Laminate, printed circuit board, and method for manufacturing printed circuit board

The laminate with a smooth copper layer and intermolecular interaction layer addresses adhesion issues in printed circuit boards, ensuring high-definition copper wiring with minimal residue and reduced transmission loss, suitable for 5G and 6G communication.

JP2024153251APending Publication Date: 2024-10-29KONICA MINOLTA INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023067028
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing methods for improving adhesion between a smooth copper layer and an etching resist layer in printed circuit boards lead to frequent cracking, voids, and residue formation, which affects the integrity of the insulating resin layer and causes transmission loss in high-frequency communication technologies like 5G and 6G.

Method used

A laminate structure with a copper layer, resist layer, and an intermolecular interaction layer having a surface roughness of 0.3 μm or less, utilizing a nitrogen-containing heterocyclic compound with specific functional groups and controlled metal impurities, ensures strong adhesion without excessive residue.

Benefits of technology

The laminate provides high smoothness and accurate copper wiring patterns with minimal residue, reducing transmission loss and preventing insulating resin peeling, suitable for high-frequency communication technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153251000001_ABST
    Figure 2024153251000001_ABST
Patent Text Reader

Abstract

To provide a laminate for use in the manufacture of a printed circuit board, in which a copper layer has high smoothness while the copper layer and a resist layer have sufficient adhesion to form a desired copper wiring, and which leaves little residue after the resist layer is peeled off, and to provide a printed circuit board in which the surface of the copper wiring is highly smooth, the copper wiring pattern is highly accurate, and which leaves little residue of the resist layer, and a method for manufacturing the printed circuit board.SOLUTION: A laminate according to the present invention is a laminate for manufacturing a printed circuit board, and has a copper layer, a resist layer, and an intermolecular interaction layer that bonds the copper layer and the resist layer, and the surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a printed circuit board, and a method for manufacturing a printed circuit board. More specifically, the present invention relates to a laminate for use in the manufacture of printed circuit boards, in which the copper layer has high smoothness while the copper layer and resist layer have sufficient adhesion to form desired copper wiring, and which leaves little residue after the resist layer is peeled off. [Background technology]

[0002] In recent years, with the advancement of the data society, there is a demand for printed circuit boards with high density and high definition copper wiring. In the manufacturing process of printed circuit boards, before patterning the copper wiring by etching, an etching resist layer is bonded to the surface of the copper layer. In order to form high density and high definition copper wiring, high adhesion is required between the copper layer and the etching resist layer.

[0003] Conventionally, in order to improve the adhesion between the copper layer and the etching resist layer, the surface of the copper layer has been roughened and adhesion has been achieved through the anchor effect. However, the roughened surface of the copper layer can cause transmission loss for the short-wavelength radio waves used in communication technologies such as 5G and 6G. Therefore, there is a demand for technology that can improve the adhesion between a smooth, non-roughened copper layer and an etching resist layer.

[0004] As a method for improving the adhesion between the smooth copper layer and the etching resist layer, it is considered to provide an adhesive layer using an organic material between the copper layer and the etching resist layer. For example, Patent Document 1 discloses a surface treatment agent containing a triazole compound as a material capable of improving the adhesion between the smooth metal layer and the resin layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-135295 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, it has been found that when the surface treatment agent described in Patent Document 1 is used in the adhesive layer, cracks and voids occur more frequently during the high-temperature process in the production of printed circuit boards, and the insulating resin layer becomes more susceptible to peeling.

[0007] After thorough investigation into the causes of the above problems in the prior art, it was found that all of the problems were caused by a portion of the peeled etching resist layer remaining as a residue on the copper layer via the adhesive layer.

[0008] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a laminate for use in the manufacture of printed circuit boards, in which the copper layer has high smoothness while the copper layer and the resist layer have sufficient adhesion to form desired copper wiring, and which leaves little residue after the resist layer is peeled off. Another problem to be solved by the present invention is to provide a printed circuit board in which the surface of the copper wiring is highly smooth, the copper wiring pattern is highly accurate, and there is little residue of the resist layer, and a method for manufacturing the printed circuit board. [Means for solving the problem]

[0009] In order to solve the above problems, the present inventors have investigated the causes of the above problems, and as a result, have found that the above problems can be solved by providing an intermolecular interaction layer between a copper layer having a surface roughness Ra of 0.3 μm or less and a resist layer, thereby completing the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0010] 1. A laminate for manufacturing a printed circuit board, comprising: A copper layer; A resist layer; an intermolecular interaction layer that bonds the copper layer and the resist layer; The surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less. A laminate comprising:

[0011] 2. The intermolecular interaction layer contains a nitrogen-containing heterocyclic compound. 2. The laminate according to claim 1,

[0012] 3. The nitrogen-containing heterocyclic compound is a compound having both a nitrogen-containing heterocycle and a functional group containing a nitrogen atom or an oxygen atom, The number of nitrogen atoms in the nitrogen-containing heterocycle is 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom. 3. The laminate according to claim 2,

[0013] 4. The functional group is -COOH, -NH2, -OH, -NHR or -NR2, and R represents an alkyl group. 4. The laminate according to claim 3,

[0014] 5. The nitrogen-containing heterocyclic compound has a structure represented by the following general formula 1 or 2: 3. The laminate according to claim 2,

[0015] [ka]

[0016] In the formula, W1 to W7 each represent a carbon atom or a nitrogen atom, and 2 to 4 of W1 to W7 each represent a nitrogen atom, and at least one represents NH. Y1 to Y5 each represent a carbon atom or a nitrogen atom, and two to four of Y1 to Y5 each represent a nitrogen atom, and at least one represents NH. Z1 represents -COOH, -NH2, -OH, -NHR or -NR2. Z2 represents -COOH, -OH, -NHR or -NR2. R represents an alkyl group. L represents a single bond or a linking group.

