Heat-seal film, packaging material, and package
A heat-sealable polypropylene film using bio-naphtha-derived propylene and phosphorus antioxidant addresses color and strength changes, maintaining mechanical properties and reducing environmental impact.
Patent Information
- Application Number
- JP2023216889
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-05
- Filing Date
- 2023-12-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polypropylene films used in packaging materials face issues with color and strength changes over time, and there is a need to reduce the use of petrochemical materials to minimize environmental impact.
A heat-sealable polypropylene film is developed using bio-naphtha-derived propylene and a specific range of phosphorus antioxidant, ensuring minimal color and strength changes over time while reducing petrochemical usage.
The film maintains excellent mechanical properties and heat-sealing capabilities with reduced environmental impact, minimizing color and strength variations over time.
Smart Images

Figure 2024149369000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat seal film produced using a raw material derived from bionaphtha, and a packaging material and a package using said heat seal film. [Background technology]
[0002] Polypropylene films are widely used as packaging materials for foods, medicines, industrial products, etc., or as parts of industrial products. Examples of the forms of use include single-layer sheets made of a single layer of polypropylene film, and laminated sheets in which polypropylene film is laminated with other sheet materials. Examples of other sheet materials to be laminated with polypropylene film include polyester resin films, polyvinyl chloride films, and paper. Polypropylene films having heat sealability are widely used as packaging materials.
[0003] In recent years, attempts have been made to replace petroleum-based raw materials with non-petroleum-based raw materials in various industrial products and packaging materials in order to reduce the environmental load. For example, Patent Document 1 proposes producing polyolefin resins from biological raw materials by cracking. However, when films were produced from the polyolefins obtained by cracking, the films showed changes in color and strength over time, and did not adequately meet the needs of customers for industrial products and packaging materials. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2018-522087 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a film material that has heat sealability and exhibits little change in color or strength over time while reducing the amount of petrochemical materials used, thereby resolving the problem of the environmental load of plastic products. [Means for solving the problem]
[0006] The present inventors have thoroughly investigated methods for producing a film using non-petrochemical materials that have a small environmental impact as raw materials, and as a result have found that by adjusting the blend amount of a phosphorus-based antioxidant in the film to a specific range, a polypropylene film can be obtained that has heat-sealing properties, is less susceptible to change in color and transparency over time, has excellent mechanical properties, and has a reduced environmental impact, thereby completing the present invention.
[0007] The present invention has the following aspects. [1] A heat seal film produced using propylene derived from bionaphtha, which has a heat seal layer containing a low melting point resin on at least one side, contains 10% by mass or more and 50% by mass or less of units based on propylene derived from bionaphtha relative to the mass of the heat seal film, and contains 300 ppm by mass or more and 1,000 ppm by mass or less of a phosphorus-based antioxidant relative to the mass of the heat seal film. [2] The heat seal film according to [1], wherein the phosphorus-based antioxidant comprises tris(2,4-di-t-butylphenyl)phosphite. [3] A laminate having a plurality of layers laminated thereon, at least one of which is made of the heat seal film described in [1] or [2] above. [4] A packaging material having the heat seal film described in [1] or [2] above. [5] A package in which an item is packaged using the packaging material described in [4] above. [6] A heat seal film containing polypropylene, having a heat seal layer containing a low melting point resin on at least one surface, The polypropylene comprises a first polypropylene (A) comprising propylene-based units derived from bionaphtha; The amount of the propylene-based unit derived from the bionaphtha is 10% by mass or more and 50% by mass or less relative to the mass of the heat seal film, A heat seal film comprising a phosphorus-based antioxidant in an amount of 300 ppm by mass or more and 1000 ppm by mass or less relative to the mass of the heat seal film. [7] The heat sealable film according to [6], wherein the first polypropylene (A) further contains units based on propylene derived from petroleum naphtha. [8] The heat sealable film according to [7], wherein the first polypropylene (A) contains units based on propylene derived from a mixture of bionaphtha and petroleum naphtha. [9] The heat seal film according to any one of [6] to [8], wherein the units based on propylene derived from the bionaphtha are 20 to 90 mass % relative to the total units of the first polypropylene (A).
[10] The heat seal film according to any one of [6] to [9], wherein the polypropylene further comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha.
[11] The heat seal film according to any one of [6] to
[10] , wherein the heat seal film has a core layer containing the first polypropylene (A) and a skin layer having a composition different from that of the core layer, and the skin layer present on at least one side is the heat seal layer.
[12] The heat seal film according to
[11] , wherein the core layer further comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha.
