Back grinding tape
The backgrind tape addresses the challenge of balancing embedding and cuttability by using a specific intermediate and adhesive layer design, ensuring effective adhesion and easy peeling without damage.
Patent Information
- Application Number
- JP2023068637
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Existing adhesive tapes for semiconductor wafers struggle to balance excellent embedding properties for uneven surfaces with good cuttability, often leading to threading and damage during the back-grinding process.
A backgrind tape comprising a base material, an intermediate layer with nanoindentation hardness of 0.001 MPa to 0.200 MPa and thickness of 50 μm or more, and an adhesive layer with nanoindentation hardness of 0.001 MPa to 0.080 MPa and thickness of 50 μm or more, with specific hardness-thickness products and unloading curve displacements to ensure both embedding and cuttability.
The tape achieves both excellent unevenness embedding properties and cuttability, reducing threading and damage to semiconductor wafers during peeling.
Smart Images

Figure 2024154677000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a backgrind tape. [Background technology]
[0002] Semiconductor wafers are used for various purposes such as personal computers, smartphones, and automobiles. In the processing of semiconductor wafers, adhesive tapes are used to protect the surface during processing. In recent years, the miniaturization and high functionality of large-scale integrated circuits (LSIs) have progressed, and the surface structure of wafers has become more complex. Specifically, the three-dimensional structure of the wafer surface has become more complex due to solder bumps, etc. Therefore, adhesive tapes used in semiconductor processing are required to be able to embed the unevenness of the wafer surface and to have strong adhesive properties. Adhesive tapes used in the back-grinding process of semiconductor wafers are required to hold the semiconductor wafer properly during the back-grinding process and to be easily peeled off after the back-grinding process. Since the thickness of the semiconductor wafer that has been subjected to the back-grinding process becomes significantly thinner, the back-grinding tape is required to be able to be peeled off without leaving any glue residue or damaging the semiconductor wafer.
[0003] In recent years, semiconductor wafers have been thinned as each product becomes smaller and thinner. In a wafer processed to be thin, if the adhesive strength of the adhesive tape is too high, the wafer may be damaged when the adhesive tape is peeled off. Therefore, in order to prevent adhesive residue on the adherend and damage to the wafer when peeled off, an adhesive tape using an ultraviolet-curing adhesive has been proposed (for example, Patent Documents 1 and 2). In addition, an adhesive tape with excellent unevenness embedding properties has been proposed as an adhesive tape suitable for processing semiconductor wafers having uneven structures such as bumps (for example, Patent Document 3). However, an adhesive tape with excellent unevenness embedding properties may cause stringing of the adhesive layer during the cutting process after tape application, and the semiconductor wafer may be damaged during the backgrinding process and the peeling process after processing. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-017758 A [Patent Document 2] JP 2013-213075 A [Patent Document 3] Patent Publication No. 2022-121480 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide a backgrind tape that is capable of both excellent embedding properties and excellent cutting properties. [Means for solving the problem]
[0006] 1. A backgrind tape according to an embodiment of the present invention includes a substrate, an intermediate layer, and an adhesive layer, the intermediate layer having a nanoindentation hardness (25° C.) of 0.001 MPa to 0.200 MPa, the adhesive layer having a nanoindentation hardness (25° C.) of 0.001 MPa to 0.080 MPa, at least one of the intermediate layer and the adhesive layer having a thickness of 50 μm or more, and the unloading curve displacement of the layer having a thickness of 50 μm or more is 8000 μm or less. 2. In the backgrind tape described in 1 above, the product of the nanoindentation hardness (MPa) and the thickness (μm) of the intermediate layer may be 0.050 to 15,000. 3. In the backgrind tape according to the above 1 or 2, the product of the nanoindentation hardness (MPa) and the thickness (μm) of the pressure-sensitive adhesive layer may be 0.001 to 1.000. 4. In the backgrind tape according to any one of the above 1 to 3, the pressure-sensitive adhesive layer may have a thickness of 1 μm to 50 μm. 5. In the backgrind tape according to any one of 1 to 4 above, the intermediate layer may contain a (meth)acrylic polymer obtained by polymerizing a monomer composition containing a monomer having a glass transition temperature of 80° C. or higher. 6. In the backgrind tape described in 5 above, the intermediate layer may contain a (meth)acrylic polymer obtained by polymerizing a monomer composition containing 5% by weight to 50% by weight of a monomer having a glass transition temperature of 80°C or higher. 7. In the backgrind tape according to any one of 1 to 6 above, the adhesive layer may be formed of an ultraviolet-curable adhesive. 8. In the backgrind tape according to any one of 1 to 7 above, the pressure-sensitive adhesive layer may be formed from a pressure-sensitive adhesive containing a polyfunctional acrylate. 9. The backgrind tape described in any one of 1 to 8 above may be adhered to a semiconductor wafer having bumps formed thereon, and the height (μm) of the bumps and the sum of the thickness (μm) of the adhesive layer and the thickness (μm) of the intermediate layer may satisfy the relationship: bump height (μm) < adhesive layer thickness (μm) + intermediate layer thickness (μm). 10. The backgrind tape described in any one of 1 to 9 above may be bonded to a semiconductor wafer having bumps formed thereon, and the height (μm) of the bumps and the thickness (μm) of the intermediate layer may satisfy the relationship: bump height (μm) < intermediate layer thickness (μm). Effect of the Invention
[0007] According to an embodiment of the present invention, a backgrind tape that is capable of achieving both excellent embedding properties and excellent cutting properties can be provided. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view of a backgrind tape according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a backgrind tape and an indenter when performing nanoindenter measurement of an intermediate layer. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a backgrind tape and an indenter when performing nanoindenter measurement of a pressure-sensitive adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A. Overall composition of backgrind tape FIG. 1 is a schematic cross-sectional view of a backgrind tape according to an embodiment of the present invention. The backgrind tape 100 according to an embodiment of the present invention includes a substrate 10, an intermediate layer 20, and a pressure-sensitive adhesive layer 30. For practical purposes, a release liner may be temporarily attached to the pressure-sensitive adhesive layer 30 in a releasable manner until use. The intermediate layer 20 may be formed of any appropriate resin or any appropriate pressure-sensitive adhesive. The intermediate layer 20 has a nanoindentation hardness (25° C.) of 0.001 MPa to 0.200 MPa. The pressure-sensitive adhesive layer 30 has a nanoindentation hardness (25° C.) of 0.001 MPa to 0.080 MPa. At least one of the intermediate layer 20 and the pressure-sensitive adhesive layer 30 has a thickness of 50 μm or more. Furthermore, the layer having a thickness of 50 μm or more has an unloading curve displacement of 8000 μm or less. A backgrind tape used in processing a semiconductor wafer having unevenness such as bumps is required to be able to embed the unevenness on the surface of the semiconductor wafer. On the other hand, a backgrind tape with excellent embedding properties has poor cut properties, and stringing may occur in the adhesive layer and / or intermediate layer during the process of cutting the backgrind tape. The stringy adhesive or intermediate layer forming composition may adhere to the semiconductor wafer. As a result, the thinly ground semiconductor wafer may be damaged when the backgrind tape is peeled off. In this way, it is difficult to achieve both embedding properties and cut properties. The present inventors have found that a backgrind tape having an adhesive layer and an intermediate layer with nanoindentation hardness and unloading curve displacement within a specific range measured in the state of the backgrind tape can achieve both excellent embedding properties and cut properties (for example, suppression of stringing of the adhesive layer and the intermediate layer), and have completed the present invention. Note that if the thickness is less than 50 μm, it can be cut without stringing with a cutter usually used in the tape cutting process.