[0017] 6. The total amount of Zn, Cr, Ni, and Sn present in the surface layer of the copper layer on the intermolecular interaction layer side is within the range of 0.001 to 1.000 at%. 2. The laminate according to claim 1,

[0018] 7. The copper layer contains at least Zn 2. The laminate according to claim 1,

[0019] 8. The resist layer contains a photosensitive resin. 2. The laminate according to claim 1,

[0020] 9. A printed circuit board having copper wiring, The surface roughness Ra of the copper wiring is 0.3 μm or less, There is no resist layer residue on the copper wiring A printed circuit board comprising:

[0021] 10. A method for manufacturing a printed circuit board using a resist layer, comprising: Step (A): A step of cleaning the surface of a copper layer having a surface roughness Ra of 0.3 μm or less with a chemical solution; Step (B): forming an intermolecular interaction layer directly on the copper layer after the cleaning; Step (C): forming a resist layer containing a photosensitive resin directly on the intermolecular interaction layer; Step (D): patterning the resist layer by exposure and development; Step (E): patterning the copper layer by etching; Step (F): peeling off the resist layer and the intermolecular interaction layer. A method for manufacturing a printed circuit board comprising the steps of:

[0022] 11. The total amount of Zn, Cr, Ni, and Sn present in the surface layer of the copper layer on the intermolecular interaction layer side in the step (B) is within the range of 0.001 to 1.000 at %. 11. The method for producing a printed circuit board according to claim 10.

[0023] 12. The pH of the chemical solution used in the step (A) at 25°C is 2 or less. 11. The method for producing a printed circuit board according to claim 10.

[0024] 13. The chemical solution used in the step (A) is an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid, and nitric acid. 11. The method for producing a printed circuit board according to claim 10. Effect of the Invention

[0025] The above-mentioned means of the present invention can provide a laminate for use in the manufacture of printed circuit boards, in which the copper layer has high smoothness while the copper layer and the resist layer have sufficient adhesion to form the desired copper wiring, and which leaves little residue after the resist layer is peeled off.

[0026] Furthermore, by the above-mentioned means of the present invention, it is possible to provide a printed circuit board having a highly smooth copper wiring surface, a highly accurate copper wiring pattern, and little residue of the resist layer, and a method for manufacturing the printed circuit board.

[0027] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.

[0028] Residues of the etching resist layer can cause cracks and voids, and also prevent the insulating resin layer, which is often designed to ensure adhesion with copper, from coming into contact with copper, making the insulating resin layer more likely to peel off.

[0029] As a result of investigating the cause of the residue, it was found that the adhesive layer was the cause. The surface treatment agent described in Patent Document 1 exerts strong adhesive strength by covalently bonding the triazole compound to the copper layer and the etching resist layer. This technology can ensure the adhesion between the copper layer and the etching resist layer, and thus enables the formation of the desired copper wiring. However, such strong adhesion by covalent bonding is too strong, preventing the etching resist layer from being peeled off cleanly, which causes residues on the etching resist layer.

[0030] In contrast, the laminate of the present invention has an intermolecular interaction layer between the copper layer and the resist layer, which bonds them together. Even when a copper layer having a high smoothness, such as a surface roughness Ra of 0.3 μm or less, is used, the intermolecular interaction layer can generate a sufficient level of adhesion between the copper layer and the resist layer to form the desired copper wiring. In addition, the adhesive strength of the intermolecular interaction is appropriately weaker than that of a covalent bond. Therefore, the intermolecular interaction layer is less likely to hinder the peeling of the etching resist layer, and the residue after the peeling of the etching resist layer can be reduced. [Brief description of the drawings]

[0031] [Figure 1] Schematic diagram showing the coordination state of nitrogen-containing heterocyclic compounds [Diagram 2] Diagram showing the copper wiring pattern formation process (copper clad laminate) [Diagram 3] Diagram showing the copper wiring pattern formation process (formation of an intermolecular interaction layer) [Figure 4] Diagram showing the copper wiring pattern formation process (forming a resist layer) [Diagram 5] Diagram showing the copper wiring pattern formation process (patterning of the resist layer) [Figure 6] Diagram showing the copper wiring pattern formation process (etching of the copper layer) [Figure 7] Diagram showing the copper wiring pattern formation process (peeling off the resist layer and the intermolecular interaction layer) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The surface modifier of the present invention is a laminate for manufacturing printed circuit boards, comprising a copper layer, a resist layer, and an intermolecular interaction layer that bonds the copper layer and the resist layer, and is characterized in that the surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less. This feature is a technical feature common to or corresponding to the following embodiments.

[0033] In an embodiment of the laminate of the present invention, the intermolecular interaction layer preferably contains a nitrogen-containing heterocyclic compound, which has a high adhesion improving effect since nitrogen atoms tend to strongly interact with components of the copper layer.

[0034] In an embodiment of the laminate of the present invention, the nitrogen-containing heterocyclic compound is a compound having both a nitrogen-containing heterocycle and a functional group containing a nitrogen atom or an oxygen atom, and the number of nitrogen atoms in the nitrogen-containing heterocycle is preferably 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom. This allows the nitrogen atom bonded to the hydrogen atom to interact with the metal and form a coordinate bond, improving the adhesion to the copper layer.

[0035] In an embodiment of the laminate of the present invention, the functional group is preferably -COOH, -NH2, -OH, -NHR or -NR2, and R represents an alkyl group. This allows the functional group to form a hydrogen bond or an ionic bond with a polar group of the resin contained in the resist layer. As a result, the nitrogen-containing heterocyclic compound can adhere to the resist layer with an interaction force stronger than π-π interaction or van der Waals force. In particular, it is preferable that the nitrogen-containing heterocyclic compound has a structure represented by the general formula 1 or general formula 2 in terms of improving adhesion between the copper layer and the resist layer.

