Toner and two-component developer

The toner formulation with amorphous polyester and a graft polymer with specific exothermic peak temperature differences addresses the issue of release agent oozing and flowing in high-speed machines, ensuring effective image separation and media uniformity across various paper types.

JP2024148784APending Publication Date: 2024-10-18CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023062227
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing toners in high-speed machines experience poor separation and image deterioration due to the release agent oozing out onto the toner surface and flowing down onto the paper surface, affecting image quality and media uniformity, especially in solid and low-density images.

Method used

A toner formulation with amorphous polyester as the binder resin and a graft polymer having specific exothermic peak temperature differences, along with a release agent, to control the release agent's seepage and prevent it from flowing down onto the paper surface while maintaining low-temperature fixability.

Benefits of technology

The solution achieves both good seepage of the release agent in solid images and suppression of its flow in low-density images, ensuring constant media speed and high-speed fixation without compromising low-temperature fixability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148784000001
    Figure 2024148784000001
  • Figure 2024148784000002
    Figure 2024148784000002
  • Figure 2024148784000003
    Figure 2024148784000003
Patent Text Reader

Abstract

To provide a toner that achieves both good seeping of a mold release agent in a solid image and prevention of flow-down of the mold release agent to a paper surface in a low density image, while maintaining low temperature fixability, and thereby achieves the uniform velocity of media in a high-speed machine.SOLUTION: A toner has a toner particle containing a binder resin, a mold release agent, and a graft polymer (A). The binder resin contains an amorphous polyester. The graft polymer (A) has two or more exothermic peaks, and the mold release agent has at least one exothermic peak in differential scanning calorimetry. When a peak temperature of the peak on the highest temperature side of the exothermic peaks of the graft polymer (A) is defined as TMax (°C), a peak temperature of the peak on the lowest temperature side as TMin (°C), and a peak temperature of the largest exothermic peak of the mold release agent as TWax (°C), the following formulas are satisfied. (1) 5.0≤TMax-TMin≤20.0, and (2) 10.0≤TWax-TMax≤40.0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner and a two-component developer used in electrophotography, electrostatic recording, electrostatic printing, and the like. [Background technology]

[0002] In recent years, full-color electrophotographic copying machines have become widespread and have begun to be applied to the printing market. In the printing market, there is a growing demand for high speed, high image quality, and high productivity while handling a wide range of media (paper types). For example, even if the paper type is changed from thick paper to thin paper, there is a demand for media uniformity, which means that printing can be continued without changing the process speed or the set temperature for heating the fixing unit according to the paper type. From the viewpoint of media uniformity, toner is required to properly separate from the fixing belt or fixing roller and to properly complete fixing to the media over a wide range of fixing temperatures from low to high.

[0003] In order to fix the toner at a wide range of temperatures, there is a method of adding a release agent to the toner to give the toner releasability. In this case, the dispersion state of the release agent in the toner has a significant effect on the properties of the toner, so it is desirable that the dispersion state is fine and uniform. Patent Document 1 proposes a technology of adding a dispersant that disperses the release agent in the toner in order to control the dispersion state of the release agent in the toner. Patent Document 2 also proposes using a toner binder consisting of a high viscosity resin, a low viscosity resin, and a dispersant to improve the dispersibility of the release agent and suppress separation failure and image deterioration. Furthermore, Patent Document 3 proposes a toner that uses a crystalline polyester as the binder resin as a toner that has excellent low-temperature fixing properties to realize fixing over a wide range of temperatures. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-013548 A [Patent Document 2] JP 2007-264349 A [Patent Document 3] JP 2004-046095 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in high-speed machines for the printing market, even if the dispersion state of the release agent in the toner is controlled by the methods described in Patent Documents 1 and 2, poor separation and image degradation may occur. This is believed to be because, in order for a release agent to be effective, it is not sufficient for it to be present uniformly in the toner; it is important that the release agent quickly seeps out onto the toner surface and remains on the toner surface when the toner is heated by the fixing member, for example.

[0006] For this reason, even if the dispersion state of the release agent is controlled in high-speed machines, if the seepage of the release agent due to heating is delayed, separation failure and image degradation may occur, especially in solid images. Also, if the seepage of the release agent is fast, in the case of low-density images such as halftone images or images with few adjacent toner particles such as dot images, the release agent may not be supported on the image surface that became liquid during fixing at the edge of the image and may flow down to the paper surface. If the release agent flows down to the paper surface, the function of the release agent may be impaired, and the separation property and the abrasion resistance of the image may decrease.

[0007] Increasing the viscosity of the toner binder resin is an effective way to prevent the release agent from seeping out of the toner surface and running off onto the paper surface, but this method also impairs low-temperature fixability and media uniformity. Therefore, in order to realize a uniform media speed in a high-speed machine, there are problems such as the seepage speed of the release agent onto the toner surface related to the separation of a solid image, and the flow-off of the release agent from the surface of a low-density image onto the paper surface. The present disclosure is directed to a toner and a two-component developer having the toner that realize a uniform media speed in a high-speed machine by maintaining low-temperature fixing properties and simultaneously achieving good seepage of the release agent in a solid image and suppression of the release agent from flowing off onto the paper surface in a low-density image. [Means for solving the problem]

[0008] At least one embodiment of the present disclosure is a toner having toner particles containing a binder resin, a release agent, and a graft polymer (A), The binder resin contains an amorphous polyester, the graft polymer (A) has two or more exothermic peaks in an exothermic curve during cooling measured by differential scanning calorimetry, The release agent has at least one exothermic peak in an exothermic curve during a temperature drop measured by differential scanning calorimetry, The peak temperature of the highest exothermic peak of the graft polymer (A) is designated as T Max (℃), and the peak temperature of the lowest exothermic peak is T Min (°C), and the peak temperature of the maximum exothermic peak among the exothermic peaks of the release agent is T Wax (℃), The T Max , the T Min And the T Wax satisfies the following formulas (1) and (2): Regarding toner. 5.0≦T Max -T Min ≦20.0 (1) 10.0≦T Wax -T Max ≦40.0 (2) Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a toner and a two-component developer containing the toner that maintain low-temperature fixing properties, while achieving both good exudation of the release agent in solid images and suppression of the release agent from running off onto the paper surface in low-density images, and that achieves media-uniform speed in high-speed machines. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. A crystalline resin is a resin in which an endothermic peak is observed in differential scanning calorimetry (DSC).

[0011] The present disclosure relates to a toner having toner particles containing a binder resin, a release agent, and a graft polymer (A), The binder resin contains an amorphous polyester, the graft polymer (A) has two or more exothermic peaks in an exothermic curve during cooling measured by differential scanning calorimetry, The release agent has at least one exothermic peak in an exothermic curve during a temperature drop measured by differential scanning calorimetry, The peak temperature of the highest exothermic peak of the graft polymer (A) is designated as T Max (℃), and the peak temperature of the lowest exothermic peak is T Min (°C), and the peak temperature of the maximum exothermic peak among the exothermic peaks of the release agent is T Wax (℃), The T Max , the T Min And the T Wax satisfies the following formulas (1) and (2): Regarding toner. 5.0≦T Max -T Min ≦20.0 (1) 10.0≦T Wax -T Max≦40.0 (2)

[0012] The inventors have continued to study a toner that maintains low-temperature fixing properties, while simultaneously suppressing the seepage of release agent in solid images and the running off of release agent onto the paper surface in half-tone images, and that can achieve media-level speed on high-speed machines.

[0013] As a result, it was found that it is important for a toner containing an amorphous polyester as a binder resin, a release agent, and a graft polymer (A) to satisfy the following requirements. First, it is necessary for the release agent to have at least one exothermic peak in an exothermic curve during temperature drop measured by differential scanning calorimetry. Second, it is important for the graft polymer (A) to have two or more exothermic peaks in an exothermic curve during temperature drop measured by differential scanning calorimetry (DSC). When the graft polymer (A) has two or more exothermic peaks, it is considered that the graft polymer (A) has two or more sites with different crystallization temperatures, that is, the graft polymer (A) has sites that have two or more different crystalline states.

[0014] When the graft polymer (A) has two or more different crystal states, there may be a "crystalline site that is more likely to contribute to adsorption to the release agent" and a "crystalline site that is more likely to contribute to dispersion in the binder resin" in the graft polymer (A). Therefore, these different crystalline sites are considered to be in a state of being more functionally separated. And since it is important for the function as a dispersant or surfactant to have an adsorption group and a dispersion group in one molecule, it is particularly important for the graft polymer (A) to have two or more different crystalline sites in one molecule. Therefore, the graft polymer (A) can be a dispersant for the release agent.

[0015] The present inventors have focused on the relationship between the two or more exothermic peaks of the graft polymer (A) and the exothermic peak observed during cooling in differential scanning calorimetry (DSC) of the release agent. First, the present inventors determined the highest exothermic peak temperature T Max and the lowest heat peak temperature T MinThat is, the difference between the heat generation peak temperature T Max (℃) and exothermic peak temperature T Min (°C) must satisfy the following formula (1). 5.0≦T Max -T Min ≦20.0 (1)

[0016] difference T Max -T Min It was found that the exudation of wax can be controlled by the temperature difference T Max -T Min The present inventors believe that this causes a time lag in melting during heat fixing, reducing the adhesive force between the release agent and the graft polymer (A), resulting in improved exudation of the release agent. Max -T Min If the temperature is less than 5.0° C., the adhesive force between the release agent and the graft polymer (A) is strong, so that the exudation of the release agent in a solid image is delayed and wrapping is likely to occur.

[0017] Furthermore, it is considered that the above-mentioned "crystalline portion that is more likely to contribute to dispersion in the binder resin" melts first, generating a diffusive force into the binder resin, and the graft polymer (A) is separated from the release agent before melting, improving the exudation property. Max -T Min It was found that the above-mentioned effect of functional separation is more pronounced at temperatures of 5.0°C or higher, and that at temperatures of 20.0°C or lower, both the adsorption to the release agent and the dispersibility in the binder resin can be achieved. T Max -T Min is preferably 5.5 to 14.0°C, more preferably 6.0 to 10.0°C. Max -T Min can be made larger or smaller depending on the structure of the polyolefin moiety and the ratio of the number of moles of ethylene structure PE to the number of moles of propylene structure PP.

[0018] T Max From the viewpoint of low-temperature fixability and releasing agent, the temperature is preferably 55.0 to 80.0°C, and more preferably 60.0 to 72.0°C. TMin is the resin viscosity and T max In view of the above, the temperature is preferably 45.0 to 70.0°C, and more preferably 55.0 to 67.0°C.

[0019] Next, the present inventors determined the highest exothermic peak temperature T Max and the exothermic peak temperature T Wax As a result, the difference T Wax -T Max It was found that this method can control the flow of the release agent onto the paper surface. That is, T Wax (℃) and T Max (℃) must satisfy the following formula (2). 10.0≦T Wax -T Max ≦40.0 (2)

[0020] This is the temperature difference T Wax -T Max The present inventors believe that the presence of a certain amount of within the above range allows the seeped release agent to rapidly crystallize together with the graft polymer (A). Furthermore, they believe that the above-mentioned "crystalline portion that is more likely to contribute to adsorption to the release agent" rapidly crystallizes together with the release agent, thereby preventing the release agent from flowing down from the toner surface of the image dots to the paper surface. And the temperature difference T Wax -T Max It was found that when the temperature difference T is less than 10.0°C, the adsorption force between the release agent and the graft polymer (A) is too strong, and the exudation property is likely to decrease. Wax -T Max It was found that the effect of suppressing the release agent from flowing off onto the paper surface occurs when the temperature difference T is 40.0℃ or less. Wax -T Max is preferably 12.0 to 30.0°C, more preferably 14.5 to 29.0°C. Wax can be controlled by the type of release agent. Max can be controlled by the polyolefin moiety.

