Photo- and moisture-curable hot melt resin composition, adhesive for electronic parts and cured body
The photo-moisture-curable hot-melt resin composition with a urethane prepolymer and photopolymerization initiator addresses the issue of long curing times in moisture-curing adhesives and short pot life in fast-crystallizing adhesives, enabling efficient and precise bonding in electronic component assembly.
Patent Information
- Application Number
- JP2023061376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional moisture-curing urethane adhesives used in smartphone assembly take too long to develop adhesive strength, impacting productivity, while fast-crystallizing hot-melt adhesives have short pot life, making precise positioning difficult.
A photo-moisture-curable hot-melt resin composition comprising a urethane prepolymer with a specific structure, a radically polymerizable compound, and a photopolymerization initiator, which delays crystallization until UV irradiation, allowing for both short-time adhesion and sufficient pot life.
The composition achieves rapid adhesive strength development after lamination while ensuring adequate pot life for precise positioning, improving workability and productivity in electronic component assembly.
Smart Images

Figure 2024148329000005 
Figure 2024148329000006 
Figure 2024148329000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a light- and moisture-curable hot-melt resin composition, an adhesive for electronic components comprising the light- and moisture-curable hot-melt resin composition, and a cured product of the light- and moisture-curable hot-melt resin composition. [Background technology]
[0002] Conventionally, double-sided tape has often been used to bond or assemble parts of smart devices such as smartphones and wearable devices. However, in recent years, as smart devices have become smaller and curved, adhesives have come to be used to accommodate narrower bonding areas and more complex bonding surfaces. Portable electronic devices such as smart devices are carried around, and may be accidentally dropped while being carried or used. For this reason, the adhesive parts of the devices are required to be shock-resistant so that the bonded parts do not fall off when dropped.
[0003] For example, Patent Document 1 discloses a moisture-curable hot melt adhesive composition containing a urethane prepolymer (i) having an isocyanate group obtained by reacting a polyester polyol (A) and a polyether polyol (B) with an isocyanate (C), and a component (ii) that does not react with the urethane prepolymer (i). Patent Document 2 discloses a moisture-curable hot melt adhesive composition containing a urethane prepolymer having an isocyanate group, which is a reaction product of a polyol component containing a polyester polyol, a polyether polyol, and a polybutadiene polyol with an isocyanate component, and an antioxidant. Patent Documents 1 and 2 disclose that the moisture-curable hot melt adhesive composition has excellent impact resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6778379 [Patent Document 2] Patent No. 6947172 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, smartphones, which are representative of smart devices, have spread throughout the world, and with technological innovation creating high demand for new models, a huge number of approximately 1.3 billion units are currently produced annually. Producing such a large number of devices requires high productivity (efficiency and speed). In the production process of these smartphones, an assembly method is often used in which the housing, which contains the communication and processing circuit boards and the battery, is bonded to the display, which is equipped with the display element, touch sensor, etc., using a moisture-curing urethane adhesive. However, with conventional moisture-curing urethane adhesives, after the adhesive is applied and bonded to the adherend, it takes several tens of minutes to several hours for the adhesive to harden due to moisture and develop sufficient adhesive strength, which creates a bottleneck in productivity.
[0006] On the other hand, as a method for developing adhesive strength in a short time after applying the adhesive and bonding it to the adherend, an adhesive has been proposed in which the urethane of a moisture-curing urethane adhesive is made crystalline to turn it into a hot melt, the adhesive is melt-applied, and the two are quickly bonded together; when the adhesive temperature drops, it crystallizes and solidifies, developing adhesive strength, and then gradually moisture cures until it is completely cured. However, in such a hot melt type moisture-curing urethane adhesive, the adhesive must be bonded in a state in which it has fluidity until the temperature of the melt-applied adhesive drops and it crystallizes and solidifies. Here, in order to quickly develop adhesive strength after bonding, the hot melt type moisture-curing urethane adhesive is required to have a high crystallization rate. However, if the crystallization rate is high, the time during which the adhesive can be bonded to the opposing adherends after the adhesive is melt-applied to the adherends, that is, the so-called pot life, is shortened. Therefore, there is an inconvenience that there is not enough time to adjust the attachment position of the opposing adherends after the adhesive is melt-applied. On the other hand, in order to ensure a sufficient pot life, it is possible to suppress the crystallinity of the adhesive and lengthen the time from melt application to crystallization and solidification, but in that case, the curing time from bonding to developing adhesive strength is long, and there is a problem that the original advantage of the hot melt type moisture-curing urethane adhesive, which is to develop adhesive strength in a short time, is lost.
[0007] Therefore, an object of the present invention is to provide a light-moisture-curable hot melt resin composition that can ensure a sufficient pot life for lamination work while quickly crystallizing and solidifying after lamination to exhibit adhesive strength, thereby achieving both ease of work during lamination and high productivity through short adhesion, as well as an adhesive for electronic components and a cured product using the same. [Means for solving the problem]
[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a resin composition comprising a urethane prepolymer (A) having a specific structure that is solid at room temperature, a radically polymerizable compound (B), and a photopolymerization initiator (C), and have completed the present invention described below. That is, the present invention provides a light-and-moisture-curable hot melt resin composition that can achieve both workability during lamination and high productivity through short adhesion times, as well as an adhesive for electronic components and a cured product using the same, due to the following effects. A radically polymerizable compound (B) is added to a crystalline urethane prepolymer (A), and the radically polymerizable compound (B) acts as a plasticizer to suppress the crystallization of the urethane prepolymer (A). This delays the time until the adhesive loses fluidity due to crystallization and becomes unable to be bonded, thereby ensuring pot life, while the radically polymerizable compound (B) is polymerized by irradiating it with active light such as UV rays a certain time before bonding. This causes the plasticizer effect of the radically polymerizable compound (B) to be lost, restoring the crystallinity of the urethane prepolymer (A), and quickly expressing adhesive strength due to crystallization and solidification after bonding. The present invention provides the following [1] to
[24] . [1] A composition comprising a hot-melt urethane prepolymer (A) that is solid at room temperature, a radical polymerizable compound (B), and a photopolymerization initiator (C), A light-curable, moisture-curable hot-melt resin composition, wherein the hot-melt urethane prepolymer (A) is a reaction product of a material containing a polyether polycarbonate polyol (a1). [2] The light-curable, moisture-curable hot-melt resin composition according to [1], wherein the hot-melt urethane prepolymer (A) is a reaction product of a polyol (Aa) and a polyisocyanate (Ab), the polyol (Aa) comprises a polyether polycarbonate polyol (a1) and a polyol (a2) different from the polyether polycarbonate polyol (a1), and the polyol (a2) is at least one selected from the group consisting of polyester polyols and polycarbonate polyols. [3] The light-and-moisture-curable hot-melt resin composition according to [2], wherein the polyether polycarbonate polyol (a1) has a linear alkylene group having 3 to 8 carbon atoms. [4] The light-curable, moisture-curable hot melt resin composition according to [2] or [3], wherein the polyester polyol contains a structural unit derived from a linear polyol and a structural unit derived from a linear polycarboxylic acid. [5] The light-and-moisture-curable hot melt resin composition according to [4], wherein the linear polyol is 1,6-hexanediol, and the linear polycarboxylic acid is at least one selected from the group consisting of adipic acid and sebacic acid. [6] The light-curable and moisture-curable hot-melt resin composition according to any one of [2] to [5], wherein the polycarbonate polyol contains a structural unit derived from a linear polyol having 8 or more carbon atoms. [7] The light-and-moisture-curable hot melt resin composition according to any one of [2] to [6], wherein the polyol (Aa) contains 40% by mass or more and 70% by mass or less of the polyether polycarbonate polyol (a1) and 30% by mass or more and 60% by mass or less of the polyol (a2). [8] The light-curable, moisture-curable hot-melt resin composition according to any one of [2] to [7], wherein the polyol (a2) has a number average molecular weight of 2,000 or more and 4,000 or less. [9] The light-and-moisture-curable hot-melt resin composition according to any one of [1] to [8], further comprising a silane coupling agent.
[10] The light-curable, moisture-curable hot melt resin composition according to [9], wherein the silane coupling agent comprises an aromatic amine-based silane coupling agent.
[11] The light-curable, moisture-curable hot melt resin composition according to any one of [1] to
[10] , comprising 90 parts by mass or more of a monofunctional radically polymerizable compound per 100 parts by mass of the radically polymerizable compound (B).
[12] The light-curable, moisture-curable hot melt resin composition according to
[11] , wherein the monofunctional radically polymerizable compound contains a nitrogen-containing compound.
[13] The light-curable, moisture-curable hot melt resin composition according to
[12] , wherein the nitrogen-containing compound includes a chain-like nitrogen-containing compound.
[14] The light-curable, moisture-curable hot melt resin composition according to
[12] or
[13] , wherein the nitrogen-containing compound includes a cyclic nitrogen-containing compound.
[15] The light-moisture-curable hot melt resin composition according to
[14] , wherein a mass ratio (cyclic / chain) of the cyclic nitrogen-containing compound to the chain nitrogen-containing compound is 0.1 or more and 2.0 or less.
[16] The light-curable moisture-curable hot melt resin composition according to any one of
[12] to
[15] , wherein the content of the nitrogen-containing compound is 10 parts by mass or more and 95 parts by mass or less per 100 parts by mass of the radical polymerizable compound (B).
[17] The light-curable hot melt resin composition according to any one of
[12] to
[16] , wherein the monofunctional radically polymerizable compound contains a monofunctional (meth)acrylic acid ester compound in addition to the nitrogen-containing compound.
[18] The light-curable, moisture-curable hot melt resin composition according to any one of [1] to
[17] , wherein a mass ratio (A / B) of the urethane prepolymer (A) to the radically polymerizable compound (B) is 70 / 30 or more and 91 / 9 or less.
[19] The light-curable hot-melt resin composition according to any one of [1] to
[18] , wherein the polyisocyanate (Ab) is at least one selected from the group consisting of an isocyanurate-modified polyisocyanate and polymeric MDI.
[20] The light-and-moisture-curable hot-melt resin composition according to any one of [1] to
[19] , which has an initial adhesive strength of 0.5 MPa or more 3 minutes after compression bonding.
[21] The first polycarbonate substrate was heated to 25°C and coated with a line width of 1.0 mm at 1000 mJ / cm 2 The light-and-moisture-curable hot-melt resin composition according to any one of [1] to
[20] , having a pot life of 60 seconds or more from application to a first polycarbonate substrate until irradiation with ultraviolet rays, when the composition is irradiated with ultraviolet rays to cause a UV reaction, and a second polycarbonate substrate is pressure-bonded to the first polycarbonate substrate one minute after completion of the ultraviolet irradiation.
