Substrate processing method and substrate processing system

The substrate processing method addresses residue issues in metal-containing resist films by using a developer and cleaning liquid with controlled solubility, combined with UV and heat treatment, effectively reducing residues and ensuring precise pattern formation for semiconductor manufacturing.

JP2024150767AActive Publication Date: 2024-10-23TOKYO ELECTRON LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024129764
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-23
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Conventional development methods for metal-containing resist films in semiconductor manufacturing leave residues on the substrate surface, leading to pattern defects due to incomplete dissolution of resist in the developer and polymerization reactions in unexposed areas.

Method used

A substrate processing method involving the use of a developer containing an organic solvent followed by a cleaning liquid with lower solubility for the resist film, combined with ultraviolet irradiation and heat treatment to promote polymerization and enhance resist dissolution, reducing residue on the substrate surface.

Benefits of technology

The method effectively reduces the amount of residue on the substrate surface, ensuring precise pattern formation by dissolving residual resist without collapsing patterns, thereby facilitating mass production of semiconductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150767000001_ABST
    Figure 2024150767000001_ABST
Patent Text Reader

Abstract

To reduce the amount of residues on a substrate surface generated during development of a metal-containing coating film.SOLUTION: A method for treating a substrate includes the steps of developing a substrate on which a metal-containing coating film has been exposed to a predetermined pattern, cleaning the substrate after development, irradiating the cleaned substrate with ultraviolet light having a wavelength of 190 to 400 nm, and supplying a pattern cleaning solution containing an organic solvent to the substrate after the ultraviolet light irradiation step.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate processing method and a substrate processing system. [Background technology]

[0002] Patent Document 1 discloses a coating and developing method including the steps of: applying a metal-containing resist to a surface of a substrate to form a resist film and exposing the resist film; developing the resist film by supplying a developer to the surface of the substrate to develop the resist film; and forming a first protective film prior to the developing step, which prevents at least the peripheral end face and the peripheral edge of the back surface side of the peripheral portion of the substrate on which the resist film is not formed from coming into contact with the developer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-047131 A Summary of the Invention [Problem to be solved by the invention]

[0004] The technology according to the present disclosure reduces the amount of residues on the substrate surface that are generated during development processing of a metal-containing coating film. [Means for solving the problem]

[0005] One aspect of the present disclosure is a method for treating a substrate, comprising the steps of: developing the substrate having a metal-containing coating film exposed to a predetermined pattern; cleaning the substrate after development; irradiating the cleaned substrate with ultraviolet light having a wavelength of 190 to 400 nm; and, after the ultraviolet light irradiation step, supplying a pattern cleaning solution containing an organic solvent to the substrate. Effect of the Invention

[0006] According to the present disclosure, it is possible to reduce the amount of residues on the substrate surface that are generated during development of a metal-containing coating film. [Brief description of the drawings]

[0007] [Figure 1] 1 is a plan view illustrating a schematic configuration of a substrate processing system according to an embodiment of the present invention; [Diagram 2] 2 is a front view showing a schematic configuration of the substrate processing system of FIG. 1. FIG. [Diagram 3] 2 is a rear view diagrammatically illustrating an outline of the configuration of the substrate processing system of FIG. 1. FIG. [Figure 4] 1 is a side cross-sectional view showing a schematic configuration of a developer supplying device according to an embodiment of the present invention; [Diagram 5] 1 is a side cross-sectional view that illustrates a schematic configuration of a cleaning liquid supplying device according to an embodiment. [Figure 6] 1 is a side cross-sectional view showing a schematic outline of a configuration of a heat treatment apparatus according to an embodiment; [Figure 7] 1 is a side cross-sectional view showing a schematic outline of a configuration of an ultraviolet irradiation device according to an embodiment. [Figure 8] 1A to 1C are explanatory views showing a state of a metal-containing coating film on a substrate in a substrate processing method according to an embodiment. [Figure 9] FIG. 2 is an explanatory diagram showing the state of an exposed portion and an unexposed portion of a metal-containing coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the manufacturing process of a semiconductor device, a photolithography process is performed, which includes forming a resist film by applying a resist to a semiconductor wafer (hereinafter referred to as "wafer"), exposing the resist film, and forming a resist pattern by developing the resist film after exposure. In recent years, the use of a resist solution containing a metal in the photolithography process has been considered in order to form a finer resist pattern.

