Conductive ink for copper-nickel alloy electrode, substrate having copper-nickel alloy electrode, and method for manufacturing them
A copper-nickel alloy conductive ink with controlled nickel content forms smooth, crack-free metal wiring, addressing cost and stability issues in printed electronics.
Patent Information
- Application Number
- JP2024116636
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing conductive inks for copper-nickel alloy electrodes are costly, lack sufficient stability, and result in irregular surfaces and cracks, limiting their practical application in printed electronics.
A conductive ink comprising a copper complex and a nickel complex, with a specific mass ratio of nickel to copper, is used to form a copper-nickel alloy, which is applied to a substrate and heated to create smooth, crack-free metal wiring.
The conductive ink enables low-cost, stable, and smooth metal wiring suitable for wearable devices, with improved oxidation resistance and reduced surface irregularities.
Smart Images

Figure 2024150614000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive ink for copper-nickel alloy electrodes, a substrate with a copper-nickel alloy electrode, and a method for producing the same. [Background technology]
[0002] In recent years, printed electronics has been developed as a wiring technology for semiconductor elements, electronic circuits, etc. Printed electronics has attracted attention because it can reduce manufacturing costs compared to existing semiconductor manufacturing technologies such as photolithography.
[0003] Inks using complexes have been developed as inks for such printed electronics (see, for example, Non-Patent Documents 1 and 2). According to Non-Patent Document 1, by using copper particles and a silver complex, it is possible to realize metal wiring having a core-shell structure in which copper particles are covered with a copper-silver alloy. According to Non-Patent Document 2, by using a copper complex and a silver complex, it is possible to realize metal wiring made of a copper-silver alloy. In all of these, by forming a copper-silver alloy, oxidation resistance is improved compared to metal wiring made of copper alone, but further improvement is required for practical use. In addition, unevenness, bumps, and cracks may occur on the electrodes during use, and stability is not sufficient. In addition, since the material contains silver, it is expensive.
[0004] Nickel particles are also used for electrodes because they are more chemically stable than copper particles and less expensive than silver particles (see, for example, Patent Document 1). Patent Document 1 discloses that nickel particles can be obtained from a nickel complex obtained from nickel formate dihydrate and an aliphatic amine, and reports that the particle size of the nickel particles can be controlled by changing the chain length of the alkyl group of the aliphatic amine.
[0005] Copper nanoparticles having a nickel-copper alloy in the surface layer have been developed (see, for example, Patent Document 2). Patent Document 2 discloses that the nickel-copper alloy in the surface layer improves oxidation resistance and is used for fine wiring by printing or coating. However, even when such copper nanoparticles are used, the ink stability is still not sufficient for practical use, and there are problems such as high baking temperature and high cost. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-064983 A [Patent Document 2] JP 2011-063828 A [Non-patent literature]
[0007] [Non-Patent Document 1] Wanli Li et al.,ACS Appl.Mater.Interfaces,2017,9,24711-24721 [Non-Patent Document 2] Wanli Li et al., Nanoscale, 2018, 10, 5254 Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the above, an object of the present invention is to provide a conductive ink for copper-nickel alloy electrodes, which is low-cost, has excellent atmospheric stability, and enables metal wiring with a smooth surface, a substrate with a copper-nickel alloy electrode, and methods for manufacturing the same. [Means for solving the problem]
[0009] The conductive ink for copper-nickel alloy electrodes according to the present invention contains a copper complex represented by general formula A and a nickel complex represented by general formula B, and the nickel content relative to the total mass of copper and nickel is in the range of 5 mass% or more and less than 80 mass%, thereby solving the above-mentioned problems. Cu(HCOO)2(L 1 ) m A Ni(HCOO)2(L 2 ) n B Here, m and n are natural numbers from 2 to 6, and L 1 are the same or different amino alcohols each having one amino group, and L 2 are the same or different aliphatic amines having one amino group, or vice versa. The amino alcohol may have one primary amino group, at least one hydroxyl group, and a saturated or unsaturated, linear, branched, or cyclic hydrocarbon group having from 1 to 20 carbon atoms. The amino alcohol may be 2-aminoethanol, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 1-amino-2-methyl-2-propanol, 2-amino-1-butanol, 1-amino-2-butanol, 2-amino-3,3-dimethyl-1-butanol, 2-amino-3-methyl-1-butanol, 2-amino-4-methyl-1-pentanol, 3-amino-1-propanol, 5-amino-1-pentanol, 6-amino-1-hexanol, or the like. The amino acid residue may be selected from the group consisting of 3-amino-2,2-dimethyl-1-propanol, 4-amino-1-butanol, 8-amino-1-octanol, 10-amino-1-decanol, 12-amino-1-dodecanol, 2-aminocyclohexanol, 4-amino-2-methyl-1-butanol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 3-amino-1,2-propanediol, and 2-amino-2-ethyl-1,3-propanediol. The aliphatic amine has one primary amino group and may have a saturated or unsaturated, linear, branched or cyclic hydrocarbon group having from 1 to 20 carbon atoms. The aliphatic amine may be selected from the group consisting of 2-ethylhexylamine, n-butylamine, tert-butylamine, benzylamine, n-hexylamine, 2-heptylamine, cyclohexylamine, and n-dodecylamine. The nickel content may be in the range of 10% by mass or more and 70% by mass or less. The nickel content may be in the range of 19 mass % or more and 67 mass % or less. The conductive ink may further contain copper and / or nickel particles. The conductive ink may further contain a monohydric alcohol and / or a polyhydric alcohol. The monohydric alcohol may be selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, and 2-methyl-2-butanol. The polyhydric alcohol may be selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentanediol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and glycerin. The method for producing the conductive ink according to the present invention comprises the steps of: 1 and mixing the amine ligand represented by the formula: 2 and mixing the copper complex and the nickel complex such that the mass ratio of the nickel complex to the copper complex is 0.05 or more and less than 6. 