[0010] The nanoindentation hardness and the displacement of the unloading curve can be obtained by nanoindentation measurement. Measurements using a nanoindenter are performed by controlling the load applied by the indenter and measuring the displacement (indentation depth of the indenter), and a load-displacement curve is created from the measurement results, and properties such as nanoindentation hardness can be obtained. A load-displacement curve is generally created with the horizontal axis representing the displacement (indentation depth) and the vertical axis representing the load (force required for indentation). For example, in the case of an adhesive layer and an intermediate layer, when an indenter is brought into contact with a measurement target, the load becomes a negative value due to the wettability and adsorption of the layer in contact with the indenter. Next, loading is performed by the indenter. In this specification, a load is applied to the intermediate layer until the indentation depth reaches 3000 nm, and to the adhesive layer until the indentation depth reaches 2000 nm. A load curve is created from the displacement from the start of loading to the maximum load. Nanoindentation hardness can be calculated from the maximum load to the indentation depth and the contact projected area. Next, the indenter is pulled out until the load becomes 0. An unloading curve is created from the amount of displacement until the load becomes 0. The adhesive layer and the intermediate layer have adhesiveness and cohesive force, and when the indenter is pulled out, the components constituting the adhesive layer and the intermediate layer may adhere to the indenter and become stringy. Therefore, the amount of displacement in the unloading curve may be a negative value. In this specification, the distance (amount of displacement) at which the displacement becomes negative in the unloading curve is referred to as the amount of unloading curve displacement. In this specification, the nanoindentation hardness and the amount of unloading curve displacement of the adhesive layer and the intermediate layer are both measured in a state where they are laminated as a back-grind tape.
[0011] The nanoindentation hardness (25°C) of the intermediate layer is 0.001MPa to 0.200MPa, preferably 0.005MPa to 0.185MPa, more preferably 0.010MPa to 0.150MPa, and even more preferably 0.015MPa to 0.100MPa. FIG. 2 is a schematic cross-sectional view of the backgrind tape and the indenter when performing the nanoindenter measurement of the intermediate layer. When performing the nanoindenter measurement of the intermediate layer, the substrate 10 side of the backgrind tape 100 is fixed to the support 300 via the adhesive layer 400 of the double-sided tape so that the side of the backgrind tape 100 and the indenter face each other, and the indenter 200 of the nanoindenter is brought into contact with the approximate center of the intermediate layer 20 from the side of the backgrind tape 100, and the measurement can be performed. In this specification, the nanoindentation hardness of the intermediate layer is measured in the state of the backgrind tape. If the nanoindentation hardness of the intermediate layer measured in the state of the backgrind tape is within the above range, a backgrind tape that can achieve both excellent embedding properties and cutting properties can be provided. Specifically, the nanoindentation hardness measured by the following method at room temperature of 25° C. is referred to as the nanoindentation hardness of the intermediate layer. <Nano indentation hardness> The back-ground tape is cut out and a measurement sample is prepared using an ultramicrotome under freezing conditions. The indenter is pressed in and pulled out at a speed of 500 nm / sec. The indenter is pressed into the intermediate layer to a depth of 3000 nm over a period of 6 seconds. The holding time after pressing is set to 0 seconds. The indenter is pulled out of the intermediate layer at the same speed as it was pressed in, and the time it takes for the indenter to be pulled out of the intermediate layer is measured. Note that the time it takes for the indenter to be pulled out may vary depending on the sample, as it is affected by physical properties such as stringiness. The maximum load Pmax (μN) and contact projected area A (μm2) at maximum depth (3000 nm) in this measurement are 2) hardness (nanoindentation hardness) (MPa) is calculated from the value of Pmax / A. In nanoindenter measurement, if the thickness of the layer to be measured is 10 times or more the indentation depth, it is considered that there is no influence of the layer laminated on the side opposite to the side where the indenter is pressed. Therefore, if the thickness of the intermediate layer is less than 20 μm, an evaluation adhesive tape with an intermediate layer thickness of 20 μm is prepared and evaluated using the above method.
[0012] The nanoindentation hardness (25°C) of the pressure-sensitive adhesive layer is 0.001MPa to 0.080MPa, preferably 0.001MPa to 0.060MPa, more preferably 0.002MPa to 0.055MPa, and even more preferably 0.003MPa to 0.050MPa. In this specification, the nanoindentation hardness of the pressure-sensitive adhesive layer is measured in the state of a back-grind tape. If the nanoindentation hardness of the pressure-sensitive adhesive layer measured in the state of a back-grind tape is within the above range, a back-grind tape that can achieve both excellent embedding properties and cutting properties of unevenness can be provided. Specifically, in this specification, the nanoindentation hardness measured by the following method at room temperature of 25°C is referred to as the nanoindentation hardness of the pressure-sensitive adhesive layer. <Nano indentation hardness> The backgrind tape is cut to a length of approximately 1 cm and a width of approximately 1 cm to prepare a sample for measurement. The indenter is pressed in and pulled out at a speed of 500 nm / sec. The indenter is pressed into the adhesive layer to a depth of 2000 nm over a period of 4 seconds. The holding time after pressing is recorded as 0 seconds. The indenter is pulled out of the adhesive layer at the same speed as it was pressed in, and the time it takes for the indenter to be pulled out of the adhesive layer is measured. Note that the time it takes to pull out may vary depending on the sample, as it is affected by physical properties such as stringiness. The maximum load Pmax (μN) and contact projected area A (μm at maximum depth (2000 nm) in this measurement are 2 ) and calculate the hardness (nanoindentation hardness) (MPa) from the value of Pmax / A. Regarding the adhesive layer, when the thickness of the adhesive layer is less than 20 μm, an evaluation adhesive tape with an adhesive layer thickness of 20 μm is prepared and evaluated by the above method.
[0013] As described above, at least one of the pressure-sensitive adhesive layer and the intermediate layer has a thickness of 50 μm or more. If at least one of them is 50 μm or more, the embedding property of the unevenness can be improved. The layer having a thickness of 50 μm or more has an unloading curve displacement of 8000 μm or less, preferably 7500 μm or less, more preferably 7000 μm or less, even more preferably 6500 μm or less, and particularly preferably 5000 μm or less. The smaller the unloading curve displacement, the more preferable it is, for example, 500 μm or more. As described above, the unloading curve displacement is measured in the state of the backgrind tape. If the unloading curve displacement measured in the state of the backgrind tape is within the above range, a semiconductor wafer that can achieve both excellent embedding property of the unevenness and cutting property can be provided. In this specification, the unloading curve displacement refers to the distance from the unloading curve of the load-displacement curve where the displacement becomes negative (i.e., the displacement from the point where the displacement becomes 0 nm to the point where the load becomes 0 on the unloading curve), when a load-displacement curve is created from the load and indentation depth during the measurement of the nanoindentation hardness.
