Heat treatment method
The heat treatment method addresses surface N concentration variations by controlling atmospheric pressure and ammonia concentration during nitriding, ensuring consistent N concentration in mass production processing.
Patent Information
- Application Number
- JP2023064905
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
AI Technical Summary
In mass production processing, variations in surface nitrogen concentration (N concentration) occur due to the loading location of products during nitriding following vacuum carburizing, making it difficult to achieve a desired surface N concentration consistently.
A heat treatment method involving vacuum carburizing followed by forced cooling, controlling atmospheric pressure in the nitriding chamber between 50 kPa to 1000 kPa, and adjusting the undecomposed NH3 concentration to a predetermined value by monitoring and regulating the ammonia gas flow, ensuring consistent surface N concentration.
The method effectively reduces variations in surface N concentration and achieves a desired, uniform N concentration across multiple workpieces by controlling atmospheric pressure and ammonia concentration during nitriding.
Smart Images

Figure 2024151517000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat treatment method in which reduced pressure carburizing and then nitriding are successively performed on a workpiece. [Background technology]
[0002] Carburizing is a surface treatment that introduces carbon atoms into the surface layer of steel and other workpieces to improve their properties, such as hardening the surface. Conventionally, gas carburizing has been used as a carburizing method, but it has problems such as a long carburizing time, and in recent years, reduced-pressure carburizing (vacuum carburizing), which is more advantageous in terms of energy saving and labor saving than gas carburizing, has been widely adopted.
[0003] In some cases, carbonitriding is performed to introduce N atoms into the surface layer along with C atoms. In carbonitriding, first, carburizing is performed to introduce C atoms into the surface layer, followed by nitriding to introduce N atoms into the surface layer. Such carbonitriding is considered to be effective in improving wear resistance, etc. For example, the following patent documents disclose a heat treatment method in which reduced pressure carburizing (vacuum carburizing) is followed by nitriding. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-17790 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in mass production processes that require the treatment of many workpieces at once, there is a problem that the N concentration on the surface of the workpieces (hereinafter sometimes referred to as "surface N concentration") is likely to vary depending on the loading location of the workpieces in the treatment chamber during the nitriding process that follows the reduced pressure carburization process, making it difficult to obtain the desired surface N concentration.
[0006] In light of the above circumstances, the present invention aims to provide a heat treatment method that makes it possible to easily control the surface N concentration when a workpiece is subjected to a series of heat treatments, which include reduced pressure carburization and then nitriding. [Means for solving the problem]
[0007] The present inventors have discovered the following while investigating the cause of the variation in surface N concentration in the nitriding treatment performed following reduced pressure carburization. (1) Rather than simply lowering the temperature to the nitriding temperature after carburizing, and then performing the nitriding treatment, it is possible to reduce the variation in the surface N concentration within the treatment chamber by forcibly applying cooling gas to the workpiece and circulating the gas within the treatment chamber. (2) The above-mentioned variation in the surface N concentration is largely dependent on the atmospheric pressure in the treatment chamber. Even when carburizing is performed in a vacuum, it is possible to reduce the variation in the surface N concentration by performing the subsequent nitriding treatment under a specified pressure higher than that during carburizing. (3) By controlling the pressure in the treatment chamber during nitriding within the above-mentioned specified range and the concentration of undecomposed NH3 in the atmosphere in the treatment chamber to an arbitrary value, it is possible to obtain a desired surface N concentration. The present invention was made based on these findings.
[0008] The heat treatment method of the present invention is a heat treatment method in which a workpiece is subjected to reduced pressure carburization treatment and then successively subjected to nitriding treatment, and is characterized in that after the reduced pressure carburization treatment, a cooling process is provided in which a cooling gas is applied to the workpiece to cool the workpiece, the atmospheric pressure in the treatment chamber during the nitriding treatment is set within a range of 50 kPa to 1000 kPa, the concentration of undecomposed NH3 sampled from within the treatment chamber is analyzed, and the amount of NH3 gas introduced into the treatment chamber is adjusted so that the concentration of undecomposed NH3 is constant.
