Method for preventing corrosion of steel structure

The cathodic protection method enhances corrosion resistance by forming an insulating and conductive coating on steel structures, using specific resin compositions and conductive pigments, effectively preventing rust in exposed areas.

JP2024148169APending Publication Date: 2024-10-17SHINTO PAINT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024060379
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-04-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing cathodic protection methods fail to provide long-term corrosion resistance in areas exposed to rainwater, leading to rust formation in damaged areas of steel structures.

Method used

A corrosion prevention method using a cathodic protection device that involves forming an insulating coating film on the steel structure, followed by a water-insoluble conductive coating film, with a DC voltage applied between the conductive coating and the steel structure, utilizing specific resin compositions and conductive pigments to enhance durability.

Benefits of technology

The method significantly improves the durability of the conductive coating film, providing effective corrosion protection for steel structures by preventing rust formation even under prolonged exposure to rainwater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148169000001_ABST
    Figure 2024148169000001_ABST
Patent Text Reader

Abstract

To provide a method for preventing corrosion, which uses an electric corrosion preventing device, improves durability of an electroconductive coating film, and improves a corrosion preventing property.SOLUTION: The method for preventing corrosion of steel structures includes: forming an insulating coating film on a surface of a steel structure; forming a water-insoluble electroconductive coating film on the surface of the insulating coating film, which is a cured coating film of any one of a cured coating film of a two pack acrylic urethane coating material that contains an electroconductive pigment, a cured coating film of a two pack polyester urethane coating material that contains an electroconductive pigment, a cured coating film of a two pack acrylic silicone urethane coating material that contains an electroconductive pigment, and a cured coating film of a two pack fluorine urethane coating material that contains an electroconductive pigment; and then applying a DC voltage between the electroconductive coating film and the steel structure, by using the electroconductive coating film as an anode and the steel structure as a cathode.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a corrosion protection method for a steel structure, and more particularly to a corrosion protection method using an electric corrosion protection device for a steel structure. [Background technology]

[0002] Steel structures exposed to the atmosphere, such as frames, bridges, tanks, and machines, contain impurities such as carbon, and the surface of the steel can be considered to be a collection of countless micro-batteries. When the steel surface comes into contact with moisture in the air or rainwater, positive ions (corrosive Fe 2+ ) moves to the cathode via moisture or rainwater, where the cations react with oxygen and other substances to form rust.

[0003] To prevent this rust from forming, anticorrosive paint has been applied to the outer surface of steel structures to form an anticorrosive coating. However, if parts of the structure become exposed due to coating defects such as uneven coating, physical damage, or deterioration of the coating, the exposed parts of the structure will corrode. For this reason, repairs and repainting are periodically performed in short periods of time, especially in salt-damaged areas near the coast.

[0004] Furthermore, to extend the time between repainting, heavy-duty anti-corrosion paint consisting of an undercoat, intermediate coat, and top coat is applied, but this complicates the application process, which leads to increased costs.

[0005] As an alternative to heavy duty coating, cathodic protection has been proposed, in which a conductive paint is applied to the steel structure and a cathodic protection device is used to apply a voltage.

[0006] Fig. 1 is a conceptual cross-sectional view of a basic cathodic protection device for implementing cathodic protection of a steel structure. As shown in Fig. 1, an insulating paint is applied as an undercoat to the surface of a steel structure 1 to form an insulating coating film 2, and a conductive coating film 3 made of conductive paint is provided on the outer surface of the insulating coating film 2. Furthermore, a DC power source 4 is connected to the steel structure 1 and the conductive coating film 3 so that the steel structure 1 serves as the cathode and the conductive coating film 3 serves as the anode, and a required voltage, for example, a voltage of about 3 V, is applied between the steel structure 1 and the conductive coating film 3 by the DC power source 4.

