as described above, as shown in Fig. 8, L-shaped angles 7, 7 made of metal (iron) are used. One side (side surface) of the angles 7, 7 is screwed to the lower edge of the panels 6, 6 constituting the panel assembly C, and the other side (lower surface) of the angles 7, 7 is welded (spot welded) to the inner peripheral surface of the iron sheet 1. A method can be preferably used. In addition, when welding the panel assembly C to the inner peripheral surface of the iron sheet 1 using the angles 7, 7 in this way, one or a plurality of angles 7 are fixed to the inner sides of the panels 6, 6 on both the left and right sides of the panel assembly C, respectively, so that the panels 6, 6 on both the left and right sides of the panel assembly C are preferably welded to the inner peripheral surface of the iron sheet 1 (in Fig. 8, one angle 7, 7 is fixed to the inner side of each of the panels 6, 6 on both the left and right sides of the panel assembly C, and the state where the panels 6, 6 on both the left and right sides of the panel assembly C are welded to the inner peripheral surface of the iron sheet 1 is shown).
[0025] Also, on the back side of the plate-like body 5 fixed to the vane bolt 4, a similar panel assembly C is arranged such that the upper parts of the outer edges on both the left and right sides of the open side are joined to the back surface of the plate-like body 5, and is erected by welding to the inner peripheral surface of the iron sheet 1. Further, when standing the panel assembly C upright on the inner peripheral surface of the iron sheet 1 on the back side of the plate-like body 5 in this way, the outer edges on both the left and right sides of the open side of the panel assembly C fixed to the back side of the plate-like body 5 are aligned with the outer edges on both the left and right sides of the open side of the panel assembly C fixed to the front surface side of the plate-like body 5. In this way, by welding the two panel assemblies C, C to the inner peripheral surface of the iron sheet 1 in a state of facing each other with the plate-like body 5 interposed therebetween, a rectangular parallelepiped panel box (closed portion) B that is wide in the front and back and has an open upper surface is formed (see Fig. 7).
[0026] <f. Box outer spraying process> Then, as described above, after forming the plywood box (blocking portion) B so as to cover the periphery of the sides of the shuttlecock bolt 4 and the two anchors 2, 2 that are in contact with the shuttlecock bolt 4, as shown in FIG. 9, a refractory layer (refractory wall) D1 of a predetermined thickness is formed by spraying an amorphous refractory (castable, etc.) on the outside of the plywood box B (shaded area in FIG. 9). When spraying the amorphous refractory, the surface of the amorphous refractory is sprayed so as to be at the same height as the upper edge of the plate-like body 5 fixed to the shuttlecock bolt 4 (i.e., to have a constant thickness). The spraying operation can be performed manually or by using a machine such as a pressure pump. After spraying the amorphous refractory on the outside of the plywood box B, a sufficient amount of time is taken to cure the formed refractory layer D1.
[0027] Then, after the refractory layer D1 formed on the outside of the plywood box (blocked portion) B has hardened, the shuttlecock bolt 4 and the plate-like body 5 are separated (the wood screws are removed) and the shuttlecock bolt 4 and nut 3 are removed from the inner peripheral surface of the steel shell 1, as shown in Fig. 10. Note that the nut 3 is point-welded to the inner peripheral surface of the steel shell 1, so it can be easily removed by heating the welded portion again. Furthermore, the pair of plywood combined bodies C, C which sandwich the front and back surfaces of the plate-like body 5 to form the plywood box B are also removed from the inner peripheral surface of the steel shell 1. When removing the plywood assemblies C, C from the inner circumferential surface of the shell 1, it is possible to remove them together with the angles 7, 7... (i.e., reheat the welded parts to remove the angles 7, 7... from the inner circumferential surface of the shell 1), or it is possible to separate the angles 7, 7... from the plywood assemblies C, C (release the fastening state by the wood screws) and remove only the plywood assemblies C, C from the inner circumferential surface of the shell 1. In this way, by removing the shuttlecock bolts 4 and nuts 3 from the inner circumferential surface of the shell 1 and removing the pair of plywood assemblies C, C, only the plate-like body 5 crosses the inside of the plywood box B (more precisely, the hollow portion formed by the plywood box B) and is held by the left and right refractory layers D1 of the plywood box B (see FIG. 10).
[0028] <g. Spraying process inside the box> As described above, after forming the refractory layer D1 on the outside of the panel box B, removing the vane bolts 4 and nuts 3 inside the panel box B from the inner peripheral surface of the iron sheet 1, and removing the pair of panel coupling bodies C, C, as shown in Fig. 11, an amorphous refractory (the same as the castable sprayed on the outside of the panel box B) is sprayed inside the panel box B (exactly, the cavity formed by the panel box B) to form the refractory layer D2 (the hatched part in Fig. 11). When spraying the amorphous refractory in this way, similar to when spraying the amorphous refractory on the outside of the panel box B, it is sprayed so that the surface of the amorphous refractory is at the same height as the upper edge of the plate-like body 5 (that is, so as to have a certain thickness). After the spraying operation of the amorphous refractory into the panel box B, the formed refractory layer D2 is cured over a sufficient period of time to complete a series of spraying operations.
[0029] Fig. 12 shows the refractory layers D1 and D2 formed by the spraying construction method S consisting of the above steps a to g. At the surface of the refractory layers D1 and D2, score lines L, L... are formed in a state where plate-like bodies 5, 5... of the same thickness and the same height are embedded in a grid pattern. That is, due to the use of the combustion furnace, the plate-like bodies 5, 5... burn and disappear, so the embedded parts of the plate-like bodies 5, 5... function as grooves (cavity parts) for absorbing (relaxing) stress concentration due to thermal expansion and thermal contraction.
