Semiconductor device

The use of an oxide semiconductor stack with varying energy gaps and dopant introduction in transistors addresses the challenges of high electrical performance and low power consumption in semiconductor devices, achieving stable and efficient operation.

JP2024149590AInactive Publication Date: 2024-10-18SEMICON ENERGY LAB CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024124436
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2011-06-17
Filing Date
2024-07-31
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing semiconductor devices using oxide semiconductors face challenges in achieving high electrical performance, low power consumption, and precise control of electrical characteristics such as threshold voltage and off-state current, particularly in transistors with negative threshold voltages leading to normally-on states.

Method used

A transistor structure utilizing an oxide semiconductor stack with multiple layers having different energy gaps, where the energy gap of one layer is 3 eV or more and another is less than 3 eV, and introducing dopants to form low-resistance regions, combined with dehydration or dehydrogenation treatments to reduce oxygen vacancies, is employed.

Benefits of technology

This configuration enables high on-state current, field-effect mobility, and low off-state current, allowing for high-speed operation and low power consumption, while ensuring stable electrical characteristics and a normally-off switching element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149590000001_ABST
    Figure 2024149590000001_ABST
Patent Text Reader

Abstract

To provide a transistor using an oxide semiconductor layer having electric characteristics required according to use, and to provide a semiconductor device having the transistor.SOLUTION: A transistor comprises a semiconductor layer, a source electrode layer or a drain electrode layer, a gate insulation film, and a gate electrode layer sequentially laminated on in this order an oxide insulation film. As the semiconductor layer, an oxide semiconductor laminate is used, the oxide semiconductor laminate includes at least two layers of oxide semiconductor layers having different bandgap from each other. Oxygen and / or dopant may be introduced to the oxide semiconductor laminate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device.

[0002] In this specification, a semiconductor device is a device that can function by utilizing semiconductor characteristics. Generally speaking, electro-optical devices, semiconductor circuits, and electronic devices are all semiconductor devices. [Background technology]

[0003] A technique for constructing transistors (also called thin-film transistors (TFTs)) using thin semiconductor films. This technology is attracting attention. The transistor is used in integrated circuits (ICs) and image display devices (display devices). It is widely used in electronic devices such as the following: Silicon-based semiconductor materials are widely known, but oxide semiconductors are also attracting attention as other materials. It is being done.

[0004] As for transistors using oxide semiconductors, In transistors using oxide semiconductors, higher electrical characteristics are required. For the purpose of achieving good electrical characteristics, low-resistance source and drain regions are fabricated using an aluminum reaction method. Techniques for forming regions have been reported (for example, see Non-Patent Document 1).

[0005] For example, indium (In), gallium (Ga), and nickel are used as active layers of transistors. A transistor using an amorphous oxide containing lead (Zn) has been disclosed (see Patent Document 1). ). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-165528 A [Non-patent literature]

[0007] [Non-Patent Document 1] N.Morosawa, Yoshihiro Ohshima, Mitsuo Morooka, Toshiaki Arai, Tatsuya Sasaoka, “A Novel Self-Aligned Top-Gate Oxide TFT for AM-OLED Displays”, SID 11 DIGEST pp479-482 Summary of the Invention [Problem to be solved by the invention]

[0008] When the on-characteristics of a transistor (e.g., on-current and field-effect mobility) are improved, the semiconductor device This enables high-speed response to input signals and high-speed operation in semiconductor devices, resulting in higher performance semiconductor devices. On the other hand, in order to reduce the power consumption of a semiconductor device, the off-state current of a transistor must be sufficiently low. In this way, the electrical characteristics required for a transistor must be determined according to the application and purpose. The electrical properties vary depending on the material and therefore it would be beneficial to have more precise control over the electrical properties.

[0009] The threshold voltage of a transistor using an oxide semiconductor for the channel formation region is plotted. This transistor structure realizes a so-called normally-off switching element. One of the objectives of the present invention is to provide a structure and a method for manufacturing the same.

[0010] The transistor has a positive threshold voltage at which the gate voltage is as close to 0V as possible. If the threshold voltage of the transistor is negative, the gate voltage Even at 0V, current flows between the source and drain electrodes, making it a so-called normally-on state. In LSI, CPU and memory, the electrical characteristics of the transistors that make up the circuits are important. These electrical characteristics affect the power consumption of a semiconductor device. Among these properties, the threshold voltage (Vth) is important. If the voltage is negative, it is difficult to control the circuit. A transistor in which a channel is formed and a drain current flows is used in an integrated circuit of a semiconductor device. It is not suitable for use as a transistor.

[0011] In addition, depending on the material and manufacturing conditions, the manufactured transistor may not be normally off. Even in this case, it is important to approach the normally-off characteristics, and the threshold voltage is Even if the transistor is normally on, the threshold voltage of the transistor is close to zero. It is also an object of the present invention to provide a structure and a manufacturing method thereof.

[0012] In order to realize a semiconductor device with higher performance, the on-characteristics of a transistor (e.g., A configuration that improves the current and field effect mobility to realize high-speed response and high-speed operation of semiconductor devices. It is also an object of the present invention to provide a method for producing the same.

[0013] As described above, transistors using oxide semiconductor layers having electrical characteristics required for specific applications can be fabricated. An object of the present invention is to provide a transistor and a semiconductor device including the transistor. [Means for solving the problem]

[0014] A semiconductor layer, a source electrode layer, a drain electrode layer, a gate insulating film, and a gate electrode layer are stacked in this order. In the layered transistor, the semiconductor layers are at least one semiconductor layer having a different energy gap. In addition, a stack of oxide semiconductor layers including two oxide semiconductor layers is used.

[0015] When the oxide semiconductor stack has a stacked structure of a first oxide semiconductor layer and a second oxide semiconductor layer, In this case, the first oxide semiconductor layer and the second oxide semiconductor layer have their own energy gaps. The order of stacking is not limited as long as the gaps are different. The side in contact with the gate insulating film is The layer may have a large gap or a small energy gap.

[0016] Specifically, in the stack of oxide semiconductor layers, the energy gap of one of the oxide semiconductor layers is The energy gap of the other oxide semiconductor layer is set to be 3 eV or more, and the energy gap of the other oxide semiconductor layer is set to be less than 3 eV. In this specification, the term "energy gap" means "band gap" or " It is used in the same sense as "forbidden band width."

[0017] When the oxide semiconductor stack has a stack structure of three or more layers, all the oxide semiconductor layers have different The energy gap may be the same as that of the other structures, or may be substantially the same. The oxide semiconductor layer may be used in a stack of a plurality of oxide semiconductor layers.

[0018] For example, the oxide semiconductor stack may be formed by stacking a first oxide semiconductor layer, a second oxide semiconductor layer, and a third oxide semiconductor layer. In the stacked structure of the oxide semiconductor layers, the energy gap of the second oxide semiconductor layer is set to be larger than that of the first oxide semiconductor layer. The energy gap of the first oxide semiconductor layer is set to be smaller than that of the second oxide semiconductor layer and the third oxide semiconductor layer. The electron affinity of the second oxide semiconductor layer is calculated based on the electron affinity of the first oxide semiconductor layer and the electron affinity of the third oxide semiconductor layer. In this case, the electron affinity of the first oxide semiconductor layer and the third oxide semiconductor layer is set to be larger than that of the second oxide semiconductor layer. The energy gap and electron affinity of the semiconductor layer can be made equal. The second oxide semiconductor layer having a small energy gap is covered with the first oxide semiconductor layer having a large energy gap. By using a structure in which the second oxide semiconductor layer and the third oxide semiconductor layer are sandwiched, This has the effect of reducing the off-current (leak current). Here, the electron affinity is the relationship between the vacuum level and This represents the energy difference with respect to the conduction band of an oxide semiconductor.

[0019] In a transistor including an oxide semiconductor layer, the energy gap of the oxide semiconductor layer For example, in a transistor using an oxide semiconductor layer, In a semiconductor device, when the energy gap of the oxide semiconductor layer is small, the on-characteristics (for example, On the other hand, the energy gap of the oxide semiconductor layer is large. If the gate insulating layer is not provided, the off-state current can be reduced.

[0020] In the case of a single oxide semiconductor layer, the size of the energy gap of the oxide semiconductor layer determines the transistor Since the electrical characteristics of the transistor are almost determined, it is necessary to give the transistor the desired electrical characteristics. It's difficult.

[0021] A stack of oxide semiconductor layers having different energy gaps is used. This allows the electrical characteristics of the transistor to be controlled more precisely, resulting in a desired It becomes possible to impart electrical properties to the transistor.

[0022] Therefore, it is possible to provide semiconductor devices that meet various purposes, such as high functionality, high reliability, and low power consumption. It is possible.

[0023] One embodiment of the configuration of the present invention disclosed in this specification is a first oxide semiconductor having a different energy gap. An oxide semiconductor stack including a conductor layer and a second oxide semiconductor layer, and a source electrode formed on the oxide semiconductor stack. a gate insulating film on the source electrode layer and the drain electrode layer; The semiconductor device includes a gate electrode layer over a gate insulating film and overlapping with an oxide semiconductor stack.

[0024] One embodiment of the configuration of the invention disclosed in this specification is a first oxide semiconductor layer, a second oxide semiconductor layer, a stack of oxide semiconductor layers including a first oxide semiconductor layer, a second oxide semiconductor layer, and a third oxide semiconductor layer in this order; a source electrode layer and a drain electrode layer, and a gate insulating film on the source electrode layer and the drain electrode layer. a gate electrode layer overlapping the oxide semiconductor stack over a gate insulating film; The oxide semiconductor layer has an energy gap smaller than that of the first oxide semiconductor layer and the third oxide semiconductor layer. This is a semiconductor device having a large energy gap.

[0025] In the above structure, the oxide semiconductor stack has an island shape, and the source electrode layer and the drain electrode layer The oxide semiconductor layer can be formed in contact with the side surface (end portion) of the oxide semiconductor stack. The side (end) of the layer is provided with a first oxide semiconductor layer, a second oxide semiconductor layer, a third oxide semiconductor layer, and a second oxide semiconductor layer. Since the side surfaces (ends) of the semiconductor layers are exposed, the first oxide semiconductor layer and the second oxide semiconductor layer The first oxide semiconductor layer and the second oxide semiconductor layer are in contact with the source electrode layer and the drain electrode layer.

[0026] One embodiment of the present invention disclosed in this specification is a semiconductor device having an oxide insulating film and a gate insulating film having a different energy gap. and forming a source semiconductor layer on the oxide semiconductor stack. A gate insulating layer is formed to cover the source electrode layer and the drain electrode layer. In this method, a gate insulating film is formed, and a gate electrode layer is formed on the gate insulating film.

[0027] One embodiment of the present invention disclosed in this specification is a semiconductor device having an oxide insulating film and a gate insulating film having a different energy gap. a mask is formed over the stack of the oxide semiconductor films, and The stack of oxide semiconductor films is etched to form an oxide semiconductor stack. A source electrode layer and a drain electrode layer are formed on the insulating layer, and the source electrode layer and the drain electrode layer are covered with the insulating layer. A method for manufacturing a semiconductor device, comprising forming a gate insulating film and forming a gate electrode layer on the gate insulating film. It is law.

[0028] In addition, a dopant is introduced into the oxide semiconductor stack using the gate electrode layer as a mask, and a self-aligned The channel formation region is sandwiched between the low-resistance The dopant is an impurity that changes the electrical conductivity of the oxide semiconductor stack. The dopant introduction method includes ion implantation, ion doping, plasma ion implantation, etc. A deposition ion implantation method or the like can be used.

[0029] A stack of oxide semiconductor layers including a low-resistance region is provided between the channel formation region in the channel length direction. As a result, the transistor has high on-characteristics (e.g., on-current and field-effect mobility). This enables high-speed operation and high-speed response.

[0030] In addition, a heat treatment (desorption treatment) for releasing hydrogen or moisture from an oxide semiconductor layer (oxide semiconductor film) may be performed. For example, in the above configuration, before forming the mask, Then, a heat treatment is performed to release hydrogen or moisture contained in the stacked oxide semiconductor film. It is preferable to do so.

[0031] In addition, oxygen, which is a main component material of an oxide semiconductor, can be removed by the dehydration or dehydrogenation treatment. In the oxide semiconductor film, oxygen is released and the amount of the oxide semiconductor film is reduced. In the area where the oxygen is removed, oxygen vacancies exist, and these oxygen vacancies cause fluctuations in the electrical characteristics of the transistor. Therefore, donor levels are generated.

[0032] Therefore, oxygen is added to the oxide semiconductor layer (oxide semiconductor film) that has been subjected to the dehydration or dehydrogenation treatment. It is preferable to supply oxygen to the oxide semiconductor layer (oxide semiconductor film). This makes it possible to compensate for oxygen vacancies in the film.

[0033] For example, an oxide insulating film containing a large amount (excessive amount) of oxygen, which serves as an oxygen supply source, is used as an oxide semiconductor layer ( By providing the insulating film in contact with the oxide semiconductor layer (oxide semiconductor film), In the above structure, oxygen can be supplied to the dehydration or dehydrogenation semiconductor film. The oxide semiconductor layer (oxide semiconductor film) and the oxide insulating film that were subjected to heat treatment were thinned. By performing heat treatment in a state where the oxide semiconductor layer (oxide semiconductor film ) may be supplied with oxygen.

[0034] In addition, the oxide semiconductor layer (oxide semiconductor film) that has been subjected to the dehydration or dehydrogenation treatment may be At least one of oxygen radicals, oxygen atoms, and oxygen ions is introduced into the film. Oxygen may be supplied. The oxygen introduction method may be an ion implantation method, an ion doping method, Plasma immersion ion implantation, plasma treatment, etc. can be used. can.

[0035] Further, the oxide semiconductor layer (oxide semiconductor film) provided in the transistor is preferably an oxide semiconductor layer. The oxide semiconductor contains regions in which the oxygen content is excessive with respect to the stoichiometric composition ratio in the crystalline state. In this case, the oxygen content is preferably within the stoichiometric composition of the oxide semiconductor. The oxygen content is set to a level exceeding the ratio of oxygen in the case of a single crystal. Oxygen may exist between the lattices of an oxide semiconductor.

[0036] Hydrogen or moisture is removed from the oxide semiconductor, and the semiconductor is highly purified to minimize the amount of impurities contained therein. By supplying oxygen to compensate for oxygen vacancies, an I-type (intrinsic) oxide semiconductor or an I-type By doing so, it is possible to obtain an oxide semiconductor that is as close to an intrinsic oxide semiconductor as possible. To bring the Fermi level (Ef) of a semiconductor to the same level as the intrinsic Fermi level (Ei) Therefore, by using the oxide semiconductor film in a transistor, the Reduces the variation in threshold voltage Vth of transistors and the threshold voltage shift ΔVth It is possible.

[0037] One embodiment of the present invention includes a transistor or a circuit including a transistor. The present invention relates to a semiconductor device, for example, a transistor in which a channel formation region is formed using an oxide semiconductor. The present invention relates to a semiconductor device having a circuit including a transistor. , LSI, CPU, power devices mounted on power circuits, memory, thyristors, converters, semiconductor integrated circuits including image sensors, and liquid crystal display panels. The present invention relates to electronic equipment that incorporates, as a component, a light-emitting display device having a magneto-optical device or a light-emitting element. Effect of the Invention

[0038] A stack of oxide semiconductor layers having different energy gaps is used. This allows the electrical characteristics of the transistor to be controlled more precisely, resulting in a desired It becomes possible to impart electrical properties to the transistor.

[0039] Therefore, it is possible to provide semiconductor devices that meet various purposes, such as high functionality, high reliability, and low power consumption. It is possible. [Brief description of the drawings]

[0040] [Figure 1] 1A to 1C illustrate one embodiment of a semiconductor device. [Diagram 2] 1A to 1C illustrate one embodiment of a semiconductor device and a manufacturing method thereof; [Diagram 3] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 4] 1A and 1B are a diagram illustrating one embodiment of a semiconductor device and an energy band diagram. [Diagram 5] 1A to 1C illustrate one embodiment of a semiconductor device and a manufacturing method thereof; [Figure 6] 1A to 1C illustrate one embodiment of a semiconductor device and a manufacturing method thereof; [Figure 7] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 8] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 9] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 10] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 11] FIG. [Figure 12] FIG. [Figure 13] FIG. [Figure 14] TEM photographs and schematic diagrams of samples of the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] Hereinafter, embodiments of the invention disclosed in this specification will be described in detail with reference to the drawings. However, the invention disclosed in this specification is not limited to the following description, and the forms and details thereof may be changed in various ways. It will be easily understood by those skilled in the art that the invention disclosed in this specification can be modified in any manner. The present invention should not be construed as being limited to the description of the following embodiments. The ordinal numbers 2 are used for convenience and do not indicate the order of steps or stacking. In addition, the present specification does not indicate specific names as matters for identifying the invention. do not have.

[0042] (Embodiment 1) In this embodiment mode, one embodiment of a semiconductor device and a manufacturing method thereof will be described with reference to FIGS. In this embodiment, a transistor having an oxide semiconductor film will be described as an example of a semiconductor device. This indicates a transistor.

[0043] A transistor can have either a single-gate structure in which one channel formation region is formed or a structure in which two are formed. The gate structure may be a double gate structure in which three gates are formed, or a triple gate structure in which three gates are formed. The semiconductor device has two gate electrode layers disposed above and below a channel region with a gate insulating film interposed therebetween. A dual gate type may also be used.

[0044] The transistor 440a and the transistor 440b shown in FIGS. 1 is an example of a planar type transistor having a structure.

[0045] As shown in FIGS. 1A and 1B, the transistors 440a and 440b are oxidized. A first oxide film having a different energy gap is formed on a substrate 400 having an insulating film 436 formed thereon. An oxide semiconductor stack 403 including a semiconductor layer 101 and a second oxide semiconductor layer 102, a source The electrode layer 405a, the drain electrode layer 405b, the gate insulating film 402, and the gate electrode layer 401 are An insulating film 407 is formed over the transistor 440a and the transistor 440b. is.

[0046] In FIG. 1, the interface between the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 is shown by a dotted line, which is a schematic representation of the oxide semiconductor stack 403. Depending on the material, film formation conditions, and heat treatment, the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 may be formed. In some cases, the interface between the oxide layer 102 and the oxide layer 102 may be unclear. In some cases, what can be called a mixed region or layer of the semiconductor layer may be formed. The same applies to the other drawings in this specification.