[0014] The backgrind tape may further include any appropriate layer other than the substrate, intermediate layer, and adhesive layer. For example, it may further include an antistatic layer. If the backgrind tape has an antistatic layer, electrostatic damage to the semiconductor element due to static electricity when the backgrind tape is peeled off can be prevented.
[0015] The thickness of the backgrind tape can be set in any appropriate range, preferably 10 μm to 1000 μm, more preferably 50 μm to 300 μm, and further preferably 100 μm to 300 μm.
[0016] B. Base material The substrate may be made of any suitable resin. Specific examples of the resin constituting the substrate include polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and polybutylene naphthalate (PBN), polyolefin resins such as ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, polyethylene, polypropylene, and ethylene-propylene copolymer, polyvinyl alcohol, polyvinylidene chloride, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyvinyl acetate, polyamide, polyimide, cellulose, fluorine resin, polyether, and polystyrene resins such as polystyrene, polycarbonate, and polyethersulfone. Preferably, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate are used. If these resins are used, the occurrence of warping can be more effectively prevented.
[0017] The substrate may further contain other components within a range that does not impair the effects of the present invention. Examples of other components include antioxidants, ultraviolet absorbers, light stabilizers, and heat stabilizers. The types and amounts of other components can be any appropriate amount depending on the purpose.
[0018] In one embodiment, the substrate has an antistatic function. If the substrate has an antistatic function, the generation of static electricity during tape peeling can be suppressed, and the destruction of the circuit due to static electricity and the adhesion of foreign matter can be prevented. The substrate may have an antistatic function by being formed from a resin containing an antistatic agent, or may have an antistatic function by forming an antistatic layer by applying a composition containing an antistatic component such as a conductive polymer, an organic or inorganic conductive material, and an antistatic agent to any appropriate film. When the substrate has an antistatic layer, it is preferable that an intermediate layer is laminated on the surface on which the antistatic layer is formed. When the substrate has an antistatic function, the surface resistance value of the substrate is, for example, 1.0×10 2 Ω / □~1.0×10 13 It is Ω / □.
[0019] The thickness of the substrate can be set to any appropriate value, and is preferably from 10 μm to 200 μm, and more preferably from 20 μm to 150 μm.
[0020] The elastic modulus of the substrate can be set to any appropriate value. The elastic modulus of the substrate is preferably 50 MPa to 6000 MPa, more preferably 70 MPa to 5000 MPa. If the elastic modulus is within the above range, a backgrind tape that can appropriately conform to the irregularities of the adherend surface can be obtained.
[0021] C. middle class The thickness of the intermediate layer is preferably 10 μm to 300 μm, more preferably 50 μm to 200 μm, even more preferably 50 μm to 150 μm, and particularly preferably 100 μm to 150 μm. If the thickness of the intermediate layer is within the above range, a backgrind tape that can well embed uneven surfaces can be obtained. As described above, when the thickness of the intermediate layer is 50 μm or more, the unloading curve displacement is 8000 μm or less.
[0022] The product of the nanoindentation hardness (MPa) and thickness (μm) of the intermediate layer is preferably 0.050 to 15,000, more preferably 0.400 to 10,000, and even more preferably 1,000 to 8,000. If the product of the nanoindentation hardness and thickness is within the above range, a backgrind tape that can better balance the embedding ability and cutting ability of irregularities can be obtained.
[0023] The intermediate layer may be formed of any suitable material, such as any suitable resin, for example, an acrylic resin, a polyethylene resin, an ethylene-vinyl alcohol copolymer, an ethylene vinyl acetate resin, or an ethylene methyl methacrylate resin, or an adhesive.
[0024] In one embodiment, the intermediate layer is preferably formed from an intermediate layer forming composition containing a (meth)acrylic polymer. The (meth)acrylic polymer preferably contains a component derived from an alkyl (meth)acrylate. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, and the like. Examples of the (meth)acrylic acid C1-C20 alkyl ester include (meth)acrylic acid C1-C20 alkyl esters such as decyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Note that "(meth)acrylic" refers to acrylic and / or methacrylic.
[0025] The intermediate layer preferably contains a (meth)acrylic polymer obtained by polymerizing a monomer composition containing a monomer having a glass transition temperature of 80° C. or higher (hereinafter also referred to as a high Tg monomer). If the intermediate layer contains a monomer having a glass transition temperature of 80° C. or higher, a backgrind tape having better cutting properties can be obtained. The glass transition temperature of the high Tg monomer is more preferably 90° C. or higher, and even more preferably 100° C. or higher. The glass transition temperature of the high Tg monomer is, for example, 180° C. or lower. In this specification, the glass transition temperature of a monomer refers to the glass transition temperature of a homopolymer of the monomer. Specific examples of high Tg monomers include cyclohexyl methacrylate (Tg: 83°C), dicyclopentanyl acrylate (Tg: 120°C), dicyclopentanyl methacrylate (Tg: 175°C), isobornyl acrylate (Tg: 94°C), isobornyl methacrylate (Tg: 150°C), t-butyl methacrylate (Tg: 118°C), methyl methacrylate (Tg: 105°C), trimethylolpropane triacrylate (Tg: >250°C), styrene (Tg: 80°C), acrylonitrile (Tg: 97°C), and N-acryloylmorpholine (Tg: 145°C). As the high Tg monomer, methyl methacrylate is preferably used. The Tg of homopolymers other than those mentioned above can be determined, for example, from "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999). In addition, when multiple Tg values are given in this document, the "conventional" value is used.
[0026] The high Tg monomer may be used in any appropriate content ratio. The content ratio of the high Tg monomer in the monomer composition is preferably 5 wt % to 50 wt %, more preferably 10 wt % to 40 wt %, and further preferably 15 wt % to 35 wt %.
[0027] The (meth)acrylic polymer may contain, as necessary, a structural unit corresponding to another monomer copolymerizable with the alkyl (meth)acrylate, for the purpose of modifying the cohesive strength, heat resistance, crosslinkability, etc. Examples of such monomers include carboxyl group-containing monomers such as acrylic acid and methacrylic acid; acid anhydride monomers such as maleic anhydride and itanoic anhydride; hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate; sulfonic acid group-containing monomers such as styrenesulfonic acid and allylsulfonic acid; nitrogen-containing monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and acryloylmorpholine; aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate; alkoxyalkyl (meth)acrylate monomers such as methoxyethyl (meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide and N-isopropylmaleimide; N-methylitaconimide and N-ethylitaconimide; Examples of the monomers include itaconimide monomers such as amide; succinimide monomers; vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, and methylvinylpyrrolidone; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate and polypropylene glycol (meth)acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, and the like such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; olefin monomers such as isoprene, butadiene, and isobutylene; and vinyl ether monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more. The content ratio of the structural unit derived from the other monomer is preferably 1 to 30 parts by weight, and more preferably 3 to 25 parts by weight, in 100 parts by weight of the (meth)acrylic polymer.
