Optical laminate and wound body
The optical laminate with optimized layer configurations and peeling forces ensures easy separation of the separator from the laminate, addressing the challenge of peeling and hue differences in organic EL display devices, thereby improving device reliability and color consistency.
Patent Information
- Application Number
- JP2024020967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-15
AI Technical Summary
The challenge in organic EL display devices is the difficulty in peeling off the separator from a laminate containing a vertically aligned liquid crystal cured film without causing cracks or detachment of the adhesive layer, especially when the film is thin, leading to potential damage and hue differences when viewed from different angles.
An optical laminate is designed with a specific configuration of layers, including a surface protection film, a light-absorbing anisotropic layer, and a separator, where the peeling forces and distances between layers are optimized to facilitate easy separation of the separator while maintaining adhesion to the adherend, using stretched polyester films and polymerizable liquid crystal compounds with dichroic dyes, ensuring the laminate can be easily bonded to display devices.
The solution allows for successful peeling off the separator without damaging the laminate, preventing cracks and maintaining consistent color tone across viewing angles, enhancing the reliability and performance of organic EL display devices.
Smart Images

Figure 2024146765000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical laminate and a wound body obtained by winding the optical laminate. [Background technology]
[0002] In an organic EL (electroluminescence) display device, in order to reduce the hue difference between the front hue when viewed from the front during white display and the oblique hue when viewed from an oblique angle, it is known to use a laminate having a vertically aligned liquid crystal cured film containing a dichroic dye and a horizontally aligned retardation film (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-076920 A Summary of the Invention [Problem to be solved by the invention]
[0004] The vertically aligned liquid crystal cured film is used by being attached to an adherend such as an organic EL display device or a circular polarizing plate, so that a pressure-sensitive adhesive layer with a separator may be laminated on one surface. A surface protective film may be releasably laminated on the other surface of the vertically aligned liquid crystal cured film in order to prevent the adhesion of dirt or the occurrence of scratches during production or transportation. A laminate in which a pressure-sensitive adhesive layer with a separator and a surface protective film are laminated on the vertically aligned liquid crystal cured film is laminated by peeling off the separator to expose the pressure-sensitive adhesive layer, and then the surface protective film is peeled off.
[0005] In particular, when the vertically aligned liquid crystal cured film is a thin film, when attempting to peel the separator from the laminate, it may be impossible to peel off only the separator, the laminate may float up from the suction stage that is holding the laminate in place by suction, a crack-like striped pattern may appear in the vertically aligned liquid crystal cured film, or the adhesive layer may break.
[0006] An object of the present invention is to provide an optical laminate including an optically absorptive anisotropic layer, which allows the separator to be easily peeled off and which can be easily attached to any adherend. [Means for solving the problem]
[0007] The present invention provides the following optical laminate and roll. [1] An optical laminate comprising a surface protective film, a first protective layer, a light absorption anisotropic layer, a second protective layer, a first pressure-sensitive adhesive layer, and a separator laminated in this order, The surface protective film and the separator each include a stretched polyester film, The light absorption anisotropic layer contains a polymer of a polymerizable liquid crystal compound and a dichroic dye, and satisfies the relationships of the following formulas (1) to (3): a peel strength F1 [N / 25 mm] between the surface protective film and the first protective layer, and a peel strength F2 [N / 25 mm] between the separator and the first pressure-sensitive adhesive layer satisfy the relationships of the following formulas (4) to (6), An optical laminate, wherein the distance from a surface of the first protective layer on the surface protection film side to a surface of the second protective layer on the first pressure-sensitive adhesive layer side is 30 μm or less. Az>(Ax+Ay) / 2 (1) 0.001≦Ax≦0.1 (2) Ax(z=60°) / Ax≧5 (3) 0.05≦F1≦0.30 (4) 0.02≦F2≦0.15 (5) 0.02≦F1-F2 (6) [In formulas (1) to (3), Ax, Ay, and Az are the absorbances of the optically absorptive anisotropic layer at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less, and represent the absorbances of linearly polarized light vibrating in the x-axis direction, y-axis direction, and z-axis direction, respectively. Ax(z=60°) is the absorbance at the maximum absorption wavelength, and represents the absorbance of linearly polarized light vibrating in the x-axis direction when the optically absorptive anisotropic layer is rotated 60° around the y-axis as the rotation axis. Here, the x-axis is an arbitrary direction within the plane of the optically absorptive anisotropic layer, the y-axis is a direction perpendicular to the x-axis in the plane of the optically absorptive anisotropic layer, The z-axis is a direction perpendicular to the x-axis and the y-axis. [2] The optical laminate according to [1], wherein the thickness of the stretched polyester film included in the surface protective film is 30 μm or more. [3] The optical laminate according to [1] or [2], wherein the thickness of the stretched polyester film included in the separator is 30 μm or more. [4] The optical laminate according to any one of [1] to [3], wherein the surface protective film is a laminate of a stretched polyester film and a second pressure-sensitive adhesive layer. [5] The optical laminate according to any one of [1] to [4], wherein the surface protective film and the stretched polyester film included in the separator are both biaxially stretched polyester films. [6] The optical laminate according to any one of [1] to [5], wherein the surface protective film and the first protective layer are in direct contact with each other. [7] The optical laminate according to any one of [1] to [6], wherein the first protective layer and the optically absorptive anisotropic layer are in direct contact with each other, or the optical laminate has only an alignment layer between the first protective layer and the optically absorptive anisotropic layer. [8] The optical laminate according to any one of [1] to [7], wherein the optically absorptive anisotropic layer and the second protective layer are in direct contact with each other. [9] The optical laminate according to any one of [1] to [8], wherein the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.
[10] The optical laminate according to any one of [1] to [9], wherein the first protective layer has a thickness of 28 μm or less.
[11] The optical laminate according to any one of [1] to
[10] , wherein the second protective layer has a thickness of 15 μm or less.
[12] A rolled body obtained by rolling the optical laminate according to any one of [1] to
[11] . Effect of the Invention
[0008] According to the present invention, the separator can be easily peeled off from the optical laminate including the light absorption anisotropic layer, and the laminate can be easily attached to any adherend. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an optical laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, preferred embodiments of the optical laminate and the roll will be described with reference to the drawings.
[0011] <Optical laminate> 1 is a cross-sectional view showing a schematic diagram of an optical laminate according to one embodiment of the present invention. The optical laminate 10 includes a surface protective film 11, a first protective layer 12, a light absorption anisotropic layer 13, a second protective layer 14, a first pressure-sensitive adhesive layer 15, and a separator 16 laminated in this order.
[0012] The surface protective film 11 and the first protective layer 12 may be in direct contact. The surface protective film 11 is usually peelably laminated to the first protective layer 12. The first protective layer 12 and the optically absorptive anisotropic layer 13 may be in direct contact, or only an alignment layer may be provided between the first protective layer 12 and the optically absorptive anisotropic layer 13. The optically absorptive anisotropic layer 13 and the second protective layer 14 may be in direct contact. The second protective layer 14 and the first pressure-sensitive adhesive layer 15 may be in direct contact. The first pressure-sensitive adhesive layer 15 and the separator 16 are usually in direct contact. The separator 16 is usually peelably laminated to the first pressure-sensitive adhesive layer 15.
[0013] Both the surface protective film 11 and the separator 16 include a stretched polyester film. Both the surface protective film 11 and the separator 16 preferably include a biaxially stretched polyester film. The stretched polyester films included in the surface protective film 11 and the separator 16 may be the same or different.
[0014] The surface protective film 11 may be a laminate of a stretched polyester film and a second pressure-sensitive adhesive layer, and the stretched polyester film and the second pressure-sensitive adhesive layer may be in direct contact with each other. When the surface protective film 11 has a second pressure-sensitive adhesive layer, the second pressure-sensitive adhesive layer side is disposed on the first protective layer 12 side in the optical laminate 10. By having the surface protective film 11 have the second pressure-sensitive adhesive layer, when the optical laminate 10 is bent, the occurrence of cracks in the light absorption anisotropic layer 13 due to stress relaxation of the second pressure-sensitive adhesive layer can be suppressed.
[0015] The surface protective film 11 may be a stretched polyester film whose surface has been subjected to a release treatment.
[0016] The surface protective film 11 may be a laminate of a stretched polyester film and a peeling force adjustment layer, and the stretched polyester film and the peeling force adjustment layer may be in direct contact with each other. When the peeling force adjustment layer side of the optical laminate 10 is disposed on the first protective layer 12 side, it is preferable that the peeling force adjustment layer and the first protective layer are in direct contact with each other. This makes it possible to omit the step of laminating the second pressure-sensitive adhesive layer on the stretched polyester film, and to reduce the overall thickness of the optical laminate 10, which is advantageous in improving the flexibility of the optical laminate 10. The peeling force adjustment layer can be formed, for example, using a silane coupling agent or the like.
[0017] The separator 16 may be a stretched polyester film with a release-treated surface. The separator 16 may be a laminate of a stretched polyester film and a release force adjustment layer, and the stretched polyester film and the release force adjustment layer may be in direct contact with each other. When the separator 16 has a release force adjustment layer, it is preferable that the release force adjustment layer and the first pressure-sensitive adhesive layer are in direct contact with each other. The release force adjustment layer can be formed, for example, by using a silane coupling agent or the like.
[0018] The light absorptive anisotropic layer 13 contains a polymer of a polymerizable liquid crystal compound and a dichroic dye, and satisfies the relationships of the following formulas (1) to (3). Az>(Ax+Ay) / 2 (1) 0.001≦Ax≦0.1 (2) Ax(z=60°) / Ax≧5 (3) [In formulas (1) to (3), Ax, Ay, and Az are the absorbances of the optically absorptive anisotropic layer 13 at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less, and represent the absorbances of linearly polarized light vibrating in the x-axis direction, y-axis direction, and z-axis direction, respectively. Ax (z=60°) is the absorbance at the above-mentioned maximum absorption wavelength, and represents the absorbance of linearly polarized light vibrating in the x-axis direction when the optically absorptive anisotropic layer 13 is rotated 60° around the y-axis as the rotation axis. Here, the x-axis is an arbitrary direction in the plane of the optically absorptive anisotropic layer 13, The y-axis is a direction perpendicular to the x-axis in the plane of the optically absorptive anisotropic layer 13. The z-axis is perpendicular to the x-axis and y-axis.]
[0019] When the optically absorptive anisotropic layer 13 satisfies the relationships of the above formulas (1) to (3), it is believed that the absorption axis of the dichroic dye is oriented in a direction perpendicular to the plane of the optically absorptive anisotropic layer 13, and therefore the optically absorptive anisotropic layer 13 can effectively transmit light from the front direction and effectively absorb light from oblique directions.
[0020] Since the absorbance Az in the z direction in the above formula (1) is measured by making light incident on the side surface of the light absorption anisotropic layer 13, it is difficult to measure. Therefore, when the angle formed by the vibration plane of the linearly polarized light that is the measurement light and the x-y plane of the light absorption anisotropic layer 13 is 90°, with respect to this vibration plane, the x-y plane of the light absorption anisotropic layer 13 is inclined by 30° and 60° in the incident direction of the linearly polarized light, and the absorbance Az in the z direction can be estimated.
[0021] Specifically, it can be estimated by the following methods or the like. With the y-axis as the rotation axis, with the light absorption anisotropic layer 13 rotated by 30° and 60°, the same linearly polarized light as the linearly polarized light used to measure Ax is made incident, and the absorbance Ax(z = 30°) and the absorbance Ax(z = 60°) are measured respectively. Similarly, with the x-axis as the rotation axis, with the light absorption anisotropic layer 13 rotated by 30° and 60°, the same linearly polarized light as the linearly polarized light used to measure Ay is made incident, and the absorbance Ay(z = 30°) and the absorbance Ay(z = 60°) are measured respectively. At this time, if Ax(z = 30°) < Ax(z = 60°) and Ay(z = 30°) = Ay(z = 60°), then Ax(z = 30°) < Ax(z = 60°) < Ax(z = 90°) = Az, and if Ay(z = 30°) < Ay(z = 60°) and Ax(z = 30°) = Ax(z = 60°), then Ay(z = 30°) < Ay(z = 60°) < Ay(z = 90°) = Az. Therefore, it can be said that the relationship of formula (1) is necessarily satisfied. Here, Ax(z = 90°) is the absorbance measured by making the same linearly polarized light as the linearly polarized light used to measure Ax incident with the y-axis as the rotation axis and the light absorption anisotropic layer 13 rotated by 90°. Ay(z = 90°) is the absorbance measured by making the same linearly polarized light as the linearly polarized light used to measure Ax incident with the x-axis as the rotation axis and the light absorption anisotropic layer 13 rotated by 90°.
[0022] In particular, when there is no absorption anisotropy in the x-y plane of the light absorption anisotropic layer 13, that is, when Ax and Ay are equal, Ax(z = 30°) = Ay(z = 30°) and Ax(z = 60°) = Ay(z = 60°). Here, let Ax(z = 30°) = Ay(z = 30°) = A(z = 30°), Ax(z = 60°) = Ay(z = 60°) = A(z = 60°), and Ax(z = 90°) = Ay(z = 90°) = A(z = 90°). Then, if A(z = 30°) < A(z = 60°), the relationship A(z = 30°) < A(z = 60°) < A(z = 90°) = Az is satisfied. Further, if A(z = 30°) > (Ax + Ay) / 2, it can be said that Az necessarily satisfies Equation (1).
[0023] The above Ax and Ay represent the absorbance in the front direction of the light absorption anisotropic layer 13. It can be said that the smaller the values of Ax and Ay, the more accurately the dichroic dye in the light absorption anisotropic layer 13 is oriented in the direction perpendicular to the plane. The values of Ax and Ay are preferably 0.3 or less. When the values of Ax and Ay exceed 0.3, the coloring in the front direction of the light absorption anisotropic layer 13 becomes strong. Therefore, since the front transmission hue deteriorates when the light absorption anisotropic layer 13 is applied to a display device, the values of Ax and Ay are each independently preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.02 or less. Also, the lower limit values of the values of Ax and Ay are each independently usually 0.001 or more, may be 0.003 or more, and may be 0.005 or more. It can be said that in the light absorption anisotropic layer 13 that satisfies the relationship of the above Equation (2), the absorption axis of the dichroic dye is accurately oriented in the direction perpendicular to the plane of the light absorption anisotropic layer 13. When the absorbance Ax exceeds 0.10, the coloring in the front direction of the light absorption anisotropic layer 13 becomes strong. Therefore, for example, when applied to an organic EL display device in combination with a circular polarizing plate or the like, the front hue tends to deteriorate.