1are the same or different amino alcohols each having one amino group, and said L 2 are the same or different aliphatic amines having one amino group, or vice versa, thereby solving the above-mentioned problem. The nickel complex may further comprise a polyhydric alcohol. The polyhydric alcohol may be selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentanediol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and glycerin. The mixing may further include adding a monohydric alcohol. The mixing may further include mixing copper particles and / or nickel particles. The copper-nickel alloy electrode-attached substrate according to the present invention comprises a substrate and an electrode containing a copper-nickel alloy located on the substrate, and the content of nickel relative to the total mass of copper and nickel in the copper-nickel alloy is in the range of 5 mass% or more and less than 80 mass%, thereby solving the above-mentioned problems. The substrate may be selected from the group consisting of polyethylene naphthalate, polyimide, and polyolefin resins. The method for producing a copper-nickel alloy electrode-bearing substrate according to the present invention comprises applying the above-mentioned conductive ink to a substrate, and heating the substrate to which the conductive ink has been applied, thereby solving the above-mentioned problem. The coating may be performed using a method selected from the group consisting of a spin coating method, a spray coating method, a dip coating method, a slit coating method, a slot coating method, a bar coating method, a roll coating method, a curtain coating method, a gravure printing method, an inkjet method, and a screen printing method. The heating may be performed at a temperature in the range of 170° C. to 250° C. for a time in the range of 1 minute to 60 minutes. The method may further include, following the heating, heating by light irradiation. Effect of the Invention
[0010] The conductive ink for copper-nickel alloy electrodes of the present invention contains a copper complex represented by the above general formula A and a nickel complex represented by the general formula B, and the nickel content is in the range of 5% by mass or more and less than 80% by mass relative to the total mass of the copper in the copper complex and the nickel in the nickel complex. By containing a specific copper complex and nickel complex, the generation of copper oxide is suppressed, the formation of a copper-nickel alloy is promoted, and the ink is inexpensive and has excellent atmospheric stability. In addition, by controlling the nickel content within the above range, smooth metal wiring without cracks is possible.
[0011] Furthermore, by using the conductive ink for copper-nickel alloy electrodes of the present invention, a copper-nickel alloy can be easily formed at low temperatures, making it possible to provide a polymer substrate with a copper-nickel alloy electrode, which can be applied to wearable devices. [Brief description of the drawings]
[0012] [Figure 1] A flowchart showing the steps of producing the conductive ink of the present invention. [Diagram 2] Schematic diagram showing a copper-nickel alloy electrode-attached substrate of the present invention. [Diagram 3] A flowchart showing the steps for producing the copper-nickel alloy electrode substrate of the present invention. [Figure 4] A diagram showing the appearance of the electrode in Example 1 [Diagram 5] FIG. 1 shows optical microscope photographs of electrodes of Examples 1 to 6. [Figure 6] FIG. 1 shows optical microscope photographs of the electrodes of Examples 7 to 10. [Figure 7] FIG. 1 shows an SEM image of the electrode of Example 1. [Figure 8] Figure showing EDS elemental mapping of the electrode in Example 1. [Figure 9] FIG. 1 shows SEM images of electrodes of Examples 7 to 9. [Figure 10] FIG. 1 shows SEM images of electrodes of Examples 17 and 18. [Figure 11] FIG. 1 shows XRD patterns of electrodes of Examples 1 to 4. [Figure 12] FIG. 1 shows the electrical resistance of electrodes in Examples 1 to 4. [Figure 13] Graph showing the dependence of the electrical resistance of the electrode on the nickel content ratio [Figure 14] Figure showing the results of oxidation resistance tests DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted.
[0014] (Embodiment 1) In the first embodiment, a conductive ink for copper-nickel alloy electrodes and a method for producing the same according to the present invention will be described.
[0015] The conductive ink for copper-nickel alloy electrodes of the present invention (hereinafter simply referred to as conductive ink) contains a copper complex represented by general formula A and a nickel complex represented by general formula B. Cu(HCOO)2(L 1 ) m A Ni(HCOO)2(L 2 ) n B Here, m and n are natural numbers from 2 to 6, and L 1 and L 2 is an amine ligand. 1 are the same or different amino alcohols each having one amino group, and L 2 are the same or different aliphatic amines having one amino group, or vice versa, i.e., L 1 are the same or different aliphatic amines having one amino group, and L 2 are the same or different amino alcohols each having one amino group. By combining such an amino alcohol with an aliphatic amine, a copper-nickel alloy can be obtained in a heat treatment after application, and therefore a stable metal wiring having excellent oxidation resistance can be provided.
