Method for manufacturing electrostatic charge image development toner
The method addresses uneven image density in toners by drying toner base particles with controlled airflow and specific resin composition, enhancing charge retention and image quality.
Patent Information
- Application Number
- JP2023060792
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Existing toners for developing electrostatic images suffer from uneven image density due to low charge retention performance, which is attributed to solvent residues and non-uniform solvent distribution within the toner base particles.
A method for producing toner by drying wet toner base particles using airflow at specific temperatures and speeds, incorporating amorphous polyester with controlled bisphenol A content and aliphatic polyhydric alcohols, and optionally crystalline polyester, to achieve uniform solvent distribution and improved charge retention.
The method effectively suppresses uneven image density by ensuring uniform solvent distribution and enhanced charge retention, resulting in high-quality image formation.
Smart Images

Figure 2024147980000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a toner for developing electrostatic images, and more particularly to a method for producing a toner for developing electrostatic images, which suppresses unevenness in density of the formed image. [Background technology]
[0002] As copiers and printers become more widespread, toners used in image formation to develop electrostatic images are required to have higher performance. In recent years, a digital printing technology called print-on-demand (POD), which prints directly without the plate-making process, has been attracting attention. POD is easier to use than conventional offset printing because it can handle short-run printing and variable printing in which the printing content is changed for each sheet. In addition, there is a growing demand for even faster printing speeds and energy savings in printing technology. In the following, the toner for developing electrostatic images will also be simply referred to as "toner".
[0003] Patent Document 1 discloses a technology for a toner in which the ratio of crystalline polyester contained in the toner base particles and the storage modulus of the toner are within specific ranges. Patent Document 2 discloses a technology for a toner in which the toner base particles contain a specific type of polyester.
[0004] These toners are high performance toners from the viewpoint of energy saving and the like, but have a problem in that the density of the formed image is easily uneven. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-66018 A [Patent Document 2] JP 2017-062344 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a method for producing a toner for developing electrostatic images, which suppresses unevenness in density of the formed images. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, the present inventors have investigated the causes of the above-mentioned problems, and as a result, have found that in a method for producing a toner for developing electrostatic images by drying wet toner base particles, by providing toner base particles with a specific composition and including a step of drying the wet toner base particles at a specific air flow temperature and speed using an air flow in a dryer, it is possible to suppress uneven density in images formed using the toner for developing electrostatic images, and have arrived at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0008] 1. A method for producing a toner for developing an electrostatic image, comprising drying wet toner base particles to produce a toner for developing an electrostatic image, comprising the steps of: the toner base particles contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from bisphenol A or a bisphenol A derivative in the amorphous polyester relative to the total number of moles of structural units derived from the polyhydric alcohol is 10 mol % or less; drying the wet toner base particles by airflow in a dryer; The temperature of the airflow is 60° C. or higher; The air flow speed is 5 m / sec or more. 2. A method for producing a toner for developing an electrostatic image, comprising the steps of:
[0009] 2. The amorphous polyester does not have a structural unit derived from bisphenol A or a bisphenol A derivative as a structural unit derived from the polyhydric alcohol. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0010] 3. The polyhydric alcohol is an aliphatic polyhydric alcohol having 5 to 7 carbon atoms. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0011] 4. The content of the amorphous polyester is 20% by mass or more based on the total mass of the toner base particles. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0012] 5. The glass transition temperature of the amorphous polyester is within the range of 30 to 70° C. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0013] 6. The glass transition temperature of the electrostatic image developing toner is within the range of 15 to 40° C. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0014] 7. The toner base particles contain crystalline polyester 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0015] 8. The melting point of the crystalline polyester is 75°C or less. 8. The method for producing a toner for developing electrostatic images according to claim 7.
[0016] 9. The crystalline polyester has a structural unit derived from an aliphatic diol and a structural unit derived from an aliphatic carboxylic acid. 8. The method for producing a toner for developing electrostatic images according to claim 7.
[0017] 10. The number of carbon atoms contained in the aliphatic diol or the aliphatic carboxylic acid is within the range of 6 to 10. 10. The method for producing a toner for developing electrostatic images according to claim 9.
[0018] 11. The toner base particles contain a release agent, The melting point of the release agent is within the range of 60 to 80°C. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0019] 12. The toner base particles have a core-shell structure. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0020] 13. The speed of the airflow is within the range of 8 to 20 m / sec. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0021] 14. The content of the solvent in the wet toner base particles is within the range of 15 to 30% by mass. 2. The method for producing a toner for developing electrostatic images according to claim 1,
[0022] 15. The method includes a step of removing the solvent from the wet toner base particles before the drying step. 2. The method for producing a toner for developing electrostatic images according to claim 1, Effect of the Invention
[0023] According to the above-mentioned means of the present invention, it is possible to provide a method for producing a toner for developing an electrostatic image, which suppresses unevenness in density of the formed image.
[0024] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.
[0025] The unevenness in density of an image formed using a toner is caused by the toner's low charge retention performance. More specifically, if the charge of a charged toner is prone to leak, the toner cannot retain the desired charge and cannot adhere to the desired position on a recording medium. As a result, the unevenness in density of the image occurs.
[0026] In a method for producing a toner by drying wet toner base particles, even if the toner base particles are sufficiently dried, solvent such as water remains in the toner base particles. It has been found that the amount of the remaining solvent and the state of the solvent in the toner base particles affect the ease of charge leakage.
[0027] The toner produced by the production method of the present invention has toner base particles containing an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, and the content of structural units derived from bisphenol A or a bisphenol A derivative in the amorphous polyester relative to the total number of moles of structural units derived from the polyhydric alcohol is 10 mol % or less.
[0028] In this way, by making the binder resin of the toner base particles have a specific composition, it is easy to make the bond distance of the ester bonds in the binder resin uniform, and it is difficult to form a part where the ester groups are locally highly dense. More specifically, it is believed that the hydrophilic parts derived from the ester bonds and the hydrophobic parts derived from the hydrocarbon groups are appropriately dispersed, which makes it possible to suppress the leakage of electric charges.
[0029] The toner production method of the present invention further comprises a step of drying the wet toner base particles with an air current in a dryer, the temperature of the air current being 60° C. or higher and the speed of the air current being 5 m / sec or higher.
[0030] It is believed that by drying the toner base particles at a relatively high temperature and rapidly in this manner, the state of the solvent in the toner base particles can be made uniform. More specifically, it is believed that the solvent adsorbed on the outermost layer of the toner base particles can be sufficiently removed and the solvent inside the toner base particles can be uniformly dispersed. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 is an explanatory diagram showing an example of a flash dryer. [Diagram 2] An explanatory diagram showing an example of a plant for performing continuous drying treatment. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing a configuration of an example of an image forming apparatus. [Figure 4] Schematic diagram showing the measurement points of reflection density in the evaluation of image unevenness DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The method for producing a toner for developing electrostatic images of the present invention is a method for producing a toner for developing electrostatic images by drying wet toner base particles, characterized in that the toner base particles contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, and the content of structural units derived from bisphenol A or a bisphenol A derivative in the amorphous polyester relative to the total number of moles of structural units derived from the polyhydric alcohol is 10 mol % or less, the method includes a step of drying the wet toner base particles with an airflow in a dryer, and the temperature of the airflow is 60° C. or higher and the speed of the airflow is 5 m / sec or higher. This feature is a technical feature common to or corresponding to the following embodiments.
[0033] In an embodiment of the present invention, from the viewpoint of charge retention performance, it is preferable that the amorphous polyester does not contain a structural unit derived from bisphenol A or a bisphenol A derivative as a structural unit derived from the polyhydric alcohol.
[0034] In an embodiment of the present invention, from the viewpoint of charge retention performance, the polyhydric alcohol is preferably an aliphatic polyhydric alcohol having 5 to 7 carbon atoms.
[0035] In an embodiment of the present invention, from the viewpoint of low-temperature fixability, the content of the amorphous polyester is preferably 20% by mass or more with respect to the total mass of the toner base particles.
[0036] In an embodiment of the present invention, from the viewpoint of achieving both low-temperature fixability and heat-resistant storage stability, the glass transition temperature of the amorphous polyester is preferably within the range of 30 to 70°C.
[0037] In an embodiment of the present invention, from the viewpoint of achieving both low-temperature fixability and heat-resistant storage stability, the glass transition temperature of the toner for developing electrostatic images is preferably within the range of 15 to 40°C.
[0038] In an embodiment of the present invention, from the viewpoint of low-temperature fixability, the toner base particles preferably contain a crystalline polyester, and the melting point of the crystalline polyester is preferably 75° C. or less.
[0039] In an embodiment of the present invention, from the viewpoint of achieving both low-temperature fixability and charge retention performance, the crystalline polyester preferably has a structural unit derived from an aliphatic diol and a structural unit derived from an aliphatic carboxylic acid, and the number of carbon atoms contained in the aliphatic diol or the aliphatic carboxylic acid is preferably within the range of 6 to 10.
[0040] In an embodiment of the present invention, from the viewpoint of separation property during toner fixing, it is preferable that the toner base particles contain a release agent, and that the melting point of the release agent is within the range of 60 to 80°C.
[0041] In an embodiment of the present invention, from the viewpoint of achieving both low-temperature fixability and heat-resistant storage stability, it is preferable that the toner base particles have a core-shell structure.
[0042] In an embodiment of the present invention, from the viewpoint of charge retention performance, the speed of the airflow is preferably within a range of 8 to 20 m / sec.
[0043] In an embodiment of the present invention, from the viewpoint of charge retention performance, the content of the solvent in the wet toner base particles is preferably within a range of 15 to 30% by mass.
[0044] In an embodiment of the present invention, from the viewpoint of charge retention performance, it is preferable to have a step of removing the solvent from the wet toner base particles prior to the drying step.
[0045] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower and upper limits.
[0046] 1. Overview of the Invention The method for producing a toner for developing electrostatic images of the present invention is a method for producing a toner for developing electrostatic images by drying wet toner base particles, characterized in that the toner base particles contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, and the content of structural units derived from bisphenol A or a bisphenol A derivative in the amorphous polyester relative to the total number of moles of structural units derived from the polyhydric alcohol is 10 mol % or less, the method includes a step of drying the wet toner base particles with an airflow in a dryer, and the temperature of the airflow is 60° C. or higher and the speed of the airflow is 5 m / sec or higher.
[0047] That is, the toner base particles are given a specific composition, and the wet toner base particles are dried under specific conditions, thereby making it possible to obtain a toner with excellent charge retention performance and to suppress unevenness in the density of the formed image.
[0048] The composition of the toner for developing electrostatic images, the physical properties of the toner for developing electrostatic images, the structure of the toner for developing electrostatic images, the developer, a method for producing the toner for developing electrostatic images, an image forming method, and an image forming apparatus will be described in this order.