[0009] According to the heat treatment method of the present invention thus defined, in a series of heat treatments consisting of reduced pressure carburization and then nitriding, the variation in surface N concentration due to the loading location is suppressed, and the undecomposed NH3 concentration is controlled to a predetermined value, thereby making it possible to obtain a desired surface N concentration.
[0010] In the heat treatment method of the present invention, the cooling temperature in the cooling step is The method may further comprise a reheating step of heating the workpiece to the temperature of the nitriding treatment after the cooling step, the temperature being lower than the temperature of the nitriding treatment.
[0011] Here, in the heat treatment method of the present invention, the carburizing treatment chamber and the nitriding treatment chamber can be constructed as separate chambers, and after the reduced pressure carburizing treatment, the workpiece can be moved from the carburizing treatment chamber to the nitriding treatment chamber and then the nitriding treatment can be performed.
[0012] In the heat treatment method of the present invention, the atmospheric pressure during the nitriding treatment can be set within a range of 50 kPa to 120 kPa.
[0013] In the heat treatment method of the present invention, the nitriding gas introduced into the treatment chamber during the nitriding treatment can be NH3 gas alone, a mixed gas of NH3 and N2, or a mixed gas of NH3, N2 and H2.
[0014] In the heat treatment method of the present invention, the nitriding treatment temperature can be set to 700°C to 1000°C.
[0015] In the heat treatment method of the present invention, the atmospheric pressure in the treatment chamber during the reduced pressure carburization treatment can be set to 0.1 kPa to 10 kPa. [Brief description of the drawings]
[0016] [Figure 1] 1 is a diagram showing a schematic configuration of a heat treatment chamber used in a heat treatment method according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a carburizing treatment chamber and a nitriding treatment chamber configured as separate chambers used in the heat treatment method of the present embodiment. [Diagram 3] FIG. 2 is a diagram showing a state in which the workpiece is loaded on a jig. [Figure 4] 4A to 4C are diagrams showing an example of a heat pattern and a pressure pattern in the heat treatment method of the embodiment. [Diagram 5] 1 is a graph based on the measurement results of the heat treatment conditions and the surface N concentration of the embodiment shown in Table 1. [Figure 6] 1 is a graph based on the measurement results of Table 2 showing heat treatment conditions and surface N concentration of an example. [Figure 7] 1 is a graph based on the measurement results of Table 3 showing heat treatment conditions and surface N concentration of an example. [Figure 8] 4 is a graph based on the measurement results of the heat treatment conditions and the surface N concentration of the examples shown in Table 4. [Figure 9] Table 5 shows the heat treatment conditions and the measurement results of the surface N concentration in the examples. [Figure 10] Table 6 shows the heat treatment conditions and the measurement results of the surface N concentration in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Next, embodiments of the present invention will be described in detail below. 1 shows a schematic configuration of a heat treatment chamber 1 used in the heat treatment method of this embodiment. The heat treatment chamber 1 performs reduced pressure carburizing and nitriding on a workpiece W as a treatment object that is loaded inside through a door (not shown). Inside the heat treatment chamber 1, there is provided a heater 5 for heating and keeping the workpiece W warm, and a convection heating fan 7 for stirring and convecting the supplied nitrogen gas, thereby promoting the temperature rise of the workpiece W during the temperature rise period.
[0018] In addition, various gas supply lines and exhaust lines are connected to the heat treatment chamber 1. In the figure, 10, 14, and 18 are gas supply nozzles, to which a first supply line 11 for supplying nitrogen gas, a second supply line 15 for supplying acetylene gas as a carburizing gas, and a third supply line 19 for supplying ammonia gas as a nitriding gas are respectively connected. Each of these supply lines includes a mass flow controller 22 for controlling the gas flow rate and an on-off valve 23. In some cases, a fourth supply line 20 for supplying hydrogen gas may also be provided.
[0019] An exhaust line 32 for exhausting gas inside the heat treatment chamber 1 is connected to the exhaust port 31, and the exhaust line 32 includes a vacuum pump 33 and an on-off valve 34. In addition, a pressure adjustment line 36 for maintaining a predetermined pressure inside the treatment chamber during the nitriding treatment is connected to the exhaust port 35. The pressure adjustment line 36 includes a pressure adjustment valve 37 and an on-off valve 38.