[0016] Furthermore, the conductive ink of the present invention satisfies the range of the nickel content relative to the total mass of the copper and nickel contained, which is 5% by mass or more and less than 80% by mass. If the nickel content is less than 5% by mass, the surface becomes uneven and smooth metal wiring cannot be obtained. If the nickel content is 80% by mass or more, cracks occur in the copper-nickel alloy, and the electrical resistance increases, so that the ink cannot function as an electrode.
[0017] L 1 The amino alcohol having one amino group, which is preferably a primary amino group, has at least one hydroxyl group, and has a linear, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms, which is saturated or unsaturated. By having a primary amino group, it coordinates with copper ions and forms a complex. By having one or more hydroxyl groups, it has excellent affinity with nickel complexes. If the carbon number is 1 to 20, a copper-nickel alloy can be obtained. From the viewpoint of affinity with nickel complexes and promotion of formation of copper-nickel alloys, the carbon number is more preferably 2 to 10, and even more preferably 2 to 5. L 1 may be the same or different, but is preferably the same from the viewpoint of yield.
[0018] As the amino alcohol having one amino group, an amino alcohol used in forming a copper complex in the production of ink using conventional copper nanoparticles can be applied. Preferably, the amino alcohol having one amino group is 2-aminoethanol, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 1-amino-2-methyl-2-propanol, 2-amino-1-butanol, 1-amino-2-butanol, 2-amino-3,3-dimethyl-1-butanol, 2-amino-3-methyl-1-butanol, 2-amino-4-methyl-1-pentanol, 3-amino-1-propanol, 5-amino-1-pentanol, 6-amino-1-pentanol, 7-amino-1-pentanol, 8-amino-1-pentanol, 9-amino-1-pentanol, 10-amino-1-pentanol, 11-amino-1-pentanol, 12-amino-1-pentanol, 13-amino-1-pentanol, 14-amino-1-pentanol, 15-amino-1-pentanol, 16-amino-1-pentanol, 17-amino-1-pentanol, 18-amino-1-pentanol, 19-amino-1-pentanol, 20-amino-1-pentanol, 21-amino-1-pentanol, 22-amino-1-pentanol, 23-amino-1-pentanol, 24-amino-1-pentanol, 25-amino-1-pentanol, 26-amino-1-pentanol, 27-amino-1-pentanol, 28-amino-1-pentanol, 29-amino-1-pentanol, 21-amino-1-pentanol, 22-amino-1-pentanol, 23-amino-1-pentan The copper complex is preferably selected from the group consisting of amino-1-hexanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-1-butanol, 8-amino-1-octanol, 10-amino-1-decanol, 12-amino-1-dodecanol, 2-aminocyclohexanol, 4-amino-2-methyl-1-butanol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 3-amino-1,2-propanediol, and 2-amino-2-ethyl-1,3-propanediol, which are readily available and promote the formation of the copper complex.
[0019] L 2 The aliphatic amine having one amino group, which is represented by the formula (I), has a primary amino group and a saturated or unsaturated, linear, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms. By having a primary amino group, it coordinates with nickel ions to form a complex. If the carbon number is 1 to 20, a copper-nickel alloy is obtained. From the viewpoint of affinity with the copper complex and promotion of the formation of the copper-nickel alloy, the carbon number is more preferably 2 to 10, and even more preferably 2 to 7. L 2 may be the same or different, but is preferably the same from the viewpoint of yield.
[0020] The aliphatic amine having one amino group is preferably selected from the group consisting of 2-ethylhexylamine, n-butylamine, tert-butylamine, benzylamine, n-hexylamine, 2-heptylamine, cyclohexylamine, and n-dodecylamine, which are readily available and promote the formation of nickel complexes.
[0021] In addition, L 2 Some of the above-mentioned aliphatic amines may have a hydroxyl group and may be amino alcohols. In this case, the amino alcohols may be the above-mentioned amino alcohols.
[0022] Also, L 1 and L 2 is a combination of the above amino alcohol and aliphatic amine, L 2 is an amino alcohol, and L 1 In the present invention, by satisfying this combination, a copper-nickel alloy is formed, resulting in smooth metal wiring. 1 Even when the amine is an aliphatic amine, some of the aliphatic amines may have a hydroxyl group, for example, the above-mentioned amino alcohol.
[0023] The formate ion in the copper formate of the general formula A and the nickel formate of the general formula B is selected from the ligand L 1 and L 2 The coordination form can be easily changed depending on the type of L. For this reason, the range of m and n is 2 to 6. For example, in the general formula A, L 1 When 2-amino-2-methyl-1-propanol (AMP) is selected as the ligand, the ligand is bidentate and m is 2. 2 When 2-amino-2-methyl-1-propanol (AMP) is selected as the ligand, the ligand is tetradentate and n is 4. Such a change in the coordination number is easily understood by those skilled in the art. The range of m and n is preferably 2 or more and 4 or less. This is preferable because it increases the metal content in the conductive ink.
