Organic semiconductor thin film and method for manufacturing the same
By applying organic semiconductor molecules with acid groups and gaseous amines, the method addresses solubility and crystallization issues, resulting in highly crystalline thin films for improved performance evaluation.
Patent Information
- Application Number
- JP2023060328
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing organic semiconductor thin films face challenges in forming stable films due to low solubility of materials and difficulty in crystallization, particularly when combining acids and amines in solvents, which affects the evaluation of their physical properties.
A method involving applying a solvent containing organic semiconductor molecules with acid groups to a substrate and then contacting them with gaseous amines, specifically using sulfonic acid groups and alkylamines, to form crystalline organic semiconductor thin films.
This approach enables the production of highly crystalline organic semiconductor thin films, enhancing their physical properties and facilitating the evaluation of their performance in devices.
Smart Images

Figure 2024147364000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic semiconductor thin film and a method for producing the same. [Background technology]
[0002] Organic semiconductors are important materials that are expected to play a key role in next-generation technology, and various research projects have been conducted on them up to the present day. The physical properties of organic semiconductors are affected not only by the structure of the organic semiconductor molecules, but also by their arrangement. For example, in a previous report by the present inventors (Non-Patent Document 1), single crystals were produced from organic semiconductor molecules having sulfonic acid groups and amines. In this case, the arrangement of the organic semiconductor molecules in the crystals could be changed by changing the type of amine. [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] R. Akai, K. Oka, N. Tohnai et al., Bull. Chem. Soc. Jpn. 2022, 95, 1178-1182. Summary of the Invention [Problem to be solved by the invention]
[0004] In many cases, the organic semiconductor in an organic semiconductor device is in the form of a thin film, and therefore, in order to evaluate the performance of the organic semiconductor device, it is preferable to evaluate the physical properties of the organic semiconductor thin film.
[0005] However, Non-Patent Document 1 discloses a method for producing single crystals (particulate) of an organic semiconductor, but does not disclose a method for producing an organic semiconductor thin film. Furthermore, the salts produced in this document are made of sulfonic acid and amine, and depending on the type of amine, the solubility in a solvent may not be very high, making it difficult to form a thin film through a solution.
[0006] Furthermore, the method of mixing an acid and an amine in a solvent and then crystallizing them, as described in Non-Patent Document 1, may be difficult to apply depending on the combination of materials, since the solubility of the materials in the solvent decreases.
[0007] An object of one aspect of the present invention is to provide a novel method for producing an organic semiconductor thin film. [Means for solving the problem]
[0008] The present invention includes the following aspects. <1> A method for producing an organic semiconductor thin film, comprising the steps of: Step 1: applying a solvent containing organic semiconductor molecules having an acid group to a substrate; Step 2: A step of contacting the organic semiconductor molecules having an acid group applied to the substrate with an amine in a gas phase. <2> The acid group is a sulfonic acid group. <1> The manufacturing method described in <3> The amine is an alkylamine. <1> or <2> The manufacturing method described in <4> A crystalline organic semiconductor thin film comprising an organic semiconductor molecule having an acid group and an amine. <5> The acid group is a sulfonic acid group. <4> The organic semiconductor thin film according to claim 1. <6> The amine is an alkylamine. <4> or <5> The organic semiconductor thin film according to claim 1. <7> <4> ~ <6> 2. An organic semiconductor device comprising the organic semiconductor thin film according to any one of claims 1 to 11. Effect of the Invention
[0009] According to one aspect of the present invention, a novel method for producing an organic semiconductor thin film is provided. [Brief description of the drawings]
[0010] [Figure 1]1 is an XRD spectrum of a BTDBS / nBuA thin film according to Example 1A. [Diagram 2] 1 is an XRD spectrum of a BTDBS / sBuA thin film according to Example 1B. [Diagram 3] 1 is an XRD spectrum of a BTDBS / tBuA thin film according to Example 1C. [Figure 4] 1 is an XRD spectrum of a BTDBS / nBuA thin film according to Example 2A. [Diagram 5] 1 is an XRD spectrum of a BTDBS / sBuA thin film according to Example 2B. [Figure 6] 1 is an XRD spectrum of a BTDBS / tBuA thin film according to Example 2C. [Figure 7] 1 is an XRD spectrum of a BTBTDS / nBuA thin film according to Example 3A. [Figure 8] 1 is an XRD spectrum of a BTBTDS / sBuA thin film according to Example 3B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An embodiment of the present invention will be described below. However, the present invention is not limited to each of the configurations described below. The present invention can be modified in various ways within the scope of the claims. The technical scope of the present invention also extends to embodiments or examples obtained by appropriately combining multiple technical means disclosed in this specification. In this case, multiple technical means may be disclosed across multiple embodiments or examples.