[13] The heat seal film according to
[11] or
[12] , wherein the skin layer comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha. Effect of the Invention
[0008] According to the present invention, a polypropylene film having heat sealability and little change in color and strength over time can be obtained while reducing the amount of petrochemical materials used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In this specification, the use of "to" indicating a range of values means that the values before and after it are included as the lower limit and upper limit. The lower and upper limits of the numerical ranges disclosed in this specification can be combined in any manner to create new numerical ranges.
[0010] <Heat seal film> The heat seal film according to one embodiment of the present invention is a polypropylene film having heat sealability (hereinafter, also referred to as "polypropylene film (F)"). The polypropylene film (F) contains polypropylene obtained by polymerization of propylene. A part of the propylene is produced from a raw material derived from bionaphtha. In this specification, "bionaphtha" means naphtha produced using biomass as a raw material. "Petroleum naphtha" means naphtha produced using petroleum as a raw material.
[0011] The polypropylene film (F) contains 10% by mass or more and 50% by mass or less, preferably 10% by mass or more and 25% by mass or less, of units based on propylene produced from raw materials derived from bionaphtha (hereinafter also referred to as "bio-naphtha-derived P units"). If the content of the bionaphtha-derived P units is less than 10% by mass, the effect of reducing the environmental load is small. In addition, if the content of the bionaphtha-derived P units exceeds 50% by mass, the change in color and strength over time is easily noticeable, and the commercial value of the product is likely to decrease. The content of the bionaphtha-derived P units is preferably 40% by mass or less, and more preferably 30% by mass or less.
[0012] The polypropylene film (F) contains a phosphorus-based antioxidant in an amount of 300 ppm or more and 1000 ppm or less, preferably 300 ppm or more and 700 ppm or less. If the content of the phosphorus-based antioxidant is 300 ppm or more, it is excellent in the effect of suppressing the change in color and strength over time. If the content of the phosphorus-based antioxidant exceeds 1000 ppm, the transparency and printing characteristics are likely to deteriorate due to bleed-out over time.
[0013] Examples of phosphorus-based antioxidants include tris(nonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, bis(2,4-di-t-butyl-6-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and tetrakis(2,4-di-t-butylphenyl) 4,4'-diphenylenediphosnite, 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, 2,2'-ethylidenebis(4,6-di-t-butylphenyl)fluorophosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl phosphite, 2-(2,4,6-tri-t-butylphenyl)-5-ethyl-5-butyl-1,3,2-oxaphosphorinane, 2,2',2''-nitrilo[triethyl-tris(3,3',5,5'-tetra-t-butyl-1,1'-biphenyl-2,2'-diyl)phosphite, etc. Among these, tris(2,4-di-t-butylphenyl)phosphite is particularly preferred. The phosphorus-based antioxidant preferably contains tris(2,4-di-t-butylphenyl)phosphite. The proportion of tris(2,4-di-t-butylphenyl)phosphite relative to the total mass of the phosphorus-based antioxidants contained in the polypropylene film (F) is preferably 80 mass% or more, more preferably 85 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more. It may be 100 mass%.
[0014] The polypropylene film (F) may contain materials other than polypropylene depending on quality requirements, as long as the effects of the present invention are not impaired. Examples of other materials include pigments, dyes, lubricants, antiblocking agents, antistatic agents, UV absorbers, plasticizers, freshness-retaining agents, deodorizers, compatibilizers, resins other than polypropylene, and antioxidants other than phosphorus-based antioxidants. The total content of the other materials relative to the mass of the polypropylene film (F) is, for example, preferably 3 mass % or less, more preferably 2 mass % or less, and may be zero.
[0015] The polypropylene contained in the polypropylene film (F) is mainly composed of units based on propylene, and is a propylene homopolymer or a copolymer having 80 mass % or more of units based on propylene. The copolymer is, for example, a copolymer having units based on propylene and units based on one or more types of α-olefins, such as ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-pentene-1. The proportion of propylene-based units relative to all the polypropylene units is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. It may be 100% by mass.
[0016] [First polypropylene (A)] In a preferred embodiment of the polypropylene film (F), the polypropylene contained in the polypropylene film (F) includes a first polypropylene (A) containing bionaphtha-derived P units. The content of the bionaphtha-derived P units relative to all units of the first polypropylene (A) is preferably from 20 to 90 mass%, more preferably from 30 to 70 mass%, and even more preferably from 40 to 50 mass%.