[0024] In the conductive ink of the present invention, the nickel content relative to the total mass of copper and nickel is preferably in the range of 10% by mass or more and 70% by mass or less. Within this range, a smooth metal wiring with little unevenness on the surface can be obtained. The nickel content is more preferably in the range of 19% by mass or more and 67% by mass or less. Within this range, a very smooth metal wiring with very little unevenness on the surface can be obtained. The nickel content is even more preferably in the range of 30% by mass or more and 50% by mass or less. Within this range, a very smooth metal wiring with oxidation resistance and very little unevenness on the surface can be obtained.
[0025] The conductive ink of the present invention preferably further contains copper particles and / or nickel particles. This allows for thick metal wiring of several μm or more. The particle size of these particles is preferably in the range of 50 nm to 1 μm, more preferably in the range of 50 nm to 400 nm. This allows for thick metal wiring with less surface irregularities and no cracks.
[0026] When copper particles are further contained, the copper particles may be contained so that the content ratio of nickel to the total mass of copper and nickel satisfies the above-mentioned range. This allows for thick metal wiring with excellent coating properties, less surface irregularities, and no cracks. The same applies to nickel particles. The same applies to the case where both particles are contained.
[0027] The conductive ink of the present invention may further contain a monohydric alcohol and / or a polyhydric alcohol, which adjusts the viscosity and allows the copper complex and nickel complex to be mixed uniformly, resulting in an ink with excellent coatability.
[0028] The monohydric alcohol is preferably an alkyl alcohol, alkenyl alcohol, or cycloalkyl alcohol having 5 or less carbon atoms, and specific examples thereof include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, 2-methyl-2-butanol, cyclopropanol, cyclobutanol, and cyclopentanol. The monohydric alcohol is preferably selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, and 2-methyl-2-butanol, which are easily available and have a boiling point of 150° C. or less, and are therefore preferable for adjusting the viscosity.
[0029] The polyhydric alcohol may be a dihydric alcohol or a trihydric alcohol. The polyhydric alcohol is preferably selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentanediol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and glycerin. These are easily available, and will result in a conductive ink in which the copper complex and the nickel complex are uniformly mixed.
[0030] The viscosity of the conductive ink may be adjusted appropriately depending on the application. For example, when the conductive ink is used for inkjet printing, monohydric alcohol and / or polyhydric alcohol may be added so that the viscosity of the conductive ink is 1 mPa s or more and 20 mPa s or less.
[0031] Next, an exemplary method for producing the conductive ink for copper-nickel alloy electrodes of the present invention will be described. FIG. 1 is a flow chart showing the steps of producing the conductive ink of the present invention.
[0032] Step S110: Copper formate and L 1 and an amine ligand represented by the formula: 1 is the same as the amino alcohol having one amino group described above, so the explanation is omitted. The obtained copper complex has the above general formula A.
[0033] The mixing ratio (mass ratio) of the amino alcohol to the copper formate is preferably in the range of 0.6 to 1.5. More preferably, the mixing ratio of the amino alcohol is in the range of 0.6 to 1.0. When two or more kinds of amino alcohols are used, the total amount of the amino alcohols is adjusted to be in the above range. The mixing may be performed at room temperature using a stirrer or the like. If a deep blue color is visually confirmed, it can be determined that a copper complex has been obtained.
[0034] Step S120: Nickel formate and L 2 and an amine ligand represented by the formula: 2 is the same as the aliphatic amine having one amino group described above, so the explanation is omitted. The obtained nickel complex has the above general formula B.
[0035] The mixing ratio (mass ratio) of the aliphatic amine to nickel formate is preferably in the range of 0.75 or more and less than 2.4. More preferably, the mixing ratio of the aliphatic amine is in the range of 1.0 or more and 2.0 or less. When two or more kinds of aliphatic amines are used, the total amount of the aliphatic amines is adjusted to be in the above range. The mixing may be performed at room temperature using a stirrer or the like. If light blue, purple, light green or dark green is visually confirmed, it can be determined that a nickel complex has been obtained.
[0036] In the mixing, a polyhydric alcohol may be added as a solvent. This makes it easier to mix nickel formate with the aliphatic amine, and promotes the formation of a nickel complex. The polyhydric alcohol may be any of the polyhydric alcohols described above.
[0037] Step S130: The copper complex obtained in step S110 and the nickel complex obtained in step S120 are mixed. Here, the mixing is performed so that the mass ratio of the nickel complex to the copper complex is equal to or greater than 0.05 and less than 6. This allows the nickel content to be in the range of equal to or greater than 5 mass% and less than 80 mass% relative to the total mass of copper and nickel in the conductive ink, resulting in metal wiring with less surface irregularities and no cracks. The mixing may be performed at room temperature using a stirrer or the like.
[0038] More preferably, the mixing is carried out so that the mass ratio of the nickel complex to the copper complex is 0.15 to 3.5, inclusive. This allows the nickel content to be in the range of 10% by mass to less than 70% by mass relative to the total mass of copper and nickel in the conductive ink, resulting in metal wiring with less surface irregularities and no cracks.
[0039] More preferably, the mixing is carried out so that the mass ratio of the nickel complex to the copper complex is equal to or greater than 0.3 and equal to or less than 3. This ensures that the nickel content relative to the total mass of copper and nickel in the conductive ink is in the range of equal to or greater than 19 mass% and less than 67 mass%, resulting in metal wiring with less surface irregularities and no cracks.