[0024] In the light absorption anisotropic layer 13, it is preferable that Ax and Ay have the same value. When Ax and Ay are different, there will be absorption anisotropy in the plane of the light absorption anisotropic layer 13. When the light absorption anisotropic layer 13 is applied to a display device, the coloring of the front hue tends to increase.
[0025] In the above formula (3), the larger the value of Ax(z=60°) / Ax, the better the light absorption anisotropy. It is preferably greater than 5, more preferably 7 or more, even more preferably 10 or more, and is preferably 50 or less.
[0026] In the optically absorptive anisotropic layer 13 that satisfies the relationship of the above formula (3), the absorption axis of the dichroic dye is considered to be oriented in a direction perpendicular to the plane of the optically absorptive anisotropic layer 13, and therefore the optically absorptive anisotropic layer 13 can effectively absorb light from oblique directions.
[0027] The above Ax (z=60°) means the oblique absorbance of the light absorption anisotropic layer 13, and can be appropriately selected according to the light leaking obliquely from the display device. Ax (z=60°) is preferably 1.0 or less, more preferably 0.5 or less, and even more preferably 0.3 or less. The lower limit is usually 0.001 or more, may be 0.003 or more, and is 0.01 or more if necessary.
[0028] The optically absorptive anisotropic layer 13 satisfying the relationships of the above formulas (1) to (3) can be adjusted, for example, by the thickness of the optically absorptive anisotropic layer 13, the conditions of the manufacturing process of the optically absorptive anisotropic layer 13, and the types or contents of the dichroic dye and polymerizable liquid crystal compound contained in the optically absorptive anisotropic layer-forming composition for obtaining the optically absorptive anisotropic layer 13.
[0029] The peel force F1 [N / 25 mm] between the surface protective film 11 and the first protective layer 12, and the peel force F2 [N / 25 mm] between the separator 16 and the first adhesive layer 15 satisfy the relationships of the following formulas (4) to (6). 0.05≦F1≦0.30 (4) 0.02≦F2≦0.15 (5) 0.02≦F1-F2 (6)
[0030] The peeling force F1 is preferably 0.08N / 25mm or more and 0.28N / 25mm or less, more preferably 0.1N / 25mm or more and 0.25N / 25mm or less, and may be 0.12N / 25mm or more and 0.23N / 25mm or less. The peeling force F2 is preferably 0.03N / 25mm or more and 0.13N / 25mm or less, more preferably 0.05N / 25mm or more and 0.10N / 25mm or less, and may be 0.06N / 25mm or more and 0.08N / 25mm or less. The difference (F1-F2) between the peeling force F1 and the peeling force F2 is preferably 0.03 or more, more preferably 0.04 or more, may be 0.05 or more, may be 0.07 or more, and is usually 0.2 or less.
[0031] The peeling force F1 can be adjusted by the surface state of the stretched polyester film contained in the surface protective film 11 due to a release treatment or the like, the composition of the adhesive composition used to form the second adhesive layer when the surface protective film 11 includes a second adhesive layer, the type of silane coupling agent or the like used to form the peeling force adjustment layer when the surface protective film 11 includes a peeling force adjustment layer, the surface treatment of the bonding surface of the surface protective film 11 and the first protective layer 12, etc. The peeling force F2 can be adjusted by the surface state of the separator 16 due to a release treatment or the like, the composition of the adhesive composition used to form the first adhesive layer 15, the surface treatment of the bonding surface of the separator 16 and the first adhesive layer 15, etc. The peeling forces F1 and F2 can be measured by the method described in the examples described later.
[0032] The distance D from the surface of the first protective layer 12 on the surface protective film 11 side to the surface of the second protective layer 14 on the first pressure-sensitive adhesive layer 15 side is 30 μm or less. The distance D is preferably 28 μm or less, may be 25 μm or less, or may be 20 μm or less, and is usually 2 μm or more, or may be 5 μm or more. When the distance D is small, it becomes easier to suppress a decrease in visibility at the bent portion when the optical laminate is bent so that the surface protective film is on the inside.
[0033] The optical laminate 10, excluding the surface protective film 11 and the separator 16, is laminated on an adherend such as an organic EL display device or a circular polarizing plate as an anti-reflection film for use. This makes it possible to suppress changes in color depending on the viewing angle of an image on the display device.
[0034] When a laminate obtained by removing the surface protective film 11 and the separator 16 from the optical laminate 10 is laminated on an adherend, for example, the laminate is laminated as follows. First, the optical laminate 10 is fixed by suction on a suction stage having a suction hole so that the surface protective film 11 side is the suction stage side. In this state, the separator 16 of the optical laminate 10 is peeled off. Next, the first pressure-sensitive adhesive layer 15 exposed by peeling off the separator 16 is attached to the adherend. Thereafter, the surface protective film 11 may be peeled off at an appropriate timing. When the distance D is small as in the optical laminate 10, the entire optical laminate tends to follow the movement of peeling off the separator, making it difficult to peel off only the separator, the optical laminate may float up from the suction stage that fixes the optical laminate by suction, or peeling off the separator may cause crack-like stripes to appear in any of the first protective layer, the light absorption anisotropic layer, the second protective layer, and the first pressure-sensitive adhesive layer, or these layers may break. However, since the optical laminate 10 satisfies the relationships of the above formulas (4) to (6), only the separator 16 can be favorably peeled off, and the laminate can be easily attached to an adherend.
[0035] <Rolled body> The wound body is obtained by winding the optical laminate 10 into a roll shape. The optical laminate 10 described above can be used. The optical laminate 10 constituting the wound body is preferably a long optical laminate.
[0036] The roll diameter (diameter) of the wound body can be, for example, 50 mm or more and 1000 mm or less. The long optical laminate wound into a roll to become a wound body may have a length of, for example, 5 m or more and 10,000 m or less in the length direction, which is the winding direction of the wound body, or 5 m or more and 5,000 m or less, or 100 m or more and 5,000 m or less, or 500 m or more and 3,000 m or less, or 1000 m or more and 3,000 m or less. The length of the width direction, which is the winding axis direction of the wound body, may be 300 mm or more and 5,000 mm or less, or 500 mm or more and 3,000 mm or less, or 500 mm or more and 2,500 mm or less, or 500 mm or more and 2,000 mm or less.
[0037] The layers of the optical laminate and the components contained in the layers will be described in detail below.
[0038] (Surface protection film) The surface protective film includes a stretched polyester film. The surface protective film may be a laminate of a stretched polyester film and a second pressure-sensitive adhesive layer, a stretched polyester film whose surface has been subjected to a release treatment, or a laminate of a stretched polyester film and a peeling force adjusting layer. The release treatment may be a method of forming a release layer by coating a release agent or the like. Examples of the release agent include a silicone-based release agent and a fluorine-based release agent. The stretched polyester film is preferably a biaxially stretched polyester film. The peeling force adjusting layer may be formed, for example, by coating a silane coupling agent.
[0039] The thickness of the stretched polyester film is preferably 30 μm or more, more preferably 35 μm or more, and may be 40 μm or more, and is usually 100 μm or less. The thickness of the second pressure-sensitive adhesive layer is 5 μm or more, may be 10 μm or more, or may be 15 μm or more, and is usually 30 μm or less.
[0040] The stretched polyester film is a film obtained by uniaxially or biaxially stretching a polyethylene terephthalate (PET) film, and is preferably a film obtained by biaxially stretching a polyethylene terephthalate (PET) film.
[0041] The tensile modulus of the stretched polyester film at a temperature of 23° C. and a relative humidity of 55% is preferably 4000 MPa or more, may be 5000 MPa or more, may be 6000 MPa or more, and is usually 20000 MPa or less. The tensile modulus can be calculated from the slope of the initial straight line in the obtained stress-strain curve by clamping both ends of a test piece having a length of 100 mm and a width of 25 mm with the upper and lower grips of a tensile tester so that the distance between the grips is 5 cm, and pulling the test piece at a pulling speed of 1 mm / min in an environment of a temperature of 23° C. and a relative humidity of 55%.
[0042] (1st protective layer) The first protective layer can support the optically absorbing anisotropic layer. The first protective layer can be a layer to which a composition for forming an optically absorbing anisotropic layer is applied to form the optically absorbing anisotropic layer. The first protective layer can have a single layer structure or a multilayer structure. When an alignment layer is used to form the optically absorbing anisotropic layer, the alignment layer can be formed on the surface of the first protective layer on the side where the optically absorbing anisotropic layer is formed.
[0043] The first protective layer may include one or more of a film substrate, a coating layer, and a glass substrate. The first protective layer preferably includes a film substrate or a coating layer, and may be a laminate of a film substrate and another layer such as a coating layer.
[0044] Examples of the resin constituting the film substrate include olefin resins such as polyethylene and polypropylene; cyclic olefin resins having a cyclo- or norbornene structure; polyvinyl alcohol; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; (meth)acrylic resins; cellulose ester resins such as triacetyl cellulose, diacetyl cellulose and cellulose acetate propionate; polyimide resins; polycarbonate; polysulfone; polyethersulfone; polyether ketone; polyphenylene sulfide; polyphenylene oxide, etc. (Meth)acrylic refers to at least one of acrylic and methacrylic. The same applies to the notation of (meth)acryloyl, etc.
[0045] The film substrate may be a commercially available cellulose ester resin film, such as "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.), "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.).
[0046] Commercially available cyclic olefin resins may be used as the cyclic olefin resin constituting the film substrate. Examples of such cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona (Germany)), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). These cyclic olefin resins can be made into a film substrate by forming a film by known means such as a solvent casting method or a melt extrusion method.
[0047] As the film substrate, a commercially available cyclic olefin resin substrate may be used. Examples of such cyclic olefin resin substrates include "S-Cina" (registered trademark), "SCA40" (registered trademark) (both manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "ARTON Film" (registered trademark) (manufactured by JSR Corporation).
[0048] When the first protective layer is a coating layer, for example, a coating layer may be formed on a film substrate, an optically absorptive anisotropic layer may be formed on the coating layer, and then the film substrate may be peeled off to form the coating layer as the first protective layer. In this case, the film substrate may be easily peeled off by performing a release treatment to form a release layer by applying a release agent or the like on the surface of the film substrate on which the coating layer is formed. The film substrate to be peeled off may be used as the above-mentioned surface protective film.
[0049] Examples of the coating layer include a layer formed by applying a hard-coating agent, an easy-adhesion composition, or a coupling agent to the surface of a film substrate, and a layer formed by applying a reactive monomer or a reactive polymer to the surface of the film substrate and then graft-polymerizing the reactive monomer or polymer by irradiating the reactive monomer or polymer with active energy rays. As a film substrate having a coating layer, a hard-coated film having a hard-coated layer as a coating layer is preferable. When the first protective layer is a hard-coated film, a light-absorption anisotropic layer is preferably laminated on the hard-coated layer side. As a coating layer, a hard-coated layer is preferable.
[0050] The hard coat layer is preferably a cured product layer of a curable composition containing an active energy ray curable resin, and more preferably a cured product layer of a composition containing an ultraviolet ray curable resin. The curable composition containing an ultraviolet ray curable resin preferably contains a (meth)acrylic compound as a curable component, and the hard coat layer is preferably formed of a (meth)acrylic resin. The (meth)acrylic compound is a compound having at least one (meth)acryloyl group, and may be a monomer, oligomer, or polymer.
[0051] Examples of the (meth)acrylic compound include (meth)acrylate compounds such as monofunctional (meth)acrylate compounds and polyfunctional (meth)acrylate compounds; urethane (meth)acrylate compounds such as polyfunctional urethane (meth)acrylate compounds; epoxy (meth)acrylate compounds such as polyfunctional epoxy (meth)acrylate compounds; carboxyl group-modified epoxy (meth)acrylate compounds; polyester (meth)acrylate compounds, etc. These can be used alone or in combination. Among these, polyfunctional (meth)acrylate compounds or urethane (meth)acrylate compounds are preferred, and it is more preferred to combine a polyfunctional (meth)acrylate compound with a urethane (meth)acrylate.
[0052] The content of the polyfunctional (meth)acrylate compound is preferably 50 parts by mass or more and 100 parts by mass or less, more preferably 60 parts by mass or more and 95 parts by mass or less, and even more preferably 70 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the solid content of the curable composition. In this specification, the solid content of the curable composition refers to the total amount of components excluding the solvent from the curable composition when the curable composition contains a solvent.
[0053] The curable composition may contain a polymerization initiator in addition to the curable component. Examples of the polymerization initiator include a photopolymerization initiator and a radical polymerization initiator, and known polymerization initiators may be used.
[0054] The curable composition can be applied to a film substrate and then irradiated with active energy rays to polymerize the curable components such as the (meth)acrylic compound and cure the composition.
[0055] The hard coat layer preferably exhibits a value of 8B or harder in a pencil hardness test (measured by placing the film substrate on a glass plate) specified in JIS K 5600-5-4:1999 "General test methods for paints - Part 5: Mechanical properties of coatings - Section 4: Scratch hardness (pencil method)" and may exhibit a value of 5B or harder.
[0056] The surface of the first protective layer on which the light absorption anisotropic layer is formed may be subjected to a surface treatment. Examples of the surface treatment method include a method of subjecting the surface of the first protective layer to corona treatment or plasma treatment under an atmosphere from vacuum to atmospheric pressure, a method of laser treatment, a method of ozone treatment, a method of flame treatment, a method of saponifying the surface of the first protective layer, and the like.
[0057] The thickness of the first protective layer is preferably 28 μm or less, and may be 0.5 μm to 25 μm, 1 μm to 20 μm, 1 μm to 15 μm, 1 μm to 10 μm, or 1 μm to 5 μm. When the thickness of the first protective layer is small, it becomes easier to suppress a decrease in visibility at the bent portion when the optical laminate is bent so that the surface protective film is on the inside.
[0058] The thickness of the film substrate that may be included in the first protective layer is preferably thin in terms of the mass that can be practically handled, but if it is too thin, the strength tends to decrease and the processability tends to be poor. From this viewpoint, the thickness of the film substrate is preferably 5 μm or more and 28 μm or less, more preferably 10 μm or more and 25 μm or less, and even more preferably 10 μm or more and 23 μm or less.
[0059] If the thickness of the coating layer that may be included in the first protective layer is too thin, the strength decreases, and if it is too thick, cracks etc. tend to occur. From this viewpoint, the thickness of the coating layer is preferably 0.5 μm or more and 20 μm or less, more preferably 1 μm or more and 15 μm or less, even more preferably 1 μm or more and 10 μm or less, and even more preferably 1 μm or more and 5 μm or less.
[0060] The tensile modulus of the first protective layer at a temperature of 23° C. and a relative humidity of 55% is preferably 100 MPa or more and 10,000 MPa or less, and may be 200 MPa or more and 8,000 MPa or less, or may be 300 MPa or more and 6,000 MPa or less. The tensile modulus can be measured by the method described above.