[0049] 2. Composition of toner for developing electrostatic images In this specification, the toner for developing electrostatic images is also simply referred to as "toner." The toner includes toner base particles. It is preferable that the toner base particles have an external additive attached to their surfaces. In addition, the term "toner base particles" refers to the material that constitutes the base of "toner particles." The "toner base particles" become "toner particles" when an external additive is added. And, "toner" refers to an aggregate of toner particles.
[0050] (1) Components of toner base particles The "toner base particles" according to the present invention preferably contain components such as a binder resin, a colorant, a wax, and a charge control agent, as necessary. The binder resin, the release agent, the colorant, and the charge control agent will be described below.
[0051] (1.1) Binder resin By including a binder resin in the toner base particles, the toner can be fixed onto a recording medium. The binder resin according to the present invention contains an amorphous polyester, which is a polycondensation product of a polyvalent carboxylic acid and a polyhydric alcohol. In addition, the binder resin may contain an amorphous resin other than the amorphous polyester and a crystalline resin, if necessary.
[0052] (Method of analyzing resin composition) The composition of each resin contained in the toner base particles can be analyzed by, for example, pyrolysis gas chromatography mass spectrometry (GC / MS: Gas Chromatography / Mass Spectrometry) method. Specifically, the amount of a monomer can be quantified by the standard addition method using a column and a detector that have been confirmed to be capable of detecting a monomer having a specific structure.
[0053] An example of detailed pyrolysis conditions and GC / MS measurement conditions is shown below. (Pyrolysis conditions) Measurement device: PY-2020iD (manufactured by Frontier Labs) Measurement mass: 0.1mg Heating temperature: 550℃ Heating time: 0.5 minutes
[0054] (GC / MS measurement conditions) Measuring device: QP2010 (Shimadzu Corporation) Column: UltraALLOY-5 (inner diameter: 0.25 mm, length: 30 m, thickness: 0.25 μm, manufactured by Frontier Labs) Temperature range: 40℃~320℃ (maintained at 320℃) Heating rate: 20℃ / min
[0055] (1.1.1) Amorphous resin In the present invention, "exhibiting amorphousness" means that in an endothermic curve obtained by differential scanning calorimetry (DSC), the material has a glass transition temperature (Tg) but does not have a melting point, i.e., a clear endothermic peak during heating. The clear endothermic peak means an endothermic peak with a half-width of 15°C or less in an endothermic curve when the material is heated at a heating rate of 10°C / min.
[0056] (1.1.1.1) Amorphous polyester From the viewpoint of low-temperature fixability, the toner according to the present invention contains an amorphous polyester. The term "amorphous polyester" refers to a polyester that exhibits amorphousness and is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (polycarboxylic acid) monomer and a divalent or higher alcohol (polyalcohol) monomer. Amorphous polyester can be synthesized by polycondensing (esterifying) the polyvalent carboxylic acid monomer and the polyalcohol monomer using a known esterification catalyst.
[0057] A polycarboxylic acid is a compound that contains two or more carboxy groups in one molecule. Examples of polyvalent carboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, mesaconic acid, dimethyl isophthalate, fumaric acid, dodecenylsuccinic acid, 1,10-dodecanedicarboxylic acid, etc. Among them, dimethyl isophthalate, terephthalic acid, dodecenylsuccinic acid, and trimellitic acid are preferable. These may be contained alone or in combination of two or more.
[0058] A polyhydric alcohol is a compound that contains two or more hydroxy groups in one molecule. Examples of polyhydric alcohols include dihydric alcohols such as ethylene glycol, propylene glycol, butanediol, diethylene glycol, pentanediol, neopentyl glycol, hexanediol, heptanediol, cyclohexanediol, octanediol, decanediol, and dodecanediol; trihydric or higher polyols such as glycerin, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, and tetraethylolbenzoguanamine; and ester compounds thereof; and hydroxycarboxylic acid derivatives. These may be contained alone or in combination of two or more.
[0059] In addition, from the viewpoint that bisphenols can be esterified like alcohols, in the present invention, the above-mentioned "polyhydric alcohol" includes bisphenol A or a derivative of bisphenol A. Examples of the derivative of bisphenol A include an ethylene oxide adduct of bisphenol A (BPA-EO) and a propylene oxide adduct of bisphenol A (BPA-PO).
[0060] Among them, the polyhydric alcohol is preferably an aliphatic polyhydric alcohol having 5 to 7 carbon atoms. Since an aliphatic polyhydric alcohol having 5 to 7 carbon atoms has a relatively small bulk, it is easy to make the bond distance of the ester bond uniform in the polyester obtained by synthesis. In addition, it is difficult to form a part where the ester group is locally highly dense. In detail, it is considered that the hydrophilic part derived from the ester bond and the hydrophobic part derived from the hydrocarbon group are appropriately dispersed, which can suppress the leakage of the electric charge.
[0061] In particular, aliphatic polyhydric alcohols having 5 to 7 carbon atoms are smaller in bulk than bisphenol A or derivatives of bisphenol A. Therefore, it is considered that aliphatic polyhydric alcohols having 5 to 7 carbon atoms can suppress charge leakage more effectively than bisphenol A or derivatives of bisphenol A.
[0062] Examples of the aliphatic polyhydric alcohol having 5 to 7 carbon atoms include pentanediol, neopentyl glycol, hexanediol, heptanediol, and cyclohexanediol.
[0063] From the viewpoint of suppressing charge leakage, the proportion of bisphenol A or a bisphenol A derivative in the polyhydric alcohol is preferably low. In the present invention, the content of structural units derived from bisphenol A or bisphenol A derivatives relative to the total number of moles of structural units derived from polyhydric alcohols is 10 mol % or less, which is believed to suppress charge leakage and uneven density of the formed image.
[0064] The content of structural units derived from bisphenol A or bisphenol A derivatives relative to the total number of moles of structural units derived from polyhydric alcohols is preferably lower, specifically, preferably 5 mol % or less, more preferably 1 mol % or less. The structural units derived from the polyhydric alcohol may not contain any structural units derived from bisphenol A or a bisphenol A derivative.
[0065] Examples of the esterification catalyst include alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; metal compounds such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds.
[0066] The polymerization temperature is not particularly limited, and is preferably within the range of, for example, 150 to 250° C. The polymerization time is not particularly limited, and is preferably within the range of, for example, 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0067] The content of the amorphous polyester is preferably 20% by mass or more, more preferably 50% by mass or more, based on the total mass of the binder resin, and is preferably 10% by mass or more, more preferably 40% by mass or more, based on the total mass of the toner base particles.
[0068] (Hybrid amorphous polyester resin) The amorphous polyester may be a hybrid crystalline polyester in which an amorphous polyester polymer segment and an amorphous polymer segment other than the amorphous polyester are chemically bonded.
[0069] (1.1.1.2) Glass transition temperature From the viewpoint of achieving both sufficient low-temperature fixability and heat-resistant storage stability, the glass transition temperature (Tg) of the amorphous resin is preferably within a range of 30 to 70°C, and more preferably within a range of 40 to 65°C.
[0070] For example, differential scanning calorimetry (DSC measurement) is performed using a differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI). Specifically, 5 mg of sample is sealed in an AL autosampler sample container φ6.8 H2.5 mm (manufactured by HITACHI) and an AL autosampler cover (manufactured by HITACHI). This is set in the sample holder of the "AS3 / DX" and the temperature is changed in the order of heating, cooling, and heating again. During the first and second heating, the temperature is raised from 0°C to 150°C at a heating rate of 10°C / min and held at 150°C for 1 minute. During cooling, the temperature is lowered from 150°C to 0°C at a cooling rate of 10°C / min and held at 0°C for 1 minute. In the measurement curve obtained during the second heating, a shift in the baseline is observed. The intersection point between the extension of the baseline before the shift and the tangent line showing the maximum slope of the shifted portion of the baseline is taken as the glass transition temperature (Tg). An empty aluminum pan is used as a reference.
[0071] (1.1.1.3) Weight average molecular weight The weight average molecular weight (Mw) of the amorphous resin is not particularly limited, and is preferably within the range of 10,000 to 100,000, for example. The weight average molecular weight of the amorphous resin can be measured in the same manner as the weight average molecular weight of the crystalline resin described below.
[0072] (1.1.2) Crystalline resins The toner base particles according to the present invention preferably contain a crystalline resin. By containing the crystalline resin, the crystalline portion melts when the crystalline resin exceeds its melting point, and the crystalline resin and the amorphous resin become compatible with each other, thereby improving the low-temperature fixability.
[0073] In the present invention, "exhibiting crystallinity" means that an endothermic curve obtained by DSC (differential scanning calorimetry) has a clear endothermic peak rather than a stepwise endothermic change at the melting point, i.e., during heating. A clear endothermic peak means a peak with a half-width of 15°C or less in an endothermic curve when the temperature is raised at a heating rate of 10°C / min.
[0074] As the crystalline resin, it is preferable to use a known crystalline resin, for example, a crystalline polyester, a crystalline polyurethane resin, etc. In particular, from the viewpoint of sharp melting during melting and compatibility with the binder resin, it is preferable to use a crystalline polyester. In other words, it is preferable that the part having a crystalline structure contains a crystalline polyester.
[0075] (1.1.2.1) Crystalline polyester The term "crystalline polyester" refers to a known polyester that exhibits crystallinity and is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol).
[0076] The crystalline polyester preferably has structural units derived from an aliphatic diol and structural units derived from an aliphatic carboxylic acid, and more preferably has only structural units derived from an aliphatic diol and structural units derived from an aliphatic carboxylic acid.
[0077] The number of carbon atoms in the aliphatic diol or aliphatic carboxylic acid is more preferably within the range of 6 to 10. It is believed that by making the crystalline polyester have a relatively non-bulky structure, it is possible to prevent the ester groups from becoming locally highly dense, thereby suppressing charge leakage.
[0078] A polycarboxylic acid is a compound that contains two or more carboxy groups in one molecule. Examples of polycarboxylic acids include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, n-dodecyl succinic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid (dodecanedioic acid), and tetradecanedicarboxylic acid (tetradecanedioic acid); alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid; and anhydrides of these carboxylic acid compounds. In addition, alkyl esters having 1 to 3 carbon atoms may be used. The crystalline polyester may contain one or more of these alone.
[0079] A polyhydric alcohol is a compound that contains two or more hydroxy groups in one molecule. Examples of polyhydric alcohols include aliphatic diols such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, dodecanediol, neopentyl glycol, and 1,4-butenediol; and trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, trimethylolpropane, and sorbitol. The crystalline polyester may contain one or more of these.
[0080] The method for synthesizing the crystalline polyester is not particularly limited, and the polyester can be synthesized by polycondensing (esterifying) the polyhydric alcohol component and the polyvalent carboxylic acid component using a known esterification catalyst.