[0021] In addition, the binder resin contains an amorphous polyester, which improves low-temperature fixability. This is because polyester has a large interaction between ester groups, such as hydrogen bonds, and can increase cohesive strength and strength compared to styrene / acrylic resins. Therefore, high elasticity can be achieved even with a low molecular weight, and low viscosity at low temperatures can be achieved, improving low-temperature fixability. It is also preferable to introduce a benzene ring into the polymer main chain, which makes it easier to increase cohesive strength and strength.

[0022] The graft polymer (A) is preferably a graft polymer having a polyolefin portion and a styrene-acrylic polymer portion. The polyolefin portion can be a "crystalline portion that is more likely to contribute to adsorption to the release agent". The polyolefin portion has the highest exothermic peak temperature T Max On the other hand, the styrene acrylic polymer portion can be a "crystalline portion that is more likely to contribute to dispersion in the binder resin." The styrene acrylic polymer portion has the lowest exothermic peak temperature T Min It is thought that this may contribute to the expression of

[0023] The polyolefin portion preferably contains (i) a copolymer of ethylene and propylene, preferably has (ii) a portion having an acid group, and preferably has (iii) a ratio of the number of moles of PE of an ethylene structure to the number of moles of PP of a propylene structure, PE / PP, of 4 to 20. By satisfying these conditions, it is easier to obtain the effect of preventing the release agent from bleeding out and running off. The polyolefin portion is more preferably an ethylene / propylene copolymer having an acid group.

[0024] The ethylene structure (PE) is a form in which ethylene reacts in a copolymer of ethylene and propylene, and the propylene structure (PP) is a form in which propylene reacts in a copolymer of ethylene and propylene. From the viewpoint of controlling the adsorptivity to the release agent and the exothermic peak temperature, (i) the copolymer of ethylene and propylene is more effective. The adsorptivity to the release agent is dominated by the ethylene structure (PE), which has a high affinity with the release agent, and the exothermic peak temperature is The temperature is easy to control with the propylene structure (PP).

[0025] In addition, the above-mentioned heat generation peak temperature T Max and the exothermic peak temperature T Min From the viewpoint of controlling the temperature difference and the exudation of the release agent, it is preferable that the graft polymer (A) has (ii) a moiety having an acid group. It is considered that the polyolefin moiety having an acid group changes the crystal state and changes the temperature difference of the exothermic peak temperature. It was also found that the exudation property can be controlled by changing the affinity with the release agent by the acid group.

[0026] Furthermore, (iii) when the ratio (PE / PP) of the number of moles of the ethylene structure (PE) to the number of moles of the propylene structure (PP) is 4 or more, a prominent exothermic peak of crystallization is likely to be obtained. On the other hand, when PE / PP is 20 or less, it was found that two or more exothermic peaks are likely to be obtained. This is believed to be because the ethylene structure (PE), which is easily crystallized in the above range, functions effectively. PE / PP is more preferably 5 to 15, and even more preferably 6 to 12.

[0027] The weight average molecular weight of the polyolefin portion of the graft polymer (A) is preferably 1,000-3,000, and more preferably 1,500-2,500. When the weight average molecular weight of the polyolefin portion is within the above range, it is believed that the polyolefin portion is easily crystallized, and the adsorption to the release agent and the exudation are more effectively obtained. On the other hand, when the weight average molecular weight is 1000 or more, the adsorption to the release agent is high, the dispersibility is better, and the effect of suppressing runoff is more easily obtained. On the other hand, when the weight average molecular weight is 3000 or less, the adsorption is more moderate, and the exudation of the release agent is more easily improved.

[0028] Furthermore, the acid value of the polyolefin portion is preferably from 0.5 to 16.0 mgKOH / g, and more preferably from 1.0 to 10.0 mgKOH / g. When the acid value of the polyolefin portion is within the above range, the exothermic peak temperature T Max and T Min It is believed that when the acid value is 0.5 mgKOH / g or more, the change in the crystallization state becomes large, which is effective in changing the temperature difference of the exothermic peak temperature. Also, when the acid value is 16.0 mgKOH / g or less, it is believed that the adsorption to the release agent is not inhibited, and the dispersibility and the effect of preventing the runoff onto the paper surface become greater.

[0029] The acid value of the graft polymer (A) is preferably from 15.0 to 40.0 mgKOH / g, more preferably from 20.0 to 30.0 mgKOH / g. When the acid value of the graft polymer (A) is within the above range, the affinity to the binder resin, the amorphous polyester, is high, so the dispersibility is improved and the chargeability is also high. When the acid value is 15.0 mgKOH / g or more, the graft polymer (A) acts as a member that retains electric charge, and the chargeability is considered to be high. Also, when the acid value is 40 mgKOH / g or less, the affinity to the amorphous polyester is high and the adsorption force to the release agent is also strong, so that the dispersibility of the release agent is more likely to be improved.

[0030] The toner preferably contains 3 to 20 parts by mass, and more preferably 5 to 15 parts by mass, of crystalline polyester per 100 parts by mass of amorphous polyester. When the content of the crystalline polyester is within the above range, low-temperature fixability due to the plasticizing effect can be obtained while maintaining the charge retention.

[0031] The toner preferably contains 1 to 20 parts by mass, and more preferably 5 to 15 parts by mass, of a release agent per 100 parts by mass of the amorphous polyester. The toner preferably contains 1 to 20 parts by mass, and more preferably 5 to 15 parts by mass, of a graft polymer (A) per 100 parts by mass of the amorphous polyester. When the content of the polymer (A) is within the above range, the dispersibility of the release agent by the graft polymer (A) is maintained, while the exudation of the release agent and the effect of suppressing the runoff of the release agent onto the paper surface are more effectively obtained. Furthermore, when the amount of the crystalline polyester and the release agent is 20.0 parts by mass or less per 100 parts by mass of the amorphous polyester, the effect of preventing the release agent from seeping out and running off onto the paper surface is more easily obtained without impairing the charge retention and storage stability.

[0032] From the viewpoint of making it easier to obtain the effect of preventing the release agent from seeping out and running off onto the paper surface, the ratio of the content of the graft polymer (A) to the content of the release agent in the toner (graft polymer (A) / release agent) on a mass basis is preferably 0.5 to 1.5, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1.

[0033] The amorphous polyester is preferably a block copolymer having two or more different amorphous polyester segments, and more preferably a block copolymer having two different amorphous polyester segments. When the amorphous polyester is a block copolymer as described above, it is easier to obtain the effect of preventing the release agent from seeping out and running off onto the paper surface. When the amorphous polyester is a block copolymer, it is believed that since the amorphous polyester contains moieties with different polarities, it interacts with each of the moieties having different crystalline states in the graft polymer (A), thereby improving dispersibility. In particular, regarding the difference between the SP value of the styrene acrylic polymer moiety of the graft polymer (A) and the SP values ​​of two or more different amorphous polyester segments that make up the block copolymer, the minimum SP value difference is 1.00 [J / cm 3 ] 0.5 The dispersibility is improved by being less than or equal to 0.50 [J / cm 3 ] 0.5 More preferably, it is 0.30 [J / cm 3 ] 0.5 The lower limit is not particularly limited, but is, for example, 0.00 [J / cm 3 ] 0.5 More than 0.10[J / cm 3 ] 0.5 The above is preferred.

[0034] In addition, due to the interaction between two or more different amorphous polyester segments of the block copolymer, cracks are likely to form inside the toner when the toner is pressurized and fixed. This is believed to improve the exudation of the release agent, and as a result, improve the separation property. In particular, the SP value difference between two or more (preferably two) different amorphous polyester segments constituting the block copolymer is 1.0 [J / cm 3 ] 0.5 It is preferable that the SP value difference is 5.0 [J / cm or more]. When the SP value difference is within the above range, cracks are more likely to occur and the exudation effect of the release agent is more likely to be obtained. In addition, from the viewpoint of compatibility with the crystalline polyester, the SP value difference is 5.0 [J / cm 3 ] 0.5 For example, the SP value difference is preferably 1.0 to 5.0 [J / cm 3 ] 0.5 and more preferably 1.0 to 3.0 [J / cm 3 ] 0.5and more preferably 1.5 to 2.5 [J / cm 3 ] 0.5 It is.

[0035] Examples of the graft polymer (A), the amorphous polyester, the release agent, etc. are given below. <Graft polymer (A)> The graft polymer (A) preferably has a polyolefin portion and a styrene-acrylic polymer portion. Examples of the olefin constituting the polyolefin portion of the graft polymer (A) include ethylene, propylene, 1-butene, isobutylene, 1-hexene, 1-dodecene, and 1-octadecene. Ethylene and propylene are particularly preferred. Examples of polyolefins include polyethylene, polyolefins, olefin copolymers, oxides of olefin copolymers, and modified olefin copolymers. Examples of copolymers include ethylene / propylene copolymers, ethylene / 1-butene copolymers, propylene / 1-hexene copolymers, and oxides thereof. From the viewpoint of adsorptivity to the release agent, ethylene / propylene copolymers and oxides of ethylene / propylene copolymers are particularly preferred. The content of the polyolefin moiety in the graft polymer (A) is preferably from 5 to 20% by mass, and more preferably from 8 to 15% by mass.

[0036] Examples of oxides of olefin copolymers include those having functional groups such as carboxyl groups, aldehyde groups, and ester groups, and epoxides. The polyolefin moiety preferably has a moiety having an acid group. To impart an acid group to an olefin copolymer, a method of converting the functional group into a functional group-containing compound or a functional group can be mentioned. Examples of oxides include oxygen, carbon dioxide, a carboxylic acid compound having a carboxyl group, an ester compound having an ester group, an aldehyde compound having an aldehyde group, and epoxides.

[0037] The method for producing the polyolefin moiety is not particularly limited, and a conventionally known method can be used. Examples of the production method include a production method using a catalyst such as a general Zieglar catalyst or a metallocene catalyst. In addition, in order to produce a graft polymer (A) in which different segments are bonded and which is likely to obtain two or more peaks in DSC, a production method using a catalyst that is likely to cause living polymerization or specific production conditions such as low temperature is more preferable. Examples of catalysts that are likely to cause living polymerization include a method using a nickel complex or a titanium complex.

[0038] As a method for imparting an acid group to the polyolefin moiety, there can be mentioned a method in which oxygen, hydrogen, carbon dioxide and other gases are supplied in an adjusted manner during the production of polyolefin using a metallocene catalyst. Another method for providing an acid group is to contact an olefin polymer with a functional group-containing compound. The temperature for contact is −78 to +300° C., preferably −78 to +200° C., and the pressure is normal pressure to 100 kg / cm. 2 , preferably at normal pressure ~50kg / cm 2 The contact time is in the range of 1 minute to 100 hours, preferably 10 minutes. ~24 hour range.