[0020] One end of a sampling line 42 for extracting the atmospheric gas within the heat treatment chamber 1 to the outside is connected to the gas outlet 41 of the heat treatment chamber 1. The sampling line 42 includes a pump 43 and an on-off valve 44. An analyzer 50 is provided on the other end of the sampling line 42, and the atmospheric gas extracted from the treatment chamber by the pump 43 is supplied to the analyzer 50.
[0021] The analyzer 50 includes an ammonia sensor for detecting the ammonia concentration, and detects the concentration of undecomposed NH3 in the ambient gas extracted through the sampling line 42. Then, a signal corresponding to the detected concentration is output to the control unit 52.
[0022] Based on a signal corresponding to the concentration of undecomposed NH3 sent from the analyzer 50, the control unit 52 controls the flow rate of the nitriding gas (here, ammonia gas) supplied into the treatment chamber via the mass flow controller 22 so that the concentration of undecomposed NH3 in the treatment chamber during the nitriding treatment remains constant at the same value as the set value.
[0023] 2 shows an example in which the carburizing chamber and the nitriding chamber used in the heat treatment method of this embodiment are configured as separate chambers. In the figure, 60 denotes a rail that serves as a conveying track extending linearly in the left-right direction in the figure, and multiple batch-type treatment chambers (here, carburizing chambers 62-1, 62-2, nitriding chamber 63, and quenching chamber 64) are arranged in a straight line along this rail 60 with their openings 78 facing in the same direction, that is, upward in the figure.
[0024] In this example, the carburizing chambers 62-1 and 62-2 perform reduced pressure carburizing treatment at a predetermined temperature (e.g., 930°C) on the workpiece W. The nitriding chamber 63 then performs nitriding treatment on the workpiece W at a predetermined temperature (e.g., 850°C).
[0025] 2, a charging table 66 is provided, and the workpiece W from the upstream process is first placed on this charging table 66. The workpiece W placed on the charging table 66 is subjected to reduced pressure carburization in the carburizing chambers 62-1, 62-2, and then to nitriding in the nitriding chamber 63. Then, the workpiece W is quenched in the quenching chamber 64.
[0026] The heat treatment equipment 1B of this example has a transport unit 70 that travels on the rails 60 in addition to the carburizing chambers 62-1, 62-2, the nitriding chamber 63, and the quenching chamber 64. The transport unit 70 has a transfer section 74 and a heat retention section 76, receives the workpiece W on the charging table 66, travels on the rails 10, and charges the workpiece W into either of the carburizing chambers 62-1, 62-2. Alternatively, the transport unit 70 receives the workpiece W that has been carburized in the carburizing chambers 62-1, 62-2 from the carburizing chambers 62-1, 62-2, travels on the rails 60, and charges the workpiece W into the nitriding chamber 63 where it is nitrided. When a plurality of batch-type carburizing chambers are provided in this way, it is possible to treat different types of parts, etc., in each of them. Furthermore, a plurality of batch-type nitriding chambers may be provided.
[0027] The transport unit has the same overall structure as the above-mentioned heat treatment chamber 1, and is equipped with a cooling fan and a nitrogen supply line for cooling the workpiece W. By controlling the frequency of this cooling fan, the strength or time of cooling can be controlled.
[0028] When the carburizing chamber and the nitriding chamber are constructed in separate chambers as in this example, it is possible to avoid ammonia reacting with the soot generated in the carburizing process and decomposing, making it easier to control the surface N concentration in the nitriding process.
[0029] 3 is a diagram showing an example of the loading state of workpieces W loaded into the treatment chamber. As shown in the figure, in this example, a large number of workpieces W are loaded on a loading jig 55, and the assembly of the large number of workpieces is loaded into the treatment chamber together with the loading jig 55. In this example, one of the objectives is to suppress the variation in surface N concentration depending on the loading location of the large number of workpieces.
[0030] 4 shows an example of a heat pattern and a pressure pattern in the heat treatment method of this embodiment. As shown in the figure, in this embodiment, the heat treatment is performed through each process of convection heating, vacuum heating, reduced pressure carburization, intermediate cooling (cooling process), heating (reheating process), pressure change, nitriding, and quenching.
