Active energy ray-curable composition, adhesive, and adhesive sheet
A polyester-based active energy ray-curable composition addresses thermal stability issues in solvent-free adhesives by using specific structural units and photoreactive compounds, ensuring excellent curability and adhesive strength for applications like adhesive tapes and labels.
Patent Information
- Application Number
- JP2024053845
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-15
AI Technical Summary
Existing solvent-free adhesives face issues with thermal stability and adhesive performance due to the inclusion of unsaturated groups that react with heat during high-temperature processes, leading to viscosity increase and gelation, which compromises their suitability for applications like hot melt coating.
A polyester-based active energy ray-curable composition is developed, containing specific structural units derived from polyhydric carboxylic acid and polyhydric alcohol, along with a photoreactive compound lacking unsaturated groups, to enhance thermal stability and adhesive strength without relying on crosslinking agents.
The composition achieves excellent active energy ray curability, thermal stability, and adhesive strength, making it suitable for solvent-free adhesive tapes and labels with improved performance in high-temperature processes.
Smart Images

Figure 2024146887000001 
Figure 2024146887000002 
Figure 2024146887000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray-curable composition, and an adhesive and an adhesive sheet which are cured products of the active energy ray-curable composition. More specifically, the present invention relates to an active energy ray-curable composition, an adhesive, and an adhesive sheet which have excellent curability by active energy rays without having an unsaturated group, and further an adhesive sheet produced using the same has excellent thermal stability, adhesive strength, and holding strength. [Background technology]
[0002] Conventionally, polyesters have been used in a wide range of applications, such as films, PET bottles, fibers, toners, electrical components, adhesives, pressure sensitive adhesives, etc., because of their excellent heat resistance, chemical resistance, durability, and mechanical strength. In addition, polyesters have high polarity due to their polymer structure, and are known to exhibit excellent adhesion to polar polymers such as polyester, polyvinyl chloride, polyimide, and epoxy resin, as well as to metal materials such as copper and aluminum.
[0003] Solvent-based adhesives, in which adhesive polymers are dissolved in a solvent, have been used as adhesives for use in adhesive sheets such as adhesive labels and adhesive tapes. In recent years, solvent-free adhesives that do not use organic solvents have been attracting attention as a way to reduce environmental impact, such as VOC (Volatile Organic Compounds) regulations and greenhouse gas emissions. Solvent-free adhesives include water-based adhesives in which adhesives are dispersed or dissolved in water, and active energy ray-curable adhesives that are cured by active energy rays such as ultraviolet rays. Water-based adhesives have problems in terms of performance, such as the amount of energy used to volatilize water being larger than that of solvent-based adhesives, and poorer water resistance than solvent-based adhesives due to the influence of the emulsifier contained in the main agent. In addition, active energy ray-curable adhesives require the incorporation of unsaturated groups into the structure that react with active energy rays to become crosslinking points in order to increase the cohesive force of the adhesive, or the inclusion of compounds having unsaturated groups in the adhesive, and there are problems with thermal stability, such as the reaction of unsaturated groups due to heating in hot melt coating, which increases the viscosity and causes gelation. For this reason, solvent-free adhesives used in hot melt coating are required to have high thermal stability and adhesive performance equal to or greater than that of solvent-based adhesives.
[0004] Patent Document 1 discloses a photocrosslinkable polyester-based pressure-sensitive adhesive composition comprising a polyester having an unsaturated group, a photoinitiator, and a crosslinking agent.
[0005] Furthermore, Patent Document 2 discloses a photocrosslinking pressure sensitive adhesive for optical members, which comprises a polyester, an unsaturated group-containing compound, a polymerization initiator, and a crosslinking agent.
[0006] Patent Document 3 discloses a radiation-cured removable pressure-sensitive adhesive sheet comprising a polyester, a radiation-curable resin having an unsaturated group, a radiation reaction initiator, and a crosslinking agent.
[0007] Furthermore, Patent Document 4 discloses an ultraviolet-curable composition comprising an epoxidized oil having an ultraviolet-active site and a polyvalent carboxylic acid. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-102476 A [Patent Document 2] JP 2009-209279 A [Patent Document 3] JP 2010-59336 A [Patent Document 4] Special Publication No. 2022-535379 Summary of the Invention [Problem to be solved by the invention]
[0009] In recent years, there has been a demand for environmentally friendly adhesives, such as biomass adhesives using plant-derived raw materials and solvent-free adhesives that do not use organic solvents, in order to reduce the environmental impact. Conventionally used heat-curing adhesives are made from petroleum-based raw materials and are diluted with organic solvents, which poses issues regarding the environmental impact of generating VOCs that can cause environmental pollution and emitting CO2 when burned and disposed of.
[0010] In addition, conventionally used active energy ray-curable adhesives have required the introduction of unsaturated groups into the adhesive as active energy ray-curable components, the incorporation of unsaturated group-containing compounds, and the inclusion of thermosetting crosslinking agents, etc. Since the reaction of unsaturated groups and crosslinking agent components proceeds due to heat, their use in solventless adhesive applications involving high-temperature heating processes such as hot melts has been difficult due to problems with thermal stability, such as an increase in viscosity during the manufacturing process, gelation, and thermal decomposition.
[0011] For example, Patent Document 1 discloses a technique related to a polyester-based photocrosslinkable pressure-sensitive adhesive composition, and since the polyester has an unsaturated group derived from a (meth)acrylate as a photocrosslinking component, there remains a problem with thermal stability.
[0012] In addition, Patent Document 2 discloses a technology related to a photo- and / or thermally crosslinkable pressure-sensitive adhesive for optical components, and since an unsaturated group-containing compound and a thermosetting crosslinking agent are used as the pressure-sensitive adhesive composition, crosslinking proceeds due to heat, so there is a problem with thermal stability and there is room for improvement in suitability for hot melt coating.
[0013] Patent Document 3 discloses a technology relating to a radiation-curable removable pressure-sensitive adhesive sheet, which contains a large amount of a radiation-curable resin having an unsaturated group, and therefore has problems remaining with respect to thermal stability and adhesive strength.
[0014] Patent Document 4 discloses a technology relating to an ultraviolet-curable composition consisting of an epoxidized oil having an ultraviolet-active site and a polyvalent carboxylic acid. Although the composition does not contain an unsaturated group as an active energy ray-curable component, the composition contains an epoxy group, which reacts with a carboxyl group due to heat and undergoes ring-opening polymerization of the epoxy group, so that the composition has problems with thermal stability at high temperatures and optical properties, such as the adhesive sheet easily turning yellow due to the epoxy group.
[0015] In view of the above background, an object of the present invention is to provide an active energy ray-curable composition having excellent adhesive strength, holding power and thermal stability, and an adhesive and an adhesive sheet obtained by curing the active energy ray-curable composition. [Means for solving the problem]
[0016] However, the present inventors have conducted extensive research in light of the above circumstances, and as a result have found that by using an active energy ray-curable composition containing a polyester (A) having a structural unit (α) derived from a polyvalent carboxylic acid and a structural unit (β) derived from a polyhydric alcohol, and a compound (B) having a photoreactive group, it is possible to obtain an active energy ray-curable composition that is excellent in active energy ray curability and further has excellent thermal stability, adhesive strength, and holding strength without containing unsaturated groups that are a cause of reduced thermal stability, and have thus completed the present invention.
[0017] That is, the gist of the present invention is the following [1] to
[13] . [1] An active energy ray-curable composition comprising a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, The active energy ray-curable composition, wherein the content of the polymerizable unsaturated group-containing compound (C) contained in the active energy ray-curable composition is less than 15 parts by mass based on 100 parts by mass of the polyester (A). [2] The active energy ray-curable composition according to [1], wherein the compound (B) having a photoreactive group is a compound (b1) having a hydrogen abstraction type photoreactive group and / or a compound (b2) having a cleavage type photoreactive group. [3] The active energy ray-curable composition according to [1] or [2], wherein the compound (B) having a photoreactive group is a hydrogen abstraction type photopolymerization initiator. [4] The active energy ray-curable composition according to any one of [1] to [3], wherein the compound (B) having a photoreactive group does not have a carboxy group or a hydroxy group as a functional group. [5] The active energy ray-curable composition according to any one of [1] to [4], wherein the glass transition temperature of the polyester (A) is from −80 to 30° C. [6] The active energy ray-curable composition according to any one of [1] to [5], wherein the polyester (A) has a weight average molecular weight of 5,000 to 500,000. [7] The active energy ray-curable composition according to any one of [1] to [6], wherein the polyester (A) has an unsaturated group concentration of 1 mmol / g or less. [8] The active energy ray-curable composition according to any one of [1] to [7], wherein the polyester resin (A) has an epoxy group concentration of 5 mmol / g or less. [9] The active energy ray-curable composition according to any one of [1] to [8], wherein the melt viscosity change rate before and after heating at 200° C. for 3 hours is 20 to 500%.
[10] The active energy ray-curable composition according to any one of [1] to [9], wherein the content of the organic solvent in the active energy ray-curable composition is less than 70 mass %.
[11] A pressure-sensitive adhesive which is a cured product of the active energy ray-curable composition according to any one of [1] to [9].
[12] The pressure-sensitive adhesive according to
[11] , wherein the pressure-sensitive adhesive has a gel fraction of 1 to 100%.
[13] An adhesive sheet comprising the adhesive according to
[11] or
[12] . Effect of the Invention
[0018] The active energy ray-curable composition of the present invention forms an adhesive having excellent active energy ray curability, thermal stability, adhesive strength, and holding power, and such an active energy ray-curable composition is particularly effective as a solventless adhesive used for adhesive tapes and adhesive labels.
[0019] In general, active energy ray-curable compositions have had to contain an unsaturated group as an active energy ray-curable component in the pressure-sensitive adhesive composition in order to enhance active energy ray curability, adhesive strength, and holding strength. However, because unsaturated groups undergo polymerization reactions due to heat, they cannot be used in the hot-melt process of solvent-free pressure-sensitive adhesives, which requires melting the resin at high temperatures, as this causes an increase in viscosity and gelation, posing issues with thermal stability. In the present invention, by using a pressure-sensitive adhesive composition consisting of a specific polyester and a compound having a photoreactive group, the composition has excellent active energy ray curability without containing unsaturated groups or crosslinking agents that become crosslinking points when exposed to active energy rays, which were previously essential, and further has excellent thermal stability, adhesive strength, and holding power. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The configuration of the present invention will be described in detail below, but these are merely examples of preferred embodiments. In the present invention, the term "class" added after the name of a compound is a concept that includes not only the compound but also derivatives of the compound. For example, the term "carboxylic acids" includes not only carboxylic acids but also carboxylic acid derivatives such as carboxylic acid salts, carboxylic acid anhydrides, carboxylic acid halides, and carboxylic acid esters. In addition, "X and / or Y (X and Y are optional configurations)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y.
[0021] An active energy ray-curable composition according to one embodiment of the present invention (hereinafter referred to as "the composition") contains a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, and the content of the polymerizable unsaturated group-containing compound (C) contained in the composition is less than 15 parts by mass per 100 parts by mass of the polyester (A). Each component contained in the composition will be described below. First, the polyester (A) will be described.
[0022] <Polyester (A)> The polyester (A) contains a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β) in the molecule. Such a polyester (A) is usually obtained by ester bonding between the polyvalent carboxylic acid (α) and the polyvalent carboxylic acid (β).
[0023] The content of the polyester (A) is 50% by mass or more, more preferably 60 to 99.5% by mass, still more preferably 70 to 99% by mass, particularly preferably 80 to 98.5% by mass, and especially preferably 85 to 98% by mass, of the entire composition.
[0024] [Polycarboxylic acid (α)] Examples of the polycarboxylic acid (α) include aliphatic polycarboxylic acids (α1), aromatic polycarboxylic acids (α2), and alicyclic polycarboxylic acids (α3). The polycarboxylic acid (α) may be used alone or in combination. Among them, aliphatic polycarboxylic acids (α1) are preferred because they are excellent in active energy curability and adhesive strength, and can reduce the melt viscosity when the molecular weight is increased, resulting in excellent coating suitability.
[0025] Examples of the aliphatic polyvalent carboxylic acid (α1) include saturated aliphatic dicarboxylic acids (α1-1) such as malonic acids, succinic acids, glutaric acids, adipic acids, trimethyladipic acids, pimelic acids, 3-methylglutaric acids, 2,2-dimethylglutaric acids, azelaic acids, sebacic acids, thiodipropionic acids, diglycolic acids, 1,9-nonanedicarboxylic acids, and hydrogenated dimer acids obtained by dimerizing unsaturated monocarboxylic acids such as oleic acid, linoleic acid, linolenic acid, and erucic acid; and unsaturated aliphatic dicarboxylic acids (α1-2) such as dimer acids obtained by dimerizing unsaturated monocarboxylic acids such as fumaric acids, maleic acids, itaconic acids, oleic acid, linoleic acid, linolenic acid, and erucic acid. Among these, it is preferable to contain a saturated aliphatic dicarboxylic acid (α1-1) because of its excellent thermal stability, and among these, succinic acids, adipic acids, azelaic acids, sebacic acids, and hydrogenated dimer acids are more preferable because of their excellent active energy ray curability, adhesive strength, and coatability.