[0017] The first polypropylene (A) preferably contains bionaphtha-derived P units and units based on propylene derived from petroleum naphtha (hereinafter also referred to as "petroleum-derived P units"). The content of the petroleum-derived P units relative to all units of the first polypropylene (A) is preferably from 10 to 80 mass%, more preferably from 30 to 70 mass%, and even more preferably from 50 to 60 mass%.
[0018] The first polypropylene (A) may be a copolymer having other units based on monomers other than propylene. The total content of the bionaphtha-derived P units and the petroleum-derived P units relative to the total units of the first polypropylene (A) is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. It may be 100% by mass.
[0019] The first polypropylene (A) preferably comprises propylene-based units produced from a mixture of bionaphtha and petroleum naphtha. The propylene produced from a mixture of bionaphtha and petroleum naphtha as the raw naphtha is a mixture of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha. The ratio of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha in the produced propylene is determined by the ratio of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha in the raw naphtha. For example, propylene (50 / 50) produced from a mixture of 50 mass% bionaphtha and 50 mass% petroleum naphtha is a mixture of 50 mass% propylene derived from the bionaphtha and 50 mass% propylene derived from the petroleum naphtha. Based on all units of the polypropylene obtained by polymerizing propylene (50 / 50), the content of bionaphtha-derived P units is 50 mass %, and the content of petroleum-derived P units is 50 mass %.
[0020] The first polypropylene (A) contained in the polypropylene film (F) may be one type or two or more types. The content of the first polypropylene (A) in the polypropylene film (F) can be designed so that the bionaphtha-derived P unit is 10% by mass or more and 50% by mass or less with respect to the mass of the polypropylene film.
[0021] [Second polypropylene (B)] The polypropylene contained in the polypropylene film (F) preferably contains, in addition to the first polypropylene (A), a second polypropylene (B) that contains petroleum-derived P units and does not contain bionaphtha-derived P units. The second polypropylene (B) may be a copolymer having units based on monomers other than propylene. The content of the petroleum-derived P units relative to all units of the second polypropylene (B) is preferably 80% by mass or more, more preferably 85% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more. It may be 100% by mass.
[0022] The second polypropylene (B) contained in the polypropylene film (F) may be one type or two or more types. The content of the second polypropylene (B) relative to the polypropylene film (F) can be designed so that the bionaphtha-derived P units in the first polypropylene (A) are 10 mass% or more and 50 mass% or less relative to the mass of the polypropylene film (F).
[0023] [Heat seal layer] The polypropylene film (F) has a heat seal layer containing a low melting point resin on at least one surface. In a preferred embodiment, the polypropylene film (F) has a core layer and a skin layer having different compositions, and the skin layer present on at least one surface is a heat seal layer containing a low melting point resin. For example, the polypropylene film (F) may have a core layer containing a mixture of the first polypropylene (A) and the second polypropylene (B), and a skin layer containing the second polypropylene (B) but not the first polypropylene (A). The skin layer may be provided on only one of the front side and the back side of the core layer, or on both sides. When a skin layer is present only on one of the front and back sides of the core layer, the skin layer is a heat seal layer containing a low melting point resin. When skin layers are present on both the front and back sides of the core layer, only one of the skin layers may be a heat seal layer containing a low melting point resin, or both skin layers may be heat seal layers containing a low melting point resin. When the polypropylene film (F) has heat seal layers on both the front and back sides, the compositions of the two heat seal layers may be the same as or different from each other.
[0024] The low melting point resin is a low melting point polypropylene, and is preferably a copolymer of one or more α-olefins and propylene. Examples of α-olefins include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, and 1-decene. It may be a random copolymer or a block copolymer. Specific examples of low melting point resins include ethylene-propylene-1-butene copolymers, propylene-α-olefin random copolymers, and mixtures thereof.
[0025] The melting point of the low melting point resin is preferably 60 to 150° C., more preferably 70 to 140° C. The low melting point resin contained in the heat seal layer may be one type or two or more types. When the heat seal layer contains two or more types of low melting point resins, it is preferable that the melting point of each low melting point resin is in the above-mentioned range. The melting point of the low melting point resin is preferably 10 to 100° C. lower than the polypropylene having the highest melting point among the polypropylenes contained in the layers other than the heat seal layer. For example, polypropylene homopolymer has the highest melting point of 162°C and is contained in any layer other than the heat seal layer.