[0031] In the first convection heating step, the workpiece W is loaded into the treatment chamber, the atmospheric gas in the treatment chamber is temporarily released outside the chamber, and then nitrogen gas is supplied into the treatment chamber through the first supply line 11, and the workpiece W is heated to a predetermined carburizing temperature (e.g., 930°C) and then soaked. Next, in the vacuum heating step, the pressure inside the treatment chamber is reduced to a predetermined pressure, and in the subsequent reduced pressure carburizing step, carburizing and subsequent diffusion are performed under reduced pressure at the predetermined carburizing temperature.
[0032] The reduced pressure carburizing process is carried out by bringing the workpiece W into contact with carburizing gas. The carburizing gas (acetylene gas in this example) is introduced into the process chamber at a gas amount determined in advance by simulation and for a set time so as to obtain the desired surface C concentration, C concentration distribution, and crystal grain size. The reduced pressure carburizing process can be carried out at a process temperature of 750 to 1050°C. To shorten the process time, it is preferable to carry out the carburizing process at a higher temperature, but the higher the process temperature, the more likely the crystal grains will become coarse, so the process time must be set taking this into consideration.
[0033] The pressure in the treatment chamber during reduced pressure carburization is preferably in the range of 0.1 kPa to 10 kPa. If the pressure is less than 0.1 kPa, the pressure fluctuations will be large when the amount of gas introduced is constantly changed, which is likely to cause variations. On the other hand, if the pressure exceeds 10 kPa, (1) the introduced carburizing gas may not reach the inside of the furnace (inside the treatment chamber), which may cause variations in the C concentration, and (2) if a large amount of carburizing gas is introduced in consideration of the above (1), a large amount of soot will be generated, which will wear out the furnace. Note that as the carburizing gas, a hydrocarbon gas, in particular acetylene, propane, etc., can be used.
[0034] After the reduced pressure carburization, the workpiece is cooled to a cooling temperature lower than the nitriding temperature (e.g., 850°C) (cooling step). After the predetermined cooling temperature is reached, the workpiece is reheated to the nitriding temperature. Specifically, in the case of a carburization temperature of 930°C, a gas flow of a cooling gas is applied to the workpiece in a high temperature state in a transport unit, and the workpiece is forcibly cooled to a low temperature of 100 to 650°C by gas cooling. The cooled workpiece is then reheated to the nitriding temperature (e.g., 850°C). By once lowering the temperature to a temperature lower than the nitriding temperature and then reheating, it is possible to further reduce the variation in the surface N concentration in the treatment chamber.
[0035] In the pressure changing step, nitrogen gas is introduced into the treatment chamber to change the atmosphere in the treatment chamber to a predetermined nitriding pressure (50 kPa to 1000 kPa), and the nitriding treatment is carried out at the nitriding treatment temperature (nitriding step).
[0036] The nitriding process is carried out by contacting the workpiece W with nitriding gas. In the nitriding process, ammonia contained in the atmosphere is decomposed on the workpiece surface as shown in the following formula (1), and N atoms are introduced into the surface layer of the workpiece. Here, [N] means the N atoms taken into the workpiece. NH3→[N]+3 / 2H2...Equation (1)
[0037] Here, the nitriding treatment is carried out at a treatment temperature of 700 to 1000°C. Below 700°C, the diffusion rate of N is slow, making it difficult to obtain the nitriding effect. Also, above 1000°C, the decomposition of ammonia in areas other than the workpiece surface progresses significantly, making it difficult to control the concentration of undecomposed NH3. In order to make it easier to control the concentration of undecomposed NH3, it is preferable to set the nitriding treatment temperature to 750°C or higher and 900°C or lower.