[0039] The contact between the olefin polymer and the functional group-containing compound can be carried out in a solvent or without a solvent. Examples of the solvent to be used include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane; oxygen-containing compounds such as diethyl ether and tetrahydrofuran; and mixtures of these.

[0040] The graft polymer (A) is preferably a graft polymer having a polyolefin moiety and a styrene-acrylic polymer moiety. Examples of the constituent components of the styrene-acrylic polymer include the following.

[0041] Examples of the monomers include styrene monomers such as styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, p-methoxystyrene, p-hydroxystyrene, p-acetoxystyrene, vinyltoluene, ethylstyrene, phenylstyrene, and benzylstyrene; alkyl esters of unsaturated carboxylic acids (the number of carbon atoms of the alkyl is 1 to 18) such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, and cycloalkyl (meth)acrylate; hydroxyalkyl esters of unsaturated carboxylic acids such as 2-hydroxyethyl (meth)acrylate; vinyl ester monomers such as vinyl acetate; vinyl ether monomers such as vinyl methyl ether; halogen-containing vinyl monomers such as vinyl chloride; and diene monomers such as butadiene and isobutylene. These monomers can be used alone or in combination of two or more.

[0042] The styrene-acrylic polymer moiety is preferably a styrene-acrylic acid ester copolymer. The styrene-acrylic polymer moiety is preferably a polymer of a monomer mixture containing styrene and a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms (preferably 3 to 18, more preferably 3 to 6). More preferably, it is a polymer of a monomer mixture containing styrene and butyl acrylate. The monomer mixture may further contain (meth)acrylic acid, 2-hydroxyethyl (meth)acrylate, etc. The content of the monomer unit derived from the styrene monomer in the graft polymer (A) is preferably 50.0% by mass or more and 85.0% by mass or less, more preferably 60.0% by mass or more and 80.0% by mass or less. The content of the monomer unit derived from the (meth)acrylic acid alkyl ester in the graft polymer (A) is preferably 2.0% by mass or more and 15.0% by mass or less, more preferably 5.0% by mass or more and 10.0% by mass or less. The monomer unit refers to the form in which the monomer substance in the polymer is reacted. The content of the styrene-acrylic polymer moiety in the graft polymer (A) is preferably from 80 to 95% by mass, and more preferably from 85 to 92% by mass.

[0043] The method of graft-polymerizing the styrene-acrylic polymer to the polyolefin is not particularly limited, and a conventionally known method can be used. In addition, as a method for easily obtaining two peaks in the DSC of the graft polymer (A), it is more preferable to multi-stage-polymerize the polyolefin and the styrene-acrylic polymer. To improve the graft rate and adjust the molecular weight of the graft polymer (A), high-temperature pressurized polymerization can be used.

[0044] The weight average molecular weight (Mw) of the graft polymer (A) is preferably 5,000 or more and 70,000 or less, and more preferably 10,000 or more and 50,000 or less. When the weight average molecular weight of the graft polymer (A) is within the above range, the polymer moves appropriately in the toner, resulting in improved dispersibility of the release agent and improved blocking resistance of the toner.

[0045] <Release agent> The releasing agent used in the toner is a material that can be crystallized and has an exothermic peak in differential scanning calorimetry (DSC), and examples thereof include the following. Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes mainly composed of fatty acid esters such as carnauba wax; partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax; saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid and fatty acids such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol. Esters with alcohols such as amides of linoleic acid, amides of oleic acid, amides of lauric acid; saturated amides of fatty acids such as methylene bisstearic acid, amides of ethylene biscapric acid, amides of ethylene bislauric acid, amides of hexamethylene bisstearic acid; unsaturated amides of fatty acids such as ethylene bisoleic acid, amides of hexamethylene bisoleic acid, amides of N,N' dioleyl adipic acid, amides of N,N' dioleyl sebacic acid; aromatic amides such as m-xylene bisstearic acid, amides of N,N' distearyl isophthalic acid. fatty metal salts such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate (commonly known as metallic soaps); waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene or acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.

[0046] Among these release agents, hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax are preferred from the viewpoint of affinity with the graft polymer (A). That is, the release agent preferably contains a hydrocarbon wax, and more preferably is a hydrocarbon wax. From the viewpoints of affinity with the polyolefin moiety which is the adsorption site of the graft polymer (A) and exudation properties, the weight average molecular weight of the release agent is preferably 250-3,000, more preferably 400-2,700, and even more preferably 450-1,500.

[0047] Similarly, from the viewpoint of affinity, the ratio of the number of moles of ethylene structure (PE) to the number of moles of propylene structure (PP) in the hydrocarbon wax (PE / PP) WAX The above-mentioned ratio (PE / PP) in the graft polymer (A) (hereinafter, (PE / PP) GRAFT In particular, the ratio (PE / PP) is preferably close to WAX and the ratio of graft polymer (A) (PE / PP) GRAFT It is preferable that the difference between the ratio (PE / PP) is less than 50. Furthermore, in terms of exudation, in order to avoid excessive adsorption, the ratio (PE / PP) WAX and ratio (PE / PP) GRAFT It is preferable that they are not identical.

[0048] The peak temperature of the maximum heat generation peak during the temperature drop measurement of the release agent by differential scanning calorimetry (DSC) is T Wax From the viewpoint of low-temperature fixing property and separation property, the peak temperature T Wax The temperature is preferably from 70 to 120°C, and more preferably from 80 to 110°C.

[0049] <Amorphous polyester> Monomers used for the amorphous polyester include polyhydric alcohols (dihydric, trihydric or higher alcohols), polyvalent carboxylic acids (dihydric, trihydric or higher carboxylic acids), acid anhydrides thereof, or lower alkyl esters thereof.

[0050] As the polyhydric alcohol monomer, the following polyhydric alcohol monomers can be used. Examples of the dihydric alcohol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, and bisphenol represented by formula (A) and its derivatives; [ka]

[0051] (In the formula, R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.) Diols represented by the formula (B) are included. [ka]

[0052] Examples of trihydric or higher alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. Among these, glycerol, trimethylolpropane, and pentaerythritol are preferably used. These dihydric alcohols and trihydric or higher alcohols can be used alone or in combination.

[0053] As the polybasic carboxylic acid monomer for the polyester resin, the following polybasic carboxylic acid monomers can be used. Examples of divalent carboxylic acid components include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctylsuccinic acid, isooctylsuccinic acid, anhydrides of these acids, and lower alkyl esters thereof. Of these, maleic acid, fumaric acid, terephthalic acid, and n-dodecenylsuccinic acid are preferably used.

[0054] Examples of trivalent or higher carboxylic acids, their anhydrides or their lower alkyl esters include 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, their anhydrides or their lower alkyl esters. Among these, 1,2,4-benzenetricarboxylic acid, i.e., trimellitic acid or its derivatives, is particularly preferred because it is inexpensive and easy to control the reaction. These divalent carboxylic acids and trivalent or higher carboxylic acids can be used alone or in combination.

[0055] The method for producing the polyester is not particularly limited, and a known method can be used. For example, the above-mentioned alcohol monomer and carboxylic acid monomer are charged at the same time, and polymerized through an esterification reaction or an ester exchange reaction and a condensation reaction to produce a polyester resin. The polymerization temperature is not particularly limited, but is preferably in the range of 180°C to 290°C. For the polymerization of the polyester, for example, a polymerization catalyst such as a titanium-based catalyst, a tin-based catalyst, zinc acetate, antimony trioxide, or germanium dioxide can be used. In particular, the amorphous polyester is more preferably a polyester polymerized using a tin-based catalyst.

[0056] The binder resin used in the toner may be a hybrid resin containing other resin components as long as it is mainly composed of an amorphous polyester. For example, a hybrid resin of a polyester resin and a vinyl resin can be mentioned. As a method for obtaining a reaction product of a vinyl resin or a vinyl copolymer unit with a polyester resin, such as a hybrid resin, a method of carrying out a polymerization reaction of one or both of the resins in the presence of a polymer containing a monomer component capable of reacting with each of the vinyl resin or the vinyl copolymer unit and the polyester resin is preferred.

[0057] For example, among the monomers constituting the polyester resin component, those capable of reacting with the vinyl copolymer include unsaturated dicarboxylic acids such as phthalic acid, maleic acid, citraconic acid, itaconic acid, and their anhydrides, etc. Among the monomers constituting the vinyl copolymer component, those capable of reacting with the polyester resin component include those having a carboxyl group or a hydroxyl group, and acrylic acid or methacrylic acid esters.

[0058] In addition, if the binder resin is mainly composed of an amorphous polyester, various resin compounds conventionally known as binder resins can be used in combination with the vinyl resins described above. Examples of such resin compounds include phenol resins, natural resin-modified phenol resins, natural resin-modified maleic resins, acrylic resins, methacrylic resins, polyvinyl acetate resins, silicone resins, polyester resins, polyurethanes, polyamide resins, furan resins, epoxy resins, xylene resins, polyvinyl butyral, terpene resins, coumaroindene resins, and petroleum-based resins. The content of the amorphous polyester in the binder resin is preferably 50 to 100% by mass, and more preferably 80 to 100% by mass.

[0059] The amorphous polyester is preferably a block copolymer having two or more different amorphous polyester segments. The method for obtaining a block copolymer from two or more different amorphous polyester segments is not particularly limited and can be appropriately selected depending on the purpose. For example, the following methods (1) to (3) can be mentioned. From the viewpoint of the freedom of molecular design, (1) and (3) are preferred, and (1) is more preferred.

[0060] (1) A method in which one amorphous polyester previously prepared by a polymerization reaction and the other amorphous polyester previously prepared by a polymerization reaction are dissolved or dispersed in an appropriate solvent, and reacted with an extender having two or more functional groups that react with the hydroxyl group at the end of the polymer chain, such as a carboxylic acid, an isocyanate group, an epoxy group, or a carbodiimide group, thereby copolymerizing the polyester.

[0061] (2) A method in which one amorphous polyester previously prepared by a polymerization reaction and the other amorphous polyester previously prepared by a polymerization reaction are fed into a twin-screw extruder together with an ester exchange catalyst, etc., and prepared by a reactive extrusion method using a twin-screw extruder, etc.

[0062] (3) A method in which a hydroxyl group of one of the amorphous polyesters previously prepared by a polymerization reaction is used as a polymerization initiation component, and another amorphous polyester is copolymerized by ring-opening polymerization from the polymer chain end of the prepared amorphous polyester.

[0063] The peak molecular weight of the amorphous polyester is preferably 3500 to 20000 in terms of low-temperature fixability, etc. The acid value of the amorphous polyester is preferably 5 mgKOH / g to 30 mgKOH / g in terms of charge retention in a high-temperature, high-humidity environment, and the hydroxyl value of the amorphous polyester is preferably 20 mgKOH / g to 70 mgKOH / g in terms of low-temperature fixability and charge retention.

[0064] The amorphous polyester is preferably a condensation polymer of a monomer mixture containing bisphenol and terephthalic acid represented by formula (A). When a block copolymer having two or more different amorphous polyester segments is used, it is preferable to contain a condensation polymer of a monomer mixture containing bisphenol and terephthalic acid represented by formula (A) (condensation polymer c1) as one of the segments. The SP value [J / cm of the condensation polymer c1] 3 ] 0.5 is preferably from 12.0 to 13.5, and more preferably from 12.5 to 13.0. As the other segment, the amorphous polyester preferably has a segment containing a linear aliphatic diol having 2 to 4 carbon atoms (preferably 2 to 3 carbon atoms) as a constituent monomer. More preferably, the other segment is a monomer condensation polymer containing a linear aliphatic diol having 2 to 4 carbon atoms (preferably 2 to 3 carbon atoms) and terephthalic acid. The SP value [J / cm of the other segment 3 ] 0.5 is preferably 10.0 to 11.5, and more preferably 10.5 to 11.0.