[0007] When a scratch (damaged part) occurs on the steel structure 1, sea salt particles, rainwater, dew point water, etc. adhere to the damaged part, and the damaged part is covered with an electrolyte, causing the damaged part to corrode and generate red rust. In response to this, when a DC voltage within an appropriate range is applied between the conductive coating film 3 and the steel structure 1, with the conductive coating film 3 as the anode and the steel structure 1 as the cathode, a corrosion protection current flows from the conductive coating film 3 to the steel structure 1 through the electrolyte, and the steel structure 1 is protected from corrosion. In other words, electricity is constantly on standby on the inner surface of the conductive coating film 3, and the potential of the steel material of the steel structure 1 located inside the conductive coating film 3 is kept in an inactive region (corrosion protection potential) via the insulating coating film 2, thereby making it possible to prevent the generation of red rust from the steel material (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 3402959 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the invention of Patent Document 1 has a problem in that even if a voltage is applied, if the damaged part is exposed to rainwater for a long period of time, rust occurs in the damaged part, resulting in poor corrosion resistance. Further improvement in corrosion resistance is desired.

[0010] The object of the present invention has been made in consideration of the above-mentioned problems, and is to provide a corrosion prevention method using an electrochemical protection apparatus, which improves the durability of a conductive coating film and improves the corrosion prevention properties of the electrochemical protection apparatus.

[0011] The electrochemical protection method disclosed herein is characterized in that an insulating coating film is formed on the surface of a steel structure, a water-insoluble conductive coating film is formed on the surface of the insulating coating film, and then a DC voltage is applied between the water-insoluble conductive coating film and the steel structure, with the water-insoluble conductive coating film as the anode and the steel structure as the cathode. Effect of the Invention

[0012] According to the present disclosure, it is possible to provide an electrochemical protection method that improves the durability of a water-insoluble conductive coating film and improves the corrosion prevention properties of an electrochemical protection device. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a conceptual cross-sectional view of a basic cathodic protection device configuration for performing cathodic protection of a steel structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A corrosion prevention method using the electrical protection apparatus of this embodiment involves forming an insulating coating on the surface of a steel structure, forming a water-insoluble conductive coating on the surface of the insulating coating, and then applying a DC voltage between the water-insoluble conductive coating and the steel structure, with the water-insoluble conductive coating as the anode and the steel structure as the cathode.

[0015] In Fig. 1, an insulating coating film 2 is formed as an electrically insulating anticorrosive coating film that covers the surface of a steel structure 1. The paint that constitutes the insulating coating film 2 is, for example, a synthetic resin paint such as chlorinated rubber, urethane resin, or epoxy resin.

[0016] Furthermore, the insulating coating film 2 is not limited to one layer, but may be composed of multiple insulating coating layers including at least one anticorrosive insulating coating layer. By configuring the insulating coating film 2 with multiple insulating coating layers including at least one anticorrosive insulating coating layer, the corrosion resistance of the steel structure 1 can be improved and the insulation between the conductive coating film 3 and the steel structure 1 can be ensured.

[0017] The present invention is a corrosion prevention method for improving the durability of a water-insoluble conductive coating film and improving the corrosion prevention properties of an electrolytic protection device.

[0018] Conventional conductive coating films have the problem that even when a voltage is applied, if the film is exposed to rainwater for a long period of time, rust will form on the damaged area, resulting in poor corrosion resistance.

[0019] The present invention believes that improving the durability of the conductive coating film and allowing electrical corrosion protection to function effectively for a long period of time will improve the durability of the system as a whole, and aims to improve the durability of the resin used in the conductive coating film.

[0020] Such a resin is one that reacts at room temperature after application to eliminate functional groups, and is preferably, for example, a two-component or three-component curable resin. Examples of such a resin include a two-component acrylic urethane resin, a two-component polyester urethane resin, a two-component acrylic silicone resin, a two-component acrylic silicone urethane resin, a fluorourethane resin, and an alkyd urethane resin.

[0021] Among these, two-component acrylic urethane resin, two-component polyester urethane resin, two-component acrylic silicone resin, and two-component fluorourethane resin are preferred because they form a highly durable water-insoluble conductive coating film. Furthermore, two-liquid type acrylic urethane resins are particularly preferred because they form water-insoluble conductive coating films with extremely high durability.