[0081] The ratio of the polyhydric alcohol component to the polybasic carboxylic acid component is not particularly limited. For example, the equivalent ratio of the hydroxyl group of the polyhydric alcohol component to the carboxyl group of the polybasic carboxylic acid component is preferably within the range of 1.5 / 1 to 1 / 1.5, more preferably within the range of 1.2 / 1 to 1 / 1.2.
[0082] Catalysts that can be used in the synthesis of crystalline polyesters include alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; metal compounds such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds.
[0083] Specific examples of tin compounds include dibutyltin oxide, tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-n-butyl titanate, tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolaminate.
[0084] Germanium compounds include germanium dioxide and the like. Examples of the aluminum compound include oxides such as polyaluminum hydroxide, aluminum alkoxides, and tributylaluminate. These may be used alone or in combination of two or more. The polymerization temperature and polymerization time are not particularly limited, and the pressure in the reaction system may be reduced during the polymerization, if necessary.
[0085] (1.1.2.2) Melting point From the viewpoint of low temperature fixability and hot offset resistance, the melting point (Tm) of the crystalline resin is preferably within a range of 55 to 90° C., and more preferably within a range of 60 to 85° C. The melting point of the crystalline resin can be controlled by the resin composition. When the crystalline resin is a crystalline polyester, the melting point of the crystalline polyester is preferably 75° C. or lower.
[0086] The melting point (Tm) is the temperature at the top of the endothermic peak, and can be measured by DSC (differential scanning calorimetry). For example, differential scanning calorimetry (DSC measurement) is performed using a differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI). Specifically, 5 mg of sample is sealed in an AL autosampler sample container φ6.8 H2.5 mm (manufactured by HITACHI) and an AL autosampler cover (manufactured by HITACHI). This is set in the sample holder of the "AS3 / DX" and the temperature is changed in the order of heating, cooling, and heating again. During the first and second heating, the temperature is raised from 0°C to 150°C at a heating rate of 10°C / min and held at 150°C for 1 minute. During cooling, the temperature is lowered from 150°C to 0°C at a cooling rate of 10°C / min and held at 0°C for 1 minute. The temperature at the top of the endothermic peak in the endothermic curve obtained during the second heating is measured as the melting point.
[0087] (1.1.2.3) Weight average molecular weight The weight average molecular weight of the crystalline resin is not particularly limited, but is preferably within a range of 1,000 to 29,000, more preferably within a range of 1,000 to 20,000, and even more preferably within a range of 1,000 to 15,000, from the viewpoints of suppressing tacking and low-temperature fixability.
[0088] The weight average molecular weight of the crystalline resin can be measured by the following method. For example, a gel permeation chromatography apparatus "HLC-8320GPC" (manufactured by Tosoh Corporation) connected with one column "TSKgel guard column SuperHZ-L" and three columns "TSKgel SuperHZM-M" (all manufactured by Tosoh Corporation) is used.
[0089] The column (TSK-) is stabilized at 40°C, and tetrahydrofuran (THF) is passed through the column at this temperature as a carrier solvent at a flow rate of 0.35 mL / min. A THF sample solution of the measurement sample (resin) adjusted to a sample concentration of 1 mg / mL is treated at room temperature for 10 minutes using a roll mill. The solution is treated with a membrane filter with a pore size of 0.2 μm to obtain a sample solution. 10 μL of this sample solution is injected into the above device together with the above carrier solvent, and detected using a refractive index detector (RI detector).
[0090] A calibration curve is created using a polystyrene standard sample with a monodisperse molecular weight distribution. The molecular weight distribution of the measurement sample is calculated based on this calibration curve. The calibration curve is created from 10 samples of "polystylene standard sample TSK standard" manufactured by Tosoh Corporation: "A-500", "F-1", "F-10", "F-80", "F-380", "A-2500", "F-4", "F-40", "F-128", and "F-700". The data collection interval in sample analysis is 300 ms.
[0091] Alternatively, as described below, the crystalline resin and the release agent in the toner may be separated, and then the weight average molecular weight of the crystalline resin may be calculated by the above-mentioned measuring method.
[0092] (Separation of crystalline resin) An example in which the crystalline resin is a crystalline polyester will be described. First, the toner is dispersed in ethanol, which is a poor solvent for the toner, and the dispersion is heated to a temperature exceeding the melting points of the crystalline polyester and the release agent. At this time, pressure may be applied if necessary. At this point, the crystalline polyester and the release agent, which have exceeded their melting points, are melted in the ethanol. Then, a mixture of the crystalline polyester and the release agent can be collected from the toner by solid-liquid separation. The mixture can be classified according to molecular weight to separate the crystalline polyester and the release agent from the toner.
[0093] (Acid value of crystalline resin) From the viewpoint of low temperature fixability and fold fixability, the acid value of the crystalline resin is preferably within a range of 9 to 30 mgKOH / g, and more preferably within a range of 15 to 23 mgKOH / g.
[0094] The acid value of a crystalline polyester is expressed as the number of milligrams of potassium hydroxide required to neutralize the carboxyl groups present in 1 g of the resin (mgKOH / g). Specifically, it is determined by the following method in accordance with JIS K0070-1992.
[0095] (1) Preparation of reagents (a) Phenolphthalein solution 1.0 g of phenolphthalein is dissolved in 90 mL of ethyl alcohol (95% by volume), and ion-exchanged water is added to make 100 mL to obtain a phenolphthalein solution.
[0096] (b) Potassium hydroxide solution Dissolve 7 g of special grade potassium hydroxide in 5 mL of ion-exchanged water, and add ethyl alcohol (95% by volume) to make 1 L. Place this solution in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave it for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container.
[0097] (c) Factor of potassium hydroxide solution Put 25mL of 0.1mol / L hydrochloric acid into an Erlenmeyer flask and add a few drops of the phenolphthalein solution. Then, titrate this with potassium hydroxide solution. Calculate the factor of the potassium hydroxide solution from the amount of potassium hydroxide solution required for neutralization.
[0098] (d) Hydrochloric acid solution 0.1 mol / L hydrochloric acid prepared in accordance with JIS K8001-1998 is used.
[0099] (2) Operation (a) Main Test Weigh out 2.0 g of toner into a 200 mL Erlenmeyer flask, add 100 mL of a toluene:ethanol (2:1) mixed solution to the Erlenmeyer flask, and dissolve for 5 hours. Next, add a few drops of phenolphthalein solution to the Erlenmeyer flask as an indicator, and titrate with potassium hydroxide solution. The end point of the titration is when the indicator remains a pale red color for approximately 30 seconds.
[0100] (b) Blank test A titration is carried out in the same manner as in the main test above, except that no sample is used, i.e., only a mixture of toluene:ethanol (2:1) is used.
[0101] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CD) × f × 5.611] / S Here, the symbols and numbers are as follows: A: Acid value (mgKOH / g) C: Amount of potassium hydroxide solution added in this test (mL) D: Amount of potassium hydroxide solution added for blank test (mL) f: Factor of 0.1 mol / L potassium hydroxide ethanol solution 5.611: Molar mass of potassium hydroxide 56.11 (g / mol) x (1 / 10) S: mass of sample (g)
[0102] (1.2) Release agent The release agent is not particularly limited, and may be any of various known release agents.For example, polyolefin waxes such as polyethylene wax and polypropylene wax; branched chain hydrocarbon waxes such as microcrystalline wax; long chain hydrocarbon waxes such as paraffin wax and Sasol wax; synthetic waxes such as Fischer-Tropsch wax; dialkyl ketone waxes such as distearyl ketone; ester waxes such as carnauba wax, montan wax, behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, trimellitic acid tristearyl, and distearyl maleate; amide waxes such as ethylenediamine behenylamide and trimellitic acid tristearylamide.
[0103] The melting point of the release agent is preferably within a range of 60 to 80° C. By having a melting point of 60° C. or more, the release agent can be prevented from volatilizing and becoming fine particles when the toner is fixed, and the environmental load can be reduced. In addition, by having a melting point of 80° C. or less, the release agent melts when the toner is fixed, and the separation performance from the fixing member is good.
[0104] The content of the release agent is preferably within a range of 1 to 30% by mass, more preferably within a range of 5 to 20% by mass, based on the total mass of the binder resin. By having the content of the release agent within the above range, sufficient fixing and separating properties can be obtained. The content of the release agent is preferably within a range of 3 to 15% by mass with respect to the total mass of the toner base particles.
[0105] (1.3) Colorants The colorant is not particularly limited, and various known dyes and pigments can be used. Examples of colorants for obtaining black toner include carbon black such as furnace black and channel black; magnetic materials such as magnetite and ferrite; dyes; and inorganic pigments including non-magnetic iron oxide.
[0106] Colorants for obtaining color toners include known dyes and organic pigments. Examples of organic pigments include CI Pigment Red 5, 48:1, 53:1, 57:1, 81:4, 122, 139, 144, 149, 166, 177, 178, 222, 238, 269, CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, 185, CI Pigment Orange 31, 43, CI Pigment Blue 15:3, 60, and 76.
[0107] Examples of dyes include CI Solvent Red 1, 49, 52, 58, 68, 11, and 122, CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162, CI Solvent Blue 25, 36, 69, 70, 93, and 95.
[0108] The colorant for obtaining the toner of each color may be contained alone or in combination of two or more kinds for each color. The content of the colorant is preferably within a range of 1 to 10% by mass, and more preferably within a range of 2 to 8% by mass, based on the total mass of the binder resin.
[0109] (1.4) Charge control agent The charge control agent may be any of a variety of known compounds. The content of the charge control agent is preferably within a range of 0.1 to 5.0% by mass with respect to the total mass of the binder resin.
[0110] (2) External additives The toner according to the present invention may further contain an external additive in the toner base particles, which can further improve the fluidity, chargeability, cleaning properties, etc. of the toner.
[0111] Examples of the external additive include inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles; inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles; inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate, etc. These may be used alone or in combination of two or more.
[0112] From the viewpoint of heat resistance storage property and environmental stability, it is preferable to subject these inorganic fine particles to a hydrophobic treatment using a silane coupling agent, a titanium coupling agent, a higher fatty acid, silicone oil or the like.
[0113] The total amount of the external additives added is preferably within a range of 0.05 to 5% by mass, and more preferably within a range of 0.1 to 3% by mass, based on the total mass of the toner.
[0114] 3. Properties of toner for developing electrostatic images (1) Toner particle size The average particle size of the toner particles is, for example, preferably in the range of 3 to 10 μm, and more preferably in the range of 4 to 8 μm, in terms of the volume-based median diameter (d50). The average particle size of the toner particles can be controlled by the concentration of the coagulant used during production, the amount of organic solvent added, the fusion time, the composition of the binder resin, and the like. By having the volume-based median diameter (d50) within the above range, extremely fine dot images at a 1200 dpi level can be faithfully reproduced.
[0115] The volume-based median diameter (d50) of the toner particles is measured and calculated using a measuring device consisting of a "Multisizer 3" (manufactured by Beckman Coulter) connected to a computer system equipped with the data processing software "Software V3.51."