[0047] In the oxide semiconductor stack 403, the first oxide semiconductor layer 101 and the second oxide semiconductor The layers 102 may be stacked in any order as long as they have different energy gaps. I can't.

[0048] Specifically, in the oxide semiconductor stack 403, the energy gap between one of the oxide semiconductor layers is The energy gap of the other oxide semiconductor layer is set to 3 eV or more, and the energy gap of the other oxide semiconductor layer is set to less than 3 eV. .

[0049] The transistor 440a illustrated in FIG. 1A is a transistor in which a second oxide semiconductor layer is formed instead of a first oxide semiconductor layer 101. In this embodiment, the semiconductor layer 102 has a larger energy gap than the semiconductor layer 101. The first oxide semiconductor layer 101 in the transistor 440a is an In-Sn-Zn oxide. (energy gap 2.6 eV to 2.9 eV, typically 2.8 eV), second oxide The compound semiconductor layer 102 is an In-Ga-Zn oxide (also written as IGZO) film ( An energy gap of 3.0 eV to 3.4 eV, typically 3.2 eV, is used.

[0050] On the other hand, the transistor 440b illustrated in FIG. 1B has a second oxide semiconductor layer 102 and a second oxide semiconductor layer 103. In this embodiment, the oxide semiconductor layer 102 has a smaller energy gap. In the transistor 440b, the first oxide semiconductor layer 101 is made of In-Ga-Z The second oxide semiconductor layer 102 is an n-type oxide film (energy gap 3.2 eV). An In-Sn-Zn oxide film (energy gap 2.8 eV) is used.

[0051] In this manner, in the oxide semiconductor stack 403, the first oxide semiconductor layer 101 and the second oxide semiconductor layer The oxide semiconductor layer 102 has a larger energy gap on the side in contact with the gate insulating film 402. It may be a layer having a small energy gap.

[0052] FIG. 4A shows an oxide semiconductor stack 403 including a first oxide semiconductor layer 101 and a second oxide semiconductor layer 102. A transistor using a three-layer structure of a semiconductor layer 102 and a third oxide semiconductor layer 103. 480a is shown.

[0053] The transistor 480a is formed by forming a first oxide film over the substrate 400 on which the oxide insulating film 436 is provided. The semiconductor device includes an oxide semiconductor layer 101, a second oxide semiconductor layer 102, and a third oxide semiconductor layer 103. A stack of oxide semiconductor layers 403, a source electrode layer 405a, a drain electrode layer 405b, a gate insulator 405b, and a gate insulating film 406 are formed on the semiconductor substrate 401. The transistor 480a includes an insulating film 407 and a gate electrode layer 401. is formed.

[0054] In FIG. 4, the boundary between the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 The surface is shown by a dotted line, which is a schematic diagram of the oxide semiconductor stack 403. Depending on the material, the film formation conditions, and the heat treatment, the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 may be formed. In some cases, the interface with the semiconductor layer 102 may become unclear. In some cases, a region that can be called a mixed region or a mixed layer of the compound semiconductor layer may be formed. The same is true for the interface between the second oxide semiconductor layer 102 and the third oxide semiconductor layer 103.

[0055] In the oxide semiconductor stack 403 of the transistor 480a, the first oxide semiconductor layer 101 , the energy gaps of the second oxide semiconductor layer 102, and the third oxide semiconductor layer 103 are not all the same and contain at least two different energy gaps.

[0056] When the oxide semiconductor stack 403 has a stacked structure of three or more layers, all of the oxide semiconductor layers The energy gaps may be different, or may be approximately the same. The oxide semiconductor stack 403 may include an oxide semiconductor layer having a groove.

[0057] An oxide semiconductor stack 403 (a first oxide semiconductor layer 101, a second oxide semiconductor layer 102, The oxide semiconductor used for the third oxide semiconductor layer 103) is at least indium ( It is preferable that the material contains In or zinc (Zn). It is particularly preferable that the material contains In and Zn. In addition, a stabilizer for reducing the variation in electrical characteristics of a transistor using the oxide is also provided. It is preferable to have gallium (Ga) as an initiator in addition to the above. It is preferable to have tin (Sn) as a riser. Also, it is preferable to have hulled steel as a stabilizer. It is preferable that the alloy contains tungsten (Hf) as a stabilizer. It is preferred that the compound has the formula:

[0058] Other stabilizers include the lanthanides lanthanum (La) and cerium ( Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), hol Ho, Erbium, Thulium, Ytterbium, Ru The element may contain one or more of the elements tetraethynyl (Te) and tetraethynyl (Lu).

[0059] For example, oxide semiconductors include indium oxide, tin oxide, zinc oxide, and oxides of binary metals. In-Zn oxide, Sn-Zn oxide, Al-Zn oxide, Zn-Mg oxide, Oxides, Sn-Mg oxides, In-Mg oxides, In-Ga oxides, ternary metal oxides Oxides such as In-Ga-Zn oxides, In-Al-Zn oxides, and In-Sn-Zn oxides, Sn-Ga-Zn oxides, Al-Ga-Zn oxides, Sn-Al-Zn oxides Oxide, In-Hf-Zn oxide, In-La-Zn oxide, In-Ce-Zn oxide oxides, In-Pr-Zn oxides, In-Nd-Zn oxides, In-Sm-Zn oxides In-Eu-Zn oxide, In-Gd-Zn oxide, In-Tb-Zn oxide , In-Dy-Zn oxide, In-Ho-Zn oxide, In-Er-Zn oxide, In-Tm-Zn oxide, In-Yb-Zn oxide, In-Lu-Zn ​​oxide, In-Sn-Ga-Zn oxides and In-Hf-Ga-Zn oxides are oxides of the basic metals. oxides, In-Al-Ga-Zn oxides, In-Sn-Al-Zn oxides, In-Sn -Hf-Zn based oxides and In-Hf-Al-Zn based oxides can be used.

[0060] In this case, for example, In-Ga-Zn oxide is a material containing In, Ga, and Zn as main components. The ratio of In, Ga, and Zn does not matter. Metal elements other than a and Zn may be present.

[0061] In addition, as an oxide semiconductor, InMO3(ZnO) m (m>0 and m is not an integer) In addition, M may be selected from Ga, Fe, Mn, and Co. It indicates one or more metal elements. In2SnO5 (ZnO) n A material expressed as (n>0, and n is an integer) may be used.

[0062] For example, In:Ga:Zn=1:1:1 (=1 / 3:1 / 3:1 / 3) or In:G In-Ga-Zn oxide with an atomic ratio of a:Zn=2:2:1 (=2 / 5:2 / 5:1 / 5) The oxides of In:Sn:Zn=1: 1:1(=1 / 3:1 / 3:1 / 3), In:Sn:Zn=2:1:3(=1 / 3:1 / 6:1 / 2) or In:Sn:Zn=2:1:5(=1 / 4:1 / 8:5 / 8) It is advisable to use an In-Sn-Zn oxide having a molecular ratio or an oxide having a composition close to that.

[0063] However, the present invention is not limited to these, and can be applied to any semiconductor characteristics (mobility, threshold, variation, etc.) required. In order to obtain the required semiconductor characteristics, the appropriate composition should be used. Carrier density, impurity concentration, defect density, atomic ratio of metal elements to oxygen, interatomic bond length, density It is preferable to make the above appropriate.

[0064] For example, high mobility can be obtained relatively easily with In-Sn-Zn oxides. Therefore, in the case of In-Ga-Zn oxides, the mobility can be increased by lowering the defect density in the bulk. It can be done.

[0065] For example, the atomic ratio of In, Ga, and Zn is In:Ga:Zn=a:b:c(a+b+ The composition of the oxide with the atomic ratio of In:Ga:Zn=A:B:C (A+B+C = 1), a, b, and c are in the vicinity of the oxide composition (aA) 2 +(bB) 2 + (cC) 2 ≦r 2 The above condition is satisfied, and r can be set to, for example, 0.05. The same is true for compounds.

[0066] The oxide semiconductor may be single-crystalline or non-single-crystalline. In the latter case, it may be amorphous or polycrystalline. In addition, the structure may include a portion having crystallinity in the amorphous state, or a non-amorphous structure. That's fine too.

[0067] Since it is relatively easy to obtain a flat surface for an amorphous oxide semiconductor, This can reduce interface scattering when fabricating a transistor, and can be achieved relatively easily and with relatively high quality. Therefore, high mobility can be obtained.

[0068] In addition, in a crystalline oxide semiconductor, defects in the bulk can be further reduced, and the surface By improving the flatness of the oxide semiconductor, it is possible to obtain a mobility equal to or higher than that of an oxide semiconductor in an amorphous state. In order to improve the flatness of the surface, it is preferable to form an oxide semiconductor on a flat surface. Specifically, the average surface roughness (Ra) is 1 nm or less, preferably 0.3 nm or less, and more preferably It is preferable to form the surface on a thickness of 0.1 nm or less.

[0069] Ra is defined in JIS B 0601:2001 (ISO4287:1997). This is a three-dimensional extension of the arithmetic mean roughness, which is currently used, so that it can be applied to curved surfaces. It can be expressed as "the average of the absolute values ​​of the deviation from the specified surface" and is defined by formula (1).

[0070]

number

[0071] In the above, S0 is the measurement surface (coordinates (x1, y1) (x1, y2) (x2, y1 )(x2, y2)) and Z0 is the average height of the measurement surface. Ra refers to the strength of the atomic force microscope (AFM). It can be evaluated using OPE.

[0072] The first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 of the oxide semiconductor stack 403 As the third oxide semiconductor layer 103, an oxide semiconductor layer that contains crystals and has crystallinity (crystal The crystals in the crystalline oxide semiconductor layer can be aligned along the crystal axis. The orientation may be random or may have a certain orientation.

[0073] For example, the crystalline oxide semiconductor layer may be formed of an oxide semiconductor material having crystals with a c-axis approximately perpendicular to the surface. A nitride semiconductor layer can be used.

[0074] The oxide semiconductor layer including crystals having a c-axis approximately perpendicular to the surface does not have a single crystal structure, It is not an amorphous structure, but a crystalline oxide semiconductor with c-axis orientation (C Axis Aligned Crystalline Oxide Semiconductor; It is a membrane called CAAC-OS.

[0075] The CAAC-OS film is neither completely single crystalline nor completely amorphous. is an oxide semiconductor film with a crystalline-amorphous mixed phase structure having crystalline and amorphous parts in the amorphous phase. The crystal part must be small enough to fit within a cube with one side less than 100 nm. In addition, transmission electron microscopes (TEM) In the observation image by a microscope, the amorphous part and the The boundary between the crystal and the crystalline part is not clear. Therefore, the CAAC-OS film does not have any in-boundary defects. The resulting decrease in electron mobility is suppressed.

[0076] The crystal parts in the CAAC-OS film have c-axes that are normal vectors to the surface on which the CAAC-OS film is formed. The triangle is aligned parallel to the normal vector of the ab plane and perpendicular to the ab plane. The metal atoms are arranged in a layered or hexagonal shape when viewed perpendicular to the c-axis. Metal atoms and oxygen atoms are arranged in layers. The orientation of the a and b axes may be different. In this specification, when it is simply described as vertical, it means that The range of 5° to 95° is also included. This also includes the range from 1° to 5°.

[0077] In the CAAC-OS film, the distribution of the crystal parts may not be uniform. In the process of forming the C-OS film, when crystal growth is performed from the surface side of the oxide semiconductor film, The proportion of crystalline parts may be higher near the surface than near the growth surface. By adding impurities to the AC-OS film, the crystalline part becomes amorphous in the impurity-added region. It may also be pawned.

[0078] The c-axis of the crystal part in the CAAC-OS film is the normal vector of the surface on which the CAAC-OS film is formed. The CAAC-OS film shape (the shape of the film on which the film is formed) is Depending on the cross-sectional shape of the surface or the cross-sectional shape of the surface, the directions may differ from each other. The direction of the c-axis of the crystal is the normal vector of the surface on which the CAAC-OS film is formed. The direction of the crystal is parallel to the normal vector of the film or surface. is formed by carrying out a crystallization treatment such as a heat treatment after the film formation.

[0079] The electrical characteristics of transistors using CAAC-OS films change when exposed to visible or ultraviolet light. Therefore, the transistor has high reliability.

[0080] There are three methods for obtaining CAAC-OS films. The first method is to set the film formation temperature at 200°C. The oxide semiconductor layer is formed at a temperature of 500° C. or more, and the c-axis is aligned approximately perpendicular to the surface. The second method is to deposit a thin film and then heat it at a temperature between 200 and 700 degrees Celsius. The third method is to form a thin film with a c-axis orientation perpendicular to the surface. After that, heat treatment is performed at 200°C to 700°C to form the second layer, and the surface is roughly This is a method for vertically aligning the c-axis.

[0081] A first oxide semiconductor layer 101, a second oxide semiconductor layer 102, and a third oxide semiconductor layer 10 The thickness of the film 3 is 1 nm or more and 100 nm or less (preferably 5 nm or more and 30 nm or less). Sputtering method, MBE (Molecular Beam Epitaxy) method, CVD method, pulsed laser deposition method, ALD (Atomic Layer Deposition) The first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 can be formed by using a method or the like as appropriate. The oxide semiconductor layer 102 and the third oxide semiconductor layer 103 are formed on the surface of the sputtering target. In contrast, a sputtering device is used to perform film formation with multiple substrate surfaces set approximately perpendicular to the substrate. A film may be formed.

[0082] In a transistor including an oxide semiconductor layer, the energy gap of the oxide semiconductor layer For example, in a transistor using an oxide semiconductor layer, In a semiconductor device, when the energy gap of the oxide semiconductor layer is small, the on-characteristics (for example, On the other hand, the energy gap of the oxide semiconductor layer is large. If the gate insulating layer is not provided, the off-state current can be reduced.

[0083] Oxide semiconductor stack 40 using multiple oxide semiconductor layers having different energy gaps 3, transistor 440a, transistor 440b, transistor The electrical characteristics of the transistor 480a can be controlled more precisely, and the desired electrical characteristics can be obtained. 440a, transistor 440b, and transistor 480a.

[0084] For example, in the oxide semiconductor stack 403 of the transistor 480a in FIG. The energy gap of the second oxide semiconductor layer 102 is set to be equal to that of the first oxide semiconductor layer 101 and the third oxide semiconductor layer 102. The energy gap of the first oxide semiconductor layer 103 is set to be smaller than that of the second oxide semiconductor layer 103. The energy gaps of the semiconductor layer 101 and the third oxide semiconductor layer 103 are approximately the same. It is possible.

[0085] FIG. 4(C) shows the energy band diagram in the film thickness direction (between E1 and E2) in FIG. 4(A). In the transistor 480a, the first The first oxide semiconductor layer 101, the second oxide semiconductor layer 102, and the third oxide semiconductor layer 1 However, it is preferable to select a material having a buried channel in the conduction band. Therefore, it is not necessary to have a depression in both the conduction band and the valence band as shown in Figure 4(C). For example, the energy band diagram may have a depression only in the conduction band. A configuration that can obtain an energy band diagram may be used.

[0086] For example, the first oxide semiconductor layer 101 in the transistor 480a may be an In-Ga- Zn-based oxide film (energy gap 3.2 eV) as the second oxide semiconductor layer 102 is an In-Sn-Zn oxide film (energy gap 2.8 eV), and the third oxide semiconductor The layer 103 is an In-Ga-Zn oxide film (energy gap 3.2 eV). .

[0087] The three-layer oxide semiconductor stack 403 includes the first oxide semiconductor layer in the transistor 480a. The oxide semiconductor layer 101 is an In-Ga-Zn oxide film, and the second oxide semiconductor layer 10 The second oxide semiconductor layer 2 is an In-Zn oxide film, and the third oxide semiconductor layer 103 is an In-Ga-Zn The first oxide semiconductor layer 101 is a Ga-Zn-based oxide film, and the second oxide semiconductor layer 102 is a Ga-Zn-based oxide film. The oxide semiconductor layer 102 is an In-Sn-Zn oxide film, and the third oxide semiconductor layer 103 is an In-Sn-Zn oxide film. The first oxide semiconductor layer 101 is a stack of Ga-Zn oxide films. a In-Zn-based oxide film as the second oxide semiconductor layer 102; The semiconductor layer 103 may be a laminate of Ga-Zn oxide films.

[0088] The second oxide semiconductor layer 102 having a small energy gap is The insulating film is sandwiched between a first oxide semiconductor layer 101 and a third oxide semiconductor layer 103. This provides an effect of further reducing the off-state current (leakage current) of the transistor 480a. can be.

[0089] An example of a manufacturing method using the transistor 440a is shown in FIGS.

[0090] First, an oxide insulating film 436 is formed over a substrate 400 .

[0091] There is no significant limitation on the substrate that can be used for the substrate 400, but at least the substrate that can be used for the subsequent heat treatment is For example, barium borosilicate glass Glass substrates such as glass and aluminoborosilicate glass, ceramic substrates, quartz substrates, and sapphire substrates In addition, single crystal semiconductors such as silicon and silicon carbide can be used. Substrates, polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, SOI substrates, etc. Any of these substrates having semiconductor elements formed thereon is called a substrate 400. It may also be used as.

[0092] A semiconductor device may be manufactured using a flexible substrate as the substrate 400. In order to manufacture a semiconductor device having such a structure, a transistor including an oxide semiconductor stack 403 is formed on a flexible substrate. The transistor 440a may be directly formed on a substrate, or the transistor including the oxide semiconductor stack 403 may be formed on another substrate. The transistor 440a may be fabricated and then peeled off and transferred to a flexible substrate. In order to peel and transfer the transistor including the oxide semiconductor stack from the substrate to the flexible substrate, A release layer may be provided between the photoresist 440a and the photoresist 440b.

[0093] The oxide insulating film 436 is formed by a plasma CVD method, a sputtering method, or the like. Silicon, silicon oxynitride, aluminum oxide, aluminum oxynitride, hafnium oxide , gallium oxide, or a mixture of these materials.

[0094] The oxide insulating film 436 may be a single layer or a stacked layer. In this embodiment, the oxide insulating film 436 A silicon oxide film formed by sputtering is used.