[0026] In order to obtain a low heat sealing temperature and stable heat sealing strength, it is preferable to use a mixture of two or more low melting point resins having different melting points. For example, the low melting point resin contained in the heat seal layer is preferably a mixture of a first low melting point resin having a melting point of 100° C. or more and 150° C. or less, and a second low melting point resin having a melting point less than 100° C. There is no particular lower limit to the melting point of the second low melting point resin, but from the viewpoint of preventing blocking, a melting point of 60° C. or more is preferable. The first low melting point resin may be, for example, an ethylene-propylene-1-butene copolymer, and the second low melting point resin may be, for example, a propylene-1-butene copolymer. The proportion of the first low melting point resin with respect to the total mass of the first low melting point resin and the second low melting point resin is, for example, preferably 65 to 95 mass %, and more preferably 75 to 90 mass %.
[0027] The heat seal layer may contain materials other than the low melting point resin as long as the effects of the present invention are not impaired. Examples of other materials include pigments, dyes, lubricants, antiblocking agents, antistatic agents, ultraviolet absorbers, plasticizers, freshness-preserving agents, deodorizers, compatibilizers, and antioxidants. The total content of the other materials relative to the mass of the heat seal layer is, for example, preferably 25% by mass or less, more preferably 5% by mass or less, and may be zero.
[0028] The polypropylene film (F) may be uniaxially or biaxially stretched. The stretching ratio is preferably 3 to 6 times in the MD direction and 8 to 12 times in the TD direction. The density of the polypropylene film (F) is not particularly limited, but is, for example, 0.90 to 0.92 g / cm 3 The density is a value measured by a dry density meter, a density gradient tube, etc. The thickness of the polypropylene film (F) is not particularly limited, but is, for example, 15 μm to 80 μm.
[0029] <Method of manufacturing heat seal film> The polypropylene film (F) can be produced by forming a resin composition containing polypropylene into a sheet to obtain an unstretched sheet having a core layer and a skin layer (heat seal layer), and then biaxially stretching the unstretched sheet to obtain the polypropylene film (F). Among these, a tenter sequential biaxial stretching method is preferred. The polypropylene film (F) having a core layer and a skin layer is preferably produced by a tenter sequential biaxial stretching method using a co-extrusion die.
[0030] <Laminate> A laminate according to one embodiment of the present invention is a laminate in which a plurality of layers are laminated, at least one of which is made of a polypropylene film (F). For example, there may be mentioned a laminate in which a plurality of polypropylene films (F) are laminated together, and a laminate in which one or more layers of polypropylene film (F) are laminated with one or more layers made of a material different from that of the polypropylene film (F). Examples of the layer made of a material different from the polypropylene film (F) include resin films other than the polypropylene film (F), paper, and the like. Examples of methods for producing the laminate include methods of laminating with other films, such as dry lamination and hot melt lamination, etc. Among these, the dry lamination method using gravure roll coating equipment is preferred. When the polypropylene film (F) is laminated so that a heat seal layer is present on the outermost surface of the laminate, a laminate having heat sealability is obtained.
[0031] <Packaging materials> The packaging material according to one embodiment of the present invention comprises a polypropylene film (F). The polypropylene film (F) may be used as a packaging material as it is, or may be used as a packaging material after being subjected to a heat sealing process. As the heat sealing process, a known processing method can be applied. For example, the ends of the polypropylene film (F) may be heat-sealed to each other to form a bag-shaped packaging material. Also, the end of the polypropylene film (F) may be heat-sealed to an end of a packaging material other than the polypropylene film (F) to form a bag-shaped packaging material.
[0032] <Package> A package according to one embodiment of the present invention is an article packaged with the packaging material according to the present invention. Examples of the goods include general goods, food, clothing, etc. As the packaging method, a known packaging method can be applied. For example, a package in which the goods are contained in a bag-shaped packaging material using a general pillow packaging machine can be exemplified.
[0033] <Example> The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to these examples. Note that, unless otherwise specified, the unit of content "%" is "mass%". Measurement and evaluation methods used in each example are shown below.