[22] An adhesive for electronic components, comprising the light-and-moisture-curable hot melt resin composition according to any one of [1] to
[21] .
[23] A cured product of the light-and-moisture-curable hot-melt resin composition according to any one of [1] to
[21] .
[24] An electronic component comprising the cured body according to
[23] . Effect of the Invention
[0009] According to the present invention, it is possible to provide a light-moisture-curable hot melt resin composition that can ensure a sufficient pot life for lamination operations while rapidly crystallizing and solidifying after lamination to exhibit adhesive strength, thereby achieving both ease of work during lamination and high productivity through short adhesion, as well as an adhesive for electronic components and a cured product using the same. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing a method for evaluating initial adhesive strength, in which FIG. 1(A) is a plan view and FIG. 1(B) is a side view. [Diagram 2] FIG. 2 is a schematic side view showing a method for evaluating impact resistance. [Diagram 3] FIG. 13 is a schematic perspective view of a shooting die used for impact resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the present invention will be described with reference to embodiments. <Urethane prepolymer (A)> The photo-curable hot melt resin composition of the present invention contains a hot melt type urethane prepolymer (A) (hereinafter referred to as urethane prepolymer (A)) that is solid at room temperature (25° C.). The urethane prepolymer (A) is preferably a reaction product of a polyol (Aa) and a polyisocyanate compound (Ab) and has an isocyanate group.
[0012] The urethane prepolymer (A) can impart moisture curing properties to the resin composition by having an isocyanate group. The isocyanate group in the urethane prepolymer (A) is not particularly limited, and may be an aromatic isocyanate group, an aliphatic isocyanate group, or a combination of these. When using these isocyanate groups in combination, the urethane prepolymer (A) may be a combination of a urethane prepolymer having an aromatic isocyanate group and a urethane prepolymer having an aliphatic isocyanate group, or the urethane prepolymer (A) may be a compound having both an aromatic isocyanate group and an aliphatic isocyanate group in one molecule. The aromatic isocyanate group is an isocyanate group directly bonded to an aromatic ring, and the aliphatic isocyanate group is an isocyanate group in which the isocyanate group is directly bonded to an aliphatic carbon atom. The aromatic isocyanate group is an isocyanate group derived from an aromatic isocyanate compound, and the details of the aromatic isocyanate compound are as described below. The aliphatic isocyanate group is an isocyanate group derived from an aliphatic isocyanate compound, and the details of the aliphatic isocyanate compound are as described below.
[0013] The urethane prepolymer (A) preferably contains an aromatic isocyanate group. When the urethane prepolymer contains an aromatic isocyanate group, the adhesive strength (final adhesive strength) of the photo- and moisture-curable hot melt resin composition after photo- and moisture-curing is easily improved. In addition, the adhesive strength of the cured product of the photo- and moisture-curable hot melt resin composition is easily maintained at a high value. The number of isocyanate groups in the urethane prepolymer (A) is not particularly limited, but it is preferable that one molecule contains two or more isocyanate groups, and it is preferable that the urethane prepolymer (A) contains isocyanate groups at both terminals.
[0014] The urethane prepolymer (A) of the present invention can be obtained by reacting a polyol (Aa) with a polyisocyanate compound (Ab). The polyol (Aa) is a compound having two or more hydroxyl groups, and the polyisocyanate compound (Ab) is a compound having two or more isocyanate groups. The reaction between the polyol compound (Aa) and the polyisocyanate compound (Ab) is carried out, for example, in a molar ratio of hydroxyl groups (OH) in the polyol to isocyanate groups (NCO) in the polyisocyanate compound, [NCO] / [OH], within the range of 1.5 to 2.5.
[0015] [Polyol (Aa)] In the present invention, the polyol (Aa) contains a polyether polycarbonate polyol (a1), and the hot melt type urethane prepolymer (A) is a reaction product of a material containing the polyether polycarbonate polyol (a1). In the present invention, by using the polyether polycarbonate polyol (a1), the pot life of the light moisture curable hot melt resin composition can be made appropriate, so that a sufficient pot life can be secured for the lamination work. In addition, the hot melt type urethane prepolymer (A) can be quickly crystallized and solidified after lamination, so that the initial adhesive strength can be easily secured. Furthermore, it is easy to make the impact resistance good. Also, the polyol (Aa) preferably contains, in addition to the polyether polycarbonate polyol (a1), a polyol (a2) different from the polyether polycarbonate polyol (a1). Here, the polyol (a2) is at least one selected from the group consisting of polyester polyols and polycarbonate polyols. In the present invention, by further using a specific polyol (a2) in addition to the polyol (a1) as the polyol (Aa) in the urethane prepolymer (A), it becomes easier to ensure sufficient pot life and to make the initial adhesive strength excellent. Furthermore, it becomes easier to make the impact resistance good. Each component will be described in detail below.
[0016] (Polyether polycarbonate polyol (a1)) The polyether polycarbonate polyol (a1) has a polyether skeleton and a carbonate bond. The polyether polycarbonate polyol (a1) is a compound having two or more hydroxyl groups in the molecule. In addition, the polyether polycarbonate polyol (a1) preferably has two or more carbonate bonds in the molecule.
[0017] In the polyether polycarbonate polyol (a1), the polyether skeleton typically has a structure in which divalent hydrocarbon groups are linked by ether bonds. The divalent hydrocarbon group is not particularly limited, but has, for example, 2 to 12 carbon atoms, preferably 3 to 8 carbon atoms. The divalent hydrocarbon group may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group having an aromatic ring, but is preferably an aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be linear, branched, or may have an alicyclic structure, but is preferably linear.
[0018] Moreover, the polyether polycarbonate polyol (a1) preferably has a linear alkylene group having 3 to 8 carbon atoms. By having the polyether polycarbonate polyol (a1) have a linear alkylene group having 3 to 8 carbon atoms, the pot life of the adhesive does not become too long, and the adhesive is quickly crystallized and solidified after bonding, making it easier to exhibit adhesive strength. The alkylene group is preferably contained in a polyether skeleton, and the divalent hydrocarbon group in the polyether skeleton is preferably a linear alkylene group having 3 to 8 carbon atoms. Therefore, the polyether skeleton preferably has a structure in which linear alkylene groups having 3 to 8 carbon atoms are linked via ether bonds, and the alkylene group more preferably has 3 to 5 carbon atoms, and most preferably has 4 carbon atoms.
[0019] The polyether polycarbonate polyol (a1) may have a structure in which a plurality of polyether skeletons are bonded via carbonate bonds. The polyether polycarbonate polyol (a1) is preferably a polyether polycarbonate diol having two hydroxyl groups in one molecule. The polyether polycarbonate diol may have hydroxyl groups at both ends of the molecule. Specifically, the polyether polycarbonate polyol (a1) is more preferably a compound represented by the following formula (1).
[0020] [ka] In the above formula (1), R represents a divalent hydrocarbon group having 2 to 12 carbon atoms, n is an integer from 2 to 90, and m is an integer from 1 to 35. In addition, in formula (1), multiple R may be the same or different.
[0021] In the above formula (1), R preferably has 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms, even more preferably 3 to 5 carbon atoms, and most preferably 4 carbon atoms. R may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group having an aromatic ring, but is preferably an aliphatic hydrocarbon group, more preferably an aliphatic saturated hydrocarbon group, and even more preferably a linear alkylene group having 3 to 8 carbon atoms. Therefore, specific preferred examples of R include a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, and an octamethylene group, and among these, a trimethylene group, a tetramethylene group, and a pentamethylene group are more preferred, and a tetramethylene group is the most preferred. These alkylene groups may be used alone or in combination of two or more kinds. In the above (1), n is 2 to 90, preferably 2 to 45, more preferably 2 to 15, even more preferably 2 to 10, and most preferably 2 to 5. Also, m is 1 to 35, preferably 1 to 15, more preferably 1 to 10, even more preferably 1 to 6, and most preferably 2 to 6.
[0022] The polyether polycarbonate polyol (a1) is preferably produced by known methods such as phosgene method and ester exchange method using polyoxyalkylene glycol as a raw material. Therefore, the above-mentioned polyether skeleton is preferably derived from polyoxyalkylene glycol. Preferable specific examples of polyoxyalkylene glycol include polypropylene glycol, polytetramethylene ether glycol, and copolymerized polyether glycol of propylene oxide and tetrahydrofuran, and among these, polytetramethylene ether glycol (PTMG) is more preferable. The polyoxyalkylene glycol may be used alone or in combination of two or more kinds.
[0023] It is preferable that the polyether polycarbonate polyol (a1) is liquid at room temperature (25° C.), while the polyol (a2) is solid at room temperature (25° C.). In the polyol (Aa), by making the polyether polycarbonate polyol (a1) liquid at room temperature (25° C.) and the polyol (a2) solid at room temperature (25° C.), the resin composition becomes a hot melt, the pot life is appropriately extended, and it is easy to improve the impact resistance.
[0024] The number average molecular weight (Mn) of the polyether polycarbonate polyol (a1) is not particularly limited, but is, for example, 600 or more, preferably 800 or more, more preferably 1,000 or more, and even more preferably 1,500 or more, and is, for example, 6,000 or less, preferably 5,000 or less, more preferably 4,000 or less, and even more preferably 3,500 or less. When the number average molecular weight of the polyether polycarbonate polyol (a1) is within the above range, it is easy to develop adhesive strength by crystallizing and solidifying quickly after bonding while ensuring a sufficient pot life.
[0025] (Polyol (a2)) The polyol (a2) used as the polyol (Aa) is at least one of polyester polyol and polycarbonate polyol as described above, and these may be used in combination. Among these, polyester polyol is more preferred from the viewpoints of initial adhesive strength and impact resistance.
[0026] <<Polyester polyol>> Examples of polyester polyols used as polyol (a2) include polyester polyols obtained by reacting polycarboxylic acid with polyol, and poly-ε-caprolactone polyols obtained by ring-opening polymerization of ε-caprolactone. Among these, polyester polyols obtained by reacting polycarboxylic acid with polyol are preferred. The polyester polyol is preferably a polyester diol. The polyester polyols may be used alone or in combination of two or more kinds.