[0022] A two-component acrylic urethane resin is composed of a base material made of an acrylic prepolymer containing two or more functional groups and an isocyanate-terminated urethane oligomer as a curing agent, and after application, a curing reaction occurs to generate urethane bonds, resulting in a cured crosslinked coating film.

[0023] The functional group of the functional group-containing acrylic prepolymer can be a hydroxyl group or the like, and the number of functional groups is 2 or more. The acrylic prepolymer having two or more functional groups is a compound containing a polymerized unit based on an acryloyl group or a methacryloyl group and two or more functional groups that react with an isocyanate, and can be obtained, for example, by copolymerizing a (meth)acrylic acid ester with a functional group-containing monomer.

[0024] Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, n-octyl (meth)acrylate, n-stearyl (meth)acrylate, etc. Examples of the functional group-containing monomer include hydroxyl group-containing (meth)acrylic acid ester such as 2-hydroxyethyl (meth)acrylate, etc.

[0025] Examples of isocyanate group-terminated urethane oligomers include tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate. The polyisocyanate compound may be a biuret type, an isocyanurate ring type, or a uretdione type dimer or trimer. If necessary, additives can be added.

[0026] If an acrylic prepolymer containing two or more functional groups is mixed with an isocyanate-terminated urethane oligomer at the time of use, the isocyanate groups of the isocyanate-terminated urethane oligomer will react with functional groups such as hydroxyl groups of the acrylic prepolymer to crosslink, forming a crosslinked coating film that will be stronger.

[0027] A two-component polyester urethane resin is composed of a base material made of a polyester prepolymer containing two or more hydroxyl groups and an isocyanate-terminated urethane oligomer as a curing agent, and after application, a curing reaction occurs to generate urethane bonds, resulting in a cured crosslinked coating film.

[0028] The number of hydroxyl groups in the polyester prepolymer containing hydroxyl groups is 2 or more. A preferred example of the polyester prepolymer having 2 or more hydroxyl groups is polyester polyol. Examples of polyester polyols include those obtained by reacting polybasic acids such as succinic acid, glutaric acid, adipic acid, isophthalic acid, and terephthalic acid with diols such as ethylene glycol, propylene glycol, butanediol, hexanediol, cyclohexanediol, and xylylene glycol. The number of hydroxyl groups can be increased by adding a small amount of polybasic acids such as tribasic acids and polyols such as triols to the reaction. If a polyester prepolymer containing two or more hydroxyl groups is mixed with the above-mentioned isocyanate-terminated urethane oligomer at the time of use, the isocyanate groups of the isocyanate-terminated urethane oligomer will react with the hydroxyl groups of the polyester prepolymer to crosslink, forming a crosslinked coating film that will be stronger.

[0029] Two-component acrylic silicone resin, two-component acrylic silicone urethane resin Fat In the acrylic prepolymer of the above two-liquid acrylic urethane resin, hydrolyzable silyl groups can be introduced into the acrylic prepolymer by copolymerizing a hydrolyzable silyl group-containing (meth)acryloxyalkyl compound, such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropylmethyldimethoxysilane, γ-(meth)acryloxypropylmethyldichlorosilane, γ-(meth)acryloxytrichlorosilane, etc. Hydrolyzable silyl groups react with each other due to moisture and bond together. In particular, two-component acrylic silicone urethane resins containing hydrolyzable silyl groups, like the two-component acrylic urethane resins mentioned above, undergo cross-linking as the isocyanate groups of the isocyanate-terminated urethane oligomer react with the hydroxyl groups of the acrylic prepolymer, and at the same time, the hydrolyzable silyl groups in the acrylic polyol react with each other to form siloxane bonds (-Si-O-Si-), resulting in further cross-linking and the formation of a stronger cross-linked coating film.