[0026] Examples of the aromatic polyvalent carboxylic acid (α2) include aromatic dicarboxylic acids such as terephthalic acids, isophthalic acids, orthophthalic acids, naphthalenedicarboxylic acids, biphenyldicarboxylic acids, furandicarboxylic acids, and thiophenedicarboxylic acids, trimellitic acids, trimesic acids, ethylene glycol bis(anhydrotrimellitates), glycerol tris(anhydrotrimellitates), pyromellitic acids, oxydiphthalic acids, 3,3',4,4'-benzophenonetetracarboxylic acids, 3,3',4,4'-diphenyltetracarboxylic acids, 3,3',4,4'-diphenylsulfonetetracarboxylic acids, 4,4'-(hexafluoroisopropylidene)diphthalic acids, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propanes, and other trivalent or higher aromatic carboxylic acids. Among these, aromatic dicarboxylic acids are preferred because they have excellent hydrolysis resistance and cohesive strength, and terephthalic acids, isophthalic acids, orthophthalic acids, naphthalenedicarboxylic acids, and furandicarboxylic acids are more preferred, with isophthalic acids, orthophthalic acids, furandicarboxylic acids, and 3,3',4,4'-benzophenonetetracarboxylic acids being particularly preferred because they reduce the crystallinity of the polyester and provide excellent tackiness and adhesive strength.
[0027] Examples of the alicyclic polyvalent carboxylic acid (α3) include cyclohexanedicarboxylic acids, cyclohexanediacetic acids, tetrahydrophthalic acids, tetrachlorophthalic acids, and hexahydrophthalic acids.
[0028] When the polyester (A) has a structural unit derived from an aliphatic polycarboxylic acid (α1), the content of the structural unit derived from the aliphatic polycarboxylic acid (α1) relative to the structural unit derived from the polycarboxylic acid (α) is preferably 20 mol% or more, more preferably 30 to 100 mol%, even more preferably 40 to 98 mol%, particularly preferably 50 to 95 mol%, particularly preferably 60 to 93 mol%, and most preferably 70 to 90 mol%. If the content of the structural unit derived from the aliphatic polycarboxylic acid (a1) is too small, the active energy ray curability tends to decrease, the melt viscosity tends to increase, the hot melt coating suitability tends to deteriorate, the glass transition temperature tends to increase, and the adhesion and tackiness tend to be insufficient, while if it is too large, the cohesive force tends to be insufficient and the holding power tends to be insufficient.
[0029] When the polyester (A) has a structural unit derived from a saturated aliphatic dicarboxylic acid (α1-1), the content of the structural unit derived from the saturated aliphatic dicarboxylic acid (α1-1) relative to the structural unit derived from the polyvalent carboxylic acid (α) is preferably 20 mol% or more, more preferably 30 to 100 mol%, even more preferably 40 to 98 mol%, particularly preferably 50 to 95 mol%, particularly preferably 60 to 93 mol%, and most preferably 70 to 90 mol%. If the content of the structural unit derived from the saturated aliphatic dicarboxylic acid (α1-1) is too small, the active energy ray curability decreases, the melt viscosity increases, the hot melt coating suitability deteriorates, or the glass transition temperature increases, resulting in insufficient adhesion and tackiness, while if it is too large, the cohesive force tends to be insufficient and the holding power tends to be insufficient.
[0030] When the polyester (A) has a structural unit derived from an unsaturated aliphatic dicarboxylic acid (α1-2), the content of the structural unit derived from the unsaturated aliphatic dicarboxylic acid (α1-2) relative to the structural unit derived from the polyvalent carboxylic acid (α) is preferably 30 mol% or less, more preferably 15 mol% or less, even more preferably 10 mol% or less, particularly preferably 5 mol% or less, especially preferably 3 mol% or less, and most preferably 0 mol% or less. If the content of the structural unit derived from the unsaturated aliphatic dicarboxylic acid (α1-2) is too high, the thermal stability tends to be insufficient.
[0031] When the polyester (A) has a structural unit derived from an aromatic polycarboxylic acid (α2), the content of the structural unit derived from the aromatic polycarboxylic acid (α2) relative to the structural unit derived from the polycarboxylic acid (α) is preferably 80 mol% or less, more preferably 1 to 60 mol%, even more preferably 3 to 50 mol%, particularly preferably 5 to 40 mol%, and particularly preferably 10 to 30 mol%. If the content of the structural unit derived from the aromatic polycarboxylic acid (α2) is too small, the cohesive force tends to be insufficient, and the holding power, heat resistance, and moist heat resistance tend to be insufficient, while if it is too large, the active energy ray curability tends to decrease, the melt viscosity tends to increase, the hot melt coating suitability tends to deteriorate, and the glass transition temperature tends to increase, resulting in insufficient tackiness and adhesive strength.
[0032] When the polyester (A) has a structural unit derived from an alicyclic polycarboxylic acid (α3), the structural unit derived from the alicyclic polycarboxylic acid (α3) relative to the structural unit derived from the polycarboxylic acid (α) is preferably 80 mol% or less, more preferably 1 to 60 mol%, even more preferably 3 to 50 mol%, particularly preferably 5 to 40 mol%, and especially preferably 10 to 30 mol%. If the content of the structural unit derived from the alicyclic polycarboxylic acid (α3) is too small, the cohesive force tends to be insufficient, and the holding power, heat resistance, and moist heat resistance tend to be insufficient, while if it is too large, the active energy ray curability tends to decrease, the melt viscosity tends to increase, the suitability for hot melt coating tends to deteriorate, and the glass transition temperature tends to increase, resulting in insufficient tackiness and adhesive strength.
[0033] The content ratio (molar ratio) of the structural units derived from an aliphatic polycarboxylic acid (α1) to the structural units derived from an aromatic polycarboxylic acid (α2) in the structural units derived from a polycarboxylic acid (α) is preferably, i.e., the structural units derived from an aliphatic polycarboxylic acid (a1) / the structural units derived from an aromatic polycarboxylic acid (a2), from 100 / 0 to 20 / 80, more preferably 99 / 1 to 40 / 60, particularly preferably 97 / 3 to 50 / 50, even more preferably 95 / 5 to 60 / 40, particularly preferably 93 / 7 to 65 / 35, and most preferably 90 / 10 to 70 / 30.
[0034] In addition, the content ratio (molar ratio) of the structural units derived from an aliphatic polycarboxylic acid (α1) and the structural units derived from an alicyclic polycarboxylic acid (α3) in the structural units derived from a polycarboxylic acid (α) is preferably, i.e., structural units derived from an aliphatic polycarboxylic acid (α1) / structural units derived from an alicyclic polycarboxylic acid (α3), from 100 / 0 to 20 / 80, more preferably 99 / 1 to 40 / 60, particularly preferably 97 / 3 to 50 / 50, even more preferably 95 / 5 to 60 / 40, particularly preferably 93 / 7 to 65 / 35, and most preferably 90 / 10 to 70 / 30.
[0035] The polyester (A) may contain, as a structural unit derived from a polyvalent carboxylic acid (α), for example, a structural unit derived from an aromatic dicarboxylic acid having a sulfonic acid group, such as sulfoterephthalic acids, 5-sulfoisophthalic acids, 4-sulfophthalic acids, 4-sulfonaphthalene-2,7-dicarboxylic acids, or 5(4-sulfophenoxy)isophthalic acids, and a structural unit derived from an aromatic dicarboxylate having a sulfonate group, such as a metal salt or ammonium salt thereof. From the viewpoint of the wet heat resistance of the polyester (A), the content of the structural units derived from the polyvalent carboxylic acid (α) is preferably 10 mol % or less, more preferably 5 mol % or less, particularly preferably 3 mol % or less, even more preferably 1 mol % or less, and most preferably 0 mol %.
[0036] [Polyhydric alcohol (β)] Examples of the polyhydric alcohol (β) include aliphatic polyhydric alcohol (β1), alicyclic polyhydric alcohol, and aromatic polyhydric alcohol. One or more types of polyhydric alcohol (β) can be used. Among them, aliphatic polyhydric alcohol (β1) is preferred because it has excellent active energy curability and adhesive strength, and can reduce the melt viscosity when the molecular weight is increased, resulting in excellent coating suitability.
[0037] Examples of the aliphatic polyhydric alcohol (β1) include linear aliphatic polyhydric alcohols (β1-1) such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and 1,10-decanediol; 1,2-propylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-ethyl-2-butylpropanediol, and the like. Examples of the dimer acids include dimer diol, which is a reduction product of dimer acids derived by dimerizing unsaturated monocarboxylic acids such as pentanediol, oleic acid, linoleic acid, linolenic acid, and erucic acid; and branched aliphatic polyhydric alcohols (β1-2) having a hydrocarbon group on at least one side chain, such as 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. Among these, linear aliphatic polyhydric alcohols (β1-1) are preferred because they lower the glass transition temperature and have excellent adhesive strength and tackiness, and ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,5-pentanediol are more preferred, with ethylene glycol, 1,3-propanediol, and 1,4-butanediol being particularly preferred. Among these, from the viewpoints of excellent active energy ray curability, hydrolysis resistance, and excellent tackiness due to reduced crystallinity, branched aliphatic polyhydric alcohols (β1-2) having a hydrocarbon group in at least one side chain are preferred, and particularly preferred are 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, dimer diol, and trimethylolpropane.
[0038] When the polyester (A) has a structural unit derived from a linear aliphatic polyhydric alcohol (β1-1), the content of the structural unit derived from a linear aliphatic polyhydric alcohol (b1-1) relative to the structural unit derived from the polyhydric alcohol (β) is preferably 10 to 100 mol%, more preferably 20 to 95 mol%, particularly preferably 30 to 90 mol%, even more preferably 35 to 85 mol%, and particularly preferably 40 to 80 mol%. If the content of the structural unit derived from a linear aliphatic polyhydric alcohol (β1-1) is too small, the adhesive strength, tackiness, and substrate adhesion tend to be insufficient, and if it is too large, the crystallinity of the polyester increases, and the adhesive strength, tackiness, and active energy ray curability tend to be insufficient.
[0039] When the polyester (A) has a structural unit derived from a branched aliphatic polyhydric alcohol (β1-2) having a hydrocarbon group in at least one side chain, the structural unit derived from the branched aliphatic polyhydric alcohol (β1-2) is preferably 5 to 100 mol%, more preferably 10 to 90 mol%, particularly preferably 15 to 80 mol%, further preferably 20 to 70 mol%, and particularly preferably 25 to 60 mol% relative to the structural unit derived from the polyhydric alcohol (β). If the content of the structural unit derived from the branched aliphatic polyhydric alcohol (β1-2) is too low, the crystallinity of the polyester tends to be high, and the adhesive strength, tackiness, and active energy ray curability tend to be insufficient, while if it is too high, the adhesive strength, tackiness, and substrate adhesion tend to be insufficient.
[0040] The content ratio (molar ratio) of the structural units derived from linear aliphatic polyhydric alcohol (β1-1) to the structural units derived from branched aliphatic polyhydric alcohol (β1-2) in the structural units derived from polyhydric alcohol (β) is preferably, (structural units derived from linear aliphatic polyhydric alcohol (β1-1) / structural units derived from branched aliphatic polyhydric alcohol (β1-2)=100 / 0 to 10 / 90, more preferably 95 / 5 to 20 / 80, particularly preferably 90 / 10 to 30 / 70, even more preferably 85 / 15 to 35 / 65, and especially preferably 80 / 20 to 40 / 60.
[0041] Examples of the alicyclic polyhydric alcohol include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediol, tricyclodecanedimethanol, and spiroglycol.
[0042] Examples of the aromatic polyhydric alcohol include paraxylene glycol, metaxylene glycol, ortho-xylene glycol, 1,4-phenylene glycol, an ethylene oxide adduct of 1,4-phenylene glycol, bisphenols such as bisphenol A, bisphenol B, bisphenol E, bisphenol F, bisphenol AP, bisphenol BP, bisphenol P, bisphenol PH, bisphenol S, bisphenol Z, 4,4'-dihydroxybenzophenone, and bisphenol fluorene, and hydrogenated products thereof, and glycols such as ethylene oxide adducts and propylene oxide adducts obtained by adding 1 to several moles of ethylene oxide or propylene oxide to the hydroxyl groups of bisphenols.
[0043] Furthermore, in order to easily obtain a polymer having a desired molecular weight, the polyhydric alcohol (β) may be, for example, a polyester diol, a polyether diol, a polycaprolactone diol, a polycarbonate diol, a hydrogenated polybutadiene diol, or a hydrogenated polyisoprene diol.
