Oil impregnated sintered bearing

By defining a hill rise ratio and groove depth, the sintered oil-impregnated bearings maintain stable oil film formation and dynamic pressure, addressing the challenges of groove deformation and ensuring effective support for rotating components.

JP2024148326AActive Publication Date: 2024-10-18NTN CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023061372
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
2043-04-05

AI Technical Summary

Technical Problem

Sintered oil-impregnated bearings face challenges in maintaining dynamic pressure grooves on the inner diameter surface, especially when the inner diameter is 1 mm or less, leading to scraping and deformation, which affects oil film formation and stability.

Method used

The solution involves defining a hill rise ratio for the dynamic pressure groove, ensuring the ratio (A+B)/D is 0.5 or less, where A and B are the widths of the hill rising portions and D is the overall width, and setting the groove depth to 0.5 μm or more, along with a sintered density of 7.3-7.9 g/cm³ and a true density ratio of 86-94%, to maintain a rectangular shape and ensure stable oil film formation.

Benefits of technology

This approach ensures stable oil film formation and improves the springback of the bearing, maintaining the dynamic pressure grooves' integrity and enhancing the bearing's ability to support rotating components without contact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148326000001_ABST
    Figure 2024148326000001_ABST
Patent Text Reader

Abstract

To provide an oil impregnated sintered bearing capable of regulating anew a hill portion rising ratio as the shape of a dynamic pressure groove, namely, securing oil film formation property while providing an index mark and satisfying the index mark.SOLUTION: The oil impregnated sintered bearing includes a radial dynamic pressure generation part having radial dynamic pressure grooves and a dynamic pressure hill portion between the dynamic pressure grooves, on the inner diameter face. In such a shape that the circularity shape of the radial dynamic pressure groove is linearly developed, when both hill portion rising width sizes at the height positions of the dynamic pressure hill portion having a size of 0.2 μm from a center line along the development direction are set as A and B, respectively, and a total hill portion width is set as D, a hill portion rising ratio E is (A+B) / D and the hill portion rising ratio E is 0.5 or lower.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintered oil-impregnated bearing. [Background technology]

[0002] Oil-impregnated sintered bearings are generally used for bearings that support the rotation of small motors such as spindle motors and fan motors in magnetic disk drives (HDDs) for polygon mirrors in laser beam printers (LBPs).

[0003] This type of sintered oil-impregnated bearing can be used, for example, in a fluid dynamic bearing device in which herringbone, spiral or other type of dynamic pressure grooves are provided on the bearing surface and the action of the dynamic pressure grooves as the shaft rotates generates a dynamic oil film in the bearing gap, thereby supporting the shaft in a floating state.

[0004] Conventionally, as described in Patent Document 1, there is a method in which a core rod having dynamic pressure grooves on the outer diameter side is inserted into the inner diameter surface of a bearing and molded to transfer the dynamic pressure grooves to the inner diameter surface of the bearing (dynamic pressure sizing). That is, when processing dynamic pressure grooves in a sintered oil-impregnated bearing, for the inner diameter surface, a core rod with dynamic pressure grooves processed on the outer diameter in advance is inserted into the inner diameter of a sintered body, and then pressure is applied from the outside of the sintered body to make the inner diameter cling to the core rod, and the sintered body is plastically deformed and pressed into the dynamic pressure grooves of the die to transfer the grooves. After the transfer, the pressure from the outside is released, causing the sintered body to spring back, and at the same time, the inner diameter that was clinging to the core rod also separates from the core rod. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3782900 Summary of the Invention [Problem to be solved by the invention]

[0006] Normally, when the inner diameter becomes small, the amount of springback becomes small, and when the core rod is pulled out, the inner diameter surface and the core rod rub against each other, and there is a risk of scraping off the dynamic pressure groove ridge portion, which is the outermost surface of the inner diameter surface of the sintered body. Also, when the inner diameter dimension of the sintered body is 1 mm or less, the amount of springback becomes small, making it difficult to transfer the dynamic pressure groove.

[0007] The cause of the hydrodynamic grooves becoming shallow is insufficient transfer or a small amount of springback, which causes the inner diameter surface and the core rod to rub against each other when the core rod is removed, resulting in the hydrodynamic groove ridge portion, which is the outermost surface, being scraped off.