[0009] However, in the development process of a metal-containing resist film exposed to a predetermined pattern, the resist dissolution material that is not sufficiently dissolved in the developer tends to remain as a residue on the wafer, and such residues cause pattern defects in the subsequent etching process. In particular, in the metal-containing resist film, the polymerization reaction of metal atoms and oxygen atoms tends to proceed little by little at the boundary with the exposed part even in the unexposed part, and since this polymerization reaction part is hardly soluble in the developer, residues tend to remain on the wafer. In the conventional development method, it is difficult to remove such residues, so that mass production of semiconductors using a metal-containing resist solution is difficult.

[0010] Therefore, the technology according to the present disclosure reduces the amount of residues on the substrate surface that are generated during development processing of a metal-containing coating film.

[0011] Hereinafter, a substrate processing method and a substrate processing system for carrying out the substrate processing method according to the present embodiment will be described with reference to the drawings. In this specification and the drawings, elements having substantially the same functional configurations are denoted by the same reference numerals, and duplicated explanations will be omitted.

[0012] Fig. 1 is a plan view showing a schematic configuration of a substrate processing system according to the present embodiment, while Fig. 2 and Fig. 3 are a front view and a rear view showing a schematic internal configuration of the substrate processing system 1.

[0013] 1, the substrate processing system 1 has a cassette station 10 where a cassette C containing a plurality of wafers W as substrates is loaded and unloaded, and a processing station 11 equipped with a plurality of various processing devices that perform predetermined processing on the wafers W. The substrate processing system 1 has a configuration in which the cassette station 10, the processing station 11, and an interface station 13 that transfers the wafers W between the processing station 11 and an exposure device 12 adjacent to the processing station 11 are integrally connected.

[0014] The cassette station 10 is provided with a cassette placement stage 20. The cassette placement stage 20 is provided with a plurality of cassette placement plates 21 on which the cassettes C are placed when the cassettes C are carried in and out of the substrate processing system 1.

[0015] The cassette station 10 is provided with a wafer transfer device 23 that is movable on a transfer path 22 extending in the X direction in Fig. 1. The wafer transfer device 23 is also movable in the up-down direction and around the vertical axis (the θ direction), and can transfer wafers W between the cassettes C on each cassette mounting plate 21 and a transfer device in the third block G3 of the processing station 11, which will be described later.

[0016] The processing station 11 is provided with a plurality of blocks, for example, four blocks G1, G2, G3, and G4, each equipped with various devices. For example, a first block G1 is provided on the front side (negative side in the X direction in FIG. 1) of the processing station 11, and a second block G2 is provided on the rear side (positive side in the X direction in FIG. 1) of the processing station 11. A third block G3 is provided on the cassette station 10 side (negative side in the Y direction in FIG. 1) of the processing station 11, and a fourth block G4 is provided on the interface station 13 side (positive side in the Y direction in FIG. 1) of the processing station 11.

[0017] 2, the first block G1 is provided with a plurality of liquid processing devices, for example, a developer supplying device 30, a resist coating device 31, and a cleaning liquid supplying device 32. The developer supplying device 30 performs a developing process on the wafer W. The resist coating device 31 supplies a resist liquid containing a metal (for example, Sn) as a metal-containing processing liquid to the wafer W to form a metal-containing resist film as a metal-containing coating film. The cleaning liquid supplying device 32 supplies a cleaning liquid containing an organic solvent to the wafer W to clean the wafer W. The number and arrangement of the developer supplying devices 30, resist coating devices 31, and cleaning liquid supplying devices 32 can be selected arbitrarily.

[0018] In these developing solution supplying device 30, resist coating device 31, and cleaning solution supplying device 32, for example, spin coating using a predetermined processing solution or coating solution is performed on the wafer W. In spin coating, for example, the processing solution or coating solution is discharged from a nozzle onto the wafer W, and the wafer W is rotated to spread the processing solution or coating solution on the surface of the wafer W.

[0019] 3, in the second block G2, a heat treatment device 40, a peripheral exposure device 41, and an ultraviolet irradiation device 42 are arranged vertically and horizontally. The heat treatment device 40 performs heat treatment such as heating and cooling of the wafer W. The peripheral exposure device 41 exposes the outer periphery of the wafer W. The ultraviolet irradiation device 42 irradiates ultraviolet light onto the wafer W. The number and arrangement of the heat treatment devices 40, peripheral exposure devices 41, and ultraviolet irradiation devices 42 can be selected arbitrarily.