[0044] Examples of the polyester diol include structural units derived from polyester diols obtained by dehydrating a diol component such as ethylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,10-decanediol, or octadecanediol with a dicarboxylic acid component or derivative thereof such as succinic acid, methylsuccinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, 1,12-dodecanoic acid, 1,14-tetradecanedioic acid, terephthalic acid, isophthalic acid, or an acid anhydride or lower alkyl ester thereof, either alone or in a mixed state.
[0045] Commercially available examples of the polyester diol include polyester diols of 3-methyl-1,5-pentanediol and adipic acid, which are sold under the trade names "Kuraray Polyol P-510," "Kuraray Polyol P-1010," "Kuraray Polyol P-2010," "Kuraray Polyol P-3010," and "Kuraray Polyol P-5010" (all manufactured by Kuraray Co., Ltd.).
[0046] Examples of the polyether diol include structural units derived from polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc., obtained by ring-opening polymerization of ethylene oxide, propylene oxide, tetrahydrofuran, etc., and copolyether diols obtained by copolymerizing these.
[0047] Commercially available examples of the polyether diol include polyether diols obtained by adding propylene oxide to propylene glycol, such as trade names "ADEKA POLYETHER P-400," "ADEKA POLYETHER P-1000," "ADEKA POLYETHER P-2000," and "ADEKA POLYETHER P-3000" (all manufactured by ADEKA Corporation).
[0048] Examples of the polycaprolactone diol include structural units derived from caprolactone-based polyester diols obtained by ring-opening polymerization of cyclic ester monomers such as ε-caprolactone and δ-valerolactone.
[0049] Examples of commercially available polycaprolactone diols include those under the trade names "PLACCEL L205AL", "PLACCEL L212AL", "PLACCEL L220AL", "PLACCEL L220PL" and "PLACCEL L230AL" (all manufactured by Daicel Chemical Industries, Ltd.).
[0050] Examples of the polycarbonate diol include structural units derived from carbonate diols such as propylene carbonate diol, hexamethylene carbonate diol, and 3-methylpentene carbonate diol, and polycarbonate diols obtained by dealcoholization reaction between polyhydric alcohols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, and 1,9-nonanediol and dialkyl carbonates such as diethylene carbonate and dimethyl carbonate.
[0051] Commercially available polycarbonate diols include, for example, trade names "PLACCEL CD205", "PLACCEL CD210", "PLACCEL CD220", "PLACCEL CD205PL", "PLACCEL CD210PL", and "PLACCEL CD220PL" (all manufactured by Daicel Chemical Industries, Ltd.).
[0052] Examples of the hydrogenated polybutadiene polyol include structural units derived from hydrogenated polybutadiene polyols such as 1,2-polybutadiene polyol and 1,4-polybutadiene polyol in which double bonds are saturated with hydrogen or halogen.
[0053] Commercially available hydrogenated polybutadiene polyols include, for example, those under the trade names "GI-1000", "GI-2000", and "GI-3000" (all manufactured by Nippon Soda Co., Ltd.).
[0054] Examples of the hydrogenated polyisoprene polyol include structural units such as hydrogenated polyisoprene polyol in which the double bonds of polyisoprene polyol are saturated with hydrogen, halogen or the like.
[0055] An example of a commercially available hydrogenated polyisoprene polyol is "Epole" (manufactured by Idemitsu Kosan Co., Ltd.).
[0056] [Trifunctional or higher polyvalent carboxylic acids and trifunctional or higher polyvalent alcohols] The polyester (A) preferably has a structural unit derived from a polyvalent carboxylic acid having three or more functional groups and / or a polyvalent alcohol having three or more functional groups, as described in the polyvalent carboxylic acid (α) and polyhydric alcohol (β), for the purpose of improving the cohesive strength by introducing a branched skeleton and enhancing the curability by active energy rays. In particular, when a crosslinked structure is formed by active energy rays, the polyester (A) having a branched skeleton increases the number of crosslinking points of the polyester (A), and a pressure-sensitive adhesive having high cohesive strength can be efficiently obtained with a small amount of exposure to active energy rays.
[0057] Examples of the trifunctional or higher polyvalent carboxylic acid include trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tris(anhydrotrimellitate), trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride. Examples of trifunctional or higher polyhydric alcohols include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. One or more of these tri- or higher functional polyvalent carboxylic acids and tri- or higher functional polyhydric alcohols can be used.
[0058] When the polyester (A) contains a structural unit derived from a trifunctional or higher polyvalent carboxylic acid and / or a trifunctional or higher polyhydric alcohol as a branched skeleton, the content of the structural unit derived from a trifunctional or higher polyvalent carboxylic acid relative to the structural unit derived from a polyvalent carboxylic acid (α) and the content of the structural unit derived from a trifunctional or higher polyhydric alcohol relative to the structural unit derived from a polyhydric alcohol (β) are each preferably 0.1 to 5 mol%, more preferably 0.3 to 4 mol%, even more preferably 0.5 to 3 mol%, and particularly preferably 1 to 2.5 mol%. If the content of both or either one is too high, the mechanical properties such as the breaking point elongation of the coating film formed by applying the pressure-sensitive adhesive tend to decrease, resulting in a decrease in adhesive strength, and also tend to cause gelation during polymerization.
[0059] When the polyester (A) contains a structural unit derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol as a branched skeleton, the content of the structural unit derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol relative to 100% by mass of all structural units of the polyester (A) is preferably 0.1 to 3% by mass, more preferably 0.2 to 4% by mass, particularly preferably 0.3 to 3% by mass, even more preferably 0.4 to 2% by mass, or 0.5 to 1.5% by mass. If the content of the structural unit derived from a trifunctional or higher polycarboxylic acid and / or a trifunctional or higher polyhydric alcohol is too high, the mechanical properties such as the elongation at break of the coating film formed by applying the pressure-sensitive adhesive tend to decrease, resulting in a decrease in adhesive strength, and also tends to cause gelation during polymerization.
[0060] [Structural units derived from cyclic esters] The polyester (A) may contain, in addition to the structural units derived from the polyvalent carboxylic acid (α) and the structural units derived from the polyhydric alcohol (β), structural units derived from a cyclic ester in order to adjust the melt viscosity and glass transition temperature and to impart biodegradability, within a range that does not impair the effects of the present invention.
[0061] Examples of the cyclic ester include aliphatic lactones such as lactide, β-propiolactone, β-butyrolactone, γ-butyrolactone, γ-hexanolactone, γ-octanolactone, δ-valerolactone, δ-hexalanolactone, δ-octanolactone, ε-caprolactone, δ-dodecanolactone, α-methyl-γ-butyrolactone, β-methyl-δ-valerolactone, glycolide, and lactide. Among these, ε-caprolactone is preferable from the viewpoint of excellent adhesion and biodegradability. These cyclic ester compounds can be used alone or in combination.
[0062] The structural units derived from cyclic esters in the polyester (A) are preferably less than 140 mol%, more preferably less than 100 mol%, particularly preferably less than 60 mol%, even more preferably less than 30 mol%, particularly preferably less than 15 mol%, and most preferably 0 mol% relative to 100 mol% of the structural units derived from polyvalent carboxylic acid (α). If the content of the structural units derived from cyclic esters is too high, the polyester (A) tends to crystallize, resulting in reduced active energy curing properties and adhesive strength, and an increased melt viscosity, which deteriorates the suitability for hot melt coating.
[0063] The polyester (A) may contain a structural unit derived from a compound having both a carboxylic acid and a hydroxyl group in the molecule in order to adjust the melt viscosity and the glass transition temperature or to impart biodegradability, within a range that does not impair the effects of the present invention.
[0064] Examples of the compound having both a carboxylic acid and a hydroxyl group in the molecule include glycolic acid, lactic acid, hydroxybutyric acid, and hydroxyhexanoic acid. Among them, lactic acid and hydroxybutyric acid are particularly preferred because they increase the ester bond concentration and have excellent adhesive strength and biodegradability. One or more of these compounds having a structural unit derived from a compound having both a carboxylic acid and a hydroxyl group in the molecule can be used.
[0065] The structural units derived from the compound having both carboxylic acid and hydroxyl group in the molecule in the polyester (A) are preferably 100 mol % or less, more preferably 80 mol % or less, particularly preferably 60 mol % or less, even more preferably 40 mol % or less, especially preferably 20 mol % or less, and most preferably 10 mol % or less, based on 100 mol % of the structural units derived from the polyvalent carboxylic acid (α). If the content of the structural units derived from the compound having both carboxylic acid and hydroxyl group in the molecule is too high, the polyester (A) tends to crystallize, resulting in a decrease in the active energy curing property and adhesive strength, and an increase in melt viscosity, which deteriorates the suitability for hot melt coating.
[0066] [Production of polyester (A)] The polyester (A) can be produced by a known method. For example, a polycarboxylic acid (α) and a polyhydric alcohol (β) are subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, which is then subjected to polycondensation to obtain a polyester, and a hydroxyl value and an acid value are further introduced as necessary to produce the polyester.
[0067] The temperature in the esterification reaction between the polyvalent carboxylic acid (α) and the polyhydric alcohol (β) is usually 180 to 280° C., and the reaction time is usually 60 minutes to 8 hours.
[0068] The temperature in the polycondensation is usually 220 to 280° C., and the reaction time is usually 20 minutes to 4 hours. In addition, the polycondensation is preferably carried out under reduced pressure.
[0069] Examples of the method for introducing an acid value into a polyester include a method for introducing a carboxy group into a polyester by an acid addition method or a depolymerization method after an esterification reaction or reduced pressure polycondensation. Among these, when a carboxy group is to be introduced into the main chain terminal of a polyester, the depolymerization method is particularly preferred since the carboxy group can be introduced efficiently. When a carboxy group is to be introduced into the side chain of a polyester, the acid addition method is preferred.
[0070] When a carboxy group is introduced into the main chain terminal of a polyester by the depolymerization method, for example, a polyvalent carboxylic acid (α) and a polyhydric alcohol (β) are subjected to an esterification reaction, optionally in the presence of a catalyst, to obtain a prepolymer, which is then subjected to polycondensation and further to depolymerization.
[0071] For the depolymerization, it is preferable to use a polyvalent carboxylic acid having 0 or 1 acid anhydride group from the viewpoint of adhesive strength. Examples of the polyvalent carboxylic acid having 0 or 1 acid anhydride group include compounds such as trimellitic acid, trimellitic anhydride, hydrogenated trimellitic anhydride, and trimesic acid. In order to suppress a decrease in molecular weight, a polyvalent carboxylic acid having 1 acid anhydride group is preferable, and examples of the polyvalent carboxylic acid having 1 acid anhydride group include trimellitic anhydride and hydrogenated trimellitic anhydride, with trimellitic anhydride being particularly preferable.
[0072] The temperature in the depolymerization is usually 200 to 260° C., and the reaction time is usually 10 minutes to 3 hours.
[0073] In producing the polyester (A) by the depolymerization method, if the content of structural units derived from a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride group exceeds 20 mol % relative to 100 mol % of the structural units derived from the polycarboxylic acid (α), the molecular weight of the resin tends to decrease significantly. Therefore, the content of structural units derived from a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride group relative to 100 mol % of structural units derived from a polycarboxylic acid (α) is preferably 20 mol % or less, more preferably 1 to 15 mol %, particularly preferably 2 to 10 mol %, and even more preferably 3 to 8 mol %.
[0074] When the carboxyl group is introduced into the side chain of the polyester by the acid addition method, for example, a polyvalent carboxylic acid (α) other than a polyvalent carboxylic anhydride and a polyhydric alcohol (β) are subjected to an esterification reaction to obtain a prepolymer, and then polycondensation is carried out, and the resulting hydroxyl group-containing prepolymer is reacted with a polyvalent carboxylic anhydride to perform acid addition. Note that, when a monocarboxylic acid, a dicarboxylic acid, or a polyfunctional carboxylic acid compound is used in the acid addition method, a decrease in molecular weight may occur due to ester exchange, so it is preferable to use a compound having at least one carboxylic anhydride.
[0075] As the depolymerization method and the acid addition method, there are a method of directly adding in a bulk state and a method of dissolving the polyester and then adding the solution. The reaction in the bulk state is rapid, but adding a large amount can cause gelation, and since the reaction occurs at high temperatures, care must be taken to prevent oxidation by blocking oxygen gas. On the other hand, addition in a solution state is a slow reaction but allows a large amount of carboxyl groups to be stably introduced.
[0076] Examples of the polyvalent carboxylic acid anhydride include succinic anhydride, maleic anhydride, orthophthalic anhydride, 2,5-norbornene dicarboxylic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride.
[0077] When producing polyester (A) by the acid addition method, if 15 mol % or more of the structural units derived from the polyvalent carboxylic acid (α) are added with respect to 100 mol % of the structural units, gelation may occur, so it is preferable to add less than 15 mol % of the acid.