[0040] In step S130, copper particles and / or nickel particles may be added. This allows for thick metal wiring of several μm or more. The amount of addition and particle size of these particles are as described above, so the explanation will be omitted. When copper particles are added, they should be added so that the nickel content relative to the total mass of copper and nickel in the final conductive ink is in the range of 5 mass% or more and less than 80 mass%. The same applies when nickel particles are added, and when both particles are added.
[0041] In step S130, a monohydric alcohol may be added. This adjusts the viscosity of the conductive ink, resulting in an ink with excellent coatability. The monohydric alcohol is as described above, so a description thereof will be omitted.
[0042] In step S110, the amine ligand L 1 In step S120, an amine ligand L 2 However, it is also possible to use an aliphatic amine in step S110 and an amino alcohol in step S120. In this case, the above-mentioned mass ratio can also be used.
[0043] (Embodiment 2) In the second embodiment, a copper-nickel alloy electrode-attached substrate and a method for producing the same according to the present invention will be described.
[0044] FIG. 2 is a schematic diagram showing a copper-nickel alloy electrode-attached substrate of the present invention.
[0045] The copper-nickel alloy electrode-attached substrate (hereinafter simply referred to as electrode-attached substrate) 200 of the present invention comprises a substrate 210 and an electrode 220 containing a copper-nickel alloy located on the substrate 210. The electrode 220 is formed from the conductive ink described in the first embodiment. Therefore, the content ratio of nickel to the total mass of copper and nickel in the copper-nickel alloy satisfies the range of 5 mass% or more and 80 mass% or less. This makes it possible to provide a substrate having smooth, crack-free electrodes or metal wiring. In particular, the formation of a copper-nickel alloy is inexpensive and has excellent atmospheric stability.
[0046] The electrode 220 may contain copper particles and / or nickel particles in addition to the copper-nickel alloy. This allows the electrode 220 to be a thick electrode of several μm or more. The particle size of these particles is preferably in the range of 50 nm to 1 μm, more preferably in the range of 50 nm to 400 nm. This allows for thick metal wiring with less surface irregularities and no cracks.
[0047] The electrode 220 may be a surface electrode that covers the entire substrate 210, or may have a predetermined pattern such as a comb shape or a lattice shape.
[0048] The substrate 210 may be a polymer substrate, a Si wafer, glass, ceramic, a metal plate, or the like. The polymer substrate is not particularly limited as long as it is resistant to a temperature of about 170°C, but may preferably be a polyester resin such as polyethylene naphthalate, polyimide, or polyolefin resin. The substrate is not limited to a plate shape, and may have a surface with a curvature. The substrate may also be a self-supporting film. A base layer such as a semiconductor film, a metal film, a dielectric film, or an organic film may be formed on the surface of the substrate. As described later, the conductive ink of the present invention can form a copper-nickel alloy by heating at a relatively low temperature of 170°C, so a polymer substrate can be used.
[0049] When the substrate 210 is a polymer substrate selected from the group consisting of polyethylene naphthalate, polyimide, and polyolefin resin, a flexible substrate with electrodes can be provided, which is advantageous for wearable devices.
[0050] Next, a method for producing an electrode-equipped substrate using the conductive ink for copper-nickel alloy electrodes of the present invention will be described. FIG. 3 is a flow chart showing the steps of producing a copper-nickel alloy electrode substrate of the present invention.
[0051] Step S310: The conductive ink for copper-nickel alloy electrodes of the present invention is applied to a substrate. The conductive ink is the same as that described in the first embodiment, and therefore the description is omitted. The substrate may be any of the above-mentioned substrates.
[0052] The method of applying the conductive ink to the substrate is not particularly limited as long as it can form a film, but for example, a method selected from the group consisting of spin coating, spray coating, dip coating, slit coating, slot coating, bar coating, roll coating, curtain coating, gravure printing, inkjet printing, and screen printing is used. If any of these methods is used, a uniform film can be formed.
[0053] Step S320: The substrate coated with the conductive ink obtained in step S310 is heated (baked). As a result, copper is precipitated from the copper complex in the conductive ink, nickel is precipitated from the nickel complex, and copper and nickel react to form a copper-nickel alloy. In addition, the amino alcohol and aliphatic amine are decomposed by heating. Here, in the process of producing a copper-nickel alloy from the conductive ink of the present invention, since copper is precipitated from the copper complex first, the amino alcohol, which is the amine ligand used to form the copper complex, can be widely used with the materials used in the manufacture of ink using the conventional copper nanoparticles exemplified above. In addition, in the precipitation of nickel from the nickel complex, if the precipitated nickel is a dense film-like body, the reactivity with copper is improved, and a sufficiently alloyed copper-nickel alloy is easily obtained. Therefore, it is preferable to use the materials exemplified above as the aliphatic amine, which is the amine ligand used to form the nickel complex, because the nickel precipitated from the nickel complex is more likely to become a dense film-like body. Even in the case of using a conductive ink manufactured using an aliphatic amine as the amine ligand used in forming a copper complex and an amino alcohol as the amine ligand used in forming a nickel complex, it is possible to obtain a sufficiently alloyed copper-nickel alloy by appropriately selecting the types of aliphatic amine and amino alcohol.
