Tyrosinase activity inhibitor
Cellulose with a cellulose I type crystal structure, particularly in the form of nanofibers or nanocrystals with anionic functional groups, addresses the need for effective tyrosinase inhibition in cosmetics, offering both whitening and moisturizing benefits.
Patent Information
- Application Number
- JP2023070198
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
There is a need for new uses of cellulose to make more effective use of this naturally-derived material, particularly in cosmetic applications where water-soluble carboxymethyl cellulose lacks tyrosinase activity inhibition, and existing cellulose derivatives do not effectively inhibit tyrosinase activity.
Utilizing cellulose with a cellulose I type crystal structure, such as cellulose nanofibers or nanocrystals, which can contain anionic functional groups like sulfate ester or carboxy groups, to inhibit tyrosinase activity.
The cellulose I type crystal structure effectively inhibits tyrosinase activity, providing a whitening effect and moisturizing properties in cosmetic formulations, enhancing their performance beyond traditional thickening functions.
Smart Images

Figure 2024155462000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a tyrosinase activity inhibitor, and more particularly to a tyrosinase activity inhibitor containing cellulose having a cellulose type I crystal structure as an active ingredient. [Background technology]
[0002] Due to growing environmental awareness, research is being conducted around the world to put biomass-derived materials to practical use. For example, cellulose is a component of plant cell walls and is the largest biomass resource on earth. When using lignocellulosic biomass such as wood (wood chips, etc.), herbs, coconut shells, and nut shells as raw materials, if the components cellulose, lignin, and hemicellulose can be used in industry without waste, it will contribute greatly to both circular resource utilization and CO2 fixation.
[0003] For example, Patent Document 1 describes particles containing carboxymethylcellulose, which have a sphericity of 0.85 or more, an average particle diameter d1 of 0.01 to 20 μm, and a maximum particle diameter d m The document describes carboxymethylcellulose particles having a diameter of less than 30 μm and a free carboxylic acid group ratio of carboxymethylcellulose, expressed as "free carboxylic acid groups not forming a salt" / ("carboxylic acid groups which have formed a salt"+"free carboxylic acid groups not forming a salt") of 0.8 or more.
[0004] Furthermore, when cellulose is made into nano-sized cellulose (also known as "nanocellulose") such as cellulose nanofiber (also known as "CNF") or cellulose nanocrystal (also known as "CNC"), it leads to improved physical properties such as strength, flexibility, and elongation when combined with resin, rubber, and even concrete, and is therefore attracting attention as a new environmentally friendly material.
[0005] For example, Patent Document 2 describes cellulose nanofibers having an average fiber diameter of 1 nm to 500 nm and having hydroxyl groups on the surface of the cellulose nanofibers modified by sulfate esterification, wherein a 0.3 mass% aqueous dispersion of the sulfate esterified cellulose nanofiber has a viscosity of 500 mPa·S to 25,000 mPa·S at 25°C and a 0.3 mass% aqueous dispersion of the sulfate esterified cellulose nanofiber has a TI value of 3 to 30 at 25°C.
[0006] Patent Document 3 describes fine cellulose fibers having a maximum fiber diameter of 1000 nm or less and a number average fiber diameter of 2 to 150 nm, in which some of the hydroxyl groups of the cellulose are oxidized to at least one functional group selected from the group consisting of carboxyl groups and aldehyde groups, and which have a cellulose type I crystal structure.
[0007] Patent document 4 describes proteinaceous cellulose microparticles comprising cellulose nanocrystals and one or more peptides, one or more proteins, or a mixture thereof, wherein the nanocrystals and the peptides and / or proteins aggregate together to form the microparticles. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2021-107482 A [Patent Document 2] International Publication No. 2018 / 131721 [Patent Document 3] JP 2008-1728 A [Patent Document 4] Special Publication No. 2022-531941 Summary of the Invention [Problem to be solved by the invention]
[0009] When it comes to cosmetic ingredients, natural ingredients are preferred due to growing environmental awareness, and plant-derived materials are also preferred from the perspective of animal welfare.
