Metal plate, manufacturing method of metal plate, mask, mask device, and manufacturing method of mask

By employing a metal plate with controlled reflectance ratios and angles, the formation of fringes in resist patterns is minimized, leading to improved dimensional accuracy of through holes and enhanced organic device manufacturing precision.

JP2024154363APending Publication Date: 2024-10-30DAI NIPPON PRINTING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024003530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-01-12
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

The occurrence of fringes in resist patterns during the manufacturing of masks leads to decreased precision in the dimensions of through holes, which affects the accuracy of organic devices such as organic EL display devices.

Method used

A metal plate for manufacturing masks is designed with specific reflectance ratios and angles to minimize the generation of fringes in resist patterns, ensuring high dimensional accuracy of through holes.

Benefits of technology

The solution effectively suppresses the formation of fringes, thereby improving the precision of through holes and enhancing the accuracy of organic device components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154363000001_ABST
    Figure 2024154363000001_ABST
Patent Text Reader

Abstract

To provide a metal plate for suppressing a generation of a fringe in a resist pattern, and a manufacturing method of the same.SOLUTION: A surface of a metal plate used for manufacturing a mask has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity. The first reflectivity is a reflectivity of first reflected light having a first emission angle, the third reflectivity is a reflectivity of the first reflected light having a third emission angle, and the first emission angle is an emission angle showing a maximum strength of the first reflected light. The third emission angle is an emission angle different from the first emission angle by a first deviation angle. The second reflectivity is a reflectivity of second reflected light having a second emission angle. The fourth reflectivity is a reflectivity of the second reflected light having a fourth emission angle. The second emission angle is an emission angle showing a maximum strength of the second reflected light. The fourth emission angle is an emission angle different from the second emission angle by a second deviation angle. A first ratio (a ratio of the third reflectivity to the first reflectivity), and a second ratio (a ratio of the fourth reflectivity to the second reflectivity) may be 0.40 or less each.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD Embodiments of the present disclosure relate to a metal plate, a method for manufacturing a metal plate, a mask, a mask device, and a method for manufacturing a mask. [Background technology]

[0002] Organic devices such as organic electroluminescence (EL) displays are attracting attention. A method for forming elements of organic devices is known in which materials constituting the elements are attached to a substrate by vapor deposition. For example, a substrate is first prepared on which a first electrode is formed in a pattern corresponding to the element. Next, an organic material is attached onto the first electrode through the through holes of a mask to form an organic layer on the first electrode. Next, a second electrode is formed on the organic layer.

[0003] A method for manufacturing a mask is known in which a metal plate is etched to form through holes. The manufacturing method includes, for example, a step of forming a first resist pattern on a first surface of the metal plate and a second resist pattern on a second surface of the metal plate, a first etching step of etching the first surface of the metal plate to form a plurality of first recesses on the first surface, a step of filling the first recesses with resin, and a second etching step of etching the second surface of the metal plate to form a plurality of second recesses on the second surface. The second recesses are connected to the first recesses to form through holes penetrating the metal plate.

[0004] If the dimensional accuracy of the resist pattern is low, the dimensional accuracy of the through hole will also be low. For example, if a fringe occurs in the resist pattern, the dimensional accuracy of the through hole will be low. A fringe is a part of the resist pattern that protrudes toward the center of the opening in the resist pattern. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-178765 A [Patent Document 2] International Publication No. 2019 / 098168 [Patent Document 3] International Publication No. 2017 / 014172 [Patent Document 4] International Publication No. 2017 / 013904 Summary of the Invention [Problem to be solved by the invention]

[0006] An embodiment of the present disclosure aims to suppress the occurrence of fringes in a resist pattern. [Means for solving the problem]

[0007] According to an embodiment of the present disclosure, a metal plate used to manufacture a mask may have a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction. The surface may have a first reflectance, a second reflectance, a third reflectance, and a fourth reflectance. The first reflectance is a reflectance of a first reflected light having a first exit angle. The third reflectance is a reflectance of the first reflected light having a third exit angle. The first reflected light is a first incident light that travels in the width direction in a plan view and enters the surface at a first specific incident angle, and is reflected by the surface. The first exit angle is an exit angle at which the first reflected light shows a maximum intensity. The third exit angle is an exit angle that differs from the first exit angle by a first deviation angle. The second reflectance is a reflectance of a second reflected light having a second exit angle. The fourth reflectance is a reflectance of the second reflected light having a fourth exit angle. The second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface. The second exit angle is an exit angle at which the second reflected light shows a maximum intensity. The fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle. The first specific incident angle and the second specific incident angle may be 20°. A first ratio that is a ratio of the third reflectance to the first reflectance may be 0.40 or less. A second ratio that is a ratio of the fourth reflectance to the second reflectance may be 0.40 or less. Effect of the Invention

[0008] According to an embodiment of the present disclosure, the occurrence of fringes in a resist pattern can be suppressed. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a plan view illustrating an example of an organic device. [Diagram 2] FIG. 2 is a plan view showing an example of an element of an organic device. [Diagram 3] FIG. 3 is a cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 2 is a plan view showing an example of an organic device group. [Diagram 5] FIG. 1 is a cross-sectional view showing an example of a deposition apparatus. [Figure 6] FIG. 2 is a plan view showing an example of a mask device. [Figure 7] FIG. 2 is a plan view showing an example of a mask. [Figure 8] FIG. 4 is a plan view showing an example of a through hole. [Figure 9] FIG. 11 is a rear view showing an example of a through hole. [Figure 10] FIG. 4 is a cross-sectional view showing an example of a through hole. [Figure 11] FIG. 1 is a diagram illustrating an example of a mask manufacturing apparatus. [Figure 12] 10A to 10C are cross-sectional views showing an example of a resist forming step. [Figure 13] FIG. 4 is a cross-sectional view showing an example of an exposure step. [Figure 14A] 1A to 1C are cross-sectional views showing an example of a patterning step. [Figure 14B] FIG. 11 is a plan view showing an example of a patterning step. [Figure 15] FIG. 4 is a cross-sectional view showing an example of a first etching step. [Figure 16] FIG. 4 is a cross-sectional view showing an example of a filling step. [Figure 17] FIG. 11 is a cross-sectional view showing an example of a second etching step. [Figure 18] FIG. 11 is a cross-sectional view showing an example of a removing step. [Figure 19] FIG. 4 is a cross-sectional view showing an example of a separation step. [Figure 20] FIG. 2 is a plan view showing an example of a surface of a metal plate. [Figure 21] 4 is a cross-sectional view showing an example of light reflection occurring on the surface of a metal plate. FIG. [Figure 22] 10 is a cross-sectional view showing an example of light being reflected on the surface of a metal plate in an exposure process. FIG. [Figure 23] FIG. 2 is a cross-sectional view showing an example of a resist pattern. [Figure 24] FIG. 1 is a plan view showing an example of a resist pattern including a fringe. [Diagram 25] FIG. 4 is a plan view showing an example of a through hole. [Figure 26] FIG. 2 shows a sample being removed from a metal plate. [Figure 27] FIG. 11 is a perspective view showing a process for measuring the reflectance of a sample. [Figure 28] 5A to 5C are cross-sectional views showing steps of measuring a first reflectance and a third reflectance of a sample. [Figure 29] 6A and 6B are diagrams illustrating an example of a measurement result of the intensity of a first reflected light. [Diagram 30] FIG. 11 is a cross-sectional view showing a step of measuring a second reflectance and a fourth reflectance of a sample. [Diagram 31] 11 is a diagram showing an example of a measurement result of the intensity of a second reflected light. FIG. [Diagram 32] FIG. 2 is a plan view showing measurement positions of a sample. [Diagram 33] FIG. 13 is a diagram showing a verification sample taken out from a metal plate. [Diagram 34] FIG. 11 is a plan view showing an example of a method for extracting a metal plate sample from a mask. [Diagram 35] FIG. 2 is a diagram showing an example of a rolling process. [Diagram 36] FIG. 1 is a diagram illustrating an example of an annealing step. [Figure 37] FIG. 1 shows the measurement results of the intensity of light used in the examples. [Figure 38A] 1 is a table showing the measurement results of the first reflectance and the third reflectance of the metal plates of Examples 1 to 11, Comparative Examples 1 to 6, and Example 12 when the incident angle was 20°. [Figure 38B] 1 is a table showing the measurement results of the second reflectance and the fourth reflectance of the metal plates of Examples 1 to 11, Comparative Examples 1 to 6, and Example 12 when the incident angle was 20°. [Figure 38C] 1 is a table showing the evaluation results of metal plates of Examples 1 to 11, Comparative Examples 1 to 6, and Example 12 in the case of an incident angle of 20°. [Figure 39] FIG. 13 is a diagram showing the measurement results of the metal plate of Example 1 in the case of an incident angle of 20°. [Diagram 40] FIG. 13 is a diagram showing the measurement results of the metal plate of Example 4 in the case of an incident angle of 20°. [Diagram 41] FIG. 13 is a diagram showing the measurement results of the metal plate of Example 6 at an incident angle of 20°. [Diagram 42] FIG. 13 is a diagram showing the measurement results of the metal plate of Example 8 at an incident angle of 20°. [Diagram 43] FIG. 13 is a diagram showing the measurement results of the metal plate of Comparative Example 1 when the incident angle is 20°. [Diagram 44] FIG. 13 is a diagram showing the measurement results of the metal plate of Comparative Example 4 when the incident angle is 20°. [Diagram 45] FIG. 2 is a diagram showing an image of the surface of a metal plate in Comparative Example 1. [Figure 46A] 1 is a table showing the measurement results of the first reflectance and the third reflectance of the verification samples of Examples 1, 4, and 8 in the case of an incident angle of 20°. [Figure 46B] 1 is a table showing the measurement results of the first reflectance and the third reflectance of the verification samples of Examples 1, 4, and 8 in the case of an incident angle of 20°. [Figure 46C] 1 is a table showing the evaluation results of verification samples of Examples 1, 4, and 8 in the case of an incident angle of 20°. [Figure 47A] 1 is a cross-sectional view showing an example of light reflection occurring on the surface of a metal plate when the incident angle is 20°. [Figure 47B]1 is a cross-sectional view showing an example of light reflection occurring on the surface of a metal plate when the incident angle is 45°. [Figure 48A] 1 is a table showing the measurement results of the first reflectance and the third reflectance of the metal plates of Examples 1 to 12 and Comparative Examples 1 to 6 in the case of an incident angle of 45°. [Figure 48B] 1 is a table showing the measurement results of the second reflectance and the fourth reflectance of the metal plates of Examples 1 to 12 and Comparative Examples 1 to 6 in the case of an incident angle of 45°. [Figure 48C] 1 is a table showing the evaluation results of metal plates of Examples 1 to 12 and Comparative Examples 1 to 6 in the case of an incident angle of 45°. [Figure 49A] 1 is a table showing the regular reflectance of metal plates in Examples 1 to 12 and Comparative Examples 1 to 6. [Figure 49B] 1 is a graph showing the relationship between specular reflectance at an incident angle of 20° and specular reflectance at an incident angle of 45°. [Figure 49C] 1 is a graph showing the relationship between specular reflectance at an incident angle of 20° and specular reflectance at an incident angle of 45°. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In this specification and drawings, unless otherwise specified, terms that refer to materials underlying a certain configuration, such as "plate," "sheet," and "film," are not to be distinguished from one another solely on the basis of differences in name.

[0011] In this specification and drawings, unless otherwise specified, terms that specify shapes, geometric conditions, and the extent thereof, such as "parallel" and "orthogonal," and values ​​of lengths and angles, are not bound by strict meanings, but are interpreted to include a range within which similar functions may be expected.

[0012] In this specification and drawings, unless otherwise specified, when a certain configuration such as a certain member or a certain region is described as being "on" or "under", "upper" or "lower" or "above" or "below" another configuration such as another member or another region, this includes the case where the certain configuration is in direct contact with the other configuration. It also includes the case where another configuration is included between a certain configuration and the other configuration, that is, where the configuration is indirectly in contact. Furthermore, unless otherwise specified, the words "on", "upper side", "upper", or "lower", "lower side", and "lower" may be used in the up-down direction.

[0013] In this specification and drawings, unless otherwise specified, the same or similar parts or parts having similar functions are denoted by the same or similar symbols, and repeated explanations may be omitted. In addition, the dimensional ratios of the drawings may differ from the actual ratios for the convenience of explanation, and some components may be omitted from the drawings.

[0014] In this specification and the drawings, unless otherwise specified, one embodiment of this specification may be combined with other embodiments to the extent that no contradiction occurs. In addition, other embodiments may be combined with each other to the extent that no contradiction occurs.

[0015] In the present specification and drawings, unless otherwise specified, when two or more steps or processes are disclosed in a method such as a manufacturing method, other steps or processes that are not disclosed may be performed between the steps or processes disclosed. In addition, the order of the steps or processes disclosed is arbitrary to the extent that no contradiction occurs.

[0016] In this specification and drawings, unless otherwise specified, a numerical range expressed by the symbol "~" includes the numerical values ​​before and after the symbol "~". For example, the numerical range defined by the expression "34 to 38% by mass" is the same as the numerical range defined by the expression "34% by mass or more and 38% by mass or less".

[0017] In one embodiment of the present specification, an example will be described in which a mask is used to form an organic layer or an electrode on a substrate when manufacturing an organic EL display device. However, the use of the mask is not particularly limited, and the present embodiment can be applied to masks used for various purposes. For example, the mask of the present embodiment may be used to form electrodes of a device for displaying or projecting images or videos for expressing virtual reality, so-called VR, or augmented reality, so-called AR. The mask of the present embodiment may also be used to form electrodes of a display device other than an organic EL display device, such as an electrode of a liquid crystal display device. The mask of the present embodiment may also be used to form electrodes of an organic device other than a display device, such as an electrode of a pressure sensor.

[0018] A first aspect of the present disclosure is a metal plate used to manufacture a mask, comprising: A surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle; the first reflected light is a first incident light that travels in the width direction in a plan view, is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, The first specific incident angle and the second specific incident angle are 20°; a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; The metal plate has a second ratio, which is a ratio of the fourth reflectance to the second reflectance, of 0.40 or less.

[0019] A second aspect of the present disclosure is the metal plate according to the first aspect described above, wherein the first deviation angle and the second deviation angle may be 2.5°.

[0020] A third aspect of the present disclosure is such that, in the metal plate according to the first or second aspect described above, the absolute value of the difference between the first specific incident angle and the first exit angle may be 0.30° or less, and the absolute value of the difference between the second specific incident angle and the second exit angle may be 0.30° or less.

[0021] A fourth aspect of the present disclosure is a metal plate according to any one of the first to third aspects described above, wherein the surface of the metal plate may include a plurality of rolling streaks extending in the longitudinal direction and a plurality of oil pits.

[0022] A fifth aspect of the present disclosure is the metal plate according to any one of the first to fourth aspects described above, wherein the metal plate may have a thickness of 80 μm or less.

[0023] A sixth aspect of the present disclosure is the metal plate according to any one of the first to fifth aspects described above, wherein the metal plate may include an iron alloy containing 34 mass % or more and 38 mass % or less of nickel.

[0024] A seventh aspect of the present disclosure may be such that, in the metal plate according to any one of the first to sixth aspects described above, an absolute value of a difference between the first ratio and the second ratio is 0.20 or less.

[0025] An eighth aspect of the present disclosure is the metal plate according to any one of the first to seventh aspects described above, wherein the first ratio and the second ratio may be 0.30 or less.

[0026] A ninth aspect of the present disclosure is the metal plate according to the eighth aspect described above, wherein the second ratio may be 0.20 or less.

[0027] A tenth aspect of the present disclosure is the metal plate according to any one of the first to ninth aspects described above, wherein the metal plate may have a regular reflectance of 35.0% or less, The regular reflectance is an average value of the first reflectance and the second reflectance.

[0028] An eleventh aspect of the present disclosure is a method for inspecting a metal plate used for manufacturing a mask, comprising: The metal plate has a surface having a longitudinal direction and a width direction perpendicular to the longitudinal direction, The inspection method includes: measuring a first reflectance, a second reflectance, a third reflectance, and a fourth reflectance of the metal plate; a first determination step of determining whether a first ratio, which is a ratio of the third reflectance to the first reflectance, is equal to or smaller than a first threshold value; a second determination step of determining whether a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is equal to or smaller than a second threshold value; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle; the first reflected light is a first incident light that travels in the width direction in a plan view, is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; The fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle.

[0029] A twelfth aspect of the present disclosure is a method for manufacturing a metal plate used to manufacture a mask, comprising the steps of: A rolling step of rolling the metal plate to reduce the thickness of the metal plate, The rolled metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle; the first reflected light is a first incident light that travels in the width direction in a plan view, is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; A second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

[0030] A thirteenth aspect of the present disclosure is a mask, comprising: A metal plate; A plurality of through holes penetrating the metal plate, The metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle; the first reflected light is a first incident light that travels in the width direction in a plan view, is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, The first specific incident angle and the second specific incident angle are 20°; a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; The mask has a second ratio, which is a ratio of the fourth reflectance to the second reflectance, of 0.40 or less.

[0031] A fourteenth aspect of the present disclosure is the mask according to the thirteenth aspect described above, wherein the metal plate may include a first surface and a second surface located opposite to the first surface, and the through hole may include a plurality of first recesses located on the first surface, a plurality of second recesses located on the second surface, and a connection portion connecting the first recesses and the second recesses, and in a plan view, a dimension of the second recesses is larger than a dimension of the first recesses, The first surface may be the surface having the first reflectance, the second reflectance, the third reflectance, and the fourth reflectance.

[0032] A fifteenth aspect of the present disclosure is a mask according to the fourteenth aspect described above, wherein the through hole may have a first through dimension in the width direction and a second through dimension in the longitudinal direction, and the ratio of the first through dimension to the second through dimension may be 0.98 or greater.