[0030] <Effects of the spraying construction method> As described above, the spraying method S sequentially performs the steps of a) setting up anchors, b) fastening nuts, c) screwing bolts, d) fastening plates, e) forming a plywood box, f) spraying outside the box, and g) spraying inside the box. Therefore, according to the spraying method S, the plates (plates 5, 5...) for forming the scorelines L, L... can be set up in a stable state without using the anchors 2, 2... attached to the surface of the shell 1, so that the refractory layers D1, D2 having uniform widths and depths of the scorelines L, L... can be easily formed on the inner or outer peripheral surface of the shell 1, regardless of the skill of the worker.
[0031] In addition, in the spraying construction method S, a. the anchor erection process involves arranging Y-shaped anchors 2, 2... on the inner surface of the steel shell 1 so that the front directions of adjacent anchors are perpendicular to each other, so that the refractory layers D1, D2 formed on the inner surface of the steel shell 1 are not easily peeled off from the inner surface of the steel shell 1.
[0032] Furthermore, in the spraying construction method S, the nuts 3, 3... used in b. nut fixing process, c. bolt screwing process, etc. are tall nuts that are long in the axial direction, so that the work of screwing the shuttlecock bolts 4, 4... into the nuts 3, 3... and the work of adjusting the orientation of the plate-like bodies 5, 5... are simple, and the refractory layers D1, D2 can be formed very easily and efficiently.
[0033] <Example of modified spray application method> The spray construction method of the present invention is not limited to the aspects of the above-mentioned embodiment, and the content of each process, such as the anchor installation process, nut fixing process, bolt screwing process, plate-shaped body fixing process, plywood box formation process, box exterior spraying process, and box interior spraying process, can be appropriately modified as necessary.
[0034] For example, the plywood box forming process is not limited to the above embodiment in which a pair of plywood combined bodies having a U-shape in plan view are fixed to the inner peripheral surface of the shell 1 with a plate-shaped body sandwiched between them. It is also possible to change the process to one in which a pair of plywood combined bodies C', C' having an L-shape in plan view are fixed to the inner peripheral surface of the shell 1 with a plate-shaped body 5 sandwiched between them, as shown in FIG. 13(a), or one in which a pair of plywood combined bodies C",C" having a semicircular (or semi-elliptical) shape in plan view are fixed to the inner peripheral surface of the shell 1 with a plate-shaped body 5 sandwiched between them, as shown in FIG. 13(b).
[0035] The spray application method according to the present invention is not limited to using wood material as the plate-like body as in the above embodiment, but can be changed to using a synthetic resin plate or the like (for example, a foamed resin plate or the like) as the plate-like body. Furthermore, the spray application method of the amorphous refractory material according to the present invention is not limited to using wood material as the plywood as in the above embodiment, but can be changed to using a synthetic resin plate or the like (for example, a polyethylene resin plate or the like) as the plywood.
[0036] Furthermore, the spraying construction method of the present invention is not limited to using castable as the amorphous refractory to be sprayed, as in the above embodiment, and the type of amorphous refractory to be sprayed can be changed appropriately as needed.
[0037] In addition, the spray construction method of the present invention is not limited to using Y-shaped anchors as in the above embodiment, but can also be changed to using anchors with shapes other than Y-shape, such as V-shaped anchors. [Industrial Applicability]
[0038] Since the spraying construction method of the present invention has excellent effects as described above, it can be suitably used as a method for forming a refractory layer (refractory wall) by spraying amorphous refractory material onto the inner or outer peripheral surface of a furnace. [Explanation of symbols]
[0039] S··Spraying method 1...Ironhide 2. Anchor 3. Nut 4··Shutter bolt 5. Plate-shaped body 6. Plywood 7. Angle C,C',C”··Plywood joint D1,D2...Refractory layer
Claims
1. A spraying method for forming a wall body made of a refractory material by spraying a shapeless refractory material onto an inner or outer peripheral surface of a steel shell covering a furnace, comprising the steps of: an anchor erecting step of erecting a plurality of anchors in a predetermined regular arrangement on an inner peripheral surface of an iron shell covering the furnace; a nut fixing step of fixing a cylindrical nut having a female thread formed on an inner peripheral surface of the shell so as to be positioned between two adjacent anchors erected on the inner peripheral surface of the shell; a bolt fastening process for fastening a shuttlecock bolt to a nut fixed to an inner peripheral surface of the shell; a plate-shaped body fixing process for fixing a wide rectangular plate-shaped body to the shuttlecock bolt screwed into the nut so that the longitudinal direction of the plate-shaped body is perpendicular to the axial direction of the bolt; a plywood box forming process for forming a closed portion made of plywood by erecting a plurality of plywood panels on the inner peripheral surface of the steel shell so as to sandwich the plate-like body and cover the sides of the two adjacent anchors and the nut located between them; A box exterior spraying process of spraying a shapeless refractory material onto the outside of the formed blocked portion; A method for spraying unshaped refractory material, comprising: a step of spraying unshaped refractory material inside a box, the step of spraying unshaped refractory material onto the inside of the formed blocked portion.
2. The method for spraying and installing unshaped refractory material as described in claim 1, characterized in that the anchor installation process involves arranging Y-shaped anchors on the inner surface of the steel shell so that the front directions of adjacent anchors are perpendicular to each other.
3. A method for spraying unshaped refractory material as described in claim 1 or 2, characterized in that the nut is a long nut that is long in the axial direction.