Laminate molding and manufacturing method of laminate molding
Additive manufacturing of weld beads with controlled compositions and conditions addresses the inefficiencies of existing residual stress methods, enhancing mechanical properties and adhesion in laminated objects by generating compressive stress efficiently.
Patent Information
- Application Number
- JP2023061572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-05
AI Technical Summary
Existing methods for controlling residual stress in laminated weld beads, such as rolling and shot peening, require special equipment and increase production lead time, and are costly.
A method involving the additive manufacturing of weld beads with specific compositions and welding conditions to generate compressive residual stress without additional processing, using an apparatus with a manipulator, heat source, and filler material supply system to form weld beads with controlled cross-sectional areas and heat inputs.
Generates compressive residual stress in laminated objects, improving mechanical properties and adhesion between layers without additional processing costs or time, while preventing crack expansion.
Smart Images

Figure 2024148444000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a layered object and a method for manufacturing a layered object. [Background technology]
[0002] Additive manufacturing objects with layered weld beads are prone to residual stress due to welding phenomena. This residual stress affects the mechanical properties of the manufactured structure. For example, it is known that compressive residual stress is desirable for improving fatigue life, but tensile residual stress tends to reduce fatigue life. Taking these effects into account, methods for controlling the distribution of residual stress have been proposed (e.g., Patent Documents 1 and 2).
[0003] Patent Document 1 describes that tensile residual stress remains throughout the entire product of a molded object, making it difficult to bond between layers, so that uniform compressive residual stress is imparted by rolling the layers to impart plastic strain to them. Patent Document 2 describes that compressive residual stress is imparted to a molded object by shot peening. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-13686 A [Patent Document 2] Special Publication No. 2019-507250 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the methods of Patent Documents 1 and 2 both require special facilities, equipment, and costs, and further increase the production lead time of the object. Therefore, an object of the present invention is to provide an additive manufacturing method and an additive manufacturing method that improve the mechanical properties of an object by generating compressive residual stress in the object without adding any new processing to the additive manufacturing process. [Means for solving the problem]
[0006] The present invention comprises the following configurations. (1) An additive manufacturing object in which weld beads formed by melting a filler metal on a base metal are repeatedly laminated, The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less The balance is Fe and unavoidably contained impurities. The cross-sectional area of the cross section perpendicular to the extension direction of the weld bead is 8.0 mm 2 Above 80.0mm 2 The filling portion includes a plurality of bead layers in which the following weld beads are arranged side by side: Among the plurality of bead layers of the filling portion, an intermediate layer including a center in the lamination direction has a compressive residual stress in the lamination direction of 47 MPa or more. Additive manufacturing. (2) A method for manufacturing an additive manufacturing object by repeatedly stacking weld beads formed by melting a filler metal on a base metal, comprising the steps of: The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less The balance is Fe and unavoidably contained impurities. The weld bead is welded to a filler metal deposition amount of 165 mm 3 / sec~200mm 3 / sec, heat input is 400J / mm~4000J / mm. When forming a filled portion by stacking bead layers in which the weld beads are arranged side by side, an intermediate bead layer including a center in a stacking direction of the weld beads among the plurality of bead layers of the filled portion is made a bead layer having a compressive residual stress in the stacking direction of 47 MPa or more. A method for manufacturing an additively manufactured object. Effect of the Invention
[0007] According to the present invention, compressive residual stress can be generated in a molded object without adding a new process to the additive manufacturing process, thereby improving the mechanical properties of the molded object. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view of a layered object. [Diagram 2] FIG. 2 is a schematic diagram of an additive manufacturing apparatus that additively manufactures an object. [Diagram 3] FIG. 3 is an explanatory diagram that illustrates a cross section of a bead model of a weld bead that forms the object illustrated in FIG. [Figure 4] FIG. 4 is a side view of the test specimen. [Diagram 5] FIG. 5 is a perspective view of the base material included in the test specimen. [Figure 6] FIG. 6 is an explanatory diagram showing a path for forming a weld bead to form a laminate. [Figure 7] FIG. 7 is an explanatory diagram showing the positions at which residual stress was measured on the test specimen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Here, an example will be described in which a layered object is manufactured by a weld bead formed by arc welding, but other manufacturing methods may be used as long as a desired shape is manufactured by melting and solidifying a material.