[0033] A sixteenth aspect of the present disclosure is a mask device, comprising: A mask according to any one of the thirteenth to fifteenth aspects described above; A mask support that supports the mask.

[0034] A seventeenth aspect of the present disclosure is a method for manufacturing a mask, comprising: Providing a metal plate; A processing step of forming a plurality of through holes in the metal plate, The metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle; the first reflected light is a first incident light that travels in the width direction in a plan view, is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view, is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; A second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

[0035] An eighteenth aspect of the present disclosure is a method for producing a mask according to the seventeenth aspect, wherein the processing step comprises: a resist forming step of forming a resist layer on the surface of the metal plate; an exposure step of exposing the resist layer to light; a developing step of developing the exposed resist layer to form a resist pattern; and an etching step of etching the metal plate.

[0036] A nineteenth aspect of the present disclosure is the method for producing a mask according to the eighteenth aspect, wherein the resist pattern includes an opening and a wall surface facing the opening, a fringe of the wall surface may have a width of 1.00 μm or less in a plan view, and the fringe may protrude toward the center of the opening at a corner, the corner being a portion where the wall surface is connected to the surface of the resist pattern facing the metal plate.

[0037] An embodiment of the present disclosure will be described in detail with reference to the drawings. Note that the embodiment described below is an example of the present disclosure, and the present disclosure is not to be interpreted as being limited to only these embodiments.

[0038] First, an organic device 100 will be described. The organic device 100 includes an organic layer or an electrode formed by using a mask. Fig. 1 is a plan view showing an example of the organic device 100 when viewed along the normal direction of the substrate of the organic device 100. In the following description, the view along the normal direction of the surface of the underlying material such as the substrate is also referred to as a planar view.

[0039] The organic device 100 includes a substrate and a plurality of elements 115 arranged along an in-plane direction of the substrate. The elements 115 are, for example, pixels. Fig. 2 is an enlarged plan view of the organic device 100. The elements 115 may be arranged along two different directions. Fig. 3 is a cross-sectional view taken along line III-III in Fig. 2.

[0040] The organic device 100 may comprise a substrate 110, a plurality of first electrodes 120, a plurality of organic layers 130, and a second electrode 140. The substrate 110 includes a first side 111 and a second side 112. The second side 112 is located opposite the first side 111.

[0041] The plurality of first electrodes 120 may be located on the first surface 111. The plurality of organic layers 130 may be located on the first electrodes 120. The second electrode 140 may be located on the organic layer 130. The second electrode 140 may extend so as to overlap the plurality of first electrodes 120 in a planar view. The element 115 is configured by a laminated structure including the first electrode 120, the organic layer 130, and the second electrode 140. The element 115 can realize some function by applying a voltage between the first electrode 120 and the second electrode 140, or by causing a current to flow between the first electrode 120 and the second electrode 140.

[0042] The organic device 100 may be an active matrix type. For example, although not shown, the organic device 100 may include a switch electrically connected to each of the multiple elements 115. The switch is, for example, a transistor. The switch can control the ON / OFF of a voltage applied to the element 115 or a current flowing through the element 115.

[0043] 2 and 3, the organic layers 130 may include a plurality of first organic layers 130A, a plurality of second organic layers 130B, and a plurality of third organic layers 130C. The first organic layer 130A, the second organic layer 130B, and the third organic layer 130C are, for example, a red light-emitting layer, a blue light-emitting layer, and a green light-emitting layer. When describing a configuration common to the first organic layer 130A, the second organic layer 130B, and the third organic layer 130C, the term and symbol "organic layer 130" are used.

[0044] 2 and 3, the multiple first electrodes 120 may include multiple 1A electrodes 120A, multiple 1B electrodes 120B, and multiple 1C electrodes 120C. The 1A electrode 120A overlaps the first organic layer 130A in a planar view. The 1B electrode 120B overlaps the second organic layer 130B in a planar view. The 1C electrode 120C overlaps the third organic layer 130C in a planar view. When describing a configuration common to the 1A electrode 120A, the 1B electrode 120B, and the 1C electrode 120C, the term and symbol "first electrode 120" are used.

[0045] One element 115 may include at least one first sub-element 115A, at least one second sub-element 115B, and at least one third sub-element 115C. The first sub-element 115A includes a 1A electrode 120A, a first organic layer 130A, and a second electrode 140. The second sub-element 115B includes a 1B electrode 120B, a second organic layer 130B, and a second electrode 140. The third sub-element 115C includes a 1C electrode 120C, a third organic layer 130C, and a second electrode 140. In the example shown in FIG. 2, one element 115 includes one first sub-element 115A, one second sub-element 115B, and two third sub-elements 115C.

[0046] The element formed by using the mask may be the organic layer 130 or the second electrode 140. The element formed by using the mask is also called a deposited layer.

[0047] The organic device 100 may include an insulating layer 160 located between two adjacent first electrodes 120 in a plan view. The insulating layer 160 may include, for example, polyimide. The insulating layer 160 may overlap an edge of the first electrode 120 in a plan view.

[0048] The components of the organic device 100 will now be described in detail.

[0049] The substrate 110 may be a plate-like member having insulating properties. The substrate 110 is preferably transparent to transmit light. The material of the substrate 110 may be, for example, a rigid material with no flexibility, such as quartz glass, Pyrex (registered trademark) glass, or a synthetic quartz plate, or a flexible material with flexibility, such as a resin film, an optical resin plate, or thin glass. The substrate 110 may be a laminate having a barrier layer on one or both sides of a resin film.

[0050] The element 115 is configured to realize some function by applying a voltage between the first electrode 120 and the second electrode 140, or by causing a current to flow between the first electrode 120 and the second electrode 140. For example, when the element 115 is a pixel of an organic EL display device, the element 115 emits light that constitutes an image.

[0051] The first electrode 120 includes a material having electrical conductivity. For example, the first electrode 120 includes a metal, a metal oxide having electrical conductivity, or other inorganic material having electrical conductivity. The first electrode 120 may include a metal oxide having transparency and electrical conductivity, such as indium tin oxide (ITO) or indium zinc oxide (IZO).

[0052] The organic layer 130 includes an organic material. When a current is applied to the organic layer 130, the organic layer 130 can perform some function. Applying a current means that a voltage is applied to the organic layer 130 or that a current flows through the organic layer 130. As the organic layer 130, a light-emitting layer that emits light when a current is applied can be used. The organic layer 130 may include an organic semiconductor material. The characteristics of the organic layer 130, such as the transmittance and refractive index, may be appropriately adjusted.

[0053] When a voltage is applied between the first electrode 120 and the second electrode 140, the organic layer 130 located therebetween is driven. When the organic layer 130 is an emitting layer, light is emitted from the organic layer 130 and extracted to the outside from the second electrode 140 side or the first electrode 120 side.

[0054] The organic layer 130 may further include a hole injection layer, a hole transport layer, an electron transport layer, an electron injection layer, a charge generation layer, and the like.

[0055] The second electrode 140 includes a material having electrical conductivity, such as a metal. The second electrode 140 is formed on the organic layer 130 by a deposition method using a mask. The second electrode 140 may be made of platinum, gold, silver, copper, iron, tin, chromium, aluminum, indium, lithium, sodium, potassium, calcium, magnesium, indium tin oxide (ITO), indium zinc oxide (IZO), carbon, or the like. These materials may be used alone or in combination of two or more. When two or more types are used, layers made of each material may be stacked. An alloy containing two or more types of materials may also be used. For example, magnesium alloys such as MgAg, and aluminum alloys such as AlLi, AlCa, and AlMg may be used. MgAg is also called magnesium silver. Magnesium silver is preferably used as the material for the second electrode 140. An alloy of alkali metals and alkaline earth metals may also be used. For example, lithium fluoride, sodium fluoride, potassium fluoride, or the like may be used.

[0056] The second electrode 140 may be a common electrode. For example, the second electrode 140 of one element 115 may be electrically connected to the second electrode 140 of the other element 115.

[0057] 2 and 3, the second electrode 140 may extend so as to overlap a plurality of the first electrodes 120. For example, the second electrode 140 may extend over the entire display area of ​​the organic device 100 in a plan view.

[0058] In the manufacturing method of the organic device 100, an organic device group 102 as shown in FIG. 4 may be manufactured. The organic device group 102 includes two or more organic devices 100. For example, the organic device group 102 may include organic devices 100 arranged in a first direction D1 and a second direction D2. The second direction D2 is a direction perpendicular to the first direction D1. The two or more organic devices 100 may have a common substrate 110. For example, the organic device group 102 may be located on the substrate 110 and include layers such as a first electrode 120, an organic layer 130, and a second electrode 140 constituting two or more organic devices 100. The organic device 100 is obtained by dividing the organic device group 102.

[0059] The first direction D1 may be the longitudinal direction of a mask, which will be described later.

[0060] Next, a method for forming a deposition layer such as the organic layer 130 by a deposition method will be described.

[0061] The deposition method performed using the mask 50 is physical deposition. Physical deposition is, for example, vacuum deposition, ion plating, sputtering, etc. When the mask 50 is used in physical deposition, a deposition layer is formed in the area of ​​the object that overlaps with the through-holes of the mask 50 in a plan view. The object is, for example, a substrate.

[0062] Fig. 5 is a diagram showing a deposition apparatus 10. The deposition apparatus 10 performs a deposition process for depositing a deposition material on a substrate 110. In the example shown in Fig. 5, the deposition apparatus 10 performs vacuum deposition.

[0063] As shown in Fig. 5, the deposition apparatus 10 may include therein a deposition source 6, a heater 8, and a mask device 15. The deposition apparatus 10 may further include an exhaust means for creating a vacuum atmosphere inside the deposition apparatus 10. The deposition source 6 is, for example, a crucible, and contains a deposition material 7 such as an organic material or a metal material. The heater 8 heats the deposition source 6 to evaporate the deposition material 7 under a vacuum atmosphere. The mask device 15 is disposed to face the crucible 6.

[0064] 5, the mask device 15 includes at least one mask 50. The mask device 15 may include a mask support 40 that supports the mask 50. The mask support 40 may include a frame 41 that includes an opening 43. The mask 50 may be fixed to the frame 41 so as to cross the opening 43 in a plan view. The frame 41 may support the mask 50 in a state where it is pulled in the plane direction so as to suppress bending of the mask 50.

[0065] 5, the mask device 15 is disposed in the deposition device 10 such that the mask 50 faces the first surface 111 of the substrate 110. The mask 50 includes a plurality of through holes 56 that allow the deposition material 7 flying from the deposition source 6 to pass through. In the following description, the surface of the mask 50 facing the substrate 110 is referred to as a first surface 551. The surface of the mask 50 positioned opposite the first surface 551 is referred to as a second surface 552.

[0066] As shown in FIG. 5, the deposition apparatus 10 may include a substrate holder 2 that holds a substrate 110. The substrate holder 2 may be movable in a thickness direction of the substrate 110. The substrate holder 2 may be movable in a surface direction of the substrate 110. The substrate holder 2 may be configured to control the inclination of the substrate 110. For example, the substrate holder 2 may include a plurality of chucks attached to the outer edge of the substrate 110. Each chuck may be independently movable in the thickness direction or surface direction of the substrate 110.

[0067] By moving at least one of the substrate holder 2 and the mask holder 3, the position of the mask 50 relative to the substrate 110 can be adjusted.

[0068] 5, the deposition apparatus 10 may include a cooling plate 4 disposed on the second surface 112 side of the substrate 110. The cooling plate 4 may have a flow path for circulating a coolant inside the cooling plate 4. The cooling plate 4 can suppress an increase in temperature of the substrate 110 during the deposition process.

[0069] As shown in FIG. 5, the deposition apparatus 10 may include a magnet 5 disposed on the second surface 112 side of the substrate 110. The magnet 5 may be disposed on the surface of the cooling plate 4 far from the substrate 110. The magnet 5 can attract the mask 50 to the substrate 110 side by magnetic force. This can reduce or eliminate the gap between the mask 50 and the substrate 110. This can suppress the occurrence of a shadow in the deposition process. The shadow is a phenomenon in which the deposition material 7 enters the gap between the mask 50 and the substrate 110, causing the shape of the deposition layer to become uneven. The shape of the deposition layer refers to the thickness of the deposition layer, the dimensions of the deposition layer in a plan view, etc. The mask 50 may be attracted to the substrate 110 side by an electrostatic chuck that utilizes electrostatic force.

[0070] 6 is a plan view showing the mask device 15 as viewed from the first surface 551 side. The mask device 15 may include a mask support 40 including a frame 41, and a mask 50 fixed to the frame 41. The mask device 15 may include two or more masks 50 arranged in the second direction D2. The frame 41 supports the mask 50 with tension applied to the mask 50 to prevent the mask 50 from bending.

[0071] The frame 41 may include a pair of first sides 411 extending in a first direction D1, a pair of second sides 412 extending in a second direction D2, and an opening 43. The second sides 412 may be longer than the first sides 411. The pair of first sides 411 and the pair of second sides 412 are in contact with the opening 43 in a plan view.

[0072] The mask 50 may include a first side edge 501 and a second side edge 502 extending in a first direction D1, and a first end 503 and a second end 504. The first end 503 and the second end 504 are ends of the mask 50 in the first direction D1.

[0073] In a plan view, the mask 50 includes a first end 51a, a second end 51b, and an intermediate portion 52. The first end 51a and the second end 51b face each other in a first direction D1. The intermediate portion 52 is located between the first end 51a and the second end 51b. The intermediate portion 52 includes a group of through holes 53.

[0074] The term "planar view" means that the object is viewed along the thickness direction of the mask 50.

[0075] The mask 50 is fixed to the second side 412. Specifically, the first end 51a is fixed to the first second side 412, and the second end 51b is fixed to the second second side 412. The first end 51a and the second end 51b may be fixed to the first second side 412 and the second second side 412 by welding. The middle portion 52 overlaps the opening 43 of the frame 41 in a plan view.

[0076] 7 is a plan view showing an example of the mask 50. The through-hole group 53 of the intermediate portion 52 includes a plurality of through-holes 56 arranged regularly in a plan view. The through-holes 56 may be arranged periodically in two directions. For example, the through-holes 56 may be arranged periodically in the first direction D1 and the second direction D2.

[0077] One through-hole group 53 corresponds to one organic device 100. For example, a plurality of first organic layers 130A included in one organic device 100 are formed of a deposition material that has passed through a plurality of through-holes 56 of one through-hole group 53. The mask 50 includes at least one through-hole group 53. The mask 50 may include two or more through-hole groups 53 aligned in the first direction D1.

[0078] The through-hole 56 will be described in detail. Fig. 8 is a plan view showing the through-hole 56 in the first surface 551. Fig. 9 is a bottom view showing the through-hole 56 in the second surface 552. Fig. 10 is a cross-sectional view taken along the line XX in Figs. 8 and 9.

[0079] The through hole 56 includes a first recess 56a, a second recess 56b, and a connection portion 563 that connects the first recess 56a and the second recess 56b. The first recess 56a is located on the first surface 551 and is a recess that is recessed toward the second surface 552. The second recess 56b is located on the second surface 552 and is a recess that is recessed toward the first surface 551. The first recess 56a and the second recess 56b are connected to each other to form the through hole 56 that penetrates the metal plate 55. The first recess 56a is formed by etching the first surface 551. The second recess 56b is formed by etching the second surface 552.

[0080] The through holes 56 may be arranged regularly in the first arrangement direction E1 and the second arrangement direction E2. The second arrangement direction E2 may be perpendicular to the first arrangement direction E1.

[0081] The first recess 56a includes a first contour 561 on the first surface 551. The first contour 561 has a dimension r1 in a plan view. The dimension r1 is defined in a direction in which the dimension of the first contour 561 is maximized. The second recess 56b includes a second contour 562 on the second surface 552. The second contour 562 has a dimension r2 in a plan view. The dimension r2 is defined in a direction in which the dimension of the second contour 562 is maximized. In the example shown in FIGS. 8 and 9, the dimensions r1 and r2 are defined in a third arrangement direction E3 that forms an angle of 45° with the first arrangement direction E1 and the second arrangement direction E2.

[0082] Two adjacent second recesses 56b may be connected or not connected. For example, two adjacent second recesses 56b in the first arrangement direction E1 or the second arrangement direction E2 may be connected. For example, two adjacent second recesses 56b in the third arrangement direction E3 or the fourth arrangement direction E4 may not be connected. The fourth arrangement direction E4 may be perpendicular to the third arrangement direction E3.

[0083] The dimension r1 may be, for example, 10 μm or more, 20 μm or more, or 30 μm or more. The dimension r1 may be, for example, 40 μm or less, 50 μm or less, or 100 μm or less. The range of the dimension r1 may be determined by a first group consisting of 10 μm, 20 μm, and 30 μm, and / or a second group consisting of 40 μm, 50 μm, and 100 μm. The range of the dimension r1 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the dimension r1 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the dimension r1 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The dimension r1 may be, for example, 10 μm or more and 100 μm or less, 10 μm or more and 50 μm or less, 10 μm or more and 40 μm or less, 10 μm or more and 30 μm or less, 10 μm or more and 20 μm or less, 20 μm or more and 100 μm or less, 20 μm or more and 50 μm or less, 20 μm or more and 40 μm or less, 20 μm or more and 30 μm or less, 30 μm or more and 100 μm or less, 30 μm or more and 50 μm or less, 30 μm or more and 40 μm or less, 40 μm or more and 100 μm or less, 40 μm or more and 50 μm or less, or 50 μm or more and 100 μm or less.