[0065] <Crystalline polyester> In the toner, a crystalline polyester can be used to improve low-temperature fixing ability and abrasion resistance. The toner particles may contain a crystalline polyester. In order to more effectively suppress the release agent from flowing off onto the paper surface, the crystalline polyester is heated to a peak temperature T CPES and the exothermic peak temperature T WAX However, it is preferable that the following formula (3) is satisfied. |T CPES -T WAX |≦40 (3)

[0066] It is believed that the closeness of the exothermic peak temperatures of the crystalline polyester and the release agent makes it possible to more effectively prevent the release agent from being washed away from the dots to the slower crystallizing side, which is in a liquid state, when cooled and solidified, and that the separation property and abrasion resistance are further improved by allowing both the release agent and the crystalline polyester to remain on the dots. For the same reason, the exothermic peak temperature T MAX and the exothermic peak temperature T CPES It is preferable that the following formula (4) is satisfied. T CPES -T MAX ≦40 (4)

[0067] The melting point of the crystalline polyester is preferably from 65 to 110°C, and more preferably from 80 to 100°C.

[0068] As monomers used for the crystalline polyester, polyhydric alcohols (dihydric, trihydric or higher alcohols), polyvalent carboxylic acids (dihydric, trihydric or higher carboxylic acids), acid anhydrides thereof or lower alkyl esters thereof are used.

[0069] The polyhydric alcohol monomer used in the crystalline polyester may be the following polyhydric alcohol monomer. The polyhydric alcohol monomer is not particularly limited, but is preferably a chain-like (more preferably straight-chain) aliphatic diol, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, 1,4-butanediol, 1,4-butadiene glycol, trimethylene glycol, tetramethylene glycol, pentamethylene glycol, hexamethylene glycol, octamethylene glycol, nonamethylene glycol, decamethylene glycol, and neopentyl glycol. Among these, particularly preferred examples are straight-chain aliphatic α,ω-diols such as ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,6-hexanediol.

[0070] Polyhydric alcohol monomers other than the above polyhydric alcohols can also be used. Among the alcohol monomers, examples of the dihydric alcohol monomer include aromatic alcohols such as polyoxyethylenated bisphenol A and polyoxypropylenated bisphenol A; 1,4-cyclohexanedimethanol, etc. Among the polyhydric alcohol monomers, examples of the trihydric or higher polyhydric alcohol monomers include aromatic alcohols such as 1,3,5-trihydroxymethylbenzene; and aliphatic alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, etc.

[0071] The polycarboxylic acid monomer used in the crystalline polyester may be the following polycarboxylic acid monomer. The polycarboxylic acid monomer is not particularly limited, but is preferably a chain (more preferably a linear) aliphatic dicarboxylic acid. Specific examples include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid, as well as hydrolyzates of these acid anhydrides or lower alkyl esters.

[0072] Polycarboxylic acids other than the above polycarboxylic acid monomers can also be used. Among the other polycarboxylic acid monomers, examples of dicarboxylic acids include aromatic carboxylic acids such as isophthalic acid and terephthalic acid, aliphatic carboxylic acids such as n-dodecylsuccinic acid and n-dodecenylsuccinic acid, and alicyclic carboxylic acids such as cyclohexanedicarboxylic acid, and also include their acid anhydrides and lower alkyl esters.

[0073] Furthermore, among the other carboxylic acid monomers, examples of polyvalent carboxylic acids having a valence of three or more include aromatic carboxylic acids such as 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and pyromellitic acid, and aliphatic carboxylic acids such as 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, and 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, as well as derivatives such as their acid anhydrides and lower alkyl esters.

[0074] From the viewpoints of electrostatic charge and dispersion effect of the graft polymer (A) in the release agent, the crystalline polyester is preferably a modified crystalline polyester having a structure in which a hydroxy group at the end of the main chain is condensed (terminally modified) with an aliphatic monocarboxylic acid having 16 to 31 carbon atoms (preferably 18 to 24 carbon atoms), or a modified crystalline polyester having a structure in which a carboxy group at the end of the main chain is condensed (terminally modified) with an aliphatic monoalcohol having 15 to 30 carbon atoms (preferably 17 to 23 carbon atoms). It is believed that modification of the main chain end with a hydroxyl group or the like suppresses charge leakage and improves charging properties. In addition, within the above range of carbon number, the inhibition of adsorption of the crystalline polyester to the release agent caused by excessive interaction between the polyolefin portion of the graft polymer (A) and the crystalline polyester can be avoided, and the dispersibility of the release agent becomes better.

[0075] Examples of aliphatic monocarboxylic acid monomers having 16 to 31 carbon atoms include palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), nonadecylic acid, arachidic acid (icosanoic acid), henicosanoic acid, docosanoic acid (behenic acid), tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid. Examples of aliphatic monoalcohols having 15 to 30 carbon atoms include palmityl alcohol (hexadecanol), margaryl alcohol (heptadecanol), stearyl alcohol (octadecanol), nonadecanol, arachidyl alcohol (icosanol), heneicosanol, behenyl alcohol, lignoceryl alcohol, ceryl alcohol, 1-heptacosanol, montanyl alcohol, 1-nonacosanol, and myricyl alcohol. can be done.

[0076] The content of the crystalline polyester is preferably 3 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the amorphous polyester from the viewpoints of low-temperature fixability, abrasion resistance, and chargeability retention in a high-temperature and high-humidity environment.

[0077] The crystalline polyester can be produced according to a conventional polyester synthesis method. For example, the carboxylic acid monomer and the alcohol monomer are subjected to an esterification reaction or an ester exchange reaction, and then the crystalline polyester can be obtained by carrying out a polycondensation reaction according to a conventional method under reduced pressure or by introducing nitrogen gas. Thereafter, at least one selected from the group consisting of the aliphatic monocarboxylic acid and the aliphatic monoalcohol is added to carry out an esterification reaction, thereby obtaining the desired crystalline polyester.

[0078] The above esterification or transesterification reaction can be carried out, if necessary, using a common esterification catalyst or transesterification catalyst such as sulfuric acid, titanium butoxide, dibutyltin oxide, manganese acetate, magnesium acetate, etc.

[0079] The polycondensation reaction can be carried out using a conventional polymerization catalyst, such as titanium butoxide, dibutyltin oxide, tin acetate, zinc acetate, tin disulfide, antimony trioxide, germanium dioxide, etc. The polymerization temperature and the amount of catalyst are not particularly limited and may be appropriately determined.

[0080] In the esterification or transesterification reaction or polycondensation reaction, in order to increase the strength of the resulting crystalline polyester, it is possible to use a method in which all of the monomers are charged at once, or in order to reduce the amount of low molecular weight components, a divalent monomer is first reacted, and then a trivalent or higher monomer is added and reacted.

[0081] <Coloring agent> The toner particles may contain a colorant as necessary. Examples of the colorant include the following. Examples of the black colorant include carbon black; and a colorant toned to black using a yellow colorant, a magenta colorant, and a cyan colorant. As the colorant, a pigment may be used alone, or a dye and a pigment may be used in combination. From the viewpoint of the image quality of a full-color image, it is preferable to use a dye and a pigment in combination.

[0082] Magenta toner pigments include the following: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0083] Dyes for magenta toner include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28. A basic dye.

[0084] Examples of pigments for cyan toners include: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45, copper phthalocyanine pigments with 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton. Examples of dyes for cyan toners include CI Solvent Blue 70.

[0085] Yellow toner pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. Yellow toner dyes include CI Solvent Yellow 162.

[0086] These colorants can be used alone or in combination, or in the form of a solid solution. The colorant is selected in consideration of hue angle, chroma, brightness, light resistance, OHP transparency, and dispersibility in toner particles. The content of the colorant is preferably 0.1 to 30.0 parts by mass based on the total amount of the resin components.

[0087] <Charge control agent> The toner particles may contain a charge control agent as necessary. By blending a charge control agent, the charge characteristics can be stabilized, and the amount of triboelectric charge can be optimally controlled according to the development system. As the charge control agent, a known one can be used, but in particular, a metal compound of an aromatic carboxylic acid is preferred, which is colorless, has a high charging speed of the toner, and can stably maintain a constant amount of charge.

[0088] Examples of negative charge control agents include metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate or sulfonate ester on the side chain, polymeric compounds having carboxylate or carboxylate ester on the side chain, boron compounds, urea compounds, silicon compounds, and calixarenes.

[0089] The charge control agent may be added internally or externally to the toner particles. The content of the charge control agent is preferably 0.2 parts by mass to 10.0 parts by mass, and more preferably 0.5 parts by mass to 10.0 parts by mass, based on 100 parts by mass of the binder resin.

[0090] <Inorganic fine particles> The toner may contain inorganic fine particles as necessary. The inorganic fine particles may be added internally to the toner particles, or may be mixed with the toner particles as an external additive. Examples of the inorganic fine particles include silica fine particles, titanium oxide fine particles, alumina fine particles, and composite oxide fine particles thereof. Among the inorganic fine particles, silica fine particles and titanium oxide fine particles are preferred for improving flowability and uniform charging. The inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof.

[0091] From the viewpoint of improving fluidity, inorganic fine particles as external additives should have a specific surface area of ​​50 m 2 / g~400m 2 From the viewpoint of improving durability and stability, it is preferable that the inorganic fine particles as the external additive have a specific surface area of ​​10 m 2 / g~50m 2 / g is preferred. In order to achieve both improved fluidity and durability and stability, inorganic fine particles having a specific surface area within the above range may be used in combination.

[0092] The content of the external additive is preferably 0.1 parts by mass to 10.0 parts by mass with respect to 100 parts by mass of the toner particles. The toner particles and the external additive can be mixed using a known mixer such as a Henschel mixer.

[0093] <Magnetic carrier> The toner can be used as a one-component developer, but in order to further improve dot reproducibility and provide stable images over a long period of time, it is preferable to use the toner as a two-component developer by mixing it with a magnetic carrier. The toner is preferably a toner for use in a two-component developer. The two-component developer contains a toner and a magnetic carrier, and the toner is preferably the toner described above.

[0094] Examples of magnetic carriers that can be used include generally known magnetic carriers, such as iron oxide; metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, strontium, and rare earth elements, alloy particles thereof, and oxide particles thereof; magnetic materials such as ferrite and magnetite; magnetic material-dispersed resin carriers (so-called resin carriers) containing a magnetic material and a binder resin that holds the magnetic material in a dispersed state; and magnetic carriers in the form of ferrite or magnetite particles having holes filled with resin.

[0095] As the magnetic carrier, the above magnetic material may be used directly, or a magnetic material obtained by using the above magnetic material as a core and coating the surface of the core with a resin may be used. From the viewpoint of improving the chargeability of the toner, it is preferable to use the above magnetic material as the magnetic carrier.