[0054] Heating is preferably performed at a temperature in the range of 170°C to 250°C for a time in the range of 1 minute to 60 minutes. This temperature range and heating time will produce a copper-nickel alloy. For heating, a hot plate, a thermostatic bath, an oven, or the like can be used. The heating atmosphere is preferably an inert gas atmosphere such as nitrogen or argon. This suppresses the production of copper oxide.
[0055] Following step S320, heating (sintering) by light irradiation may be performed. This further advances the sintering of the copper-nickel alloy particles, reducing the electrical resistance. Furthermore, the adhesion between the electrode and the substrate may also be improved. For such light irradiation, intense pulse light (IPL) or near-infrared laser may be used.
[0056] Next, the present invention will be described in detail using specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES
[0057] [reagent] Copper formate dihydrate (HCOO)2Cu 2H2O and nickel formate dihydrate (HCOO)2Ni 2H2O were purchased from Fujifilm Wako Pure Chemical Industries, Ltd. The amine ligand L shown in Table 1 was purchased from Nacalai Tesque, Inc. Ethylene glycol and isopropanol were purchased from Nacalai Tesque, Inc.
[0058] [Table 1]
[0059] [Example 1 to Example 21] In Examples 1 to 21, various conductive inks were produced using copper formate dihydrate, nickel formate dihydrate, and various amine ligands L shown in Table 1, and then electrodes were formed using the inks.
[0060] As shown in Table 2, copper formate dihydrate was mixed with 2-amino-2-methyl-1-propanol (AMP) or 2-ethylhexylamine (2EHA) to form a copper complex (step S110 in FIG. 1). Mixing was performed at room temperature (25° C.) using a stirrer (model ARE-310, manufactured by Thinky Corporation). After stirring, the mixture turned deep blue as shown in Table 2, and a copper complex was formed. The obtained copper complexes are referred to as Cu-AMP and Cu-2EHA, respectively.
[0061] [Table 2]
[0062] As shown in Table 3, nickel formate dihydrate, 2-amino-2-methyl-1-propanol (AMP), 2-ethylhexylamine (2EHA), ethylenediamine (ED), triethylenetetramine (TETA), hexylamine (HEA), or 2-heptylamine (2HEPA), and ethylene glycol (0.5 g) as a solvent were mixed to form a nickel complex (step S120 in FIG. 1). The mixing was performed at room temperature (25° C.) using a stirrer. After stirring, the color became light blue, purple, light green, or dark green as shown in Table 3, and a nickel complex was formed. The obtained nickel complexes are called Ni-AMP, Ni-2EHA, Ni-ED, Ni-TETA, Ni-HEA, and Ni-2HEPA, respectively.
[0063] [Table 3]
[0064] As shown in Table 4, the copper complex and the nickel complex were mixed (step S130 in FIG. 1). The mixing was performed using a stirrer at room temperature (25° C.). The conductive inks of Examples 11 to 16 were the same as the conductive ink of Example 1, but the conditions for forming the subsequent electrodes were different. In Examples 17 and 18, after mixing, 1 g of copper particles (average median diameter D50: 350 nm) was added to the mixture (4.4 g) of the copper complex and the nickel complex. The conductive ink of Example 21 was not mixed with the nickel complex and was a single copper complex. The nickel content ratio relative to the total mass of copper and nickel contained in the conductive ink obtained in this manner is shown in Table 4.
[0065] [Table 4]
[0066] The conductive inks of Examples 1 to 21 were applied to a polyimide substrate (manufactured by Toray Industries, Inc.) and a glass substrate (manufactured by Corning) by screen printing (step S310 in FIG. 3). The substrate was washed in an ultrasonic bath of ethanol for 15 minutes and then in distilled water for 1 minute to remove surface dirt. The substrate to which the conductive ink was applied was heated (baked) under the conditions shown in Table 5 (step S320 in FIG. 3). The heating was maintained for a predetermined time at the temperature under the conditions shown in Table 5 in a nitrogen atmosphere, and then allowed to cool. In Examples 16 and 18, following the heating, intense pulse light (IPL, manufactured by NovaCentrix, PulseForge Invent) was irradiated at 400 V for 2 ms.
[0067] [Table 5]
[0068] The electrodes of Examples 1 to 21 thus obtained were evaluated. The thickness of the electrodes was measured using a microprofile measuring instrument (manufactured by Kosaka Laboratory, model number ET200). The electrode surface was observed using an optical microscope (manufactured by Nikon Corporation) and a scanning electron microscope (SEM, manufactured by Hitachi High-Tech Corporation, S-4800). Element mapping was performed using an energy dispersive X-ray spectrometer (EDS) attached to the SEM. These results are shown in Figures 4 to 10.
[0069] The metals of the electrodes in Examples 1 to 21 were identified using an X-ray diffraction measurement device (XRD, Rigaku Corporation, SmartLab). The results are shown in Figure 11. The electrical resistance of the electrodes in Examples 1 to 21 was measured by the four-terminal method (Hioki E.E. Corporation, RM3545). These results are shown in Figures 12 and 13 and Table 6.
[0070] An oxidation resistance test was carried out on the electrodes of Examples 1, 6 to 8, and 21. In the test, each electrode was heated to 180° C. in the air, and the electrical resistance was measured after maintaining the temperature for a predetermined time. The results are shown in FIG.