[0078] [Composition ratio of polyester (A)] The ratio of structural parts derived from each component of the polyester (A) (composition ratio) was measured by a known method using NMR, for example, a method using a resonance frequency of 400 MHz. 1 H-NMR measurement (proton nuclear magnetic resonance spectroscopy), 13 It can be determined by C-NMR measurement (carbon-type nuclear magnetic resonance spectroscopy measurement) or the like.
[0079] [Glass transition temperature of polyester (A)] The glass transition temperature of the polyester (A) is preferably −80 to 30° C., more preferably −75 to 10° C., still more preferably −70 to −10° C., particularly preferably −65 to −20° C., still more preferably −60 to −30° C., particularly preferably −55 to −35° C., and most preferably −50 to −40° C. If the glass transition temperature is too high, the tackiness and adhesive strength tend to be insufficient, and the melt viscosity tends to increase, resulting in poor suitability for hot melt coating, whereas if the glass transition temperature is too low, the holding strength and heat resistance tend to be insufficient.
[0080] The method for measuring the glass transition temperature is as follows. The glass transition temperature can be determined by measurement using a differential scanning calorimeter, with the measurement conditions being a measurement temperature range of −90 to 100° C. and a temperature rise rate of 10° C. / min.
[0081] [Acid value of polyester (A)] The acid value of the polyester (A) is preferably 30 mgKOH / g or less, more preferably 10 mgKOH / g or less, particularly preferably 5 mgKOH / g or less, even more preferably 3 mgKOH / g or less, particularly preferably 1 mgKOH / g or less, and most preferably 0.5 mgKOH / g or less. If the acid value is too high, the wet heat resistance tends to be insufficient, or the heat resistance tends to decrease, making thermal decomposition more likely to proceed.
[0082] The definition and measuring method of the acid value are as follows. The acid value (mgKOH / g) can be determined by dissolving 1 g of polyester (A) in 30 g of a mixed solvent of toluene / methanol (for example, toluene / methanol=7 / 3 by volume) and subjecting the solution to neutralization titration according to JIS K 0070. In the present invention, the acid value of the polyester (A) is determined by the content of carboxy groups in the resin.
[0083] (Hydroxyl value of polyester (A)) The hydroxyl value of the polyester (A) is preferably 50 mgKOH / g or less, particularly 1 to 30 mgKOH / g, further 2 to 20 mgKOH / g, more preferably 3 to 15 mgKOH / g or less, particularly preferably 4 to 10 mgKOH / g, and most preferably 5 to 8 mgKOH / g. If the hydroxyl value is too high, the active energy ray curability tends to decrease and the cohesive strength and holding power tend to be insufficient, while if the hydroxyl value is too low, the adhesive strength and adhesion tend to be insufficient and the compatibility with the tackifier resin tends to be poor.
[0084] The hydroxyl value of the polyester (A) is determined by neutralization titration based on JIS K0070.
[0085] (Isocyanate concentration of polyester (A)) The isocyanate concentration of the polyester (A) is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, particularly preferably 0.5% or less, especially preferably 0.3% or less, and most preferably 0.1% or less. The lower limit is 0%, and it is preferable that the polyester does not contain an isocyanate group. If the isocyanate concentration is too high, the reaction proceeds due to the heat load during the production of the polyester or hot melt coating, and the pot life and coating appearance tend to be poor, and the adhesive strength tends to decrease.
[0086] The isocyanate concentration of the polyester (A) is determined by neutralization titration based on JIS K6806.
[0087] (Oxirane oxygen concentration of polyester (A)) The oxirane oxygen concentration of the polyester (A) is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, particularly preferably 0.5% or less, especially preferably 0.3% or less, and most preferably 0.1% or less. The lower limit is 0%, and it is preferable that the polyester does not contain oxirane oxygen (epoxy group). If the oxirane concentration is too high, the reaction proceeds due to the heat load during the production of the polyester or hot melt coating, and the pot life and coating appearance tend to be poor, and the adhesive strength tends to decrease.
[0088] The oxolane oxygen concentration of the polyester (A) can be determined by titration using a solution of hydrogen bromide in acetic acid based on ASTM-1652.
[0089] [Ester bond concentration of polyester (A)] The ester bond concentration of the polyester (A) is preferably 2 to 14 mmol / g, more preferably 3 to 13 mmol / g, further preferably 4 to 12 mmol / g, particularly preferably 5 to 11 mmol / g, particularly preferably 5.5 to 10 mmol / g, and most preferably 6 to 9 mmol / g. If the ester bond concentration is too high, the melt viscosity tends to increase and the coatability tends to be insufficient, whereas if the ester bond concentration is too low, the heat resistance, substrate adhesion, and adhesive strength tend to be insufficient.
[0090] The definition and measurement method of the ester bond concentration are as follows. The ester bond concentration (mmol / g) refers to the number of moles of ester bonds in 1 g of polyester (A), and is calculated from the amounts charged, for example. The calculation method is to divide the number of moles of the lesser of the charged amounts of polyvalent carboxylic acid (α) and polyhydric alcohol (β) by the total mass of polyester (A), and an example of the calculation formula is shown below. When the polyvalent carboxylic acid (α) and the polyhydric alcohol (β) are charged in equal molar amounts, either of the following calculation formulas may be used. Furthermore, when a monomer having both a carboxyl group and a hydroxyl group is used, or when polyester is produced from caprolactone or the like, the calculation method will be changed appropriately.
[0091] (When the amount of polyvalent carboxylic acid (α) is less than the amount of polyvalent alcohol (β)) Ester group concentration (mmol / g) = [(P1 / p1 × m1 + P2 / p2 × m2 + P3 / p3 × m3 ) / Z] × 1000 P: Amount of polycarboxylic acid (α) (g) p: Molecular weight of polycarboxylic acid (α) m: number of carboxy groups per molecule of polycarboxylic acid (α) Z: Finished mass (g)
[0092] (When the amount of polyhydric alcohol (β) is less than the amount of polycarboxylic acid (α)) Ester group concentration (mmol / g) = [(Q1 / q1 × n1 + Q2 / q2 × n2 + Q3 / q3 × n3 ) / Z] × 1000 Q: Amount of polyhydric alcohol (β) (g) q: Molecular weight of polyhydric alcohol (β) n: number of hydroxyl groups per molecule of polyhydric alcohol (β) Z: Finished mass (g)
[0093] The ester bond concentration can be measured by a known method using NMR or the like, for example, 1 H-NMR measurement (proton nuclear magnetic resonance spectroscopy), 13 It can also be measured by C-NMR measurement (carbon-type nuclear magnetic resonance spectroscopy).
[0094] [Unsaturated group concentration of polyester (A)] The unsaturated group concentration of the polyester (A) is preferably 1 mmol / g or less, more preferably 0.5 mmol / g or less, particularly preferably 0.1 mmol / g or less, further preferably 0.05 mmol / g or less, particularly preferably 0.01 mmol / g or less, and most preferably 0.001 mmol / g or less, per 1 g of the polyester (A). The lower limit is 0 mmol / g. If the unsaturated group concentration of the polyester (A) is too high, the unsaturated groups will react due to heat load during production of the polyester (A) or during hot melt coating, which will tend to result in poor pot life, poor coating appearance, and reduced adhesive strength. The concentration of unsaturated groups contained in the polyester (A) is 1 H-NMR measurements and 13 It can be determined from the spectrum obtained by C-NMR measurement.
[0095] [Epoxy group concentration of polyester (A)] The epoxy group concentration of the polyester (A) is preferably 5 mmol / g or less per 1 g of the polyester (A), more preferably 3 mmol / g or less, particularly preferably 2 mmol / g or less, even more preferably 1 mmol / g or less, particularly preferably 0.5 mmol / g or less, and most preferably 0.1 mmol / g or less. The lower limit is 0 mmol / g. If the epoxy group concentration of the polyester (A) is too high, the epoxy groups react due to heat load during the production of the polyester (A) or hot melt coating, and the pot life and coating appearance tend to be poor, and the adhesive strength tends to decrease. The epoxy group concentration is determined by taking the reciprocal of the epoxy equivalent calculated based on JIS K 7236.
[0096] [Peak top molecular weight (Mp), number average molecular weight (Mn) and weight average molecular weight (Mw) of polyester (A)]
[0097] The peak top molecular weight (Mp) of the polyester (A) is preferably from 5,000 to 150,000, more preferably from 10,000 to 120,000, particularly preferably from 20,000 to 100,000, further preferably from 30,000 to 90,000, and particularly preferably from 40,000 to 80,000. If the peak top molecular weight (Mp) is too low, the active energy ray curability tends to decrease, the cohesive force tends to be insufficient, and the heat resistance and the wet heat durability tend to be insufficient, whereas if the peak top molecular weight (Mp) is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coating suitability.
[0098] The number average molecular weight (Mn) of the polyester (A) is preferably from 1,000 to 150,000, more preferably from 2,500 to 120,000, particularly preferably from 5,000 to 100,000, further preferably from 10,000 to 80,000, and especially preferably from 20,000 to 60,000. If the number average molecular weight (Mn) is too low, the active energy ray curability tends to decrease, the cohesive force tends to be insufficient, and the heat resistance and the wet heat durability tend to be insufficient, whereas if the number average molecular weight (Mn) is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coating suitability.
[0099] The weight average molecular weight (Mw) of the polyester (A) is preferably 5,000 to 500,000, more preferably 10,000 to 300,000, particularly preferably 20,000 to 200,000, further preferably 30,000 to 150,000, particularly preferably 50,000 to 130,000, and most preferably 70,000 to 110,000. If the weight average molecular weight (Mw) is too low, the active energy ray curability tends to decrease, the cohesive force tends to be insufficient, and the heat resistance and the wet heat durability tend to be insufficient, whereas if the weight average molecular weight (Mw) is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coating suitability.
[0100] The peak top molecular weight (Mp), number average molecular weight (Mn) and weight average molecular weight (Mw) are measured by the following methods. The peak top molecular weight (Mp), number average molecular weight (Mn), and weight average molecular weight (Mw) were measured using a high performance liquid chromatograph (Tosoh Corporation, "HLC-8320GPC") with a column (TSKgel SuperMultipore HZ-M (exclusion limit: 2 × 10 6 The molecular weight of the filler can be calculated by converting it into the molecular weight of standard polystyrene.
[0101] The polydispersity of the polyester (A) is preferably 0.5 or more, more preferably 1 to 30, particularly preferably 1.5 to 20, even more preferably 2 to 15, particularly preferably 2.5 to 10, and most preferably 3 to 8. If the polydispersity is too low, the active energy ray curability tends to decrease, the cohesive force tends to be insufficient, and the heat resistance and the wet heat durability tend to be insufficient. If the polydispersity is too high, the adhesion and tackiness tend to be insufficient, and the melt viscosity tends to be high, resulting in insufficient coating suitability. The polydispersity is calculated by the following formula. Polydispersity=weight average molecular weight (Mw) / number average molecular weight (Mn)
[0102] The melt viscosity (130°C) of the polyester (A) is preferably 500 Pa·s or less, more preferably 1 to 400 Pa·s or less, even more preferably 3 to 300 Pa·s or less, particularly preferably 5 to 200 Pa·s or less, especially preferably 10 to 150 Pa·s or less, and most preferably 15 to 100 Pa·s. If the melt viscosity is too low, the heat resistance, holding power, adhesive power, and wet heat durability tend to be insufficient, while if it is too high, the coating film appearance tends to have streaks and the coating suitability tends to be insufficient.
[0103] The melt viscosity was measured by the following method. Using a flow tester "CFT-500EX" (manufactured by Shimadzu Corporation), the melt viscosity is measured when the polyester is extruded from the nozzle using the constant temperature method under the following conditions: test temperature 130°C, residence time 3 minutes, test force 30 (load 3 kg), die diameter 1.0 mm, die length 10 mm, stroke 20 mm.
[0104] From the viewpoint of heat resistance and coatability, the polyester (A) preferably has a small melt viscosity change rate before and after heat history (200°C, 3 hours, under air conditions). The melt viscosity change rate is preferably 20 to 500%, more preferably 30 to 400%, even more preferably 40 to 300%, particularly preferably 50 to 250%, especially preferably 60 to 200%, and most preferably 70 to 150%. If the melt viscosity change rate before and after heat history is out of the above range, the adhesive may gel or decompose, resulting in insufficient coatability, adhesive strength, and adhesion.
[0105] The polyester (A) is preferably a non-crystalline polyester in terms of active energy ray curability, tackiness, optical properties, etc. If the polyester (A) is crystalline, the active energy ray curability, tackiness, molding stability, optical properties, etc. tend to be insufficient. The non-crystalline nature can be confirmed by a differential scanning calorimeter, and refers to, for example, that no endothermic peak due to crystalline melting is observed when measured at a temperature range of −90 to 400° C. and a temperature rise rate of 10° C. / min. The measurement temperature range and temperature rise rate can be appropriately changed depending on the sample.