[0036] In an embodiment of the laminate of the present invention, the total amount of Zn, Cr, Ni, and Sn present in the surface layer on the intermolecular interaction layer side of the copper layer is preferably within the range of 0.001 to 1.000 at%. When the total amount is 0.001 at% or more, these atoms act as a trigger to facilitate favorable peeling of the resist layer. When the total amount is 1.000 at% or less, the adhesion between the copper layer and the resist layer and the adhesion between the copper layer and the insulating resin layer are not easily impaired.

[0037] In an embodiment of the laminate of the present invention, the copper layer preferably contains at least Zn, which facilitates the peeling of the resist layer more suitably by using Zn as a trigger.

[0038] In an embodiment of the laminate of the present invention, the resist layer preferably contains a photosensitive resin, which enables the resist layer to be patterned by photolithography.

[0039] The printed circuit board of the present invention is a printed circuit board having copper wiring, characterized in that the surface roughness Ra of the copper wiring is 0.3 μm or less, and no resist layer residue remains on the copper wiring.

[0040] The method for producing a printed circuit board of the present invention is a method for producing a printed circuit board using a resist layer, and is characterized by including the above steps (A) to (F).

[0041] In an embodiment of the method for producing a printed circuit board of the present invention, the total amount of Zn, Cr, Ni, and Sn present in the surface layer of the copper layer on the intermolecular interaction layer side in the step (B) is preferably within the range of 0.001 to 1.000 at%. When the total amount is 0.001 at% or more, these atoms act as a trigger to facilitate favorable peeling of the resist layer. When the total amount is 1.000 at% or less, the adhesion between the copper layer and the resist layer and the adhesion between the copper layer and the insulating resin layer are not easily impaired.

[0042] In an embodiment of the method for producing a printed circuit board of the present invention, from the viewpoint of cleaning properties, it is preferable that the pH of the chemical solution used in the step (A) at 25° C. is 2 or less.

[0043] In an embodiment of the method for producing a printed circuit board of the present invention, from the viewpoint of cleaning properties, the chemical solution used in the step (A) is preferably an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid, and nitric acid.

[0044] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" include the lower limit and upper limit.

[0045] [Overview of the laminate of the present invention] The laminate of the present invention is a laminate for manufacturing a printed circuit board, and includes a copper layer, a resist layer, and an intermolecular interaction layer that bonds the copper layer and the resist layer. The copper layer has a surface roughness Ra of 0.3 μm or less on the side of the intermolecular interaction layer.

[0046] 4 is a schematic cross-sectional view of a laminate 6. The laminate 6 illustrated in FIG.

[0047] [Intermolecular interaction layer] The "intermolecular interaction layer" according to the present invention refers to a layer that adheres to at least one of the copper layer and the resist layer using a means other than the formation of a covalent bond as the main adhesion means.

[0048] The "means other than the formation of a covalent bond" mainly refers to an intermolecular interaction, but may be a combination of an intermolecular interaction and adsorption due to an anchor effect, etc. Intermolecular interactions include electrostatic interactions, van der Waals forces, hydrogen bonds, charge transfer interactions, hydrophobic interactions, etc.

[0049] The fact that the copper layer and resist layer of the laminate are bonded by the intermolecular interaction layer can be confirmed by the absence of silicon atoms (Si) between the bonded copper layer and resist layer. The absence of silicon atoms (Si) can be confirmed by secondary ion mass spectrometry (SIMS). When silicon atoms (Si) are present, it is considered that the copper layer and resist layer are bonded by a covalent bond via a compound containing silicon atoms (Si).

[0050] The intermolecular interaction layer contains at least a compound capable of intermolecular interaction with the components of the copper layer described below (hereinafter also referred to as "compound A"). The intermolecular interaction layer may contain one or more types of compound A. The intermolecular interaction layer may contain compounds other than compound A within a range that does not impair the effects of the present invention.

[0051] It is preferable that the compound A is non-photosensitive. The term "non-photosensitive" refers to a property in which, under normal conditions in the step of forming an intermolecular interaction layer, light is not absorbed, and the bonds within the molecule are not cleaved, or the molecules are not polymerized.

[0052] Compound A is preferably a nitrogen-containing compound, more preferably a nitrogen-containing heterocyclic compound, which has a high adhesion improving effect since the nitrogen atom of such a compound is likely to strongly interact with the components of the copper layer.

[0053] The nitrogen-containing heterocyclic compound is preferably a compound having both a nitrogen-containing heterocycle and a functional group containing a nitrogen atom or an oxygen atom.

[0054] The number of nitrogen atoms in the nitrogen-containing heterocycle is 2 to 4, and at least one of the nitrogen atoms is preferably bonded to a hydrogen atom, whereby the nitrogen atom bonded to the hydrogen atom interacts with the metal to form a coordinate bond, improving the adhesion to the copper layer.

[0055] The functional group containing a nitrogen atom or an oxygen atom is preferably -COOH, -NH2, -OH, -NHR or -NR2. The functional group is particularly preferably -COOH, -NH2 or -NR2. R represents an alkyl group. This allows the functional group to form a hydrogen bond or an ionic bond with the polar group of the resin contained in the resist layer. As a result, the nitrogen-containing heterocyclic compound can adhere to the resist layer with an interaction force stronger than π-π interaction or van der Waals force.

[0056] The nitrogen-containing heterocyclic compound preferably has a structure represented by the following general formula 1 or 2 in terms of improving adhesion between the copper layer and the resist layer.