[0010] For example, carboxymethylcellulose (CMC), a representative cellulose-based material described in Patent Document 1, is water-soluble and has a thickening function, and is therefore used as a thickening agent for cosmetic ingredients.
[0011] In addition, cellulose nanofibers (CNFs) described in Patent Documents 2 to 4 are obtained by subjecting cellulose raw materials such as pulp to sulfate esterification, oxidation, or sulfuric acid hydrolysis, and then mechanically grinding them in water, and have a natural type I crystal structure and an average fiber width (fiber diameter (equivalent circle diameter)) of less than 100 nm. These CNFs also disperse stably in water due to the ionic functional groups present on their surface, and have a thickening function, so their use as thickeners for cosmetic raw materials is being considered.
[0012] Therefore, an object of the present invention is to provide a new use of cellulose for more effective use of cellulose. [Means for solving the problem]
[0013] The present inventors conducted extensive research to provide new uses for cellulose and as a result discovered that cellulose having a cellulose type I crystal structure has the effect of inhibiting tyrosinase activity, thereby completing the present invention.
[0014] That is, the gist of the present invention is as follows. (1) A tyrosinase activity inhibitor containing cellulose having a cellulose type I crystal structure as an active ingredient. (2) The tyrosinase activity inhibitor according to (1), wherein the cellulose is a cellulose nanofiber. (3) The tyrosinase activity inhibitor according to (1), wherein the cellulose is a cellulose nanocrystal. (4) The tyrosinase activity inhibitor according to (2), wherein the average fiber width of the cellulose nanofibers is 1 nm to 1,000 nm. (5) The tyrosinase activity inhibitor according to any one of (1) to (4), wherein the cellulose has a functional group on the surface. (6) The tyrosinase activity inhibitor according to (5), wherein the functional group is an anionic functional group. (7) The tyrosinase activity inhibitor according to (6), wherein the anionic functional group is a sulfate ester group and / or a carboxy group. (8) The tyrosinase activity inhibitor according to any one of (1) to (7), further comprising water. (9) The tyrosinase activity inhibitor according to any one of (1) to (7), which is in the form of a gel, an emulsion, a powder, a nonwoven fabric complex, or a film. (10) A whitening cosmetic preparation comprising the tyrosinase activity inhibitor according to any one of (1) to (9). Effect of the Invention
[0015] The present invention provides a new use of cellulose for more effective use of cellulose. [Brief description of the drawings]
[0016] [Figure 1] 1 is a graph showing the evaluation results of tyrosinase monophenolase activity in Examples 1 to 4 and Comparative Example 1. [Diagram 2] 1 is a graph showing the evaluation results of tyrosinase diphenolase activity in Examples 1 to 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Preferred embodiments of the present invention will now be described in detail. In this specification, the features of the present invention will be described with reference to the drawings as appropriate. The tyrosinase activity inhibitor of the present invention is not limited to the following embodiments, and can be embodied in various forms including modifications and improvements that can be made by those skilled in the art within the scope of the gist of the present invention.
[0018] In this specification, a range expressed by "numeric value to numerical value" means a range including the numerical value. For example, the above-mentioned "1 nm to 500 nm" indicates "1 nm or more and 500 nm or less", that is, a range from 1 nm to 500 nm including 1 nm and 500 nm.
[0019] The present invention relates to a tyrosinase activity inhibitor containing cellulose having a cellulose type I crystal structure as an active ingredient.
[0020] Here, the tyrosinase activity inhibitor means a composition containing a compound having the property of inhibiting tyrosinase activity.
[0021] Here, cellulose is a polysaccharide in which glucose is bonded via β-1,4-glycosidic bonds (C6H 10 O5) n As shown in the figure.
[0022] The cellulose type I crystal structure is a crystal structure inherent to natural cellulose, and can be identified, for example, by solid-state NMR or the degree of crystallinity described below.
[0023] There are no limitations on the degree of crystallinity of cellulose as long as it has a cellulose type I crystal structure. The degree of crystallinity of the cellulose type I crystal structure is usually 15% to 95%, and preferably 25% to 90%.