[0084] As shown in Figs. 8 to 10, in plan view, the dimensions of the second recess 56b may be larger than the dimensions of the first recess 56a. For example, the dimension r2 may be larger than the dimension r1. The ratio of the dimension r1 to the dimension r1, r2 / r1, may be, for example, 1.05 or more, 1.10 or more, or 1.15 or more. For example, r2 / r1 may be 1.30 or less, 1.50 or less, 2.00 or less, or 3.00 or less. The range of r2 / r1 may be determined by a first group consisting of 1.05, 1.10, and 1.15, and / or a second group consisting of 1.30, 1.50, 2.00, and 3.00. The range of r2 / r1 may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of r2 / r1 may be determined by a combination of any two of the values ​​included in the first group described above. The range of r2 / r1 may be determined by a combination of any two of the values ​​included in the second group described above. r2 / r1 may be, for example, 1.05 or more and 3.00 or less, 1.05 or more and 2.00 or less, 1.05 or more and 1.50 or less, 1.05 or more and 1.30 or less, 1.05 or more and 1.15 or less, 1.05 or more and 1.10 or less, 1.10 or more and 3.00 or less, 1.10 or more and 2.00 or less, 1.10 or more and 1.50 or less, 1.10 or more and 1.30 or less, or 1.10 or more and 1.20 or less. It may be 0 or more and 1.15 or less, 1.15 or more and 3.00 or less, 1.15 or more and 2.00 or less, 1.15 or more and 1.50 or less, 1.15 or more and 1.30 or less, 1.30 or more and 3.00 or less, 1.30 or more and 2.00 or less, 1.30 or more and 1.50 or less, 1.50 or more and 3.00 or less, 1.50 or more and 2.00 or less, or 2.00 or more and 3.00 or less.

[0085] 10, the dimension of the first recess 56a in the planar direction of the first surface 551 may decrease from the first surface 551 toward the connecting portion 563. The dimension of the second recess 56b in the planar direction of the first surface 551 may decrease from the second surface 552 toward the connecting portion 563.

[0086] The connecting portion 563 may have a continuous contour around the circumference in a plan view. The connecting portion 563 may define a through portion 56c where the opening area of ​​the through hole 56 is the smallest in a plan view of the mask 50.

[0087] The dimension r of the through portion 56c in plan view may be, for example, 10 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more. The dimension r may be, for example, 40 μm or less, 45 μm or less, 50 μm or less, or 60 μm or less. The range of the dimension r may be determined by a first group consisting of 10 μm, 15 μm, 20 μm, and 25 μm, and / or a second group consisting of 40 μm, 45 μm, 50 μm, and 60 μm. The range of the dimension r may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the dimension r may be determined by a combination of any two of the values ​​included in the first group described above. The range of the dimension r may be determined by a combination of any two of the values ​​included in the second group described above. The dimension r may be, for example, 10 μm or more and 60 μm or less, 10 μm or more and 50 μm or less, 10 μm or more and 45 μm or less, 10 μm or more and 40 μm or less, 10 μm or more and 25 μm or less, 10 μm or more and 20 μm or less, 10 μm or more and 15 μm or more and 15 μm or more and 60 μm or less, 15 μm or more and 50 μm or less, 15 μm or more and 45 μm or less, 15 μm or more and 40 μm or less, 15 μm or more and 25 μm or less, 15 μm or more and 20 μm or more and 60 μm or less. or more, 20 μm or more and 50 μm or less, 20 μm or more and 45 μm or less, 20 μm or more and 40 μm or less, 20 μm or more and 25 μm or less, 25 μm or more and 60 μm or less, 25 μm or more and 50 μm or less, 25 μm or more and 45 μm or less, 25 μm or more and 40 μm or less, 40 μm or more and 60 μm or less, 40 μm or more and 50 μm or less, 40 μm or more and 45 μm or less, 45 μm or more and 60 μm or less, 45 μm or more and 50 μm or less, 50 μm or more and 60 μm or less.

[0088] Dimension r1 is calculated by measuring the shape of through-hole 56 from the side of first surface 551. Dimension r2 is calculated by measuring the shape of through-hole 56 from the side of second surface 552. AMIC-2500 manufactured by Shinto S Precision Co., Ltd. is used as the measuring device.

[0089] The dimension r can be determined by the light transmitted through the through hole 56. For example, parallel light is incident on one of the first surface 551 or the second surface 552 of the mask 50 along the normal direction of the mask 50, transmitted through the through hole 56, and emitted from the other of the first surface 551 or the second surface 552. The dimension of the area occupied by the emitted light in the surface direction of the mask 50 is adopted as the dimension r of the through portion 56c. The dimension of the through portion 56c is also referred to as the penetration dimension.

[0090] The dimensions r1, r2, and r are calculated by averaging the measurement results for the 100 through holes 56. The 100 through holes 56 are extracted from the through hole group 53 that is closest to the center point of the mask 50 in the first direction D1. The 100 through holes 56 are a collection of 10 rows x 10 rows of through holes 56 located at the center of the through hole group 53 in a plan view. The dimensions of the through holes 56, the first recesses 56a, or the second recesses 56b, which will be described later, are also calculated by averaging the measurement results for the 100 through holes 56.

[0091] The materials of the metal plate 55 and the frame 41 will be described. An iron alloy containing nickel can be used as the main material of the mask 50 and the frame 41. This can reduce the difference between the thermal expansion coefficient of the mask 50 and the frame 41 and the thermal expansion coefficient of the substrate 110 containing glass. This can prevent the dimensional accuracy and positional accuracy of the deposition layer formed on the substrate 110 from decreasing due to the thermal expansion of the mask 50, the frame 41, the substrate 110, etc.

[0092] The nickel content in the iron alloy may be, for example, 28% by mass or more, 30% by mass or more, or 34% by mass or more. The nickel content in the iron alloy may be, for example, 38% by mass or less, 44% by mass or less, or 54% by mass or less. The range of the nickel content in the iron alloy may be determined by a first group consisting of 28%, 30% by mass and 34% by mass, and / or a second group consisting of 38%, 44% by mass and 54% by mass. The range of the nickel content in the iron alloy may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the nickel content in the iron alloy may be determined by a combination of any two of the values ​​included in the first group described above. The range of the nickel content in the iron alloy may be determined by a combination of any two of the values ​​included in the second group described above. The nickel content in the iron alloy may be, for example, 28% by mass or more and 54% by mass or less, 28% by mass or more and 44% by mass or less, 28% by mass or more and 38% by mass or less, 28% by mass or more and 34% by mass or less, 28% by mass or more and 30% by mass or less, 30% by mass or more and 54% by mass or less, 30% by mass or more and 44% by mass or less, 30% by mass or more and 38% by mass or less, 30% by mass or more and 34% by mass or less, 34% by mass or more and 54% by mass or less, 34% by mass or more and 44% by mass or less, 34% by mass or more and 38% by mass or less, 38% by mass or more and 54% by mass or less, 38% by mass or more and 44% by mass or less, or 44% by mass or more and 54% by mass or less.

[0093] The iron alloy may further contain cobalt in addition to nickel. For example, an iron alloy having a nickel and cobalt content of 28% by mass or more and 54% by mass or less in total and a cobalt content of 0% by mass or more and 6% by mass or less may be used as the material for the metal plate 55 of the mask 50.

[0094] The total content of nickel and cobalt in the metal plate 55 may be 28% by mass or more and 38% by mass or less. In this case, specific examples of the iron alloy containing nickel or nickel and cobalt include Invar, Super Invar, and Ultra Invar. Invar is an iron alloy containing 34% by mass or more and 38% by mass or less of nickel, the balance being iron and unavoidable impurities. Super Invar is an iron alloy containing 30% by mass or more and 34% by mass or less of nickel, cobalt, and the balance being iron and unavoidable impurities. Ultra Invar is an iron alloy containing 28% by mass or more and 34% by mass or less of nickel, 2% by mass or more and 7% by mass or less of cobalt, 0.1% by mass or more and 1.0% by mass or less of manganese, 0.10% by mass or less of silicon, 0.01% by mass or less of carbon, and the balance being iron and unavoidable impurities.

[0095] The mask 50 containing the iron alloy described above may be manufactured by a plating method.

[0096] If the temperatures of the mask 50, the frame 41, and the substrate 110 do not reach high temperatures during the deposition process, there is no particular need to set the thermal expansion coefficients of the mask 50 and the frame 41 to values ​​equivalent to that of the substrate 110. In this case, materials other than the above-mentioned iron alloys may be used as materials constituting the metal plate 55. For example, iron alloys other than the above-mentioned iron alloys containing nickel, such as iron alloys containing chromium, may be used. As the iron alloy containing chromium, for example, an iron alloy so-called stainless steel may be used. In addition, alloys other than iron alloys, such as nickel and nickel-cobalt alloys, may be used.

[0097] The thickness T of the mask 50 may be, for example, 8 μm or more, 10 μm or more, 15 μm or more, or 20 μm or more. The thickness T may be, for example, 25 μm or less, 30 μm or less, 50 μm or less, or 80 μm or less. The range of the thickness T may be determined by a first group consisting of 8 μm, 10 μm, 15 μm, and 20 μm, and / or a second group consisting of 25 μm, 30 μm, 50 μm, and 80 μm. The range of the thickness T may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the thickness T may be determined by a combination of any two of the values ​​included in the first group described above. The range of the thickness T may be determined by a combination of any two of the values ​​included in the second group described above. The thickness T may be, for example, 8 μm or more and 80 μm or less, 8 μm or more and 50 μm or less, 8 μm or more and 30 μm or less, 8 μm or more and 25 μm or less, 8 μm or more and 20 μm or less, 8 μm or more and 15 μm or less, 8 μm or more and 10 μm or less, 10 μm or more and 80 μm or less, 10 μm or more and 50 μm or less, 10 μm or more and 30 μm or less, 10 μm or more and 25 μm or less, 10 μm or more and 20 μm or less, 10 μm or more and 15 μm or more and 15 μm or more and 80 μm or less. , 15 μm or more and 50 μm or less, 15 μm or more and 30 μm or less, 15 μm or more and 25 μm or less, 15 μm or more and 20 μm or less, 20 μm or more and 80 μm or less, 20 μm or more and 50 μm or less, 20 μm or more and 30 μm or less, 20 μm or more and 25 μm or less, 25 μm or more and 80 μm or less, 25 μm or more and 50 μm or less, 25 μm or more and 30 μm or less, 30 μm or more and 80 μm or less, 30 μm or more and 50 μm or less, or 50 μm or more and 80 μm or less. The thickness T of the mask 50 may be the thickness T of the metal plate 55.

[0098] By setting the thickness T to 80 μm or less, it is possible to prevent the deposition material 7 from getting caught on the wall surface of the through-hole 56 before passing through the through-hole 56. This can improve the utilization efficiency of the deposition material 7. Furthermore, by setting the thickness T to 8 μm or more, it is possible to ensure the strength of the mask 50 and prevent the mask 50 from being damaged or deformed.

[0099] A contact measurement method is used to measure the thickness T. Specifically, the thickness T is measured by a high-precision digital length measuring machine, Litematic VL-50S, manufactured by Mitutoyo Corporation.

[0100] Next, a method for manufacturing the mask 50 will be described. Fig. 11 is a diagram showing a manufacturing apparatus 70 for manufacturing the mask 50. The manufacturing apparatus 70 includes a resist forming apparatus 71, an exposure apparatus 72, a developing apparatus 73, a resist cleaning apparatus 74, a heating apparatus 75, a first etching apparatus 76, a filling apparatus 77, a second etching apparatus 78, and a separating apparatus 79.

[0101] First, a metal plate wound in a roll shape is prepared. Then, the metal plate is unwound from the roll. The metal plate unwound from the roll is represented by the symbol 55A. The metal plate 55A is transported to the resist forming device 71, the exposure device 72, the developing device 73, the resist cleaning device 74, the heating device 75, the first etching device 76, the filling device 77, the second etching device 78, and the separation device 79 in order. In all the devices from the resist forming device 71 to the separation device 79, the metal plate 55A may be transported continuously along its length direction. Although not shown, the manufacturing method of the mask 50 may include a step of winding the metal plate 55A in a roll shape and a step of unwinding the metal plate 55A from the roll when transporting the metal plate 55A from one device to the next device.

[0102] 12, the resist forming device 71 performs a resist forming step of forming a first resist layer 61 on a first surface 551 of the metal plate 55A and a second resist layer 62 on a second surface 552. The resist layers 61 and 62 may be layers formed by applying a solution containing a resist material to the surface of the metal plate 55A and solidifying it. Alternatively, the resist layers 61 and 62 may be layers formed by attaching a film such as a dry film to the surface of the metal plate 55A.

[0103] The coating type resist layer is formed by coating the surface of the metal plate 55A with a solution containing a photosensitive material and solidifying it. At this time, a baking step may be performed to bake the resist layers 61 and 62. The photosensitive material may be a photo-dissolving type, a so-called positive type, or a photo-curing type, a so-called negative type.

[0104] The positive photosensitive material is, for example, a novolac-based positive resist such as SC500. The negative photosensitive material is, for example, a casein resist. The negative resist layer may contain an acrylic resin.

[0105] FIG. 12 is a cross-sectional view showing an example in which the resist layers 61, 62 are of a film type. As shown in FIG. 12, the resist forming step may include attaching a first dry film 61F to the first surface 551 and attaching a second dry film 62F to the second surface 552. The first dry film 61F includes a first resist layer 61 and a first support 61s that supports the first resist layer 61. It is preferable that the first support 61s has a higher rigidity than the first resist layer 61. For example, the first support 61s may be a stretched plastic film. The stretched plastic film is, for example, a stretched polyester film, a stretched polyamide film, a stretched polypropylene film, or the like. The stretched polyester film is, for example, a stretched polyester terephthalate film (also called a stretched PET film), or the like.

[0106] The second dry film 62F includes a second resist layer 62 and a second support 62s that supports the second resist layer 62. The second support 62s preferably has higher rigidity than the second resist layer 62. For example, the second support 62s may also be a stretched plastic film, similar to the first support 61s.

[0107] The thickness of the resist layers 61, 62 may be, for example, 1 μm or more, 3 μm or more, or 5 μm or more. The thickness of the resist layers 61, 62 may be, for example, 10 μm or less, 15 μm or less, or 20 μm or less. The range of the thickness of the resist layers may be determined by a first group consisting of 1 μm, 3 μm, and 5 μm, and / or a second group consisting of 10 μm, 15 μm, and 20 μm. The range of the thickness of the resist layers may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the thickness of the resist layers may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the thickness of the resist layers may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The thickness of the resist layer may be, for example, 1 μm or more and 20 μm or less, 1 μm or more and 15 μm or less, 1 μm or more and 10 μm or less, 1 μm or more and 5 μm or less, 1 μm or more and 3 μm or less, 3 μm or more and 20 μm or less, 3 μm or more and 15 μm or less, 3 μm or more and 10 μm or less, 3 μm or more and 5 μm or less, 5 μm or more and 20 μm or less, 5 μm or more and 15 μm or less, 5 μm or more and 10 μm or less, 10 μm or more and 20 μm or less, 10 μm or more and 15 μm or less, or 15 μm or more and 20 μm or less.

[0108] The exposure device 72 performs an exposure process of exposing the first resist layer 61 and exposing the second resist layer 62. As shown in Fig. 13, the first resist layer 61 is irradiated with a first exposure light L1 through a first exposure mask 63. The second resist layer 62 is irradiated with a second exposure light L2 through a second exposure mask 64. The exposure process may include a process of adjusting the relative position of the second exposure mask 64 with respect to the first exposure mask 63.

[0109] The wavelength of the exposure light L1, L2 may be, for example, 180 nm or more, 250 nm or more, or 300 nm or more. The wavelength of the exposure light L1, L2 may be, for example, 320 nm or less, 370 nm or less, or 400 nm or less. The wavelength range of the exposure light L1, L2 may be determined by a first group consisting of 180 nm, 250 nm, and 300 nm, and / or a second group consisting of 320 nm, 370 nm, and 400 nm. The wavelength range of the exposure light L1, L2 may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The wavelength range of the exposure light L1, L2 may be determined by a combination of any two of the values ​​included in the first group described above. The wavelength range of the exposure light L1, L2 may be determined by a combination of any two of the values ​​included in the second group described above. The wavelength of the exposure light L1, L2 may be, for example, 180 nm or more and 400 nm or less, 180 nm or more and 370 nm or less, 180 nm or more and 320 nm or less, 180 nm or more and 300 nm or less, 180 nm or more and 250 nm or less, 250 nm or more and 400 nm or less, 250 nm or more and 370 nm or less, 250 nm or more and 320 nm or less, 250 nm or more and 300 nm or less, 300 nm or more and 400 nm or less, 300 nm or more and 370 nm or less, 300 nm or more and 320 nm or less, 320 nm or more and 400 nm or less, 320 nm or more and 370 nm or less, or 370 nm or more and 400 nm or less.

[0110] 13, the exposure step may be performed in a state where the first support 61s is in contact with the first resist layer 61. In this case, light that has passed through the first exposure mask 63 reaches the first resist layer 61 after passing through the first support 61s. The exposure step may be performed in a state where the first exposure mask 63 is in contact with the first support 61s. Although not shown, the exposure step may be performed after the first support 61s is peeled off from the first resist layer 61.

[0111] 13, the exposure step may be performed in a state where the second support 62s is in contact with the second resist layer 62. In this case, light that has passed through the second exposure mask 64 reaches the second resist layer 62 after passing through the second support 62s. The exposure step may be performed in a state where the second exposure mask 64 is in contact with the second support 62s. Although not shown, the exposure step may be performed after the second support 62s is peeled off from the second resist layer 62.

[0112] As shown in Fig. 13, the exposure light L1 may be a parallel light including a plurality of light rays traveling parallel to each other. By using parallel light, it is possible to suppress the occurrence of fringes, which will be described later, in the resist layer. Like the exposure light L1, the exposure light L2 may also be a parallel light including a plurality of light rays traveling parallel to each other.

[0113] The declination angle of the parallel light is, for example, 3.0° or less, may be 2.0° or less, or may be 1.0° or less. The declination angle is the maximum angle between the light coming from the center of the light source and the normal line of the irradiation surface onto which the parallel light is irradiated. The declination angle is also called the central ray parallelism. The declination angle of the parallel light may be 0.1° or more.