[0028] The weight average molecular weight of the (meth)acrylic polymer is preferably from 100,000 to 1,000,000, and more preferably from 300,000 to 800,000. The weight average molecular weight can be measured by GPC (solvent: THF).
[0029] In one embodiment, the intermediate layer contains a photopolymerization initiator and does not contain an ultraviolet curing component. That is, although the intermediate layer contains a photopolymerization initiator, the intermediate layer itself is not cured by ultraviolet irradiation. Therefore, the intermediate layer can maintain its flexibility before and after ultraviolet irradiation. In addition, if the intermediate layer contains a photopolymerization initiator, the photopolymerization initiator contained in the adhesive layer moves to the intermediate layer, and as a result, the content of the photopolymerization initiator contained in the adhesive layer can be suppressed from decreasing over time. Therefore, after ultraviolet irradiation, the backgrind tape can exhibit excellent light peelability. In this specification, the ultraviolet curing component refers to a component that can be crosslinked by ultraviolet irradiation and can be cured and shrunk. Specifically, a polymer having a polymerizable carbon-carbon double bond in a side chain or at an end can be mentioned.
[0030] The photopolymerization initiator contained in the intermediate layer-forming composition (intermediate layer formed as a result) may be the same as or different from the photopolymerization initiator contained in the adhesive layer. Preferably, the intermediate layer contains the same photopolymerization initiator as the adhesive layer. If the intermediate layer and the adhesive layer contain the same photopolymerization initiator, the migration of the photopolymerization initiator from the adhesive layer to the intermediate layer can be further suppressed. As the photopolymerization initiator, the photopolymerization initiators exemplified in the adhesive composition can be used. Only one type of photopolymerization initiator may be used, or two or more types may be used in combination.
[0031] The content of the photopolymerization initiator in the intermediate layer is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the polymer constituent in the composition for forming the intermediate layer. When the content of the photopolymerization initiator contained in the intermediate layer is within the above range, a backgrind tape having excellent easy peelability after ultraviolet irradiation can be obtained. In one embodiment, the photopolymerization initiator is used in an amount equal to that of the composition forming the pressure-sensitive adhesive layer.
[0032] In one embodiment, the composition for forming an intermediate layer further includes a crosslinking agent, such as an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, a melamine-based crosslinking agent, a peroxide-based crosslinking agent, a urea-based crosslinking agent, a metal alkoxide-based crosslinking agent, a metal chelate-based crosslinking agent, a metal salt-based crosslinking agent, a carbodiimide-based crosslinking agent, or an amine-based crosslinking agent.
[0033] When the composition for forming an intermediate layer contains a crosslinking agent, the content of the crosslinking agent is preferably 0.5 to 10 parts by weight, and more preferably 1 to 8 parts by weight, per 100 parts by weight of the polymer constituent components in the composition for forming an intermediate layer.
[0034] The intermediate layer forming composition may further contain any suitable additives as necessary, such as active energy ray polymerization accelerators, radical scavengers, tackifiers, plasticizers (e.g., trimellitic acid ester-based plasticizers, pyromellitic acid ester-based plasticizers, etc.), pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, etc.
[0035] D.Adhesive layer The adhesive layer may be formed using any suitable adhesive. Typically, the adhesive contains a base polymer. Preferably, the adhesive layer is formed from an ultraviolet-curable adhesive. If the adhesive layer is formed from an ultraviolet-curable adhesive, a backgrind tape with excellent light peelability can be obtained.
[0036] D-1. Base polymer Any suitable adhesive can be used as the ultraviolet-curing adhesive. For example, it may be an adhesive obtained by adding an ultraviolet-curing monomer and / or oligomer to any suitable adhesive such as an acrylic adhesive, a rubber adhesive, a silicone adhesive, or a polyvinyl ether adhesive, or it may be an adhesive using a polymer having a polymerizable carbon-carbon double bond introduced into the side chain and / or the end as the base polymer. Preferably, an adhesive using a polymer having a polymerizable carbon-carbon double bond introduced into the side chain and / or the end as the base polymer is used.
[0037] When using a pressure-sensitive adhesive using a polymer having a polymerizable carbon-carbon double bond introduced at the side chain and / or end, a polymer having a polymerizable carbon-carbon double bond introduced at the side chain and / or end and having adhesiveness is used as the base polymer. Examples of such polymers include polymers having a polymerizable carbon-carbon double bond introduced into resins such as acrylic resins, vinyl alkyl ether resins, silicone resins, polyester resins, polyamide resins, urethane resins, and styrene-diene block copolymers. Preferably, an acrylic resin having a polymerizable carbon-carbon double bond introduced into an acrylic resin is used. By using an acrylic resin, it is easy to adjust the storage modulus and tensile modulus of the pressure-sensitive adhesive layer, and a pressure-sensitive adhesive sheet having an excellent balance between adhesive strength and peelability can be obtained. Furthermore, contamination of semiconductor wafers by components derived from the pressure-sensitive adhesive can be reduced.
[0038] Any suitable acrylic resin can be used as the acrylic resin, for example, a polymer obtained by polymerizing a monomer composition containing one or more esters of acrylic acid or methacrylic acid having a linear or branched alkyl group.
[0039] The linear or branched alkyl group is preferably an alkyl group having 30 or less carbon atoms, more preferably an alkyl group having 1 to 20 carbon atoms, and further preferably an alkyl group having 4 to 18 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an isobutyl group, an amyl group, an isoamyl group, a hexyl group, a heptyl group, a cyclohexyl group, a 2-ethylhexyl group, an octyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a lauryl group, a tridecyl group, a tetradecyl group, a stearyl group, an octadecyl group, and a dodecyl group.
[0040] The monomer composition may contain any other suitable monomer. Examples of the other monomer include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 4-hydroxyethyl (meth)acrylate, 5-hydroxypropyl (meth)acrylate, 6-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 5-hydroxypropyl (meth)acrylate, 6-hydroxypropyl (meth)acrylate, 8-hydroxypropyl (meth)acrylate, 9-hydroxypropyl (meth)acrylate, 10-hydroxypropyl (meth)acrylate, 12 ... Examples of the functional group-containing monomer include hydroxyl group-containing monomers such as hydroxymethylcyclohexyl)-methyl acrylate, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; and phosphoric acid group-containing monomers such as 2-hydroxyethylacryloylphosphate. If the functional group-containing monomer is contained, an acrylic resin in which a polymerizable carbon-carbon double bond is easily introduced can be obtained. The content ratio of the functional group-containing monomer is preferably 4 to 30 parts by weight, more preferably 6 to 20 parts by weight, based on 100 parts by weight of the total monomer components of the monomer composition.
[0041] The weight average molecular weight of the acrylic resin is preferably 100,000 or more, more preferably 300,000 or more, even more preferably 500,000 or more, and particularly preferably 800,000 to 3,000,000. Within such a range, bleeding of low molecular weight components can be prevented, and a low-contamination adhesive sheet for semiconductor wafer processing can be obtained. The molecular weight distribution (weight average molecular weight / number average molecular weight) of the (meth)acrylic resin is preferably 1 to 20, more preferably 3 to 10. By using a (meth)acrylic resin with a narrow molecular weight distribution, bleeding of low molecular weight components can be prevented, and a low-contamination adhesive sheet can be obtained. The weight average molecular weight and number average molecular weight can be determined by gel permeation chromatography measurement (solvent: tetrahydrofuran, polystyrene equivalent).