[0027] Examples of polycarboxylic acids that are raw materials for polyester polyols include divalent aromatic carboxylic acids such as terephthalic acid, isophthalic acid, 1,5-naphthalic acid, and 2,6-naphthalic acid, divalent aliphatic carboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decamethylene dicarboxylic acid, and dodecamethylene dicarboxylic acid, trivalent or higher aromatic carboxylic acids such as trimellitic acid, trimesic acid, pyromellitic acid, and naphthalene tricarboxylic acid, and trivalent or higher aliphatic carboxylic acids such as cyclohexane tricarboxylic acid and hexane tricarboxylic acid. These polycarboxylic acids may be used alone or in combination of two or more.
[0028] Examples of polyols that can be used as raw materials for polyester polyols include linear aliphatic polyols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and diethylene glycol, aliphatic polyols having a branched structure such as neopentyl glycol, and aliphatic polyols having a cyclic skeleton such as cyclohexanediol, etc. These polyols may be used alone or in combination of two or more.
[0029] Among the above, the polycarboxylic acid used in the polyester polyol is preferably a linear polycarboxylic acid. By using a linear polycarboxylic acid, the crystallinity is easily increased and the set time is easily shortened. Therefore, the initial adhesive strength is increased and the impact resistance is easily improved. In the polyester polyol, the linear polycarboxylic acid may be used alone as the polycarboxylic acid, or may be used in combination with a polycarboxylic acid other than the linear polycarboxylic acid.
[0030] The polyester polyol preferably contains a structural unit derived from a linear polycarboxylic acid, and the content thereof is, for example, 75 mol % or more and 100 mol % or less, preferably 85 mol % or more and 100 mol % or less, more preferably 95 mol % or more and 100 mol % or less, and most preferably 100 mol %, based on the total amount of structural units derived from all polycarboxylic acids.
[0031] The linear polycarboxylic acid is a divalent linear aliphatic carboxylic acid having carboxyl groups at both ends. Of the linear polycarboxylic acids, aliphatic carboxylic acids having 4 to 12 carbon atoms are preferred, and aliphatic carboxylic acids having 6 to 10 carbon atoms are more preferred. Of the above, the aliphatic carboxylic acids are therefore preferred, including adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, with adipic acid or sebacic acid being particularly preferred, and sebacic acid being particularly preferred from the viewpoints of initial adhesive strength and impact resistance.
[0032] The polyester polyol preferably contains a structural unit derived from a polycarboxylic acid selected from the group consisting of adipic acid and sebacic acid, and the content thereof is, for example, 75 mol % or more and 100 mol % or less, preferably 85 mol % or more and 100 mol % or less, more preferably 95 mol % or more and 100 mol % or less, and most preferably 100 mol %, based on the total amount of structural units derived from polycarboxylic acid. The linear polycarboxylic acids may be used alone or in combination of two or more kinds.
[0033] Among the above polyols, linear polyols are preferred as the polyols used in the polyester polyols. By using linear polyols, the crystallinity is easily increased and the set time is easily shortened. Therefore, the initial adhesive strength is increased and the impact resistance is easily improved. In the polyester polyol, the linear polyol may be used alone as the polyol, but may also be used in combination with a polyol other than the linear polyol.
[0034] The polyester polyol preferably contains a structural unit derived from a linear polyol, and the content thereof is, for example, 75 mol % or more and 100 mol % or less, preferably 85 mol % or more and 100 mol % or less, more preferably 95 mol % or more and 100 mol % or less, and most preferably 100 mol %, based on the total amount of the structural units derived from the polyol. In addition, from the viewpoint of increasing crystallinity, the polyester polyol preferably contains a constitutional unit derived from a linear polyol and a constitutional unit derived from a linear polycarboxylic acid, i.e., it is preferable that a linear polyol is used as the polyol and a linear polycarboxylic acid is used as the polycarboxylic acid.
[0035] The linear polyol is a divalent linear aliphatic polyol having hydroxyl groups at both ends. Among the linear polyols, a linear polyol having 3 to 12 carbon atoms is preferable, a linear polyol having 5 to 8 carbon atoms is more preferable, and a linear polyol having 6 carbon atoms is most preferable. Specific examples of preferred straight-chain polyols include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and diethylene glycol, and among these, 1,6-hexanediol is most preferred. Therefore, it is preferable that the polyester polyol contains a structural unit derived from 1,6-hexanediol, and the content thereof is, for example, 75 mol % or more and 100 mol % or less, preferably 85 mol % or more and 100 mol % or less, more preferably 95 mol % or more and 100 mol % or less, and most preferably 100 mol %, based on the total amount of structural units derived from the polyol. The linear polyols may be used alone or in combination of two or more kinds.
[0036] <<Polycarbonate polyol>> The polycarbonate polyol used in the polyol (a2) has a structure in which structural units derived from a polyhydroxy compound are linked by carbonate bonds. The method for producing the polycarbonate polyol is not particularly limited, and it may be produced by a known method such as the phosgene method or the ester exchange method using a polyhydroxy compound as a raw material.
[0037] The polyhydroxy compound is generally a dihydroxy compound. The polyhydroxy compound may be any of a linear aliphatic polyol, an alicyclic polyol having a branched structure or an alicyclic structure, and an aromatic polyhydroxy compound, but the polyhydroxy compound is preferably a linear polyol. The linear polyol is a divalent linear aliphatic polyol having hydroxyl groups at both ends. The linear polyol has, for example, 4 or more carbon atoms, and among them, a linear polyol having 8 or more carbon atoms is preferred. The number of carbon atoms of the linear polyol is, for example, 16 or less, and preferably 12 or less.
[0038] Examples of linear polyols that are used as raw materials for polycarbonate polyols include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, and 1,16-hexadecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol are preferred, and among these, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are more preferred, and in particular, 1,10-decanediol and 1,12-dodecanediol are most preferred.
[0039] Therefore, the polycarbonate polyol preferably contains a structural unit derived from a linear polyol, and more preferably contains a structural unit derived from a linear polyol having 8 or more carbon atoms. When the polycarbonate polyol contains a structural unit derived from a linear polyol having a relatively large number of carbon atoms, the crystallinity is increased, and the setting time of the composition tends to be appropriately fast. Therefore, the initial adhesive strength is increased, and the impact resistance is also easily improved. The constituent units derived from a linear polyol having 8 or more carbon atoms are, for example, 75 mol % or more and 100 mol % or less, preferably 85 mol % or more and 100 mol % or less, more preferably 95 mol % or more and 100 mol % or less, and most preferably 100 mol %, based on the total amount of constituent units derived from a polyhydroxy compound. The linear polyols may be used alone or in combination of two or more kinds.
[0040] The polycarbonate polyol is preferably a polycarbonate diol, and a specific example of the polycarbonate diol is a compound represented by the following formula (2).
[0041] [ka] In formula (2), R is a divalent hydrocarbon group having 4 to 16 carbon atoms, and n is an integer from 2 to 120.
[0042] In formula (2), R is preferably an aliphatic saturated hydrocarbon group. When R is an aliphatic saturated hydrocarbon group, heat resistance and flexibility tend to be good. R consisting of an aliphatic saturated hydrocarbon group may have a chain structure or a cyclic structure, but preferably has a chain structure. In addition, R of the chain structure may be either linear or branched, but is preferably linear. n is preferably 2-25, more preferably 2-20, further preferably 5-20, and most preferably 5-15. In the urethane prepolymer (A), the R contained in the polycarbonate polyol may be used alone or in combination of two or more. R is preferably a linear aliphatic saturated hydrocarbon group having 8 or more carbon atoms. By using a linear aliphatic saturated hydrocarbon group having 8 or more carbon atoms as R, crystallinity is increased and the setting time tends to be appropriately fast. Therefore, the initial adhesive strength is likely to be high and impact resistance is likely to be improved.
[0043] In the polycarbonate polyol, all of the R's may be linear aliphatic saturated hydrocarbon groups having 8 or more carbon atoms, or some of them may be linear aliphatic saturated hydrocarbon groups having 8 or more carbon atoms. In the polycarbonate polyol, R's may be linear aliphatic saturated hydrocarbon groups having 8 or more carbon atoms at a ratio of, for example, 75 mol% to 100 mol%, preferably 85 mol% to 100 mol%, more preferably 95 mol% to 100 mol%, and most preferably 100 mol% based on the total R's. The linear aliphatic saturated hydrocarbon groups having 8 or more carbon atoms preferably have 12 or less carbon atoms.
[0044] Preferred specific examples of R include a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, and a dodecamethylene group. Among these, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, and a dodecamethylene group are preferred, an octamethylene group, a decamethylene group, and a dodecamethylene group are more preferred, a decamethylene group and a dodecamethylene group are even more preferred, and a decamethylene group is even more preferred. The polycarbonate polyols may be used alone or in combination of two or more kinds.
[0045] As described above, the polyol (a2) is preferably solid at room temperature (25° C.). When the polyol (a2) is solid at room temperature, the resin composition can be easily made into a hot melt. The number average molecular weight (Mn) of the polyol (a2) is not particularly limited, but is, for example, 1,000 or more, preferably 1,500 or more, more preferably 2,000 or more, and is, for example, 6,000 or less, preferably 5,000 or less, more preferably 4,000 or less. The number average molecular weight of the polyol (a2) within the above range allows it to have moderate crystallinity. Therefore, it has moderate pot life and set time, has high initial adhesive strength, and is easy to improve impact resistance.
[0046] The number average molecular weight (Mn) of the polyether polycarbonate polyol (a1) and the polyol (a2) can be calculated from the measured hydroxyl value (mgKOH / g) by the following procedure. Specifically, first, the hydroxyl value (mgKOH / g) of the polyol is measured according to JIS K 1557-1. Next, the hydroxyl amount (mmol / g) is calculated from the measured hydroxyl value (mgKOH / g) and the formula weight of KOH. The obtained hydroxyl amount (mmol / g) is then reciprocally converted to "g / mol", and multiplied by the number of functional groups (number of hydroxyl groups) to calculate the number average molecular weight (Mn).
[0047] The urethane prepolymer (A) can be obtained by reacting a mixture of the polyether polycarbonate polyol (a1) and the polyol (a2) with the polyisocyanate (Ab). Thus, at least a part or all of the urethane prepolymer (A) has both structural units derived from the polyether polycarbonate polyol (a1) and structural units derived from the polyol (a2) in one molecule.