[0034] (1) Color The YI value of the film was measured using a spectral colorimeter / haze meter "COH7700 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd. The film was stored at 23°C for 3 months, and the YI value at the start of storage (initial YI) and the YI value after 3 months (YI after 3 months) were measured, and the YI value change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in color over time was evaluated according to the following criteria. YI value change rate = (YI after 3 months - initial YI) / initial YI x 100 ○: Change in YI value after 3 months at 23℃ is within 20% ×: When the rate of change in YI value after 3 months at 23℃ exceeds 20%
[0035] (2) Tensile strength The tensile strength in the machine direction was measured using a tensile tester in accordance with JIS K7127. Samples were cut to a size of 15 mm in the width direction × 200 mm in the machine direction, and the test was performed at a tensile speed of 200 mm / min. The strength was measured when the film broke. The film was stored at 90°C for one month, and the strength at the start of storage (initial strength) and the strength after one month (strength after one month) were measured, and the strength change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in tensile strength over time was evaluated according to the following criteria. Strength change rate = (initial strength - strength after 1 month) / initial strength x 100 ○: Strength change rate within 20% after 1 month at 90℃ ×: When the strength change rate after 1 month at 90℃ exceeds 20%
[0036] (3) Transparency The transparency of the film was measured using a transparency meter "CLARITY-METER TM-1D (product name)" manufactured by Murakami Color Research Laboratory Co., Ltd. The film was stored at 23°C for 3 months, and the transparency at the start of storage (initial transparency) and after 3 months (transparency after 3 months) were measured, and the transparency change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in transparency over time was evaluated according to the following criteria. Transparency change rate = (initial transparency - transparency after 3 months) / initial transparency x 100 ○: Transparency change rate within 20% after 3 months at 23℃ ×: When the transparency change rate after 3 months at 23℃ exceeds 20%
[0037] (4) Heat seal strength Two rectangular films with a length of 230 mm in the MD direction and a length of 50 mm in the TD direction were prepared, and samples were prepared by stacking the first skin layers or the second skin layers so that they were in contact with each other. The samples were heat-sealed using a thermal gradient tester (product name "HG-100-2" by Toyo Seiki Seisakusho Co., Ltd.) under the conditions of a heat seal temperature of 100 to 120°C, a seal pressure of 0.2 MPa, a seal time of 2 seconds, and a seal area of 10 mm x 25 mm. Using a tensile tester (product name "TGI-1kN" by Minebea Co., Ltd.), the two films were T-peeled at a tensile speed of 300 mm / min, and the maximum load recorded was taken as the heat seal strength. The heat sealability was evaluated according to the following criteria. 〇: Heat seal strength at a heat seal temperature of 120℃ is 3.0N / 25mm or more ×: Heat seal strength at a heat seal temperature of 120°C is less than 3.0N / 25mm
[0038] (5) Reducing environmental impact ○: Contains polypropylene derived from bio-naphtha, so the environmental impact is small. ×: The product has a large environmental impact because it does not contain polypropylene derived from bionaphtha.
[0039] (6) The content of phosphorus-based antioxidants in polypropylene films was measured by extracting the antioxidants in the films and performing HPLC-PDA analysis.
[0040] (7) The content of bionaphtha-derived P units in the polypropylene film was calculated based on the content of bionaphtha-derived P units in each raw material resin composition and the blending ratio of each raw material resin composition. It can also be measured by measuring the C14 concentration using accelerator mass spectrometry (AMS).
[0041] <Raw materials> [Raw material resin composition containing first polypropylene (A)] The following Bio-PPs (A1) to (A3) are all resin compositions containing polypropylene obtained by polymerizing propylene produced from raw naphtha, which is a mixture of 50% by mass of bio-naphtha and 50% by mass of petroleum naphtha, and tris(2,4-di-t-butylphenyl)phosphite, a phosphorus-based antioxidant. The content of P units derived from bio-naphtha is 50% by mass relative to the total units of polypropylene. Bio-PP (A1): 99.20% by mass of polypropylene, 0.10% by mass of phosphorus-based antioxidant, 0.70% by mass of additives other than phosphorus-based antioxidants. Bio-PP (A2): 99.19% by mass of polypropylene, 0.01% by mass of phosphorus-based antioxidant, 0.80% by mass of additives other than phosphorus-based antioxidants. Bio-PP (A3): 98.90% by mass of polypropylene, 0.40% by mass of phosphorus-based antioxidant, 0.70% by mass of additives other than phosphorus-based antioxidants.
[0042] [Raw material resin composition containing second polypropylene (B)] The following petroleum PPs (B1), (B2), and (B3) are all resin compositions containing polypropylene obtained by polymerizing propylene produced from 100% petroleum naphtha raw material, and tris(2,4-di-t-butylphenyl)phosphite, a phosphorus-based antioxidant. Petroleum PP (B1): Polypropylene 99.16% by mass, phosphorus-based antioxidant 0.04% by mass, additives other than phosphorus-based antioxidant 0.80% by mass. Petroleum PP (B2): 99.17% by mass of polypropylene, 0.03% by mass of phosphorus-based antioxidant, 0.80% by mass of additives other than phosphorus-based antioxidants.