[0106] The heat of crystalline fusion of the polyester (A) is preferably 0 J / g from the viewpoints of active energy ray curability, tackiness, optical properties, etc., but when it crystallizes, it is 50 J / g or less, preferably 30 J / g or less, particularly preferably 10 J / g or less, especially preferably 5 J / g or less, more preferably 3 J / g or less, and most preferably 1 J / g or less.
[0107] In addition, the polyester (A) is preferably made from plant-derived raw materials and has a biomass content in order to reduce the burden on the global environment. The biomass degree of the polyester (A) is preferably 10% or more, more preferably 20% or more, particularly preferably 30% or more, further preferably 40% or more, particularly preferably 50% or more, and most preferably 60% or more. The upper limit is 100%. If the biomass degree is low, the reduction of the load on the global environment tends to be insufficient.
[0108] Here, the biomass degree of the polyester (A) refers to the mass ratio of the plant-derived raw materials used in producing the polyester (A) incorporated into the resin relative to the total mass of the polyester (A), and is calculated as follows. The biomass degrees of the polyvalent carboxylic acid (α) and the polyhydric alcohol (β) are calculated from the weighted average of their respective biomass degrees. It is sufficient that the value obtained by any of the following calculation methods is within the above range. (Calculation method) Biomass ratio (%) = [(number of moles of carbon of plant-derived monomer calculated from the molar ratio of polycarboxylic acid (α) and polyhydric alcohol (β) in polyester (A)) / (number of moles of carbon of all constituent monomers in polyester (A)] × 100
[0109] The biomass degree can also be determined by analyzing the composition ratio by NMR and calculating the carbon number of the plant-derived monomer / the total carbon number.
[0110] Furthermore, the biomass degree can also be measured by the method described in “Technology for determining the origin of biofuels using natural radioactive carbon C-14” in Tokyo Metropolitan Industrial Technology Research Center Research Report, No. 4, 2009.
[0111] <Compound (B) Having a Photoreactive Group> By including the compound (B) having a photoreactive group, the present composition can have excellent active energy ray curability even without including an unsaturated group or a crosslinking agent.
[0112] The compound (B) having a photoreactive group contained in the present composition functions as a photopolymerization initiator. Examples of the compound (B) having a photoreactive group that functions as such a photopolymerization initiator include a compound (b1) having a hydrogen abstraction type reactive group (hydrogen abstraction type photopolymerization initiator) and a compound (b2) having a cleavage type photoreactive group (cleavage type photopolymerization initiator). These may be used alone or in combination of two or more. Among these, the compound (b1) having a hydrogen abstraction type reactive group (hydrogen abstraction type photopolymerization initiator) is preferred because of its excellent active energy ray curability. In addition, the compound (B) having a photoreactive group is preferably a compound (b1) having a hydrogen abstraction type photoreactive group and / or a compound (b2) having a cleavage type photoreactive group, and it is more preferable to have at least one of the compound (b1) having a hydrogen abstraction type reactive group and the compound (b2) having a cleavage type photoreactive group, in terms of excellent active energy ray curability.
[0113] When the compound (B) having a photoreactive group is used as a photopolymerization initiator, the compound (B) having a photoreactive group is not incorporated and contained in the structure of the polyester (A) by chemical bonding, but is preferably contained independently in the composition, since it has excellent optical properties after active energy ray curing, is easy to control the degree of crosslinking, and has excellent stability. Therefore, when the compound (B) having a photoreactive group is also used as a photopolymerization initiator, it is preferable that it does not have an active hydrogen group such as a carboxy group or a hydroxy group, since it has excellent active energy ray curing properties.
[0114] [Compound (b1) having a hydrogen abstraction type photoreactive group] The compound (b1) having a hydrogen abstraction type photoreactive group abstracts hydrogen from a hydrogen donor of the polyester (A) when irradiated with active energy rays, thereby causing a crosslinking reaction of the polyester (A).
[0115] The compound (b1) having a hydrogen abstraction type photoreactive group is not particularly limited, and conventionally known compounds can be used. For example, benzophenones (b1-1), thioxanthones (b1-2), anthraquinones (b1-3), ketocoumarins, and camphorquinones can be mentioned. These may be used alone or in combination of two or more. Among these, benzophenones (b1-1) are preferred because of their excellent active energy ray curability.
[0116] The benzophenones (b1-1) are not particularly limited, but examples thereof include compounds represented by the following general formula (1).
[0117] [ka]
[0118] Specific examples include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, o-benzoylmethylbenzoate, 3,3'-dimethyl-4-methoxybenzophenone, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 4-morpholinobenzophenone, 4,4'-diphenoxybenzophenone, 4-hydroxybenzophenone, 2-carboxybenzophenone, etc. Among these, benzophenone and 4-methylbenzophenone are preferred because of their excellent active energy ray curing properties.
[0119] Commercially available examples of the benzophenones (b1-1) include those sold under the trade names "OmniradBPFlakes", "Omnirad4MBZFlakes", "OmnipolPB", "EsacureTZT", "EsacureTZM", "Omnirad4PBZ", "Omnirad81", "OmniradBMF", and "OmniradOMBB" (all manufactured by IGMREJINS).
[0120] The thioxanthones (b1-2) are not particularly limited, but include compounds represented by the following general formula (2).
[0121] [ka]
[0122] Specific examples include thioxanthone-2,3-dicarboxylic acid, thioxanthone-2,7-dicarboxylic acid, thioxanthone-2,6-dicarboxylic acid, 2,2',3,3'-thioxanthone tetracarboxylic dianhydride, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone.
[0123] The anthraquinones (b1-3) are not particularly limited, but examples thereof include compounds represented by the following general formula (3).
[0124] [ka]
[0125] Specific examples include anthraquinone-2,3-dicarboxylic acid, anthraquinone-2,7-dicarboxylic acid, anthraquinone-2,6-dicarboxylic acid, 2,2',3,3'-anthraquinonetetracarboxylic dianhydride, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 2-aminoanthraquinone.
[0126] [Compound (b2) having a cleavable photoreactive group] The compound (b2) having a cleavable photoreactive group is not particularly limited as long as it is photocleaved to generate radicals upon irradiation with active energy rays, and any compound known in the art can be used. Examples of the compound (b2) having a cleavable photoreactive group include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}phenyl]-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), methyl phenylglyoxylate, 2-benzyl-2-dimethyl Examples of the arylamino-1-(4-morpholinophenyl)butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, or derivatives thereof may be mentioned. These may be used alone or in combination of two or more kinds.
[0127] Examples of commercially available products of the compound (b2) having the cleavable photoreactive group include those manufactured by IGMREJINS under the trade names "Omnirad651", "Omnirad184", "Omnirad1173", "Omnirad2959", "Omnirad127", "Omnirad907", "Omnirad369", and "OmniradTPO".
[0128] The content of the compound (B) having a photoreactive group is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 0.3 to 8 parts by mass, particularly preferably 0.5 to 7 parts by mass, especially preferably 1 to 6 parts by mass, and most preferably 1.5 to 5.5 parts by mass, based on 100 parts by mass of the polyester (A). If the content is too high, the cohesive strength of the adhesive layer after curing with active energy rays tends to become too high, resulting in a decrease in adhesive strength, whereas if the content is too low, the curability with active energy rays tends to decrease, resulting in insufficient adhesive strength and cohesive strength.
[0129] When a compound (b1) having a hydrogen abstraction type reactive group is used, the content is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 9 parts by mass, even more preferably 0.3 to 8 parts by mass, particularly preferably 0.5 to 7 parts by mass or less, particularly preferably 1 to 6 parts by mass, and most preferably 1.5 to 5.5 parts by mass, relative to 100 parts by mass of the polyester (A). If the content is too high, the cohesive strength of the adhesive after curing with active energy rays tends to become too high and the adhesive strength tends to decrease, whereas if the content is too low, the curability with active energy rays tends to decrease and the adhesive strength and cohesive strength tend to become insufficient.
[0130] In addition, as an auxiliary agent for enhancing the reaction activity of the compound (B) having a photoreactive group, triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, etc. may be used in combination. These auxiliary agents may be used alone or in combination of two or more.
[0131] <Polymerizable unsaturated group-containing compound (C)> The composition may contain a polymerizable unsaturated group-containing compound (C), which is a component that is cured by active energy rays in order to increase the cohesive strength. Examples of the polymerizable unsaturated group-containing compound (C) include urethane (meth)acrylate compounds and ethylenically unsaturated monomers having an ethylenically unsaturated group.
[0132] The urethane (meth)acrylate compound is a (meth)acrylate compound having a urethane bond in the molecule, and can be produced by reacting a hydroxyl group-containing (meth)acrylic compound with a polyisocyanate compound, and further, if necessary, with a polyol.
[0133] Examples of the hydroxyl group-containing (meth)acrylic compound include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate. Examples of the acrylate include pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified dipentaerythritol penta(meth)acrylate, and ethylene oxide-modified pentaerythritol tri(meth)acrylate. Among these, hydroxyl-containing (meth)acrylic compounds having three or more acryloyl groups are preferably used. These can be used alone or in combination of two or more.
[0134] The polyisocyanate compound is not particularly limited, and examples thereof include aromatic, aliphatic, and alicyclic polyisocyanates. Among them, tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate are particularly preferred. Examples of the polyisocyanate include polyisocyanates such as tetramethylxylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, phenylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and naphthalene diisocyanate, or trimer compounds or polymer compounds of these polyisocyanates, biuret type polyisocyanates, or reaction products of these polyisocyanates with polyols.
[0135] Such polyols are not particularly limited, and examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, butylene glycol, polybutylene glycol, 1,6-hexanediol, neopentyl glycol, cyclohexanedimethanol, hydrogenated bisphenol A, polycaprolactone, trimethylolethane, trimethylolpropane, polytrimethylolpropane, pentaerythritol, polypentaerythritol, sorbitol, mannitol, glycerin, polyglycerin, Examples of suitable polyhydric alcohols include polytetramethylene glycol; polyether polyols having at least one structure of polyethylene oxide, polypropylene oxide, or block or random copolymerization of ethylene oxide / propylene oxide; polyester polyols which are condensates of such polyhydric alcohols or polyether polyols with polybasic acids such as maleic anhydride, maleic acid, fumaric acid, itaconic anhydride, itaconic acid, adipic acid, and isophthalic acid; caprolactone-modified polyols such as caprolactone-modified polytetramethylene polyol; polyolefin-based polyols; and polybutadiene-based polyols such as hydrogenated polybutadiene polyols.
[0136] Further examples of such polyols include carboxy group-containing polyols such as 2,2-bis(hydroxymethyl)butyric acid, tartaric acid, 2,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxyethyl)propionic acid, 2,2-bis(hydroxypropyl)propionic acid, dihydroxymethylacetic acid, bis(4-hydroxyphenyl)acetic acid, 4,4-bis(4-hydroxyphenyl)pentanoic acid, and homogentisic acid; and sulfonic acid group- or sulfonate salt group-containing polyols such as 1,4-butanediol sodium sulfonate.
[0137] The method for producing the urethane (meth)acrylate compound is not particularly limited, and examples thereof include a method in which a hydroxyl group-containing (meth)acrylic compound and a polyvalent isocyanate compound are mixed in an inert gas atmosphere and reacted for 2 to 10 hours at 30 to 80° C. In this reaction, it is preferable to use a urethane catalyst such as tin octenoate, di-n-butyltin dilaurate, lead octoate, potassium octoate, potassium acetate, stannous octoate, or triethylenediamine.
[0138] In addition, when a reaction product with a polyol is used as the urethane (meth)acrylate compound, for example, the reaction product obtained by reacting the polyol with the polyvalent isocyanate compound may be reacted with a hydroxyl group-containing (meth)acrylic compound. In the reaction between such a polyvalent isocyanate compound and a polyol, it is also preferable to use a metal catalyst such as dibutyltin dilaurate or an amine catalyst such as 1,8-diazabicyclo[5.4.0]undecene-7 to promote the reaction.
[0139] The weight average molecular weight of the urethane (meth)acrylate compound is preferably 300 to 10000, more preferably 500 to 5000, particularly preferably 750 to 4000, particularly preferably 1000 to 3500, and most preferably 1250 to 3000. The method for measuring the weight average molecular weight is the same as described above.
[0140] Examples of the ethylenically unsaturated monomer having an ethylenically unsaturated group include a monofunctional monomer having one ethylenically unsaturated group in one molecule, a bifunctional monomer having two ethylenically unsaturated groups in one molecule, and a trifunctional or higher monomer having three or more ethylenically unsaturated groups in one molecule.
[0141] Examples of the monofunctional monomer include styrene, vinyl toluene, chlorostyrene, α-methylstyrene, methyl (meth)acrylate, ethyl (meth)acrylate, acrylonitrile, vinyl acetate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-phenoxy-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, glycerin mono(meth)acrylate, glycidyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, Examples of the acrylate include acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, n-stearyl (meth)acrylate, benzyl (meth)acrylate, phenol ethylene oxide modified (meth)acrylate, nonylphenol propylene oxide modified (meth)acrylate, half ester (meth)acrylate of phthalic acid derivative such as 2-(meth)acryloyloxy-2-hydroxypropyl phthalate, furfuryl (meth)acrylate, carbitol (meth)acrylate, benzyl (meth)acrylate, butoxyethyl (meth)acrylate, allyl (meth)acrylate, acryloylmorpholine, 2-hydroxyethyl acrylamide, N-methylol (meth)acrylamide, N-vinylpyrrolidone, 2-vinylpyridine, and 2-(meth)acryloyloxyethyl acid phosphate monoester.