[0061] (Light absorption anisotropic layer) The light absorbing anisotropic layer contains a polymer of a polymerizable liquid crystal compound and a dichroic dye. The light absorbing anisotropic layer may contain a polymer of one type of polymerizable liquid crystal compound, or may contain polymers of two or more types of polymerizable liquid crystal compounds. The light absorbing anisotropic layer may contain a polymer of one type of dichroic dye, or may contain two or more types of dichroic dyes.
[0062] The light absorption anisotropic layer can be formed using a light absorption anisotropic layer forming composition containing a polymerizable liquid crystal compound and a dichroic dye. The light absorption anisotropic layer forming composition can contain, as a solid content, a non-liquid crystal compound having a polymerizable group, and additives such as a polymerization initiator, a leveling agent, an alignment promoter, an antioxidant, and a photosensitizer, in addition to the polymerizable liquid crystal compound and the dichroic dye, as described below. Therefore, the light absorption anisotropic layer may contain a polymer of a non-liquid crystal compound having a polymerizable group and additives.
[0063] The polymerizable liquid crystal compound is preferably a liquid crystal compound that forms a smectic phase. The polymer of the polymerizable liquid crystal compound may or may not exhibit liquid crystallinity. The light-absorbing anisotropic layer can be formed from a light-absorbing anisotropic layer-forming composition that contains a polymerizable liquid crystal compound and a dichroic dye, and may be a liquid crystal cured film (a cured layer of the polymerizable liquid crystal compound) in which the polymerizable liquid crystal compound in the light-absorbing anisotropic layer-forming composition is polymerized and cured. The polymer of the polymerizable liquid crystal compound is a polymerized polymerizable liquid crystal compound, but a non-liquid crystal compound having a polymerizable group may be polymerized in the polymerizable liquid crystal compound, or a dichroic dye may be polymerized in the polymerizable liquid crystal compound.
[0064] The content of the polymer of the polymerizable liquid crystal compound in the light absorption anisotropic layer is preferably 40 parts by mass or more and 99.9 parts by mass or less, and may be 60 parts by mass or more and 99 parts by mass or less, or may be 70 parts by mass or more and 99 parts by mass or less, relative to 100 parts by mass of the light absorption anisotropic layer. When the content of the polymer of the polymerizable liquid crystal compound is within the above range, the orientation of the polymer of the polymerizable liquid crystal compound when forming the light absorption anisotropic layer tends to be high. The content ratio of the polymer of the polymerizable liquid crystal compound in the light absorption anisotropic layer can be calculated as the ratio of the polymerizable liquid crystal compound (the total amount when two or more kinds are included) to 100 parts by mass of the solid content of the light absorption anisotropic layer forming composition used to form the light absorption anisotropic layer. The solid content of the light absorption anisotropic layer forming composition means all components excluding volatile components such as organic solvents from the light absorption anisotropic layer forming composition.
[0065] The content of the dichroic dye in the light-absorbing anisotropic layer is preferably 0.1 to 30 parts by mass, and may be 0.5 to 20 parts by mass, 1 to 10 parts by mass, or 1 to 5 parts by mass, relative to 100 parts by mass of the light-absorbing anisotropic layer. The content of the dichroic dye in the light-absorbing anisotropic layer can be calculated as the ratio of the dichroic dye to 100 parts by mass of the solid content of the composition for forming the light-absorbing anisotropic layer. When the light-absorbing anisotropic layer contains two or more dichroic dyes, the content of the dichroic dye refers to the total amount.
[0066] The thickness of the optically absorptive anisotropic layer is preferably 0.2 μm to 5.0 μm, more preferably 0.5 μm to 4.0 μm, and even more preferably 0.5 μm to 3.0 μm. If the optically absorptive anisotropic layer is too thin, the absorption of light from oblique directions tends to be weak, whereas if the layer is too thick, the orientation of the dichroic dye tends to be disturbed, and the transmission characteristics in the front direction tend to decrease.
[0067] The surface of the optically absorptive anisotropic layer on which the second protective layer is formed may be subjected to a surface treatment, such as a corona treatment or plasma treatment under a vacuum to atmospheric pressure, a laser treatment, an ozone treatment, or a flame treatment.
[0068] (Polymerizable liquid crystal compound) The polymerizable liquid crystal compound contained in the composition for forming the light absorption anisotropic layer is used to align the dichroic dye by host-guest interaction. The polymerizable liquid crystal compound has one or more polymerizable groups in the molecule and has liquid crystal properties.
[0069] The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and a (meth)acryloyl group and a (meth)acryloyloxy group are more preferred. The liquid crystal property may be a thermotropic liquid crystal or a lyotropic liquid crystal, but when mixed with the above-mentioned dichroic dye, a thermotropic liquid crystal is preferred. In this specification, a (meth)acryloyl group means at least one of an acryloyl group and a methacryloyl group. The same applies to the notation of (meth)acrylic, etc.
[0070] When forming a polymer of a polymerizable liquid crystal compound by polymerization reaction and expressing light absorption anisotropy characteristics as a film containing the polymer and a dichroic dye, the liquid crystal state shown by the polymerizable liquid crystal compound is a smectic phase, and it is preferable that the liquid crystal state is a high-order smectic phase from the viewpoint of high performance. Among them, a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferable, and a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic F phase, or a smectic I phase is even more preferable. When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these high-order smectic phases, a light absorption anisotropic layer with higher light absorption anisotropy characteristics can be manufactured. In such an optically absorptive anisotropic layer having high optical absorption anisotropy, a Bragg peak derived from a high-order structure such as a hexatic phase or a crystalline phase is obtained in X-ray diffraction measurement. The Bragg peak is a peak derived from a periodic structure of molecular orientation, and the optically absorptive anisotropic layer can have a periodic interval of 3 to 6 Å. It is preferable that the optically absorptive anisotropic layer contains a polymer of a polymerizable liquid crystal compound oriented in a smectic phase state, from the viewpoint of obtaining higher optical absorption anisotropy.
[0071] The polymerizable liquid crystal compound may be a monomer, an oligomer in which a polymerizable group is polymerized, or a polymer. As such a polymerizable liquid crystal compound, a known compound can be used, for example, those described in JP-A-2020-76920 and JP-A-6728581.
[0072] (dichroic dye) The dichroic dye is a dye having different absorbance in the long axis direction of the molecule and absorbance in the short axis direction of the molecule. The dichroic dye preferably has a property of absorbing visible light, and more preferably has a maximum absorption wavelength (λmax) in the wavelength range of 380 to 680 nm.
[0073] Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, among which bisazo dyes and trisazo dyes are preferred. The dichroic dyes may be used alone or in combination of two or more kinds, but it is preferred to use two or more kinds in combination according to the wavelength range in which the light absorption anisotropy is required in the light absorption anisotropic layer.
[0074] The azo dye includes a compound represented by formula (I) (hereinafter sometimes referred to as "compound (I)"). K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K 3 represent each independently a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. K 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer equal to or greater than 2, multiple K 2 may be the same or different from each other. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.
[0075] Examples of the monovalent heterocyclic group include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.
[0076] K 1 and K 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 Examples of the substituent that the p-phenylene group, the naphthalene-1,4-diyl group, and the divalent heterocyclic group in the formula (I) may optionally have include an alkyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, and a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group refers to an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2).
[0077] Among the compounds (I), compounds represented by any one of formulas (I-1) to (I-8) are preferred, compounds represented by any one of formulas (I-1) to (I-3) are more preferred, and compounds represented by any one of formulas (I-1) and (I-3) are even more preferred.
[0078] [ka]
[0079] [In the formulas (I-1) to (I-8), B 1 ~B 30 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]
[0080] The anthraquinone dye is preferably a compound represented by formula (I-9). [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0081] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-10), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. Rx represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0082] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0083] In formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.
[0084] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 each independently represents a group represented by any one of formulas (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 represent, independently of each other, a group represented by any one of formulas (I-13a) to (I-13h). [ka] n6 represents an integer from 1 to 3.
[0085] Among these dichroic dyes, azo dyes are preferred from the viewpoint of alignment.
[0086] The content of the dichroic dye in the composition for forming the light absorption anisotropic layer (the total amount when two or more kinds are included) is usually 1 part by mass to 60 parts by mass, preferably 1 part by mass to 40 parts by mass, and more preferably 1 part by mass to 20 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound, from the viewpoint of obtaining good light absorption properties. If the content of the dichroic dye is less than this range, the light absorption becomes insufficient and sufficient light absorption anisotropy properties cannot be obtained, whereas if the content is more than this range, the alignment of the liquid crystal molecules of the polymerizable liquid crystal compound may be hindered.
[0087] (Method of forming optically absorptive anisotropic layer) The optically absorptive anisotropic layer can be formed, for example, by applying an optically absorptive anisotropic layer-forming composition onto the first protective layer. The optically absorptive anisotropic layer-forming composition contains a polymerizable liquid crystal compound and a dichroic dye, and may also contain a non-liquid crystal compound having a polymerizable group, a solvent, an additive, and the like, which will be described later.
[0088] The coating layer formed by coating the composition for forming an optically absorbing anisotropic layer is subjected to a drying treatment to remove the solvent, etc. The coating layer after the drying treatment is irradiated with active energy rays, etc. to polymerize the polymerizable liquid crystal compound, thereby forming an optically absorbing anisotropic layer as a cured layer (liquid crystal cured film) of the composition for forming an optically absorbing anisotropic layer on the first protective layer. The composition for forming an optically absorbing anisotropic layer may be applied to the surface of the first protective layer, or may be applied to the surface of the alignment layer formed on the surface of the first protective layer.
[0089] Examples of a method for applying the composition for forming an optically absorptive anisotropic layer include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0090] It is preferable to perform a drying treatment on the coating layer of the composition for forming the optically absorbing anisotropic layer formed on the first protective layer. When the composition for forming the optically absorbing anisotropic layer contains a solvent, the solvent in the coating layer can be removed by drying the coating layer. The drying method may be a known method, and may be one or more of natural drying, heat drying, ventilation drying, and reduced pressure drying.
[0091] The drying conditions in the drying process can be appropriately determined depending on the components contained in the composition for forming the optically absorptive anisotropic layer. For example, the drying temperature in the drying process may be 50° C. or more and 150° C. or less, or 60° C. or more and 120° C. or less. The drying time in the drying process may be 15 seconds or more and 10 minutes or less, or 0.5 minutes or more and 5 minutes or less.
[0092] When a heat treatment is performed in the drying process, the polymerizable liquid crystal compound contained in the composition for forming the light absorbing anisotropic layer can be oriented while removing the solvent in the coating layer by heating to a temperature equal to or higher than the liquid crystal phase transition temperature at which the polymerizable liquid crystal compound undergoes a phase transition. In particular, when a polymerizable liquid crystal compound that forms a smectic phase is oriented in a direction perpendicular to the surface of the light absorbing anisotropic layer, it is preferable to heat the composition in a temperature range where the compound transitions to a smectic phase. This allows the polymerizable liquid crystal compound to be oriented in a direction perpendicular to the surface of the light absorbing anisotropic layer, and the dichroic dye can also be oriented along with the orientation of the polymerizable liquid crystal compound.
[0093] After drying the coating layer formed on the first protective layer, the polymerizable liquid crystal compound and the dichroic dye are oriented and then irradiated with active energy rays to polymerize and harden the polymerizable liquid crystal compound, thereby forming a light absorption anisotropic layer.
[0094] Photopolymerization is preferred as a method for polymerizing the polymerizable liquid crystal compound. Photopolymerization is performed by irradiating active energy rays to a laminated structure including a coating layer in which a composition for forming a light-absorbing anisotropic layer is applied on a first protective layer. The active energy rays to be irradiated are appropriately selected according to the type of polymerizable liquid crystal compound contained in the coating layer (particularly, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator when a photopolymerization initiator is contained, and the amount thereof. Specifically, one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be mentioned. Among them, ultraviolet light is preferred in terms of ease of controlling the progress of the polymerization reaction and the fact that photopolymerization devices widely used in this field can be used, and it is preferable to select the type of polymerizable liquid crystal compound so that it can be photopolymerized by ultraviolet light.
[0095] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.
[0096] The UV irradiation intensity is usually 10mW / cm 2 ~3,000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a radical polymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 mJ / cm 2 ~3,000mJ / cm 2 , preferably 50 mJ / cm 2 ~2,000mJ / cm 2 , more preferably 100 mJ / cm 2 ~1,000mJ / cm 2If the accumulated light amount is less than this range, the polymerizable liquid crystal compound is not sufficiently cured, and good transferability may not be obtained when transferring the light absorption anisotropic layer on the first protective layer to an adherend. Conversely, if the accumulated light amount is more than this range, the light absorption anisotropic layer may become colored.
[0097] (Non-liquid crystal compound having a polymerizable group) A non-liquid crystal compound having a polymerizable group (hereinafter, sometimes referred to as a "non-liquid crystal compound") is a compound having a polymerizable group and not having liquid crystallinity. Examples of the polymerizable group of the non-liquid crystal compound include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, preferred polymerizable groups are a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group, more preferred polymerizable groups are a (meth)acryloyl group and a (meth)acryloyloxy group, and even more preferred polymerizable groups are a (meth)acryloyloxy group. The polymerizable group in the non-liquid crystal compound may be one type or a combination of two or more types, but is preferably the same polymerizable group as the polymerizable group of the polymerizable liquid crystal compound.
[0098] The number of polymerizable groups that the non-liquid crystal compound has is not particularly limited and may be, for example, 1 to 20, but from the viewpoint of making it easier to increase the film strength of the light absorption anisotropic layer, it is preferably 2 to 10, more preferably 3 to 6. When the non-liquid crystal compound has two or more polymerizable groups, the polymerizable groups may be the same or different from each other.
[0099] Examples of the non-liquid crystal compound include monofunctional (meth)acrylates and polyfunctional (meth)acrylates. Since the monofunctional acrylates and polyfunctional acrylates as the non-liquid crystal compounds having a polymerizable group are non-liquid crystal, they preferably do not have a mesogen structure. The monofunctional acrylates and polyfunctional acrylates may contain a urethane structure, an amino structure, an epoxy structure, an ethylene glycol structure, and / or a polyester structure in the molecule.
[0100] (solvent) The solvent that may be contained in the composition for forming the light absorption anisotropic layer is preferably one that can completely dissolve the polymerizable liquid crystal compound, and is preferably a solvent that is inactive to the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more.