[0116] Specifically, a toner sample to be measured is first added to a surfactant solution, mixed, diluted with pure water, and then ultrasonically dispersed to prepare a toner particle dispersion. For the surfactant solution, an anionic surfactant such as sodium polyoxyethylene lauryl ether sulfate is preferably used for the purpose of dispersing the toner particles.
[0117] Inject this toner particle dispersion with a pipette into a beaker containing "ISOTON II" (manufactured by Beckman Coulter) in the sample stand until the concentration indicated on the measuring device is 6 to 8%. By setting this concentration, highly reproducible measurement values can be obtained.
[0118] The measurement device is set to a particle count of 25,000 and an aperture diameter of 100 μm. The measurement range of the toner particle diameter, 2 to 60 μm, is divided into 256 parts, and the frequency value of the toner particle diameter is calculated. The particle diameter of the largest 50% of the volume cumulative fraction is defined as the volume-based median diameter (d50).
[0119] (2) Average circularity of toner particles From the viewpoint of the stability of the charging characteristics and the low-temperature fixing ability, the average circularity of the toner particles is preferably within a range of 0.930 to 1.000, and more preferably within a range of 0.950 to 0.995.
[0120] When the average circularity is within the above range, it is possible to achieve both the transferability and cleaning performance of the toner, and further, the chargeability of the toner is stable, making it possible to form high quality images.
[0121] The average circularity of the toner particles can be measured, for example, by using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation).
[0122] Specifically, the toner sample to be measured is added to a surfactant solution, mixed, diluted with pure water, and then ultrasonically dispersed to prepare a toner particle dispersion. For the surfactant solution, an anionic surfactant such as sodium polyoxyethylene lauryl ether sulfate is preferably used for the purpose of dispersing the toner particles. Then, for example, a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) is used to take an image at an appropriate concentration with a HPF (high magnification imaging) mode measurement condition and a HPF detection number of 3,000 to 10,000 particles.
[0123] The circularity of each toner particle is calculated according to the following formula. The circularity of each toner particle is then added and divided by the total number of toner particles to calculate the average circularity. If the HPF detection number is within the above range, high reproducibility can be obtained. Formula: Circularity = (perimeter of a circle with the same projected area as the particle image) / (perimeter of the projected particle image)
[0124] (3) Glass transition temperature of toner From the viewpoint of achieving both sufficient low-temperature fixability and heat-resistant storage stability, the glass transition temperature (Tg) of the toner is preferably within a range of 15 to 40° C., and more preferably within a range of 20 to 35° C. The glass transition temperature can be measured by the method described above.
[0125] 4. Structure of toner for developing electrostatic images (core-shell structure) The toner base particles may have a multi-layer structure, for example a core-shell structure having a core particle and a shell layer covering the surface of the core particle.
[0126] The shell layer does not have to cover the entire surface of the core particle, and the core particle may be partially exposed. The cross section of the core-shell structure can be confirmed by a known observation means such as a transmission electron microscope (TEM) or a scanning probe microscope (SPM).
[0127] When the toner base particle has a core-shell structure, the core particle and the shell layer can have different properties such as glass transition temperature, melting point, and hardness depending on the purpose. For example, a core particle containing a binder resin, a colorant, a release agent, and the like and having a relatively low glass transition temperature (Tg) is prepared. Then, a resin having a relatively high glass transition temperature (Tg) is aggregated and fused to the core particle to form a shell layer. The shell layer preferably contains an amorphous resin. With such a configuration, low-temperature fixability and heat-resistant storage stability can be achieved at the same time. In addition, good charge retention performance can be obtained.
[0128] 5. Manufacturing method of toner for developing electrostatic images The method for producing a toner for developing electrostatic images of the present invention is a method for producing the above-mentioned toner for developing electrostatic images, and is characterized in that it comprises a step of drying wet toner base particles by an air flow in a dryer, and the temperature of the air flow is 60° C. or higher and the speed of the air flow is 5 m / sec or higher.
[0129] The method for producing the toner base particles is not particularly limited as long as it is a method that includes a process of producing wet toner base particles and drying them. Examples of the production method include a suspension polymerization method, an emulsion aggregation method, and other known methods. Among them, the emulsion aggregation method is preferable. By using the emulsion aggregation method, it is possible to produce a toner with stable quality while suppressing costs. In addition, it is possible to easily produce toner particles with a small particle size.
[0130] In the emulsion aggregation method, first, an aqueous dispersion of amorphous polyester fine particles is mixed with an aqueous dispersion of fine particles of a release agent, a colorant, an amorphous resin other than the amorphous polyester, a crystalline resin, etc., as required, and then these fine particles are aggregated to form wet toner base particles. In the present invention, the wet toner base particles are then dried under specific conditions to prepare the toner base particles.
[0131] Here, the term "aqueous dispersion" refers to a dispersion (particles) dispersed in an aqueous medium. The aqueous medium refers to a medium in which the main component, i.e., a component that accounts for 50% by mass or more, is water.
[0132] The components other than water contained in the aqueous medium include organic solvents that dissolve in water. Examples of organic solvents that dissolve in water include methanol, ethanol, isopropanol, butanol, acetone, methyl ethyl ketone, tetrahydrofuran, etc. Among them, from the viewpoint of not dissolving the resin, alcohol-based organic solvents such as methanol, ethanol, isopropanol, and butanol are preferable.
[0133] An example of the method for producing the toner for developing electrostatic images will be described below, but the present invention is not limited thereto.
[0134] (1) A process for synthesizing amorphous polyester and preparing a dispersion of amorphous polyester microparticles (2) A process for synthesizing crystalline polyester and preparing a dispersion of crystalline polyester microparticles. (3) A step of preparing a dispersion of release agent particles (4) A step of preparing a dispersion of colorant particles (5) A process of aggregating the amorphous polyester particles, the crystalline polyester particles, the releasing agent particles, and the colorant particles to form toner base particles. (6) A process of ripening toner base particles and controlling their shape using thermal energy (7) Step of cooling the dispersion of toner base particles (8) A process of filtering the toner base particles from the aqueous medium, washing the toner base particles to remove surfactants, etc., and obtaining wet toner base particles. (9) A process for removing the solvent from the wet toner base particles (10) A process for drying the wet toner base particles using airflow in a dryer. (11) A process of adding external additives to the dried toner base particles
[0135] (1) A process for synthesizing amorphous polyester and preparing a dispersion of amorphous polyester microparticles In this step, an amorphous polyester is synthesized by a conventionally known method, and the amorphous polyester is dispersed in the form of fine particles in an aqueous medium to prepare a dispersion of amorphous polyester fine particles.
[0136] Specifically, first, the amorphous polyester is dissolved or dispersed in an organic solvent to prepare an oil phase liquid. Next, the oil phase liquid is dispersed in an aqueous medium by phase inversion emulsification or the like to form oil droplets with a desired particle size. Thereafter, the organic solvent is removed to prepare an aqueous dispersion liquid of the amorphous polyester fine particles.
[0137] The amount of the aqueous medium used is preferably within a range of 50 to 2000% by mass, and more preferably within a range of 100 to 1000% by mass, based on the total mass of the oil phase liquid. From the viewpoint of dispersion stability of the oil droplets, a surfactant may be added to the aqueous medium. Examples of the surfactant include various conventionally known anionic surfactants, cationic surfactants, nonionic surfactants, etc.
[0138] From the viewpoint of removal treatment after the formation of oil droplets, the organic solvent used for preparing the oil phase liquid is preferably one having a low boiling point and low solubility in water, specifically, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, etc. These may be used alone or in combination of two or more.
[0139] The amount of the organic solvent used is preferably within a range of 1 to 300% by mass based on the total mass of the amorphous polyester. The emulsification and dispersion of the oil phase liquid can be carried out by utilizing mechanical energy.
[0140] The toner base particles may contain internal additives such as a release agent, a charge control agent, etc., as necessary. Such internal additives may be incorporated into the toner base particles by, for example, dissolving or dispersing them in advance in a monomer solution for synthesizing the amorphous polyester.
[0141] The average particle size of the amorphous polyester fine particles is preferably within a range of 100 to 400 nm in terms of volume-based median diameter (d50). The volume-based median diameter (d50) can be measured, for example, using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).
[0142] (2) A process for synthesizing crystalline polyester and preparing a dispersion of crystalline polyester microparticles. The aqueous dispersion of the crystalline polyester fine particles can be prepared in the same manner as the aqueous dispersion of the amorphous polyester fine particles, and it is preferable to adjust the temperature during dispersion as necessary.
[0143] (3) A step of preparing a dispersion of release agent particles This step is carried out as necessary when a release agent is contained in the toner base particles. The aqueous dispersion of fine particles of the release agent can be prepared by dispersing the release agent in an aqueous medium to which a surfactant has been added at a critical micelle concentration (CMC) or higher.
[0144] The release agent can be dispersed by utilizing mechanical energy. The dispersing machine is not particularly limited, and examples thereof include ultrasonic dispersing machines, mechanical homogenizers, pressure dispersing machines such as Manton-Gaulin and pressure homogenizers, and media-type dispersing machines such as sand grinders and diamond fine mills.
[0145] The release agent fine particles preferably have a volume-based median diameter (d50) in a dispersed state within the range of 10 to 300 nm, more preferably within the range of 100 to 200 nm, and particularly preferably within the range of 100 to 150 nm. The volume-based median diameter (d50) of the release agent fine particles can be measured, for example, using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).
[0146] (4) A step of preparing a dispersion of colorant particles The aqueous dispersion of the colorant particles can be prepared in the same manner as the aqueous dispersion of the release agent particles. The release agent particles are preferably dispersed by heating to a temperature equal to or higher than the melting point, but the colorant particles do not necessarily need to be heated.
[0147] (5) A process of aggregating the amorphous polyester particles, the crystalline polyester particles, the releasing agent particles, and the colorant particles to form toner base particles. In this process, a flocculant is added at a concentration equal to or higher than the critical flocculation concentration to the aqueous dispersion in which the above-mentioned fine particles are dispersed, and the fine particles are flocculated by adjusting the temperature of the reaction solution to form toner base particles.
[0148] The flocculant is not particularly limited, and is preferably, for example, a metal salt such as an alkali metal salt or an alkaline earth metal salt. Examples of the metal salt include monovalent metal salts such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum.
[0149] Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, manganese sulfate, aluminum chloride, aluminum sulfate, polyaluminum chloride, polyaluminum hydroxide, etc. Among these, trivalent metal salts are preferred from the viewpoint of promoting aggregation with a smaller amount. These may be used alone or in combination of two or more.
[0150] (6) A process of ripening toner base particles and controlling their shape using thermal energy This step is carried out as necessary when the toner base particles are aged by thermal energy to control their shape. Specifically, in the aging treatment, the heating temperature, stirring speed, heating time, etc. are adjusted so that the circularity of the toner base particles reaches a desired value, and the dispersion liquid of the toner base particles is heated and stirred.