[0030] The two-liquid type fluorourethane resin can be used as a fluorine-containing prepolymer having fluorine in the side chain by copolymerizing a fluorine-containing (meth)acrylic acid ester such as perfluoroalkylethyl (meth)acrylate in the above two-liquid type acrylic urethane resin. Also, a polyol having fluorine in the main chain by copolymerizing a fluoroolefin with a monomer having a hydroxyl group can be used as the fluorine-containing prepolymer. Examples of the fluoroolefin include tetrafluoroethylene, chlorotrifluoroethylene, vinylidene fluoride, and perfluoropropyl vinyl ether. Examples of the monomer having a hydroxyl group that can be copolymerized with the fluoroolefin include a monomer having a hydroxyl group, a vinyl group, or a propenyl group such as hydroxybutyl vinyl ether and hydroxybutyl propenyl ether. By copolymerizing these, a polyol having two or more hydroxyl groups and fluorine in the main chain can be obtained. A two-liquid type fluorourethane resin is formed from these fluorine-containing prepolymers and an isocyanate group-terminated urethane oligomer.

[0031] In the above various resins, the blending ratio of the acrylic prepolymer (hereinafter, when the term acrylic prepolymer is used, it may include polyester prepolymer and fluorine-containing prepolymer) and the urethane oligomer can be the same as that used under normal coating conditions for paints.

[0032] The ratio (NCO / OH ratio) of the number of isocyanate groups (NCO) in the isocyanate-terminated urethane oligomer to the number of hydroxyl groups (OH) in the acrylic prepolymer containing two or more hydroxyl groups is preferably 0.5 to 1.5, and particularly preferably 0.8 to 1.2. When the NCO / OH ratio is 0.5 or more and 1.5 or less, the durability of the conductive coating film can be improved, and the cathodic protection can effectively function for a long period of time. When the NCO / OH ratio is 0.8 or more and 1.2 or less, a water-insoluble conductive coating film with extremely high durability is obtained, the durability of the coating film can be significantly improved, and an excellent cathodic protection system for steel structures can be achieved.

[0033] Examples of the conductive pigment that is mixed with the above-mentioned paint resin to impart conductivity include water-insoluble conductive pigments such as conductive carbon black, acetylene black, furnace black, thermal black, channel black, Ketchen black, Vulcan, carbon nanotubes, graphene, vapor-grown carbon fiber, and graphite. These may be used alone or in combination of two or more. As the conductive pigment, conductive carbon is preferably used in terms of performance and price.

[0034] The water-insoluble conductive paint can be obtained by mixing the above-mentioned conductive pigment with the above-mentioned resin under normal paint forming conditions.

[0035] In the case of a two-liquid type acrylic urethane resin, it is preferable to disperse the conductive pigment using an acrylic oligomer, which does not react when blended with the conductive pigment, as a pigment dispersing resin.

[0036] The resin content in the water-insoluble conductive coating film is usually 20 to 90 mass %, preferably 30 to 80 mass %, more preferably 40 to 70 mass % of the water-insoluble conductive coating film. The conductive pigment content in the water-insoluble conductive coating film is usually 15 to 60 mass %, preferably 20 to 55 mass %, more preferably 25 to 50 mass % of the water-insoluble conductive coating film.

[0037] A curing catalyst may be added to accelerate the curing reaction of the resin. The curing catalyst may be one that has been used as a urethane reaction catalyst or a hydrolyzable silyl group condensation catalyst, such as an organic titanate compound (isopropyl triisostearoyl titanate, isopropyl tri(dioctyl pyrophosphate) titanate, tetraisopropyl di(lauryl phosphite) titanate, etc.), an organic aluminum compound (acetoalkoxy aluminum diisopropylate, etc.), a tin carboxylate compound (tin dioctyl acid, dibutyltin dilaurate, dibutyltin maleate, etc.), a sulfur-containing organic tin compound such as a sulfide type or a mercaptide type (dibutyltin sulfide, etc.), triethylamine, dibutylamine-2-hexoate, cyclic amidine and its salt, etc.). These catalysts may be used alone or in combination of two or more. The amount of the curing catalyst added is usually 0.001 to 20% by weight based on the amount of the resin.