[0010] FIG. 1 is a schematic cross-sectional view of a layered object. The layered object (hereinafter referred to as the object) 100 shown here is formed by repeatedly stacking weld beads formed by melting and solidifying a filler material such as a welding wire on a base material 11. The object 100 is configured to include, for example, an outer shell portion 13 and a filling portion 15 on the base material 11. The outer shell portion 13 may be a bead wall in which weld beads having a predetermined welding cross-sectional area are connected in a cross section perpendicular to the bead extension direction shown in FIG. 1, or may be a base material wall formed by a part of the base material. The filling portion 15 is formed in a portion surrounded by the outer shell portion 13 by a weld bead having a welding cross-sectional area larger than that of the outer shell portion 13. The outer shell portion 13 is not limited to being formed on the outer peripheral edge of the filling portion 15, and may form the inner wall of a cavity defined within the filling portion 15.
[0011] The filling portion 15 is a multi-layer structure in which bead layers in which weld beads are arranged side by side are laminated. The weld beads of each bead layer constituting the filling portion 15 are formed by melting and solidifying a filler metal, and their properties change depending on the welding conditions and the heat extraction conditions from the surrounding members. Here, the layer including the interface between the base material 11 and the filling portion 15 is called a deep layer 15a, the layer including the exposed surface that is the final layer (top layer) of the bead layers laminated as the filling portion 15 is called a surface layer 15c, and the layer sandwiched between the deep layer 15a and the surface layer 15c is called an intermediate layer 15b. Note that each of the layers 15a, 15b, and 15c referred to here is not limited to a single bead layer, but includes the case where the layers are formed by multiple bead layers.
[0012] The above-described model 100 can be manufactured by, for example, an additive manufacturing apparatus that performs welding using an arc as a heat source. 2 is a schematic diagram of an additive manufacturing apparatus 200 that additively manufactures a model. The additive manufacturing apparatus 200 shown as an example includes a modeling control device 21, a manipulator 23, a filler material supply device 25, a manipulator control device 27, and a heat source control device 29.
[0013] The manipulator control device 27 controls the manipulator 23 and the heat source control device 29. A controller (not shown) is connected to the manipulator control device 27, and any operation of the manipulator control device 27 can be instructed by an operator via the controller.
[0014] The manipulator 23 is, for example, an articulated robot, and a torch 31 provided on a tip shaft is supported so that a filler material M can be continuously supplied. The torch 31 holds the filler material M in a state where it protrudes from the tip. The position and posture of the torch 31 can be set arbitrarily in three dimensions within the range of the degrees of freedom of the robot arm constituting the manipulator 23. The manipulator 23 is preferably one having six or more degrees of freedom, and is preferably one that can arbitrarily change the axial direction of the heat source at the tip. The manipulator 23 may be in various forms, such as a four- or more-axis articulated robot as shown in FIG. 1, or a robot equipped with angle adjustment mechanisms on two or more orthogonal axes.
[0015] The torch 31 has a shield nozzle (not shown), and a shielding gas is supplied from the shielding nozzle. The shielding gas blocks the atmosphere and prevents oxidation and nitridation of the molten metal during welding, thereby suppressing poor welding. The arc welding method used in this configuration may be either a consumable electrode type such as a shielded metal arc welding or a carbon dioxide gas arc welding, or a non-consumable electrode type such as a TIG (Tungsten Inert Gas) welding or a plasma arc welding, and is appropriately selected depending on the object to be molded. Here, gas metal arc welding is taken as an example for explanation. In the case of the consumable electrode type, a contact tip is arranged inside the shield nozzle, and a filler material M to which a current is supplied is held by the contact tip. The torch 31 generates an arc from the tip of the filler material M in a shielding gas atmosphere while holding the filler material M.
[0016] The filler metal supplying device 25 supplies the filler metal M toward the torch 31. The filler metal supplying device 25 includes a reel 25a on which the filler metal M is wound, and a pay-out mechanism 25b that pays out the filler metal M from the reel 25a. The filler metal M is fed to the torch 31 while being sent in the forward or reverse direction by the pay-out mechanism 25b as necessary. The pay-out mechanism 25b is not limited to a push type that is disposed on the filler metal supplying device 25 side and pushes out the filler metal M, but may be a pull type or a push-pull type that is disposed on a robot arm or the like.