[0038] In the heat treatment method of this example, one of the features is that the pressure of the atmospheric gas is increased from the reduced pressure state during the carburizing treatment, and the nitriding treatment is performed at a pressure of 50 kPa to 1000 kPa. If the nitriding treatment is performed in a reduced pressure state of 10 kPa or less, as in the carburizing treatment, the NH3 partial pressure (total amount of NH3 molecules) becomes low, and the nitriding gas introduced into the treatment chamber does not reach the center part of the treatment chamber, resulting in variation in the surface N concentration depending on the loading location in the treatment chamber. For this reason, in the heat treatment method of this example, the atmospheric pressure in the treatment chamber during nitriding is set to 50 kPa or more in order to suppress the variation in the surface N concentration. On the other hand, the upper limit of the pressure is set to 1000 kPa in consideration of the pressure resistance of the heat treatment equipment. Here, the preferable atmospheric pressure is 50 kPa to 120 kPa. Within this pressure range, it is possible to suppress the variation in the surface N concentration of the workpiece without the need to excessively increase the pressure resistance of the equipment.
[0039] During the nitriding process, the flow rate of ammonia gas introduced into the process chamber is adjusted by the mass flow controller 22 to control the atmosphere. More specifically, a portion of the atmospheric gas is sent to the analyzer 50 through the sampling line 42, and the concentration of undecomposed NH3 in the atmospheric gas is detected by an ammonia sensor in the analyzer 50. The mass flow controller 22 then adjusts the flow rate of the ammonia gas based on the difference between the detected concentration of undecomposed NH3 and the target concentration of undecomposed NH3. In this example, the amount of ammonia gas introduced into the process chamber is adjusted so that the concentration of undecomposed NH3 becomes the target value, thereby controlling the surface N concentration of the workpiece W loaded into the heat treatment chamber 1 to a desired value. Here, the nitriding gas introduced into the treatment chamber can be selected from NH3 gas alone, a mixed gas of NH3 and N2, or a mixed gas of NH3, N2, and H2.
[0040] As shown in FIG. 4, after the nitriding treatment is completed, the workpiece W is moved to a quenching chamber (not shown) and quenched by being rapidly cooled from the quenching temperature. EXAMPLES
[0041] Next, an embodiment of the present invention will be described in detail. Here, assuming mass production, a carburizing chamber and a nitriding chamber were configured as separate chambers for a large number of workpieces W (see FIG. 3) loaded on a jig under the heat treatment conditions shown in the tables of FIG. 5 to FIG. 10, and after reduced pressure carburizing, the workpieces were moved from the carburizing chamber to the nitriding chamber by a transport unit and nitriding was performed. In addition, except for FIG. 6, after reduced pressure carburizing, the workpieces were cooled to a cooling temperature lower than the nitriding temperature (cooling process), and after cooling, the workpieces were reheated to the nitriding temperature (reheating process). In the cooling process, unless otherwise specified, cooling was performed by setting the cooling fan in the transport unit to 10 Hz. After the nitriding treatment was completed, the surface N concentration was measured for a total of 10 workpieces, including 8 workpieces located at the corners (see 56a, 56b, 56c, and 56d in Fig. 2, for example) from the workpiece assembly loaded on the jig, and 2 workpieces located at the center of the workpiece assembly. At that time, EPMA analysis was performed on the surface region (region from the outermost surface to a depth of 50 μm) of the workpiece W (measurement position was a specified flat surface), and the average value of the N concentration within that region was calculated, which was used as the surface N concentration value of the workpiece W. The average value, minimum value, maximum value, representative value ((maximum value + minimum value) / 2), and variation ((maximum value - minimum value) / 2) of the 10 surface N concentration values measured for each workpiece aggregate are shown in Figures 4 to 8.
[0042] Figure 5 shows the relationship between the nitriding pressure and the surface N concentration for workpieces treated at a nitriding temperature of 850°C. As shown in the figure, the variation in the surface N concentration increases as the nitriding pressure (ambient pressure in the treatment chamber) decreases. When the nitriding pressure is low, the NH3 partial pressure also decreases, so the total amount of NH3 molecules is small, and the workpieces near the periphery absorb a lot of gas and have a high N concentration, but the NH3 molecules do not reach the workpieces in the center, resulting in a low N concentration. As is clear from the graph in Figure 5, it is effective to keep the nitriding pressure in the range of 50 kPa to 120 kPa in order to suppress the variation in the surface N concentration.