[0038] In preparing a coating material, known additives such as a diluent such as a solvent, an ultraviolet absorber, a light stabilizer, an anti-sagging agent, a leveling agent, an antifoaming agent, and a dehydrating agent may be added.

[0039] The water-insoluble conductive paint can be prepared by mixing and dispersing the above-mentioned components using a conventionally known dispersing machine, such as a paint shaker, a sand mill, a ball mill, a pebble mill, an LMZ mill, a DCP mill, a planetary ball mill, a homogenizer, a twin-screw kneader, or a thin film rotary high-speed mixer.

[0040] The method for forming a coating film on a steel structure is carried out as follows.

[0041] First, a cathode is electrically connected to the steel structure. The cathode can be made of any conductive material, such as a stainless steel or copper sheet. Next, an insulating paint is applied to the entire outer surface of the steel structure. After drying for about one week, an insulating coating film is formed. The water-insoluble conductive paint is then applied on the insulating coating film. When the water-insoluble conductive paint is applied on the insulating coating film, it reacts and hardens. After the coating film is formed, a voltage is applied. The insulating coating film has a thickness of preferably 30 μm to 1000 μm, and the water-insoluble conductive coating film has a thickness of preferably 5 μm to 300 μm.

[0042] An anode is usually electrically connected to the water-insoluble conductive coating film. The anode supplies power to the water-insoluble conductive coating film. The anode can be made of any conductive material, such as a stainless steel or copper sheet. A material that does not ionize is more preferable because it can maintain its insolubility.

[0043] An anode may be attached on the insulating coating film, and then a water-insoluble conductive coating film may be formed on the insulating coating film to electrically connect the anode to the water-insoluble conductive coating film, or an anode may be attached on the water-insoluble conductive coating film to electrically connect the anode to the water-insoluble conductive coating film. Then, a direct current voltage of preferably 2.3 to 4 V is applied to the anode. A resistor may also be inserted before the anode. This can increase the applied voltage.

[0044] When supplying voltage, a rectifier diode, a switch means, and a voltage limiting device may be provided in the DC voltage supply circuit to prevent reverse current flow. The external power source is not limited to a commercial power source, and a solar cell or a wireless power supply device may also be used.

[0045] Examples of steel materials for steel structures to which the corrosion prevention method of the present invention can be applied include cold-rolled steel sheets, hot-rolled steel sheets, galvanized steel sheets, alloy galvanized steel sheets, zinc-iron alloy plated steel sheets, zinc-aluminum alloy plated steel sheets, aluminum plated steel sheets, chrome plated steel sheets, nickel plated steel sheets, zinc-nickel alloy steel sheets, tin plated steel sheets, etc. Structures using these steel materials are not particularly limited, and examples include painted or unpainted steel structures that exist in the atmosphere, such as bridges, plants, and steel building frames. In particular, the method can be preferably applied to seaside steel structures, which are prone to rust.

[0046] Examples of surface treatments that may be optionally performed on steel materials include washing with water, washing with hot water, pickling, alkaline degreasing, polishing, chromate treatment, phosphate treatment, zinc phosphate treatment, blast treatment, composite oxide coating treatment, and the like, and these treatments may be performed alone or in combination.

[0047] The present disclosure will now be further illustrated by, but not limited to, the following examples.