[0017] The heat source control device 29 is a welding power source that supplies power required for welding by the manipulator 23. The heat source control device 29 adjusts the welding current and welding voltage supplied when forming a bead by melting and solidifying the filler metal M. In addition, the filler metal supply speed of the filler metal supply device 25 is adjusted in conjunction with the welding conditions set by the heat source control device 29, such as the welding current and welding voltage.
[0018] The heat source for melting the filler metal M is not limited to the above-mentioned arc. For example, other types of heat sources may be used, such as a heating method using both an arc and a laser, a heating method using plasma, or a heating method using an electron beam or a laser. When heating with an electron beam or a laser, the amount of heat can be controlled more precisely, and the state of the bead to be formed can be more appropriately maintained, which contributes to further improving the quality of the laminated structure.
[0019] The filler metal M may have the following composition, which is particularly effective in terms of compressive residual stress.
[0020] (Filler material) C: 0.02% or more, 0.15% or less Si: 0.50% or more, 0.90% or less Mn: 1.10% or more, 1.60% or less P: 0.025% or less S: 0.025% or less Cr: 0.30% or more, 0.60% or less Mo: 0.10% or more, 0.45% or less Ti: 0.02% or more, 0.30% or less Cu: 0.4% or less
[0021] The object-forming control device 21 controls the above-mentioned components in an integrated manner. The object-forming control device 21 is not limited to being directly connected to the manipulator control device 27, and may be configured as another computer remotely connected to the manipulator control device 27 via a network or the like.
[0022] The additive manufacturing apparatus 200 having the above-mentioned configuration operates according to a modeling program created based on a modeling plan for the object 100. The modeling program is composed of a large number of command codes, and is created based on an appropriate algorithm according to various conditions such as the shape, material, and heat input of the object. When the torch 31 is moved and the supplied filler material M is melted and solidified according to this modeling program, a linear weld bead B, which is a molten solidified body of the filler material M, is formed on the base material 11. That is, the manipulator control device 27 drives the manipulator 23 and the heat source control device 29 based on a predetermined program provided from the modeling control device 21. The manipulator 23 moves the torch 31 while melting the filler material M with an arc, according to a command from the manipulator control device 27, to form the weld bead B. In this manner, the weld beads B are sequentially formed and stacked to obtain the object 100 having the desired shape.
[0023] The molding control device 21 is configured by hardware using an information processing device such as a PC (Personal Computer). Each function of the molding control device 21 is realized by a control unit (not shown) reading out a program having a specific function stored in a storage device (not shown) and executing the program. Examples of the storage device include a memory such as a RAM (Random Access Memory) which is a volatile storage area, a ROM (Read Only Memory) which is a non-volatile storage area, and a storage such as a HDD (Hard Disk Drive) and an SSD (Solid State Drive). Examples of the control unit include a processor such as a CPU (Central Processing Unit) and an MPU (Micro Processor Unit), or a dedicated circuit.
[0024] When additive manufacturing of the shaped object 100 shown in FIG. 1 is performed by the additive manufacturing apparatus 200, the following procedure is generally performed. First, the target shape to be manufactured is sliced at the height of the weld bead to generate a slice model of multiple layers. A torch movement path (path) for forming beads with the width of the weld bead for each of the shapes of the generated slice models is obtained to generate a bead model simulating the weld bead. A weld bead B is formed along the bead model thus obtained, thereby forming a bead layer having the shape of the slice model. In this manner, a plurality of bead layers are repeatedly stacked to manufacture a shaped object of the target shape. The cross-sectional shape of the weld bead B (bead width, bead height, etc.) is adjusted according to welding conditions such as the feed speed of the filler metal M, the welding voltage, and the welding current.
[0025] The path for forming the above-mentioned weld bead B and information on the welding conditions are included in the above-mentioned molding program, and the molding control device 21 outputs a molding program corresponding to the shape of the object to be molded to the manipulator control device 27, so as to mold the desired shape of the object.