[0095] Alternatively, a nitride insulating film may be provided between the oxide insulating film 436 and the substrate 400. The insulating film is made of silicon nitride or silicon oxide nitride by plasma CVD or sputtering. It is made of aluminum nitride, aluminum oxide nitride, or a mixture of these materials. It is possible.

[0096] Next, the first oxide semiconductor film 191 and the second oxide semiconductor film 192 were formed over the oxide insulating film 436. A stack of oxide semiconductor films 493 including the oxide semiconductor films 92 is formed (see FIG. 2A).

[0097] The oxide insulating film 436 is in contact with the stack of oxide semiconductor films 493 (the stack of oxide semiconductor films 403). Therefore, there is at least an amount of oxygen in the film (bulk) that exceeds the stoichiometric composition ratio. For example, when a silicon oxide film is used as the oxide insulating film 436, , SiO 2+α (where α>0). Using such an oxide insulating film 436 Therefore, oxygen can be supplied to the oxide semiconductor film stack 493 (the oxide semiconductor film stack 403). The oxide semiconductor film stack 493 (the oxide semiconductor film stack 4 03), oxygen vacancies in the film can be compensated for.

[0098] For example, the oxide insulating film 436 containing a large amount (excessive amount) of oxygen, which serves as an oxygen supply source, is formed as an oxide semiconductor. By providing the insulating film 493 (the oxide semiconductor stack 403) in contact with the insulating film 493, the oxide insulating film 493 Oxygen is supplied from the insulating film 436 to the oxide semiconductor film stack 493 (the oxide semiconductor stack 403). The oxide semiconductor film stack 493 (the oxide semiconductor stack 403) and the oxide insulating film The insulating film 436 is at least partially in contact with the oxide semiconductor film 436. Oxygen may be supplied to the stack 493 (the oxide semiconductor stack 403).

[0099] A stack of oxide semiconductor films 493 (a first oxide semiconductor film 191 and a second oxide semiconductor film 1 In the step of forming the oxide semiconductor film stack 493 (first oxide semiconductor film 191 In order to prevent hydrogen or water from being contained in the second oxide semiconductor film 192 as much as possible, 4, a stack of oxide semiconductor films 493 (a first oxide semiconductor film 191 and a second oxide semiconductor film As a pretreatment for the formation of the oxide insulating film 43 in the preheating chamber of the sputtering device, The substrate on which the oxide insulating film 436 is formed is preheated, and hydrogen, moisture, etc. adsorbed on the substrate and the oxide insulating film 436 are removed. It is preferable to remove impurities such as fluorine and fluorine from the preheating chamber and evacuate the chamber. The iopump is preferred.

[0100] The oxide insulating film 436 includes a stack of oxide semiconductor films 493 (the stack of oxide semiconductor films 403). The region formed in contact with the substrate may be subjected to a planarization treatment. However, polishing processes (e.g., Chemical Mechanical Polishing) Polishing (CMP), dry etching, and plasma processing are used. It is possible.

[0101] The plasma treatment may be, for example, a reverse sputtering treatment in which argon gas is introduced to generate plasma. Reverse sputtering is a process in which RF is applied to the substrate side in an argon atmosphere. This method involves applying voltage using a power supply to generate plasma in the vicinity of the substrate to modify the surface. Instead of the argon atmosphere, nitrogen, helium, oxygen, etc. may be used. When the oxide insulating film 436 is subjected to the cleaning, powdery substances (particles, dust, etc.) attached to the surface of the oxide insulating film 436 are removed. (also called) can be removed.

[0102] As the planarization process, the polishing process, the dry etching process, and the plasma process may be performed multiple times. In addition, when performing the steps in combination, the order of the steps is not particularly limited. The thickness is not limited to a specific value and may be appropriately set depending on the unevenness of the surface of the oxide insulating film 436.

[0103] Note that the first oxide semiconductor film 191 and the second oxide semiconductor film 192 are formed because oxygen is not contained therein. For example, a sputtering method is used under conditions where oxygen is abundant (100% oxygen atmosphere). The oxide semiconductor is preferably in a crystalline state. The film contains a region in which the oxygen content is excessive with respect to the stoichiometric composition ratio. preferable.

[0104] Note that in this embodiment, the first oxide semiconductor film 191 is formed by a sputtering method. For example, the composition ratio of the target for this purpose is In:Sn:Zn in terms of atomic ratio. , 1:2:2, 2:1:3, 1:1:1, or 20:45:35, etc. Using the get, an In-Sn-Zn-O film is formed.

[0105] Note that in this embodiment, the second oxide semiconductor film 192 is formed by a sputtering method. For example, the composition ratio of the target for this purpose is In2O3:Ga2O3:Zn. Using an oxide target with a molar ratio of O = 1:1:2, an In-Ga-Zn oxide film was formed. The material and composition of the target are not limited to this, and may be, for example, In2O3:G A metal oxide target having a molar ratio of A2O3:ZnO=1:1:1 may be used.

[0106] The filling rate of the metal oxide target is 90% or more and 100% or less, preferably 95% or more. By using a metal oxide target with a high filling rate, the film can be formed. In addition, the oxide semiconductor film can be a dense film.

[0107] The first oxide semiconductor film 191 and the second oxide semiconductor film 192 are formed using a sintered body. The sputtering gas is a high-purity gas from which impurities such as hydrogen, water, hydroxyl groups, or hydrides have been removed. It is preferable to use:

[0108] The substrate is held in a film-forming chamber that is kept in a reduced pressure state. Then, the remaining moisture in the film-forming chamber is removed. A sputtering gas from which hydrogen and moisture have been removed is introduced, and the substrate 40 is sputtered using the above target. 0, a stack of oxide semiconductor films 493 (a first oxide semiconductor film 191 and a second oxide semiconductor film In order to remove the residual moisture in the deposition chamber, an adsorption type vacuum pump is used. For example, a cryopump, an ion pump, or a titanium sublimation pump may be used. As the exhaust means, a turbo molecular pump with a cold trap is preferable. The deposition chamber evacuated using a cryopump may be filled with, for example, hydrogen atoms, water ( Compounds containing hydrogen atoms (and more preferably compounds containing carbon atoms) such as HO are exhausted. Therefore, the stack 493 of oxide semiconductor films formed in the film formation chamber (first oxide semiconductor film By using this, the concentration of impurities in the second oxide semiconductor film 191 and the second oxide semiconductor film 192 can be reduced.

[0109] In addition, a stack 493 of the oxide insulating film 436 and the oxide semiconductor film (the first oxide semiconductor film 191 and the second oxide semiconductor film 192) are preferably formed successively without exposure to the air. The stack 493 of the oxide insulating film 436 and the oxide semiconductor film (the first oxide semiconductor film 191 and the When the first oxide semiconductor film 192 and the second oxide semiconductor film 193 are successively formed without exposure to the air, an oxide insulating film is formed. This makes it possible to prevent impurities such as hydrogen and moisture from being adsorbed onto the surface of the film 436 .

[0110] The CAAC-OS film can be formed, for example, by sputtering a polycrystalline oxide semiconductor target. The sputtering target is used to form a film by sputtering. Upon impact, the crystalline regions in the sputtering target cleave from the ab plane, forming a -b: The particles peel off as plate-like or pellet-like sputtered particles with surfaces parallel to the surface. In this case, the plate-like sputtered particles may be crystalline and may be crystalline. By reaching the plate, a CAAC-OS film can be formed.

[0111] In addition, the following conditions are preferably applied to form the CAAC-OS film.

[0112] By reducing the amount of impurities mixed in during film formation, it is possible to prevent the crystal state from being destroyed by impurities. For example, the concentration of impurities (hydrogen, water, carbon dioxide, nitrogen, etc.) present in the film formation chamber is In addition, the impurity concentration in the deposition gas may be reduced. A deposition gas having a temperature of -80°C or lower, preferably -100°C or lower, is used.

[0113] In addition, by increasing the substrate heating temperature during film formation, the migration of sputtered particles after they reach the substrate is reduced. Specifically, the substrate heating temperature is set to 100° C. or higher and 740° C. or lower, preferably The deposition temperature is set to 200°C or higher and 500°C or lower. When a plate-shaped sputtered particle reaches a substrate, migration occurs on the substrate, The flat surface of the sputtered particle adheres to the substrate.

[0114] In addition, by increasing the oxygen ratio in the deposition gas and optimizing the power, plasma damage during deposition is reduced. The oxygen ratio in the deposition gas is preferably 30% by volume or more, and more preferably 100% by volume or more. The product is %.

[0115] As an example of a sputtering target, an In-Ga-Zn-O compound target is The details are shown below.

[0116] InO X powder, GaO Y Powder and ZnO Z The powders are mixed in a specified molar ratio and pressurized. Then, it is heated at a temperature between 1000℃ and 1500℃ to produce polycrystalline In-G The target is a-Zn-O compound. X, Y, and Z are any positive numbers. The specified mole ratio is, for example, InO X powder, GaO Y Powder and ZnO Z The powder, 2:2:1, 8:4:3, 3:1:1, 1:1:1, 4:2:3 or 3:1:2 mo The powder types and their mixing ratios depend on the sputtering process to be produced. The thickness may be appropriately changed depending on the target.

[0117] A stack of oxide semiconductor films 493 (a first oxide semiconductor film 191 and a second oxide semiconductor film 1 92) is photolithographically processed to form an island-shaped oxide semiconductor stack 403 (first oxide semiconductor The semiconductor layer is processed into a conductor layer 101 and a second oxide semiconductor layer 102 (see FIG. 2B).

[0118] In addition, a resist mask for forming an island-shaped oxide semiconductor stack 403 was formed by inkjet printing. If the resist mask is formed by the inkjet method, a photomask can be used. Since no additional wiring is required, manufacturing costs can be reduced.

[0119] Note that the etching of the oxide semiconductor film may be dry etching or wet etching. For example, an etchant used for wet etching of an oxide semiconductor film may be used. The cleaning solution can be a mixture of phosphoric acid, acetic acid, and nitric acid. O07N (manufactured by Kanto Chemical Co., Ltd.) may also be used.

[0120] In this embodiment, the first oxide semiconductor film 191 and the second oxide semiconductor film 192 are formed using the same Since the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 are formed by etching using a mask, The oxide semiconductor layer 102 has the same shape as the oxide semiconductor layer 101, and the end portions of the side surfaces of the oxide semiconductor layer 102 are aligned. In the conductor stack 403, the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 The sides (ends) are exposed.

[0121] In addition, excessive hydrogen (water or water) is added to the oxide semiconductor stack 403 (the oxide semiconductor film stack 493). Heat treatment may be performed to remove (dehydrate or dehydrogenate) the carboxylic acid (including the acid group). The treatment temperature is 300°C to 700°C, or lower than the distortion point of the substrate. The process can be carried out under reduced pressure or in a nitrogen atmosphere. The substrate is placed in a furnace, and the oxide semiconductor stack 403 (the oxide semiconductor film stack 493) is Heat treatment is carried out at 450° C. for 1 hour in a nitrogen atmosphere.

[0122] The heat treatment device is not limited to an electric furnace, and may be a heat treatment device using heat conduction or heat from a heating element such as a resistance heating element. A device that heats the workpiece by radiation may be used. For example, a GRTA (Gas Reactor Transformer) apid Thermal Anneal) equipment, LRTA (Lamp Rapid T RTA (Rapid Thermal Anneal) equipment, etc. al) equipment can be used. The LRTA equipment can be a halogen lamp, a metal halide lamp, lamp, xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp This is a device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp or other light source. The GRTA device is a device that uses high-temperature gas to perform heat treatment. Inert gases such as argon or nitrogen that do not react with the workpiece during heat treatment An active gas is used.

[0123] For example, the substrate is placed in an inert gas heated to a high temperature of 650°C to 700°C as a heat treatment. After heating for several minutes, GRTA may be performed in which the substrate is taken out of the inert gas.

[0124] In the heat treatment, nitrogen or a rare gas such as helium, neon, or argon is used. It is preferable that the nitrogen or hydrogen introduced into the heat treatment device is not included. The purity of rare gases such as sodium, neon, and argon is preferably 6N (99.9999%) or higher. is 7N (99.99999%) or more (i.e. impurity concentration is 1 ppm or less, preferably 0.1 It is preferable to set the concentration to less than ppm.

[0125] In addition, after the oxide semiconductor stack 403 (the oxide semiconductor film stack 493) is heated by heat treatment, In the same furnace, high-purity oxygen gas, high-purity dinitrogen monoxide gas, or ultra-dry air (CRDS ( The moisture content measured using a cavity ring-down laser spectroscopy (CDR) dew point meter is 20 ppm or less (-55°C in terms of dew point), preferably 1 ppm or less, more preferably 10 ppb or less) may be introduced. Oxygen gas or nitrous oxide gas may be mixed with water, hydrogen, etc. It is preferable that the oxygen gas or the dioxygen gas introduced into the heat treatment device does not contain the above-mentioned. The purity of the nitrogen gas is 6N or more, preferably 7N or more (i.e., oxygen gas or nitrous oxide gas). It is preferable to keep the impurity concentration in the gas at 1 ppm or less, preferably 0.1 ppm or less. Impurities due to dehydration or dehydrogenation treatment by the action of oxygen gas or nitrous oxide gas. The oxide semiconductor's main component, oxide, was also reduced during the removal process. By supplying the oxygen, the oxide semiconductor stack 403 (the stack 493 of oxide semiconductor films) is formed. It can be highly purified and electrically made into I-type (intrinsic).

[0126] Note that the heat treatment for dehydration or dehydrogenation is performed after the stack 493 of oxide semiconductor films (first oxide After the formation of the first oxide semiconductor film 191 and the second oxide semiconductor film 192, and before the formation of the insulating film 407 In this case, the step may be performed at any timing in the process of manufacturing the transistor 440a. For example, a stack of oxide semiconductor films 493 (a first oxide semiconductor film 191 and a second oxide semiconductor film After the formation of the oxide semiconductor film 192, or after the formation of the island-shaped oxide semiconductor stack 403 (the first oxide semiconductor layer 10 This can be performed after the formation of the first and second oxide semiconductor layers 102).

[0127] The heat treatment for dehydration or dehydrogenation may be carried out multiple times or may be carried out in combination with other heat treatments. For example, after the first oxide semiconductor film 191 is formed and after the second oxide semiconductor film 19 After formation, heat treatment may be carried out twice.

[0128] The heat treatment for dehydration or dehydrogenation is performed on the oxide semiconductor stack 403 (the first oxide semiconductor Before being processed into islands as the oxide semiconductor layer 101 and the second oxide semiconductor layer 102, The stack 493 (the first oxide semiconductor film 191 and the second oxide semiconductor film 192) is an oxide If the heat treatment is performed while the insulating film 436 is covering the oxide insulating film 436, oxygen contained in the oxide insulating film 436 is oxidized by the heat treatment. This is preferable because it is possible to prevent the release of the amine compound by the addition of the amine compound.

[0129] Next, a source electrode layer and a drain electrode layer (the same layer as this The conductive film is formed to be a wiring (including wiring formed by the method described above). As a conductive film used for the source electrode layer and the drain electrode layer, for example, A metal film containing an element selected from Al, Cr, Cu, Ta, Ti, Mo, and W, or the above-mentioned Metal nitride films containing the above elements (titanium nitride film, molybdenum nitride film, tungsten nitride film) In addition, the lower or upper side of a metal film such as Al or Cu may be used. Both are made of high melting point metal films such as Ti, Mo, W, etc. or their metal nitride films (titanium nitride film A laminated structure of a silicon nitride film, a molybdenum nitride film, and a tungsten nitride film may also be used. The conductive film used for the source electrode layer and the drain electrode layer is formed of a conductive metal oxide. Conductive metal oxides include indium oxide (In2O3) and tin oxide (SnO 2), zinc oxide (ZnO), indium oxide tin oxide (In2O3-SnO2), indium oxide Indium zinc oxide (In2O3-ZnO) or silicon oxide on these metal oxide materials can be used.

[0130] A resist mask is formed on the conductive film by a photolithography process, and selective etching is performed. After forming the source electrode layer 405a and the drain electrode layer 405b by this, a resist mask In this embodiment, the source electrode layer 405a and the drain electrode layer 405b are A tungsten film having a thickness of 10 nm is formed. In this manner, the source electrode layer 405a and the drain electrode layer 405b are If the electrode layer 405b is thin, the coverage of the gate insulating film 402 formed thereon is good. In addition, when a dopant is introduced into the oxide semiconductor stack 403 in order to form a low-resistance region, , passing through the source electrode layer 405a and the drain electrode layer 405b, A dopant can also be introduced into the oxide semiconductor stack 403 below the drain electrode layer 405b. do.

[0131] In the oxide semiconductor stack 403, the first oxide semiconductor layer 101 and the second oxide semiconductor Since the side (end) of the layer 102 is exposed, the source electrode layer 405a and the drain electrode layer 4 05b is a portion of the side surface of the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102. It is formed so as to be in contact.

[0132] Next, the oxide semiconductor stack 403, the source electrode layer 405a, and the drain electrode layer 405b are A gate insulating film 402 is formed to cover the gate insulating film 402 (see FIG. 2C).

[0133] In order to improve the coverage of the gate insulating film 402, the oxide semiconductor stack 403 and the The above-described planarization treatment may also be performed on the surfaces of the source electrode layer 405a and the drain electrode layer 405b. In particular, when a thin insulating film is used as the gate insulating film 402, the oxide semiconductor stack 40 3. The surfaces of the source electrode layer 405a and the drain electrode layer 405b have good flatness. is preferred.

[0134] The thickness of the gate insulating film 402 is set to 1 nm or more and 20 nm or less. Methods such as a CVD method, a pulsed laser deposition method, and an ALD method can be used as appropriate. The insulating film 402 is formed by depositing a plurality of substrate surfaces approximately perpendicular to the sputtering target surface. The film may be formed using a sputtering device that performs film formation in a set state.

[0135] The gate insulating film 402 may be a silicon oxide film, a gallium oxide film, an aluminum oxide film, A silicon nitride film, a silicon oxynitride film, an aluminum oxynitride film, or a silicon nitride oxide film The gate insulating film 402 can be formed using an oxide semiconductor stack 403 and a It is preferable that the contact portion contains oxygen. Preferably, oxygen is present in the mixture in an amount at least greater than the stoichiometric ratio. For example, when a silicon oxide film is used as the gate insulating film 402, SiO 2+α ( In this embodiment, the gate insulating film 402 is made of SiO 2+α (where α>0) is used. This silicon oxide film is used as the gate insulating film. By using the oxide semiconductor layer 402, oxygen can be supplied to the oxide semiconductor stack 403, and the characteristics can be improved. Furthermore, the gate insulating film 402 can improve the surface roughness of the transistor to be manufactured. It is preferable to form the gate insulating film 402 in consideration of the noise and the step coverage of the gate insulating film 402 .