[0048] Example 1 A pearl mill was charged with 78.5 parts by mass of "ACRYDIC A-859-B" (acrylic prepolymer, manufactured by DIC Corporation, solid content 75%, OHV 103), 74.0 parts by mass of xylene, 65.0 parts by mass of toluene, 40.0 parts by mass of methyl isobutyl ketone, 26.0 parts by mass of PMA, "DISPERBYK-164" (dispersant, manufactured by BYK-Chemie), 50.0 parts by mass of Denka Black LI-400 (pigment, manufactured by Denka Corporation, solid content 100%), and 6.0 parts by mass of "DISPARLON 4200-20" (thickener, manufactured by Kusumoto Chemicals, solid content 20%), and mixed at room temperature for 1 hour to produce a base with the pigment dispersed therein. In addition, a liquid was prepared by mixing 23.0 parts by mass of "Duranate 24A-100" (hardening agent, manufactured by Asahi Kasei Corporation, solid content 100%, NCO 23.5%), which is an isocyanate-terminated urethane oligomer, as a hardening agent for this mixed liquid, and 15.2 parts by mass of xylene. Conductive paint A was prepared by mixing this base and curing agent in a ratio of 9:1.

[0049] On a sandblasted plate (RzJIS25μm: TP Giken), "Neo Gosei #2300PS" (Shinto Paint Co., Ltd., insulating paint, two-component epoxyamine type) was spray-painted and dried at room temperature for one day. After drying, the insulating coating film had a thickness of 120μm. On top of this, the base and hardener of the above-mentioned conductive coating A were mixed in a ratio of 9:1 and spray-painted, then dried at room temperature for one day. After drying, the conductive coating film had a thickness of 30μm. An anode terminal (1cm x 1cm x 0.3mm stainless steel plate) with an electric wire connected was attached to the surface of the conductive coating film. "Dotite D-500" (Fujikura Kasei Co., Ltd., conductive adhesive) was used to bond the anode terminal to the electric wire, and the anode terminal to the conductive film. Furthermore, "Shinto Flon #100S-HB" (Shinto Paint Co., Ltd., insulating paint, two-component fluorourethane type) was spray-painted on top of this as a protective film. After drying at room temperature for one day, the protective film had a thickness of 55μm. An anode terminal (1cm x 1cm x 0.3mm stainless steel plate) with an electric wire connected was attached to the back of the test plate. "Dotite D-500" was used to bond the cathode terminal to the electric wire, and the cathode terminal to the test plate. After that, "Neo Gosei #2300PS" was spray painted on the back of the test plate. This was called test sheet a.

[0050] Tables 1 and 2 below show the components, blend amounts, and design values ​​of the base and hardener for each conductive paint. In Example 1, the base and curing agent were prepared in the same manner as in Example 1 using the raw materials shown in Tables 1 and 2, and conductive paints B to M of the examples and conductive paints N to P of the comparative examples were produced. In Tables 1 and 2, conductive paints A to J are two-component acrylic urethane paints containing conductive pigments, conductive paint K is a two-component acrylic silicone paint containing conductive pigments, conductive paint L is a two-component polyester urethane paint containing conductive pigments, conductive paint M is a two-component fluorine urethane paint containing conductive pigments, conductive paint N is a two-component epoxy paint containing conductive pigments, conductive paint O is an acrylic urethane paint containing conductive pigments but does not use a hardener, and conductive paint P is a one-component acrylic paint containing conductive pigments. In particular, for the two-liquid type acrylic urethane paints A to F, the same base and hardener were combined with an NCO / OH ratio in the range of 0.5 to 1.5. The types of solvent, dispersant, pigment, and thickener used in the conductive paints were the same when preparing the conductive paints. In addition, the mixed P / B (pigment / binder ratio) of all the conductive paints was standardized to 0.61 by mass.

[0051] [Table 1]

[0052] [Table 2]