[0048] In the polyol (Aa), it is preferable that the polyether polycarbonate polyol (a1) is contained in an amount of 35% by mass to 75% by mass, and the polyol (a2) is contained in an amount of 25% by mass to 65% by mass. When the contents of the polyether polycarbonate polyol (a1) and the polyol (a2) are within the above ranges, the polyether polycarbonate polyol (a1) makes it easier to improve impact resistance while extending the pot life, and the polyol (a2) makes it easier to increase the initial adhesive strength and improve impact resistance. From the above viewpoints, the content of the polyether polycarbonate polyol (a1) in the polyol (Aa) is more preferably 40% by mass or more, even more preferably 50% by mass or more, and more preferably 70% by mass or less, even more preferably 65% by mass or less. The content of polyol (a2) in polyol (Aa) is more preferably 30% by mass or more, further preferably 35% by mass or more, and is more preferably 60% by mass or less, further preferably 50% by mass or less.
[0049] The polyol (Aa) may contain a polyol (other polyol) other than the polyether polycarbonate polyol (a1) and the polyol (a2) as long as the effects of the present invention are not impaired. The content of the other polyol in the polyol (Aa) is, for example, 0% by mass or more and 20% by mass or less, preferably 0% by mass or more and 10% by mass or less, more preferably 0% by mass or more and 5% by mass or less, and most preferably 0% by mass.
[0050] (Polyisocyanate (Ab)) Examples of the polyisocyanate include aromatic polyisocyanates and aliphatic polyisocyanates, such as diphenylmethane diisocyanate, liquid modified diphenylmethane diisocyanate, tolylene diisocyanate, and naphthalene-1,5-diisocyanate. Examples of the aliphatic polyisocyanate include hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, norbornane diisocyanate, transcyclohexane-1,4-diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, cyclohexane diisocyanate, bis(isocyanatemethyl)cyclohexane, and dicyclohexylmethane diisocyanate. The polyisocyanates may be used alone or in combination of two or more kinds. In the present invention, when an aromatic polyisocyanate is used in the synthesis of the urethane prepolymer (A), the urethane prepolymer (A) contains an aromatic isocyanate group, and when an aliphatic polyisocyanate is used, the urethane prepolymer (A) contains an aliphatic isocyanate group. The isocyanate compound may be a polymerized isocyanate or may be polymeric MDI. In addition, the isocyanate compound may be a chain-extended polyisocyanate compound (polyol modified product) obtained by reacting a polyol with an excess of an isocyanate compound, or an isocyanurate modified product of a polyisocyanate. Examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, and polycaprolactone diol. In the present invention, the polyisocyanate (Ab) is preferably at least one selected from the group consisting of isocyanurate-modified polyisocyanates and polymeric MDI, and more preferably polymeric MDI.
[0051] The content of the urethane prepolymer (A) in the photo-curable hot melt resin composition is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more, based on the total amount of the photo-curable hot melt resin composition. By making the content of the urethane prepolymer equal to or more than the above lower limit, it becomes easier to impart impact resistance to the photo-curable hot melt resin composition. In addition, the resin composition can be appropriately moisture-cured by the urethane prepolymer. The content of the urethane prepolymer is, for example, 90% by mass or less, preferably 88% by mass or less, more preferably 82% by mass or less, and even more preferably 80% by mass or less, in order to appropriately contain the radical polymerizable compound (B), the photopolymerization initiator (C), and other components.
[0052] <Radical polymerizable compound (B)> The photo-curable hot melt resin composition of the present invention contains a radical polymerizable compound (B). The photo-curable hot melt resin composition contains the radical polymerizable compound (B) to be photocurable, and is cured by irradiation with active energy rays such as ultraviolet rays. The photo-curable hot melt resin composition has a certain adhesive strength, which can be imparted by simply irradiating light, and therefore a certain initial adhesive strength can be ensured. In addition, before photocuring, the compound acts as a plasticizer to suppress the crystallinity of the photo-curable hot melt resin composition, thereby extending the usable time. Furthermore, the temperature during application by heating can be lowered to improve workability. The radical polymerizable compound (B) may have a radical polymerizable functional group in the molecule. The radical polymerizable functional group is preferably a compound having an unsaturated double bond, such as a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group.
[0053] Among the above, from the viewpoint of adhesiveness, the (meth)acryloyl group is preferred, that is, the radical polymerizable compound (B) preferably contains a compound having a (meth)acryloyl group. In addition, a compound having a (meth)acryloyl group is also referred to as a "(meth)acrylic compound" below. In addition, in this specification, "(meth)acryloyl group" means an acryloyl group or a (meth)acryloyl group, "(meth)acrylic" means acrylic or methacrylic, and the same applies to other similar terms.
[0054] The radical polymerizable compound (B) may contain one or both of a monofunctional radical polymerizable compound having one radical polymerizable functional group in one molecule and a polyfunctional radical polymerizable compound having two or more radical polymerizable functional groups in one molecule, but from the viewpoint of improving the initial adhesive strength of the light moisture curable hot melt resin composition, it is preferable to contain a monofunctional radical polymerizable compound. In addition, it is more preferable that the radical polymerizable compound (B) contains at least a monofunctional (meth)acrylic compound that is a (meth)acrylic compound as the monofunctional radical polymerizable compound. In addition, the monofunctional radical polymerizable compound may be a prepolymer that is polymerized and has a repeating unit, but it is usually preferable to use a monofunctional monomer that does not have a repeating unit.
[0055] In the photo-curable hot melt resin composition, the monofunctional radically polymerizable compound may be, for example, 50 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the radically polymerizable compound (B). In addition, the photo-curable hot melt resin composition preferably contains a large amount of monofunctional radical polymerizable compound in order to improve the initial adhesive strength of the photo-curable hot melt resin composition. Specifically, the photo-curable hot melt resin composition preferably contains 90 parts by mass or more of the monofunctional radical polymerizable compound, more preferably 95 parts by mass or more, and even more preferably 100 parts by mass, per 100 parts by mass of the radical polymerizable compound (B).
[0056] [Monofunctional radical polymerizable compounds] (nitrogen-containing compounds) The radical polymerizable compound (B) preferably contains a nitrogen-containing compound as a monofunctional radical polymerizable compound. By using a nitrogen-containing compound, the initial adhesive strength of the photo-curable hot melt resin composition is improved. After being applied to an adherend, the photo-curable hot melt resin composition is photocured by irradiating it with active energy rays such as ultraviolet rays, and in this case, it is generally photocured in the presence of oxygen as described below. When the radical polymerizable compound (B) contains a nitrogen-containing compound, it is presumed that the composition is appropriately photocured even in the presence of oxygen, thereby improving the initial adhesive strength.
[0057] The nitrogen-containing compound may be a nitrogen-containing compound having a cyclic structure or a chain-like nitrogen-containing compound. Examples of the nitrogen-containing compound having a cyclic structure include nitrogen-containing compounds having a lactam structure such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam, compounds containing a morpholine skeleton such as N-acryloylmorpholine, and cyclic imide compounds such as N-(meth)acryloyloxyethylhexahydrophthalimide. Among these, amide group-containing compounds such as N-vinylcaprolactam are more preferred. In this specification, the nitrogen-containing compound having a cyclic structure is also called a cyclic nitrogen-containing compound, and a radical polymerizable compound in which a nitrogen atom is included in an atom constituting the ring itself is referred to as a cyclic nitrogen-containing compound, and other nitrogen-containing compounds are referred to as chain-like nitrogen-containing compounds.
[0058] Examples of chain nitrogen-containing compounds include chain amino group-containing (meth)acrylates such as dimethylamino(meth)acrylate, diethylamino(meth)acrylate, aminomethyl(meth)acrylate, aminoethyl(meth)acrylate, and dimethylaminoethyl(meth)acrylate; chain (meth)acrylamide compounds such as diacetoneacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, N-hydroxyethylacrylamide, acrylamide, and methacrylamide; and N-vinylacetamide.
[0059] The chain-like nitrogen-containing compound may be a monofunctional urethane (meth)acrylate. By using a monofunctional urethane (meth)acrylate, the compatibility with the urethane prepolymer (A) is improved, and the initial adhesive strength is easily improved. In addition, urethane (meth)acrylate has a relatively high polarity, which makes it easier to increase the adhesive strength to glass.
[0060] As the monofunctional urethane (meth)acrylate, for example, one obtained by reacting an isocyanate compound with a (meth)acrylic acid derivative having a hydroxyl group can be used. Examples of the (meth)acrylic acid derivative having a hydroxyl group include mono(meth)acrylates of dihydric alcohols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol, and mono(meth)acrylates of trihydric alcohols such as trimethylolethane, trimethylolpropane, and glycerin.
[0061] Examples of the isocyanate compound used to obtain the urethane (meth)acrylate include alkane monoisocyanates such as butane isocyanate, hexane isocyanate, and decane isocyanate, and aliphatic monoisocyanates such as cyclic aliphatic monoisocyanates such as cyclopentane isocyanate, cyclohexane isocyanate, and isophorone monoisocyanate. More specifically, the monofunctional urethane (meth)acrylate is preferably a urethane (meth)acrylate obtained by reacting the above-mentioned monoisocyanate compound with a mono(meth)acrylate of a dihydric alcohol, and a suitable specific example thereof is 1,2-ethanediol 1-acrylate 2-(N-butylcarbamate). Of the above, the chain nitrogen-containing compound preferably contains a monofunctional urethane (meth)acrylate, and it is also preferable to use a monofunctional urethane (meth)acrylate in combination with a compound other than the monofunctional urethane (meth)acrylate, such as a (meth)acrylamide compound.
[0062] The nitrogen-containing compound may contain one or both of a chain-like nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure, but from the viewpoint of improving the initial adhesive strength of the light-moisture-curable hot melt resin composition, it is preferable to contain a nitrogen-containing compound having a cyclic structure, and it is more preferable to use a chain-like nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure in combination. Among them, it is more preferable to use a nitrogen-containing compound having a lactam structure as the cyclic nitrogen-containing compound, and at least one selected from a monofunctional urethane (meth)acrylate and a (meth)acrylamide compound as the chain-like nitrogen-containing compound in combination.
[0063] In the photo-curable hot melt resin composition, the content of the nitrogen-containing compound as a monofunctional radical polymerizable compound relative to 100 parts by mass of the radical polymerizable compound (B) is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 50 parts by mass or more, even more preferably 60 parts by mass or more, and most preferably 75 parts by mass or more, from the viewpoint of improving the initial adhesive strength of the photo-curable hot melt resin composition. In addition, the content of the nitrogen-containing compound as the monofunctional radical polymerizable compound is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less, in order to contain an appropriate amount of the radical polymerizable compound (B) other than the nitrogen-containing compound.