[0043] [Raw material resin composition containing a low melting point resin which is a second polypropylene (B)] The following Petroleum PP (BH-1) is a resin composition containing a petroleum-derived ethylene-propylene-1-butene copolymer (melting point 130°C), a petroleum-derived propylene-1-butene copolymer (melting point 75°C), and tris(2,4-di-t-butylphenyl)phosphite, a phosphorus-based antioxidant. Petroleum PP (BH-1): 86.1% by mass of ethylene-propylene-1-butene copolymer, 10.0% by mass of propylene-1-butene copolymer, 0.1% by mass of phosphorus-based antioxidant, 3.8% by mass of additives other than phosphorus-based antioxidant.
[0044] <Example 1> A heat seal film was produced using the raw material composition shown in Table 1. Using three extruders, the raw material composition for the core layer, the raw material composition for the first skin layer, and the raw material composition for the second skin layer were melt-kneaded at 230°C in each extruder, and the three layers were co-extruded so that the thickness ratio of the first skin layer / core layer / second skin layer was 8 / 84 / 8 to obtain a laminated sheet. The core layer was made of a mixture of petroleum PP (B1) and bio-PP (A1). The laminated sheet was cooled by contacting it with a roll at 30°C, stretched longitudinally at 140°C to 4.7 times its original size, and then stretched transversely at 165°C to 10 times its original size, resulting in a thickness of 30 µm and a density of 0.90 g / cm. 3 A biaxially oriented polypropylene film (heat seal film) was obtained. The first skin layer was a heat seal layer containing a low melting point resin. In this example, the content of the bionaphtha-derived P unit is 10 mass % and the content of the phosphorus-based antioxidant is 400 ppm relative to the mass of the polypropylene film.
[0045] <Example 2> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of the bionaphtha-derived P unit was 25 mass%. The first skin layer was a heat seal layer containing a low melting point resin.
[0046] <Example 3> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that both the first skin layer and the second skin layer contained a low melting point resin to form a heat seal layer.
[0047] <Comparative Example 1> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of the phosphorus-based antioxidant was 280 ppm.
[0048] <Comparative Example 2> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of the phosphorus-based antioxidant was 1510 ppm.
[0049] <Comparative Example 3> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of bionaphtha-derived P units was 0%.
[0050] <Evaluation> The polypropylene films obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated for the items shown in the tables. The results are shown in Table 1.
[0051] [Table 1]
[0052] As shown by the above results, the polypropylene films of Examples 1 to 3 had heat sealability, low environmental impact, and little change in color, mechanical properties, and transparency over time. On the other hand, the polypropylene film of Comparative Example 1 had heat sealability and was environmentally friendly, but was subject to significant changes in color and mechanical properties over time, raising concerns about problems in use. The polypropylene film of Comparative Example 2 had heat sealability, was environmentally friendly, and showed little change in color and mechanical properties over time, but its transparency deteriorated over time. The polypropylene film of Comparative Example 3 had heat sealability and showed little change in color, mechanical properties, and transparency over time, but had a large environmental impact because it did not use bionaphtha-derived polypropylene as a raw material. [Industrial Applicability]
[0053] The polypropylene film of the present invention is an excellent heat-sealable film that has heat-sealing properties and exhibits little change in color and strength over time while reducing the amount of petrochemical materials used, and is useful as an excellent packaging material.
Claims
1. A heat seal film containing polypropylene produced using propylene derived from bionaphtha, the heat seal film having a heat seal layer containing a low melting point resin on at least one side, containing 10% by mass or more and 50% by mass or less of units based on propylene derived from bionaphtha relative to the mass of the heat seal film, and containing 300 ppm by mass or more and 1000 ppm by mass or less of a phosphorus-based antioxidant relative to the mass of the heat seal film.
2. 2. The heat seal film of claim 1, wherein the phosphorus-based antioxidant comprises tris(2,4-di-t-butylphenyl) phosphite.
3. A laminate comprising a plurality of layers, at least one of which comprises the heat seal film according to claim 1 or 2.
4. A packaging material comprising the heat seal film according to claim 1 or 2.
5. A package in which an article is packaged with the packaging material according to claim 4.
Citation Information
Patent Citations
Packaging materials
JP1991124833U
Polypropylene resin composition and film made by using it
JP1996081588A
Polyolefin resin composition and film made of the same
JP2002069248A
Polypropylene resin composition, film and use thereof
JP2003055510A
Propylene-based resin film and method for producing the same
JP2011219518A