[0026] 3 is an explanatory diagram showing a schematic cross section of a bead model of a weld bead B forming the shaped object 100 shown in FIG. 1. A bead model BMa forming the outer shell portion 13 shown in FIG. 1 and a bead model BMb forming the filling portion 15 are laminated on the base material 11. The outer shell portion 13 is formed of a relatively small weld bead to improve shape accuracy, and the filling portion 15 is formed of a relatively large weld bead to improve filling efficiency. Therefore, the bead model BMb of the filling portion 15 is made larger than the bead model BMa of the outer shell portion 13. In other words, the bead models BMa and BMb are set so that the cross-sectional area of the cross section perpendicular to the extension direction of the weld bead is larger in the filling portion 15 than in the outer shell portion 13.
[0027] In order to form the weld beads of the outer shell portion 13 and the filling portion 15 into weld beads having different cross-sectional areas, the welding conditions may be made different for each. The cross-sectional area of the weld bead corresponding to the bead model BMa of the outer shell portion 13 is, for example, 2.5 mm 2 ~70mm 2 The welding conditions for forming this weld bead are as follows: the deposition amount of filler metal M is 25 mm 3 / sec~165mm 3 The heat input is set to a low heat input condition of 50 J / mm to 2500 J / mm / sec. On the other hand, the cross-sectional area of the weld bead corresponding to the bead model BMb of the filling portion 15 is, for example, 8.0 mm 2 ~80mm 2 The welding conditions for forming this weld bead are as follows: the deposition amount of filler metal M is 165 mm 3 / sec~200mm 3 / sec, and the heat input is set to 400 J / mm to 4000 J / mm. An example of welding under low heat input conditions is CMT (Cold Metal Transfer: registered trademark) welding.
[0028] In this way, when the welding conditions for the filled portion 15 are set to be larger than those for the outer shell portion 13 in terms of the amount of weld bead deposited per unit time (correlated with the bead cross-sectional area) and the amount of heat input, a relatively large compressive residual stress in the stacking direction is generated in the filled portion 15 compared to the outer shell portion 13.
[0029] In this specification, the above-mentioned "high heat input condition" means that the deposition amount (volume ratio) is at least twice as much and the heat input is at least 1.5 times as much as that under the "low heat input condition". The cross-sectional area of the weld bead may be estimated from the deposition volume per unit time based on the volume of the filler metal used (e.g., the diameter and length of the welding wire), the welding conditions, etc. Also, the shaped object after molding may be cut and observed in the manner for observing the macroscopic structure of steel (JIS G0553), and the bead cross-sectional area may be estimated from the observed boundary line of the weld bead.
[0030] It is known that when weld beads are repeatedly layered, the tensile residual stress generated in the molded object tends to turn into compressive residual stress, which improves the mechanical strength (for example, Reference 1: T. Mukherjee, W. Zhang, T. Deb Roy, An improved prediction of residual stresses and distortion in additive manufacturing, Computational Materials Science 126 (2017), PP. 360-372). Therefore, the more layers of weld beads there are, the more reliably compressive residual stress is generated, which is preferable, and it is preferable to layer at least 10 layers.
[0031] Furthermore, in a molded object described in detail below, the residual stress (residual stress in the layering direction (Z direction) of the molded object) generated in the molded object was measured using test specimens cut out from multiple locations of the filled part 15, and the residual stress value varied depending on the location of the molded object. As shown in FIG. 1, when the molded object has an outer shell part 13 on the base material 11 and a filled part 15 inside the outer shell part 13, the residual stress of the filled part 15 was measured in a region (also called the "boundary part") including the boundary (Z=0) between the base material 11 and the weld bead on the upper layer. Every part of the boundary part had a compressive residual stress of 70 MPa or more. On the other hand, the residual stress inside the filled part 15 away from the boundary part (at a depth of Z=25 mm) and the surface part including the surface layer of the filled part 15 (at a position of Z=50 mm) showed a tendency different from that of the boundary part.
[0032] The residual stress inside such a molded product is preferably 47 MPa or more, and more preferably 84 MPa or more. In particular, when the molded product has a compressive residual stress of 171 MPa or more inside, the residual stress from the boundary with the base material to the surface of the molded product is compressive regardless of location, resulting in a well-balanced residual stress distribution. In this way, the relatively large compressive residual stress inside the molded product not only improves the adhesion between the bead layers, but also suppresses the spread of defects and cracks in the thickness direction even if they occur in the molded product.