[0101] The content of the solvent in the composition for forming an optically absorptive anisotropic layer is preferably 50 to 98% by mass relative to the total amount of the composition for forming an optically absorptive anisotropic layer. In other words, the content of the solid content in the composition for forming an optically absorptive anisotropic layer is preferably 2 to 50% by mass, more preferably 5 to 30% by mass. When the content of the solid content is 50% by mass or less, the viscosity of the composition for forming an optically absorptive anisotropic layer is low, so that the optically absorptive anisotropic layer is easily formed to a substantially uniform thickness, and the optically absorptive anisotropic layer tends to be less prone to unevenness. The content of the solid content can be determined in consideration of the thickness of the optically absorptive anisotropic layer to be produced.
[0102] (Additives) The composition for forming an optically absorptive anisotropic layer may contain additives such as a polymerization initiator, such as a photopolymerization initiator or a thermal polymerization initiator, a leveling agent, an alignment promoter, an antioxidant, and a photosensitizer.
[0103] The composition for forming the light absorbing anisotropic layer may contain a polymerization initiator. The polymerization initiator is used when the composition for forming the light absorbing anisotropic layer contains a compound involved in the polymerization reaction of a polymerizable liquid crystal compound, and is a compound capable of initiating the polymerization reaction of the compound. As the polymerization initiator for initiating the polymerization reaction of the polymerizable liquid crystal compound, a photopolymerization initiator that generates active radicals by the action of light is preferable from the viewpoint of not depending on the phase state of the thermotropic liquid crystal.
[0104] The photopolymerization initiator may be any known photopolymerization initiator as long as it is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound or the like. Specifically, photopolymerization initiators capable of generating active radicals or acids under the action of light may be used, and among these, photopolymerization initiators that generate radicals under the action of light are preferred. The photopolymerization initiators may be used alone or in combination of two or more.
[0105] As the photopolymerization initiator, a known photopolymerization initiator can be used. For example, the photopolymerization initiator that generates active radicals is Self-cleavable benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, azo compounds, and the like; Hydrogen abstraction type benzophenone compounds, alkylphenone compounds, benzoin ether compounds, benzil ketal compounds, dibenzosuberone compounds, anthraquinone compounds, xanthone compounds, thioxanthone compounds, halogenoacetophenone compounds, dialkoxyacetophenone compounds, halogenobisimidazole compounds, halogenotriazine compounds, triazine compounds, etc. can be used.
[0106] As the photopolymerization initiator that generates an acid, an iodonium salt, a sulfonium salt, or the like can be used.
[0107] From the viewpoint of excellent reaction efficiency at low temperatures, the photopolymerization initiator is preferably a self-cleavage type photopolymerization initiator, and in particular, an acetophenone-based compound, a hydroxyacetophenone-based compound, an α-aminoacetophenone-based compound, or an oxime ester-based compound is preferred.
[0108] The content of the polymerization initiator in the composition for forming the light absorption anisotropic layer can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, but is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the alignment of the polymerizable liquid crystal compound.
[0109] The light-absorbing anisotropic layer forming composition may contain a leveling agent. The leveling agent is an additive that adjusts the fluidity of the light-absorbing anisotropic layer forming composition and makes the film obtained by applying the light-absorbing anisotropic layer forming composition flatter. The light-absorbing anisotropic layer forming composition may contain a fluorine-based leveling agent such as a silicon-based leveling agent, a polyacrylate-based leveling agent, or a perfluoroalkyl-based leveling agent, and preferably contains a silicon leveling agent. By containing a silicon-based leveling agent in the light-absorbing anisotropic layer forming composition, blocking of the light-absorbing anisotropic layer can be easily suppressed. When the light-absorbing anisotropic layer forming composition contains a silicon leveling agent, the content of the silicon leveling agent may be, for example, the range described below as the content in the light-absorbing anisotropic layer.
[0110] The silicon-based leveling agent is a leveling agent containing silicon atoms, and it is preferable to use a leveling agent having a polyorganosiloxane skeleton. Examples of groups bonded to silicon atoms (silicon atoms forming siloxane bonds) in polyorganosiloxane include hydrocarbon groups. Among them, preferred are alkyl groups having 1 to 10 carbon atoms, alkoxy groups having 1 to 10 carbon atoms, ester groups having 1 to 10 carbon atoms, and aryl groups, more preferred are methyl groups and phenyl groups, and even more preferred are methyl groups. The groups bonded to the silicon atoms may be of only one type or of two or more types. The number of repetitions of the siloxane unit (degree of polymerization) is not particularly limited, but is preferably 2 to 10,000, more preferably 3 to 5,000, and even more preferably 5 to 1,000.
[0111] As the silicon-based leveling agent, a commercially available product can be used. Commercially available silicone leveling agents include, for example, BYK-300, BYK-302, BYK-306, BYK-307, BYK-310, BYK-313, BYK-315N, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-342, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-370, BYK-377, BYK-378, BYK-3455, and BYK-UV3510 (all manufactured by BYK Japan Co., Ltd.), KF-945, KF-6015, and KF-6020 (all manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of those having a radical polymerizable group such as a (meth)acryloyl group added to the polyether chain include BYK-UV3500, BYK-UV3505, BYK-3510, BYK-UV3530, BYK-UV3570, BYK-UV3575, BYK-UV3576 (all manufactured by BYK Japan K.K.), KP-422, KP-416, KP-418, KP-410, KP-411, KP-412, KP-413, KP-423, KP-414, KP-415, KP-420, and KP-983 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0112] The silicon-based leveling agent is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, even more preferably 0.05 parts by mass or more and 2.0 parts by mass or less, even more preferably 0.1 parts by mass or more and 1.0 parts by mass or less, and particularly preferably 0.1 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the polymer of the polymerizable liquid crystal compound contained in the light absorption anisotropic layer. The content of the polymerizable liquid crystal compound polymer and the content of the silicon-based leveling agent can be calculated as the content of the polymerizable liquid crystal compound and the silicon-based leveling agent in the light absorption anisotropic layer forming composition. When the content of the silicon-based leveling agent is within the above range, it is easy to adjust the haze of the optical film to the above range. When the content of the silicon-based leveling agent is 5.0 parts by mass or less, it is easy to suppress repelling when the light absorption anisotropic layer forming composition is applied to the first protective layer.
[0113] In the case where the optically absorptive anisotropic layer-forming composition is directly applied to the surface of the first protective layer (when no alignment layer is used), the optically absorptive anisotropic layer-forming composition preferably contains an alignment promoter. The alignment promoter means a material that promotes the liquid crystal alignment of the polymerizable liquid crystal compound in a desired direction. Examples of the alignment promoter that promotes the alignment of the polymerizable liquid crystal compound in the vertical direction include ionic compounds consisting of nonmetallic atoms and nonionic silane compounds. The optically absorptive anisotropic layer-forming composition preferably contains at least one of ionic compounds consisting of nonmetallic atoms and nonionic silane compounds, and more preferably contains both ionic compounds consisting of nonmetallic atoms and nonionic silane compounds.
[0114] As the silane compound, a nonionic silane compound or a silane-containing ionic compound, which will be described later, can be used, and the vertical alignment regulating force can be increased by using these silane compounds. These silane compounds may be used alone or in combination of two or more, or may be used by mixing with other materials. When the silane compound is a nonionic silane compound, a silane compound having an alkyl group at the molecular end is preferred from the viewpoint of easily increasing the vertical alignment regulating force, and a silane compound having an alkyl group having 3 to 30 carbon atoms is more preferred.
[0115] When the composition for forming an optically absorptive anisotropic layer contains an ionic compound consisting of nonmetallic atoms, in the dried coating film of the composition for forming an optically absorptive anisotropic layer formed on the first protective layer, a vertical alignment regulating force for the polymerizable liquid crystal compound is exerted due to electrostatic interaction, and the polymerizable liquid crystal compound tends to be aligned in the vertical direction relative to the surface of the first protective layer in the dried coating film. This allows the polymerizable liquid crystal compound to maintain the vertical alignment state and form an optically absorptive anisotropic layer that is a liquid crystal cured film.
[0116] Examples of ionic compounds consisting of nonmetallic atoms include onium salts (more specifically, quaternary ammonium salts in which the nitrogen atom has a positive charge, tertiary sulfonium salts, and quaternary phosphonium salts in which the phosphorus atom has a positive charge). Among these onium salts, quaternary onium salts are preferred from the viewpoint of further improving the vertical alignment property of the polymerizable liquid crystal compound, and quaternary phosphonium salts or quaternary ammonium salts are more preferred from the viewpoint of improving availability and mass productivity. The onium salt may have two or more quaternary onium salt moieties in the molecule, and may be an oligomer or polymer.
[0117] The molecular weight of the ionic compound is preferably 100 or more and 10,000 or less. When the molecular weight is within the above range, it is easy to improve the vertical alignment property of the polymerizable liquid crystal compound while ensuring the coating property of the composition for forming the light absorption anisotropic layer. The molecular weight of the ionic compound is more preferably 5000 or less, and further preferably 3000 or less.
[0118] The cationic component of the ionic compound may be, for example, an inorganic cation or an organic cation. Among them, an organic cation is preferred because it is less likely to cause alignment defects of the polymerizable liquid crystal compound. Examples of the organic cation include an imidazolium cation, a pyridinium cation, an ammonium cation, a sulfonium cation, and a phosphonium cation.
[0119] Ionic compounds generally have a counter anion. Examples of the anion component that is the counter ion of the cationic component include inorganic anions and organic anions. Among them, organic anions are preferred because they are less likely to cause alignment defects of the polymerizable liquid crystal compound. It is not necessary that the cation and the anion correspond one-to-one.
[0120] Specific examples of the anion component include the following: Chloride anion [Cl - 〕, Bromide anion [Br - 〕, Iodide anion [I - 〕, Tetrachloroaluminate anion [AlCl4 - 〕, Heptachlorodialuminate anion [Al2Cl7 - 〕, Tetrafluoroborate anion [BF4 - 〕, Hexafluorophosphate anion [PF6 - 〕, Perchlorate anion [ClO4 - 〕, Nitrate anion [NO3 - 〕, Acetate anion [CH3COO - 〕, Trifluoroacetate anion [CF3COO - 〕, Fluorosulfonate anion [FSO3 -〕, Methanesulfonate anion [CH3SO3 - 〕, Trifluoromethanesulfonate anion [CF3SO3 - 〕, p-Toluenesulfonate anion [p-CH3C6H4SO3 - 〕, Bis(fluorosulfonyl)imide anion [(FSO2)2N - 〕, Bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - 〕, Tris(trifluoromethanesulfonyl)methanide anion [(CF3SO2)3C - 〕, Hexafluoroarsenate anion [AsF6 - 〕, Hexafluoroantimonate anion [SbF6 - 〕, Hexafluoroniobate anion [NbF6 - 〕, Hexafluorotantalate anion [TaF6 - 〕, Dimethylphosphinate anion [(CH3)2POO - 〕, (Poly)hydrofluorofluoride anion [F(HF) n - (For example, n represents an integer of 1 to 3), Dicyanamide anion [(CN)2N - 〕, Thiocyanine anion (SCN - 〕, Perfluorobutanesulfonate anion [C4F9SO3 - 〕, Bis(pentafluoroethanesulfonyl)imide anion [(C2F5SO2)2N - 〕, Perfluorobutanoate anion [C3F7COO-], and (Trifluoromethanesulfonyl)(trifluoromethanecarbonyl)imide anion [(CF3SO2)(CF3CO)N - 〕.
[0121] Specific examples of the ionic compound can be appropriately selected from the above-mentioned combinations of cationic and anionic components. Specific examples of the compound that is a combination of a cationic component and an anionic component include the following.
[0122] (Pyridinium salts) N-Hexylpyridinium hexafluorophosphate, N-octylpyridinium hexafluorophosphate, N-methyl-4-hexylpyridinium hexafluorophosphate, N-butyl-4-methylpyridinium hexafluorophosphate, N-octyl-4-methylpyridinium hexafluorophosphate, N-Hexylpyridinium bis(fluorosulfonyl)imide, N-Octylpyridinium bis(fluorosulfonyl)imide, N-methyl-4-hexylpyridinium bis(fluorosulfonyl)imide, N-butyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-octyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-Octylpyridinium bis(trifluoromethanesulfonyl)imide, N-methyl-4-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-butyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-octyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-Hexylpyridinium p-toluenesulfonate, N-Octylpyridinium p-toluenesulfonate, N-methyl-4-hexylpyridinium p-toluenesulfonate, N-butyl-4-methylpyridinium p-toluenesulfonate, and N-Octyl-4-methylpyridinium p-toluenesulfonate.
[0123] (Imidazolium salt) 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium p-toluenesulfonate, 1-Butyl-3-methylimidazolium methanesulfonate, etc.
[0124] (Pyrrolidinium salts) N-butyl-N-methylpyrrolidinium hexafluorophosphate, N-butyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium p-toluenesulfonate, etc.
[0125] (Ammonium salt) tetrabutylammonium hexafluorophosphate, Tetrabutylammonium bis(fluorosulfonyl)imide, Tetrahexylammonium bis(fluorosulfonyl)imide, trioctylmethylammonium bis(fluorosulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(fluorosulfonyl)imide, tetrabutylammonium bis(trifluoromethanesulfonyl)imide, tetrahexylammonium bis(trifluoromethanesulfonyl)imide, trioctylmethylammonium bis(trifluoromethanesulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(trifluoromethanesulfonyl)imide, tetrabutylammonium p-toluenesulfonate, Tetrahexylammonium p-toluenesulfonate, Trioctylmethylammonium p-toluenesulfonate, (2-hydroxyethyl)trimethylammonium p-toluenesulfonate, (2-hydroxyethyl)trimethylammonium dimethylphosphinate, 1-(3-trimethoxysilylpropyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylpropyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, N-{(3-triethoxysilylpropyl)carbamoyloxyethyl)}-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide, and N-[2-{3-(3-trimethoxysilylpropylamino)-1-oxopropoxy}ethyl]-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide.
[0126] (phosphonium salts) tributyl(2-methoxyethyl)phosphonium bis(trifluoromethanesulfonyl)imide, tributylmethylphosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[4-(trimethoxysilyl)butyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, and 1,1,1-Tributyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide. These ionic compounds may be used alone or in combination of two or more.
[0127] From the viewpoint of further improving the vertical alignment property of the polymerizable liquid crystal compound, the ionic compound preferably has a Si element and / or an F element in the molecular structure of the cationic moiety. When the ionic compound has a Si element and / or an F element in the molecular structure of the cationic moiety, the ionic compound is easily segregated on the surface of the light absorption anisotropic layer. Among them, the following ionic compounds (ii) to (iv) are preferable as ionic compounds whose constituent elements are all nonmetallic elements.