[0114] The developing device 73 performs a developing step of developing the first resist layer 61 and developing the second resist layer 62. As a result, as shown in Fig. 14A, a first opening 612 is formed in the first resist layer 61 and a second opening 622 is formed in the second resist layer 62. The first resist layer 61 in which the first opening 612 is formed is also referred to as a first resist pattern 611. The second resist layer 62 in which the second opening 622 is formed is also referred to as a second resist pattern 621.

[0115] The process of forming the first resist pattern 611 on the first surface 551 and the second resist pattern 621 on the second surface 552 is also referred to as a resist pattern forming process. The resist pattern forming process includes the above-mentioned resist forming process, exposure process, and development process. The exposure process and development process are also referred to as a patterning process.

[0116] Fig. 14B is a plan view showing metal plate 55A shown in Fig. 14A viewed from the side of first surface 551. First resist pattern 611 has width W1. Width W1 is the minimum value of the distance between two first openings 612.

[0117] The width W1 may be, for example, 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, or 30 μm or more. The width W1 may be, for example, 40 μm or less, 50 μm or less, or 60 μm or less. The range of the width W1 may be determined by a first group consisting of 10 μm, 15 μm, 20 μm, 25 μm, and 30 μm, and / or a second group consisting of 40 μm, 50 μm, and 60 μm. The range of the width W1 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the width W1 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the width W1 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The width W1 may be, for example, 10 μm or more and 60 μm or less, 10 μm or more and 50 μm or less, 10 μm or more and 40 μm or less, 10 μm or more and 30 μm or less, 10 μm or more and 25 μm or less, 10 μm or more and 20 μm or less, 10 μm or more and 15 μm or more and 15 μm or more and 60 μm or less, 15 μm or more and 50 μm or less, 15 μm or more and 40 μm or less, 15 μm or more and 30 μm or less, 15 μm or more and 25 μm or less, 15 μm or more and 20 μm or more and 60 μm or less. or more, 20 μm or more and 50 μm or less, 20 μm or more and 40 μm or less, 20 μm or more and 30 μm or less, 20 μm or more and 25 μm or less, 25 μm or more and 60 μm or less, 25 μm or more and 50 μm or less, 25 μm or more and 40 μm or less, 25 μm or more and 30 μm or less, 30 μm or more and 60 μm or less, 30 μm or more and 50 μm or less, 30 μm or more and 40 μm or less, 40 μm or more and 60 μm or less, 40 μm or more and 50 μm or less, or 50 μm or more and 60 μm or less.

[0118] The width W1 is calculated by measuring the shape of the first resist pattern 611 from the first surface 551 side. Specifically, the width W1 is calculated by averaging the measurement results of the first resist pattern 611 adjacent to 100 first openings 612. The 100 first openings 612 are a collection of 10 rows x 10 rows of first openings 612 located in the center of the group of first openings 612 corresponding to the through-hole group 53. A digital microscope VHX-7000 manufactured by Keyence Corporation is used as the measuring instrument.

[0119] The resist cleaning device 74 performs a resist cleaning process using a cleaning liquid to clean the first resist pattern 611. The resist cleaning process may clean the first resist pattern 611 and the second resist pattern 621.

[0120] The heating device 75 performs a heating step of heating the first resist pattern 611 at a processing temperature. The heating step may heat the second resist pattern 621 at the processing temperature in addition to the first resist pattern 611. By performing the heating step, it is possible to improve the adhesion of the first resist pattern 611 and the second resist pattern 621 to the metal plate 55A.

[0121] After the resist cleaning step, an irradiation step may be performed in which ultraviolet rays are irradiated onto the first resist pattern 611 and the second resist pattern 621. By performing the irradiation step, it is possible to improve the adhesion of the first resist pattern 611 and the second resist pattern 621 to the metal plate 55A.

[0122] The first etching device 76 carries out a first etching step of etching the first surface 551 by using a first etching liquid. When the first etching liquid enters the first opening 612, a first recess 56a is formed in the first surface 551 as shown in FIG.

[0123] In the first etching step, the first etching liquid may be sprayed toward the first surface 551. As shown in FIG. 15, the first etching step may be performed in a state in which the first surface 551 is positioned below the second surface 552. In this case, the first etching liquid that has come into contact with the metal plate 55 can fall from the metal plate 55 by gravity. This makes it possible to prevent the first etching liquid in which the material of the metal plate 55 has been dissolved from being in contact with the first surface 551.

[0124] The first recess 56a does not penetrate the metal plate 55. Therefore, the depth H1 of the first recess 56a is smaller than the thickness T of the metal plate 55. The depth H1 may be, for example, 2 μm or more, 3 μm or more, or 5 μm or more. The depth H1 may be, for example, 20 μm or less, 30 μm or less, or 45 μm or less. The range of the depth H1 may be determined by a first group consisting of 2 μm, 3 μm, and 5 μm, and / or a second group consisting of 20 μm, 30 μm, and 45 μm. The range of the depth H1 may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the depth H1 may be determined by a combination of any two of the values ​​included in the first group described above. The range of the depth H1 may be determined by a combination of any two of the values ​​included in the second group described above. The depth H1 may be, for example, 2 μm or more and 45 μm or less, 2 μm or more and 30 μm or less, 2 μm or more and 20 μm or less, 2 μm or more and 5 μm or less, 2 μm or more and 3 μm or less, 3 μm or more and 45 μm or less, 3 μm or more and 30 μm or less, 3 μm or more and 20 μm or less, 3 μm or more and 5 μm or less, 5 μm or more and 45 μm or less, 5 μm or more and 30 μm or less, 5 μm or more and 20 μm or less, 20 μm or more and 45 μm or less, 20 μm or more and 30 μm or less, or 30 μm or more and 45 μm or less.

[0125] The upper limit of the depth H1 may be determined according to the thickness T of the metal plate 55. For example, the depth H1 may be (T-5) μm or less. When the thickness T is 20 μm or more, the depth H1 may be (T-10) μm or less. When the thickness T is 30 μm or more, the depth H1 may be (T-20) μm or less.

[0126] H1 / T, which is the ratio of the depth H1 to the thickness T, may be, for example, 0.10 or more, 0.20 or more, or 0.30 or more. H1 / T may be, for example, 0.50 or less, 0.70 or less, or 0.90 or less. The range of H1 / T may be determined by a first group consisting of 0.10, 0.20, and 0.30, and / or a second group consisting of 0.50, 0.70, and 0.90. The range of H1 / T may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of H1 / T may be determined by a combination of any two of the values ​​included in the first group described above. The range of H1 / T may be determined by a combination of any two of the values ​​included in the second group described above. H1 / T may be, for example, 0.10 or more and 0.90 or less, 0.10 or more and 0.70 or less, 0.10 or more and 0.50 or less, 0.10 or more and 0.30 or less, 0.10 or more and 0.20 or less, 0.20 or more and 0.90 or less, 0.20 or more and 0.70 or less, 0.20 or more and 0.50 or less, 0.20 or more and 0.30 or less, 0.30 or more and 0.90 or less, 0.30 or more and 0.70 or less, 0.30 or more and 0.50 or less, 0.50 or more and 0.90 or less, 0.50 or more and 0.70 or less, or 0.70 or more and 0.90 or less.

[0127] The ratio H1 / r1 of the depth H1 to the dimension r1 of the first contour 561 of the first recess 56a may be, for example, 0.10 or more, 0.15 or more, or 0.20 or more. H1 / r1 may be, for example, 0.30 or less, 0.40 or less, or 0.50 or less. The range of H1 / r1 may be determined by a first group consisting of 0.10, 0.15, and 0.20, and / or a second group consisting of 0.30, 0.40, and 0.50. The range of H1 / r1 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of H1 / r1 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of H1 / r1 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. H1 / r1 may be, for example, 0.10 or more and 0.50 or less, 0.10 or more and 0.40 or less, 0.10 or more and 0.30 or less, 0.10 or more and 0.20 or less, 0.10 or more and 0.15 or less, 0.15 or more and 0.50 or less, 0.15 or more and 0.40 or less, 0.15 or more and 0.30 or less, 0.15 or more and 0.20 or less, 0.20 or more and 0.50 or less, 0.20 or more and 0.40 or less, 0.20 or more and 0.30 or less, 0.30 or more and 0.50 or less, 0.30 or more and 0.40 or less, or 0.40 or more and 0.50 or less.

[0128] The ranges of the depths H1, H1 / T, and H1 / r1 may be determined according to the range of the thickness T of the metal plate 55. For example, when the thickness T is 10 μm or more and 15 μm or less, the depth H1 may be 2.0 μm or more and 5.0 μm or less, H1 / T may be 0.20 or more and 0.50 or less, the dimension r1 may be 10 μm or more and 20 μm or less, and H1 / r1 may be 0.20 or more and 0.25 or less.

[0129] The filling device 77 performs a filling step of filling the first recesses 56a with the resin 65, as shown in FIG. 16. As shown in FIG. 16, the filling step may form a resin layer 65L that covers the first resist pattern 611. The resin 65 constituting the resin layer 65L is filled into the first recesses 56a. The filling step may be performed in a state in which the first surface 551 is positioned above the second surface 552.

[0130] The resin 65 has resistance to a second etching liquid used in a second etching step described later. By filling the first recesses 56a with the resin 65, it is possible to prevent the second etching liquid from penetrating into the first recesses 56a during the second etching step.

[0131] The thickness TF1 of the resin layer 65L is greater than the depth H1 of the first recess 56a. The thickness TF1 of the resin layer 65L is greater than the thickness TR1 of the first resist pattern 611. The thickness TF1 of the resin layer 65L is the distance from the surface of the resin layer 65L to the surface of the first resist pattern 611 in the thickness direction.

[0132] 16, a recess 651 may be formed on the surface of the resin layer 65L. The recess 651 is formed by the resin 65 constituting the resin layer 65L flowing toward the first recess 56a. The recess 651 may be formed at a position overlapping the first recess 56a in the thickness direction.

[0133] The thickness TR1, the thickness TF1, and the depth H1 are calculated based on a cross-sectional image of a sample of a laminate including the resin layer 65L, the first resist pattern 611, and the metal plate 55A. The cross-sectional image is calculated by observing the cross-section of the sample using a scanning electron microscope. As the scanning electron microscope, a ZEISS ULTRA55 scanning electron microscope is used.

[0134] The second etching device 78 carries out a second etching step of etching the second surface 552 using a second etching liquid. When the second etching liquid enters the second opening 622, a second recess 56b is formed in the second surface 552 as shown in FIG.

[0135] In the second etching step, the second etching liquid may be sprayed toward the second surface 552. As shown in FIG. 17, the second etching step may be performed in a state in which the second surface 552 is positioned below the first surface 551. In this case, the second etching liquid that has come into contact with the metal plate 55 can fall from the metal plate 55 by gravity. This makes it possible to prevent the second etching liquid in which the material of the metal plate 55 has been dissolved from being in contact with the metal plate 55.

[0136] After the second etching step, a removing step may be performed. The removing step may include a resin removing step of removing the resin 65. The resin 65 is removed, for example, by using an alkaline stripping liquid. The removing step may include a resist removing step of removing the first resist pattern 611 and the second resist pattern 621. The first resist pattern 611 and the second resist pattern 621 may be removed simultaneously with the resin 65 by using an alkaline stripping liquid. After the resin 65 is removed, the first resist pattern 611 and the second resist pattern 621 may be removed by using a stripping liquid different from the stripping liquid for stripping the resin 65. FIG. 18 is a cross-sectional view showing the metal plate 55A in a state in which the resin 65, the first resist pattern 611, and the second resist pattern 621 have been removed.

[0137] Fig. 19 is a plan view showing the metal plate 55A in a state in which the through-hole group 53 is formed. In Fig. 19, the symbol x represents the longitudinal direction of the metal plate 55A, and the symbol y represents the width direction of the metal plate 55A. The longitudinal direction x coincides with the above-mentioned conveying direction F1. The width direction y is perpendicular to the longitudinal direction x. The metal plate 55A includes a first side edge 55x1 and a second side edge 55x2 extending in the longitudinal direction x.

[0138] 19 , before the masks 50 are separated from the metal plate 55A, a plurality of masks 50 may be arranged in the width direction y of the metal plate 55A. The metal plate 55A may include an outer edge hole 591 that defines the outer edge of the mask 50. A bridge 595 may be connected to the outer edge of the mask 50. The bridge 595 may be connected to a first end 503 and a second end 504.

[0139] The separation device 79 performs a separation process to separate the mask 50 from the metal plate 55A. The mask 50 can be separated from the metal plate 55A by breaking the bridges 595. In this manner, the mask 50 is obtained.

[0140] As a result of repeated research by the present inventors, a phenomenon was found in which the dimensional accuracy of the through-holes 56 of the mask 50 is reduced due to recesses on the surface of the metal plate 55A. The recesses on the surface are, for example, rolling streaks, oil pits, etc. FIG. 20 is a plan view showing an example of a first surface 551 of the metal plate 55A. The first surface 551 of the metal plate 55A may include a plurality of rolling streaks 55f extending in the longitudinal direction x and a plurality of oil pits 55e. The rolling streaks 55f are recesses that appear on the surface of the metal plate 55A along the rolling direction. The oil pits 55e are recesses that appear on the surface of the metal plate 55A due to rolling oil remaining on the surface of the metal plate 55A during the rolling process.

[0141] In the rolling process, rolling oil is supplied between the metal sheet before rolling and the rolling rolls. If recesses are formed on the surface of the metal sheet before rolling, the rolling oil penetrates into the recesses. The recesses on the surface of the metal sheet before rolling are also called initial recesses. The initial recesses are formed by erosion of grain boundaries, etc. A part of the rolling oil that penetrates into the initial recesses is discharged from the initial recesses during rolling, and the other part remains in the initial recesses even after rolling. The initial recesses where the rolling oil remains are generated on the surface of the metal sheet 55A as oil pits 55e.

[0142] FIG. 21 is a cross-sectional view showing an example of light reflection occurring at a metal plate 55A. In the example shown in FIG. 21, the metal plate 55A is cut along the width direction y. Rolled streaks 55f appear in the cross section of the metal plate 55A. The symbol L_a represents light incident on the first surface 551. The symbol θ represents the angle of incidence of the incident light L_a. The symbol L_b represents light reflected at the first surface 551. The symbol φ represents the angle of emission of the reflected light L_b. The dashed dotted line marked with the symbol N represents the normal direction of the first surface 551.

[0143] As shown in FIG. 21, in an area where no concave portion such as the rolled streak 55f is formed, the emission angle φ of the reflected light L_b is approximately equal to the incidence angle θ of the incident light L_a. That is, regular reflection occurs on the first surface 551. On the other hand, in an area where a concave portion such as the rolled streak 55f is formed, the emission angle φ of the reflected light L_b deviates from the incidence angle θ of the incident light L_a. In some of the rolled streak 55f, the emission angle φ is larger than the incidence angle θ. In some of the rolled streak 55f, the emission angle φ is smaller than the incidence angle θ. The reflected light L_b having an emission angle φ different from the incidence angle θ is also called diffuse light. The concave portion such as the rolled streak 55f generates diffuse light.

[0144] The rolled streaks 55f extend along the longitudinal direction x. For this reason, the diffused light caused by the rolled streaks 55f is likely to occur in a plane parallel to the normal direction N and the width direction y of the first surface 551 as shown in FIG. 21. In other words, the rolled streaks 55f are likely to diffuse the light traveling in the width direction y in a planar view. In the following description, the light traveling in the width direction y in a planar view and incident on the surface of the metal plate 55A is also referred to as the first incident light. The light traveling in the longitudinal direction x in a planar view and incident on the surface of the metal plate 55A is also referred to as the second incident light.

[0145] The rolled streaks 55f are more likely to diffuse the first incident light than the second incident light. That is, the rolled streaks 55f have directional dependence on the diffused light. On the other hand, the directional dependence of the shape of the oil pits 55e in plan view is smaller than the directional dependence of the shape of the rolled streaks 55f. Therefore, the directional dependence of the oil pits 55e on the diffused light is smaller than the directional dependence of the rolled streaks 55f on the diffused light.

[0146] The relationship between the diffused light generated on the surface of the metal plate 55A and the dimensional accuracy of the through-holes 56 of the mask 50 will be described with reference to Figs. 22 to 25. Fig. 22 is a cross-sectional view showing an example of light being reflected on the surface of the metal plate 55A in the exposure process. The symbol L1r represents the diffused light generated by the exposure light L1 being reflected on the first surface 551. In the example shown in Fig. 22, the first resist layer 61 contains a negative type photosensitive material.

[0147] FIG. 23 is a cross-sectional view showing an example of a first resist pattern 611 formed by developing the first resist layer 61 shown in FIG. 22. The first resist pattern 611 includes a first resist layer, a first opening 612 formed in the first resist layer, and a wall surface 613 of the first resist layer facing the first opening 612. When diffused light is generated, the first resist layer 61 at the position where the first opening 612 is to be formed is exposed. As a result, for example, a fringe 614 is generated on the wall surface 613. The fringe 614 is a part of the first resist layer that protrudes at a corner toward the center of the first opening 612 in a plan view. The corner is a portion where a surface 615 of the first resist pattern 611 facing the first surface 551 of the metal plate 55A and the wall surface 613 are connected. The fringe 614 has a width W2 in a plan view.

[0148] 24 is a plan view showing an example of resist pattern 611 including fringe 614. In the first etching step, etching of the region of first surface 551 overlapping fringe 614 is prevented by fringe 614. As a result, the dimensional accuracy of first recess 56a of through hole 56 decreases.

[0149] 25 is a plan view showing an example of the first recess 56a and the through portion 56c of the through hole 56. The symbol R_ay represents the dimension of the first contour 561 of the first recess 56a in the width direction y, and the symbol R_ax represents the dimension of the first contour 561 of the first recess 56a in the longitudinal direction x. The symbol R_cy represents the dimension of the through portion 56c in the width direction y, and the symbol R_cx represents the dimension of the through portion 56c in the longitudinal direction x. The dimension R_cy is also referred to as the first through dimension. The dimension R_cx is also referred to as the second through dimension. Both the dimensional accuracy of the first contour 561 and the dimensional accuracy of the through portion 56c may be affected by the fringe 614 of the first resist pattern 611.