[0012] Unless otherwise specified in this specification, "A to B" expressing a numerical range means "A or more, and B or less."
[0013] 1. Method for producing organic semiconductor thin film A method for producing an organic semiconductor thin film according to one embodiment of the present invention includes steps 1 and 2. Step 1 is a step of applying a solvent containing organic semiconductor molecules having an acid group to a substrate. Step 2 is a step of contacting the organic semiconductor molecules having an acid group applied to the substrate with an amine in a gas phase. Each step will be described in detail below.
[0014] [1.1.Process 1] In step 1, the organic semiconductor molecule having an acid group has an organic semiconductor skeleton and an acid group. The organic semiconductor skeleton is the molecular skeleton of an organic semiconductor compound commonly used in this technical field. Therefore, it can be said that the organic semiconductor molecule having an acid group is a molecule in which some hydrogen atoms contained in an organic semiconductor compound commonly used in this technical field are substituted with acid groups.
[0015] The organic semiconductor framework generally includes a π-electron conjugated system. The number of atoms included in the π-electron conjugated system (excluding hydrogen atoms) can be, for example, 10 or more, 12 or more, or 14 or more. In one embodiment, the organic semiconductor framework includes an acene structure and / or a thiophene structure. In one embodiment, the atoms included in the organic semiconductor framework are any of carbon atoms, hydrogen atoms, oxygen atoms, nitrogen atoms, and sulfur atoms.
[0016] The type of acid group contained in the organic semiconductor molecule having an acid group is not particularly limited. In one embodiment, the acid group is one or more selected from the group consisting of a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group. A sulfonic acid group is preferred in that it is easy to form a stable crystal together with an amine.
[0017] The number and position of the acid groups contained in the organic semiconductor molecule having the acid group are not particularly limited. The number of acid groups is, for example, an even number, preferably 2. The positions of the acid groups are preferably point-symmetric positions on the organic semiconductor skeleton. With such a molecular design, the organic semiconductor skeleton is easily oriented when reacted with an amine, and therefore crystals are easily formed.
[0018] Examples of organic semiconductor molecules having acid groups include the following: Further examples include molecules in which one or both of the sulfonic acid groups in the following structural formula are substituted with a carboxylic acid group or a phosphoric acid group (one sulfonic acid group may be substituted with a carboxylic acid group and the other sulfonic acid group may be substituted with a phosphoric acid group). [ka]
[0019] In one embodiment, the organic semiconductor molecule having an acid group is 4,4'-([2,2'-bithiophene]-5,5'-diyl)dibenzenesulfonic acid (BTDBS) or benzo[b]benzo[4,5]thieno[2,3-d]-2,7-disulfonic acid (BTBTDS).
[0020] The solvent in step 1 can be appropriately selected depending on the type of organic semiconductor molecule having an acid group. Usually, a solvent that dissolves the organic semiconductor having an acid group is selected. The concentration of the organic semiconductor having an acid group in the solvent can be appropriately set.
[0021] The substrate in step 1 is not particularly limited. For example, a substrate dedicated to the formation of an organic semiconductor thin film may be used. In this case, the obtained organic semiconductor thin film can be transferred by roll-to-roll or the like to assemble an organic semiconductor device. As another example, a member constituting an organic semiconductor device may be used as the substrate.
[0022] Examples of the coating method in step 1 include drop casting, spin coating, inkjet printing, letterpress printing, intaglio printing, and lithographic printing.
[0023] [1.2.Process 2] In step 2, the amine is a compound in which one or more of the three hydrogen atoms contained in the ammonia molecule are substituted with a carbon-containing group. According to previous research by the present inventors, the orientation of the organic semiconductor skeleton can be changed by changing the bulkiness of the carbon-containing group of the amine, and thus the physical properties of the organic semiconductor can be changed.