[0053] The raw materials used to prepare the conductive paint are as follows: Acrylic A-859-B: Acrylic prepolymer, manufactured by DIC, solid content 75%, OHV 103mg-KOH / g Acrylic WBU-305: Acrylic prepolymer, manufactured by DIC, solid content 55%, OHV 52mg-KOH / g Acrydic WFU-289: Acrylic prepolymer, manufactured by DIC, solid content 50%, OHV 20mg-KOH / g Desmophen 1300BA: Polyester prepolymer, Bayer, 75% solids OHV 106mg-KOH / g Acrydic A-166: One-component acrylic resin, manufactured by DIC, solid content 45% Acrydic A-9585: Moisture-curing silicone acrylic resin, manufactured by DIC. Solids: 80% Zeffle GK-570: Fluorine resin, Daikin Industries, solids 65%, OHV 60mg-KOH / g EPICLON1050-75X: Epoxy resin, manufactured by DIC, solid content 75%, PMA: Abbreviation for propylene glycol methyl ether acetate DISPERBYK-164: Dispersant, BYK, 60% solids Denka Black LI-400: Pigment, manufactured by Denka Co., 100% solids Duranate 24A-100: Hardener, Asahi Kasei Corporation, 100% solids, 23.5% NCO Acrydic A-9540: Moisture-curing silicone hardener, manufactured by DIC, solid content 45% Duranate TPA-100: Hardener, Asahi Kasei Corporation, 100% solids, 23.1% NCO TOMAID 423: Epoxy resin hardener, manufactured by T&K TOKA, Solids 60% Disparlon 4200-20: Thickener, manufactured by Kusumoto Chemicals, solid content 20%

[0054] (Examples 1 to 22, Comparative Examples 1 to 4) Using the conductive paints B to P shown in Tables 1 and 2, test sheets b to p and a-2 to a-8 were produced in the same manner as in Example 1. Test sheets a to p were produced by changing only the conductive paint, and test sheets a-2 to a-8 were produced by using the conductive paint A but changing conditions other than the conductive paint. For the test sheets a to p and a-2 to a-8 prepared as described above, the adhesion (primary adhesion, water-resistant secondary adhesion) between the conductive coating film and the undercoat coating film was evaluated. In addition, the surfaces of the test sheets a-p and a-2-a-8 were partially cut and scratched as damaged areas. These test sheets a-p and a-2-a-8 were subjected to durability tests under the conditions of CCT cycle D (JIS K 5600-7-9) in a combined cycle tester CYP-90 (Suga Testing Machines) while applying a DC voltage in the range of 2.3 to 4.0 V using a DC stabilized power supply PS30V5A10 (As One), and the durability results were evaluated every 250 hours from 500 hours to 2000 hours and after 2500 hours. The resistance value of the coating sheet was within the range of 100 to 500 Ω / sq. The occurrence of red rust from the cut areas (hereinafter sometimes referred to as CCT results) was evaluated. The results are shown in Tables 3 and 4. Table 3 shows the results of durability tests of conductive coatings A to M under an applied voltage of 2.5 V, and Table 4 shows the results of durability tests using conductive coating A to determine whether or not there was insertion resistance, the effects of the film thickness of the undercoat coating and conductive coating, and comparative conductive paints N to P.

[0055] [Table 3]

[0056] [Table 4]

[0057] (Evaluation method) 1. Red rust occurrence 〇: The maximum rust width (bulge width) from the cut part is 0 mm, and the red rust of the cut part is less than 50%. 〇△: The maximum rust width (bulge width) from the cut part is 0 mm, and red rust is more than 50% of the cut part. △: The maximum width of rust (bulge) from the cut part is within 1 mm △×: The maximum width of rust (bulge) from the cut part is less than 3 mm ×: The maximum width of rust (bulge) from the cut is 3 mm

[0058] 2. Adhesion (primary, secondary water resistance) Primary adhesion The coating was scored at 1 mm intervals in a 10 mm x 10 mm area, adhesive tape was applied, and the number of squares in which all three layers of the coating remained when the tape was peeled off was visually counted and evaluated. For example, if 15 out of 100 pieces remained in the peel test, it was recorded as 15 / 100. -Water-resistant secondary adhesion The test plate was immersed in ion-exchanged water for 24 hours, taken out, and dried, and then subjected to the same test as for the primary adhesion to evaluate the water-resistant secondary adhesion.