[0128] Ionic compounds (ii): [ka] Ionic compounds (iii): [ka] Ionic compounds (iv) [ka]
[0129] As a method for improving the vertical alignment of a polymerizable liquid crystal compound, for example, a method of treating the surface of the substrate with a surfactant having an alkyl group with a relatively long chain length is known (see, for example, Chapter 2, Liquid Crystal Orientation and Physical Properties, of the Liquid Crystal Handbook (published by Maruzen Co., Ltd.)). Such a method for improving the vertical alignment of a liquid crystal compound with a surfactant can also be applied to ionic compounds. That is, by treating the surface of the first protective layer with an ionic compound having an alkyl group with a relatively long chain length, the vertical alignment of a polymerizable liquid crystal compound can be effectively improved.
[0130] Specifically, ionic compounds have the following relationship: 5 <M<16 It is preferable that M in the above relationship satisfies the following formula: M = (number of covalent bonds from a positively charged atom to the end of the molecular chain of the substituent with the greatest number of covalent bonds to the end of the molecular chain among the substituents directly bonded to a positively charged atom) ÷ (number of positively charged atoms) It is expressed as: When the ionic compound satisfies the above-mentioned relationship, the vertical alignment property of the polymerizable liquid crystal compound can be effectively improved.
[0131] When there are two or more positively charged atoms in the molecule of an ionic compound, for a substituent having two or more positively charged atoms, the number of covalent bonds from the positively charged atom considered as the base point to the nearest other positively charged atom is considered to be the "number of covalent bonds from the positively charged atom to the molecular chain end" as defined above in the definition of M. When an ionic compound is an oligomer or polymer having two or more repeating units, the constituent unit is considered as one molecule and the above M is calculated. When a positively charged atom is incorporated in a ring structure, the number of covalent bonds from the ring structure to the positively charged atom or the number of covalent bonds to the end of the substituent bonded to the ring structure, whichever is larger, is considered to be the "number of covalent bonds from the positively charged atom to the molecular chain end" as defined above in the definition of M.
[0132] When the composition for forming an optically absorptive anisotropic layer contains an ionic compound, the content thereof is usually preferably 0.01 to 5 mass %, more preferably 0.05 to 4 mass %, and even more preferably 0.1 to 3 mass % based on the solid content of the composition for forming an optically absorptive anisotropic layer. When the content of the ionic compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the composition for forming an optically absorptive anisotropic layer.
[0133] When the optically absorbing anisotropic layer-forming composition contains a nonionic silane compound, the nonionic silane compound reduces the surface tension of the optically absorbing anisotropic layer-forming composition, and in a dried coating film formed on the first protective layer from the optically absorbing anisotropic layer-forming composition, the nonionic silane compound is present on the surface of the dried coating film opposite the first protective layer, increasing the vertical alignment regulating force for the polymerizable liquid crystal compound, and the polymerizable liquid crystal compound tends to be aligned in the vertical direction relative to the surface of the first protective layer in the dried coating film. This allows the polymerizable liquid crystal compound to maintain a vertical alignment state and form an optically absorbing anisotropic layer that is a liquid crystal cured film.
[0134] Nonionic silane compound is a compound that is nonionic and contains Si element. Examples of nonionic silane compound include silicon polymer such as polysilane, silicone resin such as silicone oil and silicone resin, silicone oligomer, organic inorganic silane compound such as silsesquioxane and alkoxysilane (more specifically, silane coupling agent, etc.), and silane-containing compound described in the leveling agent section.
[0135] The nonionic silane compound may be of silicone monomer type or silicone oligomer (polymer) type. When the silicone oligomer is expressed in the form of (monomer)-(monomer) copolymer, it may be a copolymer containing a mercaptopropyl group, such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane copolymer, and 3-mercaptopropyltriethoxysilane-tetraethoxysilane copolymer; a copolymer containing a mercaptomethyl group, such as mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, and mercaptomethyltriethoxysilane-tetraethoxysilane copolymer; a copolymer containing a mercaptomethyl group, such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, and mercaptomethyltriethoxysilane-tetraethoxysilane copolymer; methacryloyloxypropyl group-containing copolymers such as acryloyloxypropyl trimethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl trimethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl triethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl triethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl methyldimethoxysilane-tetramethoxysilane copolymer, 3-methacryloyloxypropyl methyldimethoxysilane-tetraethoxysilane copolymer, 3-methacryloyloxypropyl methyldiethoxysilane-tetramethoxysilane copolymer and 3-methacryloyloxypropyl methyldiethoxysilane-tetraethoxysilane copolymer;3-acryloyloxypropyltrimethoxysilane-tetramethoxysilane copolymer, 3-acryloyloxypropyltrimethoxysilane-tetraethoxysilane copolymer, 3-acryloyloxypropyltriethoxysilane-tetramethoxysilane copolymer, 3-acryloyloxypropyltriethoxysilane-tetraethoxysilane copolymer, 3-acryloyloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-acryloyloxypropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-acryloyloxypropylmethyldiethoxysilane-tetramethoxysilane copolymer and 3-acryloyloxypropylmethyldimethoxysilane-tetramethoxysilane copolymer. copolymers containing acryloyloxypropyl groups, such as ethyldiethoxysilane-tetraethoxysilane copolymer; copolymers containing vinyl groups, such as vinyltrimethoxysilane-tetramethoxysilane copolymer, vinyltrimethoxysilane-tetraethoxysilane copolymer, vinyltriethoxysilane-tetramethoxysilane copolymer, vinyltriethoxysilane-tetraethoxysilane copolymer, vinylmethyldimethoxysilane-tetramethoxysilane copolymer, vinylmethyldimethoxysilane-tetraethoxysilane copolymer, vinylmethyldiethoxysilane-tetramethoxysilane copolymer, and vinylmethyldiethoxysilane-tetraethoxysilane copolymer;Examples of the copolymer include amino group-containing copolymers such as 3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer, and 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer. These nonionic silane compounds may be used alone or in combination of two or more. Among them, silane coupling agents are preferred from the viewpoint of further improving adhesion to adjacent layers.;
[0136] The silane coupling agent is a compound containing an Si element having at least one functional group selected from the group consisting of vinyl group, epoxy group, styryl group, methacryl group, acrylic group, amino group, isocyanurate group, ureido group, mercapto group, isocyanate group, carboxy group, and hydroxy group at the end, and at least one alkoxysilyl group or silanol group. By appropriately selecting these functional groups, it is possible to impart unique effects such as improving the mechanical strength of the light absorption anisotropic layer, modifying the surface of the light absorption anisotropic layer, and improving the adhesion between the light absorption anisotropic layer and an adjacent layer (for example, the first protective layer). From the viewpoint of adhesion, it is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and another different reactive group (for example, the above-mentioned functional group). It is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and a polar group. When the silane coupling agent has at least one alkoxysilyl group and at least one polar group in its molecule, the vertical alignment of the polymerizable liquid crystal compound is more easily improved, and the vertical alignment promotion effect tends to be significantly obtained. Examples of the polar group include an epoxy group, an amino group, an isocyanurate group, a mercapto group, a carboxy group, and a hydroxy group. The polar group may have a suitable substituent or a protective group in order to control the reactivity of the silane coupling agent.
[0137] Specific examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldi ... ethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, and 3-glycidoxypropylethoxydimethylsilane.
[0138] Examples of commercially available silane coupling agents include KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE- 502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007 manufactured by Shin-Etsu Chemical Co., Ltd.
[0139] When the optically absorptive anisotropic layer-forming composition contains a nonionic silane compound, the content thereof is usually preferably 0.01% by mass to 5% by mass, more preferably 0.05% by mass to 4% by mass, and even more preferably 0.1% by mass to 3% by mass, based on the solid content of the optically absorptive anisotropic layer-forming composition. When the content of the nonionic silane compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the optically absorptive anisotropic layer-forming composition.
[0140] Since the composition for forming an optically absorbing anisotropic layer contains both an ionic compound and a nonionic silane compound, the vertical alignment of the polymerizable liquid crystal compound is more easily promoted in the dried coating film formed from the composition for forming an optically absorbing anisotropic layer on the first protective layer due to the electrostatic interaction derived from the ionic compound and the surface tension reducing effect derived from the nonionic silane compound. This makes it possible to form an optically absorbing anisotropic layer, which is a liquid crystal cured film, while maintaining the polymerizable liquid crystal compound in a more precisely vertically aligned state.
[0141] (Alignment layer) The alignment layer facilitates the alignment of the polymerizable liquid crystal compound. The state of liquid crystal alignment varies depending on the properties of the alignment layer and the polymerizable liquid crystal compound, and the combination thereof can be arbitrarily selected.
[0142] When the alignment layer is made of an alignment polymer, the alignment regulating force can be adjusted as desired by the surface state or rubbing conditions. When the alignment layer is made of a photoalignment polymer, the alignment regulating force can be adjusted as desired by the polarized light irradiation conditions, etc. In addition, the liquid crystal alignment can be controlled by selecting the physical properties, such as the surface tension and liquid crystallinity, of the polymerizable liquid crystal compound.
[0143] The alignment layer is preferably insoluble in a solvent used to form a light absorption anisotropic layer on the alignment layer, and has heat resistance to the heat treatment for removing the solvent and for orienting the liquid crystal. Examples of the alignment layer include a polymer alignment layer made of an orientable polymer, a photoalignment layer, a groove alignment layer, and a stretched film stretched in the alignment direction. When applied to a long rolled film, a photoalignment layer is preferred because the alignment direction can be easily controlled.
[0144] The thickness of the alignment layer is usually in the range of 10 nm to 5000 nm, preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 to 300 nm.
[0145] Examples of the alignment polymer used in the rubbing alignment layer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and their hydrolyzates, such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. These alignment polymers may be used alone or in combination of two or more.
[0146] Rubbing methods include a method in which an oriented polymer composition is applied to a layer constituting the first protective layer, and then annealed to form an oriented polymer film constituting the surface of the first protective layer, and the film is then brought into contact with a rotating rubbing roll wrapped with a rubbing cloth.
[0147] The photo-alignment layer is made of a polymer, oligomer, or monomer having a photoreactive group. The photo-alignment layer is provided with an alignment control force by irradiating a coating layer formed by applying a composition for forming a photo-alignment layer to a layer constituting the first protective layer with polarized light. The photo-alignment layer is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0148] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of liquid crystal alignment ability, such as molecular alignment induction caused by irradiation with light, or an isomerization reaction, a dimerization reaction, a photocrosslinking reaction, or a photodecomposition reaction. Among the photoreactive groups, those that cause a dimerization reaction or a photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group that can generate the above-mentioned reaction, those having an unsaturated bond, particularly a double bond, are preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) are more preferred.
[0149] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. From the viewpoint of easy control of reactivity and expression of alignment control force during photoalignment, chalcone groups and cinnamoyl groups are preferred. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, and formazan groups, and groups having azoxybenzene as a basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0150] The polarized light may be irradiated directly from the film surface of the coating layer of the composition for forming the photo-alignment layer, or may be irradiated from the undercoat layer side and then transmitted. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized light can be irradiated by passing light from the above-mentioned light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.
[0151] (2nd protective layer) The second protective layer can suppress the diffusion of the dichroic dye contained in the light absorption anisotropic layer and suppress damage to the light absorption anisotropic layer. Examples of the second protective layer include a layer formed from a resin composition containing a water-soluble polymer (hereinafter also referred to as a "water-soluble polymer-containing resin composition") and a layer formed from a photocurable composition containing an active energy ray curable resin. Since the water-soluble polymer generally has a polarity significantly different from that of the dichroic dye, it has an excellent effect of preventing the diffusion of the dichroic dye, and therefore the second protective layer is preferably a layer formed from a water-soluble polymer-containing resin composition.
[0152] Examples of water-soluble polymers include polyacrylamide-based polymers, vinyl alcohol-based polymers such as polyvinyl alcohol, ethylene-vinyl alcohol copolymers, and (meth)acrylic acid or its anhydride-vinyl alcohol copolymers, carboxyvinyl-based polymers, polyvinylpyrrolidone, starches, sodium alginate, and polyethylene oxide-based polymers. These polymers may be used alone or in combination of two or more.
[0153] When the second protective layer is a layer formed from a water-soluble polymer-containing resin composition, the content of the water-soluble polymer in the layer is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more.
[0154] When the second protective layer is a layer formed from a water-soluble polymer-containing resin composition, a crosslinking structure may be introduced by using a crosslinking agent to increase the density of the layer. Examples of the crosslinking agent include water-soluble crosslinking agents such as ionic crosslinking agents such as glyoxylate salts and epoxy crosslinking agents; and hydrophobic crosslinking agents such as isocyanate crosslinking agents, polyaldehyde crosslinking agents such as glyoxal and glyoxal derivatives, and metal compound crosslinking agents such as zirconium chloride or titanium lactate crosslinking agents for the purpose of imparting water resistance.
[0155] The amount of the crosslinking agent added may be appropriately determined depending on the type of the crosslinking agent, etc. For example, the amount may be 0.1 to 100 parts by mass, preferably 1 to 50 parts by mass, and more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the water-soluble polymer. When the content of the crosslinking agent is within the above range, a dense second protective layer can be formed.
[0156] The water-soluble polymer-containing resin composition is usually prepared as a solution in which the water-soluble polymer is dissolved in a solvent. The solvent may be selected depending on the water-soluble polymer to be used, but typically includes water, alcohol, a mixture of water and alcohol, and the like, with water being preferred.
[0157] The solid content of the water-soluble polymer-containing resin composition obtained by adding a solvent to the components constituting the second protective layer, such as the water-soluble polymer and the crosslinking agent, is preferably 1 to 50 mass%, more preferably 2 to 30 mass%, and even more preferably 3 to 15 mass%. When the solid content of the water-soluble polymer-containing resin composition is within the above range, the viscosity of the composition is low, and therefore the coatability and handleability are improved.
[0158] The water-soluble polymer-containing resin composition may contain other components such as additives in addition to the water-soluble polymer, the crosslinking agent, and the solvent such as water. Examples of the other components include preservatives and leveling agents. When the water-soluble polymer-containing resin composition contains other components such as additives, the amount of the other components is preferably 10% by mass or less, more preferably 5% by mass or less, based on the solid content of the resin composition.
[0159] A water-soluble polymer-containing resin composition prepared by dissolving necessary components such as a water-soluble polymer and a crosslinking agent in a solvent can be applied to the surface of the light absorption anisotropic layer opposite the first protective layer, and the solvent in the coating film can be dried and removed, followed by curing to form a second protective layer.
[0160] The method for applying the water-soluble polymer-containing resin composition is not particularly limited, and examples thereof include a method for applying a composition for forming an optically absorptive anisotropic layer.