[0024] The crystallinity of the cellulose type I crystal structure can be determined by X-ray diffraction. The crystallinity of the cellulose type I crystal structure can be determined, for example, by measuring the diffraction intensity of the lattice plane (200 plane) (diffraction angle 2θ=22.6°) and the diffraction intensity of the amorphous part (lowest part between the 200 plane and the 110 plane, diffraction angle 2θ=18.5°) using an X-ray diffraction device (e.g., RINT-TTR III, manufactured by Rigaku Corporation), and calculating the crystallinity according to the following formula by the Segal method. Crystallinity of I-type crystal (%) = {1-(diffraction intensity at 18.5° / diffraction intensity at 22.6°)} x 100
[0025] As described above, the cellulose is not limited as long as it has a cellulose type I crystal structure. Examples of the cellulose include cellulose microfiber (CMF), cellulose nanofiber (CNF), and cellulose nanocrystal (CNC).
[0026] Cellulose microfibers are cellulose fibers made of cellulose and have an average fiber width on the order of microns. Therefore, the average fiber width (fiber diameter (equivalent circle diameter)) of cellulose microfibers is usually in the range of 1 μm to 1000 μm. The average fiber length of cellulose microfibers is not limited, but is usually 100 μm or more.
[0027] Cellulose nanofibers are cellulose fibers made of cellulose and have an average fiber width on the nano order. Therefore, the average fiber width (fiber diameter (equivalent circle diameter)) of cellulose nanofibers is usually in the range of 1 nm to 1000 nm. The average fiber length of cellulose nanofibers is not limited, but is usually in the range of 0.1 μm to 10 μm.
[0028] Cellulose nanocrystals are particulate crystals made of cellulose and have an average particle size on the nano-order. Therefore, the average particle size of cellulose nanocrystals is not limited, but is usually 1 nm to 1000 nm in terms of the equivalent circle diameter.
[0029] The average fiber width, average fiber length, and average particle size are not limited, but can be measured, for example, by using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation) to measure the fiber width and fiber length or equivalent circle diameter of 50 arbitrarily selected fibers or particles and calculating the arithmetic average value for each.
[0030] The cellulose microfiber, cellulose nanofiber, or cellulose nanocrystal (hereinafter also referred to as celluloses) may have a functional group on the surface. Examples of the functional group include anionic functional groups, cationic functional groups, and nonionic functional groups. The functional group is preferably anionic functional groups.
[0031] The cellulose having an anionic functional group is a cellulose in which a part of the OH group of the glucose unit in the cellulose is modified to an anion. Examples of the anionic functional group include, but are not limited to, a sulfate ester group, a carboxyl group, a phosphate ester group, a phosphite ester group, and a xanthate group. As the anionic functional group, a sulfate ester group and a carboxyl group are preferred.
[0032] For example, celluloses having sulfate ester groups are also called sulfated cellulose microfibers, sulfated cellulose nanofibers, or sulfated nanocrystals, and are celluloses in which at least one of the OH groups in the cellulose constituting the celluloses is substituted with a sulfate ester group. The sulfate ester groups of the celluloses having sulfate ester groups are preferably sulfate ester groups represented by the following formula (1) (wherein M represents a monovalent to trivalent cation).
[0033] [ka] In the general formula (I), n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.)
[0034] M in general formula (I) n+ Examples of the monovalent to trivalent cations represented by the formula (I) include hydrogen ions, metal ions, and ammonium ions. n+ When -OSO3- is a divalent or trivalent cation, the cation forms an ionic bond with two or three -OSO3-.
[0035] Examples of the metal ion include an alkali metal ion, an alkaline earth metal ion, a transition metal ion, and other metal ions.
[0036] Here, examples of alkali metal ions include lithium ions, sodium ions, potassium ions, rubidium ions, and cesium ions. Examples of alkaline earth metal ions include calcium ions and strontium ions. Examples of transition metals include iron ions, nickel ions, palladium ions, copper ions, and silver ions. Examples of other metals include beryllium ions, magnesium ions, zinc ions, and aluminum ions.