[0064] When the monofunctional radical polymerizable compound has a chain-like nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure, the mass ratio of the nitrogen-containing compound having a cyclic structure to the chain-like nitrogen-containing compound in the monofunctional radical polymerizable compound (cyclic / chain) is preferably 0.1 to 2.0, more preferably 0.2 to 1.5, and even more preferably 0.4 to 1.2. By setting the cyclic / chain mass ratio within the above range, the initial adhesive strength of the light-curable hot melt resin composition can be improved.
[0065] (Monofunctional radical polymerizable compounds other than nitrogen-containing compounds) The monofunctional radically polymerizable compound contained in the radically polymerizable compound (B) preferably contains a compound other than the above-mentioned nitrogen-containing compounds (hereinafter also referred to as a nitrogen-free compound). When the radically polymerizable compound (B) contains a nitrogen-free compound as a monofunctional radically polymerizable compound, adhesive strength and the like can be easily improved.
[0066] The nitrogen-free compound is not particularly limited as long as it is a compound having a radically polymerizable functional group, but is preferably a monofunctional (meth)acrylic compound, and more preferably a (meth)acrylic acid ester compound. Examples of monofunctional (meth)acrylic acid ester compounds include alkyl (meth)acrylates, alicyclic structure-containing (meth)acrylates, aromatic ring-containing (meth)acrylates, etc. These may be used alone or in combination of two or more, but among these, it is preferable to use one or both of alkyl (meth)acrylates and aromatic ring-containing (meth)acrylates. The total content of the alkyl (meth)acrylate, alicyclic structure-containing (meth)acrylate, and aromatic ring-containing (meth)acrylate in the radical polymerizable compound (B) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the radical polymerizable compound (B). The content is preferably 90 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 60 parts by mass or less, even more preferably 40 parts by mass or less, and most preferably 25 parts by mass or less.
[0067] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl group with a carbon number of 1 to 18, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, and stearyl (meth)acrylate. Examples of the (meth)acrylate containing an alicyclic structure include (meth)acrylates having an alicyclic structure such as cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, etc. The alicyclic structure is a ring structure in which the ring constituent elements are carbon atoms. Examples of aromatic ring-containing (meth)acrylates include phenylalkyl (meth)acrylates such as benzyl (meth)acrylate and 2-phenylethyl (meth)acrylate, and phenoxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate.
[0068] As the monofunctional (meth)acrylic acid ester compound, compounds other than alkyl (meth)acrylates, alicyclic structure-containing (meth)acrylates, and aromatic ring-containing (meth)acrylates can also be used, for example, cyclic ether group-containing (meth)acrylates can also be used. Examples of the cyclic ether group-containing (meth)acrylate include (meth)acrylates having an epoxy ring, an oxetane ring, a tetrahydrofuran ring, a dioxolane ring, a dioxane ring, and the like. Examples of epoxy ring-containing (meth)acrylates include glycidyl (meth)acrylate. Examples of oxetane ring-containing (meth)acrylates include (3-ethyloxetane-3-yl)methyl (meth)acrylate. Examples of tetrahydrofuran ring-containing (meth)acrylates include tetrahydrofurfuryl (meth)acrylate, and (meth)acrylic acid polymeric esters of tetrahydrofurfuryl alcohol. Examples of the dioxolane ring-containing (meth)acrylate include (2-methyl-2-ethyl-1,3-dioxolane-4-yl)methyl (meth)acrylate, (2,2-cyclohexyl-1,3-dioxolane-4-yl)methyl (meth)acrylate, etc. Examples of the (meth)acrylate having a dioxane ring include cyclic trimethylolpropane formal (meth)acrylate, etc. As the cyclic ether group-containing (meth)acrylate, it is preferable to use either an oxetane ring-containing (meth)acrylate or a tetrahydrofuran ring-containing (meth)acrylate, but it is also preferable to use them in combination.
[0069] In addition, examples of the monofunctional (meth)acrylic acid ester compound include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; 2-methoxyethyl (meth)acrylate; 2-ethoxyethyl (meth)acrylate; Alkoxyalkyl (meth)acrylates such as 2-butoxyethyl (meth)acrylate, alkoxyethylene glycol (meth)acrylates such as methoxyethylene glycol (meth)acrylate, ethoxyethylene glycol (meth)acrylate, and other alkoxyethylene glycol (meth)acrylates, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethyl carbitol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, ethoxytriethylene glycol (meth)acrylate, and ethoxypolyethylene glycol (meth)acrylate may also be used. Furthermore, as the monofunctional (meth)acrylic compound, a carboxyl-containing (meth)acrylic compound such as acrylic acid or methacrylic acid may be used.
[0070] [Compounds other than monofunctional radical polymerizable compounds] The radical polymerizable compound (B) may contain a polyfunctional radical polymerizable compound as long as the effects of the present invention are achieved. Examples of the polyfunctional radical polymerizable compound include bifunctional (meth)acrylic acid ester compounds, trifunctional or higher (meth)acrylic acid ester compounds, and bifunctional or higher urethane (meth)acrylates.
[0071] Examples of the bifunctional (meth)acrylic acid ester compound include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, poly Examples of the di(meth)acrylate include propylene glycol di(meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, dimethylol dicyclopentadienyl di(meth)acrylate, neopentyl glycol di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, and polybutadiene diol di(meth)acrylate.
[0072] Examples of the trifunctional or higher (meth)acrylic acid ester compound include trimethylolpropane tri(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerin tri(meth)acrylate, propylene oxide-added glycerin tri(meth)acrylate, tris(meth)acryloyloxyethyl phosphate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0073] The di- or higher functional urethane (meth)acrylate may be, for example, one obtained by reacting an isocyanate compound with a (meth)acrylic acid derivative having a hydroxyl group. Examples of the (meth)acrylic acid derivative having a hydroxyl group include mono(meth)acrylates of dihydric alcohols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, and polyethylene glycol; mono(meth)acrylates or di(meth)acrylates of trihydric alcohols such as trimethylolethane, trimethylolpropane, and glycerin; and epoxy(meth)acrylates such as bisphenol A-type epoxy(meth)acrylate.
[0074] Examples of the isocyanate compound used to obtain the urethane (meth)acrylate include polyisocyanate compounds such as isophorone diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatephenyl)thiophosphate, tetramethylxylylene diisocyanate, and 1,6,11-undecane triisocyanate.
[0075] Also, as the isocyanate compound, a chain-extended polyisocyanate compound (polyol modified product) obtained by reacting a polyol with an excess of an isocyanate compound, an isocyanurate modified product of a polyisocyanate, etc. can be used. Here, examples of the polyol include ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, polycaprolactone diol, etc. By using these polyisocyanate compounds, polyfunctional urethane (meth)acrylates can be obtained.
[0076] The content of the radical polymerizable compound (B) in the photo-moisture curable hot melt resin composition is, for example, 7.5% by mass or more, preferably 8% by mass or more, more preferably 12% by mass or more, and even more preferably 15% by mass or more, based on the total amount of the photo-moisture curable hot melt resin composition. By making the content of the radical polymerizable compound (B) equal to or more than the above lower limit, it becomes easier to extend the usable time of the photo-moisture curable hot melt resin composition and ensure a certain level of initial adhesive strength. In addition, the content of the radical polymerizable compound (B) is preferably 30% by mass or less, more preferably 27% by mass or less, and even more preferably 25% by mass or less, from the viewpoint of making the photo-curability of the photo-moisture curable hot melt resin composition appropriate and imparting good pressure-bonding properties.
[0077] In the photo-curable hot melt resin composition of the present invention, the mass ratio (A / B) of the urethane prepolymer (A) to the radical polymerizable compound (B) is preferably 70 / 30 or more and 91 / 9 or less, more preferably 72 / 28 or more and 90 / 10 or less, and even more preferably 74 / 26 or more and 85 / 15 or less. When A / B is equal to or more than the lower limit, the composition can contain a certain amount of the urethane prepolymer (A) and can easily impart good crystallinity to the composition. In addition, the radical polymerizable compound (B) is not excessively contained, and can easily impart good pressure adhesion to the composition. On the other hand, when A / B is equal to or less than the upper limit, the composition can contain a certain amount of the radical polymerizable compound (B) and can extend the pot life of the composition or impart appropriate photocurability.
[0078] <Photopolymerization initiator (C)> The light- and moisture-curable hot-melt resin composition of the present invention contains a photopolymerization initiator (C). By containing the photopolymerization initiator (C), the light- and moisture-curable hot-melt resin composition is appropriately imparted with photocurability. Examples of the photopolymerization initiator (C) include benzophenone-based compounds, acetophenone-based compounds, alkylphenone-based photopolymerization initiators, acylphosphine oxide-based compounds, titanocene-based compounds, oxime ester-based compounds, benzoin ether-based compounds, and thioxanthone. Examples of commercially available photopolymerization initiators (C) include IRGACURE184, IRGACURE369, IRGACURE379, IRGACURE379EG, IRGACURE651, IRGACURE784, IRGACURE819, IRGACURE907, IRGACURE2959, IRGACURE OXE01, IRGACURE TPO (all manufactured by BASF), benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether (all manufactured by Tokyo Chemical Industry Co., Ltd.), Omnirad TPO (manufactured by IGM Resins BV), and the like.
[0079] The content of the photopolymerization initiator (C) in the photo-curable hot melt resin composition is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 5% by mass or less, and even more preferably 0.6% by mass or more and 3% by mass or less, based on the total amount of the photo-curable hot melt resin composition. By making the content of the photopolymerization initiator within these ranges, the obtained photo-curable hot melt resin composition has excellent photocurability and storage stability. In addition, by making it within the above range, the photo-curable hot melt resin composition is appropriately cured, and the adhesive strength is easily improved.
[0080] <Filling agent> The photo-curable hot melt resin composition of the present invention may contain a filler (E). By containing a filler, the photo-curable hot melt resin composition of the present invention has a suitable thixotropy and can sufficiently retain its shape after application. As the filler, a particulate filler may be used. The filler is not particularly limited, but inorganic fillers are preferred, such as silica, talc, titanium oxide, zinc oxide, calcium carbonate, etc. Among them, silica is preferred because the resulting light-and-moisture-curable hot melt resin composition has excellent ultraviolet transmittance. The filler may be subjected to hydrophobic surface treatment such as silylation treatment, alkylation treatment, or epoxidation treatment. The fillers may be used alone or in combination of two or more. The content of the filler is not particularly limited, but is preferably from 1 to 25% by mass, more preferably from 2 to 20% by mass, based on the total amount of the light-and-moisture-curable hot-melt resin composition.