[0024] Examples of amines include alkylamines and arylamines. Of these, alkylamines are preferred. Other examples of amines include primary amines, secondary amines, and tertiary amines. Of these, primary amines are preferred.
[0025] Examples of primary amine alkylamines include methaneamine, ethanamine, propan-1-amine, butan-1-amine, pentan-1-amine, hexane-1-amine, heptan-1-amine, propan-2-amine, 2-methylpropan-1-amine, butan-2-amine, 2-methylpropan-2-amine, 2-methylbutan-1-amine, pentan-3-amine, cyclopropanamine, and cyclopentanamine. Examples of secondary amine alkylamines include dimethylamine, diethylamine, dipropylamine, dibutylamine, diisopropylamine, pyrrolidone, piperidine, and azepine. Examples of tertiary amine alkylamines include trimethylamine, N,N-dimethylethanamine, N-ethyl-N-isopropylpropan-2-amine, 1-methylpyrrolidone, and 1-methylpiperidine.
[0026] In one embodiment, the amine is butan-1-amine (n-butylamine), butan-2-amine ((rac)-sec-butylamine) or 2-methylpropan-2-amine (tert-butylamine).
[0027] In step 2, since the amine is volatile at room temperature (e.g., 20° C.), a special operation for vaporizing the amine is not essential. However, the amine may be vaporized by heating the amine or reducing the pressure of a system containing the amine.
[0028] There are no particular limitations on the conditions for contacting the organic semiconductor molecule having an acid group with the amine in step 2. The temperature and time for contacting can be appropriately selected by those skilled in the art depending on the materials used.
[0029] The organic semiconductor having an acid group, the substrate, and the coating method are as described in Section [1.1.].
[0030] [1.3. Other processes] The method for producing an organic semiconductor thin film may include a step other than step 1 and step 2.
[0031] In one embodiment, the manufacturing method includes a step of immersing the thin film formed on the substrate in a solvent. This dissolves and removes excess amine attached to the substrate. Therefore, it is preferable to select a solvent that dissolves amine but does not dissolve organic semiconductor molecules having acid groups. Examples of such solvents include ether. Examples of ethers include dimethyl ether, diethyl ether, methyl ethyl ether, and tetrahydrofuran.
[0032] In one embodiment, the manufacturing method includes a step of annealing the thin film formed on the substrate. The annealing is to leave the thin film at a temperature lower than the temperature in step 2 and higher than room temperature (e.g., 20°C). The annealing temperature and time can be appropriately selected by those skilled in the art.
[0033] [2. Organic Semiconductor Thin Films and Organic Semiconductor Devices] The crystalline organic semiconductor thin film according to one aspect of the present invention includes an organic semiconductor molecule having an acid group and an amine. The organic semiconductor molecule having an acid group and the amine are as described in Section [1]. In one embodiment, the crystalline organic semiconductor thin film is manufactured by the above-mentioned manufacturing method.
[0034] The organic semiconductor thin film is crystalline. Whether the organic semiconductor thin film is crystalline or not can be determined by the XRD spectrum. If the XRD spectrum of the organic semiconductor thin film has a peak, the organic semiconductor thin film is crystalline. In one embodiment, the XRD spectrum of the organic semiconductor thin film has the same peak as the XRD spectrum of the powder crystal formed by the organic semiconductor molecule having an acid group and an amine.
[0035] The organic semiconductor thin film is preferably composed of organic semiconductor molecules having one type of acid group and one type of amine. By selecting materials in this way, a crystalline organic semiconductor thin film can be easily obtained.
[0036] The lower limit of the area of the organic semiconductor thin film is 1 μm 2 The upper limit of the area of the organic semiconductor thin film is 100 cm. 2 The lower limit of the thickness of the organic semiconductor thin film may be 2 nm or more. The upper limit of the thickness of the organic semiconductor thin film may be 1 mm or less. Due to such characteristic features in the shape, the organic semiconductor thin film can be distinguished from particulate organic semiconductors.