[0057] [ka]

[0058] In the formula, W1 to W7 each represent a carbon atom or a nitrogen atom, and 2 to 4 of W1 to W7 each represent a nitrogen atom, and at least one represents NH. Y1 to Y5 each represent a carbon atom or a nitrogen atom, and two to four of Y1 to Y5 each represent a nitrogen atom, and at least one represents NH. Z1 represents -COOH, -NH2, -OH, -NHR or -NR2. Z2 represents -COOH, -OH, -NHR or -NR2. R represents an alkyl group. L represents a single bond or a linking group.

[0059] W1 to W7 form a fused ring.

[0060] Y1 to Y7 form a fused ring.

[0061] The linking group represented by L is, for example, an atom or an atomic group containing a carbon atom, a nitrogen atom, a sulfur atom, or an oxygen atom. Specific examples of the linking group represented by L include -O-, -S-, -N(R)-, -CO-, -SO2-, an alkylene group, an arylene group, and combinations thereof. R represents a hydrogen atom, an alkyl group, or a cycloalkyl group. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a 1,4-cyclohexylene group, a dodecylene group, a hexadecylene group, a 2-ethylhexylene group, and a 2-hexyldecylene group. Examples of the arylene group include a phenylene group, a naphthylene group, and the like.

[0062] As shown in FIG. 1, the molecular skeleton of the nitrogen-containing heterocyclic compound having the structure represented by General Formula 1 or General Formula 2 is likely to be coordinated in the vertical direction (thickness direction of the intermolecular interaction layer 3) in the intermolecular interaction layer 3. FIG. 1 shows the orientation of the nitrogen-containing heterocyclic compound using the exemplary compound (1) described later as an example. The molecular skeleton of the nitrogen-containing heterocyclic compound is coordinated in the vertical direction, so that the nitrogen atom in the ring skeleton of the nitrogen-containing heterocyclic compound interacts with the metal of the copper layer 2. This allows the alkylamino group, which is a functional group possessed by the nitrogen-containing heterocyclic compound, to approach the resist layer 4. As a result, the nitrogen-containing heterocyclic compound also interacts with the resist layer 4. The nitrogen-containing heterocyclic compound thus interacts with both the copper layer 2 and the resist layer 3, thereby improving their adhesion.

[0063] Examples of the nitrogen-containing heterocyclic compound having a structure represented by General Formula 1 or General Formula 2 are shown below. The nitrogen-containing heterocyclic compound according to the present invention is not limited to these.

[0064] [ka]

[0065] [ka]

[0066] [ka]

[0067] [Copper layer] The copper layer is a layer containing copper or a copper alloy as a main component. The term "main component" refers to a component contained in an amount of 50 mass% or more.

[0068] In addition to copper, the copper alloy may contain gold, silver, platinum, zinc, palladium, rhodium, osmium, ruthenium, iridium, copper, nickel, cobalt, iron, tin, chromium, titanium, tantalum, tungsten, indium, aluminum, lead, molybdenum, etc. The proportion of copper in the copper alloy is preferably 50 at % or more.

[0069] The copper layer of the laminate of the present invention is characterized in that the surface roughness Ra on the intermolecular interaction layer side is 0.3 μm or less, which makes the copper wiring formed from the copper layer less likely to cause cracks and voids in the high-temperature process during manufacturing, or to cause transmission loss of short-wavelength radio waves used in 5G and 6G communication technologies.

[0070] The surface roughness Ra is the arithmetic average roughness defined in JIS B 0601: 2013. The surface roughness Ra can be measured, for example, using a laser microscope (LASER MICROSCOPE VK-X100, manufactured by Keyence Corporation).

[0071] The total amount of Zn, Cr, Ni, and Sn present in the surface layer on the intermolecular interaction layer side of the copper layer is preferably within the range of 0.001 to 1.000 at%, with the total amount of elements present in the surface layer being 100 at%. When the total amount is 0.001 at% or more, these atoms act as a trigger to facilitate favorable peeling of the resist layer. When the total amount is 1.000 at% or less, the adhesion between the copper layer and the resist layer and the adhesion between the copper layer and the insulating resin layer are not easily impaired.

[0072] The copper layer preferably contains at least Zn. The amount of Zn present in the surface layer on the intermolecular interaction layer side of the copper layer is preferably within a range of 0.001 to 0.100 at%, with the total amount of elements present in the surface layer being 100 at%. When the amount of Zn is 0.100 at% or more, Zn serves as a trigger to facilitate favorable peeling of the resist layer. When the amount of Zn is 0.100 at% or less, the adhesion between the copper layer and the resist layer and the adhesion between the copper layer and the insulating resin layer are less likely to be impaired.

[0073] The elemental composition of the surface of the copper layer can be measured by the following procedure. First, a calibration curve of element amounts is created using a sample with a known elemental composition on the surface. A calibration curve in the range of 0.1 at% or more is created using data from X-ray photoelectron spectroscopy (XPS). A calibration curve in the range of less than 0.1 at% is created using data from secondary ion mass spectrometry (SIMS). Next, the elemental composition of the copper layer surface to be measured is analyzed using XPS and SIMS. The elemental composition of the copper layer surface is determined from the analysis values ​​and the calibration curve.