[0008] To prevent the inner diameter surface from being scraped by the core rod, the amount of springback can be increased. Methods of increasing the pressure from the outer diameter or increasing the density can be considered for this purpose. However, due to constraints such as dimensional accuracy, there is a limit to how much the outer diameter compression can be increased to increase the pressure, making it difficult to ensure a sufficient amount of springback. For this reason, it is difficult to completely prevent the dynamic pressure hill portion from being scraped.

[0009] When the inner diameter of the sintered body is 1 mm or less, it is unavoidable for the dynamic pressure hill portion to be scraped off, and there is a possibility that the shape may deviate from the ideal rectangular shape. However, at present, there are no indicators for determining whether the dynamic pressure hill portion is close to a rectangular shape that can ensure oil film formation, and so the determination is made based solely on the groove depth. In other words, in order to ensure stable oil film formability, it is sufficient for the dynamic pressure hill portion to be close to a rectangle in shape; therefore, an index is determined that results in a dimensional shape that ensures stable oil film formability, and if it falls within this index, the product will be able to ensure oil film formability.

[0010] In view of the above problems, the present invention provides a sintered oil-impregnated bearing that specifies a new hill rise ratio for the shape of the dynamic pressure groove, i.e., sets an index, and satisfies this index to ensure oil film formability. [Means for solving the problem]

[0011] The sintered oil-impregnated bearing of the present invention has a radial dynamic pressure generating portion on its inner diameter surface, the radial dynamic pressure generating portion having radial dynamic pressure grooves and dynamic pressure ridges between the radial dynamic pressure grooves, and in a linear development of the roundness shape of the radial dynamic pressure groove, when the rise width dimensions of both ridges at a height position of the dynamic pressure ridges that is 0.2 μm from the center line along the development direction are A and B, respectively, and the total width of the ridge is D, the ridge rise ratio E is (A+B) / D, and the ridge rise ratio E is 0.5 or less. Here, linear development refers to developing polar coordinates obtained from roundness data into Cartesian coordinates, and the Cartesian coordinates are obtained by analyzing the roundness data in terms of flatness.

[0012] In the sintered oil-impregnated bearing of the present invention, the hill rising ratio E=(width A+width B) / total hill width D is set to 0.5 or less, so that the hill rising portion can approach a rectangle.

[0013] The hill rise ratio is a ratio based on coordinate data formed by linearly expanding the roundness shape measured by the least squares center method. The ratio obtained in this manner is reliable. Here, the least squares center method determines the reference circle of the part where the square of the error is the smallest, and determines the radii of the circumscribing circle and the inscribing circle that are concentric with this reference circle. In this case, the roundness is calculated as (radius of the circumscribing circle) - (radius of the inscribing circle).

[0014] The radial dynamic pressure groove depth is preferably 0.5 μm or more. If the groove depth is 0.5 μm or more, a stable dynamic pressure can be ensured.

[0015] Sintered density is 7.3g / cm 3 ~7.9g / cm 3 It is possible to improve springback by increasing the density, but increasing the density can easily deteriorate the circulation characteristics of the lubricating oil, and if the density is low, the transferability of the grooves becomes poor. Therefore, the sintered density is set to 7.3 g / cm 3 ~7.9g / cm 3 is desirable.

[0016] The true density ratio is preferably 86% to 94%. Here, "true density ratio" refers to the value (percentage) obtained by dividing the density of the porous body constituting the sintered metal dynamic pressure bearing by the density that would be obtained if the porous body had no pores. By making the true density ratio of the sintered metal dynamic pressure bearing 86% or more, the strength of the bearing can be increased and fluctuations in the dimensions of the bearing (particularly the inner diameter dimension) can be suppressed. Furthermore, by keeping the true density ratio at 94% or less, moldability after sintering can be ensured and the internal pores can be prevented as much as possible from becoming independent pores, allowing the internal pores to be impregnated with the required amount of lubricating oil.