[0033] In the present invention, in order to obtain the above-mentioned residual stress distribution, mechanical treatments such as shot peening, which causes particles to collide with the shaped object, and rolling, which applies pressure using a pressing mechanism, are not generally performed because they require additional costs. These mechanical treatments are preferably performed only when necessary and only on specific parts within an acceptable cost range. For example, since an external force is likely to act on the outer shell 13 in a direction that causes the base material and the laminate of weld beads to peel off, these mechanical post-treatments may be performed on the periphery of the outer shell 13. In this case, the tensile stress caused by the external force is alleviated around the outer shell 13, and peeling and cracking of the base material and the laminate can be suppressed. EXAMPLES
[0034] The test specimen shown below was fabricated, and the residual stress distribution generated in the test specimen was confirmed. (Modeling of test specimen) Fig. 4 is a side view of the specimen TP, and Fig. 5 is a perspective view of a base material 11 included in the specimen TP. The specimen TP shown in Fig. 4 has a shape simulating the shaped object shown in Fig. 3, and is composed of a base material 11 and a laminate 35.
[0035] 5, the base material 11 has a flat portion 39 in which two grooves 37A, 37B having a semicircular cross section and opening at the top are formed, and a wall portion 41 erected along the longitudinal direction of the grooves 37A, 37B at one end side of the flat portion 39. A wall surface 41a of the wall portion 41 facing the flat portion 39 is a vertical surface perpendicular to the upper surface 39a of the flat portion 39. The grooves 37A, 37B are formed parallel to each other, and one end of each groove in the longitudinal direction is formed to the end of the flat portion 39.
[0036] A weld bead stack 35 was formed in a recess formed by flat portion 39 and wall portion 41 of base material 11 shown in Fig. 4. The stack 35 has an outer shell portion 47, groove wall portions 49A and 49B that cover groove portions 37A and 37B to form hollow space 39 with a circular cross section, and a filling portion 51. Groove wall portions 49A and 49B were formed under the same or similar conditions as those for outer shell portion 47.
[0037] 6 is an explanatory diagram showing the formation pass of the weld bead for forming the laminate 35. Here, the weld bead was formed in sequence on the upper surface 39a of the flat portion 39 in a plurality of passes along the longitudinal direction of the grooves 37A and 37B to form the laminate 35. Specifically, the outer shell 47 was formed by pass PSa, the groove walls 49A and 49B were formed by pass PSb, and the filling portion 51 was formed by pass PSc. FIG. 6 shows the pass for forming one bead layer on the flat portion 39, but the next layer was laminated in the same manner, and the laminate 35 having the shape shown in FIG. 4 was obtained by laminating a total of 10 layers or more.
[0038] Two types of welding conditions were applied to form the weld beads described above. Low heat input welding conditions were applied to the outer portion that forms the outer frame of the object (the rectangular frame including the outer shell portion 47, and the groove wall portions 49A and 49B), and relatively high heat input welding conditions were applied to the filling portion (filling portion 51) that surrounds the outer periphery.
[0039] An arc welding robot (ARCMAN-MP, manufactured by Kobe Steel, Ltd.) was used as the additive manufacturing device, and weld beads were laminated under the conditions shown in Table 1.
[0040] [Table 1]
[0041] In other words, the amount of welding for the outer part is 28.3 mm 3 / sec, and the heat input was low at 300.1 J / mm. For the filled area surrounded by the periphery, the deposition amount was 179.1 mm 3 The heat input conditions were high, with a heat input of 576.6 J / mm / sec. In both cases, the shielding gas was Ar gas with CO 2 A gas containing 20% of gas was used. Furthermore, for the filled portion 51, weaving was performed with an amplitude of 1 m and a cycle of 4 Hz.
[0042] The material of the base material 11 is carbon steel S35C (JIS G4051) for mechanical construction. A welding wire (MB-S63B: manufactured by Kobe Steel, Ltd.) with a wire diameter of φ12 mm was used as the filler material M. In order to suppress the occurrence of cracks in the weld bead during the forming process, the base material 11 was preheated, and then the first layer (first layer) was laminated while maintaining the temperature in the range of 200 to 300°C.