[0142] Examples of the bifunctional monomer include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide modified bisphenol A type di(meth)acrylate, propylene oxide modified bisphenol A type di(meth)acrylate, 1, Examples of such di(meth)acrylates include 6-hexanediol di(meth)acrylate, 1,6-hexanediol ethylene oxide modified di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, hydroxypivalic acid modified neopentyl glycol di(meth)acrylate, isocyanuric acid ethylene oxide modified diacrylate, and 2-(meth)acryloyloxyethyl acid phosphate diester.
[0143] Examples of the trifunctional or higher monomer include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(meth)acryloyloxyethoxytrimethylolpropane, and glycerin polyglyceride. Examples of the poly(meth)acrylate include lysidyl ether poly(meth)acrylate, isocyanuric acid ethylene oxide modified tri(meth)acrylate, ethylene oxide modified dipentaerythritol penta(meth)acrylate, ethylene oxide modified dipentaerythritol hexa(meth)acrylate, ethylene oxide modified pentaerythritol tri(meth)acrylate, ethylene oxide modified pentaerythritol tetra(meth)acrylate, and succinic acid modified pentaerythritol tri(meth)acrylate.
[0144] In addition to the above, the ethylenically unsaturated monomer may also include a Michael adduct of (meth)acrylic acid or a 2-(meth)acryloyloxyethyl dicarboxylic acid monoester, and examples of the Michael adduct of (meth)acrylic acid include a (meth)acrylic acid dimer, a (meth)acrylic acid trimer, and a (meth)acrylic acid tetramer. Examples of the 2-(meth)acryloyloxyethyl dicarboxylic acid monoester, which is a carboxylic acid having a specific substituent, include, for example, 2-(meth)acryloyloxyethyl succinic acid monoester, 2-(meth)acryloyloxyethyl phthalic acid monoester, and 2-(meth)acryloyloxyethyl hexahydrophthalic acid monoester. Furthermore, oligoester acrylate may also be used.
[0145] The unsaturated group-containing compound (C) such as the urethane (meth)acrylate compound or ethylenically unsaturated monomer may be used alone or in combination of two or more kinds.
[0146] The content of the polymerizable unsaturated group-containing compound (C) contained in the composition is less than 15 parts by mass relative to 100 parts by mass of the polyester (A), preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, especially preferably 1 part by mass or less, and most preferably 0 parts by mass. That is, the composition preferably does not contain a polymerizable unsaturated group-containing compound (C). If the content is too high, the cohesive force of the adhesive layer after curing with active energy rays becomes too high, resulting in insufficient elongation and adhesive force, and the unsaturated group reacts with heat to cause an increase in viscosity or gelation, resulting in insufficient thermal stability.
[0147] <Crosslinking agent (D)> The composition may contain a crosslinking agent (D) for the purpose of increasing the cohesive strength. The crosslinking agent (D) may be any compound having a functional group that reacts with a functional group such as a hydroxyl group or a carboxyl group contained in the polyester (A). Examples of the crosslinking agent (D) include epoxy compounds such as bisphenol A-epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, and diglycerol polyglycidyl ether; tetramethylolmethane-tri-β-aziridinyl propionate, trimethylolpropane-tri-β-aziridinyl propionate, N,N'-diphenyl ether, and the like. Aziridine compounds such as N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexaptoxymethylmelamine, hexapentyloxymethylmelamine, hexahexyloxymethylmelamine, and melamine resins, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, hexamethylene diisocyanate, diphenylmethane-4,4-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, tetramethylxylylene diisocyanate, 1,Examples of the isocyanate-based compounds include 5-naphthalene diisocyanate, triphenylmethane triisocyanate, and adducts of these polyisocyanate compounds with polyol compounds such as trimethylolpropane; biuret and isocyanurate forms of these polyisocyanate compounds; aldehyde compounds such as glyoxal, malondialdehyde, succindialdehyde, maleic dialdehyde, glutaric dialdehyde, formaldehyde, acetaldehyde, and benzaldehyde; amine compounds such as hexamethylene diamine, triethyldiamine, polyethyleneimine, hexamethylenetetraamine, diethylenetriamine, triethyltetraamine, isophoronediamine, amino resins, and polyamides; and metal chelate compounds such as acetylacetone and acetoacetyl ester coordination compounds of polymetals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium. Among these, polyisocyanate compounds are preferably used in terms of reactivity with the polyester (A). These crosslinking agents (D) may be used alone or in combination of two or more thereof, except for the hydrolysis inhibitor (E) described below.
[0148] The polyisocyanate compound is not particularly limited, and examples thereof include aromatic, aliphatic, and alicyclic polyisocyanates. Among them, tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylxylylene diisocyanate, isophorone diisocyanate, and the like. Examples of the isocyanate include polyisocyanates such as phenylene diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, phenylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and naphthalene diisocyanate, or trimer compounds or oligomer compounds of these polyisocyanates, biuret type polyisocyanates, and reaction products of these polyisocyanates and polyols. Among these, tolylene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate are preferred in terms of excellent reactivity. These can be used alone or in combination of two or more.
[0149] When a crosslinking agent (D) is used, its content can be appropriately selected depending on the amount of functional groups contained in the polyester (A), the molecular weight of the polyester (A), and the purpose of controlling the adhesive strength after irradiation with active energy rays. In general, the content is preferably 5 parts by mass or less per 100 parts by mass of the polyester (A), more preferably 3 parts by mass or less, even more preferably 2 parts by mass or less, particularly preferably 1 part by mass or less, especially preferably 0.5 parts by mass or less, and most preferably 0 part by mass. If the content of the crosslinking agent (D) is too high, the polyester (A) and the crosslinking agent (D) will react during hot melt coating, increasing the melt viscosity and resulting in insufficient pot life or impairing the appearance of the coating film due to gelation.
[0150] <Hydrolysis inhibitor (E)> The present composition preferably contains a hydrolysis inhibitor (E) from the viewpoint of improving hydrolysis resistance and moist heat resistance. The hydrolysis inhibitor (E) is not particularly limited, and may be a conventionally known one, for example, a compound that reacts with the carboxyl end group of the polyester (A) to bond, specifically, a compound having a functional group such as a carbodiimide group, an oxazoline group, etc. Among these, a carbodiimide group-containing compound is preferred because of its excellent reactivity with a carboxyl group.
[0151] As the carbodiimide group-containing compound, a known carbodiimide having one or more carbodiimide groups (-N=C=N-) in the molecule may be used, for example, a monomeric carbodiimide compound (E1) having one carbodiimide group in the molecule, and a polymeric carbodiimide compound (E2) having at least two carbodiimide groups in the molecule. Among them, a monomeric carbodiimide compound having one carbodiimide group in the molecule is preferable, because it suppresses the increase in viscosity at high temperatures, has excellent heat resistance, and is also excellent in wet heat resistance.
[0152] Examples of the monomeric carbodiimide compound (E1) include dicyclohexylcarbodiimide, diisopropylcarbodiimide, diphenylcarbodiimide, bis(methylphenyl)carbodiimide, bis(methoxyphenyl)carbodiimide, bis(nitrophenyl)carbodiimide, bis(dimethylphenyl)carbodiimide, bis(diisopropylphenyl)carbodiimide, bis(di-t-butylphenyl)carbodiimide, N-ethyl-N'-(3-dimethylaminopropyl)carbodiimide, bis(triphenylsilyl)carbodiimide, and cyclic carbodiimide. Among these, diisopropylcarbodiimide, bis(methoxyphenyl)carbodiimide, bis(diisopropylphenyl)carbodiimide, N-ethyl-N'-(3-dimethylaminopropyl)carbodiimide, and bis(triphenylsilyl)carbodiimide are preferred, and bis(diisopropylphenyl)carbodiimide is preferred in terms of excellent reactivity and compatibility with the carboxyl group of the polyester (A) and excellent durability to wet heat. These can be used alone or in combination of two or more.
[0153] The polymeric carbodiimide compound (E2) may be a compound obtained by subjecting the following diisocyanates to a decarboxylation condensation reaction. Examples of such diisocyanates include 4,4'-diphenylmethane diisocyanate, 3,3'-dimethoxy-4,4'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 3,3'-dimethyl-4,4'-diphenylether diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1-methoxyphenyl-2,4-diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate. These may be used alone or in combination of two or more.
[0154] When the hydrolysis inhibitor (E) is used, the content thereof is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, even more preferably 0.2 to 3 parts by mass, particularly preferably 0.3 to 2 parts by mass, especially preferably 0.4 to 1.5 parts by mass, and most preferably 0.5 to 1 part by mass, relative to 100 parts by mass of the polyester (A). If the content of such a hydrolysis inhibitor is too high, the active energy ray curability and adhesive strength tend to decrease, and the coating film appearance tends to become insufficient due to poor compatibility with the polyester, whereas if the content is too low, the hydrolysis resistance tends to decrease and the wet heat durability tends to become insufficient.
[0155] The content of the hydrolysis inhibitor (E) is preferably optimized depending on the acid value of the polyester (A), and the molar ratio ((ii) / (i)) of the total amount of carboxy groups (i) determined from the acid value of the polyester (A) to the total amount of functional groups (ii) of the hydrolysis inhibitor (E) is preferably 0.5≦(ii) / (i), more preferably 1≦(ii) / (i)≦1000, even more preferably 1.5≦(ii) / (i)≦500, particularly preferably 2≦(ii) / (i)≦250, especially preferably 2.5≦(ii) / (i)≦100, and most preferably 3≦(ii) / (i)≦50. If the content ratio of (ii) to (i) is too high, the coating film appearance tends to be insufficient due to poor compatibility with the polyester (A), and the active energy ray curability, adhesive strength, cohesive strength, and hydrolysis resistance tend to decrease. On the other hand, if the content ratio of (ii) to (i) is low, the hydrolysis resistance and moist heat durability tend to decrease.
[0156] <Antioxidants (F)> It is more preferable that the composition contains an antioxidant (F) since this provides excellent heat resistance to the polyester (A) and stability to the pressure-sensitive adhesive sheet, and can suppress viscosity changes under conditions involving thermal history such as hot melt coating.
[0157] Examples of the antioxidant (F) include phenol-based antioxidants, hindered phenol-based antioxidants, amine-based antioxidants, hindered amine-based antioxidants, sulfur-based antioxidants, phosphoric acid-based antioxidants, etc. Among them, at least one selected from the group consisting of hindered phenol-based antioxidants, hindered amine-based antioxidants, and phosphoric acid-based antioxidants is preferred, and the antioxidant (F) made of a hindered phenol-based compound is particularly preferred. Examples of the hindered phenol-based antioxidants include antioxidants having a hindered phenol structure in which a group with large steric hindrance, such as a tertiary butyl group, is bonded to at least one of the carbon atoms adjacent to the carbon atom on the aromatic ring to which the phenolic hydroxyl group is bonded.
[0158] When the antioxidant (F) is used, the content thereof is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, even more preferably 0.02 to 3 parts by mass, particularly preferably 0.1 to 2 parts by mass, and especially preferably 0.3 to 1.0 part by mass, relative to 100 parts by mass of the polyester (A). If the content is too low, the heat resistance tends to be insufficient, whereas if the content is too high, the active energy ray curability tends to be insufficient.
[0159] <Tackifier resin> The present composition may contain a tackifier resin, which can improve adhesive properties such as adhesive strength and tackiness.
[0160] The tackifier resin is not particularly limited, and conventionally known resins can be used. Examples of the tackifier resin include hydrocarbon resins, terpene resins, phenol resins, rosin resins, xylene resins, epoxy resins, polyamide resins, ketone resins, and elastomer resins. These may be used alone or in combination of two or more. Among them, hydrocarbon tackifier resins and terpene resins are preferred from the viewpoints of compatibility with polyester and excellent heat resistance, and hydrocarbon tackifier resins are more preferred from the viewpoint of excellent active energy ray curability.
[0161] Examples of the hydrocarbon tackifier resin include various hydrocarbon resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated aromatic hydrocarbon resins, hydrogenated aliphatic hydrocarbon resins, coumarone resins, coumarone-indene resins, etc. Among these, aromatic hydrocarbon resins and hydrogenated aromatic hydrocarbon resins are preferred from the viewpoints of excellent tackiness and heat resistance.
[0162] Examples of the terpene resin include terpene resin, terpene phenol resin, aromatic modified terpene resin, etc. Specifically, α-pinene polymer, β-pinene polymer, dipentene polymer, and terpene resin obtained by modifying these with phenol, aromatic, hydrogenation, or hydrocarbon can be used. In addition, terpene phenol resin is preferable from the viewpoint of excellent compatibility with polyester (A) and tackiness.