[0151] (7) Step of cooling the dispersion of toner base particles In this step, the dispersion liquid of the toner base particles is cooled. The cooling rate is preferably within the range of 1 to 20° C. / min. The specific method of the cooling treatment is not particularly limited. For example, a method of cooling by introducing a refrigerant from the outside of the reaction vessel, a method of cooling by directly introducing cold water into the reaction system, a method of cooling by a heat exchanger, etc. can be mentioned.
[0152] (8) A process of filtering the toner base particles from the aqueous medium, washing the toner base particles to remove surfactants, etc., and obtaining wet toner base particles. In this process, the toner base particles are separated from the cooled dispersion liquid of the toner base particles by solid-liquid separation. The resulting toner cake is then washed to remove any attached substances such as surfactants and coagulants, thereby obtaining wet toner base particles. Note that the "toner cake" here refers to an aggregate of wet toner base particles that have been coagulated into a cake-like form.
[0153] The method of solid-liquid separation is not particularly limited, and examples thereof include centrifugation, reduced pressure filtration using a Nutsche filter, etc., and filtration using a filter press, etc. In addition, in washing, it is preferable to wash with water until the electrical conductivity of the filtrate becomes 10 μS / cm or less.
[0154] (9) A process for removing the solvent from the wet toner base particles This step is carried out as necessary when reducing the amount of solvent contained in the wet toner base particles. By carrying out the solvent removal treatment, the amount of solvent contained in the obtained wet toner base particles can be reduced. In addition, by adjusting the time, rotation conditions, pressure conditions, etc., in the solvent removal treatment, the amount of solvent contained in the obtained wet toner base particles can be adjusted.
[0155] (10) A process for drying the wet toner base particles using airflow in a dryer. In this process, the wet toner base particles that have been washed and, in some cases, further subjected to a solvent removal process are dried by airflow in a dryer. The airflow temperature is 60° C. or higher, and the airflow speed is 5 m / sec or higher. By drying a toner having a specific composition under these conditions, the toner base particles can be dried at a relatively high temperature and quickly. The presence of the solvent in the toner base particles can be made uniform. Note that the "solvent" here mainly refers to water, and also includes organic solvents and the like used in the production of the toner base particles.
[0156] (10.1) Drying by airflow In the toner manufacturing method having the above-mentioned specific configuration, the wet toner base particles are dried with an air flow, and the temperature and speed of the air flow are set within a specific range, so that the state of the solvent in the toner base particles can be made uniform. More specifically, the water molecules adsorbed on the outermost layer of the toner base particles can be removed, and the water molecules inside the toner base particles can be uniformly dispersed. This is believed to improve the charge retention performance of the toner, and to produce high-quality images.
[0157] The dryer is not particularly limited as long as it is a device that dries using an air flow (air flow dryer), and examples thereof include a continuous instantaneous air flow dryer, a fluidized bed dryer, a vibration type fluidized bed dryer, etc. Among them, from the viewpoint of the toner recovery rate, a continuous instantaneous air flow dryer is preferable, and specifically, a "Flash Jet Dryer" (manufactured by Seishin Enterprise Co., Ltd.) is preferable.
[0158] The dryer has a space (chamber) in which the wet toner base particles to be dried are mixed with a high-temperature airflow and dried in the airflow, i.e., a drying section. The dryer also has an inlet for feeding the wet toner base particles into the drying section, a supply port for feeding a heated airflow, and an outlet for the dried toner base particles. The shape of the dryer may be any shape, but a piping type is preferable. More specifically, a piping type in which the toner particles are dried while being carried by an airflow in a piping-shaped chamber as shown in FIG. 1 is preferable. In order to perform drying with this dryer, a hot air supplying means for blowing hot air from the hot air supplying port of the dryer, a collecting means for collecting the dried toner base particles from the discharge port of the dryer, and a wet toner base particle supplying means for feeding the wet toner base particles from the inlet of the dryer are connected.
[0159] Fig. 1 is an explanatory diagram showing an example of a flash dryer. In the figure, 40 is a flash dryer, 42 is an inlet for wet toner base particles, 43 is a nozzle, 44 is a recovery nozzle, 45 is an outlet for dried toner base particles, 46A is a drying area, 46B is an up-stack area, 46C is a classification area, 47 is a hot air supply unit, and 48 is a hot air inlet. The wet toner base particles are introduced in the form of a cake.
[0160] When heated compressed air is supplied from hot air inlet 48 into hot air supply section 47, this compressed air (hot air) is discharged at supersonic speed into the interior of flash dryer 1 through nozzle 43 opening in hot air supply section 47. The hot air then circulates inside flash dryer 40 along the flow path in the order of drying area 46A, upstack area 46B, classification area 46C, and drying area 46A. At this time, the interior of flash dryer 40 is under a slight negative pressure near input port 42.
[0161] When wet toner base particles (water-containing cake) in a cake form are fed from the inlet 42, the toner base particles are dispersed and crushed (pulverized) by the hot air circulating inside the flash dryer 40. The solvent in the powder thus formed is then quickly removed. The powder of the toner base particles is transported to the classification area 46C by the hot air.
[0162] Dry powder pw, in which the amount of solvent in the powder is equal to or less than a predetermined value, i.e., the powder has a low specific gravity, is discharged from the discharge port 45 through the recovery nozzle 44. Powder PW, in which the amount of solvent in the powder is greater than a predetermined value, i.e., the powder has a high specific gravity, is transported to the drying area 46A and is dried again.
[0163] By using the above-mentioned airflow dryer, the solvent present in the wet toner base particles can be evaporated instantly, for example, within one minute. Then, only the powder (dry powder pw) in which the amount of solvent is equal to or less than a predetermined value is classified and discharged from the airflow dryer. The particle group consisting of the dry powder pw has a desired particle size distribution without agglomeration. In addition, the classified and discharged dry powder pw has extremely small variations in specific gravity between particles, i.e., variations in the amount of residual solvent.
[0164] The specific gravity of the dry powder pw can be controlled by adjusting the classification conditions in the classification region 46C, i.e., the centrifugal force acting on the powder. Specifically, for example, the specific gravity can be controlled by adjusting the amount of hot air supplied (air volume) to the hot air supply unit 47.
[0165] The drying process using the airflow dryer may be performed in a continuous manner or a batch manner. However, from the viewpoint of eliminating variation in drying among particles, it is preferable to perform the drying process in a continuous manner. Here, the "continuous manner" refers to a method in which the supply of wet toner base particles and the discharge of dried toner base particles are performed continuously.
[0166] Fig. 2 is an explanatory diagram showing an example of a plant for performing a continuous drying process. In the figure, 50 is a flash dryer having the configuration shown in Fig. 1. 51 is a blower that generates compressed air, and 52 is a heater that heats the air from the blower 51. The air (hot air) heated by the heater 52 is supplied to a hot air supplying section of the flash dryer 50 (hot air supplying section 47 in Fig. 1).
[0167] T1 is a thermometer for measuring the temperature of the air heated by heater 52. Hereinafter, the temperature of the air heated by heater 52 is also referred to as the "inlet temperature." T2 is a thermometer for measuring the temperature of the air exhausted from the flash dryer 50. Hereinafter, the temperature of the air exhausted from the flash dryer 50 is also referred to as the "outlet temperature."
[0168] Reference numeral 55 denotes a supplier of wet toner base particles, which is connected to the inlet (inlet 42 in FIG. 1) of the flash dryer 50. Reference numeral 56 denotes a cyclone connected to the outlet (outlet 45 in FIG. 1) of the flash dryer 50 via piping. Dried toner base particles are collected from the powder outlet of the cyclone 56. Reference numeral 57 denotes a bag filter connected to the exhaust outlet of the cyclone 56 via piping, and reference numeral 58 denotes an exhaust blower connected to the bag filter 57 via piping.
[0169] (Airflow temperature) In the present invention, the "temperature of the airflow" refers to the temperature of the airflow supplied to a housing or piping that dries wet toner base particles, and refers to the "inlet temperature" in a flash dryer. Specifically, the temperature T1 at the outlet of the heater 52 shown in FIG. 2 is measured.
[0170] From the viewpoint of the charge retention performance of the toner, the temperature of the air flow is preferably 65° C. or higher, and more preferably 70° C. or higher.
[0171] (Air flow speed) In the present invention, the "speed of airflow" refers to a value calculated from the volume of airflow converted to 0°C and 1 atmospheric pressure supplied to a dryer (casing or piping) that dries wet toner base particles and the maximum cross-sectional area perpendicular to the direction of the airflow in the drying section of the dryer that dries wet toner base particles. In FIG. 2, the dryer that dries wet toner base particles is designated as 50. The dryer in FIG. 1 is of a piping type, and the cross-sectional area here is the cross-sectional area of the piping, but more precisely, it is the cross-sectional area of the part where nozzles such as the inlet 42 for wet toner base particles, the nozzle 43, the recovery nozzle 44, and the outlet 45 for dried toner base particles are not provided. When the cross-sectional area differs depending on the location, the maximum cross-sectional area is used for calculation. When the drying section is not of a piping type, for example, when the airflow is blown into a cylindrical drying section, the maximum cross-sectional area of the drying section perpendicular to the direction of blowing the airflow is used. The cross-sectional area in this case is the cross-sectional area of a portion where nozzles such as an inlet for wet toner base particles, an airflow inlet, and a dry toner recovery port are not provided.
[0172] Specifically, it refers to the airflow speed measured using the following measurement method. An orifice is installed at the outlet of the blower 51 shown in Figure 2, the wind speed is calculated from the pressure difference before and after, and the air volume is calculated from the temperature, absolute pressure, and gas density. In addition to the orifice, a pitot tube, hot wire sensor, etc. can also be used to measure the wind speed. It should be noted that "air volume" refers to the amount (volume) of air passing through per unit time. The airflow speed is calculated using the following formula. Airflow speed = Air volume supplied to the dryer at 0℃·1 atmospheric pressure / Maximum cross-sectional area perpendicular to the airflow direction in the drying section of the dryer
[0173] From the viewpoint of the charge retention performance of the toner, the airflow speed is preferably 8 m / sec or more, more preferably 10 m / sec or more. There is no particular upper limit to the speed, and it may be, for example, 50 m / sec or less. From the viewpoint of suppressing toner aggregation and improving production efficiency, the airflow speed is preferably 35 m / sec or less. More preferably, the airflow speed is 20 m / sec or less.
[0174] It is believed that by reducing the solvent content in the wet toner base particles compared to the case of general air flow drying, the solvent contained in the toner base particles is more easily homogenized within the particles. It is also believed that the charge retention performance of the toner is improved by homogenizing the residual solvent in the particles without unevenness. It is also believed that by containing a specific resin in the toner base particles, excessive drying can be prevented even if the solvent content is reduced.