[0037] The ammonium ion is NH4 + Not only NH4 + Examples of ammonium ions include those derived from various amines in which one or more hydrogen atoms are replaced by organic groups. For example, NH + , quaternary ammonium cations, alkanolamine ions, pyridinium ions, etc.
[0038] M n+ The cation represented by the formula (I) is preferably a hydrogen ion, a sodium ion, a potassium ion, a calcium ion, or a quaternary ammonium cation. The above-listed cations may be used alone or in combination of two or more.
[0039] The sulfate modification rate of celluloses having sulfate ester groups can be set to any appropriate value depending on the application. The sulfate modification rate of celluloses having sulfate ester groups is expressed as the sulfur content (mmol) derived from sulfate ester groups per 1 g of celluloses having sulfate ester groups. The sulfur content (mmol / g) in the celluloses having sulfate ester groups is not limited, but is usually 0.1 mmol / g to 5 mmol / g, and preferably 0.3 mmol / g to 4 mmol / g.
[0040] The sulfur content (mmol / g) in celluloses having sulfate ester groups can be confirmed, for example, by combustion absorption-ion chromatography (IC) or infrared spectroscopy (IR). The sulfur content of celluloses having sulfate ester groups can be measured, for example, by the following method.
[0041] Measurement method: Combustion absorption - IC Measurement equipment: ICS-1500 manufactured by Nippon Dionex Co., Ltd. Measurement conditions: A sample (cellulose with sulfate ester groups) is weighed onto a magnetic board and burned in an oxygen atmosphere (flow rate: 1.5 L / min) in a ring furnace (1350°C). The generated gas components are absorbed in 3% hydrogen peroxide (20 ml) to obtain an absorbed solution. The absorbed solution obtained is made up to 100 ml with pure water, and the diluted solution is subjected to ion chromatography. The amount of sulfate ion (mmol) per 1 g of cellulose nanofiber is calculated from the measurement results.
[0042] For example, celluloses having carboxy groups are also called oxidized cellulose, oxidized cellulose nanofibers, or oxidized cellulose nanocrystals, or TEMPO oxidized cellulose, TEMPO oxidized cellulose nanofibers, or TEMPO oxidized cellulose nanocrystals, and are celluloses in which at least one of the OH groups in the cellulose that constitutes the celluloses has been substituted with a carboxy group.
[0043] The oxidation rate in celluloses having a carboxy group can be set to any appropriate value depending on the application. The oxidation rate in celluloses having a carboxy group is expressed as the amount of carboxy groups (mmol) per 1 g of celluloses having a carboxy group. The amount of carboxy groups introduced in the celluloses having a carboxy group (mmol / g) is not limited, but is usually 0.1 mmol / g to 5 mmol / g, and preferably 0.3 mmol / g to 4 mmol / g.
[0044] The amount of carboxyl groups introduced into the cellulose having a carboxyl group (mmol / g) can be confirmed, for example, by alkali titration. The amount of carboxyl groups introduced into the cellulose having a carboxyl group can be measured, for example, by the following method.
[0045] Measurement method: Alkali titration Measurement conditions: The sample (celluloses having carboxy groups) is weighed, 60 ml of a 0.5 to 1% by mass slurry is prepared, and the pH is adjusted to approximately 2.5 using 0.1 M aqueous hydrochloric acid, after which 0.05 M aqueous sodium hydroxide solution is added dropwise and electrical conductivity is measured. Measurements are continued until the pH reaches approximately 11. The amount of functional groups of the carboxy groups is determined using the following formula from the amount of sodium hydroxide (V) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual. Amount of carboxyl functional group (mmol / g) = V (ml) × 0.05 / mass of cellulose (g)
[0046] The celluloses having a sulfate ester group or a carboxy group may have other functional groups in addition to the sulfate ester group or the carboxy group. Here, when the celluloses having a sulfate ester group or a carboxy group have other functional groups, the other functional groups are substituted with at least one of the OH groups in the cellulose constituting the celluloses. Examples of the other functional groups include, but are not limited to, anionic functional groups and their salts, ester groups, ether groups, acyl groups, aldehyde groups, alkyl groups, alkylene groups, aryl groups, and combinations of two or more of these. When the other functional groups are combinations of two or more, the content ratio of each functional group is not limited. Among them, the other functional groups are preferably anionic functional groups and their salts, or acyl groups from the viewpoint of nano-dispersibility. As the anionic functional groups and their salts, particularly sulfate ester groups (in the case of celluloses having a carboxy group), carboxy groups (in the case of celluloses having a sulfate ester group), phosphate ester groups, phosphite ester groups, and xanthate groups are preferred. When the anionic functional groups are in the form of salts, sodium salts, potassium salts, and calcium salts are particularly preferred from the viewpoint of nano-dispersibility. A particularly preferred acyl group is an acetyl group from the viewpoint of nano-dispersibility.