[0150] As described later, the metal plate 55A according to the embodiment of the present disclosure can suppress the occurrence of the fringe 614. For example, the width W2 of the fringe 614 can be reduced. Therefore, the first recess 56a of the through hole 56 has high dimensional accuracy. This can improve the accuracy of the deposition layer of the organic device 100.

[0151] 24, symbols W21 and W22 represent the width of the fringe 614 in the width direction y, and symbols W23 and W24 represent the width of the fringe 614 in the longitudinal direction x. The width W2 of the fringe 614 corresponding to one first opening 612 is calculated by averaging W21, W22, W23, and W24.

[0152] The width of the fringe 614 may be, for example, 0.01 μm or more, 0.10 μm or more, or 0.20 μm or more. The width of the fringe 614 may be, for example, 0.40 μm or less, 0.70 μm or less, or 1.00 μm or less. The range of the width of the fringe 614 may be defined by a first group consisting of 0.01 μm, 0.10 μm, and 0.20 μm, and / or a second group consisting of 0.40 μm, 0.70 μm, and 1.00 μm. The range of the width of the fringe 614 may be defined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the width of the fringe 614 may be defined by a combination of any two of the values ​​included in the first group described above. The range of the width of the fringe 614 may be defined by a combination of any two of the values ​​included in the second group described above. The width of the fringe 614 may be, for example, 0.01 μm or more and 1.00 μm or less, 0.01 μm or more and 0.70 μm or less, 0.01 μm or more and 0.40 μm or less, 0.01 μm or more and 0.20 μm or less, 0.01 μm or more and 0.10 μm or less, 0.10 μm or more and 1.00 μm or less, 0.10 μm or more and 0.70 μm or less, or 0.1 It may be 0 μm or more and 0.40 μm or less, 0.10 μm or more and 0.20 μm or less, 0.20 μm or more and 1.00 μm or less, 0.20 μm or more and 0.70 μm or less, 0.20 μm or more and 0.40 μm or less, 0.40 μm or more and 1.00 μm or less, 0.40 μm or more and 0.70 μm or less, or 0.70 μm or more and 1.00 μm or less.

[0153] The width of the fringe 614 is calculated by averaging the widths W2 of the fringes 614 occurring on the wall surface 613 facing the five first openings 612. The five first openings 612 are aligned in the longitudinal direction x at the centers of the through-hole groups 53 that are located in the center of the corresponding mask 50 in the longitudinal direction x.

[0154] As described above, in the rolled streaks 55f, the diffused light L1r is likely to occur in the width direction y. Therefore, in the fringes 614 caused by the rolled streaks 55f, the widths W21 and W22 in the width direction y are likely to be larger than the widths W23 and W24 in the longitudinal direction x. As a result, the dimension of the through hole 56 in the width direction y is likely to be smaller than the dimension of the through hole 56 in the longitudinal direction x. For example, the dimension R_ay of the first contour 561 in the width direction y is likely to be smaller than the dimension R_ax of the first contour 561 in the longitudinal direction x. For example, the first penetration dimension R_cy of the through portion 56c in the width direction y is likely to be smaller than the second penetration dimension R_cx of the through portion 56c in the longitudinal direction x.

[0155] In the metal plate 55A of the embodiment of the present disclosure, the rolled streaks 55f may be reduced. By reducing the rolled streaks 55f, it is possible to suppress the phenomenon in which the dimension of the through hole 56 in the width direction y is smaller than the dimension of the through hole 56 in the longitudinal direction x. As a result, for example, the ratio of the dimension R_ay to the dimension R_ax becomes closer to 1.00. For example, the ratio of the first penetration dimension R_cy to the second penetration dimension R_cx becomes closer to 1.00.

[0156] The ratio of the dimension R_ay to the dimension R_ax may be, for example, 0.95 or more, 0.98 or more, or 0.99 or more. The ratio of the dimension R_ay to the dimension R_ax may be, for example, 1.00 or less, 1.01 or less, or 1.02 or less. The range of the ratio of the dimension R_ay to the dimension R_ax may be determined by a first group consisting of 0.95, 0.98, and 0.99, and / or a second group consisting of 1.00, 1.01, and 1.02. The range of the ratio of the dimension R_ay to the dimension R_ax may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the ratio of the dimension R_ay to the dimension R_ax may be determined by a combination of any two of the values ​​included in the first group described above. The range of the ratio of the dimension R_ay to the dimension R_ax may be determined by a combination of any two of the values ​​included in the second group described above. The ratio of the dimension R_ay to the dimension R_ax may be, for example, 0.95 or more and 1.02 or less, 0.95 or more and 1.01 or less, 0.95 or more and 1.00 or less, 0.95 or more and 0.99 or less, 0.95 or more and 0.98 or less, 0.98 or more and 1.02 or less, 0.98 or more and 1.01 or less, 0.98 or more and 1.00 or less, 0.98 or more and 0.99 or less, 0.99 or more and 1.02 or less, 0.99 or more and 1.01 or less, 0.99 or more and 1.00 or less, 1.00 or more and 1.02 or less, 1.00 or more and 1.01 or less, or 1.01 or more and 1.02 or less.

[0157] The ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be, for example, 0.95 or more, 0.98 or more, or 0.99 or more. The ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be, for example, 1.00 or less, 1.01 or less, or 1.02 or less. The range of the ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be determined by a first group consisting of 0.95, 0.98, and 0.99, and / or a second group consisting of 1.00, 1.01, and 1.02. The range of the ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The ratio of the first penetration dimension R_cy to the second penetration dimension R_cx may be, for example, 0.95 or more and 1.02 or less, 0.95 or more and 1.01 or less, 0.95 or more and 1.00 or less, 0.95 or more and 0.99 or less, 0.95 or more and 0.98 or less, 0.98 or more and 1.02 or less, 0.98 or more and 1.01 or less, 0.98 or more and 1.00 or less, 0.98 or more and 0.99 or less, 0.99 or more and 1.02 or less, 0.99 or more and 1.01 or less, 0.99 or more and 1.00 or less, 1.00 or more and 1.02 or less, 1.00 or more and 1.01 or less, or 1.01 or more and 1.02 or less.

[0158] Next, the metal plate 55A of the embodiment of the present disclosure will be described. The metal plate 55A includes a surface where the generation of diffused light is suppressed. The surface where the generation of diffused light is suppressed may be the first surface 551 or the second surface 552. Both the first surface 551 and the second surface 552 may be surfaces where the generation of diffused light is suppressed. In the following description, an example where the first surface 551 is a surface where the generation of diffused light is suppressed will be described.

[0159] The first surface 551 of the metal plate 55A may have a first reflectance R1, a second reflectance R2, a third reflectance R3, and a fourth reflectance R4. The ratio R3 / R1 of the third reflectance R3 to the first reflectance R1 is also referred to as the first ratio. The ratio R4 / R2 of the fourth reflectance R4 to the second reflectance R2 is also referred to as the second ratio. The metal plate 55A preferably has a reduced first ratio R3 / R1 and a reduced second ratio R4 / R2. As supported by the examples described later, the metal plate 55A having a reduced first ratio R3 / R1 and a reduced second ratio R4 / R2 can suppress the occurrence of a fringe 614 in the resist pattern 611.

[0160] The first reflectance R1 is the reflectance of the first reflected light L_by having the first exit angle φ1. The third reflectance R3 is the reflectance of the first reflected light L_by having the third exit angle φ3. The first reflected light L_by is the first incident light L_ay reflected by the first surface 551. The first incident light L_ay is light that travels in the width direction y in a plan view and enters the first surface 551 at a first specific incident angle θ1. The first specific incident angle θ1 is, for example, 20°.

[0161] It is not possible to completely prevent light diffusion on the surface of the metal plate 55A. Therefore, the first reflected light L_by has an intensity distribution according to the emission angle in a plane parallel to the normal direction N and width direction y of the first surface 551. The first emission angle φ1 is the emission angle at which the first reflected light L_by shows the maximum intensity. The third emission angle φ3 is the emission angle that differs from the first emission angle φ1 by the first deviation angle φd1. The first deviation angle φd1 is, for example, 2.5°.

[0162] The second reflectance R1 is the reflectance of the second reflected light L_bx having the second exit angle φ2. The fourth reflectance R4 is the reflectance of the second reflected light L_bx having the fourth exit angle φ4. The second reflected light L_bx is the second incident light L_ax reflected by the first surface 551. The second incident light L_ax is light that travels in the width direction x in a plan view and enters the first surface 551 at a second specific incident angle θ2. The second specific incident angle θ2 is, for example, 20°.

[0163] The second reflected light L_bx has an intensity distribution according to the emission angle in a plane parallel to the normal direction N and the longitudinal direction x of the first surface 551. The second emission angle φ2 is the emission angle at which the second reflected light L_bx exhibits the maximum intensity. The fourth emission angle φ4 is the emission angle that differs from the second emission angle φ2 by a second deviation angle φd2. The second deviation angle φd2 is, for example, 2.5°.

[0164] The first ratio R3 / R1 may be, for example, 0.00 or more, 0.05 or more, or 0.10 or more. The first ratio R3 / R1 may be, for example, 0.20 or less, 0.30 or less, or 0.40 or less. The range of the first ratio R3 / R1 may be determined by a first group consisting of 0.00, 0.05, and 0.10, and / or a second group consisting of 0.20, 0.30, and 0.40. The range of the first ratio R3 / R1 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the first ratio R3 / R1 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the first ratio R3 / R1 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The first ratio R3 / R1 may be, for example, 0.00 or more and 0.40 or less, 0.00 or more and 0.30 or less, 0.00 or more and 0.20 or less, 0.00 or more and 0.10 or less, 0.00 or more and 0.05 or less, 0.05 or more and 0.40 or less, 0.05 or more and 0.30 or less, 0.05 or more and 0.20 or less, 0.05 or more and 0.10 or less, 0.10 or more and 0.40 or less, 0.10 or more and 0.30 or less, 0.10 or more and 0.20 or less, 0.20 or more and 0.40 or less, 0.20 or more and 0.30 or less, or 0.30 or more and 0.40 or less.

[0165] Similar to the first ratio R3 / R1, the second ratio R4 / R2 is also reduced. The second ratio R4 / R2 may be, for example, 0.00 or more, 0.05 or more, or 0.10 or more. The second ratio R4 / R2 may be, for example, 0.20 or less, 0.30 or less, or 0.40 or less. The range of the second ratio R4 / R2 may be determined by a first group consisting of 0.00, 0.05, and 0.10, and / or a second group consisting of 0.20, 0.30, and 0.40. The range of the second ratio R4 / R2 may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the second ratio R4 / R2 may be determined by a combination of any two of the values ​​included in the first group described above. The range of the second ratio R4 / R2 may be determined by a combination of any two of the values ​​included in the second group described above. The second ratio R4 / R2 may be, for example, 0.00 to 0.40, 0.00 to 0.30, 0.00 to 0.20, 0.00 to 0.10, 0.00 to 0.05, 0.05 to 0.40, 0.05 to 0.30, 0.05 to 0.20, 0.05 to 0.10, 0.10 to 0.40, 0.10 to 0.30, 0.10 to 0.20, 0.20 to 0.40, 0.20 to 0.30, or 0.30 to 0.40. The second ratio R4 / R2 may be smaller than the first ratio R3 / R1.

[0166] It is preferable that the difference between the first ratio R3 / R1 and the second ratio R4 / R2 is small, which can suppress the appearance of directional dependency in the dimensions of the through-holes 56 in a plan view.

[0167] The absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be, for example, 0.02 or more, 0.05 or more, or 0.10 or more. The absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be, for example, 0.15 or less, 0.20 or less, or 0.30 or less. The range of the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be determined by a first group consisting of 0.02, 0.05, and 0.10, and / or a second group consisting of 0.15, 0.20, and 0.30. The range of the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 may be, for example, 0.02 or more and 0.30 or less, 0.02 or more and 0.20 or less, 0.02 or more and 0.15 or less, 0.02 or more and 0.10 or less, 0.02 or more and 0.05 or less, 0.05 or more and 0.30 or less, 0.05 or more and 0.20 or less, 0.05 or more and 0.15 or less, 0.05 or more and 0.10 or less, 0.10 or more and 0.30 or less, 0.10 or more and 0.20 or less, 0.10 or more and 0.15 or less, 0.15 or more and 0.30 or less, 0.15 or more and 0.20 or less, or 0.20 or more and 0.30 or less.

[0168] The metal plate 55A may have a low regular reflectance. In the embodiment of the present disclosure, the regular reflectance is an average value of the first reflectance R1 and the second reflectance R2. By setting an upper limit on the regular reflectance of the metal plate 55A, the step of detecting the alignment mark formed on the metal plate 55A can be easily performed.

[0169] The alignment mark is, for example, a portion of the metal plate 55A that has a lower reflectance than the surrounding portions. The alignment mark is, for example, a recess located on the surface of the metal plate 55A that does not penetrate the metal plate 55A. When detecting the alignment mark using a detector that detects reflected light from the metal plate 55A, the alignment mark is ideally recognized as a black portion. However, when the metal plate 55A has a high reflectance, the outline of the alignment mark may be blurred due to reflected light from the surface of the metal plate 55A located around the alignment mark.

[0170] By setting an upper limit on the regular reflectance of the metal plate 55A, it is possible to limit the amount of light reflected from the surface of the metal plate 55A located around the alignment mark, thereby preventing the contour of the detected alignment mark from becoming blurred.

[0171] The specular reflectance may be, for example, 2.0% or more, 2.6% or more, or 3.0% or more. The specular reflectance may be, for example, 26.0% or less, 31.0% or less, or 35.0% or less. The range of specular reflectance may be determined by a first group consisting of 2.0%, 2.6% and 3.0% and / or a second group consisting of 26.0%, 31.0% and 35.0%. The range of specular reflectance may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of specular reflectance may be determined by a combination of any two of the values ​​included in the first group described above. The range of specular reflectance may be determined by a combination of any two of the values ​​included in the second group described above. The regular reflectance may be, for example, 2.0% or more and 35.0% or less, 2.0% or more and 31.0% or less, 2.0% or more and 26.0% or less, 2.0% or more and 3.0% or less, 2.0% or more and 2.6% or less, 2.6% or more and 35.0% or less, 2.6% or more and 31.0% or less, 2.6% or more and 26.0% or less, 2.6% or more and 3.0% or less, 3.0% or more and 35.0% or less, 3.0% or more and 31.0% or less, 3.0% or more and 26.0% or less, 26.0% or more and 35.0% or less, 26.0% or more and 31.0% or less, or 31.0% or more and 35.0% or less.

[0172] It is preferable that the metal plate 55A satisfies the above-mentioned numerical ranges regarding the reflectance and ratio when the first specific incident angle θ1 and the second specific incident angle θ2 are 20°. The advantage of the first specific incident angle θ1 and the second specific incident angle θ2 being 20° will be described.

[0173] FIG. 47A is a cross-sectional view showing an example of light reflection occurring on the surface of the metal plate 55A when the incident angle θ is 20°. FIG. 47B is a cross-sectional view showing an example of light reflection occurring on the surface of the metal plate 55A when the incident angle θ is 45°. As shown in FIG. 47B, when the width of the recess 55g on the surface is narrow, light with an incident angle θ of 45° is unlikely to reach the bottom of the recess 55g. As shown in FIG. 47A, light with an incident angle θ of 20° is more likely to reach the bottom of the recess 55g than light with an incident angle θ of 45°. The reflectance measured using light with an incident angle θ of 20° can include the effect of light reflection caused by the bottom of the recess 55g. By using light with an incident angle θ of 20°, the diffused light caused by the recess 55g can be properly evaluated.

[0174] In the exposure process, the exposure light is incident on the resist layer on the metal plate 55A along the normal direction of the surface of the metal plate 55A. That is, the incident angle of the exposure light is 0° or approximately 0°. Light with an incident angle θ of 20° is preferable to light with an incident angle θ of 45° in that it is closer to the incident angle of the exposure light.

[0175] The metal plate 55A may satisfy the above-mentioned numerical ranges regarding the reflectance and the ratio not only when the first specific incident angle θ1 and the second specific incident angle θ2 are 20°, but also when the first specific incident angle θ1 and the second specific incident angle θ2 are 45°. However, the diffused light generated on the surface of the metal plate 55A when the incident angle θ is 45° is different from the diffused light generated on the surface of the metal plate 55A when the incident angle θ is 20°. Therefore, the metal plate 55A that satisfies the above-mentioned numerical ranges regarding the reflectance and the ratio when the angles θ1 and θ2 are 45° does not necessarily satisfy the above-mentioned numerical ranges regarding the reflectance and the ratio when the angles θ1 and θ2 are 20°.

[0176] The first exit angle φ1 may be approximately equal to the first specific incident angle θ1. By suppressing the generation of diffused light, the difference between the first specific incident angle θ1 and the first exit angle φ1 can be reduced. The absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be, for example, 0.0° or more, 0.1° or more, or 0.2° or more. The absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be, for example, 0.3° or less, 1.0° or less, or 2.0° or less. The range of the absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be determined by a first group consisting of 0.0°, 0.1°, and 0.2°, and / or a second group consisting of 0.3°, 1.0°, and 2.0°. The range of the absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be determined by a combination of any one of the values ​​included in the above-mentioned first group and any one of the values ​​included in the above-mentioned second group. The range of the absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be determined by a combination of any two of the values ​​included in the above-mentioned first group. The range of the absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be determined by a combination of any two of the values ​​included in the above-mentioned second group. The absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1 may be, for example, 0.0° or more and 2.0° or less, 0.0° or more and 1.0° or less, 0.0° or more and 0.3° or less, 0.0° or more and 0.2° or less, 0.0° or more and 0.1° or less, 0.1° or more and 2.0° or less, 0.1° or more and 1.0° or less, 0.1° or more and 0.3° or less, 0.1° or more and 0.2° or less, 0.2° or more and 2.0° or less, 0.2° or more and 1.0° or less, 0.2° or more and 0.3° or less, 0.3° or more and 2.0° or less, 0.3° or more and 1.0° or less, or 1.0° or more and 2.0° or less.