[0161] The drying temperature and time for forming the second protective layer from the coating film of the water-soluble polymer-containing resin composition are not particularly limited, and may be appropriately determined depending on the composition of the water-soluble polymer-containing resin composition used. The drying treatment can be carried out, for example, by blowing hot air, and the temperature is usually within a range of 40 to 100° C., preferably 60 to 100° C. The drying time is usually 10 to 600 seconds.
[0162] Examples of the active energy ray curable resin contained in the photocurable composition include (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, silicone resins, etc. The active energy ray curable resin is preferably an epoxy resin.
[0163] The photocurable composition is applied to the surface of the optically absorptive anisotropic layer opposite to the first protective layer, and the second protective layer can be formed by irradiating the surface with active energy rays. As described above, the surface of the optically absorptive anisotropic layer on which the second protective layer is to be formed may be subjected to a surface treatment.
[0164] The thickness of the second protective layer is preferably 15 μm or less, and may be from 0.1 μm to 12 μm, preferably from 0.5 μm to 10 μm, and more preferably from 1 μm to 5 μm.
[0165] The tensile modulus of the second protective layer at a temperature of 23° C. and a relative humidity of 55% is preferably 100 MPa or more and 5000 MPa or less, and may be 200 MPa or more and 4000 MPa or less, or may be 300 MPa or more and 1000 MPa or less. The tensile modulus can be measured by the method described above.
[0166] (1st adhesive layer, 2nd adhesive layer) The first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer (hereinafter also referred to as "pressure-sensitive adhesive layer") can be formed using a pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition or a reaction product of the pressure-sensitive adhesive composition exhibits adhesive properties when it is attached to an adherend, and is known as a pressure-sensitive adhesive. In addition, the pressure-sensitive adhesive layer formed using the active energy ray-curable pressure-sensitive adhesive composition described below can be irradiated with active energy rays to adjust the degree of crosslinking or adhesive strength.
[0167] As the adhesive composition, a conventionally known adhesive having excellent optical transparency can be used without any particular limitation, and for example, an adhesive composition containing a base polymer such as an acrylic polymer, a urethane polymer, a silicone polymer, or a polyvinyl ether can be used. The adhesive composition may be an active energy ray curable adhesive composition or a heat curable adhesive composition. Among these, an adhesive composition using an acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, removability (reworkability), weather resistance, heat resistance, etc., is preferable. The adhesive layer is preferably composed of a reaction product of an adhesive composition containing a (meth)acrylic resin, a crosslinking agent, and a silane compound, and may contain other components.
[0168] The adhesive composition for forming the adhesive layer may contain a base polymer such as an acrylic polymer, a urethane polymer, a silicone polymer, or a polyvinyl ether. The adhesive composition may be an active energy ray curable adhesive, a heat curable adhesive, or the like. Among these, an adhesive having a (meth)acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, removability (reworkability), weather resistance, heat resistance, and the like, is preferred. The adhesive layer is preferably composed of a reaction product of an adhesive containing a (meth)acrylic resin, a crosslinking agent, and a silane compound, and may contain other components.
[0169] The adhesive layer may be formed using an active energy ray curable adhesive. The active energy ray curable adhesive is prepared by blending an ultraviolet curable compound such as a multifunctional acrylate with the above-mentioned adhesive composition, forming an adhesive layer, and then curing the adhesive layer by irradiating it with ultraviolet light, thereby forming a harder adhesive layer. The active energy ray curable adhesive has a property of being cured by irradiation with energy rays such as ultraviolet rays and electron beams. The active energy ray curable adhesive has adhesiveness even before irradiation with energy rays, and therefore has a property of being able to adhere to an adherend and to be cured by irradiation with energy rays to adjust the adhesion.
[0170] The thickness of the first adhesive layer is not particularly limited, but is usually 5 μm or more and 300 μm or less, optionally 10 μm or more and 250 μm or less, optionally 15 μm or more and 100 μm or less, or optionally 20 μm or more and 50 μm or less.
[0171] The thickness of the second adhesive layer is not particularly limited, but is usually 5 μm or more and 100 μm or less, optionally 10 μm or more and 80 μm or less, optionally 12 μm or more and 50 μm or less, or optionally 15 μm or more and 30 μm or less.
[0172] (Separator) The separator includes a stretched polyester film. The stretched polyester film is preferably a biaxially stretched polyester film. The thickness of the stretched polyester film is preferably 30 μm or more, more preferably 35 μm or more, and may be 40 μm or more, and is usually 100 μm or less.
[0173] The stretched polyester film is a film obtained by uniaxially or biaxially stretching a polyethylene terephthalate (PET) film, and is preferably a film obtained by biaxially stretching a polyethylene terephthalate (PET) film.
[0174] The separator may be a stretched polyester film with a release treatment applied to one side thereof, or may be a laminate of a stretched polyester film and a peel strength adjustment layer. The release treatment may be a method of forming a release layer by coating a release agent or the like. Examples of the release agent include silicone-based release agents and fluorine-based release agents. The peel strength adjustment layer may be formed, for example, by coating a silane coupling agent.
[0175] The tensile modulus of the stretched polyester film at a temperature of 23° C. and a relative humidity of 55% is preferably 4000 MPa or more, may be 5000 MPa or more, or may be 6000 MPa or more, and is usually 20000 MPa or less. The tensile modulus can be measured by the method described above. EXAMPLES
[0176] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. "%" and "parts" in the examples and comparative examples are by mass % and parts by mass unless otherwise specified.
[0177] [Preparation and production of surface protection film] (Preparation of Pressure-Sensitive Adhesive Composition (a)) Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube to replace the air in the reactor with nitrogen gas. Then, 93 parts of 2-ethylhexyl acrylate, 5.5 parts of 8-hydroxyoctyl acrylate, 1.5 parts of acrylic acid, and 60 parts of a solvent (ethyl acetate) were added to the reactor. Then, 0.1 parts of azobisisobutyronitrile as a polymerization initiator were dropped over 2 hours, and the reaction was carried out at 65°C for 6 hours to obtain an acrylic resin solution. The weight average molecular weight of the acrylic polymer contained in the acrylic resin solution was about 500,000 in terms of standard polystyrene by gel permeation chromatography.
[0178] To 100 parts of the acrylic polymer contained in the acrylic resin solution obtained above, 2.0 parts of 1-octylpyridinium dodecylbenzenesulfonate was added as an antistatic agent and stirred, and then 1.5 parts of Coronate HX (an isocyanurate of hexamethylene diisocyanate compound: manufactured by Tosoh Corporation) was added and mixed with stirring to obtain a pressure-sensitive adhesive composition (a).
[0179] (Preparation of Surface Protection Films (1) to (3)) Stretched polyethylene terephthalate films (hereinafter also referred to as "stretched PET films") (1) to (3) having thicknesses of 38 μm, 50 μm, and 75 μm were prepared, and the pressure-sensitive adhesive composition (a) obtained above was applied thereto, followed by drying at a temperature of 90° C. to remove the solvent, thereby forming a second pressure-sensitive adhesive layer (1) having a thickness of 15 μm, thereby obtaining surface protective films (1) to (3). The thicknesses of the stretched PET films (1), (2), and (3) in the surface protective films (1), (2), and (3) were 38 μm, 50 μm, and 75 μm, respectively.
[0180] (Preparation of Surface Protection Film (4)) A silane coupling agent, KBM-5103 (manufactured by Shin-Etsu Silicone), was dissolved in o-xylene to a concentration of 0.25% to prepare a composition for forming a release force adjusting layer (1). The composition for forming a release force adjusting layer (1) was applied to the surface opposite to the release-treated surface of a stretched PET film (thickness 38 μm, manufactured by Lintec Corporation SP-PLR382050) with one side subjected to release treatment using a bar coater, and dried in an oven at a temperature of 120° C. for 1 minute to form a release force adjusting layer (1) with a thickness of 40 nm, which was used as a surface protective film (4).
[0181] (Preparation of Surface Protection Film (5)) Surface protection film (5) was prepared in the same manner as surface protection film (4), except that a stretched PET film (thickness 75 μm, CAO manufactured by Fujiko Co., Ltd.) having a release treatment applied to one side was used instead of the stretched PET film (thickness 38 μm) having a release treatment applied to one side.
[0182] (Preparation of Surface Protection Film (6)) As the surface protective film (6), a stretched PET film (thickness 38 μm, SP-PLR382050 manufactured by Lintec Corporation) with one side subjected to a release treatment was prepared.
[0183] (Preparation of Surface Protection Film (7)) As a surface protective film (6), a stretched PET film (thickness 75 μm, CAO manufactured by Fujiko Co., Ltd.) having one side subjected to a release treatment was prepared.
[0184] [Preparation of composition for forming optically absorptive anisotropic layer] (Preparation of Optically Absorbent Anisotropic Layer-Forming Composition (1)) The components shown below were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic layer (1). Polymerizable liquid crystal compound (1): 75 parts Polymerizable liquid crystal compound (2): 25 parts Dichroic dye (1): 1 part Polymerization initiator (Irgacure 369, manufactured by BASF): 6 parts Non-liquid crystal compound having a polymerizable group (dipentaerythritol hexaacrylate (6 functional groups)): 1.5 parts Leveling agent (F-556, manufactured by DIC): 0.25 parts Solvent (o-xylene): 300 parts
[0185] The polymerizable liquid crystal compounds (1) and (2) have the structures shown below and were synthesized according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). ·Polymerizable liquid crystal compound (1): [ka] ·Polymerizable liquid crystal compound (2): [ka]
[0186] The dichroic dye (1) used was an azo-based dye having the following structure and described in the Examples of JP 2013-101328 A. The maximum absorption wavelength of the dichroic dye (1) measured in a chloroform solution was 600 nm. Dichroic dyes (1): [ka]
[0187] (Preparation of Optically Absorbent Anisotropic Layer-Forming Composition (2)) A composition for forming an optically absorptive anisotropic layer (2) was prepared in the same manner as in the preparation of the composition for forming an optically absorptive anisotropic layer (1), except that the solvent (o-xylene) was changed to a solvent (cyclopentanone).
[0188] (Preparation of Optically Absorbent Anisotropic Layer-Forming Composition (3)) The components shown below were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic layer (3). Polymerizable liquid crystal compound (1): 75 parts Polymerizable liquid crystal compound (2): 25 parts Dichroic dye (1): 2.5 parts Dichroic dye (2): 2.5 parts Dichroic dye (3): 2.5 parts Polymerization initiator (Irgacure 369, manufactured by BASF): 6 parts Leveling agent (polyacrylate compound (BYK-361N; manufactured by BYK-Chemie): 1.2 parts Solvent (o-xylene): 250 parts
[0189] As the dichroic dyes (2) and (3), azo dyes described in the examples of JP-A-2013-101328 were used. Dichroic dyes (2): [ka] Dichroic dyes (3): [ka]
[0190] (Preparation of Optically Absorbent Anisotropic Layer-Forming Composition (4)) The polymerizable liquid crystal compound (3) and the polymerizable liquid crystal compound (4) were mixed in a mass ratio of 90:10 to obtain a mixture. To 100 parts by mass of the obtained mixture, 0.25 parts by mass of the leveling agent "F-556", 1.5 parts by mass of the dichroic dye (1), 1.5 parts by mass of the ionic compound (molecular weight: 645) shown below, which was prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of the silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369) as a photopolymerization initiator were added. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80°C for 1 hour to obtain a composition for forming an optically absorbing anisotropic layer (4).
[0191] ·Polymerizable liquid crystal compound (3) [ka]
[0192] ·Polymerizable liquid crystal compound (4) [ka]
[0193] Ionic compounds [ka]
[0194] [Preparation of Water-Soluble Polymer-Containing Resin Composition] According to the synthesis scheme below, a water-soluble polymer consisting of the structural units shown below was obtained. [ka]
[0195] In 400g of dimethyl sulfoxide, 20g of polyvinyl alcohol having a molecular weight of 1000 (manufactured by Wako Pure Chemical Industries, Ltd.), 0.55mg of N,N-dimethyl-4-aminopyridine as a nucleophile, and 4.6g of triethylamine were dissolved, and the temperature was raised to 60°C while stirring. Then, a solution in which 10.5g of methacrylic anhydride was dissolved in 50g of dimethyl sulfoxide was dropped over 1 hour, and the mixture was reacted by heating and stirring at a temperature of 60°C for 14 hours. After the obtained reaction solution was cooled to room temperature, 481g of methanol was added to the reaction solution and stirred to mix completely, so that the ratio (mass) of the reaction solution to methanol was adjusted to 1:1. The water-soluble polymer was crystallized by a crystallization method by gradually adding 1500mL of acetone to this solution. The obtained solution containing white crystals was filtered, thoroughly washed with acetone, and then vacuum dried to obtain 20.2g of water-soluble polymer. The obtained water-soluble polymer was dissolved in water to prepare a 3% water-soluble polymer aqueous solution as a water-soluble polymer-containing resin composition.
[0196] [Preparation of Photocurable Composition] The components shown below were mixed and then defoamed to prepare a photocurable composition. The cationic photopolymerization initiator was mixed as a 50% propylene carbonate solution, and the parts are indicated by the solid content. Cationic polymerizable compound (1) [3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (product name: OXT-221, manufactured by Toagosei Co., Ltd.)]: 60.0 parts Cationic polymerizable compound (2) [3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (product name: CEL2021P, manufactured by Daicel Corporation)]: 32.5 parts Cationic polymerizable compound (3) [1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (trade name: EHPE3150, manufactured by Daicel Corporation)]: 7.5 parts Photocationic polymerization initiator [CPI-100P (manufactured by San-Apro Co., Ltd., 50% by weight solution)]: 2.3 parts Photosensitizer [9,10-dibutoxyanthracene]: 1.0 parts Photosensitizer assistant [1,4-diethoxynaphthalene]: 1.0 part
[0197] [Preparation of Pressure-Sensitive Adhesive Composition (b)] A mixed solution of 81.8 parts of ethyl acetate, 90.0 parts of butyl acrylate, 5.0 parts of methyl acrylate and 5.0 parts of acrylic acid was charged into a reaction vessel equipped with a cooling tube, a nitrogen introduction tube, a thermometer and a stirrer, and the air in the apparatus was replaced with nitrogen gas to make it oxygen-free, while raising the internal temperature to 55 ° C. Then, a solution of 0.15 parts of azobisisobutyronitrile (polymerization initiator) dissolved in 10 parts of ethyl acetate was added in its entirety. After adding the polymerization initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while maintaining the internal temperature at 54 to 56 ° C., and the addition of ethyl acetate was stopped when the concentration of the (meth)acrylic resin reached 35%, and the temperature was kept at this temperature until 6 hours had passed since the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20%, and an acrylic resin solution was prepared. The resulting acrylic resin had a weight average molecular weight Mw of 1.6 million and a molecular weight distribution Mw / Mn of 4.5. Mw and Mn were measured in terms of standard polystyrene using two "TSKgel GMHHR-H(S)" columns manufactured by Tosoh Corporation connected in series as columns in a GPC apparatus, tetrahydrofuran as an eluent, a sample concentration of 2 mg / mL, a sample introduction amount of 100 μL, a temperature of 40° C., and a flow rate of 1 mL / min.