[0020] For example, in the third block G3, a plurality of transfer devices 50, 51, 52, 53, 54, 55, 56 are provided in this order from the bottom up, while in the fourth block G4, a plurality of transfer devices 60, 61, 62 are provided in this order from the bottom up.

[0021] 1 and 3, a region surrounded by the first block G1 to the fourth block G4 forms a wafer transfer region D. In the wafer transfer region D, a wafer transfer device 70 is disposed.

[0022] Each of the wafer transfer devices 70 has a transfer arm 70a that is movable in, for example, the Y direction, the X direction, the θ direction, and the up and down direction. A plurality of wafer transfer devices 70 are arranged one above the other, and each wafer transfer device 70 moves within the wafer transfer region D and can transfer the wafer W to a predetermined device at approximately the same height in each of the blocks G1 to G4.

[0023] In addition, in the wafer transfer region D, a shuttle transfer device 80 is provided which linearly transfers the wafer W between the third block G3 and the fourth block G4.

[0024] The shuttle transfer device 80 is movable linearly, for example, in the Y direction in Fig. 3. The shuttle transfer device 80 moves in the Y direction while supporting the wafer W, and can transfer the wafer W between the delivery device 52 in the third block G3 and the delivery device 62 in the fourth block G4.

[0025] 1, a wafer transfer device 90 is provided next to the third block G3 on the positive side in the X direction. The wafer transfer device 90 has a transfer arm 90a that is movable in, for example, the X direction, the θ direction, and the up and down directions. The wafer transfer device 90 moves up and down while supporting a wafer W, and can transfer the wafer W to each delivery device in the third block G3.

[0026] The interface station 13 is provided with a wafer transfer device 100 and a delivery device 101. The wafer transfer device 100 has a transfer arm 100a that is movable in, for example, the Y direction, the θ direction, and the up and down directions. The wafer transfer device 100 supports a wafer W on, for example, the transfer arm 100a, and can transfer the wafer W between each delivery device in the fourth block G4, the delivery device 101, and the exposure device 12.

[0027] The above-described substrate processing system 1 is provided with a control unit 200. The control unit 200 is configured by a computer equipped with, for example, a CPU, a memory, and the like, and has a program storage unit (not shown). The program storage unit stores programs for controlling various processes in the substrate processing system 1. The above-described programs may be recorded in a computer-readable storage medium H and installed from the storage medium H to the control unit 200. A part or all of the programs may be realized by dedicated hardware (circuit board). It does not matter whether the storage medium H is a temporary storage medium or a non-temporary storage medium.

[0028] Next, various apparatuses for carrying out the substrate processing method according to the present embodiment will be individually and specifically described.

[0029] <Developer supply device> 4 is a side cross-sectional view showing a schematic outline of the configuration of the developer supplying apparatus 30 according to this embodiment. The developer supplying apparatus 30 has a processing vessel 110, and a loading / unloading port (not shown) for the wafer W is formed on the side of the processing vessel 110. A spin chuck 111 is provided in the processing vessel 110 as a substrate holding unit. The spin chuck 111 horizontally holds the wafer W as a substrate. The spin chuck 111 is connected to a rotating unit 112 that can be raised and lowered, and the rotating unit 112 is connected to a rotation driving unit 113 formed of a motor or the like. Therefore, the held wafer W can be rotated by driving the rotation driving unit 113.

[0030] A filter device 114 is provided on the ceiling of the processing vessel 110 , and a downflow of purified air is formed in the processing vessel 110 via an air supply part 115 .

[0031] A cup 116 is disposed outside the spin chuck 111 to prevent the scattering of the developing solution, cleaning solution, and mists thereof from scattering around. A drain pipe 117 and an exhaust pipe 118 are provided at the bottom of the cup 116. The exhaust pipe 118 is connected to an exhaust device 119 such as an exhaust pump.

[0032] A developer nozzle 120 is disposed in the processing vessel 110 as a developer supply unit that discharges a developer toward the surface of the wafer W. The developer nozzle 120 is provided on a nozzle support unit 121, such as an arm, which can be moved up and down by a drive mechanism (not shown) as indicated by a reciprocating arrow A shown by a dashed line in the figure, and can also be moved horizontally as indicated by a reciprocating arrow B shown by a dashed line. A developer is supplied to the developer nozzle 120 from a developer supply source 123 via a supply pipe 122.