[0136] The material of the gate insulating film 402 is hafnium oxide, yttrium oxide, hafnium Silicate (HfSi x O y x>0, y>0), nitrogen-doped hafnium silicate (HfSiO x N y (x>0, y>0)), hafnium aluminate (HfAl x O y (x>0, y>0)), and the use of high-k materials such as lanthanum oxide allows the gate Furthermore, the gate insulating film 402 may have a single layer structure or a multilayer structure. It can also be used as a structure.

[0137] Then, the gate electrode layer 401 is formed by plasma CVD or sputtering. The gate electrode layer 401 is formed on the insulating film 402. Metallic materials such as tinsten, aluminum, copper, chromium, neodymium, scandium, etc. The gate electrode layer 401 can be formed using an alloy material containing these metals as main components. Semiconductor films, such as polycrystalline silicon films doped with impurity elements such as phosphorus, A silicide film such as nickel silicide may be used. The gate electrode layer 401 has a single-layer structure. Alternatively, a laminated structure may be used.

[0138] The material of the gate electrode layer 401 is indium tin oxide or indium oxide containing tungsten oxide. Indium oxide, indium zinc oxide with tungsten oxide, indium zinc oxide with titanium oxide Indium oxide, indium tin oxide with titanium oxide, indium zinc oxide, silicon oxide A conductive material such as indium tin oxide doped with the above-mentioned conductive material can also be used. It is also possible to use a laminated structure of an electrically conductive material and the above-mentioned metal material.

[0139] In addition, a layer of the gate electrode layer 401 in contact with the gate insulating film 402 is made of a metal oxide containing nitrogen. In-Ga-Zn-O films containing nitrogen and In-Sn-O films containing nitrogen , In-Ga-O film containing nitrogen, In-Zn-O film containing nitrogen, Sn- O film, nitrogen-containing In-O film, and metal nitride film (InN, SnN, etc.) can be used. These films have a work function of 5 electron volts or more, preferably 5.5 electron volts or more. When used as a gate electrode layer, the threshold voltage of the electrical characteristics of a transistor is increased to a positive value. Thus, a so-called normally-off switching element can be realized.

[0140] Through the above steps, the transistor 440a of this embodiment is manufactured (see FIG. 2D). A plurality of oxide semiconductor layers having different energy gaps (first oxide semiconductor layer 101 The oxide semiconductor stack 403 including the first oxide semiconductor layer 102 and the second oxide semiconductor layer 103 is used. As a result, the electrical characteristics of the transistors 440a and 440b can be controlled with greater precision. This allows the transistors 440a and 440b to have desired electrical characteristics.

[0141] Next, the oxide semiconductor stack 403, the source electrode layer 405a, the drain electrode layer 405b, An insulating film 407 is formed on the gate insulating film 402 and the gate electrode layer 401 (see FIG. 2(E)). .

[0142] The insulating film 407 is formed by a plasma CVD method, a sputtering method, a vapor deposition method, or the like. The insulating film 407 is typically a silicon oxide film, a silicon oxynitride film, or a silicon oxide nitride film. For example, an inorganic insulating film such as an aluminum oxide film or a gallium oxide film can be used.

[0143] The insulating film 407 may be an aluminum oxide film, a hafnium oxide film, or a magnesium oxide film. film, zirconium oxide film, lanthanum oxide film, barium oxide film, or metal nitride film (e.g. , aluminum nitride film) can also be used.

[0144] The insulating film 407 may be a single layer or a multilayer, for example, a silicon oxide film and an aluminum oxide film. A stack of the above can be used.

[0145] The insulating film 407 is formed by mixing impurities such as water and hydrogen into the insulating film 407 by a method such as sputtering. In addition, the insulating film 407 is preferably formed by using an appropriate method. If the insulating film in contact with the conductor stack 403 is a film containing excess oxygen, the oxide semiconductor stack 40 This is preferred because it provides a source of oxygen to 3.

[0146] In this embodiment, a silicon oxide film having a thickness of 100 nm is formed as the insulating film 407 by sputtering. The silicon oxide film is formed by sputtering. Typically, under an argon atmosphere, oxygen atmosphere, or a mixture of rare gas and oxygen atmosphere. This can be done.

[0147] In order to remove residual moisture in the deposition chamber of the insulating film 407, similarly to the deposition of the oxide semiconductor film, It is preferable to use an adsorption type vacuum pump (such as a cryopump). The concentration of impurities contained in the insulating film 407 formed in the film formation chamber evacuated by using a vacuum pump can be reduced. In addition, as an exhaust means for removing residual moisture in the film forming chamber of the insulating film 407, a turbo A molecular pump plus a cold trap may also be used.

[0148] The insulating film 407 is formed using a sputtering gas of hydrogen, water, a hydroxyl group, or hydrogen. It is preferable to use a high-purity gas from which impurities such as oxides have been removed.

[0149] As shown in FIG. 3B, an insulating film is provided as an interlayer insulating film over the transistor 440d. As a film, an insulating film 416 is formed between the transistor 440d and the insulating film 407, and an interlayer insulating film The insulating film 416 may be formed using a material and a method similar to those of the insulating film 407. For example, an aluminum oxide film can be used as the insulating film 416. By using a silicon oxide film as 407, the insulating film provided on the transistor 440d can be formed. For example, a laminate of an aluminum oxide film and a silicon oxide film can be used. The transistor 440d is formed by etching the gate insulating film 402 using the gate electrode layer 401 as a mask. The oxide semiconductor stack 403 is exposed by a lithography process. In this example, the insulating film 416 is provided so as to be in contact with the insulating film 416 .

[0150] The insulating film 407 and the insulating film 416 can be formed over the oxide semiconductor stack 403. The aluminum oxide film that can be formed is permeable to both impurities such as hydrogen and moisture, and oxygen. It has a high blocking effect that does not let anything pass through.

[0151] Therefore, the aluminum oxide film is free from hydrogen, which is a variable factor during and after the manufacturing process. Impurities such as moisture may be mixed into the oxide semiconductor stack 403, and the main components of the oxide semiconductor may be It functions as a protective film that prevents oxygen, which is a separation material, from being released from the oxide semiconductor stack 403. .

[0152] In addition, a planarizing insulating film may be formed to reduce surface irregularities caused by the transistors. The smoothing insulating film is made of organic materials such as polyimide, acrylic, and benzocyclobutene resins. In addition to the above organic materials, low-dielectric constant materials (low-k materials) can be used. In addition, by stacking a plurality of insulating films made of these materials, A planarizing insulating film may be formed.

[0153] In addition, openings reaching the source electrode layer 405a and the drain electrode layer 405b are formed in the insulating film 407. A wiring layer is formed in the opening and electrically connected to the source electrode layer 405a and the drain electrode layer 405b. The wiring layer may be used to connect to other transistors to form various circuits. It is possible.

[0154] The source electrode layer 405a and the drain electrode layer 405b are The etching process for forming the opening reaching the layer 405b results in partial over-etching. The source electrode layer and the drain electrode layer may have a laminated structure. A conductive film that also functions as a gate stopper is provided as a source electrode layer and a drain electrode layer. It is possible.

[0155] As shown in FIG. 3A, the transistor 440c has a source electrode layer and a drain electrode layer stacked thereon. This is an example of a layered structure, and the source electrode layer 404a and the source electrode layer 40 5a, the drain electrode layer 404b and the drain electrode layer 405b are laminated as the drain electrode layer. As in the transistor 440c, the gate insulating film 402, the insulating film 407, and The source electrode layer 405a and the drain electrode layer 405b are connected to the source electrode layer 404a and the drain electrode An opening is formed so as to reach the layer 404b, and the source electrode layer 404a and the drain electrode layer 404b are formed in the opening. Alternatively, wiring layers 465a and 465b may be formed to electrically connect to the wiring layers 465a and 465b.

[0156] In the transistor 440c, the source electrode layer 404a and the drain electrode layer 404b are formed as openings. The source electrode layer 404a also functions as an etching stopper during formation. The source electrode layer 405a is a tungsten film or a tantalum nitride film. The drain electrode layer 405b can be formed using a copper film, an aluminum film, or the like. The source electrode layer 404a, the source electrode layer 405a, the drain electrode layer 404b, and the drain electrode layer 405c can be formed. When the thickness of the layered film of the drain electrode layer 405b is set to about 5 nm or more and 15 nm or less, This can improve the coverage of the gate insulating film 402.

[0157] The wiring layer 465a and the wiring layer 465b are connected to the gate electrode layer 401, the source electrode layer 405a, and the drain electrode layer 405b. The wiring layer 405b can be formed using the same material and method as the wiring layer 405b. 465a, and a wiring layer 465b are a laminate of a tantalum nitride film and a copper film, or a tantalum nitride film and A lamination with a tungsten film can be used.

[0158] A sidewall insulating layer may be provided on the side surface of the gate electrode layer 401. After forming an insulating film covering the electrode layer 401, this is etched by RIE (Reactive ion etching). The insulating film is applied by anisotropic etching using the reactive ion etching (RIE) method. Then, a sidewall insulating layer may be formed in a self-aligned manner on the sidewall of the gate electrode layer 401. The insulating film is not particularly limited. For example, TEOS (Tetraethyl-Ortho o-Silicate) or silane, etc., reacted with oxygen or nitrous oxide, etc. The insulating film is made of silicon oxide, which has good step coverage. Formed by methods such as Zuma CVD, atmospheric pressure CVD, bias ECRCVD, and sputtering In addition, low temperature oxidation (LTO) is also possible. Silicon oxide formed by a deposition method may also be used.

[0159] The oxide semiconductor stack 403, which is highly purified and has oxygen vacancies filled, is free from impurities such as hydrogen and water. The hydrogen concentration in the oxide semiconductor stack 403 was 5×10 19 atom s / cm 3 Less than or equal to 5×10 18 atoms / cm 3 The oxide is as follows. The hydrogen concentration in the semiconductor stack 403 was measured by secondary ion mass spectrometry (SIMS). This is measured by y Ion Mass Spectrometry.

[0160] The oxide film produced by the present embodiment is highly purified and contains an excess of oxygen to compensate for the oxygen deficiency. The transistor 440a using the stacked layer of semiconductor layers 403 has a current value in an off state (off current The current value was set at 100 zA / μm (1 zA (zeptoampere)) per 1 μm of channel width at room temperature. ) is 1 × 10 -21 A) or less, preferably 10zA / μm or less, more preferably 1zA / It is possible to reduce the capacitance to a level of 100 yA / μm or less, more preferably to a level of 100 yA / μm or less.

[0161] As described above, semiconductor devices that meet various objectives such as high functionality, high reliability, and low power consumption can be provided. can be provided.

[0162] (Embodiment 2) In this embodiment mode, another embodiment of a semiconductor device and a manufacturing method of the semiconductor device will be described with reference to FIGS. The parts and steps having the same or similar functions as those in the above embodiment are the same as those in the above embodiment. The embodiment can be carried out in the same manner as in the first embodiment, and the repeated explanation will be omitted. The details are omitted.

[0163] In this embodiment, in a manufacturing method of a semiconductor device according to the disclosed invention, The oxide semiconductor stack that has been subjected to the oxidation treatment is subjected to oxygen (at least oxygen radicals, oxygen atoms, oxygen An example of supplying oxygen into the film by introducing oxygen ions (including either an ion or an elemental ion) will be described.

[0164] By the dehydration or dehydrogenation treatment, oxygen, which is a main component material of the oxide semiconductor, is simultaneously In the oxide semiconductor stack, oxygen may be released from the portion where oxygen is released, and the amount of oxygen may decrease. In the present embodiment, oxygen vacancies exist, and the oxygen vacancies cause a change in the electrical characteristics of the transistor. -level occurs.

[0165] Therefore, it is preferable to supply oxygen to the oxide semiconductor stack that has been subjected to dehydration or dehydrogenation treatment. By supplying oxygen to the oxide semiconductor stack, oxygen vacancies in the film can be compensated for. By using the oxide semiconductor stack in a transistor, a transistor caused by oxygen vacancies can be prevented. By reducing the variation in the threshold voltage Vth of the transistor and the threshold voltage shift ΔVth, In addition, the threshold voltage can be shifted in the positive direction to make the transistor normally off. It is also possible.

[0166] FIG. 5A corresponds to FIG. 2C, and shows a substrate 400 provided with an oxide insulating film 436. A first oxide semiconductor layer 101 and a second oxide semiconductor layer 102 having different energy gaps are formed on the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 having different energy gaps. The oxide semiconductor stack 403 including the layer 102, the source electrode layer 405a, and the drain electrode layer 405 b, a gate insulating film 402 is formed.

[0167] Next, oxygen 431 (at least an oxygen radical, an oxygen atom, or an oxygen atom) is added to the oxide semiconductor stack 403. ions, or ions that are the same or different from the cations, to form the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102. The oxygen excess regions 111 and 112 are formed in the oxide semiconductor stack 403 including the oxide semiconductor layer 102. (See FIG. 5(B)).

[0168] The oxygen excess regions 111 and 112 have a stoichiometric composition when the oxide semiconductor is in a crystalline state. The region includes at least a portion where the oxygen content is excessive relative to the ratio. The oxygen 431 supplied to the excess regions 111 and 112 causes the first oxide semiconductor layer 101 and oxygen vacancies present in the oxide semiconductor stack 403 including the second oxide semiconductor layer 102. It can be compensated for.

[0169] On the oxide semiconductor stack 403 having the oxygen excess regions 111 and 112 and the gate insulating film 402 A gate electrode layer 401 is formed, and a transistor 430 is manufactured (see FIG. 5C).

[0170] Oxygen is introduced into the oxide semiconductor stack 403 that has been subjected to dehydration or dehydrogenation treatment. By supplying the oxide semiconductor layer 403, the oxide semiconductor layer 403 is highly purified and becomes an i-type (intrinsic) oxide semiconductor layer. A transistor having the highly purified and i-type (intrinsic) oxide semiconductor stack 403 can be formed. The change in electrical characteristics of the sintered body 430 is suppressed, and the sintered body 430 is electrically stable.

[0171] The oxygen introduction method includes ion implantation, ion doping, plasma immersion An implantation method, a plasma treatment, or the like can be used.

[0172] In the case where oxygen is introduced into the oxide semiconductor stack 403, the oxide semiconductor stack 40 3 or through other films such as the gate insulating film 402 and the insulating film 407. Oxygen may be introduced into the oxide semiconductor stack 403. When oxygen is introduced through another film, Ion implantation method, ion doping method, plasma immersion ion implantation method In the case where oxygen is directly introduced into the exposed oxide semiconductor stack 403, , plasma treatment, etc. can also be used.

[0173] Oxygen can be introduced into the oxide semiconductor stack 403 after dehydration or dehydrogenation treatment. In addition, the oxide semiconductor stack that has been subjected to the dehydration or dehydrogenation treatment may be Oxygen may be introduced into 403 multiple times.

[0174] For example, in the first embodiment, oxygen is introduced into the oxide semiconductor stack 403 by absorbing oxygen from the exposed oxide A source electrode layer 405 is formed on the stack of the oxide semiconductor films 403 or the stack of the oxide semiconductor films 403. a, after forming the drain electrode layer 405b, the gate insulating film 402, the gate electrode layer 401 This can be performed after the formation of the insulating film 407 (after the formation of the insulating film 416).

[0175] In addition, oxygen is introduced into the oxygen-excess regions 111 and 112 in the oxide semiconductor stack 403. The oxygen concentration introduced by the process is 1×10 18 atoms / cm 3 5×10 or more 21 at oms / cm 3 It is preferable that:

[0176] In an oxide semiconductor, oxygen is one of the main components. The oxygen concentration in the conductor laminate 403 was measured by SIMS (Secondary Ion Mass Spectroscopy). It is difficult to estimate accurately using methods such as NMR spectrometer. It is difficult to determine whether oxygen has been intentionally added to the oxide semiconductor stack 403. It can be said that.

[0177] By the way, oxygen has 17 O and 18 There are isotopes such as O and their existence in nature The ratios of these atoms in the oxygen system are known to be approximately 0.037% and 0.204% of all oxygen atoms, respectively. In other words, when these isotopes are intentionally added to the oxide semiconductor stack 403, The concentrations of these isotopes can be estimated by methods such as SIMS. By measuring the oxygen concentration in the oxide semiconductor stack 403, it is possible to estimate the oxygen concentration more accurately. Therefore, by measuring the concentrations of these, it is possible to determine whether the oxide semiconductor stack 403 is intentionally formed. Alternatively, it may be possible to determine whether oxygen has been added intentionally.

[0178] After oxygen is introduced into the oxide semiconductor film, heat treatment is preferably performed.

[0179] As in the transistor 430 of this embodiment, oxygen is directly introduced into the oxide semiconductor stack 403. In this case, the oxide insulating film 436 in contact with the oxide semiconductor stack 403 and the gate insulating film 402 The film does not necessarily have to contain a large amount of oxygen. In order to prevent hydrogen from being desorbed from the layer 403, and to prevent impurities including hydrogen, water, etc. from being desorbed from the oxide semiconductor The layer 403 is protected from impurities such as oxygen, hydrogen, and water, including hydrogen, so that they do not re-enter the layer 403. It is preferable to provide a film having a high insulating effect (blocking effect) as the insulating film 407. For example, Oxidation that has a high blocking effect against both impurities such as hydrogen and moisture, and oxygen. An aluminum film or the like may be used.

[0180] Of course, the oxide insulating film 436 and the gate insulating film 402 in contact with the oxide semiconductor film are formed by removing oxygen. Further, oxygen is directly introduced into the oxide semiconductor stack 403, and oxygen is supplied by a plurality of methods. The law may be carried out.

[0181] In this embodiment, oxygen is introduced into the oxide semiconductor stack 403 as an example. The introduction of the element was performed on the gate insulating film 402 and the oxide insulating film 436, which are in contact with the oxide semiconductor stack 403. The insulating film 416, the insulating film 407, and the like may be formed using the oxide semiconductor film. Oxygen is introduced into the gate insulating film 402, the oxide insulating film 436, the insulating film 416, and the insulating film 407. By providing an excess of oxygen, oxygen can be supplied to the oxide semiconductor stack 403. Cut.