[0177] The second exit angle φ2 may be approximately equal to the second specific incident angle θ2. By suppressing the generation of diffuse light, the difference between the second specific incident angle θ2 and the second exit angle φ2 can be reduced. The numerical range of the absolute value of the difference between the second specific incident angle θ2 and the second exit angle φ2 may be the same as the above-mentioned numerical range of the absolute value of the difference between the first specific incident angle θ1 and the first exit angle φ1.

[0178] A method for measuring the first reflectance R1, the second reflectance R2, the third reflectance R3 and the fourth reflectance R4 will be described with reference to FIGS.

[0179] First, a metal plate 55A extending in a longitudinal direction x is prepared as shown in Fig. 26. The dimension W of the metal plate 55A in the width direction y may be set so that the metal plate 55A includes a plurality of masks 50 arranged in the width direction y as shown in Fig. 19.

[0180] The dimension W of the metal plate 55A may be, for example, 300 mm or more, 400 mm or more, or 500 mm or more. The dimension W of the metal plate 55A may be, for example, 600 mm or less, 800 mm or less, or 1000 mm or less. The range of the dimension W of the metal plate 55A may be determined by a first group consisting of 300 mm, 400 mm, and 500 mm, and / or a second group consisting of 600 mm, 800 mm, and 1000 mm. The range of the dimension W of the metal plate 55A may be determined by a combination of any one of the values ​​included in the first group described above and any one of the values ​​included in the second group described above. The range of the dimension W of the metal plate 55A may be determined by a combination of any two of the values ​​included in the first group described above. The range of the dimension W of the metal plate 55A may be determined by a combination of any two of the values ​​included in the second group described above. The dimension W of the metal plate 55A may be, for example, 300 mm or more and 1000 mm or less, 300 mm or more and 800 mm or less, 300 mm or more and 600 mm or less, 300 mm or more and 500 mm or less, 300 mm or more and 400 mm or less, 400 mm or more and 1000 mm or less, 400 mm or more and 800 mm or less, 400 mm or more and 600 mm or less, 400 mm or more and 500 mm or less, 500 mm or more and 1000 mm or less, 500 mm or more and 800 mm or less, 500 mm or more and 600 mm or less, 600 mm or more and 1000 mm or less, 600 mm or more and 800 mm or less, or 800 mm or more and 1000 mm or less.

[0181] A sample 85 is prepared by cutting a part of the metal plate 55A. The sample 85 is taken out from the second region 55A2 of the metal plate 55A. The second region 55A2 is located between the first region 55A1 and the third region 55A3 in the width direction y. The first region 55A1, the second region 55A2, and the third region 55A3 are regions defined by virtually dividing the metal plate 55A. The first region 55A1, the second region 55A2, and the third region 55A3 are arranged in the width direction y from the first side edge 55x1 to the second side edge 55x2. The first region 55A1 includes the first side edge 55x1 and has a dimension of 100 mm in the width direction y. The third region 55A3 includes the second side edge 55x2 and has a dimension of 100 mm in the width direction y. When the dimension of the metal plate 55A in the width direction y is 500 mm, the second region 55A2 has a dimension of 300 mm in the width direction y.

[0182] Sample 85 is located at the center of second region 55A2 in width direction y. The distance from the tip of metal plate 55A to sample 85 in longitudinal direction x is 1000 mm. "Tip of metal plate 55A" means the tip of metal plate 55A in a rolled state.

[0183] The dimension Ky1 of the sample 85 in the width direction y is 50 mm, and the dimension Kx1 of the sample 85 in the longitudinal direction x is 60 mm.

[0184] 27 is a perspective view showing a process of measuring the reflectance of the sample 85. As described above, the first incident light L_ay travels in the width direction y in a plan view and is incident on the first surface 551. In the first measurement process of the first reflectance and the third reflectance, the first reflected light L_by that is reflected by the first surface 551 and travels in the width direction y in a plan view is detected. The first incident light L_ay and the first reflected light L_by travel within a first plane P1. The first plane P1 is parallel to the normal direction N and the width direction y of the first surface 551.

[0185] As described above, the second incident light L_ax travels in the longitudinal direction x in plan view and is incident on the first surface 551. In the second measurement process of the second reflectance and the fourth reflectance, the second reflected light L_bx that is reflected by the first surface 551 and travels in the longitudinal direction x in plan view is detected. The second incident light L_ax and the second reflected light L_bx travel within the second plane P2. The second plane P2 is parallel to the normal direction N and the longitudinal direction x of the first surface 551.

[0186] Fig. 28 is a cross-sectional view showing a first measurement step of measuring a first reflectance R1 and a third reflectance R3 of a sample 85. A measurement device 80 for measuring the reflectance includes a projector 81 and a receiver 82. The projector 81 emits light toward a first surface 551. The receiver 82 detects the light reflected by the first surface 551. In the step of measuring the first reflectance R1 and the third reflectance R3, as shown in Figs. 27 and 28, the emission and detection of light are performed on a first plane P1 in Fig. 27.

[0187] The projector 81 includes a light source that generates light. The light source is, for example, a halogen lamp. The light incident on the first surface 551 may be parallel light. In this case, the projector 81 may include an optical system for generating parallel light. The optical system includes, for example, a condenser lens, a collimator lens, an aperture, and a neutral density filter.

[0188] The receiver 82 includes a photodetector that detects the light reflected by the first surface 551. When the light reflected by the first surface 551 is parallel light, the receiver 82 may include an optical system for forming an image of the parallel light on the photodetector. The optical system includes, for example, a telescope lens.

[0189] The receiver 82 is movable within the first plane P1 so as to detect the first reflected light L_by having various emission angles. For example, the receiver 82 can move along a first rotation direction RDy within the first plane P1 with the light irradiation position P as the center. This allows the intensity of the first reflected light L_by to be detected at various emission angles, as shown in Fig. 29. In the graph shown in Fig. 29, the horizontal axis represents the emission angle of the first reflected light L_by, and the vertical axis represents the intensity of the first reflected light L_by.

[0190] 29, the intensity of the first reflected light L_by has a maximum value S1 at a first emission angle φ1. The maximum value of the intensity of the first reflected light L_by is also referred to as a first maximum intensity. The first reflectance R1 is calculated by dividing the first maximum intensity S1 by a reference intensity.

[0191] The reference intensity is calculated in a calibration process. In the calibration process, light is emitted from the projector 81 toward the receiver 82. That is, in a situation where the measurement device 80 is set to a transmission measurement mode, the light emitted from the projector 81 is directly incident on the receiver 82. In the transmission measurement mode, the incidence angle and the reception angle are both 0°. The intensity of the light detected by the receiver 82 in the calibration process is the reference intensity. The reference distance between the projector 81 and the receiver 82 is configured to be the same as the optical path length in the measurement process. In the measurement process, the measurement device 80 is set to a reflection measurement mode. The optical path length is the propagation distance of the light emitted from the projector 81, reflected by the surface of the metal plate 55, and reaching the receiver 82.

[0192] The receiver 82 measures the intensity of the first reflected light L_by while moving along the first rotation direction RDy so that the emission angle of the first reflected light L_by changes by 0.1°. The intensity of the first reflected light L_by decreases as it deviates from the first emission angle φ1. As described above, the third reflectance R3 is the reflectance of the first reflected light L_by having the third emission angle φ3. The third reflectance R3 is calculated by dividing the intensity of the first reflected light L_by having the third emission angle φ3 by the reference intensity.

[0193] The third exit angle φ3 is an exit angle that differs from the first exit angle φ1 by a first deviation angle φd1. There are two candidates for the third exit angle φ3. The first candidate is a 31st exit angle φ31 that is larger than the first exit angle φ1 by the first deviation angle φd1. The second candidate is a 32nd exit angle φ32 that is smaller than the first exit angle φ1 by the first deviation angle φd1.

[0194] When the intensity S31 of the first reflected light L_by having the 31st exit angle φ31 is greater than the intensity S32 of the first reflected light having the 32nd exit angle, the 31st exit angle φ31 is adopted as the third exit angle φ3. That is, the third reflectance R3 is calculated by dividing the intensity S31 of the first reflected light L_by having the 31st exit angle φ31 by the reference intensity.

[0195] When the intensity S32 of the first reflected light L_by having the 32nd exit angle φ32 is greater than the intensity S31 of the first reflected light having the 31st exit angle, the 32nd exit angle φ32 is adopted as the third exit angle φ3. That is, the third reflectance R3 is calculated by dividing the intensity S32 of the first reflected light L_by having the 32nd exit angle φ32 by the reference intensity.

[0196] 29, the intensity S32 of the first reflected light L_by having the 32nd emission angle φ32 is greater than the intensity S31 of the first reflected light having the 31st emission angle. Therefore, the third reflectance R3 is calculated by dividing the intensity S32 by the reference intensity.

[0197] Fig. 30 is a cross-sectional view showing a second measurement step of measuring the second reflectance R2 and the fourth reflectance R4 of the sample 85. In the step of measuring the second reflectance R2 and the fourth reflectance R4, as shown in Figs. 27 and 30, light emission and detection are performed in the second plane P2 in Fig. 27.

[0198] The receiver 82 is movable within the second plane P2 so as to detect the second reflected light L_bx having various emission angles. For example, the receiver 82 can move along the second rotation direction RDx within the second plane P2 with the light irradiation position P as the center. This allows the intensity of the second reflected light L_bx to be detected at various emission angles, as shown in Fig. 31. In the graph shown in Fig. 31, the horizontal axis represents the emission angle of the second reflected light L_bx, and the vertical axis represents the intensity of the second reflected light L_bx.

[0199] 31, the intensity of the second reflected light L_bx shows a maximum value S2 at the second emission angle φ2. The maximum value of the intensity of the second reflected light L_bx is also referred to as the second maximum intensity. The second reflectance R2 is calculated by dividing the second maximum intensity S2 by the above-mentioned reference intensity.

[0200] The receiver 82 measures the intensity of the second reflected light L_bx while moving along the second rotation direction RDx so that the emission angle of the second reflected light L_bx changes by 0.1°. The intensity of the second reflected light L_bx decreases as it deviates from the second emission angle φ2. As described above, the fourth reflectance R4 is the reflectance of the second reflected light L_bx having the fourth emission angle φ4. The fourth reflectance R4 is calculated by dividing the intensity of the second reflected light L_bx having the fourth emission angle φ4 by the reference intensity.

[0201] The fourth exit angle φ4 is an exit angle that differs from the second exit angle φ2 by the second deviation angle φd2. There are two candidates for the fourth exit angle φ4. The first candidate is the 41st exit angle φ41 that is larger than the second exit angle φ2 by the second deviation angle φd2. The second candidate is the 42nd exit angle φ32 that is smaller than the second exit angle φ2 by the second deviation angle φd2.

[0202] When the intensity S41 of the second reflected light L_bx having the 41st exit angle φ41 is greater than the intensity S42 of the second reflected light having the 42nd exit angle, the 41st exit angle φ41 is adopted as the fourth exit angle φ4. That is, the fourth reflectance R4 is calculated by dividing the intensity S41 of the second reflected light L_bx having the 41st exit angle φ41 by the reference intensity.

[0203] When the intensity S42 of the second reflected light L_bx having the 42nd exit angle φ42 is greater than the intensity S41 of the second reflected light having the 41st exit angle, the 42nd exit angle φ42 is adopted as the fourth exit angle φ4. That is, the fourth reflectance R4 is calculated by dividing the intensity S42 of the second reflected light L_bx having the 42nd exit angle φ42 by the reference intensity.

[0204] 31, the intensity S42 of the second reflected light L_bx having the 42nd emission angle φ42 is greater than the intensity S41 of the second reflected light having the 41st emission angle. Therefore, the fourth reflectance R4 is calculated by dividing the intensity S42 by the reference intensity.

[0205] FIG. 32 is a plan view showing the measurement positions of the sample 85. The first reflectance R1 and the third reflectance R3 are measured at the first measurement position Py1 and the second measurement position Py2, respectively. The average values ​​of the measurement results at the first measurement position Py1 and the second measurement position Py2 are adopted as the final first reflectance R1 and the third reflectance R3. The first measurement position Py1 and the second measurement position Py2 are symmetrical in the width direction y with respect to the center point 85c. The symbol Ky2 represents the distance between the center point of the first measurement position Py1 and the center point of the second measurement position Py2 in the width direction y. The distance Ky2 is 15 mm. The center point 85c is located at the center of the sample 85 in the plan view.

[0206] The second reflectance R2 and the fourth reflectance R4 are measured at the third measurement position Px1 and the fourth measurement position Px2, respectively. The average values ​​of the measurement results at the third measurement position Px1 and the fourth measurement position Px2 are adopted as the final second reflectance R2 and the fourth reflectance R4. The third measurement position Px1 and the fourth measurement position Px2 are symmetrical positions in the longitudinal direction x with respect to the center point 85c. The symbol Kx2 represents the distance between the center point of the third measurement position Px1 and the center point of the fourth measurement position Px2 in the longitudinal direction x. The distance Kx2 is 15 mm.

[0207] In FIG. 32, the symbols Sx and Sy represent the dimensions of the first measurement position Py1, the second measurement position Py2, the third measurement position Px1, and the fourth measurement position Px2 in the longitudinal direction x and the width direction y. The dimensions Sx and Sy correspond to the dimensions of the luminous flux of the incident light reaching the surface of the metal plate 55A. At the first measurement position Py1 and the second measurement position Py2, the dimension Sy is determined according to the aperture diameter of the diaphragm and the first specific incident angle θ1. When the aperture diameter of the diaphragm is 10.5 mm and the first specific incident angle θ1 is 20°, the dimension Sy at the first measurement position Py1 and the second measurement position Py2 is 11.2 mm. The dimension Sx at the first measurement position Py1 and the second measurement position Py2 is 10.5 mm. At the third measurement position Px1 and the fourth measurement position Px2, the dimension Sx is determined according to the aperture diameter of the diaphragm and the second specific incident angle θ2. When the aperture diameter of the diaphragm is 10.5 mm and the second specific incident angle θ2 is 20°, the dimension Sx at the third measurement position Px1 and the fourth measurement position Px2 is 11.2 mm. The dimension Sy at the third measurement position Px1 and the fourth measurement position Px2 is 10.5 mm.

[0208] The reflectance measuring step may include a verifying step of measuring the reflectance of a verifying sample. Fig. 33 is a diagram showing verifying samples taken out from a metal plate. In the example shown in Fig. 33, in addition to the above-mentioned sample 85, a first verifying sample 85A to a fourth verifying sample 85D are taken out from a metal plate 55A.

[0209] The first verification sample 85A and the second verification sample 85B are taken out from the second region 55A2, similarly to the sample 85. The first verification sample 85A and the second verification sample 85B are located at the center of the second region 55A2 in the width direction y. The first verification sample 85A is located downstream of the sample 85 in the longitudinal direction x. The downstream side is the side away from the tip of the metal plate 55A wound in a roll. The distance between the center point of the sample 85 and the center point of the first verification sample 85A in the longitudinal direction x is 1 m. The second verification sample 85B is located upstream of the sample 85 in the longitudinal direction x. The upstream side is the side approaching the tip of the metal plate 55A wound in a roll. The distance between the center point of the sample 85 and the center point of the second verification sample 85B in the longitudinal direction x is 1 m.

[0210] The reflectance and reflectance-related parameters of the first verification sample 85A and the second verification sample 85B fall within the above-mentioned numerical ranges defined for the reflectance and reflectance-related parameters of the sample 85. For example, the first ratio R3 / R1 and the second ratio R4 / R2 calculated from the first verification sample 85A and the second verification sample 85B are 0.40 or less. The verification using the first verification sample 85A and the second verification sample 85B ensures that the reflectance and reflectance-related parameters of the target metal plate 55A fall within the above-mentioned numerical ranges regardless of the position of the metal plate 55A in the longitudinal direction x.

[0211] The third verification sample 85C is taken out of the first region 55A1. The third verification sample 85C is located at the center of the first region 55A1 in the width direction y. The fourth verification sample 85D is taken out of the third region 55A3. The fourth verification sample 85D is located at the center of the third region 55A3 in the width direction y. The third verification sample 85C, the sample 85, and the fourth verification sample 85D are aligned along the width direction y. The distance between the center point of the sample 85 and the center point of the third verification sample 85C in the width direction y is 200 mm. The distance between the center point of the sample 85 and the center point of the fourth verification sample 85D in the width direction y is 200 mm.

[0212] The reflectance and reflectance-related parameters of the third verification sample 85C and the fourth verification sample 85D fall within the above-mentioned numerical ranges defined for the reflectance and reflectance-related parameters of sample 85. For example, the first ratio R3 / R1 and the second ratio R4 / R2 calculated from the third verification sample 85C and the fourth verification sample 85D are 0.40 or less. The verification using the third verification sample 85C and the fourth verification sample 85D ensures that the reflectance and reflectance-related parameters of the target metal plate 55A fall within the above-mentioned numerical ranges regardless of the position of the metal plate 55A in the width direction y.

[0213] Next, a method for manufacturing the metal plate 55A will be described. In the embodiment of the present disclosure, an example will be described in which the metal plate 55A is made of a rolled material of an iron alloy containing nickel.

[0214] First, iron, nickel and other raw materials are prepared. For example, the raw materials are prepared so that the ratio of iron and nickel to the total raw materials is about 64% by weight and about 36% by weight, respectively. Next, the raw materials are crushed as necessary, and then a melting process is performed in which the raw materials are melted in a melting furnace. For example, the raw materials are melted and mixed using gas discharge such as arc discharge. In this way, a base material for a metal plate can be obtained.