[0017] It is preferable that the dynamic pressure groove angle of the radial dynamic pressure groove is 25° to 60° with respect to the circumferential direction. If the dynamic pressure groove angle of the bearing part is less than 25°, the axial tearing when the pin is removed is likely to become large, and conversely, if the dynamic pressure groove angle exceeds 60°, the dynamic pressure will be weak.

[0018] The inner diameter dimension can be set to 0.2 mm to 1.0 mm. Generally, when forming the dynamic pressure grooves, in order to obtain a bearing in which the amount of springback of the sintered body (bearing) is small after the dynamic pressure grooves are transferred and the dynamic pressure groove ridges are scraped off and oil film formability is ensured, if the ridge rise ratio E is set to 0.5 or less, then even if the inner diameter dimension is 0.2 mm to 1.0 mm, the rise of the ridge can be made close to a rectangle, and oil film formability can be sufficiently ensured. Effect of the Invention

[0019] In the present invention, the ridge rising ratio E = (width A + width B) / total ridge width D is set to 0.5 or less, so that the ridge rising portion can be made closer to a rectangle, thereby providing a sintered oil-impregnated bearing that can ensure the formation of an oil film. [Brief description of the drawings]

[0020] [Figure 1] 1 is a cross-sectional view of a spindle motor using a fluid dynamic bearing device of the present invention. [Diagram 2]1 is a cross-sectional view of a sintered oil-impregnated bearing according to the present invention. [Diagram 3] 1 is a block diagram showing steps of a method for manufacturing a sintered oil-impregnated bearing according to the present invention. FIG. [Figure 4] 1A and 1B show a sizing process, in which (a) is a simplified diagram of sizing, and (b) is a simplified diagram during sizing. [Diagram 5] 1A and 1B show a groove machining process, in which (a) is a simplified diagram before groove machining, and (b) is a simplified diagram during groove machining. [Figure 6] FIG. 2 is an explanatory diagram of the shapes of the dynamic pressure grooves and dynamic pressure hills in a state where the dynamic pressure grooves of the sintered oil-impregnated bearing according to the present invention are linearly expanded. [Figure 7] FIG. 13 is a waveform diagram showing measurements of dynamic pressure grooves and dynamic pressure hills of the invention. [Figure 8] FIG. 1 is a waveform diagram showing a pair of hill-groove shapes of the invention. [Figure 9] FIG. 13 is a waveform diagram showing measurements of dynamic pressure grooves and dynamic pressure hills of a comparative product. [Figure 10] FIG. 13 is a waveform diagram showing a pair of hill-groove shapes of a comparative product. [Figure 11] FIG. 1 is a graph showing the results of an oil film formation test of the product of the present invention. [Figure 12] FIG. 1 is a graph showing the results of an oil film formation test for comparative products. [Figure 13] FIG. 11 is a diagram showing the measurement results of roundness measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] 1 shows a spindle motor used in a disk drive device of an HDD. This spindle motor includes a fluid dynamic bearing device 1, a disk hub 3 fixed to a shaft member 2 of the fluid dynamic bearing device 1, a stator coil 4 and a rotor magnet 5 facing each other with a radial gap therebetween, and a bracket 6. The stator coil 4 is fixed to the bracket 6, and the rotor magnet 5 is fixed to the disk hub 3. A housing 7 of the fluid dynamic bearing device 1 is fixed to the inner diameter surface of the bracket 6. A predetermined number of disks 10 (two in the illustrated example) are held on the disk hub 3. When current is applied to the stator coil 4, the rotor magnet 5 rotates, and as a result, the disks 10 held by the disk hub 3 rotate integrally with the shaft member 2.

[0022] The fluid dynamic bearing device 1 comprises a sintered oil-impregnated bearing 8 according to one embodiment of the present invention, a shaft member 2 inserted into the inner periphery of the sintered oil-impregnated bearing 8, a bottomed cylindrical housing 7 to which the sintered oil-impregnated bearing 8 is fixed to its inner diameter surface, and a seal member 9 disposed at the opening of the housing 7. For convenience, in the following explanation of the fluid dynamic bearing device 1, the opening side of the housing 7 in the axial direction will be referred to as the upper side, and the opposite side as the lower side.