[0042] A polymer having a polymerizable carbon-carbon double bond introduced at the side chain and / or end can be obtained by any suitable method. For example, it can be obtained by reacting (for example, condensation reaction, addition reaction) a resin obtained by any suitable polymerization method with a compound having a polymerizable carbon-carbon double bond. Specifically, when an acrylic resin is used, an acrylic resin (copolymer) having a structural unit derived from a monomer having any suitable functional group is polymerized in any suitable solvent, and then a functional group of the acrylic resin is reacted with a compound having a polymerizable carbon-carbon double bond that can react with the functional group to obtain an acrylic resin having a polymerizable carbon-carbon double bond introduced therein. The amount of the compound having a polymerizable carbon-carbon double bond to be reacted is preferably 4 to 30 parts by weight, more preferably 4 to 20 parts by weight, relative to 100 parts by weight of the resin. Any suitable solvent can be used as the solvent, and examples thereof include various organic solvents such as ethyl acetate, methyl ethyl ketone, and toluene.
[0043] When the resin and the compound having a polymerizable carbon-carbon double bond are reacted as described above, it is preferable that the resin and the compound having a polymerizable carbon-carbon double bond each have a functional group capable of reacting with each other. Examples of the combination of functional groups include a carboxyl group / epoxy group, a carboxyl group / aziridine group, and a hydroxyl group / isocyanate group. Among these combinations of functional groups, the combination of a hydroxyl group and an isocyanate group is preferable because of the ease of tracking the reaction.
[0044] Examples of compounds having a polymerizable carbon-carbon double bond include 2-isocyanatoethyl methacrylate, methacryloisocyanate, 2-methacryloyloxyethyl isocyanate (2-isocyanatoethyl methacrylate), and m-isopropenyl-α,α-dimethylbenzyl isocyanate.
[0045] D-2. Photopolymerization initiator As the photopolymerization initiator, any suitable initiator can be used. Examples of the photopolymerization initiator include acylphosphine oxide photoinitiators such as ethyl 2,4,6-trimethylbenzylphenylphosphinate and (2,4,6-trimethylbenzoyl)-phenylphosphine oxide; α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenylketone; methoxyacetophenone, Acetophenone compounds such as 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; ketal compounds such as benzil dimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; 1-phenone-1,1-propanedione-2-( o-Ethoxycarbonyl)oxime and other photoactive oxime compounds; benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone and other benzophenone compounds; thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone compounds; camphorquinone; halogenated ketones acylphosphonates, and α-hydroxyacetophenones such as 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl-2-methylpropane-1. Preferably, 2,2-dimethoxy-2-phenylacetophenone and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl-2-methylpropane-1 can be used. The photopolymerization initiator may be used alone or in combination of two or more kinds.
[0046] As the photopolymerization initiator, commercially available products may be used, for example, Omnirad 127 and Omnirad 651, both of which are products of IGM Resins.
[0047] The photopolymerization initiator is used in any appropriate amount. The content of the photopolymerization initiator is preferably 0.5 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of the base polymer. If the content of the photopolymerization initiator is less than 0.5 parts by weight, there is a risk that the adhesive will not be sufficiently cured when irradiated with ultraviolet light. If the content of the photopolymerization initiator is more than 10 parts by weight, there is a risk that the storage stability of the adhesive will decrease.
[0048] The adhesive preferably further contains a multifunctional acrylate. If the adhesive further contains a multifunctional acrylate, the elasticity of the adhesive layer is reduced, and a backgrind tape having better unevenness embedding properties can be obtained. In addition, the adhesive strength is reduced by ultraviolet irradiation, and a backgrind tape having better light peelability can be obtained. Examples of the multifunctional acrylate include (meth)acrylate oligomers and monomers. Specific examples of the oligomer include hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy(meth)acrylate, polyester(meth)acrylate, urethane(meth)acrylate, and further, various oligomers such as urethane-based, polyether-based, polyester-based, polycarbonate-based, and polybutadiene-based oligomers. The molecular weight of these oligomer components is suitably within the range of about 100 to 30000. These can be used alone or in combination of two or more kinds.
[0049] The polyfunctional acrylate is used in any suitable content. For example, it is 1 to 80 parts by weight, preferably 10 to 50 parts by weight, and more preferably 25 to 45 parts by weight, per 100 parts by weight of the base polymer. If the content of the polyfunctional acrylate is within the above range, the elasticity of the adhesive layer is reduced, and a backgrind tape having better unevenness embedding properties can be obtained. In addition, the adhesive strength is reduced by ultraviolet irradiation, and a backgrind tape having better light peelability can be obtained.
[0050] D-3. Additives The pressure-sensitive adhesive may contain any suitable additives as necessary, such as crosslinkers, catalysts (e.g., platinum catalysts), tackifiers, plasticizers, pigments, dyes, fillers, antioxidants, conductive materials, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, and solvents.
[0051] In one embodiment, the adhesive further includes a crosslinking agent. Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, and a chelate-based crosslinking agent. The content ratio of the crosslinking agent is preferably 0.01 to 10 parts by weight, more preferably 0.02 to 5 parts by weight, and even more preferably 0.025 to 0.5 parts by weight, relative to 100 parts by weight of the base polymer contained in the adhesive. The flexibility of the adhesive layer can be controlled by the content ratio of the crosslinking agent. If the content of the crosslinking agent is less than 0.01 parts by weight, the adhesive may become a sol, and the adhesive layer may not be formed. If the content of the crosslinking agent is more than 10 parts by weight, the adhesion to the semiconductor wafer may decrease, and the semiconductor wafer may not be sufficiently protected.
[0052] In one embodiment, an isocyanate-based crosslinking agent is preferably used. An isocyanate-based crosslinking agent is preferred because it can react with various functional groups. Particularly preferably, a crosslinking agent having three or more isocyanate groups is used. If an isocyanate-based crosslinking agent is used as the crosslinking agent and the content of the crosslinking agent is within the above range, a pressure-sensitive adhesive layer that has excellent peelability and significantly less adhesive residue even after heating can be formed.
[0053] The thickness of the adhesive layer can be set to any appropriate value. The thickness of the adhesive layer is preferably 1 μm to 50 μm, more preferably 2 μm to 40 μm, and even more preferably 5 μm to 30 μm. If the thickness of the adhesive layer is within the above range, it can exert sufficient adhesive strength to the semiconductor wafer. As described above, when the thickness of the adhesive layer is 50 μm or more, the unloading curve displacement is 8000 μm or less.
[0054] The product of the nanoindentation hardness (MPa) and thickness (μm) of the pressure-sensitive adhesive layer is preferably 0.001 to 1.000, more preferably 0.050 to 1.000, even more preferably 0.075 to 0.800, and particularly preferably 0.100 to 0.600. If the product of the nanoindentation hardness and thickness is within the above range, a backgrind tape that can better balance the ability to embed irregularities and the ability to cut can be obtained.