[0182] As described above, a semiconductor device including a stack of oxide semiconductor layers and having stable electrical characteristics is provided. Therefore, a highly reliable semiconductor device can be provided.

[0183] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0184] (Embodiment 3) In this embodiment mode, another embodiment of a semiconductor device and a manufacturing method of the semiconductor device will be described with reference to FIGS. The parts and steps having the same or similar functions as those in the above embodiment are the same as those in the above embodiment. The embodiment can be carried out in the same manner as in the first embodiment, and the repeated explanation will be omitted. The details are omitted.

[0185] In this embodiment, in a method for manufacturing a semiconductor device according to the disclosed invention, This is an example of forming a low-resistance region in a layer. The low-resistance region is formed by changing the conductivity of the oxide semiconductor stack. The semiconductor layer can be formed by introducing an impurity (also called a dopant) that causes the semiconductor layer to have a high conductivity.

[0186] FIG. 6A corresponds to FIG. 2D, and shows a substrate 400 provided with an oxide insulating film 436. A first oxide semiconductor layer 101 and a second oxide semiconductor layer 102 having different energy gaps are formed on the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 having different energy gaps. The oxide semiconductor stack 403 including the layer 102, the source electrode layer 405a, and the drain electrode layer 405 b, a gate insulating film 402 and a gate electrode layer 401 are formed.

[0187] Next, a gate insulating film 4 is formed on the oxide semiconductor stack 403 using the gate electrode layer 401 as a mask. 02, the dopant 421 passes through the source electrode layer 405a and the drain electrode layer 405b. is selectively introduced to form low resistance regions 121a, 121b, 122a, and 122b.

[0188] In this embodiment, the source electrode layer 405a and the drain electrode layer 405b are formed as thin films. Therefore, the oxide semiconductor stack 403 below the source electrode layer 405a and the drain electrode layer 405b The dopant 421 is introduced into the low resistance regions 121a, 121b, 122a, and 122b. An example of the generated data is shown below.

[0189] The thicknesses of the source electrode layer 405a and the drain electrode layer 405b and the amount of the dopant 421 introduced Depending on the conditions, the oxide semiconductor under the source electrode layer 405a and the drain electrode layer 405b If the dopant 421 is not introduced into the stack 403, the concentration is low and the source voltage A region having a higher resistance than a low-resistance region other than the electrode layer 405a or the drain electrode layer 405b. In addition, depending on the conditions for introducing the dopant 421, the first oxide semiconductor The dopant 421 is introduced only into the layer 101 and the second oxide semiconductor layer 102. When a region is formed, the first oxide semiconductor layer 101 and the second oxide semiconductor layer 102 There may be a dopant concentration distribution in the semiconductor.

[0190] The dopant 421 is an impurity that changes the electrical conductivity of the oxide semiconductor stack 403. Panto 421 contains group 15 elements (typically phosphorus (P), arsenic (As), and ammonium ions). Sb), boron (B), aluminum (Al), nitrogen (N), argon (Ar ), helium (He), neon (Ne), indium (In), fluorine (F), chlorine (C l), titanium (Ti), and zinc (Zn) are used. can be done.

[0191] The dopant 421 is implanted into the insulating film 407, the source electrode layer 405a, and the drain electrode layer 405b. The dopant 421 passes through the oxide electrode layer 405b and is introduced into the oxide semiconductor stack 403. The introduction methods include ion implantation, ion doping, and plasma immersion ion implantation. In this case, the dopant 421 alone can be used. It is preferable to use ions of fluoride or chloride.

[0192] The dopant 421 introduction process is carried out by controlling the implantation conditions such as the acceleration voltage and the dose amount, and the insulating layer through which the dopant 421 is passed. The thickness of the insulating film 407 may be appropriately set and controlled. Boron is used as the dopant, and boron ions are implanted by ion implantation. The dose of 21 is 1×10 13 ions / cm 2 5×10 or more 16 ions / cm 2 below This can be done as follows.

[0193] The concentration of dopant 421 in the low resistance region is 5×10 18 / cm 3 More than 1×10 22 / cm 3 It is preferable that:

[0194] The dopant 421 may be introduced while the substrate 400 is being heated.

[0195] Note that the process of introducing the dopant 421 into the oxide semiconductor stack 403 may be performed multiple times. In addition, a plurality of dopants may be used.

[0196] After the dopant 421 is introduced, a heat treatment may be performed. The temperature is 300°C to 700°C, preferably 300°C to 450°C, for 1 hour in an oxygen atmosphere. It is preferable to carry out the heating under nitrogen atmosphere, reduced pressure, or air (ultra-dry air). Processing may be carried out.

[0197] When the oxide semiconductor stack 403 is a crystalline oxide semiconductor film, the dopant 421 is introduced. In this case, the heat treatment is performed after the introduction of the dopant 421. By performing this treatment, the crystallinity of the oxide semiconductor stack 403 can be restored.

[0198] Therefore, in the oxide semiconductor stack 403, the low-resistance regions 121c are sandwiched between the channel formation region 121c. The first oxide semiconductor layer 101 in which the first oxide semiconductor layer 121a and the first oxide semiconductor layer 121b are provided and the channel formation region 12 A second oxide semiconductor layer 102 in which low-resistance regions 122a and 122b are provided with a second oxide semiconductor layer 102 and a second oxide semiconductor layer 102c sandwiched therebetween. is formed.

[0199] Through the above steps, the transistor 420 of this embodiment is manufactured (see FIG. 6B).

[0200] In addition, like the transistor 440d described in Embodiment 1, the gate insulating film 402 is The oxide semiconductor stack 403 is partially exposed by etching using the electrode layer 401 as a mask. In the transistor in contact with the insulating film 416, a dopant is introduced to form a low resistance region. A transistor 425 having the above structure is shown in FIG.

[0201] The transistor 425 is formed by introducing a dopant using the gate electrode layer 401 as a mask. The low resistance regions 121a, 121b, 122a, 122c are sandwiched between the hole formation regions 121c, 122c. 22b. Also, a source electrode layer through which the dopant is introduced, The drain electrode layer may also be doped with dopants. The dopant is also introduced into the source electrode layer and the drain electrode layer, and the source electrode layer 4 containing the dopant 15a, which is an example of a drain electrode layer 415b containing a dopant.

[0202] Low resistance regions 121a and 121b are provided on either side of a channel formation region 121c in the channel length direction. The first oxide semiconductor layer 101 and the low-resistance region 122c are sandwiched between the first oxide semiconductor layer 101 and the channel formation region 122c. and a second oxide semiconductor layer 102 provided with the oxide semiconductor layers 122a and 122b. 403, transistor 420 and transistor 425 have on-characteristics (e.g. For example, the on-state current and field effect mobility are high, enabling high-speed operation and high-speed response.

[0203] In addition, a dopant is introduced into the transistor 430 having the oxygen excess region shown in the second embodiment. FIG. 6C shows a transistor 423 in which a low-resistance region is formed by inserting a gate insulating film.

[0204] The transistor 423 is the same as the transistor 430 in FIG. a first oxide semiconductor layer 101 including an oxygen excess region 112; and a second oxide semiconductor layer In the transistor including the oxide semiconductor stack having the layer 102, the gate electrode layer 4 A dopant is introduced using 01 as a mask to form a channel forming region 121c containing excess oxygen. Low resistance regions 121d, 121e, and 122c containing dopants and excess oxygen are disposed between the low resistance regions 121d, 121e, and 122c. 22d, 122e, and low resistance regions 121a, 121b, 122a, 12 It is produced by forming 2b.

[0205] In the channel length direction, low resistance regions 121d, 121e, and 121c are disposed on either side of the channel formation region 121c. The first oxide semiconductor layer 101 in which the first oxide semiconductor layer 21a and the first oxide semiconductor layer 121b are provided and the channel formation region 122 A second oxide film having low resistance regions 122d, 122e, 122a, and 122b sandwiched between the first oxide film 122a and the second oxide film 122b. The oxide semiconductor stack 403 including the oxide semiconductor layer 102 is 423 has high on-characteristics (e.g., on-current and field-effect mobility), high-speed operation, and high-speed response. This becomes possible.

[0206] In addition, as in the transistor 480a described in Embodiment 1, the oxide semiconductor stack 403 In a three-layer transistor, oxygen and dopants are introduced to form an oxygen excess region and a low resistance region. A transistor 480b having a resistor region formed therein is shown in FIG.

[0207] The transistor 480b includes a first oxide semiconductor layer 101, a second oxide semiconductor layer 102, Oxygen was introduced into the oxide semiconductor stack 403 including the third oxide semiconductor layer 103 to form an oxygen permeation. After forming the gate electrode layer 401, the gate electrode layer 401 is used as a mask to The oxygen-excessive channel formation regions 121c, 122c, and 123c are sandwiched between the channels. The low resistance regions 121d, 121e, 122d, and 122e containing dopants and excess oxygen are e, 123d, and 123e, and low resistance regions 121a, 121b, and 122a containing dopants. , 122b, 123a, and 123b.

[0208] In the channel length direction, low resistance regions 121d, 121e, and 121c are disposed on either side of the channel formation region 121c. The first oxide semiconductor layer 101 in which the first oxide semiconductor layer 21a and the first oxide semiconductor layer 121b are provided and the channel formation region 122 A second oxide film having low resistance regions 122d, 122e, 122a, and 122b sandwiched between the first oxide film 122a and the second oxide film 122b. The semiconductor layer 102 and the low resistance regions 123d and 123e sandwich the channel forming region 123c. and a third oxide semiconductor layer 103 on which the oxide semiconductor layers 123a and 123b are provided. By including layer 403, the transistor 480b has on-characteristics (e.g., on-current and The high electron mobility (electron field effect mobility) enables high-speed operation and high-speed response.

[0209] Transistor 420, transistor 423, transistor 425, transistor 480b In the above, the low resistance regions 121a, 121b, 122a, and 122b are source regions or drain regions. The low resistance regions 121a, 121b, 122a, and 123a can function as in-regions. By providing 22b, between the low resistance regions 121a, 121b, 122a, and 122b Therefore, the electric field applied to the channel formation regions 121c and 122c formed in the semiconductor substrate 120 can be reduced. In addition, the low resistance regions 121a, 121b, 122a, and 122b are formed of oxide semiconductor layers. The layer 403 is electrically connected to the source electrode layer 405a and the drain electrode layer 405b. As a result, the oxide semiconductor stack 403, the source electrode layer 405a, and the drain electrode layer 405 Therefore, the contact resistance between the transistor 420 and the transistor 4b can be reduced. The electrical properties of 23 can be improved.

[0210] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0211] (Embodiment 4) A semiconductor device having a display function using the transistor as an example shown in any one of Embodiments 1 to 3. A semiconductor device (also called a display device) can be manufactured. A system-on-panel is formed by forming part or the whole circuit on the same substrate as the pixel section. It is possible.

[0212] In FIG. 7A, a pixel portion 4002 provided on a first substrate 4001 is surrounded by a A sealant 4005 is provided and the semiconductor device is sealed with a second substrate 4006. In A), a region surrounded by a sealant 4005 on a first substrate 4001 and The semiconductor layer is formed of a single crystal semiconductor film or a polycrystalline semiconductor film on a separately prepared substrate in a different region. A scanning line driver circuit 4004 and a signal line driver circuit 4003 are also mounted. A signal line driver circuit 4003 and a scanning line driver circuit 4004 or a signal line driver circuit 4005 are provided to the pixel portion 4002. Various signals and potentials are transmitted through the FPC (Flexible Printed Circuit). )Powered by 4018a and 4018b.

[0213] In FIG. 7B and FIG. 7C, a pixel portion 4002 is provided on a first substrate 4001, and a scanning A sealant 4005 is provided so as to surround the line driver circuit 4004. A second substrate 4006 is provided on the substrate 4002 and the scanning line driver circuit 4004. The pixel portion 4002 and the scanning line driver circuit 4004 are formed by a first substrate 4001 and a sealant 4002. The display element is sealed by the second substrate 4005 and the second substrate 4006. In C), the area surrounded by the sealant 4005 on the first substrate 4001 and The semiconductor layer is formed of a single crystal semiconductor film or a polycrystalline semiconductor film on a separately prepared substrate in a different region. In FIG. 7B and FIG. 7C, a signal line driver circuit 4003 is mounted. A signal line driver circuit 4003 and a scanning line driver circuit 4004 or a signal line driver circuit 4005 are provided to the pixel portion 4002. The various signals and potentials are supplied from the FPC4018.

[0214] In addition, in FIG. 7B and FIG. 7C, a signal line driver circuit 4003 is formed separately, and the first substrate 4 001, but the present invention is not limited to this configuration. Alternatively, only a part of the signal line driver circuit or a part of the scanning line driver circuit may be formed and mounted. It may be formed separately and mounted.

[0215] The method of connecting the separately formed drive circuit is not particularly limited, and may be any of the following: ip On Glass) method, wire bonding method, or TAB (Tape A A method such as a utomated bonding method can be used. This is an example in which a signal line driver circuit 4003 and a scanning line driver circuit 4004 are implemented by the OG method. FIG. 7B shows an example in which a signal line driver circuit 4003 is mounted by the COG method, and FIG. 4003) is an example in which a signal line driver circuit 4003 is mounted by the TAB method.

[0216] The display device includes a panel in which a display element is sealed, and a controller for the panel. and modules in which ICs, etc., including the above, are mounted.

[0217] In this specification, the term "display device" refers to an image display device, a display device, or an optical Also refers to connectors, such as FPC or TAB tape. Modules with TCP attached, TAB tape or TCP with printed wiring board attached The IC (integrated circuit) is directly mounted on the installed module or display element using the COG method. The display device includes all of the modules installed in the display device.

[0218] The pixel portion and the scanning line driver circuit provided on the first substrate have a plurality of transistors. The transistor described in any one of Embodiments 1 to 3 can be used. do.

[0219] Examples of display elements provided in the display device include liquid crystal elements (also called liquid crystal display elements), light-emitting elements ( The light-emitting element can be used as a light-emitting display element. This category includes elements whose brightness can be controlled, specifically inorganic EL (Electroluminescent) Luminescence, organic electroluminescence, etc. Also, electronic ink, etc. A display medium whose contrast changes depending on use can also be applied.

[0220] One mode of a semiconductor device will be described with reference to FIGS. 7 and 8. FIG. 8 shows the M Equivalent to the cross-sectional view at -N.

[0221] As shown in FIG. 7 and FIG. 8, the semiconductor device has a connection terminal electrode 4015 and a terminal electrode 4016. The connection terminal electrode 4015 and the terminal electrode 4016 are terminals of the FPC 4018. and electrically connected via an anisotropic conductive film 4019 .

[0222] The connection terminal electrode 4015 is formed from the same conductive film as the first electrode layer 4030. 016 is a transistor having the same conductor as the source and drain electrode layers of the transistors 4010 and 4011. It is formed of a conductive film.

[0223] A pixel portion 4002 and a scanning line driver circuit 4004 are provided on a first substrate 4001. 7 and 8, the transistor included in the pixel portion 4002 is 4004 and a transistor 4011 included in the scanning line driver circuit 4004. In FIG. 8A, an insulating film 4020 is provided over the transistors 4010 and 4011. 8B, an insulating film 4021 is further provided. It is an insulating film that functions as a base film.

[0224] The transistor 4010 and the transistor 4011 are the transistors according to any one of Embodiments 1 to 3. In this embodiment, the transistor shown in Embodiment 1 can be used. 13. An example in which a transistor having a structure similar to that of the transistor 440a is used will be described.

[0225] The transistor 4010 and the transistor 4011 have an energy gap A transistor having an oxide semiconductor stack including at least two oxide semiconductor layers having different structures An oxide semiconductor using a plurality of oxide semiconductor layers having different energy gaps By using stacked layers, the electrical characteristics of a transistor can be controlled with greater precision. In this way, desired electrical characteristics can be imparted to the transistors 4010 and 4011. It becomes Noh.

[0226] Therefore, the semiconductor device of this embodiment shown in FIG. 7 and FIG. 8 has high functionality, high reliability, or It is possible to provide semiconductor devices that meet various objectives, such as low power consumption.

[0227] The transistor 4010 provided in the pixel portion 4002 is electrically connected to a display element. The display element is not particularly limited as long as it can display an image. can be used.

[0228] FIG. 8(A) shows an example of a liquid crystal display device using a liquid crystal element as a display element. In the liquid crystal element 4013 which is a display element, a first electrode layer 4030 and a second electrode layer 403 1, and a liquid crystal layer 4008. The liquid crystal layer 4008 is sandwiched between two layers functioning as alignment films. The second electrode layer 4031 is formed on the second substrate. The first electrode layer 4030 and the second electrode layer 4031 are disposed on the liquid crystal layer 400 The structure is such that the layers are stacked via 8.

[0229] Also, 4035 is a columnar spacer obtained by selectively etching the insulating film. It is provided to control the thickness (cell gap) of the liquid crystal layer 4008. A pacer may be used.

[0230] When liquid crystal elements are used as display elements, thermotropic liquid crystal, low molecular weight liquid crystal, high molecular weight liquid crystal, etc. For example, a liquid crystal, a polymer-dispersed liquid crystal, a ferroelectric liquid crystal, an antiferroelectric liquid crystal, etc. can be used. Depending on the conditions, the liquid crystal material (liquid crystal composition) can be in a cholesteric phase, a smectic phase, or a cubic phase. The phases shown are biaxial, chiral nematic, isotropic, etc.

[0231] In addition, the liquid crystal layer 4008 may be made of a liquid crystal composition that exhibits a blue phase without using an alignment film. The blue phase is one of the liquid crystal phases. When the temperature of a cholesteric liquid crystal is increased, the cholesteric The blue phase is a phase that appears just before the transition from the black phase to the isotropic phase. The blue phase can be expressed by using a liquid crystal composition in which the above-mentioned liquid crystals are mixed. In order to widen the range of the blue phase, a polymerizable monomer and a polymerization initiator are added to the liquid crystal composition that exhibits the blue phase. The liquid crystal layer can be formed by adding a polymer stabilizer. The liquid crystal composition that exhibits this phase has a short response time and is optically isotropic, so no alignment treatment is required. The viewing angle dependence is small. Also, since there is no need to provide an alignment film, rubbing treatment is not required. Therefore, electrostatic damage caused by the rubbing process can be prevented, and the manufacturing process This reduces defects and damage to the liquid crystal display device during the manufacturing process. A transistor including an oxide semiconductor film can be prevented from being affected by static electricity. This can cause the electrical characteristics of the transistor to vary significantly and deviate from the design range. A liquid crystal display device having a transistor including an oxide semiconductor film and capable of exhibiting a blue phase can be provided. It is more effective to use a crystalline composition.