[0081] <Moisture curing catalyst> The photo-curable hot melt resin composition may contain a moisture curing catalyst that accelerates the moisture curing reaction of the urethane prepolymer. By using the moisture curing catalyst, the moisture curable hot melt resin composition has better moisture curing properties and is more likely to have high adhesive strength. Specific examples of the moisture curing catalyst include amine compounds and metal catalysts, and amine compounds are preferred. Examples of the amine compounds include compounds having a morpholine skeleton such as di(methylmorpholino)diethyl ether, 4-morpholinopropylmorpholine, and bis(2-morpholinoethyl)ether, dimethylamino group-containing amine compounds having two dimethylamino groups such as bis(2-dimethylaminoethyl)ether and 1,2-bis(dimethylamino)ethane, triethylamine, 1,4-diazabicyclo[2.2.2]octane, and 2,6,7-trimethyl-1,4-diazabicyclo[2.2.2]octane. Examples of the metal catalyst include tin compounds such as di-n-butyltin dilaurate, di-n-butyltin diacetate, and tin octoate; zinc compounds such as zinc octoate and zinc naphthenate; and other metal compounds such as zirconium tetraacetylacetonate, copper naphthenate, and cobalt naphthenate. The content of the moisture curing accelerator catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the urethane prepolymer (A).
[0082] <Coupling Agent> The photo-curable hot melt resin composition may contain a coupling agent. By including a coupling agent in the photo-curable hot melt resin composition, the adhesive strength can be easily improved. Examples of the coupling agent include a silane coupling agent, a titanate coupling agent, and a zirconate coupling agent. Among coupling agents, silane coupling agents are preferred because they have excellent effect of improving adhesion.Furthermore, among silane coupling agents, mercaptan-based silane coupling agents and amine-based silane coupling agents are preferred because they have excellent effect of improving impact resistance, amine-based silane coupling agents are more preferred, amine-containing silane coupling agents having aromatic rings in molecules are even more preferred, and aromatic amine-containing silane coupling agents having aromatic amines are particularly preferred.
[0083] Examples of the amine-based silane coupling agent include N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, etc. Among these, N-phenyl-3-aminopropyltrimethoxysilane is preferred. Examples of the mercaptan-based silane coupling agent include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropylmethyldiethoxysilane.
[0084] As the silane coupling agent, silane coupling agents other than the mercaptan-based silane coupling agent and the amine-based silane coupling agent may be used. Other silane coupling agents include, for example, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane, 3-(meth)acryloyloxypropylmethyldimethoxysilane, 3-(meth)acryloyloxypropylmethyldiethoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane. , 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropylmethyldimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, tedyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, and the like.
[0085] Examples of the titanate coupling agent include titanium diisopropoxybis(acetylacetonate), titanium tetraacetylacetonate, and titanium diisopropoxybis(ethylacetoacetate). Examples of the zirconate coupling agent include zirconium tetra-normal-propoxide and zirconium tetra-normal-butoxide. The coupling agent may be used alone or in combination of two or more kinds.
[0086] The content of the coupling agent is preferably 0.05 parts by mass or more and 8 parts by mass or less, more preferably 0.2 parts by mass or more and 6 parts by mass or less, and even more preferably 0.5 parts by mass or more and 4 parts by mass or less, relative to 100 parts by mass of the urethane prepolymer (A). By setting the content of the coupling agent within these ranges, it becomes easier to improve the adhesive strength without affecting various performances of the cured product.
[0087] <Coloring agent> The photo-curable hot melt resin composition of the present invention may contain a colorant. Examples of the colorant include iron oxide, titanium black, aniline black, cyanine black, fullerene, carbon black, and resin-coated carbon black. The photo-curable hot melt resin composition contains a colorant, which improves the light-shielding properties. Among these, titanium black is preferred. Titanium black has the property of sufficiently blocking light with wavelengths in the visible light region while transmitting light with wavelengths near the ultraviolet region, so that the photo-curing properties of the photo-curable hot melt resin composition can be prevented from decreasing. The content of the colorant in the photo- and moisture-curable hot melt resin composition is not particularly limited, but is preferably 0.05% by mass or more and 8% by mass or less, more preferably 0.1% by mass or more and 2% by mass or less, based on the total amount of the photo- and moisture-curable hot melt resin composition. By keeping the content of the colorant within these ranges, the photo- and moisture-curable hot melt resin composition can be provided with appropriate light-shielding properties while maintaining good adhesiveness.
[0088] <Other ingredients> The light-and-moisture-curable hot melt resin composition of the present invention may contain, in addition to the above-mentioned urethane prepolymer (A) and radically polymerizable compound (B), a curable resin that is cured by heat, active energy rays, moisture, etc., such as a thermosetting resin, a light-curable resin, or a moisture-curable resin, or may contain a thermoplastic resin. Examples of active energy rays include visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays.
[0089] The photo-curable hot melt resin composition of the present invention may contain additives (also referred to as "other additives") other than the photopolymerization initiator (C), filler, moisture curing accelerating catalyst, coupling agent, and colorant. Examples of the other additives include plasticizers, tackifiers, antioxidants, surfactants, flame retardants, wax particles, ionic liquids, foamed particles, expanding particles, and reactive diluents.
[0090] <Initial adhesive strength> The initial adhesive strength is an adhesive strength measured 1 to 5 minutes after the start of bonding, in which a light-and-moisture-curable hot-melt resin composition is melted and applied to an adherend, irradiated with ultraviolet (UV) light of a predetermined energy, and then the applied and irradiated light-and-moisture-curable hot-melt resin composition is bonded to another adherend and pressed thereto. The photo-curable hot melt resin composition of the present invention has an initial adhesive strength after 3 minutes of compression of, for example, 0.5 MPa or more, preferably an initial adhesive strength after 3 minutes of compression of 1.0 MPa or more, and more preferably an initial adhesive strength after 1 minute of compression of 1.0 MPa or more. If the initial adhesive strength 3 minutes after compression is 0.5 MPa or more, it becomes easier to prevent the adherends from shifting apart due to slight external force, or to prevent the adherends from floating apart due to repulsive force from parts built into the adherends. In addition, the initial adhesive strength is preferably 0.5 MPa or more, more preferably 0.7 MPa or more, and even more preferably 1.0 MPa or more, when the photo-moisture-curable hot melt resin composition is melt-coated, then attached to another adherend and pressed against it, and 5 minutes have passed since the start of pressing. Specifically, the initial adhesive strength can be measured by the method described in the Examples.
[0091] The initial adhesive strength can be adjusted, for example, by the components constituting the urethane prepolymer (A), and as described above, it is easy to make it equal to or greater than a certain value by giving the light-moisture-curable hot melt resin composition moderate crystallinity. More specifically, the initial adhesive strength can be increased by using a polyol having moderate crystallinity as the polyol (a2), which is the raw material of the urethane prepolymer (A). In addition, by using a polyol with low crystallinity (preferably liquid) in combination with the polyether polycarbonate polyol (a1), it is easy to increase the initial adhesive strength while obtaining a moderate flexibility. The initial adhesive strength can also be adjusted by the component composition and amount of the radically polymerizable compound (B).
[0092] <Pot life> The photo-curable hot melt resin composition of the present invention is typically used in a bonding process in which the photo-curable hot melt resin composition is melted and applied to a first adherend, irradiated with UV of a predetermined energy, and then a second adherend is bonded and pressure-bonded via the applied and UV-irradiated photo-curable hot melt resin composition. In the bonding process, the first adherend is melt-coated, UV is irradiated, and the second adherend is pressure-bonded one minute after UV irradiation, and the pot life is the time that the composition can be left standing from the completion of melt coating until UV irradiation. More specifically, the solution was applied to a first polycarbonate substrate, the temperature of which was adjusted to 25° C., with a line width of 1.0 mm, and the dose was 1000 mJ / cm 2 . 2 The pot life is defined as the time that the composition can be left after being applied to the first polycarbonate substrate and before being irradiated with ultraviolet light, when the composition is irradiated with ultraviolet light of 1000 nm and a second polycarbonate substrate is pressed to the first polycarbonate substrate at 0.04 MPa for 10 seconds one minute after the end of the ultraviolet light irradiation. The photo-curable hot melt resin composition of the present invention has a pot life of 60 to 300 seconds, preferably 90 to 300 seconds, and more preferably 120 to 300 seconds. If the pot life is 60 seconds or longer, when it is necessary to precisely adjust the attachment position of the second adherend relative to the first adherend, sufficient time is ensured for the position adjustment, making it easier to prevent defects due to misalignment of the attachment position. On the other hand, by making the pot life 300 seconds or less, the development of the initial adhesive strength after pressure bonding is not delayed, and the above-mentioned initial adhesive strength after 3 minutes is easily developed.
[0093] Typical moisture-curing hot melt resin adhesives have a moderately high crystallinity and a relatively fast solidification rate, which means that the time it takes for the adhesive resin to crystallize and solidify and demonstrate adhesive strength after the adherends are bonded together - the so-called set time - can be made suitably short. On the other hand, if the crystallinity is too high, the composition will solidify before being attached to the adherends, and will not wet with the attached adherends, failing to exhibit adhesive strength. On the other hand, if the crystallinity is too low, the adhesive will remain in a liquid state for a long time even after bonding of the adherends, and it will take a long time to crystallize and solidify to develop adhesive strength. However, in the photo-curable hot melt resin composition of the present invention, the radical polymerizable compound (B) acts as a plasticizer, suppressing crystallinity before UV irradiation and maintaining a liquid state after melt application. This allows for a long usable time before lamination. Next, when the radical polymerizable compound (B) reacts with UV irradiation to increase its molecular weight and loses its plasticizer effect, the high crystallinity of the urethane prepolymer (A) is restored and the urethane prepolymer (A) is rapidly solidified and crystallized to demonstrate adhesive strength. The initial adhesive strength being at a certain level or higher is an indication that the urethane prepolymer (A) is in a state where it will crystallize and solidify to develop adhesive strength.
[0094] <Impact resistance> The photo-curable hot melt resin composition of the present invention is prepared by laminating a pair of adherends with the photo-curable hot melt resin composition therebetween, and then photo-curing the resin composition to obtain a measurement sample. When an impact resistance test is carried out on the sample, the durability is preferably 50 or more, more preferably 100 or more, and even more preferably 150 or more. In the present invention, the high durability leads to good impact resistance, and even if an electronic device is dropped during use, the parts bonded by the resin composition can be prevented from falling off when dropped. The impact resistance test is performed using a DuPont drop impact tester by repeatedly dropping a 200g stainless steel weight from a height of 150mm onto one of the adherends until one of the adherends peels off. The number of times the weight is dropped before one of the adherends peels off is defined as the durability, and the higher the durability, the better the impact resistance.