[0043] Fig. 6 shows the relationship between the nitriding pressure and the surface N concentration for a workpiece treated at a nitriding temperature of 800°C, which is different from the example in Fig. 5. It can be seen that, even when treated at a nitriding temperature of 800°C, it is effective to set the nitriding pressure within the range of 50 kPa to 120 kPa, just as when treated at a nitriding temperature of 850°C. In this example, the nitriding treatment was started immediately after exposure to cooling gas for a predetermined period of time.
[0044] Fig. 7 shows the relationship between the total surface area of the workpieces loaded on the jig and the surface N concentration after nitriding. As shown in the figure, when the undecomposed NH3 concentration is controlled to a predetermined value (0.2%, 0.5%, 1.0%), a substantially constant surface N concentration is obtained even if the total surface area of the nitriding-treated workpieces is different. Therefore, in this example, as shown in Fig. 8, by controlling the undecomposed NH3 concentration to a desired constant value, the same surface N concentration can be obtained regardless of the surface area of the workpieces to be treated.
[0045] The relationship between the nitriding temperature and the surface N concentration is shown in Figure 9. As shown in the figure, if the nitriding pressure is within the range of 50 kPa to 120 kPa, the variation in the surface N concentration is suppressed to 0.02 to 0.03%, even when the nitriding temperature is changed within the range of 700 to 900°C.
[0046] Figure 10 shows the relationship between gas cooling conditions and surface N concentration. As shown in the figure, if the workpiece is cooled to a cooling temperature lower than the nitriding temperature after reduced pressure carburizing and then reheated to the nitriding temperature, the variation in surface N concentration is suppressed to 0.02-0.03%, even when the nitriding temperature is changed in the range of 750-850°C.
[0047] Although the embodiment and examples of the present invention have been described in detail above, these are merely examples, and the present invention can be configured in various modified forms without departing from the spirit and scope of the present invention. In the above embodiment, the cooling temperature in the cooling step is set lower than the temperature of the nitriding treatment, After the cooling step, the workpiece is reheated to the nitriding temperature, but the nitriding may be started directly after applying cooling gas for a prescribed period of time. Also, in the above Fig. 2, the carburizing chamber and the nitriding chamber are constructed as separate chambers, and after reduced pressure carburizing, the workpiece is moved from the carburizing chamber to the nitriding chamber for nitriding, but it is also possible to use a single treatment chamber and perform reduced pressure carburizing and then nitriding consecutively.
Claims
1. A heat treatment method in which a workpiece is subjected to reduced pressure carburization and then successively subjected to nitriding, comprising the steps of: a cooling step of applying a cooling gas to the workpiece to cool the workpiece after the reduced pressure carburizing treatment, The atmospheric pressure in the treatment chamber during the nitriding treatment is set within a range of 50 kPa to 1000 kPa, and undecomposed NH 3 Analyze the concentration of the undecomposed NH 3 NH introduced into the processing chamber so that the concentration is constant. 3 A heat treatment method characterized by adjusting the amount of gas.
2. The cooling temperature in the cooling step is lower than the temperature in the nitriding treatment, 2. The heat treatment method according to claim 1, further comprising a reheating step of heating the workpiece to a temperature for the nitriding treatment after the cooling step.
3. 3. The heat treatment method according to claim 1, wherein a carburizing chamber and a nitriding chamber are separate chambers, and after the reduced pressure carburizing treatment, the workpiece is moved from the carburizing treatment chamber to the nitriding treatment chamber and then the nitriding treatment is carried out.
4. 4. The heat treatment method according to claim 3, wherein the atmospheric pressure during the nitriding treatment is set within a range of 50 kPa to 120 kPa.
5. The nitriding gas introduced into the treatment chamber during the nitriding treatment is NH 3 Gas alone or NH 3 and N 2 or NH 3 and N 2 and H 2 4. The heat treatment method according to claim 3, wherein the mixed gas is a gas mixture of the above.
6. 4. The heat treatment method according to claim 3, wherein the nitriding treatment temperature is 700°C to 900°C.
7. 4. The heat treatment method according to claim 3, wherein the atmospheric pressure in the treatment chamber during the reduced pressure carburization treatment is 0.1 kPa to 10 kPa.
Citation Information
Patent Citations
Heat treatment equipment
JP2015017790A
Cited By
Surface nitriding strengthening treatment equipment and process for bench vice
CN121496318A