[0033] Also disposed within the processing vessel 110 is a cleaning liquid nozzle 130 serving as a cleaning liquid supply unit that discharges a cleaning liquid toward the surface of the wafer W. The cleaning liquid nozzle 130 is provided on a nozzle support unit 131, such as an arm, which can be moved up and down by a drive mechanism (not shown) as indicated by a reciprocating arrow C shown by a dashed line in the figure, and can also be moved horizontally as indicated by a reciprocating arrow D shown by a dashed line. A cleaning liquid is supplied to the cleaning liquid nozzle 130 from a cleaning liquid supply source 133 via a supply pipe 132.

[0034] According to the developing solution supplying apparatus 30 of this embodiment, the developing solution or cleaning solution can be spread over the entire wafer W by supplying the developing solution or cleaning solution to the center of the wafer W while rotating the wafer W. However, the method of supplying the developing solution or cleaning solution is not particularly limited as long as it is a method capable of supplying the developing solution or cleaning solution to the surface of the wafer W, and therefore the configuration of the developing solution supplying apparatus 30 is not limited to the configuration described in this embodiment. The configuration of the apparatus is appropriately changed depending on the developing method to be adopted, such as paddle development or spray development.

[0035] <Cleaning liquid supply device> 5 is a side cross-sectional view showing a schematic outline of the configuration of the cleaning liquid supplying apparatus 32 according to this embodiment. The cleaning liquid supplying apparatus 32 has a housing 140, and a loading / unloading port (not shown) for the wafer W is formed on a side surface of the housing 140. A spin chuck 141 serving as a substrate holding unit is provided inside the housing 140. The spin chuck 141 horizontally holds the wafer W serving as a substrate. The spin chuck 141 is connected to a rotating unit 142 that can be raised and lowered, and the rotating unit 142 is connected to a rotation driving unit 143 constituted by a motor or the like. Therefore, the held wafer W can be rotated by driving the rotation driving unit 143.

[0036] A filter device 144 is provided on the ceiling of the housing 140 , and a downflow of purified air is formed within the housing 140 via an air intake section 145 .

[0037] A cup 146 is disposed outside the spin chuck 141 to prevent the scattering of the cleaning liquid and the mist thereof from scattering around. A drain pipe 147 and an exhaust pipe 148 are provided at the bottom of the cup 146. The exhaust pipe 148 is connected to an exhaust device 149 such as an exhaust pump.

[0038] A cleaning liquid nozzle 150 is disposed in the housing 140 as a cleaning liquid supply unit that discharges a cleaning liquid (a pattern cleaning liquid described later) toward the surface of the wafer W. The cleaning liquid nozzle 150 is provided on a nozzle support unit 151 such as an arm, and the nozzle support unit 151 can be moved up and down by a drive mechanism (not shown) as indicated by a reciprocating arrow E shown by a dashed line in the figure, and can also be moved horizontally as indicated by a reciprocating arrow F shown by a dashed line. A cleaning liquid is supplied to the cleaning liquid nozzle 150 from a cleaning liquid supply source 153 via a supply pipe 152.

[0039] According to the cleaning liquid supplying device 32 of the present embodiment, the cleaning liquid is supplied to the center of the wafer W while rotating the wafer W, thereby making it possible to spread the cleaning liquid over the entire wafer W. However, the method of supplying the cleaning liquid is not particularly limited as long as it is a method capable of supplying the cleaning liquid to the surface of the wafer W, and therefore the configuration of the cleaning liquid supplying device 32 is not limited to the configuration described in this embodiment.

[0040] <Heat treatment equipment> 6 is a side cross-sectional view showing a schematic outline of the configuration of the heat treatment apparatus 40 according to this embodiment. The heat treatment apparatus 40 has a processing vessel 160, and a loading / unloading port (not shown) for the wafer W is formed on a side surface of the processing vessel 160. A mounting table 161 is provided in the processing vessel 160 as a substrate holder for mounting the wafer W. A heater 162 is provided in the mounting table 161 as a heating section for the wafer W. The mounting table 161 has a plurality of through holes 163 formed therein. Lift pins 164a that move up and down within the through holes 163 are provided on a lift pin support 164. The lift pin support 164 is raised and lowered by a lift mechanism 165.

[0041] The heat treatment apparatus 40 is not limited to the configuration described in this embodiment, but may have any configuration capable of heating the wafer W.