[0232] The specific resistance of the liquid crystal material is 1×10 9 Ω cm or more, preferably 1×10 11 Ω cm or more, and more preferably 1×10 12 In addition, this specification The resistivity values ​​stated herein are those measured at 20°C.

[0233] The size of the storage capacitor provided in the liquid crystal display device is determined by the lead of the transistor arranged in the pixel portion. The capacitance is set so that the charge can be held for a predetermined period of time, taking into account factors such as the capacitance of the capacitor. The size of the oxide film may be set in consideration of the off-state current of the transistor. By using a transistor having a semiconductor film, the liquid crystal capacitance of each pixel is It is sufficient to provide a storage volume having a size of 1 / 3 or less, preferably 1 / 5 or less, of the capacity of the do.

[0234] The transistor including the oxide semiconductor film disclosed in this specification has a current value in an off state ( Therefore, the retention time of electric signals such as image signals can be controlled to be low. The write interval can be set to a longer value when the power is on. This reduces the frequency of flash operations, thereby reducing power consumption.

[0235] In addition, a transistor including an oxide semiconductor film disclosed in this specification has high field-effect mobility. Since the actuator can be precisely controlled, high-speed operation is possible. By using such a transistor in a liquid crystal display device, In addition, a driver transistor used in the driver circuit portion can be formed on the same substrate. That is, a semiconductor device formed from a silicon wafer or the like is used as a separate driving circuit. Since there is no need for a pixel region, the number of components in the semiconductor device can be reduced. However, by using transistors that can be driven at high speed, high-quality images can be provided. Therefore, high reliability can be achieved as a semiconductor device.

[0236] There are two types of LCD displays: TN (Twisted Nematic) and IPS (In-P lane-Switching) mode, FFS (Fringe Field Switching) mode ching) mode, ASM(Axially Symmetric aligned) Micro-cell mode, OCB (Optical Compensated B) irefringence mode, FLC (Ferroelectric Liqui d Crystal) mode, AFLC (AntiFerroelectric Liq. uid Crystal) mode can be used.

[0237] In addition, normally black type liquid crystal display devices, such as those using a vertical alignment (VA) mode, The liquid crystal display device may be a transmission type liquid crystal display device. There are several types of vertical alignment modes, including: For example, MVA (Multi-Domain Vertical Alignment) mode, PVA (Patterned Vertical Alignment) mode , ASV (Advanced Super View) mode, etc. can be used. The present invention can also be applied to VA type liquid crystal display devices. VA type liquid crystal display devices are: It is a type of method for controlling the arrangement of liquid crystal molecules in a liquid crystal display panel. VA type liquid crystal display devices are When no voltage is applied, the liquid crystal molecules are oriented vertically to the panel surface. In addition, a pixel is divided into several regions (subpixels), each of which is oriented in a different direction. This is called multi-domain or multi-domain design, which is designed to defeat molecules in a complex manner. The following method can be used.

[0238] In addition, in display devices, they are used as black matrices (light-shielding layers), polarizing members, phase difference members, reflectors, etc. Optical members (optical substrates) such as a prevention member are provided as appropriate. For example, a polarizing substrate and a retardation substrate Alternatively, a backlight or a sidelight may be used as the light source. It's fine.

[0239] The display method in the pixel section uses the progressive method, interlace method, etc. In addition, the color elements controlled by pixels when displaying colors are RGB (R is The color is not limited to the three colors red, green, and blue. For example, RGBW (W stands for white). , or RGB plus one or more colors such as yellow, cyan, magenta, etc. The size of the display area may be different for each dot of the color element. The present invention is not limited to color display devices, but is applicable to monochrome display devices. It is also possible.

[0240] In addition, a light-emitting element that utilizes electroluminescence is used as a display element included in the display device. The light-emitting element utilizing electroluminescence is made of a light-emitting material They are classified according to whether they are organic or inorganic compounds. Generally, the former are called organic E The latter is called an inorganic EL element.

[0241] In an organic EL element, electrons and holes are released from a pair of electrodes by applying a voltage to the light-emitting element. are injected into layers containing light-emitting organic compounds, causing a current to flow. The rears (electrons and holes) recombine to form an excited state in the light-emitting organic compound. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.

[0242] Inorganic EL elements are divided into dispersion-type inorganic EL elements and thin-film-type inorganic EL elements according to their element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of a light-emitting material are dispersed in a binder. The emission mechanism is a donor-acceptor reaction that utilizes the donor and acceptor levels. Thin-film inorganic EL elements are made by sandwiching a light-emitting layer between dielectric layers. The structure is sandwiched between electrodes, and the light emission mechanism utilizes the inner shell electron transition of metal ions. In this example, the light-emitting element is an organic EL element. do.

[0243] In order to extract light emitted from the light-emitting element, at least one of the pair of electrodes needs to be light-transmitting. Then, a transistor and a light emitting element are formed on the substrate, and light is emitted from the surface opposite the substrate. The top emission is from the top surface, the bottom emission is from the surface on the substrate side, and the bottom emission is from the surface on the substrate side and the opposite side to the substrate. There are light emitting devices with a double-sided emission structure that emits light from both sides, and light emitting devices of any emission structure can be used. It is possible.

[0244] FIG. 8B shows an example of a light-emitting device using a light-emitting element as a display element. The element 4513 is electrically connected to the transistor 4010 provided in the pixel portion 4002. The light-emitting element 4513 includes a first electrode layer 4030, an electroluminescent layer 4511, and a second electrode layer 4512. The light-emitting element 4513 has a stacked structure of two electrode layers 4031, but is not limited to the structure shown. The configuration of the light emitting element 4513 can be changed appropriately according to the direction of the light to be extracted from the do.

[0245] The partition 4510 is formed using an organic insulating material or an inorganic insulating material, particularly a photosensitive resin. An opening is formed on the first electrode layer 4030 using a material, and the sidewall of the opening is a continuous curved It is preferable to form the inclined surface so that the inclined surface is formed with a certain rate.

[0246] The electroluminescent layer 4511 may be composed of a single layer or may be composed of a plurality of layers stacked together. It doesn't matter whether it is done or not.

[0247] In order to prevent oxygen, hydrogen, moisture, carbon dioxide, and the like from entering the light-emitting element 4513, the second electrode layer A protective film may be formed on the insulating film 4031 and the partition wall 4510. The protective film may be made of silicon nitride. A silicon nitride oxide film, a DLC film, etc. can be formed on the first substrate 400. The space sealed by the first substrate 4001, the second substrate 4006, and the sealant 4005 is filled with a filler 45. 14 is provided and sealed. In this way, it is highly airtight and degassing is possible to prevent exposure to the outside air. Protective films with low damage (laminated films, UV-cured resin films, etc.) and covering materials It is preferable to package (enclose) the

[0248] Filler 4514 can be inert gas such as nitrogen or argon, or ultraviolet curing resin or Thermosetting resin can be used, and PVC (polyvinyl chloride), acrylic, polyimide, etc. Mido, epoxy resin, silicone resin, PVB (Polyvinyl Butyral) or EVA (Elastomer) For example, nitrogen may be used as a filler. stomach.

[0249] If necessary, a polarizing plate or a circular polarizing plate (including an elliptical polarizing plate) may be provided on the light-emitting surface of the light-emitting element. Optical films such as retardation plates (λ / 4 plates, λ / 2 plates) and color filters may be provided as appropriate. In addition, the polarizing plate or the circular polarizing plate may be provided with an anti-reflection film. Anti-glare treatment can be applied to diffuse reflected light and reduce glare.

[0250] It is also possible to provide electronic paper that drives electronic ink as a display device. Electronic paper is also called an electrophoretic display (electrophoretic display) and is similar to paper. It is possible to make it as easy to read as other display devices, consume less power, and have a thinner and lighter shape. This has the advantage that

[0251] The electrophoretic display device may have various forms, but it has a first particle having a positive charge and A microcapsule containing a negatively charged second particle and a negatively charged second particle is introduced into a solvent or solute. By applying an electric field to the microcapsules, The particles in the cell are moved in opposite directions to each other, and only the color of the particles that have gathered on one side is displayed. In addition, the first particles or the second particles contain a dye, and they do not migrate in the absence of an electric field. The color of the first particle and the color of the second particle are different (including colorless). )

[0252] In this way, the electrophoretic display device is a so-called This is a display that utilizes the dielectrophoretic effect.

[0253] The microcapsules dispersed in a solvent are called electronic ink. The electronic ink can be printed on surfaces such as glass, plastic, fabric, and paper. A color display is also possible by using a color filter or particles having a pigment.

[0254] The first particles and the second particles in the microcapsules are made of a conductive material, an insulating material, Semiconductor materials, magnetic materials, liquid crystal materials, ferroelectric materials, electroluminescent materials, A material selected from the group consisting of magnetochromic material, magnetophoretic material, and a composite material thereof. Just use it.

[0255] In addition, display devices using the twist ball display method can also be used as electronic paper. The twist ball display method uses black and white spherical particles as the display element. The insulating layer is disposed between a first electrode layer and a second electrode layer, and the first electrode layer and the second electrode layer are electrically connected to each other. This is a method of displaying information by controlling the orientation of spherical particles by applying a potential difference to the electrode layer. be.

[0256] In addition, in FIG. 7 and FIG. 8, the first substrate 4001 and the second substrate 4006 are made of glass. In addition to a glass substrate, a flexible substrate can also be used. For example, a light-transmitting plastic substrate can be used. As for plastic, FRP (Fibreglass) is used. s-Reinforced Plastics) plate, PVF (Polyvinyl fluoride) A film, a polyester film or an acrylic resin film can be used. If transparency is not required, metal substrates such as aluminum and stainless steel (metal film For example, aluminum foil may be covered with a PVF film or polyester film. It is also possible to use a sheet sandwiched between two sheets.

[0257] In this embodiment, an aluminum oxide film is used as the insulating film 4020.

[0258] The aluminum oxide film provided as the insulating film 4020 over the oxide semiconductor film is resistant to hydrogen, moisture, and the like. The membrane has a high blocking effect against both impurities such as urea and oxygen. stomach.

[0259] Therefore, the aluminum oxide film is free from hydrogen, which is a variable factor during and after the manufacturing process. The intrusion of impurities such as moisture into the oxide semiconductor film and the intrusion of the oxide semiconductor into the main component material The oxide semiconductor film functions as a protective film for preventing release of oxygen from the oxide semiconductor film.

[0260] The insulating film 4021 functioning as a planarizing insulating film is made of acrylic, polyimide, or benzosilane. Heat-resistant organic materials such as clobutene resins, polyamides, and epoxies can be used. In addition to the above organic materials, low-k materials and siloxane resins are also available. , PSG (phosphorus glass), BPSG (borophosphorus glass), etc. can be used. The insulating film may be formed by stacking a plurality of insulating films made of these materials.

[0261] The method for forming the insulating film 4021 is not particularly limited. Depending on the material, it may be formed by sputtering, S OG method, spin coating, dip, spray coating, droplet ejection method (inkjet method, etc.), Printing method (screen printing, offset printing, etc.), doctor knife, roll coater, car A ten coater, a knife coater, or the like can be used.

[0262] A display device transmits light from a light source or a display element to display an image. All thin films such as the substrate, insulating film, and conductive film installed in the part are designed to be transparent to light in the visible light wavelength range. It shall be translucent.

[0263] A first electrode layer and a second electrode layer (a pixel electrode layer, a common electrode layer, a pair of electrodes) for applying a voltage to the display element In the case of the electrode layer, the direction of the light to be extracted, the location of the electrode layer, and The light transmitting property or the light reflecting property can be selected depending on the pattern structure of the electrode layer.

[0264] The first electrode layer 4030 and the second electrode layer 4031 are made of indium oxide containing tungsten oxide. oxide, indium zinc oxide with tungsten oxide, indium oxide with titanium oxide Indium tin oxide containing titanium oxide, indium tin oxide, indium zinc oxide , indium tin oxide doped with silicon oxide, graphene, and other light-transmitting conductive materials Fees can be used.

[0265] The first electrode layer 4030 and the second electrode layer 4031 are made of tungsten (W) or molybdenum. (Mo), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (N b) Tantalum (Ta), Chromium (Cr), Cobalt (Co), Nickel (Ni), Titanium Metals such as titanium (Ti), platinum (Pt), aluminum (Al), copper (Cu), and silver (Ag), It can be formed by using one or more of the following metals: Cut.

[0266] The first electrode layer 4030 and the second electrode layer 4031 are made of a conductive polymer (conductive polymer). The conductive polymer may be a conductive composition containing a conductive polymer. For example, a so-called π-electron conjugated conductive polymer can be used. or its derivatives, polypyrrole or its derivatives, polythiophene or its derivatives, or a copolymer of two or more of aniline, pyrrole and thiophene or a derivative thereof Conductors, etc.

[0267] In addition, since transistors are easily damaged by static electricity, etc., a protection circuit for protecting the driver circuit is also required. It is preferable that the protection circuit is configured using a non-linear element.

[0268] As described above, by using the transistor described in any of Embodiments 1 to 3, various It is possible to provide semiconductor devices having various functions.

[0269] (Embodiment 5) By using the transistor as an example shown in any one of the first to third embodiments, information on an object is read. Therefore, a semiconductor device having an image sensor function for detecting a reflected light can be manufactured.

[0270] FIG. 9A shows an example of a semiconductor device having an image sensor function. FIG. 9(B) is a cross-sectional view showing a part of the photosensor.

[0271] The photodiode 602 has one electrode connected to a photodiode reset signal line 658 and the other One electrode of the transistor 640 is electrically connected to the gate of the transistor 640. One of the source or drain is connected to the photosensor reference signal line 672, and the other of the source or drain is connected to the photosensor reference signal line 672. The other terminal is electrically connected to one of the source and drain terminals of the transistor 656. The transistor 656 has a gate connected to a gate signal line 659 and a source or drain connected to a photodiode. The sensor output signal line 671 is electrically connected to the sensor output signal line 671.

[0272] Note that in the circuit diagrams in this specification, a transistor including an oxide semiconductor film is not clearly shown. To make it easy to understand, the symbol for a transistor using an oxide semiconductor film is marked with “OS.” In FIG. 9A, a transistor 640 and a transistor 656 are the same as those in the first embodiment. The transistors shown in the above to 3 can be used, and the transistor is a transistor using an oxide semiconductor film. In this embodiment, a transistor having a structure similar to that of the transistor 440a shown in the first embodiment is used. An example of applying a transistor is shown below.

[0273] FIG. 9B shows a photodiode 602 and a transistor 640 in the photosensor. 6 is a cross-sectional view showing a TFT substrate 601 on which a photodiode functioning as a sensor is provided. A photodiode 602 and a transistor 640 are provided. A substrate 613 is provided on the resistor 640 using an adhesive layer 608 .

[0274] On the transistor 640, an insulating film 631, an insulating film 632, an interlayer insulating film 633, and an interlayer insulating film The photodiode 602 is provided on the interlayer insulating film 633. An electrode layer 641 formed on the interlayer insulating film 633 and an electrode layer 642 formed on the interlayer insulating film 634 Between the first semiconductor film 606a and the second semiconductor film 606b, a first semiconductor film 606c and a second semiconductor film 606d are formed in this order from the interlayer insulating film 633 side. 6b, and a third semiconductor film 606c.

[0275] The electrode layer 641 is electrically connected to a conductive layer 643 formed on the interlayer insulating film 634. 642 is electrically connected to the conductive layer 645 via the electrode layer 641. The conductive layer 645 is The photodiode 602 is electrically connected to the gate electrode layer of the transistor 640. It is electrically connected to the transistor 640 .

[0276] Here, the first semiconductor film 606a is a semiconductor film having a p-type conductivity, and the second semiconductor film A high resistance semiconductor film (I-type semiconductor film) is used as 606b, and an n-type semiconductor film is used as the third semiconductor film 606c. A pin-type photodiode in which semiconductor films having different conductivity types are stacked is shown as an example.

[0277] The first semiconductor film 606a is a p-type semiconductor film, and is an amorphous semiconductor film containing an impurity element that imparts p-type. The first semiconductor film 606a can be formed of a group 13 silicon film. Using semiconductor material gas containing impurity elements (e.g. boron (B)), plasma CVD method Silane (SiH4) can be used as the semiconductor material gas. i2H6, SiH2Cl2, SiHCl3, SiCl4, SiF4, etc. may also be used. In addition, after forming an amorphous silicon film that does not contain impurity elements, the film is then subjected to diffusion or ion implantation. Impurity elements may be introduced into the amorphous silicon film by using an ion implantation method or the like. It is preferable to diffuse the impurity element by heating or the like after introducing the impurity element. In this case, the method for forming the amorphous silicon film includes the LPCVD method, the vapor phase growth method, Alternatively, a sputtering method or the like may be used. It is preferable to form the film so that the thickness is 0 nm or less.

[0278] The second semiconductor film 606b is an I-type semiconductor film (intrinsic semiconductor film) and is made of amorphous silicon. The second semiconductor film 606b is formed by amorphous silicon using a semiconductor material gas. A fast silicon film is formed by plasma CVD. The semiconductor material gas is silane. (SiH4) can be used. Alternatively, Si2H6, SiH2Cl2, SiHCl3, S iCl4, SiF4, etc. may be used. The second semiconductor film 606b is formed by LPCVD. The second semiconductor film 606b may be formed by vapor deposition, sputtering, or the like. It is preferable to form the film so that the thickness is 00 nm or more and 1000 nm or less.