[0096] The resin that coats the core is not particularly limited, and any known resin can be selected and used as long as it does not impair the toner properties. For example, resins such as (meth)acrylic resin, silicone resin, urethane resin, polyethylene, polyethylene terephthalate, polystyrene, and phenolic resin, or copolymers or polymer mixtures containing these can be used. From the viewpoint of charging characteristics and prevention of adhesion of foreign matter to the carrier surface, it is preferable to use a (meth)acrylic resin or a silicone resin. In particular, a (meth)acrylic resin having an alicyclic hydrocarbon group such as a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclopentyl group, a cyclobutyl group, or a cyclopropyl group is particularly preferable because it makes the surface (coating surface) of the resin coating layer that covers the surface of the magnetic material smooth and can suppress adhesion of toner-derived components such as binder resins, release agents, and external additives.

[0097] <Developer> When the toner is mixed with a magnetic carrier to be used as a two-component developer, the mixing ratio of the magnetic carrier is preferably 2% by mass to 15% by mass, and more preferably 4% by mass to 13% by mass, in terms of the toner concentration in the two-component developer.

[0098] <Toner manufacturing method> The method for producing the toner is not particularly limited, and any known method such as a pulverization method, a suspension polymerization method, a dissolution suspension method, an emulsion aggregation method, or a dispersion polymerization method can be used. The procedure for producing toner by the pulverization method will be described below. The pulverization method includes, for example, a raw material mixing step of mixing an amorphous polyester as a binder resin, a release agent, a graft polymer (A), and other components such as a crystalline polyester, a colorant, and a charge control agent as required, a step of melting and kneading the mixed raw materials to obtain a resin composition, and a step of pulverizing the obtained resin composition to obtain toner particles. The method includes the steps of:

[0099] In the raw material mixing process, materials constituting the toner particles, such as amorphous polyester (binder resin), release agent, graft polymer (A), and other components such as crystalline polyester, colorant, charge control agent, etc. as required, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include double con mixers, V-type mixers, drum mixers, super mixers, Henschel mixers, Nauta mixers, and Mechano Hybrids (manufactured by Nippon Coke & Engineering Co., Ltd.).

[0100] Next, the mixed materials are melt-kneaded to disperse the release agent in the binder resin. In the melt-kneading process, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of continuous production. For example, a KTK twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with two rolls or the like and cooled with water or the like in a cooling process.

[0101] The cooled resin composition is then pulverized to a desired particle size in a pulverization process. In the pulverization process, the resin composition is coarsely pulverized using a pulverizer such as a crusher, a hammer mill, or a feather mill. The resin composition is then finely pulverized using a pulverizer such as a Cryptron System (Kawasaki Heavy Industries), a Super Rotor (Nisshin Engineering), a Turbo Mill (Turbo Kogyo), or an air jet type pulverizer.

[0102] Thereafter, as necessary, the mixture is classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation).

[0103] The obtained toner particles may be used as a toner as it is. If necessary, an external additive may be added to the surface of the toner particles to obtain a toner. As a method for adding an external additive, a method may be used in which the classified toner and various known external additives are mixed in a predetermined amount and stirred and mixed using a mixing device such as a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), or a Nobilta (manufactured by Hosokawa Micron Corporation) as an external additive machine.

[0104] The methods for measuring various physical properties of the toner and raw materials are described below. (Method of separating each material from toner) By utilizing the difference in solubility of each material contained in the toner in a solvent, each material can be separated from the toner. First separation: The toner is dissolved in methyl ethyl ketone (MEK) at 23° C., and the soluble matter (amorphous polyester, crystalline polyester, release agent, graft polymer (A), colorant) is separated from the insoluble matter (inorganic fine particles, etc.). Second separation: The soluble fraction (amorphous polyester, crystalline polyester, release agent, graft polymer (A), colorant) obtained in the first separation is dissolved in tetrahydrofuran (THF) at 23°C, and the insoluble fraction (amorphous polyester, graft polymer (A), colorant) and the soluble fraction (crystalline polyester, release agent) are separated. Third separation: The soluble matter (crystalline polyester, release agent) obtained in the second separation is dissolved in hexane at 23°C, and the soluble matter (release agent) is separated from the insoluble matter (crystalline polyester). In addition, the insoluble matter obtained in the second separation (amorphous polyester, graft polymer (A), colored The agent was dissolved in chloroform and subjected to preparative HPLC (Japan Analytical Industry Co., Ltd. LC-9130 NEXT The fraction is collected using a preparative column (60 cm).

[0105] <Maximum heat generation peak temperature of release agent T Wax , the highest exothermic peak temperature T of the graft polymer (A) Max、 The lowest heat peak temperature T Min Measurements > Maximum heat generation peak temperature T of release agent Wax , the highest exothermic peak temperature T of the graft polymer (A) Max、 The lowest heat peak temperature T Min is measured in accordance with ASTM D3418-82 using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the device detection unit, and the heat of fusion of indium is used for heat correction. Specifically, 3 mg of the release agent or graft polymer (A) is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and the temperature-endothermic curve is measured under the following conditions.

[0106] Heating rate: 10℃ / min Measurement start temperature: 30℃ End of measurement temperature: 180℃ Measurements are performed in the range of 30 to 180°C at a heating rate of 10°C / min. The temperature is raised to 180°C once and held for 10 minutes, after which the temperature-heating curve is measured under the following conditions. Cooling rate: 10℃ / min Measurement start temperature: 180℃ End of measurement temperature: 30℃ From the exothermic peak temperature of the temperature-exothermic amount curve obtained during this temperature drop, the exothermic peak temperature T Wax , the highest exothermic peak temperature T of the graft polymer (A) Max、 The lowest heat peak temperature T Min get.

[0107] <Method of measuring the ratio (PE / PP) of the number of moles of ethylene structure (PE) to the number of moles of propylene structure (PP) in the polyolefin portion of the graft polymer (A)> The ratio (PE / PP) of the number of moles of ethylene structure (PE) to the number of moles of propylene structure (PP) in the polyolefin portion of the graft polymer (A) is measured by: 1 H-NMR, 13 C-NMR was performed under the following conditions. Measuring device: FT NMR device JNM-EX400 (manufactured by JEOL Ltd.) Measurement frequency: 400MHz ( 13 C-NMR: 125MHz) Pulse condition: 5.0μs Frequency range: 10500Hz Number of times: 64 Measurement temperature: 30℃ Sample: 50 mg of the measurement sample is placed in a sample tube with an inner diameter of 5 mm, deuterated chloroform (CDCl3) is added as a solvent, and this is dissolved in a constant temperature bath at 40°C to prepare the sample.

[0108] Obtained 1 H-NMR, 13 From the C-NMR chart, the integral value S of the peaks assigned to the ethylene structure (PE) and propylene structure (PP), which are the components in the polyolefin portion of the graft polymer (A), is PE、 S PP Calculate. The ratio (PE / PP) of the moles of the ethylene structure (PE), which is a component of the polyolefin portion, to the moles of the propylene structure (PP) is expressed by the integral value S PE、 S PP The number of moles of each is calculated using the number of hydrogen atoms in the constituent elements to be assigned. In addition, a more detailed structural analysis can be performed using a two-quantum filter. 1 H- 1 H shift-correlated two-dimensional NMR measurements (DQF-COSY) and other techniques are performed to identify the detailed structure from the obtained spectra. Similarly, the structure of the polyolefin can be determined during the production of the polyolefin.

[0109] <Method of measuring acid value and weight average molecular weight of polyolefin part of graft polymer (A) in toner> The acid value of the polyolefin portion in the graft polymer (A) in the toner and the weight average molecular weight of the polyolefin portion are calculated in the same manner as in the calculation of the (PE / PP) ratio of the polyolefin portion described above. 1 H-NMR, 13 C-NMR, 1 H-NMR, 13 Calculations are made using the results of C-NMR and DQF-COSY. The acid value and weight average molecular weight of the graft polymer (A) itself isolated by the above "Method for separating each material from the toner" can be measured by the following neutralization titration and GPC.

[0110] <Method of measuring acid value of graft polymer (A)> The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of the graft polymer (A) is measured in accordance with JIS K 0070-1992, and specifically, is measured according to the following procedure. (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 ml of ethyl alcohol (95% by volume) and add ion-exchanged water to make 100 ml to obtain a phenolphthalein solution. Dissolve 7 g of special grade potassium hydroxide in 5 ml of water and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is determined by placing 25 ml of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution, from the amount of potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0111] (2) Operation (A) Main Test A 2.0 g sample of the graft polymer (A) is weighed out accurately in a 200 ml Erlenmeyer flask, and 100 ml of a mixed solution of toluene / ethanol (2:1) is added and dissolved over 5 hours. Then, several drops of the phenolphthalein solution are added as an indicator, and titration is performed using the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used). (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the addition amount (ml) of the potassium hydroxide solution in the blank test, C is the addition amount (ml) of the potassium hydroxide solution in this test, f is the factor of the potassium hydroxide solution, and S is the mass (g) of the sample.

[0112] <Measurement of the weight-average molecular weight of the graft polymer (A) by GPC> The weight-average molecular weight (Mw) of the o-dichlorobenzene-soluble component of the graft polymer (A) at 100 °C is measured by gel permeation chromatography (GPC) as follows. First, crystalline polyester C is dissolved in o-dichlorobenzene at 100 °C over 1 hour. Then, the resulting solution is filtered through a solvent-resistant membrane filter "MAESORIDISC" (manufactured by Tosoh Corporation) with a pore diameter of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of the components soluble in o-dichlorobenzene is 0.1% by mass. Using this sample solution, the measurement is carried out under the following conditions. Apparatus: HLC-8121GPC / HT (manufactured by Tosoh Corporation) Column: TSKgel GMHHR-H HT (7.8 cm I.D × 30 cm) in series (manufactured by Tosoh Corporation) Detector: RI for high temperature Temperature: 135 °C Solvent: o-dichlorobenzene Flow rate: 1.0 mL / min Sample: Inject 0.4 mL of a 0.1% sample. When calculating the molecular weight of the sample, a molecular weight calibration curve prepared with a monodisperse polystyrene standard sample is used. Furthermore, it is calculated by performing polyethylene conversion using a conversion formula derived from the Mark-Houwink viscosity equation. Also, in the same way, the weight-average molecular weight of the polyolefin in the manufacturing process is calculated.

[0113] <Content of crystalline polyester, content of release agent, and content of graft polymer (A) in toner> Based on the mass of each material separated by the above-mentioned "method for separating each material from toner", the content can be calculated.

[0114] <Calculation of the SP value of each segment of the amorphous polyester block copolymer, and the SP value of the styrene acrylic polymer portion of the graft polymer> The SP value of each segment of the amorphous polyester block copolymer and the SP value of the styrene acrylic polymer portion of the graft polymer are calculated as follows according to the calculation method proposed by Fedors. For the atoms or atomic groups in the molecular structure, the evaporation energy (Δei) (cal / mol) and molar volume (Δvi) (cm) are calculated from the table in "Polym. Eng. Sci., 14(2), 147-154 (1974)". 3 / mol), (ΣΔei / ΣΔvi) 0.5 SP value (cal / cm 3 ) 0.5 Let us assume that. The unit of SP value is 1 (cal / cm 3 ) 0.5 =2.045(J / cm 3 ) 0.5 It can be converted by: EXAMPLES

[0115] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In the following formulations, the parts are by weight unless otherwise specified.