[0215] The temperature during melting is set depending on the raw material, and is, for example, 1500° C. or higher. The melting process may include a process of feeding aluminum, manganese, silicon, etc. into the melting furnace for deoxidization, dehydration, denitrification, etc. The melting process may be performed under a low pressure state lower than atmospheric pressure and in an atmosphere of an inert gas such as argon gas.

[0216] After the base material is removed from the melting furnace, a grinding step may be performed to scrape off the surface of the base material. This allows oxide coatings such as scale to be removed. The specific grinding method is not particularly limited. For example, a so-called grinding method may be adopted in which a grinding wheel is rotated to scrape off the surface of the base material. For example, a so-called pushing method may be adopted in which the base material is pushed into a cutting tool to scrape off the surface of the base material. The grinding step may be performed so that the thickness of the base material is uniform.

[0217] Next, a rolling step is performed to roll the base material made of an iron alloy containing nickel. This results in a metal plate extending in the longitudinal direction x. A number of rolling steps may be performed until a metal plate 55A having a final thickness T is obtained. FIG. 35 is a diagram showing the final rolling step for obtaining a metal plate 55A having a final thickness T.

[0218] In the rolling process, the metal sheet 55A is conveyed toward a rolling device 66 including a pair of rolling rolls 95a, 95b while applying a tensile force in the longitudinal direction x. The rolling rolls are also called work rolls. The metal sheet that reaches between the pair of rolling rolls 95a, 95b is rolled by the pair of rolling rolls 95a, 95b. As a result, the thickness of the metal sheet is reduced and the metal sheet is stretched along the longitudinal direction x. A recess such as a rolling streak 55f is formed on the surface of the metal sheet 55A. The metal sheet 55A may be wound around a core 96 to produce a wound body 58.

[0219] The specific configuration and procedure for carrying out the rolling process are not particularly limited. For example, the rolling process may include a hot rolling process and / or a cold rolling process. In the hot rolling process, the metal plate is rolled at a temperature equal to or higher than the temperature at which the crystal arrangement of the iron alloy constituting the metal plate is changed. In the cold rolling process, the metal plate is rolled at a temperature equal to or lower than the temperature at which the crystal arrangement of the iron alloy is changed. In addition, the direction in which the base material or the metal plate is passed between a pair of rolling rolls 95a, 95b is not limited to one direction.

[0220] In the rolling process, the pressure of the rolling actuator may be adjusted to adjust the shape of the metal sheet. Also, in addition to the rolling rolls 95a and 95b, the shape of the backup roll may be appropriately adjusted.

[0221] In the rolling process such as the cold rolling process, rolling oil may be supplied between the metal sheet and the rolling rolls 95a, 95b. This allows the temperature of the metal sheet to be controlled. Examples of the rolling oil include kerosene, neat oil, mineral oil, etc.

[0222] In the rolling process, the viscosity of the rolling oil may be adjusted. In order to suppress the formation of recesses such as the oil pits 55e and the rolling streaks 55f, it is preferable that the viscosity of the rolling oil is low.

[0223] In the rolling step, the rolling speed, that is, the conveying speed of the metal plate, may be adjusted. In order to suppress the formation of recesses such as oil pits 55e and rolling streaks 55f, a low rolling speed is preferable.

[0224] In the rolling process, the surface roughness of the rolling rolls may be adjusted. In order to suppress the formation of recesses such as oil pits 55e and rolling streaks 55f, it is preferable that the surface roughness of the rolling rolls is low.

[0225] The image of the metal plate 55A of Comparative Example 1 shown in Fig. 45, which will be described later, suggests that the more the rolling streaks 55f, the higher the first ratio R3 / R1. It is preferable to reduce the ratio of the rolling streaks 55f on the surface of the metal plate 55A. Adjustment of the viscosity of the rolling oil and the rolling speed is considered to be useful for reducing the ratio of the rolling streaks 55f.

[0226] An analysis step may be performed before, after, or during the rolling step to analyze the quality and characteristics of the metal sheet. For example, the metal sheet may be irradiated with fluorescent X-rays to analyze the composition. Also, the amount of thermal expansion and contraction of the metal sheet may be measured by thermomechanical analysis (TMA).

[0227] Thereafter, in order to remove residual stress accumulated in the metal plate 55A by rolling, an annealing step may be performed using an annealing device 97 as shown in FIG. 36 to anneal the metal plate 55A. The annealing step may be performed while pulling the metal plate 55A in the longitudinal direction x as shown in FIG. 36. That is, the annealing step may be performed as continuous annealing while being transported, rather than so-called batch-type annealing. In this case, it is preferable to set the temperature and transport speed so as to suppress the occurrence of deformation such as buckling and bending in the metal plate 55A. By performing the annealing step, it is possible to obtain the metal plate 55A from which residual strain has been removed to some extent. Note that FIG. 36 shows an example in which the metal plate 55A is transported in the horizontal direction during the annealing step, but this is not limited to this. The metal plate 55A may be transported in other directions, such as the vertical direction, during the annealing step.

[0228] The conditions of the annealing step are appropriately set according to the thickness and rolling reduction of the metal sheet 55A, and for example, the annealing step is performed within a range of 500° C. to 600° C. for 30 to 90 seconds. Note that the number of seconds above represents the time required for the metal sheet 55A to pass through a space adjusted to the annealing temperature in the annealing device 97. The annealing temperature may be set so as not to cause softening of the metal sheet 55A.

[0229] The lower limit of the annealing temperature may be lower than the above-mentioned 500°C. For example, the annealing temperature may be 400°C or higher, or 450°C or higher. The upper limit of the annealing temperature may be higher than the above-mentioned 600°C. For example, the temperature of the annealing step may be 700°C or lower, or 650°C or lower. The temperature range of the annealing step may be determined by a combination of any one of the above-mentioned multiple upper limit candidate values ​​and any one of the above-mentioned multiple lower limit candidate values. For example, the temperature of the annealing step may be 400°C or higher and 700°C or lower, or 450°C or higher and 650°C or lower. The temperature range of the annealing step may be determined by a combination of any two of the above-mentioned multiple upper limit candidate values. For example, the temperature of the annealing step may be 650°C or higher and 700°C or lower. The temperature range of the annealing step may be determined by a combination of any two of the above-mentioned multiple lower limit candidate values. For example, the temperature of the annealing step may be 400°C or higher and 450°C or lower.

[0230] The time of the annealing step may be 40 seconds or more, or 50 seconds or more. The lower limit of the time of the annealing step may be shorter than the above-mentioned 30 seconds. For example, the time of the annealing step may be 10 seconds or more, or 20 seconds or more. The time of the annealing step may be 80 seconds or less, 70 seconds or less, or 60 seconds or less. The upper limit of the time of the annealing step may be longer than the above-mentioned 90 seconds. For example, the time of the annealing step may be 100 seconds or less. The range of the time of the annealing step may be determined by a combination of any one of the above-mentioned multiple upper limit candidate values ​​and any one of the above-mentioned multiple lower limit candidate values. For example, the time of the annealing step may be 10 seconds or more and 100 seconds or less, 20 seconds or more and 90 seconds or less, 30 seconds or more and 80 seconds or less, 40 seconds or more and 70 seconds or less, or 50 seconds or more and 60 seconds or less. The range of the time of the annealing step may be determined by a combination of any two of the above-mentioned multiple upper limit candidate values. For example, the time of the annealing step may be 90 seconds or more and 100 seconds or less. The time range of the annealing step may be determined by a combination of any two of the above-mentioned multiple lower limit candidate values. For example, the time of the annealing step may be 10 seconds or more and 20 seconds or less.

[0231] Preferably, the annealing step is performed in a non-reducing atmosphere or an inert gas atmosphere. Here, the non-reducing atmosphere means an atmosphere that does not contain a reducing gas such as hydrogen. "Does not contain a reducing gas" means that the concentration of the reducing gas such as hydrogen is 10% or less. In the annealing step, the concentration of the reducing gas may be 8% or less, 6% or less, 4% or less, 2% or less, or 1% or less. Also, the inert gas atmosphere means an atmosphere in which the concentration of an inert gas such as argon gas, helium gas, or nitrogen gas is 90% or more. In the annealing step, the concentration of the inert gas may be 92% or more, 94% or more, 96% or more, 98% or more, or 99% or more. By performing the annealing step in a non-reducing atmosphere or an inert gas atmosphere, it is possible to suppress the generation of nickel compounds such as nickel hydroxide on the surface layer of the metal plate 55A. The annealing device 97 may have a mechanism for monitoring the concentration of the inert gas or a mechanism for adjusting the concentration of the inert gas.

[0232] A cleaning step for cleaning the metal plate 55A may be performed before the annealing step. This makes it possible to prevent foreign matter from adhering to the surface of the metal plate 55A during the annealing step. For example, a hydrocarbon-based liquid can be used as a cleaning liquid for cleaning.

[0233] Thereafter, a slitting process may be performed in which both ends of the metal plate 55A obtained by the rolling process are cut off over a predetermined range in the width direction so that the width of the metal plate 55A falls within a predetermined range. This slitting process is performed to remove cracks that may occur at both ends of the metal plate 55A due to rolling. By performing such a slitting process, it is possible to prevent the phenomenon in which the metal plate 55A breaks, that is, so-called plate breaks, from occurring starting from the cracks.

[0234] The width of the portion cut off in the slitting step may be adjusted so that the shape of the metal plate 55A after the slitting step is symmetrical in the width direction. The slitting step may be performed before the above-mentioned annealing step.

[0235] According to the present embodiment, by using metal plate 55A including a surface that satisfies the above-mentioned conditions regarding the first and second ratios of reflectance, it is possible to suppress the occurrence of fringes 614 in resist pattern 611. Therefore, first recess 56a of through hole 56 of mask 50 has high dimensional accuracy.

[0236] Next, a method for inspecting the metal plate 55A will be described. The inspection method may be performed as one step of a manufacturing method for the metal plate 55A. The inspection method may be performed to select the metal plates 55A that are on sale.

[0237] The inspection method for the metal plate 55A may include a measurement step, a first judgment step, and a second judgment step. In the measurement step, the above-mentioned first reflectance R1, second reflectance R2, third reflectance R3, and fourth reflectance R4 of the metal plate 55A are measured. In the first judgment step, it is judged whether the first ratio R3 / R1 is equal to or less than a first threshold. The first threshold is, for example, 0.40. The first threshold may be 0.30 or 0.20. In the second judgment step, it is judged whether the second ratio R4 / R2 is equal to or less than a second threshold. The second threshold is, for example, 0.40. The second threshold may be 0.30 or 0.20.

[0238] The inspection method for the metal plate 55A may include a third determination step. In the third determination step, it is determined whether the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 is equal to or less than a third threshold. The third threshold is, for example, 0.30. The third threshold may be 0.20 or 0.15.

[0239] The inspection method for the metal plate 55A may include a fourth determination step. In the fourth determination step, it is determined whether the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 is equal to or greater than a fourth threshold value. The fourth threshold value is, for example, 0.02. The fourth threshold value may be 0.05 or 0.10.

[0240] The measuring step is preferably performed at least at a first specific incident angle θ1 and a second specific incident angle θ2 of 20°. The measuring step may be further performed at a first specific incident angle θ1 and a second specific incident angle θ2 other than 20°. For example, the measuring step may be further performed at a first specific incident angle θ1 and a second specific incident angle θ2 of 45°.

[0241] The first to fourth judgment steps are preferably performed based on the results of the measurement steps at the first specific incident angle θ1 and the second specific incident angle θ2 of 20°. The first to fourth judgment steps may be further performed based on the results of the measurement steps at the first specific incident angle θ1 and the second specific incident angle θ2 other than 20°. For example, the first to fourth judgment steps may be further performed based on the results of the measurement steps at the first specific incident angle θ1 and the second specific incident angle θ2 of 45°. However, as described above, the diffused light generated on the surface of the metal plate 55A when the incident angle θ is 45° is different from the diffused light generated on the surface of the metal plate 55A when the incident angle θ is 20°. Therefore, the metal plate 55A that is determined to be acceptable in the judgment step based on the results of the measurement steps at the first specific incident angle θ1 and the second specific incident angle θ2 of 45° does not necessarily exhibit excellent characteristics.

[0242] Next, an example of a method for manufacturing the organic device 100 will be described.

[0243] First, a substrate 110 on which a first electrode 120 is formed is prepared. The first electrode 120 is formed, for example, by forming a conductive layer constituting the first electrode 120 on the substrate 110 by a sputtering method or the like, and then patterning the conductive layer by a photolithography method or the like. An insulating layer 160 located between two adjacent first electrodes 120 may be formed on the substrate 110.

[0244] Next, the organic layer 130 including the first organic layer 130A, the second organic layer 130B, etc. is formed on the first electrode 120. The first organic layer 130A is formed by a deposition method using a first mask 50 having a through hole 56 corresponding to the first organic layer 130A. The second organic layer 130B is also formed by a deposition method using a second mask 50 having a through hole 56 corresponding to the second organic layer 130B. The third organic layer 130C is also formed by a deposition method using a third mask 50 having a through hole 56 corresponding to the third organic layer 130C.

[0245] Subsequently, a step of forming the second electrode 140 on the organic layer 130 is performed. In this manner, the organic device 100 can be obtained.

[0246] According to the present embodiment, as described above, it is possible to suppress the occurrence of fringes in the first resist pattern 611. Therefore, the first recess 56a of the through hole 56 of the mask 50 has high dimensional accuracy. This allows the accuracy of the deposition layer of the organic device 100 to be improved. EXAMPLES

[0247] Next, the embodiments of the present disclosure will be described more specifically with reference to examples. However, the embodiments of the present disclosure are not limited to the description of the following examples as long as they do not depart from the gist of the disclosure.

[0248] Example 1 A metal plate 55A made of an iron alloy containing 36 mass% nickel and the remainder iron and unavoidable impurities was prepared. The metal plate 55A had a thickness T of 10 μm and a dimension of 500 mm in the width direction y. The manufacturing method of the metal plate 55A included the above-mentioned rolling step and annealing step.

[0249] An inspection method for inspecting the metal plate 55A was carried out. The inspection method included the above-mentioned measuring step, the first judgment step, the second judgment step, and the third judgment step.

[0250] In the measurement step, the first reflectance R1, the second reflectance R2, the third reflectance R3, and the fourth reflectance R4 of the metal plate 55A were measured by a goniophotometer. As the goniophotometer, a GP-200 manufactured by Murakami Color Laboratory Co., Ltd. was used.

[0251] The measurement process included the above-mentioned calibration process, first measurement process, and second measurement process. The calibration process is performed in the transmission mode of the GP-200. In the transmission mode, light emitted from the projector 81 is directly incident on the receiver 82. The projector 81 includes an aperture and a neutral density filter. In the calibration process, the "HIGH VOLT" value of the GP-200 is set so that the maximum value of the light intensity calculated by the GP-200 is 85%. The specific settings of the GP-200 were as follows: Light source: 12V, 50W halogen lamp Measurement mode: Through-pass mode ·Incidence angle: 0° Receiver 82 receiving angle: -5.0°~+5.0°, 0.1° intervals Projector 81 aperture diameter: 10.5mm Receiver 82 aperture diameter: 9.1mm Sensitivity: 950 HIGH VOLT:474 Neutral density filters: a combination of 1 / 10 and 1 / 100 neutral density filters

[0252] In the calibration process, the maximum light intensity calculated by the GP-200 may deviate from 85%. If the maximum value deviates from 85%, the reference intensity is set taking the deviation into account. For example, if the maximum light intensity is 84.9% and the neutral density filter is a combination of a 1 / 10 neutral density filter and a 1 / 100 neutral density filter, the reference intensity is set to 84900.

[0253] 37 is a diagram showing the measurement results of the light intensity in the calibration process. "Start" is the spectrum measured at the start of the calibration process. "End" is the spectrum measured at the end of the calibration process.

[0254] The first and second measurement steps are performed in the reflection mode of GP-200. In the first and second measurement steps, a sample 85 of a metal plate 55A is placed on the sample stage of GP-200. In Example 1 and Examples 4 and 8 described below, a sample stage including a groove for attracting the sample 85 was used. The diameter of the groove was 30 mm. In Examples 2, 3, 5 to 7, 9 to 11 and Comparative Examples 1 to 6 described below, the sample 85 attached to a magnet was placed on the sample stage.

[0255] In the first and second measurement steps, the value of "HIGH VOLT" set in the calibration step was used. The configuration of the neutral density filter was adjusted so that the maximum value of the light intensity calculated by the GP-200 was 10% or more and 90% or less. In Example 1, Examples 2, 3, 5 to 11 described later, and Comparative Examples 1, 3 to 6, the neutral density filter is a combination of a 1 / 2 neutral density filter and a 1 / 100 neutral density filter. In Example 4 described later, the neutral density filter is a combination of a 1 / 10 neutral density filter and a 1 / 100 neutral density filter. In Comparative Example 2 described later, the neutral density filter is a 1 / 100 neutral density filter.

[0256] The specific settings of the GP-200 in the first and second measurement steps were as follows: Light source: 12V, 50W halogen lamp Measurement mode: Reflection mode ·Incidence angle: 20° Receiver 82 light receiving angle: 5.0°~35.0°, 0.1° interval Tilt angle: 0° Projector 81 aperture diameter: 10.5mm Receiver 82 aperture diameter: 9.1mm Sensitivity: 950 HIGH VOLT:474

[0257] The results of the first measurement step are shown in Figure 38A. In the first measurement step, the first reflectance R1 and the third reflectance R3 were measured at the first measurement position Py1 and the second measurement position Py2, respectively. "Ex.1" means Example 1. "Average" means the average value of the first ratio R3 / R1 at the first measurement position Py1 and the first ratio R3 / R1 at the second measurement position Py2.