[0023] A flange portion 2b provided at the lower end of the shaft member 2 is housed between a lower end surface 8e of the sintered oil-impregnated bearing 8 and an upper end surface 7b1 of the bottom portion 7b of the housing 7 facing it.

[0024] A first radial dynamic pressure generating portion 8a and a second radial dynamic pressure generating portion 8b are formed at two locations axially separated on the inner diameter surface of the sintered oil-impregnated bearing 8. The first radial dynamic pressure generating portion 8a has a plurality of dynamic pressure grooves 8a1 and dynamic pressure ridge portions 8a2 formed between the dynamic pressure grooves 8a1, and the second radial dynamic pressure generating portion 8b has a plurality of dynamic pressure grooves 8b1 and dynamic pressure ridge portions 8b2 formed between the dynamic pressure grooves 8b1. In this embodiment, the dynamic pressure grooves 8a1, 8b1 are arranged in a herringbone pattern, for example, as shown in FIG. 2.

[0025] In the entire surface or a partial annular region of the lower end surface 8e of the sintered oil-impregnated bearing 8, a thrust dynamic pressure generating portion is formed, for example, in a region where a plurality of dynamic pressure grooves are arranged in a spiral shape (not shown).

[0026] In the hydrodynamic bearing device configured as above, when the shaft member 2 rotates, the region in which the dynamic pressure grooves 8a1, 8b1 are formed on the inner diameter surface of the sintered oil-impregnated bearing 8 form a radial bearing gap between it and the opposing outer circumferential surface 2a of the shaft member 2. As the shaft member 2 rotates, the lubricating oil in the radial bearing gap is forced toward the axial center of the dynamic pressure grooves 8a1, 8b1, and its pressure increases. In this way, the dynamic pressure action of the lubricating oil generated by the dynamic pressure grooves 8a1, 8b1 forms a first radial bearing portion R1 and a second radial bearing portion R2 that support the shaft member 2 in a non-contact manner in the radial direction.

[0027] At the same time, the pressure of the lubricating oil film formed in the thrust bearing gap between the lower end surface 8e (dynamic pressure groove forming area) of the sintered oil-impregnated bearing 8 and the opposing upper end surface of the flange portion 2b, and in the thrust bearing gap between the upper end surface 7b1 (dynamic pressure groove forming area) of the bottom portion 7b of the housing 7 and the opposing lower end surface of the flange portion 2b, is increased by the dynamic pressure action of the dynamic pressure grooves. Then, the pressure of these oil films forms a first thrust bearing portion T1 and a second thrust bearing portion T2 that support the flange portion 2b (shaft member 2) in the thrust direction in a non-contact manner.

[0028] An annular groove (not shown) and a plurality of radial grooves (not shown) provided on the inner diameter side of the annular groove are formed on the upper end surface 8d of the sintered oil-impregnated bearing 8. A plurality of axial grooves 8c1 are provided at equal intervals in the circumferential direction on the outer peripheral surface 8c of the sintered oil-impregnated bearing 8. The space on the outer diameter side of the flange portion 2b of the shaft member 2 communicates with the seal space via these axial grooves 8c1, the annular groove, the radial grooves, etc., thereby preventing the generation of negative pressure in this space.

[0029] The sintered oil-impregnated bearing 8 is manufactured in the steps shown in Fig. 3. That is, the manufacturing process is carried out in the order of a powder compacting step S1, a sintering step S2, a sizing step (dimensional sizing step) S3, a sealing step (rotational sizing step) S4, and a dynamic pressure groove forming step S5. The powder compacting step S1 is a step of compressing and molding metal powder such as Cu powder, Cu alloy powder, Fe powder, and Fe powder coated with Cu into a cylindrical shape, the sintering step S2 is a step of sintering the powder compact obtained in the powder compacting step at a predetermined sintering temperature, the dimensional sizing step S3 is a step of sizing the sintered body obtained in the sintering step to a predetermined dimension by applying a compressive force, the sealing step S4 is a step of performing a sealing treatment on the inner diameter surface by rolling the material of the surface layer of the inner diameter surface of the sintered body, and the dynamic pressure groove forming step S5 is a step of forming dynamic pressure grooves on the inner diameter surface after the sealing treatment on the inner diameter surface.