[0116] [Example 1] <Production of polyolefin a-1> (Catalyst Adjustment) Production of supported metallocene catalysts A 2000 ml reactor purged with nitrogen gas was charged with 87.5 ml (0.25 mol in terms of Al atoms) of a toluene solution of methylaluminoxane (concentration: 3 mol / l, product name: PMAO, manufactured by Toso Akzo Co., Ltd.) and 1.0 mmol of a mixture of chiral dimethylsilylene(2,3,5-trimethylcyclopentadienyl)(2',4',5'-trimethylcyclopentadienyl)zirconium dichloride and its meso isomer, dimethylsilylene(2,3,5-trimethylcyclopentadienyl)(2',3',5'-trimethylcyclopentadienyl)zirconium dichloride (meso isomer content 1 mol%) as a bridged metallocene compound, and the mixture was kept at 25°C for 30 minutes with stirring to cause a reaction, yielding a reaction product of the metallocene compound and aluminoxane.

[0117] Next, 25 g of silica (SYLOPOL(R)948, manufactured by Grace Davison Co.) with an average particle size of 51 μm, which had been calcined at 750°C for 8 hours in a reduced pressure atmosphere, was added to the reactor, and the temperature of the reactor was raised to 100°C. The temperature was then kept for 1 hour under stirring to dissolve the reaction product and silica obtained above. A contact reaction with moss was carried out to obtain a slurry containing a solid product carrying the reaction product. After the temperature of the reactor was cooled to -10°C, 1000 ml of n-hexane was added and stirred for 5 minutes, after which the stirring was stopped and the solvent was separated by decantation.

[0118] Subsequently, while maintaining the temperature of the reactor at -10°C, 1 liter of n-hexane was added to the reactor and stirred and washed for 5 minutes, then the stirrer was stopped and the washing solvent was separated by decantation, and the washing operation was repeated to obtain a solid product, a metallocene-supported catalyst, on which the reaction product of the metallocene compound and the aluminoxane was supported. Furthermore, 500 ml of n-hexane was added to the reactor to disperse the metallocene-supported catalyst and form a slurry.

[0119] (Preparation of pre-activated catalyst) 1000 ml of n-hexane was placed in a nitrogen-purged stainless steel reactor having an internal volume of 2000 ml, and the prepared slurry containing the metallocene supported catalyst was placed in the reactor while the temperature of the reactor was maintained at 0° C. Next, while maintaining the temperature of the reactor at 0° C., propylene gas was supplied at a supply rate of 0.03 mol / min for 30 minutes to polymerize the propylene homopolymer, which was supported on the metallocene supported catalyst. During this polymerization reaction, unreacted propylene gas was discharged outside the reactor. After the polymerization time had elapsed, the supply of propylene gas was stopped, and the reactor temperature was then raised to 25°C while the gas phase of the reactor was replaced with nitrogen and the solvent was separated by decantation. The pre-activated catalyst obtained was washed with n-hexane and finally dispersed in 1000 ml of toluene to make the pre-activated catalyst into a slurry.

[0120] (Polyolefin Polymerization) The polymerization of polyolefin was carried out in two stages. In the first stage, 500 ml of toluene was charged into a 1000 ml glass autoclave that had been thoroughly purged with nitrogen, and a mixed gas of ethylene (PE) 15 L / hr, propylene (PP) 5 L / hr, and oxygen gas 20 ml / hr were fed to saturate the liquid and gas phases. Then, 5 ml of the slurry in which the pre-activated catalyst was dispersed in the above toluene and 1.25 mmol of methylaluminoxane in terms of aluminum atom were added to start the polymerization. The polymerization was carried out at 50°C for 1 minute. In the second step, the mixture ratio was changed to 18 liters / hr of ethylene and 2 liters / hr of propylene, and polymerization was carried out for 3 minutes, after which a small amount of isobutanol was added to terminate the polymerization. The resulting polymer solution was added to 1.5 liters of methanol containing a small amount of hydrochloric acid to precipitate polyolefin a-1. The precipitated polyolefin a-1 was washed with methanol and dried under reduced pressure.

[0121] The resulting polyolefin a-1 had a weight average molecular weight (Mn) of 1950, a ratio of the number of moles of ethylene structure (PE) to the number of moles of propylene structure (PP) (PE / PP) of 9, and an acid value of 1.0 mgKOH / g.

[0122] <Production of polyolefins a-2 to a-15> Polyolefins a-2 to a-15 were obtained by carrying out the reaction in the same manner as in the production example of polyolefin a-1, except that the gas ratios and polymerization times in the first and second stages were changed as shown in Table 1. The physical properties are shown in Table 2. [Table 1]

[0123] [Table 2] The unit of acid value is mgKOH / g.

[0124] <Production of Graft Polymer (A)b-1> Polyolefin a-1: 10.0 parts by mass Xylene: 25.0 parts by weight The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. The atmosphere in the flask was then replaced with nitrogen gas, and the temperature was gradually raised to 175°C while stirring. Styrene: 78.0 parts by weight Butyl acrylate (BA): 8.25 parts by weight Methacrylic acid (МAA): 3.75 parts by weight Xylene: 10.0 parts by weight Di-t-butylperoxyhexahydroterephthalate: 0.5 parts by mass The above material was then added dropwise over 3 hours and stirred for an additional 30 minutes.The solvent was then distilled off to obtain a graft polymer (A) b-1.

[0125] The obtained graft polymer (A)b-1 had a maximum exothermic peak temperature T Max is 68.8℃, the lowest heat peak temperature T Min is 62.1℃, T Max -T MinThe temperature was 6.7°C. The acid value was 23.7 mgKOH / g. The weight average molecular weight was 19,500. The SP value was 10.55 [J / cm 3 ] 0.5 It was.

[0126] <Production of Graft Polymers (A) b-2 to b-19> Graft polymers (A) b-2 to b-19 were obtained by carrying out the reaction in the same manner as in the production example of graft polymer (A) b-1, except that the types of polyolefins and the types and ratios of styrene / acrylic resins were changed as shown in Table 3. The physical properties are shown in Table 4. [Table 3]

[0127] [Table 4]

[0128] <Production example of amorphous polyester c-1> (Production Example of Segment 1 of Amorphous Polyester c-1) Propylene oxide adduct of bisphenol A (average number of moles added: 2.2 mol) : 4.5 parts by mass (34.1 mol%) Ethylene oxide adduct of bisphenol A (average number of moles added: 2.2 mol) : 27.7 parts by mass (22.7 mol%) ·Terephthalic acid: 26.5 parts by mass (42.6mol%) ·Fumaric acid: 0.2 parts by mass (0.5mol%) The above materials were weighed into a reaction vessel equipped with a stirrer that had been thoroughly heated and dried. 0.5 parts by mass of tin 2-ethylhexanoate (esterification catalyst) was added to 100 parts by mass of the above mixture, and the vessel was heated to 260°C while introducing nitrogen gas into the vessel to maintain an inert atmosphere, and segment 1 of amorphous polyester c-1 was polymerized. The SP value was 10.8 [J / cm 3 ] 0.5 It was.

[0129] (Production Example of Segment 2 of Amorphous Polyester c-1) Ethylenediol: 20.7 parts by mass (41.2 mol%) Terephthalic acid: 79.3 parts by mass (58.8 mol%) The above materials were weighed into a reaction vessel equipped with a stirrer that had been thoroughly heated and dried. 0.5 parts by mass of tin 2-ethylhexanoate (esterification catalyst) was added to 100 parts by mass of the above mixture, and the vessel was heated to 200°C while nitrogen gas was introduced into the vessel to maintain an inert atmosphere, and segment 2 of amorphous polyester c-1 was polymerized. The SP value was 12.7 [J / cm 3 ] 0.5 Therefore, the SP value difference between segment 1 and segment 2 of the amorphous polyester c-1 was 1.9 [J / cm 3 ] 0.5 It became.

[0130] Segment 1 of amorphous polyester c-1: 89.3 parts by mass (50.0 mol%) Segment 2 of amorphous polyester c-1: 10.7 parts by mass (50.0 mol%) The above materials were put into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen introduction tube, and a thermocouple. Then, 0.5 parts by mass of tin 2-ethylhexanoate (esterification catalyst) was added as a catalyst for 100 parts by mass of the total amount of segments. Next, the flask was purged with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 2.5 hours while stirring at a temperature of 200°C. Furthermore, the pressure in the reaction vessel was reduced to 8.3 kPa, and after maintaining it for 1 hour, it was cooled to 180°C and returned to atmospheric pressure. A block polymer, amorphous polyester c-1, was obtained.

[0131] <Production Example of Amorphous Polyester c-2> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 73.2 parts by mass (56.0 mol%) Terephthalic acid: 26.6 parts by mass (43.7 mol%) Trimellitic anhydride: 0.2 parts by mass (0.3 mol%) Titanium tetrabutoxide (esterification catalyst): 0.5 parts by mass The above materials were weighed into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 5 hours while stirring at a temperature of 200°C. After confirming that the softening point reached a temperature of 96°C, the temperature was lowered to stop the reaction, and amorphous polyester c-2 was obtained.

[0132] <Production Example of Crystalline Polyester d-1> Ethylene glycol: 18.2 parts by mass (48.8 mol%) Tetradecanedioic acid: 71.9 parts by mass (46.3 mol%) ·Behenic acid: 10.0 parts by mass (4.9 mol%) Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 2 hours at a temperature of 200°C with stirring. The pressure in the reaction vessel was then lowered to 8.3 kPa, and the reaction was continued for 5 hours while maintaining the temperature at 200° C. After that, the reaction was stopped by lowering the temperature to obtain crystalline polyester d-1. The melting point was 90° C.

[0133] <Production Example of Crystalline Polyester d-2> Hexanediol: 35.5 parts by mass (51.8 mol%) Dodecanedioic acid: 63.8 parts by mass (47.8 mol%) ·Behenic acid: 0.7 parts by mass (0.4 mol%) Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 2 hours at a temperature of 200°C with stirring. The pressure in the reaction vessel was then lowered to 8.3 kPa, and the reaction was continued for 5 hours while maintaining the temperature at 200° C. The temperature was then lowered to terminate the reaction, yielding crystalline polyester d-2, whose melting point was 68° C.

[0134] <Toner 1 Manufacturing Example> Graft polymer (A) b-1: 5 parts by mass Amorphous polyester c-1: 100 parts by weight Crystalline polyester d-1: 10 parts by weight Release agent W1: 5 parts by weight Fischer-Tropsch wax (weight average molecular weight: 500, exothermic peak temperature 86.6°C) Carbon black: 5 parts by weight The above materials were mixed using a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 1500 rpm for a rotation time of 5 min, and then kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Co., Ltd.) set at a temperature of 130°C. The kneaded product obtained was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The obtained coarsely crushed product was finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). Further, classification was carried out using Faculty (F-300, manufactured by Hosokawa Micron Corporation) to obtain toner particles 1. The operating conditions were a classification rotor rotation speed of 11,000 rpm and a dispersion rotor rotation speed of 7,200 rpm. The SP value difference between the styrene acrylic polymer portion of the graft polymer (A) b-1 and the segment 1 of the amorphous polyester c-1 was 0.25 [J / cm 3 ] 0.5 It became.