[0047] In the case of cellulose microfibers, the average fiber width of the cellulose microfibers is not limited, but is equivalent to the average fiber width of the normal cellulose microfibers defined above, and is usually in the range of 1 μm to 1000 μm. The average fiber width of the cellulose microfibers is preferably 1 μm to 800 μm, more preferably 1 μm to 500 μm.
[0048] The average fiber length of the cellulose microfiber is not limited, but is the same as the average fiber length of the normal cellulose microfiber defined above, and is usually 10 μm or more, for example, 100 μm or more, or may be 1000 μm or more. The upper limit of the average fiber length of the cellulose microfiber is not limited, and the average fiber length of the cellulose microfiber can be, for example, several tens of meters.
[0049] As the cellulose microfiber, for example, wood pulp, cotton, etc. can be used as it is. Also, the fibers such as wood pulp and cotton may be subjected to a slight defibration treatment to produce cellulose microfiber. Furthermore, the cellulose microfiber can also be produced by spinning the cellulose nanofiber described below.
[0050] By using cellulose microfibers, costs can be reduced because no chemical treatment is required for production, or even if chemical treatment is performed, the degree of treatment can be light, compared to cellulose nanofibers, for example. Also, cellulose nanofibers tend to have high viscosity, so they are dispersed in water at a solid content of about 2%, whereas cellulose microfibers can be dispersed in water even at a solid content of 5% or more, making them easy to handle.
[0051] In the case of cellulose nanofibers, the average fiber width of the cellulose nanofibers is not limited, but is equivalent to the fiber width of the cellulose nanofibers defined above, and is usually in the range of 1 nm to 1000 nm. The average fiber width of the cellulose nanofibers is preferably 1 nm to 500 nm, and more preferably 1 nm to 100 nm. If the average fiber width is less than 1 nm, the performance aspects such as the strength of the nanofibers may be reduced.
[0052] The average fiber length of the cellulose nanofibers is not limited, but is the same as the fiber length of the cellulose nanofibers defined above, and is usually 0.1 μm or more and 10 μm or less, and preferably 0.1 μm or more and 6 μm or less.
[0053] Cellulose nanofibers can be produced using, for example, plant-derived components such as wood pulp and cotton, cellulose produced by acetic bacteria, and / or non-plant components such as the exoskeleton of sea squirts.
[0054] By using cellulose nanofibers, it is possible to obtain an aqueous dispersion that has excellent dispersibility in water and does not settle for a long period of time. In addition, since cellulose nanofibers have a thickening effect, the viscosity of an aqueous dispersion containing cellulose nanofibers increases and the dispersion has thixotropy.
[0055] In the case of cellulose nanocrystals, the average particle size of the cellulose nanocrystals is not limited, but is equivalent to the average particle size of the cellulose nanocrystals defined above, and is usually in the range of 1 nm to 1000 nm as a circle equivalent diameter. The average particle size of the cellulose nanocrystals is preferably 1 nm to 750 nm, more preferably 1 nm to 500 nm.
[0056] Cellulose nanocrystals can be produced using, for example, plant-derived components such as wood pulp and cotton, cellulose produced by acetic bacteria, and / or non-plant components such as the exoskeleton of sea squirts.