[0175] The content of the solvent in the wet toner base particles is preferably within the range of 15 to 30% by mass, and more preferably within the range of 15 to 25% by mass. By keeping the content within the above range, the residual solvent in the particles can be uniformized without unevenness. In addition, the occurrence of drying unevenness and aggregation of the toner base particles can be suppressed.
[0176] The content of the solvent in the wet toner base particles can be adjusted by the above-mentioned solvent removal treatment, if necessary. The content of the solvent in the wet toner base particles can be measured by the Karl Fischer method or the heat drying / mass measurement method.
[0177] From the viewpoint of the charge retention performance of the toner, the temperature of the compressed air discharged from the flash dryer (outlet temperature) is preferably (Tg±10)°C, where (Tg) is the glass transition temperature of the toner. Furthermore, by having an outlet temperature of (Tg-10)°C or higher, a sufficient evaporation rate of the solvent can be obtained, and water bridges formed between the toner base particles can be prevented from forming and causing aggregation. By having an outlet temperature of (Tg+10)°C or lower, the surface of the obtained toner base particles can be softened, and thus causing aggregation can be prevented. The glass transition temperature (Tg) of the toner is preferably within the range of 15 to 40°C, and more preferably within the range of 20 to 35°C.
[0178] In the drying process, the amount of residual solvent in the toner base particles discharged from the flash dryer is measured. It is preferable to control the amount of wet toner base particles supplied to the flash dryer so that the amount of residual solvent is maintained at a predetermined value or less. The amount of residual solvent in the discharged toner base particles can be measured by the Karl Fischer method or the heat drying / mass measurement method.
[0179] In the drying process, it is preferable to constantly measure the outlet temperature of the flash dryer and control the amount of wet toner base particles supplied to the flash dryer so that the outlet temperature is maintained within a certain range, thereby controlling the amount of residual solvent in the discharged toner base particles within a certain range.
[0180] The residual solvent content of the dried toner base particles is preferably 2% by mass or less, more preferably 1% by mass or less. By keeping the residual solvent content within the above range, the moisture content of the toner base particles can be relatively reduced. As a result, a toner with excellent charge retention performance can be obtained.
[0181] (10.2) Post-drying After the wet toner base particles are dried by an air stream, further post-drying may be carried out in order to adjust the amount of residual solvent and other non-volatile substances in the toner.
[0182] Dryers used in the post-drying treatment include vacuum freeze dryers, reduced pressure dryers, stationary shelf dryers, mobile shelf dryers, fluidized bed dryers, vibration type fluidized bed dryers, rotary dryers, stirring dryers, etc. Among these, fluidized bed dryers and vibration type fluidized bed dryers are preferred.
[0183] In the case where the dried toner base particles are aggregated by weak interparticle attractive forces, the aggregates may be subjected to a crushing treatment. Examples of the crushing treatment device include mechanical crushing devices such as a jet mill, a Henschel mixer, a coffee mill, and a food processor.
[0184] (11) A process of adding external additives to the dried toner base particles This step is carried out as necessary when an external additive is added to the toner base particles. The toner base particles can be used as they are as toner. From the viewpoints of fluidity, chargeability, cleaning properties, etc., external additives such as so-called fluidizing agents and cleaning assistants may be added to the toner base particles. Examples of the mixing device for the external additive include mechanical mixers such as a Henschel mixer and a coffee mill.
[0185] The method for producing the toner for developing electrostatic images of the present invention includes at least the above step (10). If necessary, the method may include step (9). The above steps (1) to (9) are only an example of a method for producing the toner base particles, and the present invention is not limited thereto.
[0186] The toner base particles according to the present invention may have a core-shell structure. Furthermore, by having a shell layer, both low-temperature fixability and heat resistance can be achieved. When a shell layer is formed, it is preferable to form the shell layer after forming the core particles in step (5). The shell layer is preferably made of an amorphous resin. The method for forming the shell layer is not particularly limited, and a conventionally known method can be used.
[0187] 6. Developer The toner can be used as a magnetic or non-magnetic one-component developer, or may be mixed with a carrier to form a two-component developer.
[0188] When the toner is used as a two-component developer, the carrier may be magnetic particles made of a conventionally known material. Examples of materials for the magnetic particles include metals such as iron, ferrite, and magnetite; alloys of these metals with aluminum; and alloys of metals such as lead. Among these, the magnetic particles are preferably ferrite particles.
[0189] The carrier may be a coated carrier in which the surfaces of magnetic particles are coated with a coating agent such as resin, or a dispersion type carrier in which fine magnetic powder is dispersed in a binder resin.
[0190] The volume-based median diameter (d50) of the carrier is preferably within a range of 20 to 100 μm, and more preferably within a range of 25 to 80 μm. The volume-based median diameter (d50) of the carrier can be measured, for example, by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.
[0191] The mixing device used for mixing the toner and carrier is not particularly limited, and examples thereof include a Nauta mixer, a W-cone type mixer, and a V-type mixer.
[0192] The toner content in the developer is preferably within a range of 4.0 to 8.0% by mass with respect to the total mass of the developer.
[0193] 7.Image forming method It is preferable to form an image by electrophotography using the developer. The developer may be a magnetic or non-magnetic one-component developer, or a two-component developer. An example of an image forming method using a two-component developer will be described below, but the present invention is not limited to this.
[0194] In the electrophotographic method, it is preferable to have a charging step of charging the surface of an image holder, an electrostatic image forming step of forming an electrostatic image on the charged surface of the image holder, a developing step of developing the electrostatic image formed on the surface of the image holder as a toner image using the above-mentioned developer, a transfer step of transferring the toner image formed on the surface of the image holder to the surface of a recording medium, a fixing step of fixing the toner image transferred to the surface of the recording medium, and a cleaning step of the image holder surface.
[0195] (Electrifying process) In this step, the electrophotographic photoreceptor is charged. The charging method is not particularly limited, and a known method such as a charging roller method in which the electrophotographic photoreceptor is charged by a charging roller can be used.
[0196] (Process for forming electrostatic image) In this process, an electrostatic image is formed on an electrophotographic photoreceptor (electrostatic image holder).
[0197] The electrophotographic photoreceptor is not particularly limited, and for example, a drum-shaped organic photoreceptor can be used.
[0198] The electrostatic image is formed, for example, by uniformly charging the surface of the electrophotographic photosensitive member by a charging means and imagewise exposing the surface of the electrophotographic photosensitive member to light by an exposing means. The term "electrostatic image" refers to an image formed on the surface of an electrophotographic photosensitive member by such a charging means.
[0199] The charging means and the exposure means are not particularly limited, and known methods in the electrophotographic system can be used.
[0200] (Developing process) In this process, the electrostatic image is developed with the developer to form a toner image.
[0201] The toner image is formed by using a developing means including a stirrer that uses a developer to frictionally stir and charge the toner, and a rotatable magnet roller.
[0202] Specifically, in the developing means, for example, toner and a carrier are mixed and stirred, and the toner is charged by friction during this process. The toner is held on the surface of a rotating magnet roller, forming a magnetic brush. The magnet roller is disposed in the vicinity of an electrophotographic photoreceptor. A portion of the toner constituting the magnetic brush moves to the surface of the electrophotographic photoreceptor by electrical attraction. As a result, an electrostatic image is developed by the toner, and a toner image is formed on the surface of the electrophotographic photoreceptor.
[0203] (Transfer process) In this process, the toner image is transferred to a recording medium.
[0204] The transfer is performed by peeling and charging the toner image onto the recording medium.
[0205] Examples of the transfer means include a corona transfer device using corona discharge, a transfer belt, a transfer roller, and the like.
[0206] In the transfer step, for example, an intermediate transfer member is used, and a toner image is primarily transferred onto the intermediate transfer member. Then, the toner image is secondarily transferred onto a recording medium. Alternatively, a toner image formed on an electrophotographic photoreceptor may be directly transferred onto a recording medium.
[0207] (Fixing process) In this process, the unfixed image (toner image) is fixed to the recording medium by passing the recording medium onto which the unfixed image (toner image) has been transferred between a heated fixing belt or roller and a pressure member.
[0208] The fixing process may be performed, for example, by a belt fixing method or a roller fixing method. These methods are configured with a fixing belt or a fixing roller as a fixing rotor, and a pressure roller. The pressure roller is provided in a state of being in pressure contact with the fixing belt or the fixing roller so as to form a fixing nip portion.
[0209] (Cleaning process) In this step, the developer remaining on a developer carrier such as a photoconductor or an intermediate transfer body that has not been used for image formation or that has not been transferred is removed from the developer carrier.
[0210] The cleaning method is not particularly limited. For example, a blade that scrapes the surface of the photoconductor may be used. The blade is provided so that its tip is in contact with the object to be cleaned, such as the photoconductor.
[0211] (Recording medium) The recording medium is not particularly limited. For example, it may be plain paper from thin paper to thick paper, coated printing paper such as fine paper, art paper or coated paper, commercially available paper such as Japanese paper or postcard paper, resin films such as polypropylene (PP) film, polyethylene terephthalate (PET) film, triacetyl cellulose (TAC) film, cloth, etc. In addition, the color of the recording medium is not particularly limited, and recording media of various colors may be used.
[0212] 8. Image forming equipment In the above image forming method, for example, an image forming apparatus as shown in Fig. 3 can be used. Fig. 3 is a schematic cross-sectional view showing the configuration of one example of the image forming apparatus. This image forming apparatus 100 is called a tandem type color image forming apparatus. The image forming apparatus 100 has four sets of image forming sections (image forming units) 10Y, 10M, 10C, and 10Bk arranged vertically in a row. The image forming apparatus 100 also has an intermediate transfer unit 7, a paper feed means 21, and a fixing means 24. An original image reading device SC is disposed on the upper part of the main body A of the image forming apparatus 100.
[0213] The intermediate transfer unit 7 has an endless belt-like intermediate transfer member 70 that can rotate around rollers 71, 72, 73, and 74. The intermediate transfer unit 7 also has primary transfer rollers 5Y, 5M, 5C, and 5Bk, and a cleaning means 6b.
[0214] The four image forming units 10Y, 10M, 10C, and 10Bk have drum-shaped photoconductors 1Y, 1M, 1C, and 1Bk at their centers, respectively. Each image forming unit has charging means 2Y, 2M, 2C, and 2Bk arranged around the photoconductor, exposure means 3Y, 3M, 3C, and 3Bk, rotating developing means 4Y, 4M, 4C, and 4Bk, and cleaning means 6Y, 6M, 6C, and 6Bk for cleaning the photoconductors 1Y, 1M, 1C, and 1Bk.
[0215] The image forming units 10Y, 10M, 10C, and 10Bk form yellow, magenta, cyan, and black toner images, respectively. The charging process, the exposure process, and the development process are processes for forming a toner image on a photoconductor. In the image forming apparatus 100, these processes are performed by the image forming units 10Y, 10M, 10C, and 10Bk using the toner. The details will be described below. It is preferable that the toner is mixed with a carrier and used as a two-component developer.