[0042] <Ultraviolet irradiation device> 7 is a side cross-sectional view showing a schematic outline of the configuration of the ultraviolet irradiation device 42 according to this embodiment. The ultraviolet irradiation device 42 has a housing 170, and a loading / unloading port (not shown) for the wafer W is formed on a side surface of the housing 170. A mounting table 171 is provided in the housing 170 as a substrate holder for mounting the wafer W thereon. The mounting table 171 has a plurality of through holes 172 formed therein. Lift pins 173a that move up and down within the through holes 172 are provided on a lift pin support portion 173. The lift pin support portion 173 is raised and lowered by a lift mechanism 174.

[0043] Above the mounting table 171, a UV lamp 175 is disposed as an ultraviolet ray irradiator for irradiating the surface of the wafer W mounted on the mounting table 171 with ultraviolet rays. The UV lamp 175 in this embodiment radially irradiates ultraviolet rays having a wavelength of 190 to 400 nm. The ultraviolet ray irradiator 42 is not limited to the configuration described in this embodiment, and may have a configuration capable of irradiating the wafer W with ultraviolet rays having a wavelength of 190 to 400 nm. For example, a KrF exposure device having a wavelength of 248 nm is used as the ultraviolet ray irradiator 42.

[0044] The substrate processing system 1 according to this embodiment is configured as described above. Next, a substrate processing method for the wafer W in the substrate processing system 1 will be described.

[0045] When performing the developing process on the wafer W, first, in the resist coating apparatus 31, a metal-containing resist film R is formed on the surface of the wafer W (FIG. 8(a)).

[0046] Thereafter, the wafer W undergoes edge exposure processing in the edge exposure device 41, exposure processing in the exposure device 12, and PEB processing in the heat treatment device 40, so that an unexposed resist film R1 and an exposed resist film R2 are present on the surface of the wafer W (FIG. 8(b)). At this time, the resist film R2 in the exposed portion is in a state where a polymerization reaction has progressed overall, and the resist film R1 in the unexposed portion is in a state where a polymerization reaction has not progressed overall.

[0047] During the exposure process of the resist film R, due to the characteristics of the exposure machine, the exposure is performed in a state where the exposure intensity changes periodically as shown in Fig. 9. In more detail, the exposure intensity is low enough in the horizontal center of the unexposed resist film R1 that the polymerization reaction does not proceed, while the exposure intensity is higher in the vicinity of the boundary with the exposed resist film R2 than in the central portion. Therefore, in the unexposed resist film R1 near the boundary with the exposed resist film R2, there exists an area A1 where the polymerization reaction has proceeded, even though it is an unexposed area.

[0048] In addition, while the exposure intensity is high enough to allow the polymerization reaction to proceed sufficiently in the horizontal center of the exposed resist film R2, the exposure intensity is lower in the vicinity of the boundary with the unexposed resist film R1 than in the central portion. Therefore, in the exposed resist film R2 near the boundary with the unexposed resist film R1, there is a region A2 where the polymerization reaction has not progressed as much as in the central portion of the exposed resist film R2.

[0049] Next, the wafer W exposed to a predetermined pattern is transferred to a developer supplying device 30, where a developer is supplied to the surface of the wafer W. The developer supplied here contains an organic solvent. This dissolves the resist film R1 in the unexposed portion formed on the surface of the wafer W (FIG. 8(c)). The type of developer containing an organic solvent is not particularly limited as long as it is a processing liquid that does not dissolve the resist film R2 in the exposed portion. The developer may also be a mixture of two or more types of organic solvents. For example, 2-heptanone or a mixture of PGMEA (propylene glycol monomethyl ether acetate) and acetic acid may be used as the developer.

[0050] Most of the resist dissolved in the developer is removed from the surface of the wafer W together with the drained developer, but dissolved resist material that is not completely dissolved in the developer may remain as residue on the surface of the wafer W. In particular, the unexposed resist film R1 shown in FIG. 8(b) has an area A1 where a polymerization reaction has progressed, and this area A1 is less soluble in an organic solvent than other areas of the unexposed resist film R1. For this reason, the resist film R1 does not completely dissolve in this area A1, and dissolved resist material is likely to remain on the surface of the wafer W.