[0163] Examples of the phenol-based resin that can be used include condensates of various phenols, such as phenol, m-cresol, 3,5-xylenol, p-alkylphenol, and resorcin, with formaldehyde.Furthermore, resol obtained by subjecting the phenols and formaldehyde to an addition reaction in the presence of an alkali catalyst, novolak obtained by subjecting the phenols and formaldehyde to a condensation reaction in the presence of an acid catalyst, and rosin-modified phenolic resin obtained by adding phenol to rosins, such as unmodified or modified rosin or derivatives thereof, in the presence of an acid catalyst, followed by thermal polymerization, can be used.
[0164] Examples of the rosin-based resin include rosin resin, polymerized rosin resin, hydrogenated rosin resin, rosin ester resin, hydrogenated rosin ester resin, rosin phenol resin, polymerized rosin ester, and the like. Specific examples of the rosin-based resin that can be used include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin, modified rosins obtained by hydrogenating, disproportionating, polymerizing, or otherwise chemically modifying these, and derivatives of these.
[0165] From the viewpoint of wet heat resistance, the tackifier resin preferably has an acid value of 30 mgKOH / g or less, particularly 15 mgKOH / g or less, further 10 mgKOH / g or less, particularly 6 mgKOH / g or less, and most preferably 3 mgKOH / g. When multiple types of tackifier resins are used in combination, the average thereof is preferably within the above range.
[0166] The softening point of the tackifier resin (measured, for example, by the ring and ball method) is preferably 60 to 170° C., more preferably 80 to 160° C., even more preferably 90 to 150° C., and particularly preferably 100 to 140° C. If the softening point is within the above range, tackiness and adhesive strength can be improved, which is preferable.
[0167] In the present invention, the tackifier resin is preferably derived from plants from the viewpoint of protecting the global environment. Examples of the tackifier resin derived from plants include terpene resins and rosin resins.
[0168] When a tackifier resin is used, its content is preferably 50 parts by mass or less, more preferably 0.1 to 30 parts by mass, even more preferably 1 to 20 parts by mass, particularly preferably 2 to 15 parts by mass, and especially preferably 3 to 10 parts by mass, relative to 100 parts by mass of the polyester (A). When the content is within the above range, tackiness and adhesive strength can be improved, which is preferable, and when the content is too high, the glass transition temperature of the adhesive layer increases, resulting in insufficient tackiness and adhesive strength, and the active energy ray curability tends to decrease.
[0169] <Composition> In the present composition, in addition to the polyester (A), the compound (B) having a photoreactive group, the compound (C) containing an unsaturated group, the crosslinking agent (D), the hydrolysis inhibitor (E), the antioxidant (F) and the tackifier resin, other components such as catalysts, plasticizers, ultraviolet absorbers, antistatic agents, silane coupling agents, fluxes, flame retardants, dispersants, emulsifiers, defoamers, leveling agents, ion trapping agents and other additives, as well as inorganic or organic fillers, powders such as metal powders and pigments, particulate additives and the like can be blended as long as the effects of the present invention are not impaired. In addition, the composition may contain a small amount of impurities contained in the manufacturing raw materials of the adhesive components. These can be used alone or in combination of two or more.
[0170] When the present composition contains these other components, the content thereof is preferably 70 mass % or less, more preferably 0.001 to 50 mass %, particularly preferably 0.005 to 30 mass %, and even more preferably 0.01 to 10 mass %, of the total composition.
[0171] The present composition can be obtained, for example, by preparing the polyester (A) and necessary optional components, mixing them during the production of the polyester (A), and dispersing them by heating and melting them, or by mixing them into a solution of the polyester (A) dissolved in an organic solvent, and dispersing them using a mixing roller or the like.
[0172] The melt viscosity (130°C) of the composition is preferably 500 Pa·s or less, more preferably 1 to 400 Pa·s, even more preferably 3 to 300 Pa·s, particularly preferably 5 to 200 Pa·s, especially preferably 10 to 150 Pa·s, and most preferably 15 to 100 Pa·s. If the melt viscosity is too low, the coating appearance will tend to have an orange peel, resulting in poor coatability, and the heat resistance, holding power, adhesive power, and wet heat durability will tend to be insufficient, while if the melt viscosity is too high, the coating appearance will tend to have streaks, resulting in insufficient coatability.
[0173] From the viewpoint of thermal stability and coatability, it is preferable that the melt viscosity change rate before and after a heat resistance test (temperature 200°C, 3 hours, under air conditions) is small. The melt viscosity change rate is preferably 20 to 500%, more preferably 30 to 400%, even more preferably 40 to 300%, particularly preferably 50 to 250%, especially preferably 60 to 200%, and most preferably 70 to 150%. If the melt viscosity change rate before and after the thermal history is out of the above range, the adhesive will gel or decompose, resulting in insufficient coatability, and insufficient adhesive strength and adhesion. The melt viscosity change rate (%) is calculated from the following formula. Melt viscosity change rate (%) = [(130°C melt viscosity after heat resistance test) / (130°C melt viscosity before heat resistance test)] × 100
[0174] The composition thus obtained has active energy ray curability even without an unsaturated group, and therefore has excellent thermal stability, and forms an adhesive having excellent adhesion and holding power. In particular, the composition is useful as a solventless active energy ray curable composition for use in adhesive tapes for electronic components, adhesive tapes for labels, etc.
[0175] <Organic Solvent> The present composition is preferably used as a solvent-free active energy ray-curable composition, but an organic solvent may be blended in order to appropriately adjust the viscosity of the pressure-sensitive adhesive composition and to facilitate handling when forming a coating film.
[0176] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; esters such as ethyl acetate, etc.; ethers such as ethylene glycol monomethyl ether, etc.; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, etc.; alcohols such as methanol, ethanol, etc.; alkanes such as hexane, cyclohexane, etc.; aromatics such as toluene, xylene, etc. Among these, ketone-based solvents and ester-based solvents are preferred from the viewpoint of VOC emission regulations, and particularly preferred are methyl ethyl ketone, cyclohexanone, and ethyl acetate, and more preferably methyl ethyl ketone and ethyl acetate, which have low boiling points and excellent drying efficiency. The above-mentioned solvents may be used alone or as a mixture of two or more kinds in any combination and ratio.
[0177] The content of the organic solvent is preferably less than 70% by mass, more preferably 50% by mass or less, even more preferably 30% by mass or less, particularly preferably 10% by mass or less, especially preferably 5% by mass or less, and most preferably 1% by mass or less, based on the composition (including the solvent). The lower limit is 0% by mass, and it is preferable that the composition does not contain a solvent. If the content of the solvent is too high, the amount of energy required to volatilize the solvent in the coating process increases, and the effect of reducing the environmental load tends to be insufficient.
[0178] <Active energy ray-curable composition> An active energy ray-curable composition according to one embodiment of the present invention contains a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, and the content of the polymerizable unsaturated group-containing compound (C) contained in the active energy ray-curable composition is less than 15 parts by mass relative to 100 parts by mass of the polyester (A). As the polyester (A) contained in the active energy ray-curable composition, the same polyesters as those explained above for the polyester (A) can be used. In addition, the active energy ray-curable composition may contain the compound (B) having a photoreactive group, the polymerizable unsaturated group-containing compound (C), the crosslinking agent (D), the hydrolysis inhibitor (E), the antioxidant (F), a tackifier resin, additives, and the like, which are explained in the present composition, and the preferable physical properties and contents thereof are also the same.
[0179] <Adhesive> The adhesive according to one embodiment of the present invention can be obtained by curing (crosslinking) this composition or the active energy ray-curable composition, and can provide an adhesive that exhibits excellent heat resistance, adhesive strength, and holding power. In the present invention, "crosslinking" means intentionally crosslinking the composition by heat and / or light, etc., more preferably by light, and particularly preferably by active energy rays such as ultraviolet rays and electron beams. The degree of crosslinking can be controlled depending on the desired physical properties and applications.
[0180] The degree of crosslinking can be confirmed by the gel fraction of the adhesive, which is preferably 1 to 100%, more preferably 3 to 90%, even more preferably 5 to 80%, particularly preferably 10 to 70%, especially preferably 15 to 60%, most preferably 20 to 50%, and especially preferably 25 to 45%. If the gel fraction is too low, the heat resistance, holding power, adhesive strength, and wet heat durability tend to be insufficient, and if it is too high, the tackiness and adhesive strength tend to be insufficient. The gel fraction is a measure of the degree of crosslinking, and is calculated, for example, by the following method. That is, an adhesive sheet (without a release sheet) in which an adhesive layer is formed on a polymer sheet (e.g., a PET film, etc.) serving as a substrate is wrapped in a 200-mesh SUS wire net, and immersed in toluene or ethyl acetate at 23°C for 24 hours, and the gel fraction is the mass percentage of the insoluble adhesive component remaining in the wire net after immersion relative to the mass of the adhesive component before immersion. However, the mass of the substrate is subtracted.
[0181] The pressure-sensitive adhesive can then be formed into a sheet-like pressure-sensitive adhesive layer to obtain a pressure-sensitive adhesive sheet. Such a pressure-sensitive adhesive layer is preferably formed on one or both sides of the supporting substrate. In the present invention, the term "sheet" is used to include the meanings of "film" and "tape."
[0182] <Adhesive sheet> The pressure-sensitive adhesive sheet can be produced, for example, as follows. The pressure-sensitive adhesive sheet can be produced according to a known general pressure-sensitive adhesive sheet production method. For example, the composition is applied to a substrate, dried, and a release sheet is attached to the opposite surface of the pressure-sensitive adhesive composition layer, followed by curing as necessary to obtain the pressure-sensitive adhesive sheet of the present invention having a pressure-sensitive adhesive layer containing a pressure-sensitive adhesive on a substrate.
[0183] Alternatively, the pressure-sensitive adhesive sheet of the present invention can be obtained by coating the composition on a release sheet, drying, laminating a substrate to the pressure-sensitive adhesive composition layer on the opposite side, and curing if necessary.
[0184] Alternatively, a substrate-less double-sided pressure-sensitive adhesive sheet can be produced by forming a pressure-sensitive adhesive layer on a release sheet and laminating a release sheet to the opposite side of the pressure-sensitive adhesive layer.
[0185] When using the obtained pressure-sensitive adhesive sheet or substrate-less double-sided pressure-sensitive adhesive sheet, the release sheet is peeled off from the pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is attached to an adherend.
[0186] Examples of the substrate include polyesters such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, polybutylene succinate, polylactic acid, polyethylene terephthalate / isophthalate copolymer, polybutylene adipate / terephthalate copolymer, hydroxybutyrate / hydroxyhexanoate copolymer, and polycaprolactone; polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; polyethylene fluoride resins such as polyvinyl fluoride, polyvinylidene fluoride, and polyethylene fluoride; polyamides such as nylon 6 and nylon 6,6; polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer. Examples of the substrate include a sheet made of at least one synthetic resin selected from the group consisting of polymers, polyvinyl alcohol, vinylon, etc.; cellulose-based resins such as cellulose triacetate and cellophane; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; fluororesins; polystyrene; polycarbonate; acrylonitrile-butadiene-styrene copolymers; acrylonitrile-styrene-acrylic acid ester copolymers; polyarylates; polyimides; cycloolefin polymers; urethane acrylate-based resins; polyesters; metal foils of aluminum, copper, and iron; paper such as fine paper and glassine paper; woven fabrics and nonwoven fabrics made of glass fiber, natural fibers, synthetic fibers, etc. These substrates can be used as a single layer or as a multilayered body in which two or more types are laminated.
[0187] Among these, substrates made of polyester, nonwoven fabric, and polyolefin resin are particularly preferred.
[0188] The substrate may be a foam substrate, for example, a foam sheet made of a synthetic resin foam such as polyurethane foam, polyethylene foam, polyacrylate foam, etc. Among these, polyurethane foam and polyethylene foam are preferred because of their excellent balance of heat resistance, conformability to the adherend, and adhesive strength.
[0189] The thickness of the substrate is, for example, preferably from 1 to 1000 μm, particularly preferably from 3 to 500 μm, further preferably from 5 to 250 μm, and particularly preferably from 10 to 100 μm.
[0190] As the release sheet, for example, a sheet made of any of the various synthetic resins exemplified above as the base material, paper, cloth, nonwoven fabric, etc. that has been subjected to a release treatment can be used. As the release sheet, it is preferable to use a silicone-based release sheet.
[0191] The composition may be applied using, for example, a hot melt roll coater, a glue gun, a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, or the like.
[0192] As drying conditions, the drying temperature is preferably 60 to 140° C., particularly preferably 80 to 120° C., and the drying time is preferably 0.5 to 30 minutes, particularly preferably 1 to 5 minutes.