[0135] Toner particles 1: 100 parts by weight Silica microparticle A: Fumed silica surface-treated with hexamethyldisilazane (Median diameter (D50) based on number is 120 nm): 4 parts by mass Small inorganic particles: Titanium oxide particles surface-treated with isobutyltrimethoxysilane (Median diameter (D50) based on number is 10 nm): 1 part by mass The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 1900 rpm for a rotation time of 10 minutes to obtain Toner 1 exhibiting negative charging properties.

[0136] <Production of toner 2 to 27> Toners 2 to 27 were obtained by the same production procedure as in the production example of toner 1, except that the types and ratios of graft polymer A, release agent, amorphous polyester, and crystalline polyester were changed as shown in Table 5. The amount of amorphous polyester was also 100 parts by mass in toners 2 to 27. In toner 27, the SP value difference between the styrene acrylic polymer portion of b-19 and segment 1 of amorphous polyester c-1 was 0.40 [J / cm 3 ] 0.5 It became. The toner thus obtained was used in the above-mentioned method. Max , T Min and T Wax When measured, the same results were obtained as for the material used. [Table 5] In the table, the SP value difference A indicates the minimum SP value difference between the SP value of the styrene acrylic polymer portion of the graft polymer (A) and the SP values ​​of two or more different amorphous polyester segments constituting the block copolymer. The SP value difference B indicates the SP value difference between two or more different amorphous polyester segments constituting the block copolymer.

[0137] The release agent types in the table are as follows: W1: Fischer-Tropsch wax (weight average molecular weight 500, exothermic peak temperature 86.6°C) W2: Paraffin wax (weight average molecular weight 300, exothermic peak temperature 75.0°C) W3: Fischer-Tropsch wax (weight average molecular weight 1000, exothermic peak temperature 103.7°C)

[0138] <Magnetic core manufacturing example> Process 1 (weighing and mixing process) Fe2O3: 61.7% by mass MnCO3: 34.2% by mass Mg(OH)2: 3.0% by mass SrCO3: 1.1% by mass The ferrite raw material was weighed so that Thereafter, the mixture was ground and mixed for 2 hours in a dry ball mill using zirconia balls (φ10 mm).

[0139] Step 2 (pre-firing step) After crushing and mixing, the mixture was sintered in air at 950℃ for 2 hours in a burner-type sintering furnace to produce calcined ferrite. The composition of the ferrite is as follows: (MnO) a (MgO) b (SrO) c (Fe2O3) d In the above formula, a = 0.40, b = 0.07, c = 0.01, d = 0.52

[0140] Process 3 (Crushing process) The calcined ferrite was crushed to about 0.5 mm using a crusher, and then 30 parts by mass of water was added to 100 parts by mass of the calcined ferrite, and the mixture was crushed in a wet ball mill using zirconia balls (φ1.0 mm) for 2 hours. After separating the balls, the mixture was crushed in a wet bead mill using zirconia beads (φ1.0 mm) for 3 hours to obtain a ferrite slurry.

[0141] Process 4 (granulation process) To the ferrite slurry, 2.0 parts by mass of polyvinyl alcohol was added as a binder per 100 parts by mass of the calcined ferrite, and the mixture was granulated into spherical particles of 40 μm using a spray dryer (manufacturer: Okawara Kakoki).

[0142] Step 5 (Main firing step) In order to control the sintering atmosphere, the spherical particles were sintered in an electric furnace under a nitrogen atmosphere (oxygen concentration: 1.0% by volume) at 1150° C. for 4 hours.

[0143] Step 6 (sorting step) The aggregated particles were disintegrated, and then sieved through a sieve with 250 μm openings to remove coarse particles, thereby obtaining porous magnetic core particles.

[0144] Process 7 (resin filling process) 100.0 parts by mass of porous magnetic core particles were placed in the stirring vessel of a mixer (NDMV type universal stirrer manufactured by Dalton). While maintaining the temperature at 60°C, nitrogen was introduced while reducing the pressure to 2.3 kPa. The silicone resin solution was added dropwise under reduced pressure so that the resin component amounted to 7.5 parts by mass relative to the porous magnetic core particles. After the addition was completed, stirring was continued for 2 hours. After that, the temperature was raised to 70°C, the solvent was removed under reduced pressure, and the silicone resin composition obtained from the silicone resin solution was filled into the particles of the porous magnetic core particles. After cooling, the filled core particles obtained were transferred to a mixer (a drum mixer UD-AT type manufactured by Sugiyama Heavy Industries Co., Ltd.) having a spiral blade in a rotatable mixing container, and heated to 220°C at a heating rate of 2 (°C / min) under nitrogen atmosphere and normal pressure. The resin was cured by heating and stirring at this temperature for 60 minutes. After heat treatment, low magnetic products were separated by magnetic separation and classified with a sieve with an opening of 150 μm to obtain magnetic cores.

[0145] <Method of producing coating resin> 80 parts by weight of cyclohexyl methacrylate and 20 parts by weight of methyl methacrylate were added to a four-neck flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a rotary stirrer. Further, 100 parts by mass of toluene, 100 parts by mass of methyl ethyl ketone, and 2.0 parts by mass of azobisisovaleronitrile were added. The obtained mixture was kept at 70° C. for 10 hours under a nitrogen gas flow, and after the polymerization reaction was completed, washing was repeated to obtain a coating resin solution (solid content 35% by mass).

[0146] <Production example of coating resin coating liquid> Toluene and methyl ethyl ketone were added to the coating resin solution in a ratio of 1:1 so that the resin solid content ratio was 5% by mass. The resulting mixture was shaken and stirred for 15 minutes using a paint shaker (manufactured by RADIA Co., Ltd.) to obtain a coating resin coating liquid.

[0147] <Magnetic Carrier 1 Manufacturing Example> Using a magnetic core, the coating resin coating liquid was added to a planetary mixer (Nauta Mixer VN type manufactured by Hosokawa Micron Corporation) maintained at a temperature of 60°C under reduced pressure (1.5 kPa) so that the coating resin coating liquid was 3.0 parts by mass as solid content per 100 parts by mass of magnetic core. The method of addition was to add 1 / 3 of the resin coating liquid, and perform solvent removal and coating operations for 20 minutes. Next, another 1 / 3 of the resin coating liquid was added, and solvent removal and coating operations were performed for 20 minutes, and another 1 / 3 of the resin coating liquid was added, and solvent removal and coating operations were performed for 20 minutes.

[0148] The resulting mixture was then transferred to a mixer (UD-AT type drum mixer manufactured by Sugiyama Heavy Industries Co., Ltd.) equipped with a spiral blade in a rotatable mixing container, and heat-treated for 2 hours at 120°C in a nitrogen atmosphere while stirring at 10 revolutions per minute. Low magnetic particles were removed from the resulting mixture by magnetic separation, and the mixture was passed through a sieve with 150 μm openings and then classified with an air classifier to obtain magnetic carrier 1.

[0149] <Production Example of Two-Component Developer 1> 92.0 parts of magnetic carrier 1 and 8.0 parts of toner 1 were mixed in a V-type mixer (V-20, manufactured by Seishin Enterprise Co., Ltd.) to obtain two-component developer 1.

[0150] <Production Examples of Two-Component Developers 2 to 27> In the manufacturing example of the two-component developer 1, the same operation was carried out except that the materials were changed as shown in Table 6, to obtain two-component developers 2 to 27. [Table 6]

[0151] [evaluation] The above two-component developer 1 was used for evaluation. The image forming apparatus used was a modified Canon imagePRESSC810 digital commercial printer, with a two-component developer placed in the cyan developer unit. The apparatus was modified so that the fixing temperature, process speed, developer carrier DC voltage VDC, electrostatic latent image carrier charging voltage VD, and laser power could be freely set.

[0152] In particular, evaluation was performed at a high process speed to demonstrate superior performance in high-speed printing compared to conventional methods. In addition, image output evaluation was performed by outputting a FFh image (solid image) with the desired image ratio, adjusting VDC, VD, and laser power so that the amount of toner on the FFh image on the paper was as desired, and performing the evaluation described below. FFh is defined as 2 This is a hexadecimal value representing 56 gradations, with 00h being the 1st gradation (white background) out of 256 gradations, and FFh being the 256th gradation (solid area) out of 256 gradations.

[0153] [Bleeding of release agent on solid images] ·Paper:CS-064(64.0g / m 2 ) (Sold by Canon Marketing Japan Inc.) Toner load on paper: 1.20mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: A 2cm x 20cm image is placed on the long edge of the A4 paper with a 2mm margin from the leading edge of the paper. Test environment: High temperature and humidity environment: Temperature 30℃ / Humidity 80%RH (hereinafter referred to as "H / H") Fixing temperature: 140℃ to 5℃ increments Process speed: 644mm / sec The above evaluation image was output, and the winding resistance was evaluated at the highest fixing temperature at which winding did not occur according to the following criteria. If the evaluation was A to C, it was judged to be good. (Evaluation Criteria) A: 165℃ or higher B: 155℃ or higher and less than 165℃ C: 145℃ or higher but lower than 155℃ D: Less than 145℃

[0154] [Releasing agent runoff in halftone images] ·Paper:CS-064(64.0g / m 2 ) (Sold by Canon Marketing Japan Inc.) Toner load on paper: 0.08mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: A 2cm x 20cm image is placed on the long edge of the A4 paper with a 2mm margin from the leading edge of the paper. Test environment: Normal temperature and low humidity environment: Temperature 23℃ / Humidity 5%RH (hereinafter referred to as "N / L") Fixing temperature: 140℃ to 5℃ increments Process speed: 644mm / sec The above evaluation images were output, and the run-off property of the release agent in the halftone images was evaluated at the highest fixing temperature at which hot offset did not occur according to the following criteria. If the evaluation was A to C, it was judged to be good. (Evaluation Criteria) A: 200℃ or higher B: 190℃ or higher but less than 200℃ C: 180℃ or higher but lower than 190℃ D: Less than 180℃

[0155] [Abrasion resistance] Paper: Image Coat Gloss 158 (158.0 g / m 2 ) (Sold by Canon Marketing Japan Inc.) Toner load on paper: 0.05mg / cm 2 (2Fh image) (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: 3m x 15cm image placed in the center of the A4 paper. Fixing test environment: Normal temperature and humidity environment (temperature 23°C / humidity 50% RH (hereinafter N / N)) Fixing temperature: 180℃ Process speed: 644mm / sec The above evaluation image was printed out and the abrasion resistance was evaluated. The difference in reflectance was used as the evaluation index for the abrasion resistance. First, the image portion of the evaluation image was rubbed (10 times back and forth) with a new evaluation paper under a load of 0.5 kgf using a Gakushin type abrasion fastness tester (AB-301: manufactured by Tester Sangyo Co., Ltd.). Then, the image portion was rubbed (10 times back and forth) with a new evaluation paper using a reflectometer (REFLECTOMETER MODEL Using a test strip (TC-6DS: manufactured by Tokyo Denshoku Co., Ltd.), the reflectance of the part that has been rubbed with a new evaluation paper and the reflectance of the part that has not been rubbed are measured.