[0059] (Evaluation Results) 1. Examples 1 to 13 The cured coatings of two-component acrylic urethane paint, the cured coatings of two-component polyester urethane paint containing conductive pigment, the cured coatings of two-component acrylic silicone paint containing conductive pigment, and the cured coatings of two-component fluoro urethane paint containing conductive pigment showed good CCT results and adhesion, and showed good durability. Among these, the cured coatings of two-component acrylic urethane paint with an NCO / OH ratio of 0.8 to 1.2, the cured coatings of two-component polyester urethane paint containing conductive pigment, and the cured coatings of two-component acrylic silicone paint containing conductive pigment showed particularly excellent CCT results.

[0060] 2. Examples 14 to 16 A resistor was inserted in front of the anode to increase the applied voltage in Examples 15 and 16. In the applied voltage range of 2.3 V to 4.0 V, all of the samples showed excellent CCT results and good adhesion.

[0061] 3. Examples 17 to 22 In the range of 60 to 1000 μm for the undercoat film thickness and 20 to 100 μm for the conductive coating film thickness, both showed excellent CCT results and good adhesion.

[0062] 4. Comparative Examples 1 to 4 The two-component epoxy paint of Comparative Example 1 started to blister after 1000 hours CCT. The acrylic urethane paint without a hardener of Comparative Example 2 and the one-component acrylic paint of Comparative Example 3 showed blistering of less than 1 mm after 2500 hours CCT, but had poor adhesion. In Comparative Example 4, where no voltage was applied, swelling occurred even after 500 hours.

[0063] 5.The above results show that the cured coatings of two-liquid type acrylic urethane paint containing conductive pigment, the cured coatings of two-liquid type polyester urethane paint containing conductive pigment, the cured coatings of two-liquid type acrylic silicone paint containing conductive pigment, and the cured coatings of two-liquid type fluorine urethane paint containing conductive pigment have good durability compared to the cured coatings of the current epoxy / amine-based paint containing conductive pigment. Among these, the cured coatings of two-liquid type acrylic urethane paint containing conductive pigment with an NCO / OH ratio of 0.8 to 1.2, the cured coatings of two-liquid type polyester urethane paint containing conductive pigment, and the cured coatings of two-liquid type acrylic silicone paint containing conductive pigment showed particularly excellent CCT results, and it is believed that the cured coatings of two-liquid type acrylic urethane paint with an NCO / OH ratio of 0.8 to 1.2 functioned as an excellent water-insoluble conductive coating. From the above, it has been found that the corrosion protection method for steel structures of the present invention, in which an insulating coating film is formed on the surface of a steel structure, a water-insoluble conductive coating film is formed on the surface of the insulating coating film, and then a DC voltage is applied between the conductive coating film and the steel structure with the conductive coating film as the anode and the steel structure as the cathode, is an excellent method for corrosion protection for steel structures. [Explanation of symbols]

[0064] 1 Steel structures 2. Insulating coating 3. Conductive coating 4 DC power supply

Claims

1. A method for protecting a steel structure from corrosion, comprising forming an insulating coating film on the surface of a steel structure, forming a water-insoluble conductive coating film on the surface of the insulating coating film, and then applying a DC voltage between the conductive coating film and the steel structure with the conductive coating film as the anode and the steel structure as the cathode.

2. 2. The corrosion protection method for steel structures according to claim 1, characterized in that the water-insoluble conductive coating film is any one of a cured coating film of a two-component acrylic urethane paint containing a conductive pigment, a cured coating film of a two-component polyester urethane paint containing a conductive pigment, a cured coating film of a two-component acrylic silicone paint containing a conductive pigment, and a cured coating film of a two-component fluorourethane paint containing a conductive pigment.

3. 3. The corrosion protection method for steel structures according to claim 1 or 2, characterized in that the water-insoluble conductive coating film is a coating film produced by a curing reaction between a base material made of a prepolymer containing two or more hydroxyl groups and a curing agent made of an isocyanate group-terminated urethane oligomer, and the ratio of the number of the isocyanate groups to the number of the hydroxyl groups is 0.5 or more and 1.5 or less.

Citation Information

Patent Citations

  • Corrosion protection device for steel structures

    JP3402959B2