[0216] The image forming units 10Y, 10M, 10C, and 10Bk are different in the colors of the toner images formed on the photoconductors 1Y, 1M, 1C, and 1Bk, respectively. Other than the colors, they have the same configuration. The image forming unit 10Y will be described in detail as an example.
[0217] The image forming unit 10Y has a charging unit 2Y, an exposure unit 3Y, a developing unit 4Y, and a cleaning unit 6Y arranged around the photoconductor 1Y, which is an image forming body. The image forming unit 10Y forms a yellow (Y) toner image on the photoconductor 1Y. In this embodiment, at least the photoconductor 1Y, the charging unit 2Y, the developing unit 4Y, and the cleaning unit 6Y of the image forming unit 10Y are provided so as to be integrated.
[0218] The charging means 2Y is a means for applying a uniform potential to the photoreceptor 1Y. The charging means may be of a contact or non-contact roller charging type, and is preferably of a contact roller charging type.
[0219] The exposure means 3Y is a means for exposing the photoconductor 1Y, to which a uniform potential has been applied by the charging means 2Y, based on an image signal (yellow) to form an electrostatic charge image corresponding to the yellow image. Examples of the exposure means 3Y include those composed of LEDs and imaging elements in which light-emitting elements are arranged in an array in the axial direction of the photoconductor 1Y, and those composed of a laser optical system.
[0220] The developing means 4Y has, for example, a developing sleeve incorporating a magnet and rotating while holding a two-component developer, and a voltage application device that applies a DC or AC bias voltage between the photoconductor 1Y and this developing sleeve.
[0221] The cleaning means 6Y has a cleaning blade provided so that its tip contacts the surface of the photoreceptor 1Y, and also has a brush roller provided upstream of the cleaning blade, which contacts the surface of the photoreceptor 1Y. The cleaning blade has a function of removing residual toner adhering to the photoreceptor 1Y and also a function of scraping the surface of the photoreceptor 1Y.
[0222] The brush roller has the functions of removing residual toner adhering to the photoreceptor 1Y, collecting residual toner removed by the cleaning blade, and rubbing the surface of the photoreceptor 1Y. That is, the brush roller comes into contact with the surface of the photoreceptor 1Y, and at the contact point, rotates in the same direction as the photoreceptor 1Y. The brush roller removes residual toner and paper powder on the photoreceptor 1Y, and also transports and collects the residual toner removed by the cleaning blade.
[0223] In the image forming apparatus 100, an intermediate transfer body is used in the process of transferring the toner image formed on the photoconductor to a transfer medium. After the toner image is primarily transferred onto the intermediate transfer body, the toner image is secondarily transferred onto a recording medium.
[0224] The toner images of each color formed by the image forming units 10Y, 10M, 10C, and 10Bk are transferred successively onto a rotating endless belt-like intermediate transfer body 70 of the intermediate transfer body unit 7 by primary transfer rollers 5Y, 5M, 5C, and 5Bk as primary transfer means. Then, a composite color image is formed. The endless belt-like intermediate transfer member 70 is a semiconductive endless belt-like second image carrier that is wound around a plurality of rollers 71, 72, 73, and 74 and supported rotatably.
[0225] The color image synthesized on the endless belt-like intermediate transfer body 70 is then transferred to a recording medium P. The recording medium here is an image support that bears the fixed final image, and examples of such a recording medium include plain paper and transparent sheets.
[0226] Specifically, the recording medium P accommodated in a paper feed cassette 20 is fed by a paper feed unit 21. The recording medium P passes through a plurality of intermediate rollers 22A, 22B, 22C, and 22D and a registration roller 23, and is transported to a secondary transfer roller 5b serving as a secondary transfer unit.
[0227] Then, the color image is collectively transferred (secondarily transferred) from the endless belt-like intermediate transfer body 70 onto the recording medium P by the secondary transfer roller 5b. The recording medium P onto which the color image has been transferred is fixed by the fixing means 24, and is sandwiched between the paper discharge rollers 25 and placed on the paper discharge tray 26 outside the machine.
[0228] The fixing means 24 may be, for example, a heat roller fixing type. The heat roller fixing type is configured with a heating roller having a heat source inside and a pressure roller that is in pressure contact with the heating roller so as to form a fixing nip portion.
[0229] Meanwhile, a color image is transferred onto the recording medium P by a secondary transfer roller 5b as a secondary transfer means. Thereafter, residual toner is removed from the endless belt-like intermediate transfer body 70 from which the recording medium P has been separated by curvature by a cleaning means 6b.
[0230] During image formation, the primary transfer roller 5Bk is always in contact with the photoconductor 1Bk. The other primary transfer rollers 5Y, 5M, and 5C are in contact with the corresponding photoconductors 1Y, 1M, and 1C only when a color image is formed. The secondary transfer roller 5b is in contact with the endless belt-like intermediate transfer member 70 only when the recording medium P passes therethrough and secondary transfer is performed.
[0231] In the image forming apparatus 100, the housing 8 including the image forming units 10Y, 10M, 10C, and 10Bk and the intermediate transfer unit 7 can be pulled out from the apparatus main body A via support rails 82L and 82R.
[0232] Although a color laser printer has been described using the image forming apparatus 100 shown in Fig. 3, the image forming apparatus can also be applied to monochrome laser printers and copy machines. In addition, the exposure light source may be a light source other than a laser, for example, an LED light source. EXAMPLES
[0233] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified. In the following examples, operations were carried out at room temperature (25° C.) unless otherwise specified.
[0234] 1. Preparation of toner for developing electrostatic images (1) Preparation of amorphous polyester dispersion (1.1) Synthesis of amorphous polyester 1 (AP-1) Bisphenol A ethylene oxide adduct 11.0 parts by mass Bisphenol A propylene oxide adduct 29.0 parts by mass Ethylene glycol 34.0 parts by mass Propylene glycol 41.0 parts by mass Terephthalic acid 100.0 parts by mass Dodecenylsuccinic acid 130.0 parts by mass Trimellitic acid 15.0 parts by mass
[0235] The monomer components were charged into a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube. Next, the inside of the reaction vessel was replaced with dry nitrogen gas, and 0.3 mass% of tin dioctanoate was charged into the reaction vessel based on the total mass of the monomer components. The temperature was raised to 235°C over 1 hour under a nitrogen gas flow, and the monomers were reacted for 3 hours. The pressure in the reaction vessel was reduced to 10.0 mmHg, and the reaction was continued with stirring until the reaction product reached the desired molecular weight, at which point the reaction was terminated. The resulting amorphous polyester 1 had a glass transition temperature of 61° C. and a weight average molecular weight of 42,000.
[0236] (1.2) Synthesis of amorphous polyesters 2 to 9 (AP-2 to AP-9) Amorphous polyesters 2 to 9 (AP-2 to AP-9) were synthesized in the same manner as in the synthesis of amorphous polyester 1, except that the polyhydric alcohol monomer component was changed as shown in Table I.
[0237] The polyhydric alcohol components used in the synthesis of each amorphous polyester are shown in Table I. Note that "-" indicates that the corresponding component was not used.
[0238] [Table 1]
[0239] (1.3) Preparation of amorphous polyester dispersion 1 (AP-1) Amorphous polyester 1 (AP-1) 100.0 parts by mass Methyl ethyl ketone 60.0 parts by mass Isopropyl alcohol 15.0 parts by weight The above ingredients were placed in a reaction vessel equipped with a stirrer and dissolved at 60°C.
[0240] 10% ammonia aqueous solution 3.5 parts by weight The reaction vessel was then cooled to 35°C before the above ingredients were added.
[0241] Ion-exchanged water 300.0 parts by mass The above components were then dropped into the reaction vessel over a period of 3 hours. Next, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to obtain amorphous polyester dispersion 1 (AP-1). The median particle size of the obtained amorphous polyester was 150 nm.
[0242] (1.4) Preparation of amorphous polyester dispersions 2 to 9 (AP-2 to AP-9) Amorphous polyester dispersions 2 to 9 were obtained in the same manner as in the preparation of amorphous polyester dispersion 1, except that amorphous polyester 1 was changed to amorphous polyester 2 to 9.
[0243] (2) Preparation of crystalline polyester dispersion (2.1) Synthesis of crystalline polyester 1 (CP-1) 1,10-Decanedicarboxylic acid 350.0 parts by mass 1,6-Hexanediol 170.0 parts by mass The monomer components were charged into a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube. Next, the inside of the reaction vessel was replaced with dry nitrogen gas, and 0.3 mass% of tin dioctanoate was charged into the reaction vessel based on the total mass of the monomer components. After stirring and reacting for 3 hours at 160°C under a nitrogen gas flow, the temperature was further raised to 180°C over 1.5 hours. Then, the pressure inside the reaction vessel was reduced to 3 kPa, and the reaction was terminated when the desired molecular weight was reached, to obtain crystalline polyester 1 (CP-1). The melting point of the obtained crystalline polyester 1 (CP-1) was 73°C, and the weight average molecular weight was 28,000.
[0244] (2.2) Preparation of Crystalline Polyester Dispersion 1 (CP-1) Crystalline polyester 1 (CP-1) 100.0 parts by mass Methyl ethyl ketone 60.0 parts by mass Isopropyl alcohol 15.0 parts by weight The above ingredients were placed in a reaction vessel equipped with a stirrer and dissolved at 65°C.
[0245] 10% ammonia aqueous solution 5.0 parts by weight The reaction vessel was then cooled to 60° C. before the above ingredients were added.
[0246] Ion-exchanged water 300.0 parts by mass The above components were then dropped into the reaction vessel over a period of 3 hours. Next, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to obtain a crystalline polyester dispersion 1 (CP-1). The median particle size of the obtained crystalline polyester was 150 nm.
[0247] (3) Preparation of release agent dispersion Paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd.) 100.0 parts by mass Anionic surfactant "Neogen (registered trademark) RK" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 1.0 parts by mass Ion-exchanged water 350.0 parts by mass The above components were mixed, heated to 100°C, and dispersed using a homogenizer "Ultra Turrax T50" (manufactured by IKA). After that, the mixture was dispersed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin) to obtain a release agent dispersion. The median particle size of the resulting release agent was 200 nm.
[0248] (4) Preparation of cyan colorant dispersion Cyan pigment (Dainichi Seika Chemicals Co., Ltd., Pigment Blue 15:3 (copper phthalocyanine)) 45.0 parts by mass Anionic surfactant "Neogen (registered trademark) R" (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 2.0 parts by mass Ion-exchanged water 250.0 parts by mass The above components were mixed and dispersed using a high-pressure impact disperser, Ultimizer HJP30006 (manufactured by Sugino Machine Co., Ltd.), to obtain a cyan colorant dispersion. The median particle size of the obtained colorant was 150 nm.