[0279] The third semiconductor film 606c is an n-type semiconductor film and is an amorphous film containing an impurity element that imparts n-type conductivity. The third semiconductor film 606c is formed of a fast silicon film. It is formed by the plasma CVD method using a semiconductor material gas containing silicon (e.g. phosphorus (P)). Silane (SiH4) can be used as the semiconductor material gas. SiH2Cl2, SiHCl3, SiCl4, SiF4, etc. may also be used. After forming an amorphous silicon film that does not contain elements, the material is then doped with silicon using diffusion or ion implantation. An impurity element may be introduced into the amorphous silicon film by ion implantation or the like. After the element is introduced, the impurity element may be diffused by heating or the like. The method for forming the amorphous silicon film includes the LPCVD method, the vapor phase growth method, or the sputtering method. The thickness of the third semiconductor film 606c is 20 nm or more and 200 nm or less. It is preferable to form it so that the bottom is facing downward.

[0280] The first semiconductor film 606a, the second semiconductor film 606b, and the third semiconductor film 606c are Instead of an amorphous semiconductor, a polycrystalline semiconductor may be used. Semi Amorphous Semiconductor (SAS )) It may be formed using a semiconductor.

[0281] Microcrystalline semiconductors are metastable, intermediate between amorphous and single crystal, when considering the Gibbs free energy. In other words, a semiconductor that has a third state that is stable in terms of free energy The crystals are of a short-range order and have lattice distortion. Microcrystalline silicon, a typical example of a microcrystalline semiconductor, is a type of Raman The spectrum shows single crystal silicon at 520 cm -1 It is shifted to the lower wavenumber side. That is, 520 cm, which indicates single crystal silicon. -1 and 480 cm, which indicates amorphous silicon. - 1 The Raman spectrum of microcrystalline silicon has a peak between the two. Contains at least 1 atomic % or more of hydrogen or halogen to terminate the ring bonds. In addition, it contains rare gas elements such as helium, argon, krypton, and neon. By increasing the thickness of the semiconductor film, the lattice distortion is further promoted, and the stability is increased, resulting in a good microcrystalline semiconductor film. .

[0282] This microcrystalline semiconductor film is formed by a high-frequency plasma CVD method with a frequency of several tens to several hundreds of MHz. Alternatively, it can be formed by a microwave plasma CVD apparatus with a frequency of 1 GHz or more. Representative examples include SiH4, Si2H6, SiH2Cl2, SiHCl3, SiCl4, and S It can be formed by diluting silicon-containing compounds such as iF4 with hydrogen. In addition to compounds containing hydrogen (e.g. silicon hydride) and hydrogen, helium, argon, krypton, neon forming a microcrystalline semiconductor film by diluting the semiconductor film with one or more rare gas elements selected from the group consisting of fluorine and fluorine; In these cases, the flow rate ratio of hydrogen to the compound containing silicon (e.g., silicon hydride) is 5 times or more and 200 times or less, preferably 50 times or more and 150 times or less, and more preferably 100 times Furthermore, in the gas containing silicon, carbide gases such as CH4, C2H6, GeH 4. Germanium gas such as GeF4, F2, etc. may be mixed in.

[0283] In addition, the mobility of holes generated by the photoelectric effect is smaller than that of electrons, so Photodiodes exhibit better characteristics when the p-type semiconductor film side is used as the light receiving surface. From the surface of the substrate 601 on which the in-type photodiode is formed, the photodiode 602 This example shows how the light received by the semiconductor film is converted into an electrical signal. Since light from the semiconductor film side having the pattern becomes disturbance light, the electrode layer uses a conductive film with light blocking properties. In addition, the n-type semiconductor film side can be used as the light receiving surface.

[0284] The insulating film 632, the interlayer insulating film 633, and the interlayer insulating film 634 are made of an insulating material. Depending on the material, sputtering, plasma CVD, SOG, spin coating, and die deposition are used. Spray coating, droplet ejection method (inkjet method, etc.), printing method (screen printing, offset printing, etc.), doctor knife, roll coater, curtain coater, knife coater It can be formed using the above.

[0285] In this embodiment, an aluminum oxide film is used as the insulating film 631. The film can be formed by a sputtering method or a plasma CVD method.

[0286] The aluminum oxide film provided as the insulating film 631 over the oxide semiconductor film is resistant to hydrogen, moisture, and the like. High blocking effect that prevents impurities and oxygen from passing through the membrane .

[0287] Therefore, the aluminum oxide film is free from hydrogen, which is a variable factor during and after the manufacturing process. The intrusion of impurities such as moisture into the oxide semiconductor film and the intrusion of the oxide semiconductor into the main component material The oxide semiconductor film functions as a protective film for preventing release of oxygen from the oxide semiconductor film.

[0288] The insulating film 632 may be made of an inorganic insulating material such as a silicon oxide layer, a silicon oxynitride layer, An oxide insulating film such as an aluminum oxide layer or an aluminum oxynitride layer, or a silicon nitride layer , a nitride such as a silicon oxynitride layer, an aluminum nitride layer, or an aluminum oxynitride layer. A single layer or a stacked layer of an insulating film can be used.

[0289] The interlayer insulating films 633 and 634 function as planarizing insulating films to reduce surface irregularities. The interlayer insulating films 633 and 634 are preferably made of, for example, polyimide or acrylic. Heat-resistant organic resins such as resins, benzocyclobutene-based resins, polyamides, and epoxy resins In addition to the above organic insulating materials, low-dielectric materials can be used. k materials), siloxane resin, PSG (phosphorus glass), BPSG (borophosphorus glass), etc. A single layer or a laminate of these can be used.

[0290] By detecting the light incident on the photodiode 602, information on the detected object is read. In addition, when reading the information of the detected object, a light source such as a backlight is used. It is possible.

[0291] As described above, a plurality of oxide semiconductor layers having different energy gaps as semiconductor layers By using a stack of oxide semiconductor layers using This allows precise control, making it possible to impart desired electrical characteristics to the transistor. By using such transistors, various advantages such as high functionality, high reliability, and low power consumption can be achieved. A semiconductor device suited to a particular purpose can be provided.

[0292] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is.

[0293] (Embodiment 6) The transistor shown in any one of the first to third embodiments is a transistor stacked in a multi-layer structure. The present invention can be suitably used for a semiconductor device having an integrated circuit on a semiconductor device. As an example of a semiconductor device, a storage medium (memory element) will be described.

[0294] In the embodiment, a transistor that is a first transistor formed on a single crystal semiconductor substrate A second transistor formed using a semiconductor film is disposed above the transistor 140 with an insulating film interposed therebetween. A semiconductor device including the transistor 162 is manufactured. The transistors shown in any one of the examples in the above paragraphs 3 and 4 can be suitably used as the transistor 162. In this embodiment, the transistor 162 may be the transistor shown in the first embodiment. 4 shows an example in which a transistor having a structure similar to that of the transistor 440a is used.

[0295] The semiconductor materials and structures of the stacked transistors 140 and 162 may be the same. This embodiment is directed to a material suitable for the circuit of a storage medium (memory element). The above is an example in which a transistor having the above material and structure is used.

[0296] FIG. 10 shows an example of the configuration of a semiconductor device. FIG. 10(A) shows a cross section of the semiconductor device. 10(B) shows a plan view of the semiconductor device. This corresponds to the cross sections taken along lines C1-C2 and D1-D2 in FIG. 10(B). FIG. 10A shows an example of a circuit diagram in which the semiconductor device is used as a memory element. The semiconductor device shown in FIG. 10B has a transistor using a first semiconductor material in the lower part. The second semiconductor material is used as the second semiconductor material. In the embodiment, the first semiconductor material is a semiconductor material other than an oxide semiconductor, and the second semiconductor material is The oxide semiconductor is a semiconductor material other than the oxide semiconductor. Use of ruthenium, silicon germanium, silicon carbide, gallium arsenide, etc. In addition, organic semiconductor materials may be used. Transistors using such semiconductor materials can easily operate at high speed. The characteristics of transistors using solid semiconductors enable them to retain electric charge for long periods of time.

[0297] The semiconductor device in FIG. 10 will be described with reference to FIGS.

[0298] The transistor 140 is disposed on a substrate 185 that includes a semiconductor material (such as silicon). A channel forming region 116 is formed by arranging impurity layers 116 so as to sandwich the channel forming region 116. A region 120, a metal compound region 124 in contact with the impurity region 120, and a channel forming region 1 A gate insulating film 108 is provided on the gate insulating film 108. The electrode 110 is a ferroelectric material.

[0299] The substrate 185 containing the semiconductor material may be a single crystal semiconductor substrate such as silicon or silicon carbide, a multi-crystal The semiconductor substrates used are crystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, and SOI substrates. Generally, an "SOI substrate" is a substrate in which a silicon semiconductor film is provided on an insulating surface. In this specification, however, it refers to a substrate having a structure in which a material other than silicon is formed on an insulating surface. In other words, the term "SOI substrate" includes a semiconductor film having a structure in which a semiconductor film is provided. The film is not limited to a silicon semiconductor film. In addition, the SOI substrate may be made of an insulating material such as a glass substrate. The present invention also includes a configuration in which a semiconductor film is provided on a substrate via an insulating film.

[0300] The method for producing SOI substrates is to implant oxygen ions into a mirror-polished wafer and then heat it at high temperatures. By this, an oxide layer is formed at a certain depth from the surface, and the chips in the surface layer are removed. A method for eliminating microvoids formed by hydrogen ion irradiation and a method for forming microvoids by heat treatment. A method of cleaving a semiconductor substrate by using a long distance, or a method of growing a single crystal semiconductor film on an insulating surface by crystal growth For example, a method for forming a film may be used.

[0301] For example, ions are added from one surface of a single crystal semiconductor substrate to form a single crystal semiconductor substrate. A weakened layer is formed at a certain depth from the surface of the single crystal semiconductor substrate, and An insulating film is formed on one of the substrates. The single crystal semiconductor substrate and the element substrate are stacked with the insulating film between them. In the laminated state, a crack is generated in the weakened layer, and the single crystal semiconductor substrate is separated at the weakened layer. A heat treatment is performed to form a single crystal semiconductor film on the element substrate as a semiconductor film from the single crystal semiconductor substrate. The SOI substrate produced by the above method can also be used favorably.

[0302] An element isolation insulating layer 106 is provided on the substrate 185 so as to surround the transistor 140. In order to achieve high integration, the transistor 140 may be resized as shown in FIG. It is preferable to have a structure that does not have a sidewall insulating layer that becomes a sidewall. When the characteristics of the gate electrode 140 are important, a side wall is provided on the side of the gate electrode 110. A wall insulating layer may be provided to provide impurity regions 120 including regions with different impurity concentrations.

[0303] The transistor 140 using a single crystal semiconductor substrate can operate at high speed. By using this transistor as a read transistor, data can be read at high speed. Two insulating films are formed to cover the transistor 140. As a process before forming the stator 162 and the capacitance element 164, the two insulating layers are subjected to CMP processing. Then, the planarized insulating film 128 and the insulating film 130 are formed, and at the same time, the upper surface of the gate electrode 110 is Expose.

[0304] The insulating film 128 and the insulating film 130 are typically a silicon oxide film, a silicon oxynitride film, or an oxide Aluminum film, aluminum oxynitride film, silicon nitride film, aluminum nitride film, nitride An inorganic insulating film such as a silicon oxide film or an aluminum nitride oxide film can be used. The film 128 and the insulating film 130 are formed by using a plasma CVD method, a sputtering method, or the like. It is possible.

[0305] In addition, organic materials such as polyimide, acrylic resin, and benzocyclobutene resin can be used. In addition to the above organic materials, low-dielectric constant materials (low-k materials) can also be used. When using organic materials, an insulating film can be formed by wet methods such as spin coating and printing. 128 and an insulating film 130 may be formed.

[0306] Note that the insulating film 130 that is in contact with the semiconductor film is a silicon oxide film.

[0307] In this embodiment, the insulating film 128 is a 50 nm-thick oxynitride film formed by a sputtering method. A silicon film is formed, and an oxide film having a thickness of 550 nm is formed as the insulating film 130 by a sputtering method. A silicon film is formed.

[0308] On the insulating film 130 that has been sufficiently planarized by CMP processing, oxide semiconductors with different energy gaps are formed. In this embodiment, a sputtering method is used to stack oxide semiconductor films. Thus, an In-Sn-Zn oxide layer and an In-Ga-Zn oxide layer are formed in this order on the insulating film 130. The layers are stacked on top of each other.

[0309] Next, the stack of oxide semiconductor films is selectively etched to form an island-shaped stack of oxide semiconductor films 144. A source electrode or drain electrode 142 a and a source electrode 142 b are formed on the oxide semiconductor stack 144. A gate or drain electrode 142b is formed.

[0310] A gate insulating film 146 and a gate electrode layer 148 are formed over the oxide semiconductor film. 148 is formed by forming a conductive layer and then selectively etching the conductive layer. It can be achieved.

[0311] The gate insulating film 146 is formed by depositing an oxide film using a plasma CVD method, a sputtering method, or the like. Silicon film, silicon nitride film, silicon oxynitride film, silicon oxynitride film, aluminum oxide film Aluminum film, aluminum nitride film, aluminum oxynitride film, aluminum nitride oxide film, aluminum oxide film, A fluorine film, a gallium oxide film, or an aluminum oxide film can be formed.

[0312] A gate electrode layer 148, a source electrode or drain electrode 142a, a source electrode or drain The conductive layer that can be used for the electrode 142b can be formed by PVD such as sputtering. The conductive layer can be formed by a CVD method such as a plasma CVD method. The material may be an element selected from Al, Cr, Cu, Ta, Ti, Mo, and W, or the above-mentioned Alloys containing the elements Mn, Mg, Zr, Be, Nd, and Sc can be used. Any one of these materials or a combination of two or more of these materials may be used.

[0313] The conductive layer may have a single layer structure or a laminated structure of two or more layers. A single layer structure of a titanium nitride film or titanium film, a single layer structure of an aluminum film containing silicon, Two-layer structure with titanium film laminated on titanium nitride film, two-layer structure with titanium film laminated on titanium nitride film Examples include a three-layer structure in which a titanium film, an aluminum film, and a titanium film are laminated. In addition, when the conductive layer has a single-layer structure of a titanium film or a titanium nitride film, the conductive layer has a tapered shape. A source electrode or drain electrode 142a and a source electrode or drain electrode 142 It has the advantage of being easy to process into b.

[0314] Next, an insulating film is formed on the oxide semiconductor stack 144, the gate insulating film 146, and the gate electrode layer 148. In this embodiment, an aluminum oxide film is formed as the insulating film 150. do.

[0315] The aluminum oxide film provided as the insulating film 150 on the oxide semiconductor stack 144 is Blocking effect that prevents impurities such as water and oxygen from passing through the membrane (blocking effect) ) is high.

[0316] Therefore, the aluminum oxide film is free from hydrogen, which is a variable factor during and after the manufacturing process. Impurities such as moisture may be mixed into the oxide semiconductor stack 144, and the main components constituting the oxide semiconductor may be deteriorated. It functions as a protective film that prevents oxygen, which is a component, from being released from the oxide semiconductor stack 144. .

[0317] Moreover, a separate insulating film may be formed on the insulating film 150 .

[0318] The insulating film is a silicon oxide film formed by plasma CVD or sputtering. Silicon nitride film, silicon oxynitride film, silicon oxynitride film, aluminum nitride film, oxide Aluminum film, aluminum oxynitride film, aluminum nitride oxide film, hafnium oxide film Alternatively, a gallium oxide film can be used.

[0319] An electrode is formed on the insulating film 150 in a region overlapping the source electrode or drain electrode 142a. A layer 153 is formed.

[0320] Next, the insulating film 152 is formed over the transistor 162 and the electrode layer 153. The layer 2 can be formed by sputtering or CVD. Inorganic insulators such as silicon oxide nitride, silicon nitride, hafnium oxide, and aluminum oxide The material may be polyimide, acrylic, benzoxazole, etc. Organic materials such as cyclobutene resins can be used. The organic materials can be applied by coating, printing, etc. A wet method such as a printing method or an ink jet method can be used.

[0321] Next, a source electrode or a drain electrode is formed on the gate insulating film 146, the insulating film 150, and the insulating film 152. An opening is formed so as to reach the inner electrode 142b. The opening is formed by using a mask or the like. This is done by selective etching.

[0322] Thereafter, a wiring 156 that contacts the source electrode or drain electrode 142b is formed in the opening. In addition, in FIG. 10A, the connection between the source electrode or drain electrode 142b and the wiring 156 is not shown. The connection points are not shown.

[0323] The wiring 156 is formed by a PVD method such as a sputtering method, a plasma CVD method, or the like. After forming a conductive layer using the VD method, the conductive layer is etched to form The material of the conductive layer is selected from Al, Cr, Cu, Ta, Ti, Mo, and W. The elements mentioned above and alloys containing the elements mentioned above can be used. Mn, Mg, Z Any one of R, Be, Nd, and Sc, or a combination of two or more of these materials may be used. The details are similar to those of the source electrode or drain electrode 142a.

[0324] Through the above steps, the transistor 162 and the capacitor 164 are formed. The transistor 162 has at least two oxide semiconductor layers with different energy gaps. The transistor has an oxide semiconductor stack 144 including different energy layers. The oxide semiconductor stack 144 using a plurality of oxide semiconductor layers having a gap is used. This allows the electrical characteristics of the transistor 162 to be controlled more precisely, It is possible to impart electrical characteristics to the transistor 162. In the present embodiment, the oxide semiconductor stack 144 is highly purified and an oxide semiconductor layer containing excess oxygen is formed to fill the oxygen vacancies. Therefore, the off-state current of the transistor 162 is reduced, and the electrical characteristics of the transistor 162 are changed. The capacitance element 164 is electrically stable because the capacitance is suppressed. a gate electrode 142a, an oxide semiconductor stack 144, a gate insulating film 146, and an electrode layer 153, It is composed of:

[0325] In the capacitance element 164 of FIG. 10, the gate insulating film 146 and the insulating film 150 are laminated. As a result, the insulation between the source electrode or drain electrode 142a and the electrode layer 153 is sufficiently improved. Of course, in order to ensure a sufficient capacitance, the insulating film 150 may be used. Alternatively, a capacitor element 164 having an insulating film may be used. Furthermore, if capacitance is not required, the capacitance element 164 may be omitted. It is also possible to do so.