[0055] The adhesive layer may be one layer or two or more layers. When the adhesive layer is two or more layers, at least one adhesive layer formed using an adhesive containing the photopolymerization initiator may be included. When the adhesive layer is two or more layers, the adhesive layer formed using an adhesive containing a photopolymerization initiator is preferably formed on the surface of the adhesive sheet that contacts the semiconductor wafer. The adhesive layer that is not formed by an ultraviolet curing adhesive may be formed by any appropriate adhesive composition. This adhesive composition may be an ultraviolet curing adhesive or a pressure sensitive adhesive.
[0056] The adhesive layer may have any suitable adhesive strength. The adhesive strength of the adhesive layer to a silicon wafer before ultraviolet irradiation is preferably 0.50N / 20mm to 30N / 20mm, more preferably 1.00N / 20mm to 25N / 20mm, and even more preferably 1.50N / 20mm to 20N / 20mm. In this specification, the adhesive strength of the adhesive layer refers to a value measured by cutting a backgrind tape to a width of 20mm and a length of 80mm, pressing the adhesive layer of the backgrind tape to the mirror surface of a silicon mirror wafer by moving a 2kg roller back and forth once in an atmosphere of 23°C, leaving it at 23°C for 30 minutes, and then performing a 180° peel test at a pulling speed of 300mm / min in an atmosphere of 23°C and 50%RH.
[0057] The adhesive strength of the adhesive layer to a silicon wafer after ultraviolet irradiation is preferably 0.001 N / 20 mm to 1.000 N / 20 mm, more preferably 0.005 N / 20 mm to 0.850 N / 20 mm, and even more preferably 0.005 N / 20 mm to 0.800 N / 20 mm. The adhesive strength after ultraviolet irradiation is measured by cutting the backgrind tape to a width of 20 mm and a length of 80 mm, pressing the adhesive layer onto the mirror surface of a silicon mirror wafer by rolling a 2 kg roller back and forth once in an atmosphere of 23°C, leaving it at 23°C for 30 minutes, and then irradiating the adhesive layer with ultraviolet (UV) at an integrated light intensity of 1000 mJ / cm. 2 (365 nm equivalent) from the substrate side of the backgrind tape, and then a 180° peel test is performed under conditions of 23°C, 50% RH atmosphere, and a tensile speed of 300 mm / min, and the value is measured.
[0058] E. Backgrind Tape Manufacturing Method The backgrind tape can be manufactured by any suitable method. In one embodiment, the backgrind tape can be manufactured, for example, by forming an intermediate layer on a substrate, and then forming a pressure-sensitive adhesive layer on the intermediate layer. The pressure-sensitive adhesive layer and the intermediate layer may be formed by applying the composition forming the pressure-sensitive adhesive layer and the composition forming the intermediate layer to the substrate or intermediate layer to form each layer, or may be formed on any suitable release liner and then transferred. As the coating method, various methods such as bar coater coating, air knife coating, gravure coating, gravure reverse coating, reverse roll coating, lip coating, die coating, dip coating, offset printing, flexographic printing, and screen printing can be adopted. In addition, a method of forming a pressure-sensitive adhesive layer or an intermediate layer on a release liner and then laminating it to a substrate may be adopted.
[0059] F. Uses of Backgrind Tape The backgrind tape according to the embodiment of the present invention can be suitably used in the backgrind process of the semiconductor device manufacturing process. The backgrind tape is required to hold the silicon wafer properly during backgrinding, and to have a light peelability that allows the ground wafer to be peeled off without damaging it during peeling. The backgrind tape according to the embodiment of the present invention can achieve both excellent irregularity embedding properties and cutting properties. Therefore, the backgrind tape according to the embodiment of the present invention can be suitably used in the processing of semiconductor devices.
[0060] In one embodiment, it is preferable that the sum of the bump height (μm), the adhesive layer thickness (μm), and the intermediate layer thickness (μm) satisfy the relationship of bump height (μm) < adhesive layer thickness (μm) + intermediate layer thickness (μm). Also, the bump height (μm) and the intermediate layer thickness (μm) satisfy the relationship of bump height (μm) < intermediate layer thickness (μm). If such a relationship is satisfied, a backgrind tape with better unevenness embedding properties can be obtained. EXAMPLES
[0061] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0062] [Example 1] 1. Preparation of intermediate layer-forming composition As monomer components, 73.7% by weight of butyl acrylate (BA), 19.2% by weight of methyl methacrylate (MMA), and 7.1% by weight of 2-hydroxyethyl acrylate (HEA) (manufactured by Toa Gosei Co., Ltd., trade name: Aclix (registered trademark) HEA) were used. A monomer composition (solid content concentration: 40%) was prepared by mixing 0.3% by weight of a polymerization initiator (manufactured by Tokyo Chemical Industry Co., Ltd., trade name: 2,2'-azobis(isobutyronitrile) (AIBN)) with respect to the total weight of the monomer components and a solvent (ethyl acetate). The obtained monomer composition was placed in a 1L round-bottom separable flask, a polymerization experimental apparatus equipped with a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade, and nitrogen replacement was performed at room temperature for 2 hours while stirring. Thereafter, the mixture was kept at 65° C. for 6 hours while stirring under a nitrogen flow to carry out solution polymerization, thereby obtaining a resin solution (solid content: 40% by weight). 100 parts by weight of the solid content of the obtained resin solution was mixed with 0.1 parts by weight of a polyisocyanate compound (manufactured by Tosoh Corporation, product name "Coronate L") and 1 part by weight of a photopolymerization initiator (manufactured by IGM Resins, product name: Omnirad 127D) to prepare an intermediate layer forming composition (solid content 23%) containing ethyl acetate.
[0063] 2. Preparation of Pressure-Sensitive Adhesive Composition The monomer components used were 76.8% by weight of butyl acrylate (BA), 7.5% by weight of methyl methacrylate (MMA), and 8.7% by weight of 2-hydroxyethyl acrylate (manufactured by Toagosei Co., Ltd., product name: Aclix (registered trademark) HEA). The monomer composition was prepared by mixing 0.3% by weight of a polymerization initiator (manufactured by Tokyo Chemical Industry Co., Ltd., product name: 2,2'-azobis(isobutyronitrile) (AIBN)) based on the total weight of the monomer components and a solvent (ethyl acetate). A product (solid content concentration: 37.5%) was prepared. The obtained monomer composition was put into a polymerization experimental apparatus equipped with a 1 L round-bottom separable flask, a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade, and the atmosphere was replaced with nitrogen at room temperature for 2 hours while stirring. Thereafter, the solution was polymerized by holding at 65°C for 6 hours while stirring under a nitrogen inflow, to obtain a resin solution. The solution was then aged by holding at 78°C for 2 hours. The resin solution obtained was stirred so that sufficient air was introduced, and 7.0% by weight of a compound having a radiation polymerizable carbon-carbon double bond (manufactured by Showa Denko K.K., product name "Karens MOI") was added. Furthermore, 0.05% by weight of dibutyltin dilaurate IV (manufactured by Wako Pure Chemical Industries, Ltd.) was added relative to the weight of the compound having a radiation polymerizable carbon-carbon double bond, and a solvent (ethyl acetate) was appropriately added to adjust the solid content concentration to 25%, followed by stirring. The solution was then stored at 50°C for 24 hours to obtain a polymer solution (solid content: 25%). 100 parts by weight of the solid content of the obtained polymer solution was mixed with 0.75 parts by weight of a polyisocyanate compound (manufactured by Tosoh Corporation, product name "Coronate L"), 1 part by weight of a photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 127D"), and 40 parts by weight of a multifunctional acrylate (manufactured by Toagosei Co., Ltd., product name "Aronix (registered trademark) M-321") to prepare a pressure-sensitive adhesive composition (solid content 15%) containing ethyl acetate.