[0249] (5) Toner production (5.1) Preparation of Toner 1 Amorphous polyester dispersion 1 (AP-1) (solid content equivalent) 54.5 parts by mass Crystalline polyester dispersion 1 (CP-1) (solid content equivalent) 15.0 parts by mass Release agent dispersion (solid content equivalent) 4.5 parts by weight Cyan colorant dispersion (solid content equivalent) 6.0 parts by mass 6.3 parts by weight of 10% aluminum sulfate aqueous solution Ion-exchanged water 650.0 parts by mass
[0250] The above components were placed in a round stainless steel flask. Then, using a homogenizer "Ultra Turrax T50" (manufactured by IKA), they were mixed and dispersed at 5000 rpm for 10 minutes. After that, the reactants in the flask were heated to 40°C while stirring. Thereafter, the temperature was raised at 0.5°C per minute, and the temperature was maintained when the particle size of the reactants reached 5.5 μm.
[0251] Amorphous polyester dispersion 1 (AP-1) (solid content equivalent) 20.0 parts by mass The above ingredients were then added dropwise over a period of 1 hour.
[0252] Ethylenediaminetetraacetic acid (EDTA) tetrasodium salt "Chilest 40" (manufactured by Chelest Co., Ltd.) 11.0 parts by mass After the above components were added, an aqueous sodium hydroxide solution was added to adjust the pH of the reaction solution to 8. Then, the temperature of the reaction solution was increased to 82.5° C., and the pH of the reaction solution was then decreased by 0.05 every 10 minutes with nitric acid, and stirring was continued for 45 minutes.
[0253] The reaction solution was cooled to 40°C or less, stirring was stopped, and the aggregates were removed by filtration using a filter with 45 μm openings. The pH of the reaction solution was adjusted to 4 with hydrochloric acid, and a water-containing cake (aggregate of toner base particles) was taken out using a centrifuge. While centrifuging, the water-containing cake was washed with ion-exchanged water in an amount 10 times the solid content of the toner base particles, and then dehydrated for 10 minutes to take out the water-containing cake of toner base particles 1.
[0254] Next, a drying process was performed using a "Flash Jet Dryer" (manufactured by Seishin Co., Ltd.). The airflow temperature measured and calculated by the above-mentioned method was set to 80°C, and the airflow speed was set to 10 m / sec. The obtained water-containing cake 1 was supplied to a dryer and dried so that the outlet temperature of the dryer became 35°C. The moisture content of the aggregate of toner base particles after the drying process was measured and was found to be 1.2% by mass relative to the total mass of the toner base particles.
[0255] Toner base particles 1 100.0 parts by weight Hydrophobic silica particles (number average primary particle size: 12 nm, hydrophobicity: 68) 1.0 parts by mass Hydrophobic titanium oxide particles (number average primary particle size: 20 nm, hydrophobicity: 63) 0.5 parts by mass Sol-gel silica (number average primary particle size: 110 nm) 1.0 parts by mass The above components were mixed for 20 minutes in a Henschel mixer (manufactured by Nippon Coke & Engineering Co., Ltd.) at a rotor peripheral speed of 40 m / sec and at 32° C. After mixing, coarse particles were removed using a sieve with 45 μm openings, and toner 1 was obtained.
[0256] (5.2) Preparation of Toners 2 to 21 In the preparation of Toner 1, the type of amorphous polyester, the dehydration time in the washing step, and the airflow temperature and airflow speed in the drying step were changed as shown in Table II. Otherwise, Toners 2 to 21 were prepared in the same manner as in the preparation of Toner 1. The airflow temperature and airflow velocity were measured and calculated by the above-mentioned method.
[0257] 2. Preparation of two-component developer Toner 6.0 parts by weight Ferrite carrier (volume average particle size 60 μm) 100.0 parts by mass By mixing the above components, two-component developers 1 to 21 were each prepared.
[0258] 3. Evaluation (1) Low-temperature fixability A multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta, Inc.) was used as a fixing device, which was modified so that the surface temperatures of the upper fixing belt and the lower fixing roller could be changed. Then, each of the obtained two-component developers was loaded into the multifunction printer in order. The multifunction printer was modified so that the fixing temperature, toner adhesion amount, and system speed could be freely set.
[0259] Under normal temperature and humidity conditions (temperature 20°C, humidity 50% RH), A4 size high-quality paper "NPI high-quality (127.9 g / m 2 The amount of toner attached to a paper sheet (manufactured by Nippon Paper Industries Co., Ltd.) was measured at 11.3 g / m 2 Then, an experiment was carried out to fix an image of 100 mm x 100 mm size.
[0260] The experiment to fix the image was repeated by changing the fixing temperature from 110°C in 2°C increments until it reached 180°C. The lowest fixing temperature at which image staining due to fixing offset was not visually confirmed was defined as the lowest fixing temperature (UO avoidance temperature). The low-temperature fixing ability was evaluated according to the following evaluation criteria. The results are shown in Table II below.
[0261] (Evaluation Criteria) A: The minimum fixing temperature is less than 135° C. (excellent toner with excellent low-temperature fixing properties). B: The minimum fixing temperature is 135° C. or higher and lower than 140° C. (a level that does not cause any practical problems). C: The minimum fixing temperature is 140° C. or higher (the toner is not sufficiently fixed at the target paper feed speed, and is at a level that is problematic in practical use).
[0262] (2) Image Unevenness Each of the obtained two-component developers was placed in a developing machine in a developing means of a commercially available full-color copier "bizhub PRESS (registered trademark) C1060" (Konica Minolta, Inc.), and the following evaluations were performed.
[0263] Under conditions of 30°C temperature and 85% RH (high temperature and high humidity), POD gloss coated paper 128g / m 2 " (Oji Paper Co., Ltd.) with a toner adhesion of 4 g / m 2 A solid patch image of 20 mm x 20 mm size was output. The density of the 20 mm square image on this print was then measured at five points using a fluorescent spectrodensitometer "FD-7" (Konica Minolta, Inc.) to determine the reflection density difference (difference between the maximum and minimum values) of the solid image and evaluate it according to the following criteria. In this evaluation, a reflection density difference of 0.10 or less was considered to be acceptable. As shown in Figure 4, five points were selected in the image: the intersection of the diagonals as the center point, and the midpoints between the center point and the four corners.
[0264] (Evaluation Criteria) A: The reflection density difference is 0.05 or less, which is at a level that does not cause any practical problems. B: The reflection density difference is more than 0.05 and 0.10 or less, which is at a level that does not cause any practical problems. C: The reflection density difference exceeds 0.10, which is a practically problematic level.
[0265] The evaluation results are shown in Table II. In the table, "content*1" indicates the content of structural units derived from bisphenol A or bisphenol A derivatives relative to the total number of moles of structural units derived from polyhydric alcohol in the amorphous polyesters AP-1 to AP-9. The content was measured by the pyrolysis gas chromatography mass spectrometry (GC / MS) described above.
[0266] [Table 2]
[0267] From the examples and comparative examples, it is evident that the images formed using the toner produced by the method of the present invention can suppress unevenness in density.
[0268] Comparison of Examples 1 to 3 shows that the amorphous polyester does not have a structural unit derived from bisphenol A or a bisphenol A derivative as a structural unit derived from a polyhydric alcohol, and therefore the reflection density difference in image unevenness is reduced.
[0269] A comparison of Examples 1, 10 to 13, and 17 shows that image unevenness can be further suppressed by keeping the air flow speed within the range of 8 to 20 m / sec. [Explanation of symbols]
[0270] 100 Image forming device 1Y, 1M, 1C, 1Bk photoconductor 2Y, 2M, 2C, 2Bk Charging means 3Y, 3M, 3C, 3Bk exposure method 4Y, 4M, 4C, 4Bk developing means 5Y, 5M, 5C, 5Bk Primary transfer roller 5b Secondary transfer roller 6Y, 6M, 6C, 6Bk, 6b Cleaning means 7 Intermediate transfer unit 8. Cabinet 10Y, 10M, 10C, 10Bk Image forming unit 20 Paper feed cassette 21 Paper feeding means 22A, 22B, 22C, 22D Intermediate rollers 23 Resist Roller 24 Fixing Method 25 Paper ejection roller 26 Output tray 40 Flash dryer 42 Inlet 43 Nozzle 44 Recovery nozzle 45 Outlet 46A Drying Area 46B Upstack Area 46C Classification area 47 Hot air supply section 48 Hot air inlet 50 Flash dryer 51 Blower 52 Heater 55 Feeder 56 Cyclone 57 Bag Filter 58 Blower 59 Piping 70 Endless belt type intermediate transfer body 71, 72, 73, 74 Roller 82L, 82R Support rails SC Original Image Scanner P Transfer material pw Low specific gravity dry powder PW High specific gravity powder
Claims
1. A method for producing a toner for developing an electrostatic image, comprising drying wet toner base particles to produce a toner for developing an electrostatic image, the method comprising the steps of: the toner base particles contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from bisphenol A or bisphenol A derivatives in the amorphous polyester relative to the total number of moles of structural units derived from the polyhydric alcohol is 10 mol % or less; drying the wet toner base particles by airflow in a dryer; The temperature of the airflow is 60° C. or higher; The air flow speed is 5 m / sec or more.
2. A method for producing a toner for developing an electrostatic image, comprising the steps of:
2. The amorphous polyester does not have a structural unit derived from bisphenol A or a bisphenol A derivative as a structural unit derived from the polyhydric alcohol.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
3. The polyhydric alcohol is an aliphatic polyhydric alcohol having 5 to 7 carbon atoms.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
4. The content of the amorphous polyester is 20% by mass or more based on the total mass of the toner base particles.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
5. The glass transition temperature of the amorphous polyester is within a range of 30 to 70° C.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
6. The glass transition temperature of the toner for developing an electrostatic image is within a range of 15 to 40° C.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
7. The toner base particles contain a crystalline polyester.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
8. The melting point of the crystalline polyester is 75° C. or less. The method for producing a toner for developing an electrostatic image according to claim 7 .
9. The crystalline polyester has a structural unit derived from an aliphatic diol and a structural unit derived from an aliphatic carboxylic acid. The method for producing a toner for developing an electrostatic image according to claim 7 .
10. The number of carbon atoms contained in the aliphatic diol or the aliphatic carboxylic acid is within the range of 6 to 10. The method for producing a toner for developing an electrostatic image according to claim 9 .
11. the toner base particles contain a release agent, The melting point of the release agent is within the range of 60 to 80° C.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
12. The toner base particles have a core-shell structure.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
13. The air flow speed is within a range of 8 to 20 m / sec.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
14. The content of the solvent in the wet toner base particles is within a range of 15 to 30% by mass.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
15. The method further comprises the step of removing the solvent from the wet toner base particles prior to the drying step.
2. The method for producing a toner for developing an electrostatic image according to claim 1.
Citation Information
Patent Citations
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2016066018A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2017062344A