[0193] The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet or substrate-less double-sided pressure-sensitive adhesive sheet is preferably 1 to 500 μm, particularly preferably 3 to 200 μm, further preferably 5 to 100 μm, and particularly preferably 10 to 50 μm. If the thickness of the pressure-sensitive adhesive layer is too thin, the adhesive strength tends to decrease, whereas if the thickness is too thick, the uniformity of the coating film tends to decrease, resulting in poor appearance, or air bubbles tend to enter the coating film, resulting in insufficient optical properties.
[0194] The thickness of the adhesive layer is determined by subtracting the measured thickness of the components other than the adhesive layer from the measured thickness of the entire adhesive sheet using a Mitutoyo ID-C112B.
[0195] Furthermore, such a pressure-sensitive adhesive sheet may be protected by providing a release sheet on the outer side of the pressure-sensitive adhesive layer, if necessary. In a pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive layer is formed on one side of a substrate, the substrate may be subjected to a release treatment on the side opposite to the pressure-sensitive adhesive layer, and the release-treated surface may be used to protect the pressure-sensitive adhesive layer. EXAMPLES
[0196] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.
[0197] The glass transition temperature (°C), acid value (mgKOH / g), hydroxyl value (mgKOH / g), epoxy group concentration (mmol / g), ester bond concentration (mmol / g), unsaturated group concentration (mmol / g), crystalline heat of fusion (J / g), number average molecular weight (Mn), weight average molecular weight (Mw), peak top molecular weight (Mp), polydispersity, melt viscosity (Pa s), and biomass degree were measured as described in this specification.
[0198] <Production of Polyester (A)> The compositions shown in Table 1 below are the composition ratios of the finished product (resin composition ratios), and are the relative ratios (molar ratios) of the amounts of the constituent monomers of the obtained polyester and their mass %.
[0199] [Production of Polyester (A-1)] In a reaction vessel equipped with a thermometer, a stirrer, a rectification column, and a nitrogen inlet tube, 96.1 parts of isophthalic acid (IPA) as a polyvalent carboxylic acid (α), 467.8 parts of sebacic acid (SebA), 130.3 parts of 1,4-butanediol (1,4BG) as a polyhydric alcohol (β), 271 parts of neopentyl glycol (NPG), 29.7 parts of 1,6-hexanediol (1,6HG), 5 parts of trimethylolpropane (TMP), and 0.1 parts of tetrabutyl titanate as a catalyst were charged, and the internal temperature was raised to 260°C over 2.5 hours, and an esterification reaction was carried out at 260°C for 1.5 hours. Next, 0.1 parts of tetrabutyl titanate was added as a catalyst, the pressure inside the system was reduced to 2.5 hPa, and a polymerization reaction was carried out over 2 hours to obtain polyester (A-1).
[0200] [Production of Polyesters (A-2, A-3)] Polyesters (A-2, A-3) were obtained in the same manner as A-1, except that the resin composition was changed as shown in Table 1 below.
[0201] The resin composition of the obtained polyester (structural units derived from the components) is shown in Table 1, and various physical properties are shown in Table 2. In addition, the abbreviations in Table 1 are as follows. [Polycarboxylic acid (α)] [Saturated aliphatic dicarboxylic acids (α1-1)] ·SebA: Sebacic acid (derived from biomass) AdA: Adipic acid · SuA: succinic acid (derived from biomass) [Aromatic polycarboxylic acids (α2)] ·IPA: Isophthalic acid [Polyhydric alcohol (β)] [Straight-chain aliphatic polyhydric alcohol (β1-1)] ·EG: Ethylene glycol (derived from biomass) 1,3PG: 1,3-propanediol (derived from biomass) 1,4BG: 1,4-butanediol (derived from biomass) 1,6HG: 1,6-Hexanediol [Branched aliphatic polyhydric alcohol (β1-2) having a hydrocarbon group in at least one side chain] NPG: Neopentyl glycol ·TMP: Trimethylolpropane
[0202] [Table 1]
[0203] [Table 2]
[0204] <Compound (B) Having a Photoreactive Group> As the compound (B) having a photoreactive group, the following was prepared. (b1-1(1)): Benzophenone (IGM REJINS, a compound having a benzophenone-based hydrogen abstraction type photoreactive group, "Omnirad BP Flake") (b1-1(2)): 4-methylbenzophenone (IGM REJINS, a compound having a benzophenone-based hydrogen abstraction type photoreactive group, "Omnirad 4MBZ Flakes")
[0205] <Hydrolysis inhibitor (E)> The following hydrolysis inhibitors were prepared: (E-1): Bis(diisopropylphenyl)carbodiimide (manufactured by Rhein Chemie, monomeric carbodiimide compound "Stabaxol I Powder")
[0206] <Acid value inhibitor (F)> The following antioxidants were prepared: (F-1): Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF Japan, hindered phenol antioxidant "Irganox1010")
[0207] <Production of Pressure-Sensitive Adhesive Composition> A pressure-sensitive adhesive composition was produced as described below using the polyester (A) obtained above, the compound having a photoreactive group (B), the unsaturated group-containing compound (C), the hydrolysis inhibitor (E), and the antioxidant (F).
[0208] Example 1 100 parts of the polyester (A-1) obtained above was mixed with 5 parts of a compound (B1-1) having a hydrogen abstraction type photoreactive group, 1 part of a hydrolysis inhibitor (E-1), and 0.1 part of an antioxidant (F-1), and the mixture was stirred and mixed at 130°C for 1 hour to obtain a pressure-sensitive adhesive composition.
[0209] (Examples 2 to 4, Comparative Example 1) A pressure-sensitive adhesive composition was obtained in the same manner as in Example 1, except that the components were blended as shown in Table 3.
[0210] <PET-based adhesive sheet with one-sided release film> The adhesive composition obtained above was applied to a polyethylene terephthalate (PET) film (Toray Industries, Inc., Lumirror T60, thickness 38 μm) to a thickness of about 25 μm, and then a release-treated PET film (release film) (Mitsui Chemicals Tocello, Inc., SP-PET-01-BU, thickness 38 μm) was attached to the adhesive layer to protect its surface, and the adhesive layer was then irradiated with a high-pressure mercury UV irradiation device at a peak irradiance of 150 mW / cm. 2 The adhesive sheet was irradiated with ultraviolet light at an integrated light quantity of 150 mJ or 3000 mJ to obtain a PET substrate pressure-sensitive adhesive sheet with a one-sided release film.
[0211] The resulting PET-based pressure-sensitive adhesive sheet with a single-sided release film was subjected to the following evaluations. The evaluation results are shown in Table 3 below.
[0212] [Gel fraction] The PET adhesive sheet with one-sided release film obtained above was cut into a size of 4 cm x 4 cm, and the release film was peeled off. This was wrapped in a 200-mesh SUS wire net and immersed in toluene at 23°C for 24 hours, and the mass of the insoluble adhesive component remaining in the wire net relative to the mass of the adhesive component before immersion, minus the mass of the PET substrate, was measured, and the mass percentage was calculated according to the following formula to obtain the gel fraction (%). Gel fraction (%) = Mass of undissolved adhesive component remaining in the wire mesh after immersion / Mass of adhesive component before immersion × 100
[0213] [Adhesive strength (peel strength) (to SUS-BA)] A SUS-BA plate was prepared as an adherend. The PET adhesive sheet with one-sided release film obtained above was cut to 25 mm x 200 mm in an environment of 23 ° C and 50% RH, and then the release film was peeled off, and the adhesive layer side was pressed and attached to a SUS-BA plate by rolling a 2 kg roller twice. Then, after leaving it for 30 minutes in the same atmosphere, the 180 degree peel strength (N / 25 mm) was measured using an autograph (Shimadzu Corporation, Autograph AG-X 50N) at a peel speed of 300 mm / min, and evaluated according to the following evaluation criteria. (Evaluation Criteria) ◎ Adhesive strength of 5N / 25mm or more, no adhesive residue on the substrate 〇 Adhesive strength is 3N / 25mm or more and less than 5N / 25mm, and no adhesive residue remains on the substrate. △ Adhesive strength is 1N / 25mm or more and less than 3N / 25mm, and no adhesive residue remains on the substrate. × Adhesive strength is less than 1N or glue remains on the substrate
[0214] [Holding power] The PET-based adhesive sheet with one-sided release film obtained above was cut to a size of 25mm x 50mm in an environment of 23°C and 50% RH, the release film was then peeled off, and the sheet was pressed and attached to a stainless steel plate (SUS304) by rolling a 2kg roller back and forth twice (attached area 25mm x 25mm), and the holding power was measured for 24 hours at 40°C under a load of 1kg using a creep tester (Tester Sangyo Co., Ltd., holding power tester BE-501 with constant temperature and humidity chamber). The evaluation criteria are as follows. (Evaluation Criteria) 〇 No misalignment △ Misalignment is 1.0 mm or less × Misalignment is greater than 1.0 mm or the product has fallen
[0215] [Thermal stability] A heat resistance test (temperature 200°C, 3 hours, in air) was conducted using the PET substrate adhesive sheet with one-sided release film that had not been exposed to UV rays, and the melt viscosity at 130°C was measured before and after the heat resistance test using a flow tester "CFT-500EX" (manufactured by Shimadzu Corporation). The rate of change in melt viscosity was calculated using the following formula and evaluated. Melt viscosity change rate (%) = [(130°C melt viscosity after heat resistance test) / (130°C melt viscosity before heat resistance test)] × 100 (Evaluation Criteria) ◎ More than 30% and up to 300% ○: Between 20% and 30%, or between 300% and 500% △: Between 10% and 20%, or between 500% and 1000% × Less than 10% or more than 1000%
[0216] [Table 3]
[0217] The results in Table 3 above show that in the present invention, the adhesive compositions and adhesive layers of the adhesive sheets of Examples 1 to 4 have excellent active energy ray curability, and further have excellent adhesive strength, holding strength, and thermal stability, despite not containing unsaturated groups. In contrast, the adhesive composition and the adhesive layer of the adhesive sheet of Comparative Example 1 were poor in active energy ray curability, adhesive strength, and holding power, and did not satisfy the object of the present invention. [Industrial Applicability]
[0218] The composition contains a polyester made of a polyvalent carboxylic acid and a polyhydric alcohol, and a compound having a photoreactive group, and since it has active energy ray curing properties even without an unsaturated group, it forms an adhesive having excellent thermal stability, adhesion and holding power. In particular, the adhesive composition is useful as a solventless adhesive for electronic components, labels, etc.
Claims
1. An active energy ray-curable composition comprising a polyester (A) having a structural unit derived from a polyvalent carboxylic acid (α) and a structural unit derived from a polyhydric alcohol (β), and a compound (B) having a photoreactive group, The content of the polymerizable unsaturated group-containing compound (C) contained in the active energy ray-curable composition is less than 15 parts by mass based on 100 parts by mass of the polyester (A).
2. The active energy ray-curable composition according to claim 1, wherein the compound (B) having a photoreactive group is a compound (b1) having a hydrogen abstraction type photoreactive group and / or a compound (b2) having a cleavage type photoreactive group.
3. 2. The active energy ray-curable composition according to claim 1, wherein the compound (B) having a photoreactive group is a compound having a hydrogen abstraction type photoreactive group.
4. The active energy ray-curable composition according to claim 1 , wherein the compound (B) having a photoreactive group does not have a carboxy group or a hydroxy group as a functional group.
5. 2. The active energy ray-curable composition according to claim 1, wherein the glass transition temperature of the polyester (A) is −80 to 30° C.
6. 2. The active energy ray-curable composition according to claim 1, wherein the weight average molecular weight of the polyester (A) is 5,000 to 500,000.
7. The active energy ray-curable composition according to claim 1 , wherein the polyester (A) has an unsaturated group concentration of 1 mmol / g or less.
8. The active energy ray-curable composition according to claim 1, wherein the epoxy group concentration of the polyester (A) is 5 mmol / g or less.
9. 2. The active energy ray-curable composition according to claim 1, which has a melt viscosity change rate of 20 to 500% before and after heating at 200° C. for 3 hours.
10. The active energy ray-curable composition according to claim 1 , wherein the content of the organic solvent in the active energy ray-curable composition is less than 70 mass %.
11. A pressure-sensitive adhesive which is a cured product of the active energy ray-curable composition according to claim 1.
12. The pressure-sensitive adhesive according to claim 11, wherein the pressure-sensitive adhesive has a gel fraction of 1 to 100%.
13. A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive according to claim 11.
Citation Information
Patent Citations
Photo crosslinkable polyester adhesive composition
JP2009102476A
Pressure-sensitive adhesive for optical member and optical member, and photo- and / or heat-crosslinking pressure-sensitive adhesive composition for optical member
JP2009209279A
Radiation-curable, repeelable self-adhesive sheet
JP2010059336A
Pressure-sensitive adhesive made from UV-cured vegetable oil-based polyester
JP2022535379A
Cited By
Adhesive composition, bonding film, laminate equipped with adhesive layer, electromagnetic shield material, and laminate