[0071] FIG. 4 is a diagram showing the external appearance of the electrode of Example 1.
[0072] The upper part of Fig. 4 shows an electrode on a glass substrate, and the lower part of Fig. 4 shows an electrode on a polyimide substrate. According to Fig. 4, the electrodes on all of the substrates exhibit a metallic luster, and no irregularities or cracks were observed by visual inspection. Although not shown, the same was true for the electrodes of Examples 6 to 9 and Examples 11 to 20. If the conductive ink of the present invention is used, electrodes can be formed at relatively low temperatures, so polymer substrates can also be used.
[0073] FIG. 5 shows optical microscope photographs of the electrodes of Examples 1 to 6. FIG. 6 shows optical microscope photographs of the electrodes of Examples 7 to 10.
[0074] According to FIG. 5, the surface of the electrode of Example 1 was uniform, smooth, and free of irregularities. Although not shown, the surfaces of the electrodes of Examples 19 and 20 were also uniform, smooth, and free of irregularities. On the other hand, the surfaces of the electrodes of Examples 2 to 5 were non-uniform and had irregularities, spots, cracks, and the like, despite having the same nickel content (nickel content relative to the total mass of copper and nickel contained in the conductive ink) as the electrode of Example 1. This shows that a conductive ink containing a copper complex consisting of copper formate and a specified amino alcohol, and a nickel complex consisting of nickel formate and a specified aliphatic amine having one amino group is effective for metal wiring with a smooth surface. The electrical properties of the electrode of Example 5, which had cracks, were not measured.
[0075] Comparing the surfaces of the electrodes of Example 1 and Examples 6 to 10 in Figures 5 and 6, there was a tendency for the surfaces to become more uniform and smooth as the nickel content increased, but cracks occurred when the nickel content reached 80 mass% or more. In particular, it was found that uniform metal wiring was obtained when a conductive ink with a nickel content of 15% by mass or more to 70% by mass or less was used. This showed that a nickel content of 5% by mass or more and less than 80% by mass in the conductive ink is effective.
[0076] FIG. 7 is a diagram showing an SEM image of the electrode of Example 1. FIG. 8 shows EDS elemental mapping of the electrode of Example 1. FIG. 9 shows SEM images of the electrodes of Examples 7 to 9. FIG. 10 shows SEM images of the electrodes of Examples 17 and 18. As shown in FIG.
[0077] According to Fig. 7, it was found that the electrode of Example 1 was composed of particles having an average particle size of 75 nm or more and 150 nm or less. According to Fig. 8, it was found that the particles were composed of copper (Cu) and nickel (Ni), and that Cu and Ni were uniformly dispersed within the particles.
[0078] According to FIG. 9, the electrodes of Examples 7 to 9 are all made of particles having a particle size in the range of 10 nm or more and 1 μm or less. However, when comparing the particle sizes of the electrodes of Example 1 and Examples 7 to 9, it was found that the particle size depends on the nickel content, that is, the smaller the nickel content, the larger the particle size, and the higher the nickel content, the smaller the particle size.
[0079] FIG. 10 shows that in the electrode of Example 18 which was irradiated with light after heating, sintering between particles had progressed more than in the electrode of Example 17.
[0080] FIG. 11 is a diagram showing XRD patterns of the electrodes of Examples 1 to 4.
[0081] According to FIG. 11, the electrodes of Examples 1 to 3 showed only Cu(111) and Cu(200) peaks. This revealed that the electrodes of Examples 1 to 3 contained an alloy in which copper and nickel were uniformly mixed. This result was consistent with the result of FIG. 8. Although not shown, the electrodes of Examples 6 to 9 and Examples 11 to 20 also showed XRD patterns similar to that of the electrode of Example 1. On the other hand, the electrode of Example 4 showed Cu(111) and Cu(200) peaks and Ni(111) and Ni(200) peaks, indicating insufficient alloying.
[0082] FIG. 12 is a diagram showing the electrical resistance of the electrodes in Examples 1 to 4. In FIG. FIG. 13 is a graph showing the nickel content dependence of the electrical resistance of the electrode.
[0083] According to FIG. 12, the electrode of Example 1 had the smallest electrical resistance, and was shown to be effective as an electrode. FIG. 13 shows the relationship between the electrical resistance and the nickel content of the electrodes of Example 1, Example 6 to Example 10, and Example 21. According to FIG. 13, the electrical resistance increased in the electrode of Example 10 in which cracks occurred, but the electrodes of Example 1 and Example 6 to Example 9 in which cracks did not occur showed low electrical resistance similar to the electrode of Example 21 which did not contain nickel. From this, it was shown that a conductive ink containing a copper complex made of copper formate and a specified amino alcohol, and a nickel complex made of nickel formate and a specified aliphatic amine having one amino group, and having a nickel content in the range of 5 mass % or more and less than 80 mass %, is effective for metal wiring.
[0084] These results are summarized in Table 6. In Table 6, the symbols in the column "Formation of copper-nickel alloy" have the following meanings: circle: An alloy in which copper and nickel were uniformly mixed was formed, triangle: Copper and nickel were not sufficiently alloyed, cross: No nickel complex was used in the manufacture of the conductive ink. In addition, the "Morphology" column briefly shows the surface state of each of the electrodes described above.