[0030] A raw material powder mixing step is carried out before the powder compacting step S1. Here, the raw material powder mixing step is a step of producing raw material powder for the sintered oil-impregnated bearing 8 by mixing a plurality of types of powder.

[0031] Figures 4(a) and (b) show a processing device for performing the sizing process (dimension sizing process) S3, and this processing device is composed of, as its main elements, a sizing pin 12 that presses into the inner diameter surface 11a of the cylindrical sintered body 11, a die 16 that presses into the outer peripheral surface 11b of the sintered body 11, and a first punch 17 (upper punch) and a second punch 18 (lower punch) that restrain both axial end surfaces of the sintered body 11 from the top and bottom (axial direction).

[0032] An upper punch 17 is fitted onto the outer periphery of the sizing pin 12 so as to be slidable in the vertical direction. The sizing pin 12 and the upper punch 17 are raised and lowered by independent drive sources. In this embodiment, the sizing pin 12 is lowered in synchronization with the upper punch 17. In the die 16, the sizing pin 12 and the upper punch 17 are driven to rise and fall independently by a drive means (not shown). In this embodiment, the lower punch 18 is fixed to a stationary member of the device (e.g., a pedestal, etc.).

[0033] 4(a), the sintered compact 11, which is the workpiece, is placed on the upper end surface of the lower punch 18. The die 16 is placed on the outer diameter side of the sintered compact 11, with the entire outer circumferential surface 11b of the sintered compact 11 accommodated therein and with a slight gap remaining between the die 16 and the outer circumferential surface 11b. The sizing pin 12 and the upper punch 17 are placed axially above the sintered compact 11.

[0034] From the above state, as shown in Fig. 4(b), the sizing pin 12 is lowered and pressed into the inner circumference of the sintered compact 11. At this time, the outer peripheral surface 11b of the sintered compact 11 is restrained from being displaced in the outward direction by the die 16, so that the inner diameter surface 11a and its surface layer of the sintered compact 11 are subjected to a compressive force by the pressing of the sizing pin 12, and are displaced in the outward direction. As a result, the inner diameter surface 11a of the sintered compact 11 is sized to a predetermined inner diameter dimension.

[0035] Additionally, the upper punch 17 is lowered together with the sizing pin 12, and the upper punch 17 is pressed against the upper end surface of the sintered compact 11. As a result, the sintered compact 11 is restrained from both axial sides by the upper and lower punches 17, 18, and the sintered compact 11 is sized to a predetermined axial dimension.

[0036] After the above steps are completed, the die 16 is lowered while maintaining the restraining state by the die 16 and the upper and lower punches 17, 18, thereby releasing the compressive force in the inner diameter direction of the sintered compact 11. Next, the sizing pin 12 is raised, thereby releasing the compressive force in the outer diameter direction of the sintered compact 11. Finally, the upper punch 17 is raised, and the sintered compact 11 fixed to the sizing pin 12 is taken out of the processing device.

[0037] In the next sealing process (rotational sizing process) S4, a sizing pin with a substantially polygonal cross section is pressed into the inner diameter surface of the sintered body, and the sizing pin is rotated in this state (not shown). The corners of the sizing pin that come into contact with the inner diameter surface of the sintered body are rounded to a substantially arc-shaped cross section. This rotational sizing causes the material of the surface layer of the inner diameter surface of the sintered body to be rolled by the sizing pin, crushing the openings on the inner diameter surface and reducing the surface porosity of the inner diameter surface. In particular, since the sintered body contains a relatively large amount of copper, the surface layer of the inner diameter surface of the sintered body has high rollability, and the openings on the inner diameter surface are easily crushed.