[0198] To 100 parts of the solid content of the acrylic resin solution obtained above, 0.15 parts on an active ingredient basis of a crosslinking agent (manufactured by Tosoh Corporation: product name "Coronate L" (a solution of a trimethylolpropane adduct of tolylene diisocyanate in ethyl acetate (solid content concentration 75%)) and 0.2 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: product name "KBM-403") were added, and ethyl acetate was further added to make the solid content concentration 13%, to obtain a pressure-sensitive adhesive composition (b).
[0199] [Preparation of separator with adhesive layer] (Preparation of Separator (1) with Adhesive Layer) A release-treated stretched PET film (SP-PLR382050, manufactured by Lintec Corporation, thickness 38 μm) was used as the separator (1), and the pressure-sensitive adhesive composition (b) obtained above was applied to the release-treated surface of this stretched PET film and dried to form a first pressure-sensitive adhesive layer (1) having a thickness of 20 μm. This resulted in a separator (1) with a pressure-sensitive adhesive layer having a layer structure of separator (1) / first pressure-sensitive adhesive layer (1).
[0200] (Preparation of separator (2) with adhesive layer) A stretched PET film (75 μm thick, Fujiko Co., Ltd. CAO) with a release treatment applied to one side was used as the separator (2), and the adhesive composition (b) obtained above was applied to the release-treated surface of the stretched PET film and dried to form a first adhesive layer (2) with a thickness of 25 μm. This resulted in a separator (2) with an adhesive layer having a layer structure of separator (2) / first adhesive layer (2).
[0201] (Preparation of separator (3) with adhesive layer) A silane coupling agent, KBE-903 (Shin-Etsu Silicone), was dissolved in o-xylene to a concentration of 0.25% to prepare a composition for forming a release force adjusting layer (2). The composition for forming a release force adjusting layer (2) was applied to the release-treated surface of a stretched PET film (thickness 38 μm) (SP-PLR382050, manufactured by Lintec Corporation) that had been subjected to a release treatment, using a bar coater, and dried in an oven at a temperature of 120° C. for 1 minute to form a release force adjusting layer (2) with a thickness of 40 nm. This was used as a separator (3).
[0202] The adhesive composition (b) obtained above was applied to the peel strength adjusting layer (2) of the separator (3) and dried to form a first adhesive layer (1) having a thickness of 20 μm, thereby obtaining a separator (3) with an adhesive layer having a layer structure of separator (3) / first adhesive layer (1).
[0203] (Preparation of separator (4) with adhesive layer) The release-treated surface of a stretched PET film (SP-PLR382050, manufactured by Lintec Corporation, thickness 38 μm) that had been subjected to a release treatment was subjected to corona treatment three times to obtain a separator (4). The corona treatment was carried out using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The pressure-sensitive adhesive composition (b) obtained above was applied to the corona-treated surface and dried to form a first pressure-sensitive adhesive layer (1) having a thickness of 20 μm. This resulted in a separator (4) with a pressure-sensitive adhesive layer having a layer structure of separator (4) / first pressure-sensitive adhesive layer (1).
[0204] Example 1 A triacetyl cellulose film (KC2UA, manufactured by Konica Minolta, Inc., thickness 25 μm) serving as the first protective layer (1) was subjected to a corona treatment once using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The light absorption anisotropic layer forming composition (1) prepared above was applied to the corona-treated surface of the cut-out first protective layer using a bar coater, and then dried for 1 minute in a drying oven set at a temperature of 100° C. Next, ultraviolet light was irradiated (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 500 mJ / cm ) using a high-pressure mercury lamp (Uniqure VB-15201BY-A, manufactured by Ushio Inc.). 2 ) to form an optically absorptive anisotropic layer (1) in which the polymerizable liquid crystal compound and the dichroic dye were aligned perpendicular to the coating plane. The optically absorptive anisotropic layer (1) had a thickness of 1.0 μm. This resulted in a first laminate (1) having a layer structure of first protective layer (1) / optically absorptive anisotropic layer (1).
[0205] Next, the light absorption anisotropic layer (1) of the first laminate (1) was subjected to a corona treatment, and then the water-soluble polymer-containing resin composition prepared above was applied using a bar coater and dried for 2 minutes at a temperature of 100° C. to form a second protective layer (1) having a thickness of 1 μm and made of a water-soluble polymer film. This resulted in a second laminate (1) having a layer structure of the first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1).
[0206] The second protective layer (1) side of the second laminate (1) was bonded to the first pressure-sensitive adhesive layer (1) side of the separator (1) with a pressure-sensitive adhesive layer, and the first protective layer (1) side of the second laminate was bonded to the second pressure-sensitive adhesive layer (1) side of the surface protective film (1) to obtain an optical laminate (1). The layer structure of the optical laminate (1) was the surface protective film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0207] Example 2 An optical laminate (2) was obtained in the same manner as in Example 1, except that a corona treatment was performed once on the second pressure-sensitive adhesive layer (1) of the surface protection film (1) and the first protective layer (1) side of the second laminate under conditions of an output of 0.3 kW and a treatment speed of 3 m / min using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) The layer structure of the optical laminate (2) was the surface protection film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0208] Example 3 After a corona treatment was performed on the light absorption anisotropic layer (1) of the first laminate (1), a photocurable composition was applied using a bar coater, and the integrated amount of UVA was about 500 mJ / cm 2 . 2 (Measurement device: measured value using UV Power Puck II manufactured by FusionUV) and the photocurable composition was cured to form a second protective layer (2). The thickness of the second protective layer (2) was 3 μm. In this way, a second laminate (2) having a layer structure of the first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (2) was obtained.
[0209] Except for using the second laminate (2) instead of the second laminate (1), an optical laminate (3) was obtained in the same manner as in Example 1. The layer structure of the optical laminate (3) was the surface protective film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (2) / first pressure-sensitive adhesive layer (1) / separator (1).
[0210] Example 4 An optical laminate (4) was obtained in the same manner as in Example 1, except that a cycloolefin polymer (COP) film (ZF14-023, manufactured by Zeon Corporation, thickness 23 μm) was used as the first protective layer (2) instead of the first protective layer (1), and the optically absorptive anisotropic layer-forming composition (2) was used instead of the optically absorptive anisotropic layer-forming composition (1). The optically absorptive anisotropic layer (2) had a thickness of 1.0 μm. The layer structure of the optical laminate (4) was the surface protective film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (2) / optically absorptive anisotropic layer (2) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0211] Example 5 An optical laminate (5) was obtained in the same manner as in Example 4, except that a cycloolefin polymer (COP) film (ZF14-023, manufactured by Zeon Corporation, thickness 13 μm) was used as the first protective layer (3) instead of the first protective layer (2). The layer structure of the optical laminate (5) was surface protection film (1) (stretched PET film / second pressure-sensitive adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0212] Example 6 Except for using the surface protective film (2) instead of the surface protective film (1), an optical laminate (6) was obtained in the same manner as in Example 5. The layer structure of the optical laminate (6) was the surface protective film (2) (stretched PET film (2) / second pressure-sensitive adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0213] Example 7 Except for using the surface protective film (3) instead of the surface protective film (1), an optical laminate (7) was obtained in the same manner as in Example 5. The layer structure of the optical laminate (7) was the surface protective film (3) (stretched PET film (3) / second pressure-sensitive adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0214] Example 8 Except for using the separator with an adhesive layer (2) instead of the separator with an adhesive layer (1), an optical laminate (8) was obtained in the same manner as in Example 7. The layer structure of the optical laminate (8) was the surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (2) / separator (2).
[0215] Example 9 (Preparation of first protective layer (4) with stretched PET film) The following components were mixed and stirred at 50° C. for 4 hours to obtain a composition for forming a hard coat layer (hereinafter also referred to as “composition for forming an HC layer”). Polyfunctional acrylate compound having the following structure (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester A-DPH" (dipentaerythritol hexaacrylate): 50 parts [ka] Urethane acrylate polymer (Daicel-Allnex Corporation, "Ebecryl 4858", functional group number: 2, weight average molecular weight: 450, functional group number per unit molecular weight: 44.4 × 10 -4 ):50 copies Radical polymerization initiator (BASF, "Irgacure 907" (2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane)): 3 parts Solvent (methyl ethyl ketone): 10 parts
[0216] After a corona treatment was performed on the release-treated surface of a release-treated stretched PET film (SP-PLR382050 manufactured by Lintec Corporation), the above-prepared composition for forming an HC layer was applied by a bar coating method (#2 30 mm / s). The obtained coating film of the composition for forming an HC layer was exposed to light at a dose of 500 mJ / cm using a UV irradiation device (SPOT CURE SP-7 manufactured by Ushio Inc.). 2 By irradiating the film with ultraviolet light (365 nm standard), a hard coat layer having a thickness of 2 μm was formed, and this hard coat layer was used as the first protective layer (4). The thickness was measured using a laser microscope (OLS3000 manufactured by Olympus Corporation). As a result, a first protective layer (3) with a stretched PET film having a layer structure of stretched PET film / first protective layer (4) was obtained.
[0217] A first laminate (2) was obtained in the same manner as in the preparation of the first laminate (1) described in Example 1, except that a first protective layer (4) with a stretched PET film was used instead of the first protective layer (1) and a composition for forming an optically absorptive anisotropic layer (3) was used instead of the composition for forming an optically absorptive anisotropic layer (1). The thickness of the optically absorptive anisotropic layer (3) was 1.0 μm. The first laminate (2) has a layer structure of a first protective layer (4) with a stretched PET film (stretched PET film / first protective layer (4)) / optically absorptive anisotropic layer (3).
[0218] Except for using the first laminate (2) instead of the first laminate (1), a second laminate (3) was obtained by the procedure described in Example 1. The second laminate (3) has a layer structure of a first protective layer (4) with a stretched PET film (stretched PET film / first protective layer (4)) / light absorption anisotropic layer (3) / second protective layer (1).
[0219] The second protective layer (1) side of the second laminate (3) was bonded to the first pressure-sensitive adhesive layer (1) side of the separator (1) with a pressure-sensitive adhesive layer, and then the stretched PET film of the second laminate (3) was peeled off and removed. The first protective layer (4) thus exposed was bonded to the second pressure-sensitive adhesive layer (1) side of the surface protective film (1) to obtain an optical laminate (9). The layer structure of the optical laminate (9) was the surface protective film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0220] Example 10 Except for using a surface protective film (3) instead of the surface protective film (1) and a separator with an adhesive layer (2) instead of the separator with an adhesive layer (1), an optical laminate (10) was obtained in the same manner as in Example 9. The layer structure of the optical laminate (10) was the surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first adhesive layer (2) / separator (2).
[0221] Example 11 After the release force adjusting layer (1) of the surface protective film (4) was subjected to a corona treatment, the above-prepared HC layer-forming composition was applied by a bar coating method (#2 30 mm / s). The obtained coating film of the HC layer-forming composition was exposed to a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) at an exposure dose of 500 mJ / cm. 2 A hard coat layer having a thickness of 2 μm was formed by irradiating the film with ultraviolet light (365 nm standard), and this hard coat layer was used as the first protective layer (4). The thickness was measured using a laser microscope (OLS3000, manufactured by Olympus Corporation). As a result, a first protective layer (4) with a surface protective film (4) having a layer structure of surface protective film (4) / first protective layer (4) was obtained.
[0222] The optically absorbing anisotropic layer (3) was formed on the first protective layer (4) with the surface protective film (4) instead of the first protective layer (1) by the procedure described in Example 9. After corona treatment was performed on the surface of the optically absorbing anisotropic layer (3) opposite to the first protective layer (4), the water-soluble polymer-containing resin composition prepared above was applied using a bar coater and dried at a temperature of 100°C for 2 minutes to form a second protective layer (1) having a thickness of 1 μm made of a water-soluble polymer film. This second protective layer (1) and the first adhesive layer (1) of the separator (3) with an adhesive layer were bonded to obtain an optical laminate (11). The layer structure of the optical laminate (11) was the surface protective film (4) (stretched PET film) / first protective layer (4) / optically absorbing anisotropic layer (3) / second protective layer (1) / first adhesive layer (1) / separator (3).
[0223] Example 12 Except for using a surface protective film (5) instead of the surface protective film (4) and a separator with an adhesive layer (1) instead of the separator with an adhesive layer (3), an optical laminate (12) was obtained in the same manner as in Example 11. The layer structure of the optical laminate (12) was surface protective film (5) (stretched PET film) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first adhesive layer (1) / separator (1).
[0224] Comparative Example 1 Except for using the surface protective film (6) instead of the surface protective film (5) and the composition for forming an optically absorptive anisotropic layer (1) instead of the composition for forming an optically absorptive anisotropic layer (3), an optical laminate (c1) was obtained in the same manner as in Example 12. The layer structure of the optical laminate (c1) was the surface protective film (6) (stretched PET film) / first protective layer (4) / optically absorptive anisotropic layer (1) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0225] Comparative Example 2 An optical laminate (c2) was obtained in the same manner as in Example 10, except that, when bonding the second pressure-sensitive adhesive layer (1) of the surface protective film (3) and the first protective layer (4) together, the bonding surfaces were subjected to a corona treatment, the composition for forming a light-absorbing anisotropic layer (1) was used instead of the composition for forming a light-absorbing anisotropic layer (3), and the separator with a pressure-sensitive adhesive layer (4) was used instead of the separator with a pressure-sensitive adhesive layer (2). The layer structure of the optical laminate (c2) was the surface protective film (3) (stretched PET film (3) / second pressure-sensitive adhesive layer (1)) / first protective layer (4) / light-absorbing anisotropic layer (1) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (4).
[0226] [Reference example 1] (Preparation of composition for forming photoalignment layer) The following components described in JP2013-033249A were mixed, and the resulting mixture was stirred at 80°C for 1 hour to obtain a composition for forming a photoalignment layer. Photoalignment polymer having the structure shown below: 2 parts [ka] Solvent (o-xylene): 98 parts
[0227] (Formation of photo-alignment layer) After a corona treatment was applied to the surface of a cycloolefin polymer (COP) film (ZF14-050, manufactured by Zeon Corporation, thickness 50 μm) as the first protective layer (5), the composition for forming a photo-alignment layer prepared above was applied and dried at a temperature of 120° C. to obtain a dry film. A photo-alignment layer was formed by irradiating polarized UV onto this dry film, and a film with a photo-alignment layer was obtained. The polarized UV treatment was performed using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) under the condition that the intensity measured at a wavelength of 365 nm was 100 mJ. The thickness of the photo-alignment layer was 100 nm.