[0043] After lamination of the weld bead layer, annealing heat treatment was performed in order to evaluate residual stress remaining reliably in the laminate 35. The annealing treatment was performed under conditions of increasing the temperature at 100° C. / hr, and then holding at 580° C. for 6 hr.
[0044] (Estimation of metal composition of test specimen) Table 2 shows the composition standard (see C1M1T of JIS Z 3312) of the filler metal M used to fabricate the above test specimen TP, an example of the composition of the deposited metal (product specification value listed in the catalog), and an example of the composition of the filled part of a simple test specimen (not shown) fabricated by combining outer shell fabrication and filling fabrication.
[0045] [Table 2]
[0046] From Table 2, the composition of the molded object does not generally deviate from the component specifications of the filler metal. Only Mn deviates slightly from the component specifications, but this is thought to be because Mn is relatively easily oxidized and is consumed by the generation of slag, etc. Taking the above into consideration, it is estimated that the metal composition in the filled part 51 of the test specimen and the metal composition that affects the residual stress are within the ranges shown below. C: 0.02% or more, 0.15% or less Si: 0.50% or more, 0.90% or less Mn: 1.00% or more, 1.60% or less P:0.025% or less S: 0.025% or less Cr: 0.30% or more, 0.60% or less Mo: 0.10% or more, 0.45% or less Ti: 0.02% or more, 0.30% or less Cu: 0.4% or less The remainder is iron and unavoidable impurities (O, Al, etc.)
[0047] (residual stress in test specimen) The residual stress of the test specimen TP formed as described above was measured using a strain gauge method (cutting method). FIG. 7 is an explanatory diagram showing the residual stress measurement positions of the test specimen TP. In order to investigate the introduction of various residual stresses from the test specimen TP, measurements were taken at multiple locations P1 to P11 in the outer shell and filled portion of the test specimen TP. In addition, for each of the locations P1 to P11, the residual stress was measured at each depth position of the surface layer (Z=0 mm) of the filled portion 51, the middle layer (Z=25 mm), and the deep layer (Z=50 mm) which is the position of the upper surface 39a of the flat portion 39. The measurement results of the residual stress for each layer at each location are shown in Table 3. Note that the signs in Table 3 indicate that minus (-) means compressive residual stress and plus (+) means tensile residual stress.
[0048] [Table 3]
[0049] The evaluation results of each of the portions P1 to P11 of the test specimen TP were judged according to the following criteria. ◎: Compressive residual stress occurs in each layer, and the magnitude is 100 MPa or more in all cases. ○: Compressive residual stress occurs in each layer, and the magnitude is 50 MPa or more in all cases, but does not correspond to ◎. △: Compressive residual stress occurs in each layer, and the magnitude is 25 MPa or more in all cases, but does not correspond to ◎ or ○. ×: Other than ◎, ○, △
[0050] Examples of areas with well-balanced compressive residual stress from deep layers to the surface include P2 and P3. At these areas P2 and P3, the compressive residual stress is 25 MPa or more at least at a depth of z=25 mm, which is a desirable state. Furthermore, as in areas P1, P4, and P5, the compressive residual stress further increases away from the outer shell 47 and the wall of the base material 11 41. From this, it was confirmed that the compressive residual stress definitely increases at positions closer to the center of the laminate 35, and the residual stress distribution is balanced toward the compression side.
[0051] In addition, when comparing the parts P1 to P8 in the region of the filled portion 51 with the parts P9 to P11 in the region of the outer shell portion 47, it was confirmed that no large compressive residual stress was generated in the outer shell portion 47 formed by the weld beads with a relatively low heat input. This shows that repeatedly stacking weld beads formed with a relatively high heat input is preferable for introducing compressive residual stress. In addition, with regard to the extension direction of the weld beads, there was a tendency for the compressive residual stress to be relatively larger on the inside (middle part) than on the end side (for example, comparison between P3 and P8, comparison between P1 and P4, and comparison between P2 and P7). The above-mentioned similar tendency can be confirmed from the above-mentioned literature 1.
[0052] In addition, it is preferable that the intermediate layer 15b has a compressive residual stress of 84 MPa or more, since the residual stress in the lamination direction is almost entirely compressive residual stress, and furthermore, it is preferable that the intermediate layer 15b has a compressive residual stress of 171 MPa or more, since a larger compressive residual stress distribution can be obtained.