[0326] FIG. 10C shows an example of a circuit diagram in which the semiconductor device is used as a memory element. In FIG. 10C, one of the source electrode and the drain electrode of the transistor 162 is One of the electrodes of the capacitor 164 and the gate electrode of the transistor 140 are electrically connected. In addition, the first wiring (also called the source line) and the transistor The source electrode of 140 is electrically connected to the second wiring (2nd Line: bit line Also referred to as a drain electrode of the transistor 140 is electrically connected to A third wiring (also called a first signal line) and the source of the transistor 162 The other of the drain electrode and the drain electrode is electrically connected to a fourth wiring (4th Line The second signal line (also referred to as a second signal line) is electrically connected to the gate electrode of the transistor 162. A fifth line (also called a word line) and a capacitance element 16 The other electrode of 4 is electrically connected.

[0327] The transistor 162 including an oxide semiconductor has an extremely low off-state current. Therefore, by turning off the transistor 162, the source of the transistor 162 One of the electrodes or drain electrodes of the capacitor 164 and the transistor 140 The potential of the node (hereinafter, node FG) that is electrically connected to the gate electrode of By providing the capacitance element 164, This makes it easier to hold the charge given to the gate FG and to read out the held information. become.

[0328] When storing (writing) information in the semiconductor device, the potential of the fourth wiring is first This sets the potential at which the transistor 162 is turned on, thereby turning the transistor 162 on. Thus, the potential of the third wiring is supplied to the node FG, and a predetermined amount of charge is accumulated in the node FG. Here, the charges that give two different potential levels (hereinafter, low level Either a charge or a high level charge is given. The potential of the fourth wiring is set to a potential at which the transistor 162 is turned off. By turning off 162, node FG is in a floating state, so As described above, a certain amount of charge is stored in the node FG. By storing and holding information, the memory cell can store information.

[0329] Since the off-state current of the transistor 162 is controlled to be extremely small, The charge stored in the memory is retained for a long time, making refresh operations unnecessary. Or, the frequency of refresh operations can be reduced significantly, so power consumption can be reduced sufficiently. In addition, even if the power supply is cut off, the memory can be stored for a long period of time. It is possible to retain the content.

[0330] When reading out the stored information, a predetermined potential (constant potential) is applied to the first wiring. When an appropriate potential (read potential) is applied to the fifth wiring in this state, the potential is held at the node FG. Depending on the amount of charge transferred, transistor 140 assumes different states. If 40 is an n-channel type, then when a high-level charge is held at node FG, The apparent threshold voltage V of the transistor 140 th_H A low-level charge is applied to node FG. The apparent threshold voltage V of transistor 140 when held th_L Lower Here, the apparent threshold is the threshold voltage required to turn the transistor 140 on. Therefore, the potential of the fifth wiring is V th _H and V th_L By setting the potential V0 at the midpoint between For example, if a high level charge is applied during writing, The potential of the fifth wire is V0 (> V th_H ), transistor 140 is in the "on state" When a low-level charge is applied, the potential of the fifth wire becomes V0( <V t h_L ), the transistor 140 remains in the “off state”. The potential of the wiring is controlled to read out the on / off state of the transistor 140 (the The stored information can be read out by reading out the potential of the wiring 2.

[0331] In addition, when the stored information is rewritten, a predetermined amount of electricity is consumed by the rewriting. By supplying a new potential to the node FG that holds the load, the node FG is Specifically, the potential of the fourth wiring is held when the transistor 162 is turned on. This causes the transistor 162 to be turned on. A potential (electric potential related to new information) is supplied to node FG, and a predetermined amount of charge is stored in node FG. After that, the potential of the fourth wiring is set to a potential at which the transistor 162 is turned off. By turning off the transistor 162, the node FG receives the new information. That is, a predetermined amount of charge is stored in the node FG by the first write. While the charge is held, the same operation as the first write (second write) is performed. , it is possible to overwrite the stored information.

[0332] The transistor 162 described in this embodiment has at least two layers with different energy gaps. and the off-state current is controlled to be sufficiently low. By using such transistors, A semiconductor device capable of retaining memory contents is obtained.

[0333] As described above, the oxide semiconductor layer having a plurality of oxide semiconductor layers with different energy gaps can be used. By using stacked semiconductor layers, the electrical characteristics of transistors can be controlled with greater precision. This makes it possible to impart desired electrical characteristics to the transistor. It is possible to provide semiconductor devices that meet various objectives, such as high reliability or low power consumption. .

[0334] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination.

[0335] (Embodiment 7) The semiconductor device disclosed in this specification can be applied to various electronic devices (including game machines). The electronic device can be, for example, a television device (television or television receivers), computer monitors, digital cameras, digital video cameras digital photo frames, mobile phones (also called mobile phones or mobile phone devices), ), portable game machines, personal digital assistants, audio playback devices, pachinko machines and other large game machines, etc. Examples of electronic devices including the semiconductor device described in the above embodiment will be described. By providing the semiconductor device described in the above embodiment, a high-performance and high-reliability To provide electronic devices with qualities suited to various purposes, such as high performance or low power consumption. can be done.

[0336] FIG. 11A shows a notebook personal computer, which includes a main body 3001 and a housing 300 2, a display unit 3003, a keyboard 3004, etc. By applying the semiconductor device shown in any one of the above to the display portion 3003, high performance and It is possible to provide a highly reliable notebook personal computer.

[0337] FIG. 11B shows a portable digital assistant (PDA), which includes a display unit 3023 and a display unit 3024 on a main body 3021. An external interface 3025 and operation buttons 3024 are provided. The stylus 3022 is an accessory of the semiconductor device shown in any one of the first to sixth embodiments. By applying the body device to the display unit 3023, a mobile information terminal with higher performance and reliability can be obtained. (PDA).

[0338] FIG. 11C shows an example of an electronic book. For example, the electronic book has a housing 2701 and The housing 2701 and the housing 2703 are made up of two housings. The opening and closing operations can be performed with the shaft portion 2711 as an axis. With this configuration, it becomes possible to operate like a paper book.

[0339] A display unit 2705 is incorporated in the housing 2701, and a display unit 2707 is incorporated in the housing 2703. The display unit 2705 and the display unit 2707 are configured to display a continuous screen. Alternatively, a different screen may be displayed. For example, a text is displayed on the right display unit (display unit 2705 in FIG. 11C) and An image can be displayed on the display portion (the display portion 2707 in FIG. 11C). The semiconductor device shown in any one of 1 to 6 can be applied to the display portion 2705 and the display portion 2707. As a result, a high-performance and highly reliable electronic book can be obtained. When using a transmissive or reflective LCD device, it is expected that it will be used in relatively bright conditions. Therefore, solar panels will be installed to generate electricity and charge the battery. It is also possible to use a lithium-ion battery as the battery, which can reduce the size of the device. This has the advantage that

[0340] FIG. 11C shows an example in which an operating unit and the like are provided in the housing 2701. For example, The housing 2701 includes a power supply 2721, operation keys 2723, a speaker 2725, etc. The operation keys 2723 can be used to turn pages. A keyboard and a pointing device may be provided on the rear of the housing. On the front and sides, there are external connection terminals (earphone terminal, USB terminal, etc.), a recording medium insertion part, etc. Furthermore, the electronic book may be configured to have a function as an electronic dictionary. You may do so.

[0341] The electronic book may be configured to transmit and receive information wirelessly. It is also possible to purchase and download desired book data from the server. be.

[0342] FIG. 11D shows a mobile phone that is composed of two housings, a housing 2800 and a housing 2801. The housing 2801 includes a display panel 2802, a speaker 2803, a microphone, and a 2804, pointing device 2806, camera lens 2807, external connection terminal The housing 2800 also includes a solar cell for charging the mobile phone. The housing 28 is provided with an antenna, a memory slot 2810, and an external memory slot 2811. The semiconductor device according to any one of the first to sixth embodiments is incorporated in a display panel. By applying this to the 2802 panel, a high-performance and highly reliable mobile phone can be achieved. .

[0343] The display panel 2802 is equipped with a touch panel, and in FIG. The multiple operation keys 2805 are indicated by dotted lines. It also implements a boost circuit to boost the input voltage to the voltage required for each circuit.

[0344] The display direction of the display panel 2802 changes appropriately depending on the usage mode. Since it has a camera lens 2807 on the same surface as 2802, video telephony is possible. The speaker 2803 and the microphone 2804 are not limited to voice calls, but can also be used for video calls, Recording and playback are possible. Furthermore, the housing 2800 and the housing 2801 can be slid. As shown in 11(D), the device can be folded from the unfolded state to the overlapped state, making it suitable for carrying. This makes it possible to miniaturize the device.

[0345] The external connection terminal 2808 can be connected to various cables such as AC adapters and USB cables. It is possible to charge the battery and to communicate data with a personal computer, etc. A recording medium can be inserted into the memory slot 2811 to accommodate larger amounts of data storage and transfer. do.

[0346] In addition to the above functions, even if the device has infrared communication function, TV reception function, etc. good.

[0347] FIG. 11(E) shows a digital video camera, which includes a main body 3051, a display unit (A) 3057, An eyepiece 3053, an operation switch 3054, a display unit (B) 3055, a battery 3056, etc. The semiconductor device according to any one of the first to sixth embodiments is configured as a display device. By applying this to the display part (A) 3057 and the display part (B) 3055, a high-performance and highly reliable device can be achieved. The imaging device may be a digital video camera.

[0348] FIG. 11F shows an example of a television device. The television device includes a housing 96. The display unit 9603 is incorporated in the camera 01. The display unit 9603 can display images. In addition, in this embodiment, a structure in which a housing 9601 is supported by a stand 9605 is used. The semiconductor device described in any one of Embodiments 1 to 6 is applied to the display portion 9603. This makes it possible to provide a television apparatus with high performance and high reliability.

[0349] The television device can be operated using an operation switch on the housing 9601 or a separate remote control. In addition, the remote control device can be operated by transmitting the information output from the remote control device. A display unit for displaying information may be provided.

[0350] The television set is assumed to be equipped with a receiver and a modem. It can receive television broadcasts and can also communicate by wire or wirelessly via a modem. By connecting to a network, communication can be one-way (sender to receiver) or two-way (sender to It is also possible to communicate information between the sender and the recipient, or between the recipients themselves.

[0351] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is. EXAMPLES

[0352] In this embodiment, a first oxide semiconductor layer is formed on the first oxide semiconductor layer. A second oxide semiconductor layer having a thickness smaller than that of the first oxide semiconductor layer is formed, and a third oxide semiconductor layer is formed on the second oxide semiconductor layer. A sample with a nitride semiconductor layer is prepared, and the ionization potential of the sample is measured. The energy band diagram was calculated based on the results. The potential value is the sum of the band gap and the electron affinity. The value is obtained by measuring a single film of the material using an ellipsometer.

[0353] The sample is a single crystal silicon substrate with a 5 nm thick IGZO film and a 5 nm thick In-Sn The deposition conditions for each layer were: The film was formed by sputtering at a substrate temperature of 300°C in an oxygen atmosphere (100% oxygen). The target used was an oxide target with an atomic ratio of In:Ga:Zn=1:1:1. The In-Sn-Zn oxide film is formed by In:Sn:Zn= An oxide target with an atomic ratio of 2:1:3 is used.

[0354] In addition, a quartz substrate was used as the substrate, and the cross section of a sample obtained by laminating films under the same film forming conditions was photographed. The TEM photograph is shown in Figure 14(A). A schematic diagram is shown in Figure 14(B). In FIG. 1B, the interface of the oxide semiconductor layer is shown by a dotted line, but this is merely a schematic illustration. Depending on the material, film formation conditions, and heat treatment, the interface with each oxide semiconductor layer may become unclear. The sample photographed in FIG. 14(A) is a first film having a thickness of 5 nm on a quartz substrate 1000. IGZO film 1001, In-Sn-Zn oxide film 1002, 5 nm thick The second IGZO film 1003 is laminated on the In-Sn-Zn oxide film. The interface of the IGZO film can be seen. In FIG. 14(A), the second IGZO film 1003 and The In-Sn-Zn oxide film 1002 contains crystals and has a crystalline structure with a c-axis orientation. It can be seen that the first layer is an oxide semiconductor (CAAC). The IGZO film 1001 has an amorphous structure. In FIG. 14(A), two of the three layers are The second IGZO film is an oxide semiconductor film having a crystal structure, but is not particularly limited thereto. Only 1003 may have a crystal structure, or all three layers may have a crystal structure, or the three layers The entire structure may be amorphous.

[0355] Ultraviolet photoelectron spectroscopy (UPS) was performed while sputtering was being performed on the sample surface. Ionization by violet Photoelectron Spectroscopy The results of measuring the potential are shown in FIG.

[0356] In FIG. 12, the horizontal axis represents the sputtering time from the sample surface, and the vertical axis represents the ionization time. The potential is shown in Fig. 1. The sputtering of the IGZO film and the In-Sn-Zn oxide film The boundary of the sample is shown assuming that the rates are equal. It can be seen that the ionization potential is reduced in the In-Sn-Zn oxide film. The ionization potential represents the energy difference from the vacuum level to the valence band.

[0357] The conduction band is calculated by subtracting the band gap measured by ellipsometry from the ionization potential. The energy was calculated and the band structure of this laminated film was created. The band gaps of the Sn-Zn oxide films were set to 3.2 eV and 2.8 eV, respectively. The result is shown in Figure 13. In Figure 13, the energy band diagram is filled in like the one shown in Figure 4(C). It can be seen that an in-between channel is formed.

[0358] In this embodiment, IGZO films are used as the first oxide semiconductor layer and the third oxide semiconductor layer. has a higher ionization potential than the first oxide semiconductor layer and the third oxide semiconductor layer. The second oxide semiconductor layer has a small energy gap and is made of In-Sn The stacked layer using the -Zn-based oxide film has the energy band diagram shown in Figure 13 or Figure 4(C). It was confirmed that the first oxide semiconductor layer, the second oxide semiconductor layer, and The combination of materials for the third oxide semiconductor layer is not particularly limited, and may be any of the materials shown in FIG. Considering the energy gap of the material used by the implementer, the energy band diagram shown in For example, the first oxide semiconductor layer and the third oxide semiconductor layer may be made of a material selected from the materials. The first oxide semiconductor layer is an IGZO film, and the second oxide semiconductor layer is an indium zinc oxide film. A stacked layer using an oxide film may also be used. [Explanation of symbols]

[0359] 101 Oxide semiconductor layer 102 Oxide semiconductor layer 103 Oxide semiconductor layer 106 Element isolation insulating layer 108 Gate insulating film 110 Gate electrode 111 Oxygen excess region 112 Oxygen excess region 116 Channel formation region 120 Impurity region 121a Low resistance area 121b Low resistance region 121c Channel forming region 121d Low resistance region 121e Low resistance region 122a Low resistance area 122b Low resistance region 122c Channel formation region 122d Low resistance region 122e low resistance area 123a Low resistance area 123b Low resistance region 123c Channel forming region 123d low resistance region 123e Low resistance region 124 Metal compound area 128 Insulating film 130 Insulating film 140 Transistor 142a Drain electrode 142b Drain electrode 144 Oxide Semiconductor Stacking 146 Gate insulating film 148 Gate electrode layer 150 Insulating film 152 Insulating film 153 Electrode layer 156 Wiring 162 Transistor 164 Capacitive element 185 Substrate 191 Oxide Semiconductor Film 192 Oxide Semiconductor Film 400 Substrates 401 Gate electrode layer 402 Gate insulating film 403 Oxide Semiconductor Stacking 404a Source electrode layer 404b Drain electrode layer 405a Source electrode layer 405b Drain electrode layer 407 Insulating Film 415a Source electrode layer 415b Drain electrode layer 416 Insulating film 420 Transistor 421 Dopant 423 Transistor 425 Transistor 430 Transistor 431 Oxygen 436 Oxide insulating film 440a transistor 440b transistor 440c transistor 440d transistor 465a Wiring layer 465b Wiring layer 480a transistor 480b transistor 493 Lamination 601 Substrate 602 Photodiode 606a Semiconductor film 606b Semiconductor film 606c Semiconductor film 608 Adhesive layer 613 Substrate 631 Insulating film 632 Insulating film 633 Interlayer insulating film 634 Interlayer insulating film 640 Transistor 641 Electrode layer 642 Electrode layer 643 Conductive Layer 645 Conductive Layer 656 Transistor 658 Photodiode reset signal line 659 Gate signal line 671 Photo sensor output signal line 672 Photosensor reference signal line 1000 quartz substrate 1001 IGZO membrane 1002 In-Sn-Zn oxide film 1003 IGZO membrane 2701 Case 2703 Case 2705 ​​Display section 2707 Display section 2711 Shaft 2721 Power supply 2723 Operation key 2725 Speaker 2800 Chassis 2801 Case 2802 Display Panel 2803 Speaker 2804 Microphone 2805 Operation key 2806 Pointing Device 2807 Camera lenses 2808 External connection terminal 2810 Solar Cell 2811 External memory slot 3001 Main unit 3002 Case 3003 Display section 3004 Keyboard 3021 Main unit 3022 Stylus 3023 Display section 3024 Operation button 3025 External Interface 3051 Main unit 3053 Eyepiece 3054 Operation switch 3056 Battery 4001 Substrate 4002 Pixel section 4003 Signal line driver circuit 4004 Scanning line driver circuit 4005 Sealing material 4006 Substrate 4008 Liquid crystal layer 4010 Transistor 4011 Transistor 4013 Liquid crystal element 4015 Connection terminal electrode 4016 Terminal electrode 4018 FPC 4019 Anisotropic conductive film 4020 Insulating film 4021 Insulating film 4023 Insulating film 4030 Electrode layer 4031 Electrode layer 4032 Insulating film 4033 Insulating film 4510 Bulkhead 4511 Electroluminescent layer 4513 Light emitting element 4514 Filling material 9601 Case 9603 Display section 9605 Stand

Claims

[Claim 1] an oxide semiconductor stack including a first oxide semiconductor layer and a second oxide semiconductor layer having different energy gaps; a source electrode layer and a drain electrode layer over the oxide semiconductor stack; a gate insulating film on the source electrode layer and the drain electrode layer; a gate electrode layer formed on the gate insulating film and overlapping with the oxide semiconductor stack;

Citation Information

Patent Citations

  • Semiconductor device

    JP2003046081A

  • Thin-film transistor using amorphous oxide layer

    JP2007073701A

  • Transistor and electronic device

    JP2007096126A

  • Thin film field effect transistor and display using the same

    JP2009212497A

  • Transistor and method of manufacturing the same

    JP2009218562A