[0038] In the next dynamic pressure groove forming step (groove sizing step) S5, the sintered body 28 is corrected to a predetermined dimensional accuracy by a sizing die 30 shown in FIG. 5, and dynamic pressure grooves are molded on the inner diameter surface 28a of the sintered body 28. Specifically, as shown in FIG. 5(a), a core rod 31 is inserted into the inner circumference of the sintered body 28 via a gap, and the axial width of the sintered body 28 is restrained by upper and lower punches 32 and 33. While maintaining this state, as shown in FIG. 5(b), the sintered body 28 is pressed into the inner circumference of a die 34. As a result, the sintered body 28 is compressed from the outer periphery, and the inner diameter surface 28a of the sintered body 28 is pressed against a molding die 31a formed on the outer periphery of the core rod 31, and the shape of the molding die 31a is transferred to the inner diameter surface 28a of the sintered body 28, forming dynamic pressure grooves 8a1 and 8b1 (see FIG. 2). Thereafter, the sintered body 28, the core rod 31, and the upper and lower punches 32, 33 are raised, and the sintered body 28 and the core rod 31 are taken out from the inner periphery of the die 34. At this time, the inner diameter surface 28a of the sintered body 28 expands in diameter due to springback, and the core rod 31 is peeled off from the molding die 31a of the outer periphery of the core rod 31. Then, the core rod 31 is pulled out from the inner periphery of the sintered body 28.

[0039] The internal pores of the sintered body 28 thus formed are impregnated with lubricating oil by a method such as vacuum impregnation, thereby completing the oil-impregnated sintered bearing 8 shown in FIG.

[0040] Incidentally, when the core rod 31 is pulled out from the inner circumference of the sintered body 28, it is inevitable that the dynamic pressure hills 8a2 and 8b2 are scraped to some extent. However, the dynamic pressure hills 8a2 and 8b2 are required to have a rectangular shape in order to form an oil film. Therefore, in the present invention, an index is set to ensure the oil film formability. That is, as shown in FIG. 6, it was found that the dimension setting approximates the rectangular shape required for the oil film formation.

[0041] In this case, when the dimensions of the rising widths of both hill portions at a height position of hill portion 8a2 (8b2) where dimension L from center line O along the expansion direction is 0.2 μm in a linear expansion of the circular shape of dynamic pressure generating portion 8a (8b), are A and B, respectively, and the total width of the hill portion is D, the hill portion rising ratio E is (A+B) / D, and the hill portion rising ratio E is 0.5 or less. Here, linear expansion means expanding the polar coordinates obtained from the circularity data into Cartesian coordinates, and the Cartesian coordinates are obtained by analyzing the circularity data in terms of flatness.

[0042] In this way, by limiting the hill portion rise ratio E = (width A + width B) / total hill portion width D to 0.5 or less, in other words, by determining the index for the hill portion rise ratio E to 0.5 or less, the rise portion of the dynamic pressure hill portion 8a2 (8b2) of the finished sintered oil-impregnated bearing becomes closer to a rectangle, and oil film formability can be ensured.

[0043] The radial dynamic pressure groove depth d1 is preferably 0.5 μm or more. If the groove depth d1 is 0.5 μm or more, a stable dynamic pressure can be ensured.

[0044] Sintered density is 7.3g / cm 3 ~7.9g / cm 3 It is possible to improve springback by increasing the density, but increasing the density tends to deteriorate the circulation characteristics of the lubricating oil, and if the density is low, the transferability of the grooves becomes poor. Therefore, the sintered density is set to 7.3 g / cm 3 ~7.9g / cm 3 is desirable.

[0045] The true density ratio is preferably 86% to 94%. Here, "true density ratio" refers to the value (percentage) obtained by dividing the density of the porous body constituting the sintered metal dynamic pressure bearing by the density that would be obtained if the porous body had no pores. By making the true density ratio of the sintered metal dynamic pressure bearing 86% or more, the strength of the bearing can be increased and fluctuations in the dimensions of the bearing (particularly the inner diameter dimension) can be suppressed. Furthermore, by keeping the true density ratio at 94% or less, moldability after sintering can be ensured and the internal pores can be prevented as much as possible from becoming independent pores, allowing the internal pores to be impregnated with the required amount of lubricating oil.

[0046] It is preferable that the dynamic pressure groove angle θ of the radial dynamic pressure groove (see FIG. 2) is 25° to 60° with respect to the circumferential direction. If the dynamic pressure groove angle θ is less than 25°, the axial tearing when the pin is removed tends to become large, and conversely, if the dynamic pressure groove angle θ exceeds 60°, the dynamic pressure becomes weak.