[0051] Next, a cleaning liquid is supplied to the wafer W on which the dissolved resist remains. The cleaning liquid supplied here contains an organic solvent, just like the developing liquid. Therefore, when the dissolved resist comes into contact with the cleaning liquid, the dissolved resist begins to dissolve. Then, the dissolved resist that has completely dissolved in the cleaning liquid is removed from the surface of the wafer W together with the waste cleaning liquid (FIG. 8(d)). This reduces the amount of dissolved resist remaining as residue on the surface of the wafer W.

[0052] In the above-mentioned step of supplying a cleaning liquid to the wafer W, a processing liquid having a lower solubility for the metal-containing resist film R than the developer is used as the cleaning liquid in order to avoid dissolving the pattern. Here, the "solubility of the metal-containing resist film R" of the developer or cleaning liquid is an index indicating the ease of dissolving the metal-containing resist film R in the developer or cleaning liquid. For example, when two types of processing liquids are supplied in equal amounts to the resist film R, the processing liquid having a smaller amount of dissolution (volume reduction) of the resist film R per unit time out of the two types of processing liquids is the processing liquid having a relatively smaller solubility for the metal-containing resist film R.

[0053] Generally, the developer has a solubility that does not dissolve the resist film R2 in the exposed area, but if a cleaning solution with a higher solubility than the developer is used, the resist film R2 in the exposed area may dissolve and the pattern shape may collapse. In addition, the polymerization reaction in the region A2 in the exposed resist film R2 is not as advanced as in other regions in the exposed resist film R2, so the region A2 is easily dissolved in an organic solvent. Therefore, if the solubility of the resist film R is the same in the cleaning solution and the developer, the region A2 may dissolve slightly, causing the pattern shape to collapse. Therefore, by using a treatment solution with a lower solubility in the resist film R than the developer as the cleaning solution, the resist soluble matter remaining on the surface of the wafer W can be dissolved without collapsing the pattern.

[0054] The type of the cleaning liquid containing an organic solvent is not particularly limited as long as the cleaning liquid has a smaller solubility of the resist film R than the developing liquid. The cleaning liquid may be a mixture of two or more organic solvents. For example, when the developing liquid is 2-heptanone, a processing liquid such as MIBC (methyl isobutyl carbinol) or PGMEA (propylene glycol monomethyl ether acetate) may be used as the cleaning liquid. For example, when the developing liquid is a mixture of PGMEA and acetic acid, a processing liquid such as 2-heptanone, MIBC, PGMEA, PGME (propylene glycol monomethyl ether), a mixture of PGMEA and PGME, or nBA (n-butyl acetate) may be used as the cleaning liquid. In this embodiment, since the developing liquid supply device 30 is provided with the cleaning liquid nozzle 130, the supply of the cleaning liquid following the supply of the developing liquid is performed by the developing liquid supply device 30, but the supply of the cleaning liquid may be performed by transporting the wafer W to the cleaning liquid supply device 32, for example.

[0055] According to the substrate processing method of the present embodiment, by performing the above-mentioned steps of supplying a developer to the wafer W and supplying a cleaning liquid to the wafer W, the amount of dissolved resist remaining as residue on the surface of the wafer W can be reduced, and a predetermined resist pattern can be formed on the wafer W.

[0056] Depending on the types and processing conditions of the metal-containing resist solution, developer, cleaning solution, etc., the dissolved resist remaining on the surface of the wafer W may be removed to an extent that satisfies the required quality at the stage where the step of supplying the cleaning solution to the wafer W shown in Fig. 8(d) is completed. In that case, the series of development steps for forming a resist pattern is completed at the step of supplying the cleaning solution to the wafer W shown in Fig. 8(d).

[0057] On the other hand, in order to further reduce the amount of residue remaining on the surface of the wafer W after the step of supplying the cleaning liquid to the wafer W, the following steps are carried out as necessary.

[0058] First, the wafer W cleaned with a cleaning liquid is transferred to the ultraviolet irradiation device 42, and the surface of the wafer W is irradiated with ultraviolet rays having a wavelength of 190 to 400 nm. In this process, for example, KrF exposure with a wavelength of 248 nm is performed. No mask is used during the irradiation of ultraviolet rays, and the entire wafer W is uniformly irradiated with ultraviolet rays. This causes the exposure reaction of the entire resist film R2 in the exposed portion to proceed further, and the exposure reaction also proceeds in the region A2 in the resist film R2 where the exposure reaction has not progressed relatively, similarly to other regions (FIG. 8(e)). Note that when the wavelength of the ultraviolet rays is less than 190 nm, a reaction occurs in which the C-O bond of the resist film R2 is broken by the irradiation of the ultraviolet rays, but the exposure reaction of the resist film R2 does not occur. In this embodiment, the irradiation of ultraviolet rays is performed by the ultraviolet irradiation device 42, but it may be performed by, for example, the exposure device 12.