[0037] An organic semiconductor device according to an embodiment of the present invention includes the organic semiconductor thin film described above. Examples of the organic semiconductor device include an organic thin film transistor, an organic solar cell, and an organic light-emitting diode. EXAMPLES
[0038] The following abbreviations are used for the materials used in this example. [ka]
[0039] [Example 1: Preparation of BTDBS thin film] A thin film containing BTDBS and amine was prepared by a manufacturing method according to one embodiment of the present invention. The crystallinity of the obtained thin film was examined by XRD. The manufacturing procedure of the thin film is as follows. 1. BTDBS was dissolved in DMSO to prepare an 8 mg / mL solution. 2. The solution was drop-cast onto a glass preparation and then dried at 100°C. 3. The preparation was placed in a mayonnaise jar, and then the amine was allowed to diffuse by vapor. The reaction temperature was 30°C or 60°C. The reaction time was 12 hours. In this way, a BTDBS / amine thin film was obtained.
[0040] [Example 1A: Preparation of BTDBS / nBuA thin film] Using nBuA as the amine, a BTDBS / nBuA thin film was prepared. The normalized XRD spectrum is shown in Figure 1. For reference, the XRD spectrum based on a single crystal obtained by mixing BTDBS and nBuA in a solvent and the XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTDBS / nBuA thin film was obtained (see especially the peaks near 2θ = 3.1°, 6.2°, and 9.3°).
[0041] [Example 1B: Preparation of BTDBS / sBuA thin film] A thin film of BTDBS / sBuA was prepared using sBuA as the amine. The normalized XRD spectrum is shown in Figure 2. For reference, the XRD spectrum based on a single crystal obtained by mixing BTDBS and sBuA in a solvent and the XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a thin film of BTDBS / sBuA with high crystallinity was obtained (see especially the peaks near 2θ=3.9°, 7.8°, and 11.7°). Comparing the XRD spectra before normalization, the sample with a reaction temperature of 60°C had a higher peak. Therefore, it is possible that a thin film with high crystallinity can be obtained by increasing the reaction temperature.
[0042] [Example 1C: Preparation of BTDBS / tBuA thin film] A thin film of BTDBS / tBuA was prepared using tBuA as the amine. The normalized XRD spectrum is shown in Figure 3. For reference, the XRD spectrum based on a single crystal obtained by mixing BTDBS and sBuA in a solvent and the XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a thin film of BTDBS / sBuA with high crystallinity was obtained (see especially the peaks near 2θ=4.2°, 8.4°, and 12.6°). Comparing the XRD spectra before normalization, the sample with a reaction temperature of 60°C had a higher peak. Therefore, it is possible that a thin film with high crystallinity can be obtained by increasing the reaction temperature.
[0043] Example 2: Study of manufacturing conditions for BTDBS thin film The manufacturing conditions for the thin film in Example 1 were modified, and the crystallinity of the resulting thin film was examined by XRD. The modified manufacturing conditions were as follows. Condition 1: Immersion in ether 1. BTDBS was dissolved in DMSO to prepare an 8 mg / mL solution. 2. The solution was drop-cast onto a glass preparation and then dried at 100°C. 3. After placing the preparation in a mayonnaise jar, the amine was allowed to diffuse by vapor. The reaction temperature was 30°C. The reaction time was 12 hours. 4. The thin film obtained in step 3 was immersed in diethyl ether for 30 minutes, then taken out and dried. The operation in step 4 was repeated twice in total. In this way, a BTDBS / amine thin film was obtained. ●Condition 2: Annealing 1. BTDBS was dissolved in DMSO to prepare an 8 mg / mL solution. 2. The solution was drop-cast onto a glass preparation and then dried at 100°C. 3. After placing the preparation in a mayonnaise jar, the amine was allowed to diffuse by vapor. The reaction temperature was 30°C. The reaction time was 12 hours. 4. The thin film obtained in step 3 was annealed at 60° C. for 2 hours. In this way, a BTDBS / amine thin film was obtained. ●Condition 3: Shortening the crystallization time 1. BTDBS was dissolved in DMSO to prepare an 8 mg / mL solution. 2. The solution was drop-cast onto a glass preparation and then dried at 100°C. 3. The preparation was placed in a mayonnaise jar, and then the amine was allowed to diffuse by vapor. The reaction temperature was 60°C. The reaction time was 30 minutes. In this way, a BTDBS / amine thin film was obtained.