[0095] <Manufacturing method> In the production of the photo-curable hot melt resin composition of the present invention, first, a urethane prepolymer (A) is prepared. As described above, the urethane prepolymer (A) can be obtained by reacting the polyol (Aa) with the polyisocyanate compound (Ab). Thereafter, the radical polymerizable compound (B), the photopolymerization initiator (C), and, if necessary, a moisture curing accelerating catalyst, a coupling agent, and other components other than these are added to the urethane prepolymer (A) and mixed with a known mixer to obtain a photo-curable hot melt resin composition. The mixture may be heated appropriately during mixing. The mixer is not particularly limited, but examples thereof include a homodisper, a homomixer, a universal mixer, a planetary mixer, a planetary stirring device, a kneader, and a three-roll mixer.
[0096] <How to use> The photo-curable hot melt resin composition of the present invention is cured and used as a cured product. The photo-curable hot melt resin composition of the present invention is used, for example, as an adhesive, and the cured photo-curable hot melt resin composition may be used to bond, for example, a pair of adherends.
[0097] The photo-curable hot melt resin composition of the present invention may be heated until it melts, and applied to one of the adherends in the molten state, and then the applied photo-curable hot melt resin composition may be irradiated with UV light, and then the other adherend may be superimposed on the one of the adherends. As a result, the adherends are temporarily fixed by the photo-curable hot melt resin composition that has been cooled and solidified. The photo-curable hot melt resin composition may be heated to, for example, 40°C or higher and 130°C or lower, preferably 50°C or higher and 100°C or lower, and melted. Subsequently, by irradiating UV light, the photopolymerization initiator (C) is activated and the radically polymerizable compound (B) undergoes a polymerization reaction, thereby eliminating the plasticizer effect and promoting the crystallization of the urethane prepolymer (A). After bonding to the adherends, the material quickly solidifies, temporarily fixing the adherends in place. Thereafter, the photo- and moisture-curable hot-melt resin composition is hardened by moisture, for example, by being left in the atmosphere, and the adherends are fixed together with a higher adhesive strength (final adhesive strength) by the hardened photo- and moisture-curable hot-melt resin composition than at the time of temporary fixation.
[0098] The photo-curable hot melt resin composition of the present invention is preferably used as an adhesive for electronic components, for example. The adherend is not particularly limited, but is preferably various electronic components constituting electronic devices, more preferably electronic components constituting portable electronic devices. The material of the adherend may be any of metal, glass, plastic, etc. In addition, the shape of the adherend is not particularly limited, and examples thereof include a film, sheet, plate, panel, tray, rod (rod), box, and housing. Examples of portable electronic devices include, but are not limited to, mobile phones such as smartphones, digital cameras, wearable devices, portable game devices, tablet computers, notebook computers, and action cameras, with smartphones and wearable devices being preferred among these.
[0099] Electronic components may have a cured product of the photo- and moisture-curable hot melt resin composition, but generally have a substrate, and therefore electronic devices such as portable electronic devices in which the photo- and moisture-curable hot melt resin composition of the present invention is used may have a cured product of the photo- and moisture-curable hot melt resin composition and a substrate, on which various electronic circuits are generally provided.
[0100] In electronic devices, for example, substrates may be used as adherends and bonded to each other via the photo-moisture-curable hot-melt resin composition of the present invention, or the substrate may be bonded to other electronic components (e.g., a housing) of the electronic device via the photo-moisture-curable hot-melt resin composition of the present invention. For example, the light-curable hot melt resin composition of the present invention may be used to obtain an assembled part by, for example, bonding substrates together inside an electronic device, etc. The assembled part thus obtained has a first substrate, a second substrate, and the cured body of the present invention, and at least a portion of the first substrate is bonded to at least a portion of the second substrate via the cured body. EXAMPLES
[0101] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0102] In the present examples, various physical properties were measured as follows.
[0103] (Pot life) In the evaluation of the pressure-bonding property described below, the coating was applied to a first polycarbonate substrate adjusted to 25°C with a line width of 1.0 mm, and left for a predetermined time, after which UV was irradiated under the conditions shown in Tables 1 and 2 using a 365 nm UV-LED as a light source, and one minute after the end of the UV irradiation, the second polycarbonate substrate was pressure-bonded at 0.03 MPa for 10 seconds. This operation was repeated, with the predetermined time from coating to UV irradiation initially being 30 seconds, and then gradually lengthening every 30 seconds thereafter, and the longest time at which the pressure-bonding property described below was "○" was defined as the usable time. When UV irradiation was not performed, the pot life was defined as the longest time during which the pressure bondability was "good" from the time of application to the time of lamination of the polycarbonate substrate.
[0104] (Initial adhesive strength) As shown in FIG. 1(a), a first substrate 11 measuring 90 mm×50 mm and 5 mm thick with a circular hole 11A with a diameter of 12 mm in the center, and a second substrate 12 measuring 50 mm×50 mm and 5 mm thick were prepared. Both the first substrate 11 and the second substrate 12 were polycarbonate plates. Spacers 15A and 15B were attached to both side ends of the second substrate 12 (see FIG. 1(b)). The spacers 15A and 15B were tapes measuring 3 mm wide, 50 mm long, and 0.15 mm thick. The photo-curable hot melt resin composition 10 was heated and melted at the heating and application temperatures shown in Tables 1 and 2 and applied to the hole 11A of the first substrate 11 at the center in a circular shape of φ25 mm at an application speed of 12 mm / s, a width of 1 mm±0.2 mm, and a height of 0.3 mm±0.05 mm using a dispenser (Musashi Engineering Co., Ltd., "Shotmaster200DS").
[0105] The time when the above application is completed is set to 0 seconds, and within the specified pot life, a 365 nm UV-LED is used as the light source, and the applied light-moisture-curing hot melt resin composition is irradiated with a UV dose of 1,000 mJ / cm. 2 UV irradiation was performed so that
[0106] One minute after the UV irradiation was completed, the first and second substrates 11 and 12 were placed on the first substrate 11 through the photo-curable hot melt resin composition 10 so that the centers of the first and second substrates 11 and 12 were aligned. Then, a 250 g weight was placed on the second substrate 12 for 10 seconds, and a pressure of about 0.03 MPa was applied to press the first and second substrates 11 and 12 through the photo-curable hot melt resin composition 10 to obtain a measurement sample 13. At this time, the distance between the first and second substrates 11 and 12 was maintained at 0.15 mm by the spacers 15A and 15B. The 250 g weight was removed from the measurement sample 13, and the measurement sample 13 was left at 25°C and 50% RH. Next, the measurement sample 13 was arranged so that the first substrate 11 was on the upper side and the second substrate 12 was on the lower side, and in a state in which the first substrate 11 was supported by a stainless steel jig, a rod-shaped member 14 having a circular cross section with a diameter of 10 mm was inserted into the hole 11A. Then, as shown in FIG. 1(b), the second substrate 12 was pressed vertically downward by the rod-shaped member 14 at a speed of 10 mm / min, and the stress when the second substrate 12 peeled off from the first substrate 11 was measured and used as the initial adhesive strength. The initial adhesive strength was measured from 1 to 5 minutes after the start of pressure bonding by adjusting the time left at 25°C and 50% RH. The measurement from application to the measurement of the initial adhesive strength was performed in an environment of 25°C and 50% RH. When UV irradiation was not performed, the UV irradiation was omitted, and the second substrate 12 was superimposed within a predetermined pot life.
[0107] In the dispenser, the photo-curable hot melt resin composition was filled in a 30cc syringe (Musashi Engineering, "PSY-30F"), and a needle with an inner diameter of 0.66 mm (Musashi Engineering, "PN-20G-A") was set at the tip of the syringe. The syringe heating holder and temperature control unit used were "TCU-02" manufactured by Musashi Engineering. The method of discharging the photo-curable hot melt resin composition from the syringe was a method of pushing with air pressure, and the air pressure control unit used was "ML-5000XII" manufactured by Musashi Engineering. The discharge amount of the photo-curable hot melt resin composition was adjusted by varying the air pressure between 0.01 and 0.30 MPa.
[0108] (Crimping ability) In the evaluation of the initial adhesive strength, the pressure-bonding property was evaluated based on whether the light-and-moisture-curable hot-melt resin composition applied in a circular shape was crushed to a thickness of 0.2 mm or less. A 250 g weight was left stationary for 10 seconds, and if the light-and-moisture-curable hot-melt resin composition was crushed to a thickness of 0.2 mm or less, it was marked as "◯", and if not crushed, it was marked as "X".
[0109] (Impact resistance test) 2, after obtaining a measurement sample 13 using the same procedure as for the initial adhesive strength, the measurement sample 13 was left for 72 hours in an environment of 25° C. and 50% RH. After being left for 72 hours, the first substrate 11 was placed on the upper side and the second substrate 12 was placed on the lower side, and the first substrate 11 was supported by a stainless steel jig.
[0110] Also, a stainless steel shooting die 16 shown in Fig. 3 was prepared. The shooting die 16 is a rod-shaped member with a head 16B at one end, and the rod-shaped portion 16A of the shooting die 16 has a cylindrical small diameter portion 16C with a diameter of 10 mm and a length of 17 mm at the other end and a cylindrical large diameter portion 16D with a length of 65 mm at the head 16B side, and the large diameter portion 16D and the small diameter portion 16C are connected via a connecting portion 16E with a length of 3 mm. The diameter of the connecting portion 16E tapers gradually from the large diameter portion 16D to the small diameter portion 16C. Head 16B has a cylindrical base portion 16F with a diameter of 30 mm and a height of 15 mm connected to large diameter portion 16D, and is provided at one end side of base portion 16F with tip 16G with an end face diameter of 16 mm and a height of 3 mm.
[0111] As shown in FIG. 2, the shooting die 16 was placed upright on the center of the second substrate 12 with the large diameter portion 16D of the rod-shaped portion 16A inserted into a support hole (not shown) of a DuPont drop impact tester, and the small diameter portion 16C of the rod-shaped portion 16A inserted into the hole 11A of the first substrate 11. In this state, a 200 g stainless steel weight 17 was repeatedly dropped vertically downward onto the tip 16G of the head 16B from a position 150 mm above the tip 16G of the head 16B using a DuPont drop impact tester, and the number of times the weight 17 was dropped until the second substrate 12 peeled off due to the impact of the weight 17 was evaluated as the durability. A higher durability indicates higher impact resistance.