[0059] Next, the wafer W irradiated with ultraviolet rays is transported to the heat treatment device 40 and heated. This further promotes the polymerization reaction of the resist film R2, the entire film of which has been sufficiently exposed, and the resist film R2 hardens and changes into a strong resist film R3 (FIG. 8(f)). In this embodiment, the wafer W is heated after the ultraviolet irradiation in the heat treatment device 40, but if the ultraviolet irradiation device 42 has a mechanism for heating the wafer W, the wafer W may be heated in the ultraviolet irradiation device. In addition, if the same module is capable of irradiating the wafer W with ultraviolet rays and heating the wafer W, the wafer W may be heated during or after the irradiation with ultraviolet rays.

[0060] Next, the heated wafer W is transferred to a cleaning liquid supplying device 32, and a cleaning liquid is supplied onto the surface of the wafer W. In addition, the "cleaning liquid" supplied here will be referred to as a "pattern cleaning liquid" in the following description for convenience's sake to distinguish it from the cleaning liquid supplied in the step shown in Fig. 8(d). The pattern cleaning liquid contains an organic solvent, and when the pattern cleaning liquid comes into contact with the dissolved resist material remaining on the surface of the wafer W, the dissolved resist material dissolves (Fig. 8(g)).

[0061] Since the resist film R3 hardened through ultraviolet irradiation and heat treatment is less soluble in organic solvents, it is possible to use a processing liquid as the pattern cleaning liquid that has a higher solubility for the resist film R than the cleaning liquid used before the ultraviolet irradiation. Therefore, it is possible to dissolve the dissolved resist material that could not be completely removed in the cleaning process of the wafer W shown in FIG. 8(d). The dissolved resist material dissolved in the pattern cleaning liquid is removed from the surface of the wafer W together with the drainage of the pattern cleaning liquid. This makes it possible to further reduce the amount of dissolved resist material remaining as residue on the surface of the wafer W.

[0062] The pattern cleaning liquid containing an organic solvent is not particularly limited as long as it is a treatment liquid in which the cured resist film R3 does not dissolve. The pattern cleaning liquid may be a mixture of two or more organic solvents. For example, an alkaline treatment liquid such as a treatment liquid containing TMAH (tetramethylammonium hydroxide) may be used as the pattern cleaning liquid. As an example, a TMAH aqueous solution having a mass percent concentration of 2.38% may be used as the pattern cleaning liquid. Also, a treatment liquid containing an organic acid such as acetic acid, formic acid, or citric acid may be used as the pattern cleaning liquid. In addition, since the cured resist film R3 is less soluble in an organic solvent than the resist film R2 before ultraviolet irradiation, it is also possible to select a treatment liquid that has a higher solubility of the resist film R than the developer as the pattern cleaning liquid.

[0063] In this embodiment, the supply of the pattern cleaning liquid is performed by the cleaning liquid supplying device 32, but if the developer supplying device 30 has a function of supplying a pattern cleaning liquid, the supply of the pattern cleaning liquid to the wafer W may be performed by the developer supplying device 30.

[0064] After cleaning with the pattern cleaning liquid, the wafer W is washed with pure water and dried, completing a series of development steps.

[0065] As described above, by irradiating the wafer W with ultraviolet light having a wavelength of 190 to 400 nm after supplying the developing solution, then heating the wafer W, and then supplying a pattern cleaning solution to the wafer W, the amount of resist dissolved material remaining as residue on the surface of the wafer W can be further reduced.

[0066] The embodiments disclosed herein should be considered as illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.

[0067] The substrate processing method according to the present disclosure can also be applied to processing substrates other than semiconductor wafers, such as FPD (flat panel display) substrates. [Explanation of symbols]

[0068] 1. Substrate Processing System 30 Developer supply device 32 Cleaning liquid supply device 200 Control section R Metal-containing resist film W wafer

Claims

1. A method for processing a substrate, comprising the steps of: developing the substrate on which the metal-containing coating film has been exposed in a predetermined pattern; cleaning the substrate after development; irradiating the cleaned substrate with ultraviolet light having a wavelength of 190 to 400 nm; a step of supplying a pattern cleaning liquid containing an organic solvent to the substrate after the step of irradiating with ultraviolet light.