[0044] [Example 2A: Preparation of BTDBS / nBuA thin film] Using nBuA as the amine, a BTDBS / nBuA thin film was prepared under conditions 1 and 2. The normalized XRD spectrum is shown in FIG. 4. As a reference, the XRD spectrum based on the thin film prepared in Example 1A (thin film reacted at 60°C), a single crystal obtained by mixing BTDBS and nBuA in a solvent, and an XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTDBS / nBuA thin film was obtained (see especially the peaks near 2θ=3.1°, 6.2°, and 9.3°).
[0045] [Example 2B: Preparation of BTDBS / sBuA thin film] Using sBuA as the amine, a BTDBS / sBuA thin film was prepared under conditions 1 to 3. The normalized XRD spectrum is shown in FIG. 5. As a reference, the XRD spectrum based on the thin film prepared in Example 1B (thin film reacted at 60°C), a single crystal obtained by mixing BTDBS and sBuA in a solvent, and an XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTDBS / sBuA thin film was obtained (see especially the peaks near 2θ=3.9°, 7.8°, and 11.7°).
[0046] [Example 2C: Preparation of BTDBS / tBuA thin film] Using tBuA as the amine, a BTDBS / tBuA thin film was prepared under conditions 1 and 3. The normalized XRD spectrum is shown in FIG. 6. As a reference, the XRD spectrum based on the thin film prepared in Example 1C (thin film reacted at 60°C), a single crystal obtained by mixing BTDBS and tBuA in a solvent, and an XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTDBS / tBuA thin film was obtained (see especially the peaks near 2θ=4.2°, 8.4°, and 12.6°).
[0047] Example 3: Preparation of BTBTDS thin film A thin film containing BTBTDS and amine was prepared by a manufacturing method according to one embodiment of the present invention. The crystallinity of the obtained thin film was examined by XRD. The manufacturing procedure of the thin film is as follows. 1. BTBTDS was dissolved in DMSO to prepare a 5 mg / mL solution. 2. The solution was drop-cast onto a glass preparation and then dried at 100°C. 3. After placing the preparation in a mayonnaise jar, the amine was allowed to diffuse by vapor. The reaction temperature was 30°C or 60°C. The reaction time was 12 hours. In this way, a BTBTDS / amine thin film was obtained.
[0048] [Example 3A: Preparation of BTBTDS / nBuA thin film] Using nBuA as the amine, a BTBTDS / nBuA thin film was prepared. The normalized XRD spectrum is shown in Figure 7. For reference, the XRD spectrum based on a single crystal obtained by mixing BTBTDS and nBuA in a solvent and the XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTBTDS / nBuA thin film was obtained (see especially the peaks near 2θ = 3.8°, 7.6°, and 11.4°).
[0049] [Example 3B: Preparation of BTBTDS / sBuA thin film] A BTBTDS / sBuA thin film was prepared using sBuA as the amine. The normalized XRD spectrum is shown in Figure 8. For reference, the XRD spectrum based on a single crystal obtained by mixing BTBTDS and sBuA in a solvent and the XRD spectrum calculated by simulation are also shown. As can be seen from the figure, a highly crystalline BTBTDS / sBuA thin film was obtained (see especially the peaks near 2θ = 4.0°, 8.0°, and 12.0°). [Industrial Applicability]
[0050] The present invention can be used in organic semiconductor devices and the like.
Claims
1. A method for producing an organic semiconductor thin film, comprising the steps of: Step 1: applying a solvent containing organic semiconductor molecules having an acid group to a substrate; Step 2: A step of contacting the organic semiconductor molecules having an acid group applied to the substrate with an amine in a gas phase.
2. The method according to claim 1 , wherein the acid group is a sulfonic acid group.
3. The process according to claim 1 , wherein the amine is an alkylamine.
4. A crystalline organic semiconductor thin film comprising an organic semiconductor molecule having an acid group and an amine.
5. The organic semiconductor thin film according to claim 4 , wherein the acid group is a sulfonic acid group.
6. The organic semiconductor thin film according to claim 4 , wherein the amine is an alkylamine.
7. An organic semiconductor device comprising the organic semiconductor thin film according to any one of claims 4 to 6.