[0074] XPS is performed under the following conditions. XPS measurement device: Quantera SXM (ULVAC-PHI, Inc.) X-ray source: Monochromated Al-Kα radiation, 100 μm, 25 W, 15 kV Signal extraction angle: 45 degrees Analysis area: 500μm×500μm

[0075] In XPS, first, wide scan measurement is performed with a pass energy of 224 eV in the binding energy range of -20 to 1270 eV to determine which elements are detected. Next, narrow scan measurement is performed with a pass energy of 140 eV for all detected elements. Wide scan and narrow scan are performed at different positions on the same sample. Quantitative determination of the elemental composition on the surface of the copper layer is performed using analysis software MultiPak made by ULVAC-PHI. For the spectrum of each element, the background is determined by the Shirley method for elements other than copper, and by the linear method for copper. The elemental composition on the surface of the copper layer is obtained by using the relative sensitivity coefficient method from the obtained peak area.

[0076] SIMS measures the intensities of various metal ions under the following conditions. Equipment: TRIFT5 nanoTOF (ULVAC-PHI) Primary ion: Bi3 ++ Primary ion current: 2.0pA Data collection time: 60 seconds Repetition frequency: 8.2kHz Charge neutralization: ON Secondary ion polarity: Positive Mass scan range: m / z=0.5~2000

[0077] The copper layer may be a metal foil, a plating, or a film formed by a vacuum film forming method or the like.

[0078] The thickness of the copper layer is not particularly limited and may be, for example, a thickness corresponding to the thickness of the copper wiring pattern to be formed.

[0079] The copper layer may be a copper layer of a copper-clad laminate in which the copper layer is formed on an insulating layer, in which case the insulating layer of the copper-clad laminate is, for example, a resin sheet or a prepreg.

[0080] [Resist layer] The resist layer functions as a resist against etching of the copper layer, and is preferably made of, for example, an ultraviolet-curable epoxy resin containing an alkali-soluble resin, an ultraviolet-curable acrylic resin, or a polyimide.

[0081] The resist layer preferably contains a photosensitive resin. This allows the resist layer to be patterned by photolithography. The resist layer containing the photosensitive resin may be either a negative type in which the portion exposed to light forms a pattern, or a positive type in which the portion not exposed to light forms a pattern.

[0082] [Printed circuit board manufacturing method] The laminate of the present invention is used for manufacturing printed circuit boards, which include printed wiring boards (PWBs) before electronic components are mounted, and printed circuit boards (PCBs) after electronic components are mounted.

[0083] In the manufacture of a printed circuit board using the laminate of the present invention, for example, a copper wiring pattern is formed through the following steps. Step (A): A step of cleaning the surface of a copper layer having a surface roughness Ra of 0.3 μm or less with a chemical solution. Step (B): A step of forming an intermolecular interaction layer directly on the copper layer after the cleaning. Step (C): forming a resist layer containing a photosensitive resin directly on the intermolecular interaction layer. Step (D): patterning the resist layer by exposure and development. Step (E): patterning the copper layer by etching. Step (F): A step of peeling off the resist layer and the intermolecular interaction layer.

[0084] Examples of the above steps will be described with reference to FIGS.

[0085] In step (A), the surface of the copper layer having a surface roughness Ra of 0.3 μm or less is cleaned with a chemical solution. This makes it possible to remove dirt, antioxidants, oxide films, etc. adhering to the surface of the copper layer 2, which inhibit the interaction between the intermolecular interaction layer 3 and the copper layer 2. Figure 2 shows an example in which a copper-clad laminate 5 in which the copper layer 2 is formed on the insulating layer 1 is used.

[0086] The pH of the chemical solution used in step (A) at 25° C. is preferably 2 or less from the viewpoint of cleaning properties.

[0087] From the viewpoint of cleaning properties, the chemical solution used in step (A) is preferably an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid, and nitric acid.

[0088] After step (A), the surface of the copper layer 2 may be washed with water.

[0089] The insulating layer 1 is an insulating layer that serves as the base material of the printed circuit board. The insulating layer 1 is made of an insulating material such as resin, and may be a prepreg in which a base material such as paper or glass is impregnated with resin.

[0090] In step (B), an intermolecular interaction layer 3 is formed directly on the washed copper layer 2 (see FIG. 3). Specifically, an intermolecular interaction layer forming composition is applied directly on the copper layer 2 to form the intermolecular interaction layer 3.

[0091] The composition for forming an intermolecular interaction layer contains a compound (compound A) capable of intermolecular interaction with a component of the copper layer.

[0092] From the viewpoint of solubility, the composition preferably contains at least water or an alcohol as a solvent, such as methanol, ethanol, or 2-propanol.

[0093] The solvent may be a mixture of two or more types of water or alcohols. Specifically, the mass ratio of water to alcohol is preferably within a range of 100:0 to 50:50, and more preferably within a range of 100:0 to 75:25.

[0094] The content of compound A in the composition for forming an intermolecular interaction layer used in the step (B) is, for example, 0.001 to 0.1% by mass.

[0095] The composition for forming an intermolecular interaction layer may contain other components in addition to those described above, as long as the effects of the present invention are not impaired. Examples of the other components include surfactants, preservatives, stabilizers, acids, bases, pH adjusters, etc.

[0096] Between step (B) and the next step (C), it is preferable to have a step of washing the copper-clad laminate 5 on which the intermolecular interaction layer 3 has been formed with water. This makes it possible to remove excess components of the composition for forming the intermolecular interaction layer that have insufficient interaction with the copper layer 2.

[0097] In step (C), a resist layer 4 containing a photosensitive resin is formed directly on the intermolecular interaction layer 3 (see FIG. 4). The laminate 6 in this state includes an insulating layer 1, a copper layer 2, the intermolecular interaction layer 3, and a resist layer 4.

[0098] The resist layer 4 can be formed by laminating a dry film resist or by applying a liquid resist material.

[0099] In step (D), the resist layer 4 is patterned by exposure and development (see FIG. 5). Specifically, the resist layer 4 is first exposed to light using a photomask capable of exposing the resist layer 4 in an arbitrary pattern. Thereafter, unnecessary portions of the resist layer 4 are dissolved and removed using a developer, thereby patterning the resist layer 4.