[0228] The composition for forming an optically absorbing anisotropic layer (3) was applied onto the optical alignment layer of the film with the optical alignment layer using a bar coater, and the polymerizable liquid crystal compound was subjected to phase transition to a liquid phase by heating and drying in a drying oven at a temperature of 120°C for 1 minute, and then cooled to room temperature to cause the polymerizable liquid crystal compound to undergo phase transition to a smectic liquid crystal state. Next, the composition was exposed to light at a dose of 1000 mJ / cm using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 By irradiating the layer formed from the composition for forming an optically absorbing anisotropic layer (3) with ultraviolet light of wavelengths of 365 nm (based on 365 nm), the polymerizable liquid crystal compound contained in the dried film was polymerized while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, forming an optically absorbing anisotropic layer (4) oriented horizontally. After corona treatment was performed on the optically absorbing anisotropic layer (4), the water-soluble polymer-containing resin composition prepared above was applied using a bar coater and dried at a temperature of 100° C. for 2 minutes to form a second protective layer (1) having a thickness of 1 μm, which was made of a water-soluble polymer film. Furthermore, the first adhesive layer (1) of the separator with an adhesive layer (1) was laminated to the surface protective film (1) to obtain an optical laminate (r1). The layer structure of the optical laminate (r1) was: surface protection film (1) (stretched PET film (1) / second pressure-sensitive adhesive layer (1)) / first protective layer (5) (COP film) / photoalignment layer / light absorption anisotropic layer (4) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0229] [Reference example 2] A corona treatment was performed on the first protective layer (2) (COP film, ZF14-023), and the composition for forming a light absorption anisotropic layer (4) was applied thereon using a bar coater and heated at 120°C for 60 seconds. After that, ultraviolet light was irradiated from the applied surface using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (integrated light amount at a wavelength of 365 nm in a nitrogen atmosphere: 500 mJ / cm2). 2 ) to form an optically absorptive anisotropic layer (5). The thickness of the optically absorptive anisotropic layer (5) was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 1.2 μm.
[0230] An optical laminate (r2) was obtained in the same manner as in Example 1, except that a surface protective film (3) was used instead of the surface protective film (1), and a laminate in which an optically absorbing anisotropic layer (5) was formed on the first protective layer (2) obtained above was used instead of the laminate of the first protective layer (1) and the optically absorbing anisotropic layer (1). The layer structure of the optical laminate (r2) was the surface protective film (3) (stretched PET film (3) / second pressure-sensitive adhesive layer (1)) / first protective layer (2) / optically absorbing anisotropic layer (5) / second protective layer (1) / first pressure-sensitive adhesive layer (1) / separator (1).
[0231] [Thickness measurement] The thickness was measured using a contact type film thickness gauge or a laser microscope (OLS3000, manufactured by Olympus Corporation).
[0232] [Measurement of distance D] In the optical laminate, the distance D from the surface of the first protective layer on the surface protection film side to the surface of the second protective layer on the first pressure-sensitive adhesive layer side was measured from the layer cross section using a laser microscope (OLS3000 manufactured by Olympus Corporation). The results are shown in Tables 1 to 3.
[0233] [Measurement of absorbance] The laminated structure of the first protective layer / light absorption anisotropic layer / second protective layer of the optical laminate was attached to a glass of 4 cm x 4 cm x 0.7 mm thickness via a pressure-sensitive adhesive (manufactured by Lintec Corporation) with a thickness of 25 μm, and this was used as a test piece (1). The laminated structure was arranged with the second protective layer side on the glass side. In Reference Example 1, the laminated structure of the COP film / photo-alignment layer / light absorption anisotropic layer (r1) of the optical laminate was attached to the glass side via the pressure-sensitive adhesive to obtain a test piece (1). The test piece (1) was set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation's "UV-2450") to measure the absorbance, and Ax and Ax (z = 60) were determined. Since the absorbance of the first protective layer and the second protective layer can be regarded as 0 (zero), Ax and Ax(z=60) measured for the measurement sample (1) can be said to be the absorbance of the light absorption anisotropic layer. The results are shown in Tables 1 to 3.
[0234] The x-axis represents an arbitrary direction in the plane of the optically absorptive anisotropic layer, the y-axis represents a direction perpendicular to the x-axis in the film plane, and the z-axis represents the thickness direction of the optically absorptive anisotropic layer. Ax represents the absorbance at the maximum absorption wavelength of the optically absorptive anisotropic layer, and the absorbance of linearly polarized light oscillating in the x-axis direction. Ax (z=60) represents the absorbance at the maximum absorption wavelength when the optically absorptive anisotropic layer is rotated 60° around the y-axis as the rotation axis, and the absorbance of linearly polarized light oscillating in the x-axis direction.
[0235] When measuring the absorbance, the test piece (1) was set in an ultraviolet-visible spectrophotometer (Shimadzu Corporation, "UV-2450"), and Ax was measured after correcting the absorbance at a wavelength of 800 nm to zero. For Ax (z = 60), the test piece (1) was set and tilted in the same manner, and Ax (z = 60) was measured after correcting the absorbance at a wavelength of 800 nm to zero.
[0236] Whether the optically absorptive anisotropic layer satisfied the relationship of the above formula (1) (Az>(Ax+Ay) / 2) was determined by the following procedure. With the test piece (1) rotated 30° and 60° so as to include the y-axis, Ax(z=30°) and Ax(z=60°) were measured by incidenting the same linearly polarized light as used to measure Ax. Similarly, with the test piece (1) rotated 30° and 60° so as to include the x-axis, Ay(z=30°) and Ay(z=60°) were measured by incidenting the same linearly polarized light as used to measure Ay. When there is no absorption anisotropy in the xy plane, i.e., when Ax and Ay are equal, Ax(z=30°)=Ay(z=30°) and Ax(z=60°)=Ay(z=60°), so Ax(z=30°) and Ay(z=30°) were defined as A(z=30°), Ax(z=60°) and Ay(z=60°) were defined as A(z=60), and Ax(z=90°) and Ay(z=90°) were defined as A(z=90). When in the relationship of A(z = 30°) < A(z = 60°), in order to satisfy the relationship of A(z = 30°) < A(z = 60°) < A(z = 90°) = Az, if A(z = 30°) > (Ax + Ay) / 2 or A(z = 60°) > (Ax + Ay) / 2, it was determined that the relationship of the above formula (1) was satisfied. The results are shown in Tables 1 to 3.
[0237] [Measurement of Peel Forces F1 and F2] Using a test piece (2) cut out from the optical laminate to a size of 25 mm in width × 100 mm in length, the peel forces F1 and F2 were measured according to the following procedure. The results are shown in Tables 1 to 3.
[0238] (Measurement of Peel Force F1) The separator was peeled from the test piece (2), and the exposed first adhesive layer was attached to a glass substrate. Then, the surface protection film was peeled 50 mm from the end in the length direction. In this state, during the low-speed peeling test, one end in the length direction of the test piece (2) was clamped with the upper and lower grips of a tensile testing machine (AUTOGRAPH AG-1S testing machine, manufactured by Shimadzu Corporation), and the glass substrate was clamped with the other grip part, and in an environment of a temperature of 23°C and a relative humidity of 50%, it was pulled in the 180° direction at a tensile speed of 300 mm / min to peel, and the peel force at that time was recorded on a chart. During the high-speed peeling test, using a high-speed peeling tester (VPA-H100, manufactured by Kyowa Interface Science), one end in the length direction (one side with a width of 25 mm) of the surface protection film peeled above was clamped with one grip part of the high-speed peeling tester, and the glass substrate was clamped with the other grip part of the high-speed peeling tester, and under the conditions of a temperature of 23°C and a relative humidity of 50%, it was pulled in the 180° direction at a peeling speed of 10,000 mm / min to peel, and the peel force at that time was recorded on a chart. Since the data is not stable immediately after the start of measurement and immediately before the end of measurement, 20% of the data after the start of measurement and 20% of the data before the end of measurement were cut, and the average value was calculated only from the 60% range of the relatively stable middle part, and this was taken as the peel force F1 [N / 25 mm].
[0239] (Measurement of Peel Force F2) A 25 mm wide x 22 cm long double-sided tape (Nicetack (trade name), manufactured by Nichiban Co., Ltd.) was attached to the entire surface of one side of a glass substrate (EAGLE XG, manufactured by Corning Incorporated) in parallel with the long side direction, and the surface of the surface protection film side of the test piece (2) was attached. Then, the separator was peeled off 50 mm from the end in the length direction. In this state, the separator was peeled off from the first adhesive layer in the same manner as in the measurement of the peel force F1, and the peel force at that time was recorded on a chart. Since the data was not stable immediately after the start of the measurement and immediately before the end of the measurement, the data for 20% after the start of the measurement and the data for 20% after the end of the measurement were cut, and the average value was calculated only from the relatively stable intermediate 60% range, and this was taken as the peel force F2 [N / 25 mm].
[0240] [Evaluation of peelability] The optical laminate was cut into a size of 2.5 cm x 20 cm to prepare a test piece (3). The surface protective film side of the test piece (3) was placed on a suction stage and fixed by vacuum suction. In this state, the separator was peeled off in the 180° direction along the long side of the test piece (3) at a low peeling speed (about 300 mm / min) and a high peeling speed (about 10,000 mm / min), and the releasability and appearance after peeling at each peeling speed were evaluated according to the following criteria. A: There is no abnormality in peelability, and no abnormality in appearance after peeling. B: When peeling the separator, the surface protection film side may lift off the suction stage. However, if you stop peeling the separator and then start peeling again, it can be peeled off smoothly and there is no abnormality in the appearance after peeling. C: When the separator is peeled off, the surface protective film side may float from the suction stage. In addition, crack-like stripes may occur in any of the first protective layer, the light absorption anisotropic layer, the second protective layer, and the first pressure-sensitive adhesive layer of the optical laminate. D: When peeling off the separator, the surface protective film side floats off the suction stage, making it impossible to peel off the separator. In addition, numerous crack-like stripes may appear on any of the first protective layer, the light absorption anisotropic layer, the second protective layer, and the first pressure-sensitive adhesive layer of the optical laminate, leading to breakage.
[0241] [Flexibility test] The optical laminate was cut into a size of 100 mm in length × 10 mm in width using a super cutter to obtain a test piece (4). A bending test of the test piece (4) was performed by a cylindrical mandrel method using a bending resistance tester (manufactured by TR Giken Co., Ltd.). In the bending test, the test piece (4) was wrapped around a cylindrical mandrel with a diameter of 2 mm so that the surface protection film was on the inside, and the long side of the test piece (4) was bent at a temperature of 25°, and then the test piece was returned to its state before bending, and the visibility at the bent part was confirmed and evaluated according to the following criteria. A: No decrease in visibility was observed in the bent portion of the test piece (4) before and after the bending test. B: A slight decrease in visibility of the bent portion of the test piece (4) was confirmed before and after the bending test. C: A decrease in visibility of the bent portion of the test piece (4) was confirmed before and after the bending test.
[0242] [Table 1]
[0243] [Table 2]
[0244] [Table 3] [Explanation of symbols]
[0245] 10 optical laminate, 11 surface protective film, 12 first protective layer, 13 light absorption anisotropic layer, 14 second protective layer, 15 first pressure-sensitive adhesive layer, 16 separator.
Claims
1. An optical laminate comprising a surface protective film, a first protective layer, a light absorption anisotropic layer, a second protective layer, a first pressure-sensitive adhesive layer, and a separator laminated in this order, The surface protective film and the separator each include a stretched polyester film, The light absorption anisotropic layer contains a polymer of a polymerizable liquid crystal compound and a dichroic dye, and satisfies the relationships of the following formulas (1) to (3): a peel force F1 [N / 25 mm] between the surface protective film and the first protective layer, and a peel force F2 [N / 25 mm] between the separator and the first pressure-sensitive adhesive layer satisfy the relationships of the following formulas (4) to (6), An optical laminate, wherein the distance from a surface of the first protective layer on the surface protection film side to a surface of the second protective layer on the first pressure-sensitive adhesive layer side is 30 μm or less. Az>(Ax+Ay) / 2 (1) 0.001≦Ax≦0.1 (2) Ax (z=60°) / Ax≧5 (3) 0.05≦F1≦0.30 (4) 0.02≦F2≦0.15 (5) 0.02≦F1-F2 (6) [In formulas (1) to (3), Ax, Ay, and Az are the absorbances of the optically absorptive anisotropic layer at the maximum absorption wavelength in the wavelength range of 380 nm or more and 780 nm or less, and represent the absorbances of linearly polarized light vibrating in the x-axis direction, y-axis direction, and z-axis direction, respectively. Ax (z=60°) is the absorbance at the maximum absorption wavelength, and represents the absorbance of linearly polarized light vibrating in the x-axis direction when the optically absorptive anisotropic layer is rotated 60° around the y-axis as the rotation axis. Here, the x-axis is any one direction within the plane of the optically absorptive anisotropic layer, the y-axis is a direction perpendicular to the x-axis in the plane of the optically absorptive anisotropic layer, The z-axis is a direction perpendicular to the x-axis and the y-axis.
2. 2. The optical laminate according to claim 1, wherein the stretched polyester film included in the surface protective film has a thickness of 30 μm or more.
3. 2. The optical laminate according to claim 1, wherein the thickness of the stretched polyester film included in the separator is 30 μm or more.
4. The optical laminate according to claim 1 , wherein the surface protective film is a laminate of a stretched polyester film and a second pressure-sensitive adhesive layer.
5. The optical laminate according to claim 1 , wherein the surface protective film and the stretched polyester film included in the separator are both biaxially stretched polyester films.
6. The optical laminate according to claim 1 , wherein the surface protective film and the first protective layer are in direct contact with each other.
7. The optical laminate according to claim 1 , wherein the first protective layer and the optically absorptive anisotropic layer are in direct contact with each other, or only an alignment layer is provided between the first protective layer and the optically absorptive anisotropic layer.
8. The optical laminate according to claim 1 , wherein the optically absorptive anisotropic layer and the second protective layer are in direct contact with each other.
9. The optical laminate according to claim 1 , wherein the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.
10. The optical laminate according to claim 1 , wherein the first protective layer has a thickness of 28 μm or less.
11. The optical laminate according to claim 1 , wherein the second protective layer has a thickness of 15 μm or less.
12. A wound body obtained by winding the optical laminate according to any one of claims 1 to 11.
Citation Information
Patent Citations
Vertically aligned liquid crystal cured film and laminate including the same
JP2020076920A