[0258] The results of the second measurement step are shown in Fig. 38B. In the second measurement step, the second reflectance R2 and the fourth reflectance R4 were measured at the third measurement position Px1 and the fourth measurement position Px2, respectively. "Average" refers to the average of the second ratio R4 / R2 at the third measurement position Px1 and the second ratio R4 / R2 at the fourth measurement position Px2.

[0259] FIG. 39 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step, and the spectrum of the second reflected light L_bx detected in the second measurement step.

[0260] After the measurement step, the first, second and third determination steps were carried out. The results of these determination steps are shown in Figure 38C. The value of the first ratio R3 / R1 shown in Figure 38C is the average value shown in Figure 38A. The value of the second ratio R4 / R2 shown in Figure 38C is the average value shown in Figure 38B.

[0261] In the "First Judgment" and "Second Judgment" columns, "A" means that the first ratio R3 / R1 or the second ratio R4 / R2 was 0.30 or less. In the "First Judgment" and "Second Judgment" columns, "B" means that the first ratio R3 / R1 or the second ratio R4 / R2 was more than 0.30 and 0.40 or less. In the "First Judgment" and "Second Judgment" columns, "C" means that the first ratio R3 / R1 or the second ratio R4 / R2 was more than 0.40.

[0262] In the "Third Judgment" column, "A" means that the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 was 0.20 or less. In the "Third Judgment" column, "B" means that the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 was more than 0.20 and 0.40 or less. In the "Third Judgment" column, "C" means that the absolute value of the difference between the first ratio R3 / R1 and the second ratio R4 / R2 was more than 0.40.

[0263] In the "Final Decision" column, "A" means that the results of the first, second, and third decisions were all "A." In the "Final Decision" column, "B" means that the results of the first, second, and third decisions included at least one "B" but no "C." In the "Final Decision" column, "C" means that the results of the first, second, and third decisions included at least one "C."

[0264] A first evaluation and a second evaluation were carried out on the processing accuracy of metal plate 55A. The results of the first evaluation and the second evaluation are shown in Fig. 38C. In the first evaluation, width W2 of fringe 614 of first resist pattern 611 formed on the surface of metal plate 55A was measured. In the second evaluation, the size of first opening 612 of first resist pattern 611 was measured.

[0265] In the first and second evaluations, a first resist pattern 611 and a second resist pattern 621 were formed on the metal plate 55A by carrying out the resist forming step, the exposure step, and the development step shown in Fig. 12 to Fig. 14B. The wavelength of the exposure light L1, L2 of the exposure device 72 was 365 nm, and the declination angle was 2.0° or less. Then, a heating step was carried out in which the resist patterns 611, 621 were heated at a processing temperature of 200°C or more.

[0266] A scanning electron microscope was used to observe the sample including the first resist pattern 611 in plan view. The scanning electron microscope used was a ZEISS ULTRA55. The observation conditions were as follows: Acceleration voltage: 1.5kV Working distance: 3.0mm Aperture: 30μm High Current Magnification: 800x to 3000x

[0267] The width W2 of the fringe 614 of the first resist pattern 611 was calculated based on the planar image of the first resist pattern 611. The width W2 was calculated by averaging W21, W22, W23, and W24 shown in Fig. 24. The width W2 was 0.40 µm.

[0268] Based on the planar image of the first resist pattern 611, the dimensions of the first openings 612 of the first resist pattern 611 on the surface 615 were calculated. Specifically, the dimensions of the first openings 612 were measured in the first arrangement direction E1, the second arrangement direction E2, the third arrangement direction E3, and the fourth arrangement direction E4 shown in FIG. 14B. The dimensions of 30 first openings 612 were measured. Therefore, the number of measured values ​​of the dimensions of the first openings 612 is 120. Next, the average value AVE and the standard deviation σ of the measured dimensions of the 120 were calculated. In the "Resolution" column of FIG. 38C, "OK" means that the following conditions (1) and (2) were satisfied. In the "Resolution" column of FIG. 38C, "NG" means that at least one of the following conditions (1) and (2) was not satisfied. Condition (1): The difference between the average value AVE and the design value is 1.8 μm or less Condition (2): 2σ is 1.5 μm or less The design value of the dimension of the first opening 612 was 42 μm.

[0269] (Examples 2 to 11, Comparative Examples 1 to 6, and Example 12) A metal plate 55A was prepared, which was made of an iron alloy containing 36 mass% nickel and the remainder being iron and unavoidable impurities. The metal plates 55A of Examples 2 to 11, Comparative Examples 1 to 6, and Example 12 differ from the metal plate 55A of Example 1 in at least one of the thickness T and the conveying speed in the rolling process.

[0270] The same inspection method as in Example 1 described above was performed on metal plates 55A of Examples 2 to 11, Comparative Examples 1 to 6, and Example 12. The result of the first measurement step is shown in FIG. 38A. The result of the second measurement step is shown in FIG. 38B. The results of the first judgment step, second judgment step, and third judgment step are shown in FIG. 38C. "Comp.1" means Comparative Example 1.

[0271] FIG. 40 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step of Example 4, and the spectrum of the second reflected light L_bx detected in the second measurement step of Example 4. FIG. 41 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step of Example 6, and the spectrum of the second reflected light L_bx detected in the second measurement step of Example 6. FIG. 42 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step of Example 8, and the spectrum of the second reflected light L_bx detected in the second measurement step of Example 8. FIG. 43 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step of Comparative Example 1, and the spectrum of the second reflected light L_bx detected in the second measurement step of Comparative Example 1. FIG. 44 is a diagram showing the spectrum of the first reflected light L_by detected in the first measurement step of Comparative Example 4, and the spectrum of the second reflected light L_bx detected in the second measurement step of Comparative Example 4.

[0272] The same first evaluation as in the above-mentioned Example 1 was performed on the metal plates 55A of Examples 4 and 8 and Comparative Examples 1 and 4. The same second evaluation as in the above-mentioned Example 1 was performed on the metal plates 55A of Examples 2 to 11 and Comparative Examples 1 to 6. The results of the first and second evaluations are shown in FIG.

[0273] In Examples 1 to 11 and 12, the results of the first judgment and the second judgment were "A" or "B." In Examples 1 to 11, the result of the second evaluation regarding the resolution of the resist pattern was "OK." In Comparative Examples 1 to 6, at least one of the results of the first judgment or the second judgment was "C." In Comparative Examples 1 to 6, the result of the second evaluation regarding the resolution of the resist pattern was "NG." It can be seen that the first ratio R3 / R1 and the second ratio R4 / R2 are useful indexes regarding the metal plate 55A used to manufacture a mask.

[0274] 45 is an image showing the results of observing, using a scanning electron microscope, the surface of metal plate 55A of Comparative Example 1. The surface of metal plate 55A of Comparative Example 1 contained more rolling streaks than oil pits.

[0275] (Verification sample) Regarding the metal plate 55A of Examples 1, 4, and 8, the reflectance of the first verification sample 85A to the fourth verification sample 85D shown in FIG. 33 was measured. The result of the first measurement step is shown in FIG. 46A. In the first measurement step, the first reflectance R1 and the third reflectance R3 of the first verification sample 85A to the fourth verification sample 85D were measured at the first measurement position Py1 and the second measurement position Py2, respectively. The result of the second measurement step is shown in FIG. 46B. In the second measurement step, the second reflectance R2 and the fourth reflectance R4 of the first verification sample 85A to the fourth verification sample 85D were measured at the third measurement position Px1 and the fourth measurement position Px2, respectively. After the measurement step, the first judgment step, the second judgment step, and the third judgment step were performed. The results of these judgment steps are shown in FIG. 46C.

[0276] In Figures 46A, 46B, and 46C, "Samp." refers to sample 85 in Figure 33. The measurement results and judgment results of "Samp." are the same as the measurement results and judgment results of Examples 1, 4, and 8 shown in Figures 38A to 38C. "Ver.1" to "Ver.4" refer to first verification sample 85A to fourth verification sample 85D in Figure 33.

[0277] 46C, the measurement results of the first verification sample 85A to the fourth verification sample 85D were almost the same as the measurement result of sample 85. Specifically, the absolute values ​​of the differences between the values ​​of the first ratio R3 / R1 and the second ratio R4 / R2 of the first verification sample 85A to the fourth verification sample 85D and the values ​​of the first ratio R3 / R1 and the second ratio R4 / R2 of sample 85 were 0.020 or less. The judgment results of the first verification sample 85A to the fourth verification sample 85D were the same as the judgment result of sample 85.

[0278] (Change in incident angle) A measurement step was carried out to measure the reflectance of the metal plate 55A of Examples 1 to 12 and Comparative Examples 1 to 6 at an incident angle of 45°. The specific settings of the GP-200 in the first measurement step and the second measurement step were as follows. Light source: 12V, 50W halogen lamp Measurement mode: Reflection mode ·Incidence angle: 45° Receiver 82 light receiving angle: 30.0°~60.0°, 0.1° intervals Tilt angle: 0° Projector 81 aperture diameter: 10.5mm Receiver 82 aperture diameter: 9.1mm Sensitivity: 950 HIGH VOLT:444

[0279] The results of the first measurement step are shown in Figure 48A, and the results of the second measurement step are shown in Figure 48B.

[0280] After the measurement step, the first, second and third judgment steps were carried out. The results of these judgment steps are shown in FIG. 48C. The value of the first ratio R3 / R1 shown in FIG. 48C is the average value shown in FIG. 48A. The value of the second ratio R4 / R2 shown in FIG. 48C is the average value shown in FIG. 48B. The judgment criteria of "A", "B" and "C" in the columns "First Judgment", "Second Judgment", "Third Judgment" and "Final Judgment" are the same as the judgment criteria for the case of an incident angle of 20°.

[0281] As shown in FIG. 48C, the final judgment results of the metal plates 55A of Examples 1 to 12 in the case of an incident angle of 45° were "A", similar to the result in the case of an incident angle of 20°. The final judgment results of the metal plates 55A of Comparative Examples 2 to 4 in the case of an incident angle of 45° were "C", similar to the result in the case of an incident angle of 20°. On the other hand, the final judgment results of the metal plates 55A of Comparative Examples 1 and 5 to 6 in the case of an incident angle of 45° were "B", different from the result in the case of an incident angle of 20°. It can be seen that the metal plates 55A judged to be pass when the incident angle is 45° do not necessarily exhibit excellent characteristics.

[0282] Fig. 49A is a table showing the regular reflectance of the metal plates of Examples 1 to 12 and Comparative Examples 1 to 6. The regular reflectance when the incident angle is 20° is the average value of the first reflectance R1 at the first measurement position Py1 and the first reflectance R1 at the second measurement position Py2 shown in Fig. 38A, and the second reflectance R2 at the third measurement position Px1 and the second reflectance R2 at the fourth measurement position Px2 shown in Fig. 38B. The regular reflectance when the incident angle is 45° is the average value of the first reflectance R1 at the first measurement position Py1 and the first reflectance R1 at the second measurement position Py2 shown in Fig. 48A, and the second reflectance R2 at the third measurement position Px1 and the second reflectance R2 at the fourth measurement position Px2 shown in Fig. 48B.

[0283] Figures 49B and 49C are graphs showing the relationship between specular reflectance when the angle of incidence is 20° and specular reflectance when the angle of incidence is 45°. The horizontal axis of the graph indicates specular reflectance when the angle of incidence is 20°, and the vertical axis of the graph indicates specular reflectance when the angle of incidence is 45°. The horizontal axis of the graph in Figure 49B ranges from 0% to 35%. The horizontal axis of the graph in Figure 49C ranges from 0% to 20%.

[0284] It is believed that there is some correlation between the specular reflectance at an incident angle of 20° and the specular reflectance at an incident angle of 45°. However, as shown in Figure 49C, when the specular reflectance is low, for example, when the specular reflectance at an incident angle of 20° is 20% or less, the degree of correlation is small.

Claims

1. A metal plate used to manufacture a mask, A surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle, the first reflected light is a first incident light that travels in the width direction in a plan view and is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view and is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, The first specific incident angle and the second specific incident angle are 20°; a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; A metal plate, wherein a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

2. 2. The metal plate of claim 1, wherein the first deviation angle and the second deviation angle are 2.5 degrees.

3. an absolute value of a difference between the first specific incident angle and the first exit angle is 0.30° or less; The metal plate according to claim 1 , wherein an absolute value of a difference between the second specific incident angle and the second exit angle is 0.30° or less.

4. The metal plate according to any one of claims 1 to 3, wherein the surface of the metal plate includes a plurality of rolling streaks extending in the longitudinal direction and a plurality of oil pits.

5. The metal plate according to any one of claims 1 to 3, wherein the metal plate has a thickness of 80 µm or less.

6. The metal plate according to any one of claims 1 to 3, wherein the metal plate comprises an iron alloy containing 34% by mass or more and 38% by mass or less of nickel.

7. The metal plate according to any one of claims 1 to 3, wherein an absolute value of a difference between the first ratio and the second ratio is 0.20 or less.

8. The metal plate according to any one of claims 1 to 3, wherein the first ratio and the second ratio are 0.30 or less.

9. The metal sheet of claim 8 , wherein the second ratio is less than or equal to 0.

20.

10. The metal plate has a regular reflectance of 35.0% or less, The metal plate according to any one of claims 1 to 3, wherein the regular reflectance is an average value of the first reflectance and the second reflectance.

11. 1. A method for inspecting a metal plate used for manufacturing a mask, comprising the steps of: The metal plate has a surface having a longitudinal direction and a width direction perpendicular to the longitudinal direction, The inspection method includes: measuring a first reflectance, a second reflectance, a third reflectance, and a fourth reflectance of the metal plate; a first determination step of determining whether a first ratio, which is a ratio of the third reflectance to the first reflectance, is equal to or smaller than a first threshold value; a second determination step of determining whether a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is equal to or smaller than a second threshold value; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle, the first reflected light is a first incident light that travels in the width direction in a plan view and is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a first maximum intensity; the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view and is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a second maximum intensity; The fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle.

12. A method for manufacturing a metal plate used for manufacturing a mask, comprising the steps of: A rolling step of rolling the metal plate to reduce the thickness of the metal plate, The rolled metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle, the first reflected light is a first incident light that travels in the width direction in a plan view and is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a maximum intensity, the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view and is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a maximum intensity, the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; A method for manufacturing a metal plate, wherein a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

13. A mask, A metal plate; A plurality of through holes penetrating the metal plate, The metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle, the first reflected light is a first incident light that travels in the width direction in a plan view and is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a maximum intensity, the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view and is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a maximum intensity, the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, The first specific incident angle and the second specific incident angle are 20°; a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; A mask, wherein a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

14. The metal plate includes a first surface and a second surface located opposite to the first surface, the through hole includes a plurality of first recesses located on the first surface, a plurality of second recesses located on the second surface, and a connection portion connecting the first recesses and the second recesses, In a plan view, a dimension of the second recess is larger than a dimension of the first recess; 14. The mask of claim 13, wherein the first surface is the surface having the first reflectivity, the second reflectivity, the third reflectivity, and the fourth reflectivity.

15. The through hole has a first through dimension in the width direction and a second through dimension in the longitudinal direction; 15. The mask of claim 14, wherein a ratio of the first penetration dimension to the second penetration dimension is greater than or equal to 0.

98.

16. A mask according to any one of claims 13 to 15, A mask device comprising: a mask support for supporting the mask.

17. A method for manufacturing a mask, comprising the steps of: Providing a metal plate; A processing step of forming a plurality of through holes in the metal plate, The metal plate has a surface having a longitudinal direction of the metal plate and a width direction perpendicular to the longitudinal direction, the surface has a first reflectivity, a second reflectivity, a third reflectivity, and a fourth reflectivity; the first reflectance is a reflectance of a first reflected light having a first exit angle; the third reflectance is a reflectance of the first reflected light having a third exit angle, the first reflected light is a first incident light that travels in the width direction in a plan view and is incident on the surface at a first specific incident angle, and is reflected by the surface; the first exit angle is an exit angle at which the first reflected light exhibits a maximum intensity, the third exit angle is an exit angle that differs from the first exit angle by a first deviation angle, the second reflectance is a reflectance of a second reflected light having a second exit angle; the fourth reflectance is a reflectance of the second reflected light having a fourth exit angle, the second reflected light is a second incident light that travels in the longitudinal direction in a plan view and is incident on the surface at a second specific incident angle, and is reflected by the surface; the second exit angle is an exit angle at which the second reflected light exhibits a maximum intensity, the fourth exit angle is an exit angle that differs from the second exit angle by a second deviation angle, a first ratio which is a ratio of the third reflectance to the first reflectance is 0.40 or less; a second ratio, which is a ratio of the fourth reflectance to the second reflectance, is 0.40 or less.

18. The processing step includes: a resist forming step of forming a resist layer on the surface of the metal plate; an exposure step of exposing the resist layer to light; a developing step of developing the exposed resist layer to form a resist pattern; The method for manufacturing a mask according to claim 17, further comprising: an etching step of etching the metal plate.

19. the resist pattern includes an opening and a wall surface facing the opening, The width of the fringe of the wall surface in a plan view is 1.00 μm or less, the fringe projects toward the center of the opening at the corners; The method for manufacturing a mask according to claim 18 , wherein the corner is a portion where a surface of the resist pattern facing the metal plate and the wall surface are connected.

Citation Information

Patent Citations

  • Method of forming casein resist pattern

    JP2000178765A

  • Metal mask substrate, metal mask substrate control method, metal mask, and metal mask production method

    WO2017013904A1

  • Metal mask substrate for vapor deposition, metal mask for vapor deposition, production method for metal mask substrate for vapor deposition, and production method for metal mask for vapor deposition

    WO2017014172A1

  • Metal plate for producing vapor deposition masks, inspection method for metal plates, production method for metal plates, vapor deposition mask, vapor deposition mask device, and production method for vapor deposition masks

    WO2019098168A1