[0053] Furthermore, the presence of the outer shell portion 47 around the filling portion 51 allows the outer edge shape of the laminate 35 to be formed with high precision. Moreover, since the weld bead of the filling portion 51 is prevented from dripping off, the filling portion 51 can be formed under high heat input conditions that result in a larger weld cross-sectional area. This allows the compressive residual stress generated in the filling portion 51 to be further increased, resulting in a configuration with excellent mechanical properties. In this way, by providing the outer shell portion 47, the average value of the compressive residual stress of the filling portion 51 can be made even larger than the average value of the compressive residual stress of the outer shell portion 47, thereby improving the mechanical properties of the laminate 35 including the filling portion 51.
[0054] As described above, the present specification discloses the following: (1) An additive manufacturing object in which weld beads formed by melting a filler metal on a base metal are repeatedly laminated, The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less The balance is Fe and unavoidably contained impurities. The cross-sectional area of the cross section perpendicular to the extension direction of the weld bead is 8.0 mm 2 Above 80.0mm 2 The filling portion includes a plurality of bead layers in which the following weld beads are arranged side by side: Among the plurality of bead layers of the filling portion, an intermediate layer including a center in the lamination direction has a compressive residual stress in the lamination direction of 47 MPa or more. Additive manufacturing. With this additive manufacturing product, the compressive residual stress of the additive manufacturing product is 47 MPa or more, which improves the adhesion between the bead layers. In addition, even if defects or cracks occur in the product, the expansion of the defects and cracks in the thickness direction can be suppressed, resulting in a configuration with excellent mechanical properties.
[0055] (2) The layered object according to (1), comprising an outer shell portion joined to the filling portion along at least a portion of the outer periphery of the filling portion. With this additive manufacturing product, the presence of the outer shell on the outer periphery of the filled part allows the outer shape to be formed with high precision. Moreover, since dripping of the weld bead of the filled part is prevented, the product can be formed under high heat input conditions that result in a larger weld cross-sectional area. This further increases the compressive residual stress that is generated, resulting in a configuration with excellent mechanical properties.
[0056] (3) The additive manufacturing object according to (2), wherein the average value of the compressive residual stress of the filling portion is greater than the average value of the compressive residual stress of the outer shell portion. According to this layered object, by providing an outer shell portion, the mechanical properties of the layered body 35 including the filling portion 51 can be improved.
[0057] (4) The filling portion includes a deep layer including an interface with the base material, a surface layer including an exposed surface of the filling portion, and the intermediate layer sandwiched between the deep layer and the surface layer, The layered object according to any one of (1) to (3), wherein the compressive residual stress of the intermediate layer is 84 MPa or more. This layered product is preferable because the residual stress in the layering direction is almost entirely compressive residual stress.
[0058] (5) The layered object according to (4), wherein the compressive residual stress of the intermediate layer is 171 MPa or more. With this layered object, the residual stress from the boundary with the base material to the surface of the object is compressive regardless of location, resulting in a well-balanced residual stress distribution.
[0059] (6) A method for manufacturing an additive manufacturing object by repeatedly stacking weld beads formed by melting a filler metal on a base metal, comprising the steps of: The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less The balance is Fe and unavoidably contained impurities. The weld bead is welded to a filler metal deposition amount of 165 mm 3 / sec~200mm 3 / sec, heat input is 400J / mm~4000J / mm. When forming a filled portion by stacking bead layers in which the weld beads are arranged side by side, an intermediate bead layer including a center in a stacking direction of the weld beads among the plurality of bead layers of the filled portion is made a bead layer having a compressive residual stress in the stacking direction of 47 MPa or more. A method for manufacturing an additively manufactured object. According to this manufacturing method for additive manufacturing, the compressive residual stress of the additive manufacturing object can be increased to 47 MPa or more by adjusting the conditions of the amount of filler metal deposited and the amount of heat input. This not only improves the adhesion between the bead layers, but also suppresses the expansion of defects and cracks in the thickness direction even if they occur in the molded object, resulting in a configuration with excellent mechanical properties.