[0047] The inner diameter dimension d (see FIG. 2) can be set to 0.2 mm to 1.0 mm. Generally, when forming the dynamic pressure grooves, in order to obtain a bearing in which the amount of springback of the sintered body (bearing) is small after the dynamic pressure grooves are transferred and the dynamic pressure groove ridges are scraped off and oil film formability is ensured, if the ridge rise ratio E is set to 0.5 or less, then even if the inner diameter dimension is 0.2 mm to 1.0 mm, the rising portion of the ridge can be made close to a rectangle, and sufficient oil film formability can be ensured.

[0048] An embodiment of the present invention has been described above, however, the present invention is not limited to the above embodiment and various modifications are possible. For example, the above embodiment shows a case where the sintered oil-impregnated bearing 8 is fixed and the shaft member 2 rotates, but the present invention is not limited to this. It is also possible to adopt a configuration in which the shaft member 2 is fixed and the sintered oil-impregnated bearing 8 rotates, or a configuration in which both the shaft member 2 and the sintered oil-impregnated bearing 8 rotate.

[0049] Incidentally, in the process of forming the dynamic pressure grooves, in the process of pulling out the core rod 31 from the sintered body 28, the sintered body 28 may be heated and then pulled out. That is, the sintered body 28 is heated by a heating means (for example, by blowing hot air from a hot air blower) and the core rod 31 is pulled out. This heating makes the temperature of the sintered body 28 higher than the temperature of the core rod 31, and the inner diameter of the sintered body 28 becomes larger than the outer diameter of the core rod 31, making it easier to pull out the core rod 31.

[0050] A fluid dynamic bearing device incorporating an oil-impregnated sintered bearing 8 according to the present invention can be used not only in spindle motors used in disk drive devices for HDDs, but also in a wide range of other small motors, such as spindle motors incorporated in other information devices, polygon scanner motors in laser beam printers, color wheels in projectors, or cooling fan motors. EXAMPLES

[0051] Next, as described above, the groove shape of the formed radial dynamic pressure groove was determined, and the measurement chart of this groove shape is shown in Figures 7 and 9. That is, this measurement chart is based on coordinate data formed by linearly developing the roundness shape measured by a roundness measuring machine (RONCOM NEX 200 DX-11 manufactured by Tokyo Seimitsu Co., Ltd.) using the least squares center method. Here, the least squares center method determines the reference circle where the square of the error is the smallest, and determines the radii of the circumscribing circle and the inscribing circle that are concentric with this reference circle. In this case, the roundness is calculated as (radius of the circumscribing circle) - (radius of the inscribing circle).

[0052] The sintered oil-impregnated bearing used was a cylindrical body with an inner diameter of 0.6 mm, an outer diameter of 1.4 mm, and a total length of 1.7 mm. The core rod 31 had an outer diameter of 0.6 mm, and the shape of the mold formed on the outer peripheral surface had a diameter of 1.4 mm.

[0053] Incidentally, Fig. 13 shows the roundness profile measured by the least squares central method, and Fig. 7 and Fig. 9 show coordinate data formed by linearly developing the roundness profile shown in Fig. 13. Fig. 8 shows three patterns a, b, and c of the waveform of the measurement chart in Fig. 7, and Fig. 10 shows three patterns a1, b1, and c1 of the waveform of the measurement chart in Fig. 9.

[0054] The hill rise ratio E was then calculated for each of a, b, c, a1, b1, and c1. In this case, the hill rise ratio E was 0.17 for the pattern a of the example product, 0.17 for the pattern b of the example product, 0.25 for the pattern c of the example product, 0.13 for the pattern a1 of the comparison product, 0.66 for the pattern b1 of the comparison product, and 0.32 for the pattern c1 of the comparison product. The radial groove depth was 0.878 μm for the example product and 0.565 μm for the comparison product.