[0112] The components used in each of the Examples and Comparative Examples were as follows. <Polyol> (Polyether polycarbonate polyol) PEPCD: Polyether polycarbonate diol (polyether skeleton: derived from PTMG), manufactured by Mitsubishi Chemical Corporation, "PEPCD NT-2002", liquid at room temperature
[0113] (Polyester diol) PEsD1: Toyokuni Oil Mills, "HS 2H-200S", polyol: 1,6-hexanediol (HD), polycarboxylic acid: sebacic acid (SA), solid at room temperature PEsD2: Toyokuni Oil Mills, "HS 2H-351A", polyol: 1,6-hexanediol (HD), polycarboxylic acid: adipic acid (AA), solid at room temperature
[0114] (Polycarbonate polyol) PCD1: Mitsubishi Chemical Corporation, "BENEBiOL NL2000D", polycarbonate diol derived from 1,10-decanediol (1,10-DDO), solid, solid at room temperature
[0115] <Polyisocyanate compounds> Sumidur 44S41, diphenylmethane diisocyanate (MDI), manufactured by Sumika Covestro
[0116] <Radical polymerizable compound> Cyclic nitrogen-containing compound: Tokyo Chemical Industry Co., Ltd., "NVC", N-vinyl-ε-caprolactam Monofunctional urethane acrylate: "Viscoat #216" manufactured by Osaka Organic Chemical Industry Co., Ltd., 1,2-ethanediol-1-acrylate-2-(N-butylcarbamate) Monofunctional acrylate a: "Viscoat #192" manufactured by Osaka Organic Chemical Industry Co., Ltd., phenoxyethyl acrylate Monofunctional acrylate b: "DMAA" manufactured by KJ Chemicals, dimethylacrylamide
[0117] <Photopolymerization initiator> "Omnirad TPO" manufactured by IGM Resin BV, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide
[0118] <Coupling Agent> Shin-Etsu Chemical Co., Ltd. "KBM-573", N-phenyl-3-aminopropyltrimethoxysilane <Moisture curing catalyst> San-Apro "U-cat660M", bis(2-morpholinoethyl) ether
[0119] [Example 1] 60 parts by mass of PEPCD and 40 parts by mass of PEsD1 as polyol (Aa) were placed in a 500 mL separable flask. The flask was stirred and dehydrated at 110°C under vacuum (20 mmHg or less) until the moisture content was 200 ppm or less. Nitrogen was then sealed in to bring the pressure to normal, and 22 parts by mass of diphenylmethane diisocyanate as polyisocyanate compound (Ab) was placed in the flask, which was then stirred and reacted at 80°C for 3 hours to obtain a urethane prepolymer (A) having an isocyanate group. To the obtained urethane prepolymer (A), N-vinyl-ε-caprolactam, 1,2-ethanediol-1-acrylate-2-(N-butylcarbamate), phenoxyethyl acrylate, and dimethylacrylamide as the radical polymerizable compound (B), diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide as the photopolymerization initiator (C), a coupling agent, and a moisture curing catalyst were added in the amounts shown in Table 1, and the mixture was stirred at a temperature of 80°C using a planetary mixer (Thinky Corporation, "Awatori Rentaro") to obtain the light-to-moisture curing hot melt resin composition of Example 1.
[0120] [Examples 2 to 9, Comparative Examples 1 to 2] The same procedure as in Example 1 was carried out, except that the amount of the polyol raw material, the amount of the polyisocyanate compound, and the amount of the radical polymerizable compound used in the synthesis of the urethane prepolymer were changed as shown in Tables 1 and 2.
[0121] [Reference examples 1 and 2] In Examples 1 and 7, the initial adhesive strength when UV irradiation was not performed is shown in Reference Examples 1 and 2.
[0122] [Table 1] *In the radical polymerization component (B) of Tables 1 and 2, the mmol% column indicates the mass% of each component in the radical polymerization component (B).
[0123] [Table 2]
[0124] As shown in Table 1, the photo-curable hot melt resin composition of each Example contained a urethane prepolymer obtained from a polyol having polyether polycarbonate polyol (a1), either a polyester polyol or a polycarbonate polyol, a radical polymerizable compound, and a photopolymerization initiator. Therefore, while having a pot life of 60 seconds or more, the initial adhesive strength 3 minutes after pressure bonding was 0.5 MPa or more, and both workability during lamination and high productivity due to short-time adhesion were achieved. Furthermore, the impact resistance was also excellent.
[0125] In contrast, the moisture-curable hot-melt resin composition of Comparative Example 1, which did not contain a radical polymerizable compound or a photopolymerization initiator, had a short pot life of 30 seconds when the initial adhesive strength 3 minutes after pressing was 0.5 MPa or more, and when the pot life was 150 seconds, it was not possible to obtain an initial adhesive strength of 1 MPa or more within 5 minutes after pressing. Furthermore, the light-and-moisture-curable hot-melt resin composition of Comparative Example 2, which did not contain polyether polycarbonate polyol, crystallized too quickly after UV irradiation and did not have a sufficient usable time, so it could not be crushed in the compression adhesion evaluation, and the initial adhesive strength could not be evaluated. In Reference Examples 1 and 2, the same compositions as in Examples 1 and 7 were not irradiated with UV light, but without UV irradiation, the crystallization was slow due to the continued plasticization by the radical polymerizable compound, and no initial adhesive strength was observed in a short time. This clearly shows the plasticizing effect of the addition of the radical polymerizable compound and the effect of promoting crystallization by the UV reaction.
Claims
1. The composition comprises a hot-melt urethane prepolymer (A) that is solid at room temperature, a radical polymerizable compound (B), and a photopolymerization initiator (C), The hot melt type urethane prepolymer (A) is a reaction product of a material containing polyether polycarbonate polyol (a1).
2. the hot-melt urethane prepolymer (A) is a reaction product of a polyol (A-a) and a polyisocyanate (A-b); the polyol (A-a) contains a polyether polycarbonate polyol (a1) and a polyol (a2) different from the polyether polycarbonate polyol (a1); The light-curable, moisture-curable hot melt resin composition according to claim 1, wherein the polyol (a2) is at least one selected from the group consisting of polyester polyols and polycarbonate polyols.
3. The light-curable, moisture-curable hot melt resin composition according to claim 2, wherein the polyether polycarbonate polyol (a1) has a linear alkylene group having 3 to 8 carbon atoms.
4. The light-curable, moisture-curable hot melt resin composition according to claim 2 or 3, wherein the polyester polyol contains a structural unit derived from a linear polyol and a structural unit derived from a linear polycarboxylic acid.
5. The light moisture curable hot melt resin composition according to claim 4, wherein the linear polyol is 1,6-hexanediol, and the linear polycarboxylic acid is at least one selected from the group consisting of adipic acid and sebacic acid.
6. The light-and-moisture-curable hot melt resin composition according to claim 2 or 3, wherein the polycarbonate polyol contains a structural unit derived from a linear polyol having 8 or more carbon atoms.
7. The polyol (A-a) contains 40% by mass or more of polyether polycarbonate polyol (a1) and 30% by mass or more of polyol (a2), and the light-curable hot melt resin composition according to claim 2 or 3.
8. The photo-curable hot melt resin composition according to claim 2 or 3, wherein the polyol (a2) has a number average molecular weight of 2,000 or more and 4,000 or less.
9. The light-curable, moisture-curable hot-melt resin composition according to claim 1 or 2, further comprising a silane coupling agent.
10. The photo-curable hot melt resin composition according to claim 9 , wherein the silane coupling agent comprises an aromatic amine-based silane coupling agent.
11. The photo-curable, moisture-curable hot melt resin composition according to claim 1 or 2, comprising 90 parts by mass or more of a monofunctional radically polymerizable compound relative to 100 parts by mass of the radically polymerizable compound (B).
12. The light moisture-curable hot melt resin composition according to claim 11 , wherein the monofunctional radical polymerizable compound includes a nitrogen-containing compound.
13. The light moisture-curable hot melt resin composition according to claim 12 , wherein the nitrogen-containing compound comprises a chain-like nitrogen-containing compound.
14. The light moisture-curable hot melt resin composition according to claim 12 or 13, wherein the nitrogen-containing compound comprises a cyclic nitrogen-containing compound.
15. The photo-curable hot melt resin composition according to claim 14, wherein a mass ratio (cyclic / chain) of the cyclic nitrogen-containing compound to the chain nitrogen-containing compound is 0.1 or more and 2.0 or less.
16. The light-curable, moisture-curable hot melt resin composition according to claim 12 or 13, wherein the content of the nitrogen-containing compound is 10 parts by mass or more and 95 parts by mass or less relative to 100 parts by mass of the radical polymerizable compound (B).
17. The light moisture-curable hot melt resin composition according to claim 12 or 13, wherein the monofunctional radical polymerizable compound contains a monofunctional (meth)acrylic acid ester compound in addition to the nitrogen-containing compound.
18. 3. The photo-curable hot melt resin composition according to claim 1, wherein the mass ratio (A / B) of the urethane prepolymer (A) to the radical polymerizable compound (B) is 70 / 30 or more and 91 / 9 or less.
19. The photo-curable hot melt resin composition according to claim 1 or 2, wherein the polyisocyanate (A-b) is at least one selected from the group consisting of isocyanurate-modified polyisocyanates and polymeric MDI.
20. The light-and-moisture-curable hot-melt resin composition according to claim 1 or 2, wherein the initial adhesive strength after 3 minutes of pressure bonding is 0.5 MPa or more.
21. The solution was applied to a first polycarbonate substrate, the temperature of which was adjusted to 25° C., with a line width of 1.0 mm, and applied at 1000 mJ / cm 2 UV reaction is caused by exposing the material to ultraviolet light.
3. The light-and-moisture-curable hot melt resin composition according to claim 1, wherein the composition has a pot life of 60 seconds or more from application to the first polycarbonate substrate until irradiation with ultraviolet light when the second polycarbonate substrate is pressure-bonded to the first polycarbonate substrate one minute after the end of the ultraviolet light irradiation.
22. 3. An adhesive for electronic components comprising the photo- and moisture-curable hot melt resin composition according to claim 1 or 2.
23. A cured product of the light-curable, moisture-curable hot melt resin composition according to claim 1 or 2.
24. An electronic component comprising the cured body according to claim 23.
Citation Information
Patent Citations
Reactive hot-melt adhesive composition and adherend bonding method
JP2019006854A
Radical-curable hot-melt urethane resin composition and moldings for optical use
WO2012096111A1
Resin composition
WO2015056478A1
Polyurethane resin and method for producing same
WO2023013510A1
Impact-resistant reactive hot melt adhesive composition
JP6778379B2