[0060] (7) A method for manufacturing an additive manufacturing object described in (6), in which an outer shell portion that is joined to the filling portion along at least a portion of the outer peripheral edge of the filling portion is formed under conditions in which the deposition amount and the heat input are lower than those of the weld bead that forms the filling portion. According to this method for manufacturing an additive manufacturing object, the presence of an outer shell on the outer periphery of the filled part allows the outer shape to be formed with high precision. Moreover, since dripping of the weld bead of the laminated filled part is prevented, the product can be formed under high heat input conditions resulting in a larger weld cross-sectional area. This further increases the compressive residual stress generated, resulting in a structure with excellent mechanical properties. [Explanation of symbols]
[0061] 11 Base material 13 Outer shell 15 Filling section 15a deep 15b Middle class 15c surface layer 21 Modeling control device 23 Manipulator 25 Filler metal supply device 27 Manipulator control device 29 Heat source control device 31 Torch 35 Laminate 37A,37B Groove 39 Flat area 39a Top side 41 Wall 41a Wall 45 Wall 47 Outer shell 49A,49B Groove wall 51 Filling section 100 Models (Layered Models) 200 Additive Manufacturing Equipment TP test specimen
Claims
1. An additive manufacturing object in which weld beads formed by melting a filler metal on a base metal are repeatedly laminated, The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less, The balance is Fe and unavoidably contained impurities. The cross-sectional area of the cross section perpendicular to the extension direction of the weld bead is 8.0 mm 2 More than 80.0 mm 2 The filling portion includes a plurality of bead layers in which the following weld beads are arranged side by side: An intermediate layer including a center in a lamination direction among the plurality of bead layers of the filling portion has a compressive residual stress in the lamination direction of 47 MPa or more. Additive manufacturing.
2. and an outer shell portion joined to the filling portion along at least a portion of the outer periphery of the filling portion. The layered object according to claim 1 .
3. The average value of the compressive residual stress of the filling portion is greater than the average value of the compressive residual stress of the outer shell portion. The layered object according to claim 2.
4. The filling portion includes a deep layer including an interface with the base material, a surface layer including an exposed surface of the filling portion, and the intermediate layer sandwiched between the deep layer and the surface layer, The compressive residual stress of the intermediate layer is 84 MPa or more. The layered object according to claim 1 .
5. The compressive residual stress of the intermediate layer is 171 MPa or more. The layered object according to claim 4.
6. A method for manufacturing an additive manufacturing object by repeatedly stacking weld beads formed by melting a filler metal on a base material, comprising: The composition of the layered object is, in mass%, C: 0.02% or more, 0.15% or less, Si: 0.50% or more, 0.90% or less, Mn: 1.00% or more, 1.60% or less, P: 0.025% or less, S: 0.025% or less, Cr: 0.30% or more, 0.60% or less, Mo: 0.10% or more, 0.45% or less, Ti: 0.02% or more, 0.30% or less, Cu: 0.4% or less, The balance is Fe and unavoidably contained impurities. The weld bead is welded to a filler metal deposition amount of 165 mm 3 / sec~200mm 3 / sec, and the heat input is 400 J / mm to 4000 J / mm. When forming a filled portion by stacking bead layers in which the weld beads are arranged side by side, an intermediate bead layer including a center in a stacking direction of the weld beads among the plurality of bead layers of the filled portion is made into a bead layer having a compressive residual stress in the stacking direction of 47 MPa or more. A method for manufacturing an additively manufactured object.
7. forming an outer shell portion joined to the filling portion along at least a part of an outer periphery of the filling portion under conditions in which the deposition amount and the heat input amount are lower than those of a weld bead forming the filling portion; The method for producing a layered object according to claim 6 .
Citation Information
Patent Citations
Welding material for building-up of journal part of high chrome rotor, high chrome rotor and production therefor
JP1998006080A
Method and apparatus for manufacturing components using sequential deposition of layers - Patents.com
JP2019507250A
Shaping plan assistance method, and shaping plan assistance device
JP2022020393A
Method for manufacturing laminated modeling, manufacturing system of laminated modeling and manufacturing program for laminated modeling
JP2022074401A
Manufacturing method for additive manufactured article and additive manufactured article
WO2020230592A1
Cited By
Additional processing device, additional processing method, and additional processing program
JP7745121B1