[0055] Next, an oil film formation test was carried out on a bearing having a radial dynamic pressure generating portion with the waveforms shown in Figures 7 and 9 and a bearing having a radial dynamic pressure generating portion with the waveforms shown in Figures 8 and 10, and the results are shown in Figures 11 and 12. The oil film formation test conditions are shown in Table 1 below. [Table 1]

[0056] In this case, a bearing unit radial oil film formation rate tester manufactured by NTN Corporation was used, and the rotation speed was set to 10,000 min -1 The ambient temperature is room temperature (24°C to 27°C), the diametral gap (clearance between the outer diameter surface of the shaft member and the inner diameter surface of the bearing) is 4μm, the radial load is 0.1N, and the oil is an ester type with a kinetic viscosity of 24mm at 40°C. 2 The test time was 140 seconds, and the measurement item was the oil film formation rate (waveform), with the state where the shaft and bearing were not in contact being taken as 100%.

[0057] As can be seen from the test results (Figures 11 and 12), the rotation speed of the invention was 10,000 min-1 In this case, the oil film formation rate was 100% between 0.125 minutes and 2.125 minutes, whereas in the comparative product, the oil film formation rate was not 100% between 0.125 minutes and 2.125 minutes.

[0058] This shows that in the embodiment, in all patterns a, b, and c, the hill rise ratio E was 0.25 or less, and the radial groove depth was 0.878 μm, which is deep, and sufficient dynamic pressure could be secured. That is, in the embodiment, the dynamic pressure hill portion could be made to approach a rectangular shape. Therefore, in the embodiment, the oil film formation rate was 100% between 0.125 minutes and 2.125 minutes. In contrast, the hill rise ratio E was 0.13 in pattern a1, 0.32 in pattern c1, and 0.66 in pattern b1, which exceeded 0.5. In addition, the radial groove depth was 0.565 μm. That is, in patterns a1 to c1, the dynamic pressure hill portion could not be made to approach a rectangular shape. Therefore, in the comparative product, the oil film formation rate was not 100% between 0.125 minutes and 2.125 minutes. [Explanation of symbols]

[0059] E ratio θ Dynamic pressure groove angle 8 Sintered oil-impregnated bearing 8a Radial dynamic pressure generating section 8a1 Dynamic pressure groove 8a2 Dynamic pressure hill 8b Radial dynamic pressure generating section 8b1 Dynamic pressure groove 8b2 Dynamic pressure hill

Claims

1. A sintered oil-impregnated bearing having a radial dynamic pressure generating portion on its inner diameter surface, the radial dynamic pressure generating portion having radial dynamic pressure grooves and dynamic pressure ridges between the dynamic pressure grooves, A sintered oil-impregnated bearing characterized in that, when the circularity shape of the radial dynamic pressure groove is linearly expanded, the rise width dimensions of both hill portions at a height position of the dynamic pressure hill portion that is 0.2 μm from the center line along the expansion direction are A and B, respectively, and the total width of the hill portion is D, the hill portion rise ratio E is (A+B) / D, and the hill portion rise ratio E is 0.5 or less.

2. 2. The sintered oil-impregnated bearing according to claim 1, wherein the hill rise ratio is a ratio based on coordinate data formed by linearly expanding a roundness profile measured by a least squares central method.

3. 3. The sintered oil-impregnated bearing according to claim 1, wherein the radial dynamic pressure groove depth is 0.5 μm or more.

4. Sintered density is 7.3 g / cm 3 ~7.9g / cm 3 3. The sintered oil-impregnated bearing according to claim 1 or 2, characterized in that

5. 3. The sintered oil-impregnated bearing according to claim 1, wherein the true density ratio is 86% to 94%.

6. 3. The sintered oil-impregnated bearing according to claim 1, wherein the dynamic pressure groove angle of the radial dynamic pressure groove is 25° or more and 60° or less with respect to the circumferential direction.

7. 3. The sintered oil-impregnated bearing according to claim 1, wherein the inner diameter is 0.2 mm to 1.0 mm.

Citation Information

Patent Citations

  • Method for determining lateral misalignment of cylindrical electrochemical machining electrode during manufacturing of fluid-dynamic bearing, involves determining lateral misalignment of electrode based on shape, depth and pitch of curve

    DE102009009889A1

  • Fluid dynamic pressure bearing arrangement and method of manufacturing the same

    JP2010084825A

  • Dynamic pressure bearing and manufacturing method thereof

    JP2018040458A

  • Hydrodynamic bearings and hydrodynamic bearing units

    JP3782900B2