2. heating the substrate during or after the irradiation with ultraviolet light; 2. The substrate processing method according to claim 1, further comprising the step of supplying the pattern cleaning liquid after the step of heating the substrate.

3. In the developing step, a developer containing an organic solvent is supplied to the substrate; In the cleaning step, a cleaning liquid containing an organic solvent is supplied to the substrate; the cleaning solution has a lower solubility for the metal-containing coating film than the developer, 3. The substrate processing method according to claim 1, wherein the pattern cleaning solution has a higher solubility for the metal-containing coating film than the cleaning solution.

4. 4. The substrate processing method according to claim 3, wherein at least one of the developing solution and the cleaning solution is a mixed solution of two or more kinds of organic solvents.

5. 4. The method of claim 3, wherein the developer is 2-heptanone.

6. 6. The substrate processing method according to claim 5, wherein the cleaning liquid is methyl isobutyl carbinol or propylene glycol monomethyl ether acetate.

7. 4. The substrate processing method according to claim 3, wherein the developer is a mixture of propylene glycol monomethyl ether acetate and acetic acid.

8. 8. The substrate processing method according to claim 7, wherein the cleaning liquid is any one processing liquid selected from the group consisting of 2-heptanone, methyl isobutyl carbinol, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, a mixed liquid of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, and n-butyl acetate.

9. 9. The substrate processing method according to claim 1, wherein the pattern cleaning liquid is an alkaline processing liquid or a processing liquid containing an organic acid.

10. A substrate processing system for processing a substrate, comprising: a developing section for developing the substrate; a cleaning unit for cleaning the substrate; A control unit that controls operations of the developing unit and the cleaning unit; an ultraviolet ray irradiation unit that irradiates the substrate with ultraviolet rays having a wavelength of 190 to 400 nm; a pattern cleaning solution supply unit for supplying a pattern cleaning solution to the substrate, The control unit is developing the substrate on which the metal-containing coating film has been exposed in a predetermined pattern; cleaning the substrate after development; irradiating the cleaned substrate with ultraviolet light having a wavelength of 190 to 400 nm; a step of supplying a pattern cleaning liquid containing an organic solvent to the substrate after the step of irradiating with ultraviolet light.

11. A heating unit for heating the substrate is provided, 11. The substrate processing system according to claim 10, wherein the control unit is configured to perform a step of heating the substrate during or after the irradiation with ultraviolet light, and to perform a step of supplying the pattern cleaning liquid after the step of heating the substrate.

12. the control unit executes control to supply a developing solution containing an organic solvent to the substrate in the developing step, and to supply a cleaning solution containing an organic solvent to the substrate in the cleaning step; the cleaning solution has a lower solubility for the metal-containing coating film than the developer, The substrate processing system according to claim 10 , wherein the pattern cleaning solution has a higher solubility for the metal-containing coating film than the cleaning solution.

13. The substrate processing system according to claim 12 , wherein at least one of the developing solution and the cleaning solution is a mixed solution of two or more kinds of organic solvents.

14. The substrate processing system of claim 12, wherein the developer is 2-heptanone.

15. 15. The substrate processing system of claim 14, wherein the cleaning liquid is methyl isobutyl carbinol or propylene glycol monomethyl ether acetate.

16. The substrate processing system of claim 12 , wherein the developer is a mixture of propylene glycol monomethyl ether acetate and acetic acid.

17. 17. The substrate processing system according to claim 16, wherein the cleaning liquid is any one processing liquid selected from the group consisting of 2-heptanone, methyl isobutyl carbinol, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, a mixed liquid of propylene glycol monomethyl ether acetate and propylene glycol monomethyl ether, and n-butyl acetate.

18. 18. The substrate processing system according to claim 10, wherein the pattern cleaning liquid is an alkaline processing liquid or a processing liquid containing an organic acid.

Citation Information

Patent Citations

  • Development processing method

    JP2006059918A

  • Method for forming resist pattern and method for producing mold

    JP2015053459A

  • Development unit, substrate processing apparatus, development method, and substrate processing method

    JP2017147328A

  • Photosensitive resin composition, method for producing cured film, cured film, liquid crystal display device and organic el display device

    WO2014088017A1

  • Polymer, positive resist composition, and resist pattern forming method

    WO2017130870A1