[0064] 3. Tape Preparation The intermediate layer forming composition obtained in 1 was applied to the silicone-treated surface of a 38 μm thick polyester release liner (manufactured by Mitsubishi Chemical Corporation, product name "Diafoil (registered trademark)") and heated at 120° C. for 120 seconds to remove the solvent, forming an intermediate layer with a thickness of 100 μm. Next, a 50 μm thick PET film (manufactured by Toray Industries, Inc., product name "Lumirror (registered trademark)") was bonded to the surface of the intermediate layer as a substrate. Separately, the adhesive composition obtained in 2. was applied to the silicone-treated surface of a 75 μm-thick polyester release liner and heated at 120° C. for 120 seconds to remove the solvent, forming an adhesive layer 20 μm thick. Next, the release liner was peeled off from the intermediate layer, and the adhesive layer was laminated and transferred to the surface of the intermediate layer from which the release liner had been peeled off. The adhesive layer was then stored at 50°C for 72 hours to obtain an adhesive tape (backgrind tape) having a substrate / intermediate layer / adhesive layer in that order.
[0065] [Examples 2 to 4] Except for changing the monomer composition, the intermediate layer-forming composition, and the pressure-sensitive adhesive layer-forming composition as shown in Table 1, the same procedure as in Example 1 was carried out to obtain a pressure-sensitive adhesive tape (backgrind tape).
[0066] [Example 5] As monomer components, 64% by weight of butyl acrylate (BA), 33% by weight of methyl methacrylate (MMA), and 3% by weight of 2-hydroxyethyl acrylate (HEA) (manufactured by Toa Gosei Co., Ltd., trade name: Aclix (registered trademark) HEA) were used. A 10% by weight aqueous solution of the monomer components and emulsifier (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "Aqualon KH-1025") and water were put into a glass bottle, and nitrogen bubbling was performed for 5 minutes. Next, the mixture was stirred for 5 minutes at 6000 rpm with a homodisper to obtain an emulsified monomer. A 10% by weight aqueous solution of the emulsifier (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "Aqualon KH-1025") was put into a separable flask equipped with a cooling tube, and nitrogen replacement was performed for 1 hour while stirring. The mixture was then kept at 70°C for 20 minutes. Next, 0.02 parts by weight of a 5% aqueous solution of an azo polymerization initiator (manufactured by Fujifilm, product name "VA-057") was added, and immediately, the emulsified monomer was dropped over 3 hours. After the dropwise addition was completed, maturation was carried out at 70°C for 3 hours. Next, salting out was carried out, and the solution after salting out was filtered, and the filtrate was dried to obtain a polymer. This polymer was dissolved in ethyl acetate to obtain a polymer solution with a solid content of 35% by weight. 100 parts by weight of the solid content of the obtained polymer solution was mixed with 0.1 parts by weight of a polyisocyanate compound (product name "Coronate L", manufactured by Tosoh Corporation) and 1 part by weight of a photopolymerization initiator (product name: Omnirad 127D, manufactured by IGM Resins) to prepare an intermediate layer forming composition containing ethyl acetate. An adhesive tape (backgrind tape) was obtained in the same manner as in Example 1, except that the intermediate layer forming composition obtained above was used and the monomer composition of the base polymer of the adhesive composition, the composition of the intermediate layer forming composition, and the composition of the adhesive layer forming composition were changed as shown in Table 1.
[0067] [Examples 6 to 8] Except for changing the monomer composition, the intermediate layer-forming composition, and the pressure-sensitive adhesive layer-forming composition as shown in Table 1, the same procedure as in Example 1 was carried out to obtain a pressure-sensitive adhesive tape (backgrind tape).
[0068] (Comparative Examples 1 to 4) Except for changing the monomer composition, the intermediate layer-forming composition, and the pressure-sensitive adhesive layer-forming composition as shown in Table 1, the same procedure as in Example 1 was carried out to obtain a pressure-sensitive adhesive tape (backgrind tape).
[0069] [Table 1]
[0070] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Table 2. 1. Nanoindenter measurement of the intermediate layer The adhesive tapes obtained in the examples and comparative examples were cut out and prepared as measurement samples using an ultramicrotome under freezing conditions. Specifically, the adhesive tapes were rapidly frozen under a liquid nitrogen atmosphere, and cut in the thickness direction under a freezing atmosphere of -30°C using an ultramicrotome (manufactured by Yamato Koki Kogyo Co., Ltd., a freezing microtome) to prepare cross sections. After the cross sections were prepared, the samples were left at room temperature for 2 hours or more, and nanoindenter measurements were performed. A nanoindenter (product name: Triboindenter) manufactured by Hysitron Inc. was used for the measurements. A Berkovich indenter (triangular pyramid, indenter interior angle: 142.35°, angle between center line and surface: 65.35°, indenter aspect ratio: 1:8) was used as the indenter. The measurements were performed under conditions of 25°C, using a single indentation measurement. The backgrind tape was fixed with a support as shown in FIG. 2. Specifically, the substrate side surface of the backgrind tape and the support (brass base) were bonded together with a double-sided tape (manufactured by Nitto, product name "No. 5605", thickness of adhesive layer: 0.05 mm). When bonding, one end of the brass base and one end of the backgrind tape were bonded together so that they were flush with each other. As shown in the example, the flush side and the indenter were placed so that they corresponded, and the Berkovich indenter was brought into contact with the approximate center of the intermediate layer on the side of the backgrind tape (the cross-section side prepared above) and measurements were performed. The indenter was pressed in and pulled out at a speed of 500 nm / sec. The indenter was pressed into the intermediate layer to a depth of 3000 nm over 6 seconds, and the holding time was 0 seconds. Next, the indenter was pulled out of the intermediate layer at the same speed as the pressing, and the time until the indenter was pulled out of the intermediate layer was measured. The maximum load Pmax (μN) and the contact projected area A (μm 2 ) hardness (nanoindentation hardness) (MPa) was calculated from the value of Pmax / A. A load-displacement curve was created from the load and the indentation depth during the above measurement. The distance at which the displacement became negative (i.e., the amount of displacement from the point at which the displacement became 0 nm to the point at which the load became 0 on the unloading curve) was measured from the unloading curve, and this was taken as the unloading curve displacement (μm). If the unloading curve displacement is 8000 μm or less, the cutting ability may be good. The measurements were performed using three samples, and the average values were used as the nanoindentation hardness and the displacement amount of the unloading curve.