[0100] After development, the resist layer 4 is preferably washed with water.

[0101] The exposure conditions and development conditions are not particularly limited, and conventionally known conditions can be used.

[0102] In step (E), the copper layer 2 is patterned by etching through the resist layer 4 (see FIG. 6). Specifically, the intermolecular interaction layer 3 and the copper layer 2 in the portion where the resist layer 4 has been removed are dissolved by wet etching using an etching solution. This results in patterning of the copper layer 2. At this time, the intermolecular interaction layer 3 may also be patterned together with the copper layer 2.

[0103] The etching conditions are not particularly limited, and conventionally known conditions can be applied.

[0104] In the step (F), the resist layer 4 and the intermolecular interaction layer 3 are peeled off from the copper-clad laminate 5 (see FIG. 7).

[0105] Although there is no particular limitation on the method for removing the resist layer 4 and the intermolecular interaction layer 3, it is preferable to remove them using a remover liquid. The remover liquid is not particularly limited, and a conventionally known remover liquid can be used.

[0106] By the above steps, the copper wiring pattern 7 can be formed.

[0107] In this method for forming the copper wiring pattern 7, the intermolecular interaction layer 3 is used to improve adhesion between the copper layer 2 and the resist layer 4 in the step (E). This makes it possible to prevent the etching solution from penetrating between the copper layer 2 and the resist layer 4, and thus makes it possible to form a high-density and high-definition copper wiring pattern 7.

[0108] [Printed circuit board] By using the laminate of the present invention, it is possible to produce a printed circuit board having copper wiring with a surface roughness Ra of 0.3 μm or less, and no resist layer residue on the copper wiring.

[0109] Such a printed circuit board is suitable for use in 5G and 6G communication technologies because it is less likely to cause transmission loss of short-wavelength radio waves due to the surface roughness Ra of the copper wiring being 0.3 μm or less. In addition, such a printed circuit board has a low frequency of cracks and voids occurring in the high-temperature process during manufacturing because there is no residue of the resist layer on the copper wiring. Furthermore, in such a printed circuit board, an insulating resin layer formed on the copper wiring is less likely to peel off because there is no residue of the resist layer on the copper wiring. EXAMPLES

[0110] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0111] [Preparation of treatment solution and copper-clad laminate] <Preparation of processing solution> The compounds shown in Table I were added to a solvent consisting of 20 mass % ethanol and 80 mass % ion-exchanged water so as to be 20 mass ppm, to prepare treatment liquids 1 to 26. Treatment liquids 1 to 24 are compositions for forming an intermolecular interaction layer.

[0112] [Table 1]

[0113] Comparative compounds A and B are compounds having the following structures, respectively: Comparative compounds A and B are compounds that form covalent bonds with a component contained in the copper layer and a component contained in the resist layer.

[0114] [ka]

[0115] <Adjusting the surface roughness Ra of the copper layer of copper-clad laminate> A copper-clad laminate (R-1766, manufactured by Panasonic) having a metal layer formed on an insulating layer was subjected to half-etching treatment using a sulfuric acid / peroxide-based etching solution. By adjusting the etching time, copper-clad laminates A to C with copper layers having the following surface roughness Ra were produced.

[0116] Copper-clad laminate A: Surface roughness Ra = 0.25 μm Copper-clad laminate B: Surface roughness Ra = 0.10 μm Copper-clad laminate C: Surface roughness Ra = 0.35 μm

[0117] [Example 1] <Preparation of Laminate and Printed Wiring Board> The steps (A) to (C) were carried out as described below to produce a laminate 1.

[0118] [Process (A)] The copper-clad laminate A prepared above was washed with a hydrochloric acid cleaning solution (manufactured by Sanwa Chemical Industry Co., Ltd., CP-30). Next, the copper-clad laminate A was washed using a chemical solution (hydrochloric acid, pH 1.1) and a spray-type cleaning device. Next, the copper layer was washed with water.

[0119] [Process (B)] The treatment liquid 1 prepared above was applied onto the copper layer using a spray type coating device. The surface onto which the treatment liquid was applied was then washed with water. The processed product was then drained with a PVA roller and dried with an air knife at 80°C to form an intermolecular interaction layer with a thickness of 5 nm.

[0120] [Process (C)] A dry film resist (AK-4034, manufactured by Asahi Kasei Corporation) was laminated on the intermolecular interaction layer by a hot roll laminator. The lamination conditions were roll temperature: 105°C, air pressure: 0.35 MPa, and lamination speed: 1.5 m / min. The dry film resist (AK-4034, manufactured by Asahi Kasei Corporation) used had a support made of a polyethylene terephthalate film on one side and a protective layer made of a polyethylene film on the other side. The lamination was performed by peeling off the protective layer while adhering the surface where the protective layer was located to the copper layer via the adhesive layer. This formed a resist layer that would become an etching resist.

[0121] By the above steps (A) to (C), a laminate 1 having a copper layer, an intermolecular interaction layer, and a resist layer was produced.

[0122] <Preparation of Laminates 2 to 7> Laminates 2 to 7 were produced in the same manner as in the production of laminate 1, except that the copper-clad laminate and the treatment solution were changed as shown in Table II. Note that laminates 5 and 6 have a covalent bond layer instead of an intermolecular interaction layer. Since step (B) was not performed in the production of laminate 7, laminate 7 does not have an intermolecular interaction layer.

[0123] <Preparation of printed wiring board> Using each of the produced laminates, steps (D) to (F) were carried out as described below to produce printed wiring boards.