[0085] [Table 6]
[0086] Table 6 shows that by using a conductive ink that contains a copper complex consisting of copper formate and a specified amino alcohol, and a nickel complex consisting of nickel formate and a specified aliphatic amine having one amino group, and in which the nickel content is in the range of 5% by mass or more and less than 80% by mass, it is possible to provide smooth metal wiring without any unevenness.
[0087] FIG. 14 shows the results of the oxidation resistance test.
[0088] According to Fig. 14, the electrodes of Example 1 and Examples 6 to 8 obtained using the conductive ink of the present invention maintained low resistance even after heating in the air, but the electrode of Example 21, which does not contain nickel, increased in resistance as the heating time in the air increased, and it no longer functioned as an electrode. This is because the electrodes of Example 1 and Examples 6 to 8 were made of a copper-nickel alloy, and therefore did not produce copper oxide even when heated in the air. This demonstrated that the conductive ink of the present invention is advantageous for producing electrodes made of a copper-nickel alloy with excellent oxidation resistance. [Industrial Applicability]
[0089] By using the conductive ink of the present invention, it is possible to provide metal wiring that is low-cost, has excellent atmospheric stability, and has a smooth surface, using inexpensive materials. [Explanation of symbols]
[0090] 200 Copper-nickel alloy electrode substrate 210 Substrate 220 Electrodes containing copper-nickel alloy
Claims
1. Contains a copper complex represented by general formula A and a nickel complex represented by general formula B, Further containing copper particles and / or nickel particles, A conductive ink for copper-nickel alloy electrodes, wherein the nickel content relative to the total mass of copper and nickel is in the range of more than 0 mass% and less than 80 mass%. Copper (HCO) 2 (L) 1 ) m ・・・A H 2 (L 2 ) n ・・・B Here, m and n are natural numbers from 2 to 6, and L 1 are the same or different amino alcohols each having one amino group, L 2 are the same or different aliphatic amines having one amino group, or vice versa.
2. The conductive ink according to claim 1 , wherein the copper particles and / or nickel particles have a particle size in the range of 50 nm to 1 μm.
3. The conductive ink according to claim 2 , wherein the copper particles and / or nickel particles have a particle size in the range of 50 nm to 400 nm.
4. The conductive ink according to any one of claims 1 to 3, wherein the amino alcohol has one primary amino group, at least one hydroxyl group, and a linear, branched, or cyclic hydrocarbon group that is saturated or unsaturated and has 1 to 20 carbon atoms.
5. The amino alcohols include 2-aminoethanol, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 1-amino-2-methyl-2-propanol, 2-amino-1-butanol, 1-amino-2-butanol, 2-amino-3,3-dimethyl-1-butanol, 2-amino-3-methyl-1-butanol, 2-amino-4-methyl-1-pentanol, 3-amino-1-propanol, 5-amino-1-pentanol, 6-amino-1-hex ...
5. The conductive ink of claim 4, wherein the at least one amino group is selected from the group consisting of amino-2,2-dimethyl-1-propanol, 4-amino-1-butanol, 8-amino-1-octanol, 10-amino-1-decanol, 12-amino-1-dodecanol, 2-aminocyclohexanol, 4-amino-2-methyl-1-butanol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 3-amino-1,2-propanediol, and 2-amino-2-ethyl-1,3-propanediol.
6. The conductive ink according to any one of claims 1 to 5, wherein the aliphatic amine has one primary amino group and a saturated or unsaturated, linear, branched or cyclic hydrocarbon group having from 1 to 20 carbon atoms.
7. 7. The conductive ink of claim 6, wherein the aliphatic amine is selected from the group consisting of 2-ethylhexylamine, n-butylamine, tert-butylamine, benzylamine, n-hexylamine, 2-heptylamine, cyclohexylamine, and n-dodecylamine.
8. The conductive ink according to any one of claims 1 to 7, further comprising a monohydric alcohol and / or a polyhydric alcohol.
9. 9. The conductive ink of claim 8, wherein the monohydric alcohol is selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, and 2-methyl-2-butanol.
10. 10. The conductive ink according to claim 8, wherein the polyhydric alcohol is selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentanediol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol, and glycerin.
11. A substrate; an electrode containing a copper-nickel alloy located on the substrate; Equipped with The electrode further contains copper particles and / or nickel particles; A substrate with a copper-nickel alloy electrode, wherein the content of nickel in the copper-nickel alloy is in the range of more than 0 mass% and less than 80 mass% relative to the total mass of copper and nickel.
12. The copper-nickel alloy electrode-attached substrate according to claim 11, wherein the content of nickel in the copper-nickel alloy is in the range of 5% by mass or more and less than 80% by mass with respect to the total mass of copper and nickel.
Citation Information
Patent Citations
Curable aqueous dispersion
JP1998182774A
Low-viscosity precursor compositions and methods for depositing conductive electron features
JP2005537386A
Electrically conductive ink composition and electric conduction part produced using the same
JP2012131894A
Conductive adhesive material, conductive laminate, method for manufacturing conductive laminate, wiring board, display device, and solar cell module
JP2013125655A
Method of producing conductive layer containing laminate
JP2014139893A