[0071] 2. Nanoindenter measurement of adhesive layer The adhesive tapes obtained in the examples and comparative examples were cut into a length of about 1 cm by about 1 cm to be used as measurement samples. The release liner was peeled off, and the hardness of the adhesive layer and the displacement of the unloading curve were measured. A nanoindenter (product name: Triboindenter) manufactured by Hysitron Inc. was used for the measurement. The measurement was performed by single indentation measurement using a Berkovich indenter (triangular pyramid, indenter interior angle: 142.35°, angle between the center line and the surface: 65.35°, indenter aspect ratio: 1:8) at 25°C. As shown in FIG. 3, the measurement was performed by contacting the indenter with the approximate center of the adhesive layer of the measurement sample. The indenter was pressed and pulled out at a speed of 500 nm / sec. The indenter was pressed into the adhesive layer to a depth of 2000 nm over 4 seconds, and the holding time was set to 0 seconds. Next, the indenter was pulled out from the adhesive layer at the same speed as the pressing, and the time it took for the indenter to be pulled out from the adhesive layer was measured. 2 ) and the hardness (nanoindentation hardness) (MPa) was calculated by Pmax / A. For pressure-sensitive adhesive tapes with a pressure-sensitive adhesive layer thickness of less than 20 μm, pressure-sensitive adhesive tapes for evaluation with a pressure-sensitive adhesive layer thickness of 20 μm were prepared and evaluated by the above method. A load-displacement curve was created from the load and the indentation depth during the above measurement. The distance at which the displacement became negative (i.e., the amount of displacement from the point at which the displacement became 0 nm to the point at which the load became 0 on the unloading curve) was measured from the unloading curve, and this was taken as the unloading curve displacement (μm). If the unloading curve displacement is 8000 μm or less, the cutting ability may be good. The measurements were performed using three samples, and the average values were used as the nanoindentation hardness and the displacement amount of the unloading curve.
[0072] 3. Embeddability The adhesive tapes obtained in the examples and comparative examples were cut to 230 cm x 400 cm. The cut adhesive tapes were attached to a wafer (8 inches, bump height 75 μm, diameter 90 μm, pitch 200 μm) using a tape attachment device (manufactured by Nitto Seiki Co., Ltd., product name: DR-3000III). The attachment was performed under the following conditions. Roller pressure: 0.40MPa Roller speed: 5mm / sec Table temperature: 80℃ After attachment, the state of attachment of the adhesive sheet and the wafer was observed using a laser microscope (magnification: 100 times). In addition, the adhesive tape and the wafer were photographed from the adhesive tape side with the adhesive tape facing up, and the image was binarized (8-bit grayscale, brightness: 0-255, threshold: 114) using image analysis software (Image J (free software)). Then, five bumps were randomly selected from the wafer, and the number of dots used to display one bump was measured. The image of only the bump without the tape attached had 220 dots, and the closer the dot number measured with the adhesive tape attached to 220, the better the embedding property. Note that when adhesive tape is attached to a semiconductor wafer with bumps, the dot number is usually about 820. The average dot number of any five bumps of 830 or less was evaluated as ◯ (good), and the average dot number exceeding 830 was evaluated as × (bad).
[0073] 4. Thread pulling The adhesive tapes obtained in the examples and comparative examples were cut to 230 cm x 400 cm. The cut adhesive tape was attached to an 8-inch silicon mirror wafer using a tape attachment device (manufactured by Nitto Seiki Co., Ltd., product name: DR-3000III), and then the adhesive tape attached to the wafer was cut to match the shape of the wafer. For cutting, a cutter blade dedicated to the tape attachment device DR-3000III was used, and a new cutter blade was used for each measurement. The attachment was performed under the following conditions. Roller pressure: 0.27MPa Roller speed: 20mm / sec Table temperature: 23℃ Cutter speed: 200mm / sec Cutter temperature: 180℃ The laminate of the adhesive tape and the wafer after cutting was observed from the side of the wafer with a digital microscope, and the intermediate layer was evaluated as "absent" if there was no stringiness, and "present" if there was stringiness. It is preferable that the intermediate layer does not have stringiness.
[0074] [Table 2]
[0075] The adhesive tape of the embodiment of the present invention had excellent surface embedding properties for the surface of a semiconductor wafer having irregularities. In addition, stringiness was suppressed, and damage to the wafer during peeling could be suppressed. [Industrial Applicability]
[0076] The backgrind tape according to the embodiment of the present invention can be suitably used as a backgrind tape for semiconductor wafer processing. [Explanation of symbols]
[0077] 10 Base material 20 Middle Class 30 Adhesive layer 100 Backgrind Tape 200 indenter 300 Support
Claims
1. The adhesive sheet includes a substrate, an intermediate layer, and a pressure-sensitive adhesive layer. the nanoindentation hardness (25° C.) of the intermediate layer is 0.001 MPa to 0.200 MPa; the pressure-sensitive adhesive layer has a nanoindentation hardness (25° C.) of 0.001 MPa to 0.080 MPa; At least one of the intermediate layer and the pressure-sensitive adhesive layer has a thickness of 50 μm or more; A backgrind tape, wherein the layer having a thickness of 50 μm or more has an unloading curve displacement of 8000 μm or less.
2. 2. The backgrind tape according to claim 1, wherein the product of nanoindentation hardness (MPa) and thickness (μm) of the intermediate layer is 0.050 to 15,000.
3. 2. The backgrind tape according to claim 1, wherein the product of the nanoindentation hardness (MPa) and the thickness (μm) of the pressure-sensitive adhesive layer is 0.001 to 1.
000.
4. The backgrind tape according to claim 1, wherein the pressure-sensitive adhesive layer has a thickness of 1 μm to 50 μm.
5. 2. The backgrind tape according to claim 1, wherein the intermediate layer comprises a (meth)acrylic polymer obtained by polymerizing a monomer composition containing a monomer having a glass transition temperature of 80° C. or higher.
6. The backgrind tape according to claim 5, wherein the intermediate layer comprises a (meth)acrylic polymer obtained by polymerizing a monomer composition containing 5% by weight to 50% by weight of a monomer having a glass transition temperature of 80° C. or higher.
7. The backgrind tape according to claim 1 , wherein the adhesive layer is formed of an ultraviolet-curable adhesive.
8. The backgrind tape according to claim 1 , wherein the adhesive layer is formed of an adhesive containing a multifunctional acrylate.
9. It is bonded to a semiconductor wafer on which bumps are formed, The backgrind tape of claim 1, wherein the height (μm) of the bump, the sum of the thickness (μm) of the adhesive layer and the thickness (μm) of the intermediate layer satisfy the relationship: height (μm) of the bump < thickness (μm) of the adhesive layer + thickness (μm) of the intermediate layer.
10. It is bonded to a semiconductor wafer on which bumps are formed, 2. The backgrind tape according to claim 1, wherein the height (μm) of the bumps and the thickness (μm) of the intermediate layer satisfy the relationship: height (μm) of bumps < thickness (μm) of intermediate layer.
Citation Information
Patent Citations
Adhesive film
JP2019065168A
Back grinding tape
JP2020025016A
Optical laminate and method for manufacturing the same
JP2021091117A
Glass unit manufacturing method and adhesive sheet
JP2021509427A
Semiconductor wafer surface protection film and method for manufacturing semiconductor device
WO2017006549A1