[0124] [Process (D)] The resist layer of the laminate was exposed using a chrome glass mask and a parallel light exposure machine (Oak Corporation, HMW-801). The exposure conditions were 60 mj / cm, which is the recommended condition for dry film resist. 2 was adopted.

[0125] The support was peeled off from the exposed resist layer. After that, the resist layer was developed by dissolving and removing the unexposed parts using a developer consisting of an aqueous solution of 1% by mass of sodium carbonate (Na2CO3) and an alkaline developer. The development conditions were a temperature of 30°C and a development time of 3 minutes. Then, the processed product was washed with water.

[0126] By the above operations, the resist layer was patterned so that the copper wiring pattern after etching had a circuit width of 140 μm and a circuit length of 760 mm.

[0127] [Process (E)] The intermolecular interaction layer (or covalent bond layer) and the copper layer were etched by a dip method using an etching solution consisting of an aqueous solution of 2% by mass of hydrogen chloride (HCl) and 2% by mass of ferric chloride (FeCl3). The etching conditions were a temperature of 30°C and a dip time of 1 minute.

[0128] By the above operations, the intermolecular interaction layer (or the covalent bond layer) and the copper layer were patterned.

[0129] [Process (F)] The resist layer and the intermolecular interaction layer (or the covalent bond layer) were peeled off from the copper-clad laminate at a temperature of 50° C. using a stripping solution consisting of an aqueous solution of 3 mass % sodium hydroxide (NaOH).

[0130] By the above operations, a printed wiring board was produced.

[0131] <Evaluation of adhesion of resist layer> The copper wiring pattern on the printed wiring board was observed under a microscope, and the adhesion of the resist layer was evaluated according to the following criteria. The evaluation results are shown in Table II. "AA" and "A" were deemed to be acceptable for practical use.

[0132] AA: The remaining rate of copper wiring is 97% or more. A: The remaining rate of copper wiring is 95% or more but less than 97%. B: The remaining rate of copper wiring is less than 95%.

[0133] <Evaluation of peelability of resist layer> The copper wiring pattern on the printed wiring board was observed under a microscope. Based on the results of this observation and the time required for step (F), the peelability of the resist layer was evaluated according to the following criteria. The evaluation results are shown in Table II. "AA" and "A" were deemed to be acceptable for practical use.

[0134] AA: No resist layer residue was left, and the time required to complete stripping of the resist layer was shortened. A: There was no residue of the resist layer, but the time required to complete peeling of the resist layer was not shortened. B: Residue of the resist layer is present.

[0135] <Evaluation of transmission loss> A strip line was formed using a low dielectric polyphenylene ether resin film (Panasonic, multi-layer board material MEGTRON7, thickness 60 μm). A high-frequency signal was transmitted to the circuit formed on the copper foil of this printed wiring board using a network analyzer N5291A manufactured by Keysight Technologies, and the transmission loss was measured. The characteristic impedance was set to 50 Ω. The transmission loss was evaluated according to the following criteria based on the transmission loss at a frequency of 30 GHz. The evaluation results are shown in Table II. "AA" and "A" were deemed to be acceptable for practical use.

[0136] AA: The transmission loss is greater than -25 dB / 760 mm. A: The transmission loss is greater than -28dB / 760mm and less than -25dB / 760mm. B: Transmission loss is -28dB / 760mm or less.

[0137] [Table 2]

[0138] From the results of Example 1, it is found that the laminate of the present invention has a high smoothness of the copper layer, while the copper layer and the resist layer have sufficient adhesion to form the desired copper wiring, and the resist layer leaves little residue after peeling off. It is also found that the printed circuit board produced using the laminate of the present invention has a high smoothness of the copper wiring surface, a high-precision copper wiring pattern, and leaves little residue of the resist layer.

[0139] [Example 2] Laminates 8 to 31 were produced and evaluated using the treatment solutions shown in Table III in the same manner as in Example 1. The evaluation results are shown in Table III.

[0140] [Table 3]

[0141] From the results of Example 2, it can be confirmed that by incorporating any of the exemplary compounds (1) to (24) in the intermolecular interaction layer, it is possible to prepare a laminate in which the copper layer has high smoothness while the copper layer and the resist layer have sufficient adhesion to form the desired copper wiring, and which leaves little residue after the resist layer is peeled off.

[0142] [Example 3] Laminates 32 to 42 were produced and evaluated using the treatment solutions shown in Table IV in the same manner as in Example 1. The evaluation results are shown in Table IV.

[0143] In Example 3, in the chemical cleaning of the copper-clad laminate in step (A), the chemicals shown in Table V were used instead of the chemical (hydrochloric acid, pH 1.1). The pH of the chemicals shown in Table V is the value at 25° C. The time of chemical cleaning with the chemicals shown in Table V was adjusted as shown in Table V.

[0144] Chemical solution A is a 0.4 mass % aqueous solution of hydrogen chloride (hydrochloric acid). Chemical solution B is a 5 mass % aqueous solution of hydrogen chloride (hydrochloric acid). Chemical solution C is a 5 mass % aqueous solution of sodium carbonate. Chemical solution D is a 0.01% by mass aqueous solution of formic acid. Chemical solution E is a 0.05 mass % aqueous solution of sulfuric acid. Chemical solution F is a 0.04 mass % aqueous solution of nitric acid.

[0145] The element amounts [at %] of Zn, Cr, Ni, and Sn present in the surface layer on the intermolecular interaction layer side of the copper layer used in the laminates 32 to 42, with the total amount of elements present in the surface layer being 100 at %, were measured between steps (A) and (B) using the following method.