[0156] The difference in reflectance before and after rubbing was calculated using the following formula. The resulting difference in reflectance was evaluated according to the following evaluation criteria. If the evaluation was A to C, it was determined to be good. Reflectance difference = reflectance before friction - reflectance after friction (Evaluation Criteria) A: Less than 1.0% B: 1.0% or more and less than 2.0% C: 2.0% or more and less than 4.0% D: 4.0% or more

[0157] [Charge retention] ·Paper: GFC-081 (81.0g / m 2 )(Canon Marketing Japan Inc.) Toner load on paper: 0.35mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: Place a 2cm x 5cm image in the center of the A4 paper. Fixing test environment: High temperature and humidity environment: Temperature 30℃ / Humidity 80%RH (hereinafter referred to as "H / H") Process speed: 644mm / sec The toner on the electrostatic latent image carrier was collected by suction using a metal cylinder and a cylindrical filter, and the amount of triboelectric charge of the toner was calculated. Specifically, the amount of triboelectric charge of the toner on the electrostatic latent image carrier was measured using a Faraday Cage. A Faraday Cage is a coaxial double cylinder, with the inner and outer cylinders insulated. If a charged body with a charge Q is placed inside the inner cylinder, electrostatic induction will result in the same effect as if a metal cylinder with a charge Q exists. The amount of induced charge was measured using an electrometer (Kessley 6517A, Kessley), and the amount of charge Q (mC) divided by the mass M (kg) of the toner in the inner cylinder (Q / M) was determined as the amount of triboelectric charge of the toner. Triboelectric charge of toner (mC / kg)=Q / M First, the above evaluation image was formed on an electrostatic latent image carrier, and before it was transferred to the intermediate transfer body, the rotation of the electrostatic latent image carrier was stopped, and the toner on the electrostatic latent image carrier was sucked and collected using a metallic cylindrical tube and a cylindrical filter, and the [initial Q / M] was measured.

[0158] Next, the developer was left in the evaluation machine in a H / H environment for two weeks, and then the same operations as before the leaving were performed to measure the charge amount Q / M (mC / kg) per unit mass on the electrostatic latent image carrier after leaving it. The initial Q / M per unit mass on the electrostatic latent image carrier was set as 100%, and the maintenance rate of Q / M per unit mass on the electrostatic latent image carrier after leaving it ([Q / M after leaving it] / [initial Q / M]×100) was calculated and judged according to the following criteria. If the evaluation was A to C, it was judged to be good. (Evaluation Criteria) A: Retention rate is 95% or higher B: Retention rate is between 90% and 95% C: Retention rate is between 85% and 90% D: Retention rate is less than 85%

[0159] [Dispersibility of release agent (F / M)] The resin particles classified in the classification step of the production example of toner 1 and the fine particle-side powder separated from the resin particles and recovered were used to measure the endothermic heat (ΔH) of the maximum endothermic peak derived from the release agent. The ΔH of the resin particles is M, and the ΔH of the fine particle powder is F, and the dispersibility of the release agent is evaluated by the value obtained by dividing F by M (F / M). If the release agent is not finely dispersed and exists in the kneaded material as large domains, the domains become the grinding interface during the grinding process, and the domains of the release agent are liberated from the resin. The liberated release agent is recovered as fine particle powder in the classification process, so if the dispersibility of the release agent is low, the release agent that formed domains is recovered in the fine particle powder.

[0160] Therefore, the dispersibility of the release agent was evaluated by comparing the endothermic heat (ΔH) of the maximum endothermic peak originating from the release agent of the resin particles and the fine particle side powder, and judged according to the following evaluation criteria. If the evaluation was A to C, it was judged to be good. (Evaluation Criteria) A: F / M is 1.00 or more and less than 1.05 B: F / M is 1.05 or more and less than 1.10 C: F / M is 1.10 or more and less than 1.20 D: F / M is 1.20 or higher

[0161] [Low temperature fixability] The low temperature fixability was evaluated under the following conditions. ·Paper: GFC-081 (81.0g / m 2 ) (Sold by Canon Marketing Japan Inc.) Toner load on paper: 0.90mg / cm 2 (Adjusted by DC voltage VDC of developer carrier, charging voltage VD of electrostatic latent image carrier, and laser power) Evaluation image: Place a 2cm x 5cm image in the center of the A4 paper. Test environment: Low temperature and low humidity environment: Temperature 15℃ / Humidity 10%RH (hereinafter referred to as "L / L") Fixing temperature: 140℃ Process speed: 435mm / sec The above evaluation image was output, and the low-temperature fixing property was evaluated. The image density reduction rate was used as an evaluation index for the low-temperature fixing property.

[0162] The image density reduction rate was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite Corporation). First, the image density in the center was measured. Next, the area where the image density was measured was subjected to 4.9 kPa (50 g / cm 2 The fixed image is rubbed (five times back and forth) with Silbon paper under a load of 1000 g / m2, and the image density is measured again. The rate of decrease in image density before and after rubbing was calculated using the following formula. The rate of decrease in image density obtained was evaluated according to the following evaluation criteria. If the evaluation was A to C, it was judged to be good. Image density reduction rate = (Image density before rubbing - Image density after rubbing) / (Image density before rubbing) x 100 (Evaluation Criteria) A: Image density reduction rate is less than 3.0% B: Image density reduction rate: 3.0% or more and less than 5.0% C: Image density reduction rate: 5.0% or more and less than 8.0% D: Image density reduction rate 8.0% or more The evaluation results are shown in Table 7.

[0163] <Examples 2 to 22 and Comparative Examples 1 to 4> The evaluation was carried out in the same manner as in Example 1, except that two-component developer 2 to two-component developer 27 were used. The evaluation results are shown in Table 7.

[0164] [Table 7]

[0165] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles containing a binder resin, a release agent, and a graft polymer (A), The binder resin contains an amorphous polyester, the graft polymer (A) has two or more exothermic peaks in an exothermic curve during cooling measured by differential scanning calorimetry, The release agent has at least one exothermic peak in an exothermic curve during a temperature drop measured by differential scanning calorimetry, The peak temperature of the highest exothermic peak of the graft polymer (A) is designated as T Max (℃), and the peak temperature of the lowest exothermic peak is T Min (°C), and the peak temperature of the maximum exothermic peak among the exothermic peaks of the release agent is T Wax (℃), The T Max , the T Min And the T Wax satisfies the following formulas (1) and (2): A toner characterized by: 5.0≦T Max -T Min ≦20.0 (1) 10.0≦T Wax -T Max ≦40.0 (2) (Configuration 2) The toner according to configuration 1, wherein the graft polymer (A) is a graft polymer having a polyolefin portion and a styrene-acrylic polymer portion. (Configuration 3) The polyolefin portion is (i) a copolymer of ethylene and propylene; (ii) having a moiety having an acid group; (iii) The toner according to configuration 2, wherein the ratio of the number of moles of the ethylene structure PE to the number of moles of the propylene structure PP (PE / PP) is 4 to 20. (Configuration 4) The toner according to configuration 2 or 3, wherein the polyolefin portion of the graft polymer (A) has a weight average molecular weight of 1,000 to 3,000. (Configuration 5) 5. The toner according to any one of configurations 2 to 4, wherein the acid value of the polyolefin portion is 0.5 to 16.0 mgKOH / g. (Configuration 6) The toner according to any one of configurations 1 to 5, wherein the acid value of the graft polymer (A) is 15.0 to 40.0 mgKOH / g. (Configuration 7) 7. The toner according to any one of Configurations 1 to 6, wherein the toner contains 3 to 20 parts by mass of a crystalline polyester per 100 parts by mass of the amorphous polyester. (Configuration 8) The toner according to any one of Configurations 1 to 7, wherein the toner contains 1 to 20 parts by mass of the release agent and 1 to 20 parts by mass of the graft polymer (A) per 100 parts by mass of the amorphous polyester. (Configuration 9) the amorphous polyester is a block copolymer having two or more different amorphous polyester segments, Regarding the difference between the SP value of two or more different amorphous polyester segments constituting the block copolymer and the SP value of the styrene acrylic polymer portion of the graft polymer (A), The minimum SP value difference is 1.00 [J / cm 3 ] 0.5 Within The difference in SP value between the two or more different amorphous polyester segments constituting the block copolymer is 1.0 [J / cm 3 ] 0.5 The toner according to any one of Configurations 1 to 8, wherein: (Configuration 10) The toner according to any one of configurations 1 to 9, wherein the release agent comprises a hydrocarbon wax. (Configuration 11) A two-component developer, The two-component developer contains a toner and a magnetic carrier, A two-component developer, wherein the toner is the toner according to any one of configurations 1 to 10.

Claims

1. A toner having toner particles containing a binder resin, a release agent, and a graft polymer (A), The binder resin contains an amorphous polyester, the graft polymer (A) has two or more exothermic peaks in an exothermic curve during cooling measured by differential scanning calorimetry, The release agent has at least one exothermic peak in an exothermic curve during a temperature drop measured by differential scanning calorimetry, The peak temperature of the highest exothermic peak among the exothermic peaks of the graft polymer (A) is designated as T Max (°C), and the peak temperature of the lowest exothermic peak is T Min (° C.), and the peak temperature of the maximum exothermic peak among the exothermic peaks of the release agent is T Wax (℃), The T Max , the T Min and the T Wax satisfies the following formulas (1) and (2): A toner characterized by: 5.0≦T Max -T Min ≦20.0 ・・・(1) 10.0≦T Wax -T Max ≦40.0 ・・・(2)

2. 2. The toner according to claim 1, wherein the graft polymer (A) is a graft polymer having a polyolefin portion and a styrene-acrylic polymer portion.

3. The polyolefin portion is (i) comprises a copolymer of ethylene and propylene; (ii) having a moiety having an acid group; (iii) The toner according to claim 2, wherein the ratio of the number of moles of the ethylene structure PE to the number of moles of the propylene structure PP (PE / PP) is 4 to 20.

4. 4. The toner according to claim 3, wherein the polyolefin portion of the graft polymer (A) has a weight average molecular weight of 1,000 to 3,000.

5. 4. The toner according to claim 3, wherein the acid value of the polyolefin portion is from 0.5 to 16.0 mgKOH / g.

6. 6. The toner according to claim 1, wherein the graft polymer (A) has an acid value of 15.0 to 40.0 mgKOH / g.

7. 6. The toner according to claim 1, wherein the toner contains 3 to 20 parts by mass of the crystalline polyester per 100 parts by mass of the amorphous polyester.

8. The toner according to any one of claims 1 to 5, wherein the toner contains 1 to 20 parts by mass of the release agent and 1 to 20 parts by mass of the graft polymer (A) per 100 parts by mass of the amorphous polyester.

9. the amorphous polyester is a block copolymer having two or more different amorphous polyester segments, Regarding the difference between the SP value of two or more different amorphous polyester segments constituting the block copolymer and the SP value of the styrene acrylic polymer portion of the graft polymer (A), The minimum SP value difference is 1.00 [J / cm 3 ] 0.5 Within The SP value difference between the two or more different amorphous polyester segments constituting the block copolymer is 1.0 [J / cm 3 ] 0.5 The above-mentioned is described in any one of claims 1 to 5. Toner.

10. The toner according to any one of claims 1 to 5, wherein the release agent comprises a hydrocarbon wax.

11. A two-component developer, The two-component developer contains a toner and a magnetic carrier, A two-component developer, wherein the toner is the toner according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Color toner for developing electrostatic charge image

    JP2004046095A

  • Toner binder

    JP2007264349A

  • Dispersant for toner, resin composition for toner, and method for producing resin composition for toner

    JP2011013548A