[0146] First, a calibration curve of the amount of elements was created using a sample with a known elemental composition on the surface. The calibration curve for the range of 0.1 at% or more was created using data from X-ray Photoelectron Spectroscopy (XPS). The calibration curve for the range of less than 0.1 at% was created using data from secondary ion mass spectrometry (SIMS).

[0147] Next, the elemental composition of the surface of the copper layer to be measured was analyzed by XPS and SIMS. The elemental composition of the surface of the copper layer was calculated from the analytical values ​​and the calibration curve.

[0148] XPS was performed under the following conditions. XPS measurement device: Quantera SXM (ULVAC-PHI, Inc.) X-ray source: Monochromated Al-Kα radiation, 100 μm, 25 W, 15 kV Signal extraction angle: 45 degrees Analysis area: 500μm×500μm

[0149] In XPS, first, wide scan measurement was performed with pass energy = 224 eV in the binding energy range of -20 to 1270 eV to determine what elements were detected. Next, narrow scan measurement was performed with pass energy = 140 eV for all detected elements. Wide scan and narrow scan were performed at different positions of the same sample. Quantification of the elemental composition of the copper layer surface was performed using analysis software MultiPak manufactured by ULVAC-PHI. For the spectrum of each element, the background was obtained by the Shirley method for elements other than copper, and by the linear method for copper. The elemental composition of the copper layer surface was obtained by using the relative sensitivity coefficient method from the obtained peak area.

[0150] The intensities of various metal ions were measured by SIMS under the following conditions. Equipment: TRIFT5 nanoTOF (ULVAC-PHI) Primary ion: Bi3 ++ Primary ion current: 2.0pA Data collection time: 60 seconds Repetition frequency: 8.2kHz Charge neutralization: ON Secondary ion polarity: Positive Mass scan range: m / z=0.5~2000

[0151] The measurement results are shown in Table V. In Table V, "-" indicates that the amount of the element is below the detection limit (0.001 at%) of the above measurement method.

[0152] [Table 4]

[0153] [Table 5]

[0154] From the results of Example 3, the following can be confirmed. The amount of dissimilar metals (metals other than Cu) on the surface of the copper layer can be adjusted by changing the type of chemical solution and cleaning time in process (A). The less dissimilar metals there are on the surface of the copper layer, the better the adhesion between the copper layer and the resist layer tends to be. The more dissimilar metals there are on the surface of the copper layer, the better the peelability of the resist layer tends to be.

[0155] Furthermore, from the above, it can be confirmed that the adhesion and removability of the resist layer can be controlled by the conditions of step (A). [Explanation of symbols]

[0156] 1. Insulation layer 2 Copper Layer 3 Intermolecular interaction layer 4 Resist layer 5 Copper-clad laminate 6 Laminate 7 Copper wiring pattern

Claims

1. A laminate for manufacturing a printed circuit board, a copper layer; a resist layer; an intermolecular interaction layer that bonds the copper layer and the resist layer; The surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less. A laminate characterized by:

2. The intermolecular interaction layer contains a nitrogen-containing heterocyclic compound. The laminate according to claim 1 .

3. the nitrogen-containing heterocyclic compound is a compound having both a nitrogen-containing heterocycle and a functional group containing a nitrogen atom or an oxygen atom, The number of nitrogen atoms in the nitrogen-containing heterocycle is 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom. The laminate according to claim 2 .

4. The functional group is —COOH, —NH 2 , —OH, —NHR or —NR 2 and R represents an alkyl group. The laminate according to claim 3 .

5. The nitrogen-containing heterocyclic compound has a structure represented by the following general formula 1 or 2: The laminate according to claim 2 . 【Chemical 1】 [In the formula, W 1 ~W 7 represents a carbon atom or a nitrogen atom. 1 ~W 7 Among these, 2 to 4 represent nitrogen atoms, and at least one represents NH. Y 1 ~Y 5 represents a carbon atom or a nitrogen atom. 1 ~Y 5 Among these, 2 to 4 represent nitrogen atoms, and at least one represents NH. Z 1 is -COOH, -NH 2 , —OH, —NHR or —NR 2 Represents Z. 2 is —COOH, —OH, —NHR or —NR 2 R represents an alkyl group. L represents a single bond or a linking group.

6. The total amount of Zn, Cr, Ni, and Sn present in the surface layer of the copper layer on the intermolecular interaction layer side is within the range of 0.001 to 1.000 at %. The laminate according to claim 1 .

7. The copper layer contains at least Zn. The laminate according to claim 1 .

8. The resist layer contains a photosensitive resin. The laminate according to claim 1 .

9. A printed circuit board having copper wiring, The surface roughness Ra of the copper wiring is 0.3 μm or less, There is no residue of the resist layer on the copper wiring A printed circuit board characterized by:

10. A method for manufacturing a printed circuit board using a resist layer, comprising: Step (A): A step of cleaning the surface of a copper layer having a surface roughness Ra of 0.3 μm or less with a chemical solution; Step (B): forming an intermolecular interaction layer directly on the washed copper layer; Step (C): forming a resist layer containing a photosensitive resin directly on the intermolecular interaction layer; Step (D): patterning the resist layer by exposure and development; Step (E): patterning the copper layer by etching; Step (F): peeling off the resist layer and the intermolecular interaction layer. A method for manufacturing a printed circuit board.

11. In the step (B), the total amount of Zn, Cr, Ni, and Sn present in the surface layer of the copper layer on the intermolecular interaction layer side is within the range of 0.001 to 1.000 at %. The method for manufacturing a printed circuit board according to claim 10.

12. The pH of the chemical solution used in the step (A) at 25°C is 2 or less. The method for manufacturing a printed circuit board according to claim 10.

13. The chemical solution used in the step (A) is an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid, and nitric acid. The method for manufacturing a printed circuit board according to claim 10.

Citation Information