[0057] By using cellulose nanocrystals, it is possible to obtain an aqueous dispersion that has excellent dispersibility in water and does not settle for a long period of time. In addition, since cellulose nanocrystals have a thickening effect, the viscosity of an aqueous dispersion containing cellulose nanocrystals increases and the dispersion has thixotropy.
[0058] The average fiber width, average fiber length, or average particle size of cellulose can be measured by, for example, measuring the fiber width (fiber diameter (equivalent circle diameter)), fiber length, or equivalent circle diameter of 50 arbitrarily selected fibers or particles using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation) as described above, and calculating the arithmetic mean value. The average fiber width, average fiber length, or average particle size can be set within a desired range by adjusting the concentration of a reagent such as sulfuric acid, the amount of pulp relative to the reaction solution, and the reaction time.
[0059] In addition, celluloses are hygroscopic. That is, celluloses usually contain water when stored in the air. Therefore, the celluloses of the present invention, i.e., the celluloses contained in the tyrosinase activity inhibitor of the present invention, may also contain water. In the celluloses of the present invention, the water content is not limited, but is usually 1% by mass to 10% by mass, preferably 1% by mass to 5% by mass, based on the total mass of the celluloses. As long as the celluloses of the present invention have a cellulose I type crystal structure, they have a tyrosinase activity inhibitory effect even if they contain water.
[0060] The cellulose used in the present invention may have a cellulose type I crystal structure known in the art, and the production method thereof is also known.
[0061] The tyrosinase activity inhibitor of the present invention may further contain a solvent, for example, water, alcohol, for example, ethanol, oil, or a mixture thereof, or an emulsion, for example, an emulsion of oil and water.
[0062] When the tyrosinase activity inhibitor of the present invention contains a solvent, the content of the solvent is usually 0.1% by mass to 99.99% by mass, for example, 1% by mass to 99.99% by mass, based on the total mass of the tyrosinase activity inhibitor. The tyrosinase activity inhibitor of the present invention may be composed of a cellulose and a solvent.
[0063] Even if the tyrosinase activity inhibitor of the present invention contains a solvent, the cellulose contained in the tyrosinase activity inhibitor of the present invention has a tyrosinase activity inhibitory effect so long as it has a cellulose I type crystal structure.
[0064] In the tyrosinase activity inhibitor of the present invention, the solvent is preferably water. When the tyrosinase activity inhibitor of the present invention contains water, the content of water is usually 1% by mass to 99.99% by mass, for example 5% by mass to 99.99% by mass, based on the total mass of the tyrosinase activity inhibitor. The tyrosinase activity inhibitor of the present invention may be composed of cellulose and water.
[0065] Even if the tyrosinase activity inhibitor of the present invention contains water, the cellulose contained in the tyrosinase activity inhibitor of the present invention has a tyrosinase activity inhibitory effect so long as it has a cellulose I type crystal structure.
[0066] The tyrosinase activity inhibitor of the present invention may further comprise one or more additives.
[0067] Examples of additives include powder components, fats and oils, waxes, hydrocarbon oils, higher fatty acids, higher alcohols, synthetic ester oils, silicone oils, water-soluble polymers, sequestering agents, lower alcohols, polyhydric alcohols, sugars, amino acids, organic amines, polymer emulsions, vitamins, and from the standpoint of function, surfactants, moisturizers, thickeners, film-forming agents, UV absorbers, skin nutrients, antioxidants, antioxidant assistants, dispersants, excipients, lubricants, binders, disintegrants, solubilizers, suspending agents, isotonicity agents, buffers, pH adjusters, pH stabilizers, soothing agents, preservatives, antioxidants, colorants, sweeteners, adsorbents, humectants, antibacterial agents, and the like.
[0068] The content of the additives is not limited because it varies depending on the application required for the additives. When the tyrosinase activity inhibitor of the present invention contains additives, the total content of the additives is, for example, usually 0.1% by mass to 99.99% by mass, preferably 1% by mass to 99.99% by mass, based on the total mass of the tyrosinase activity inhibitor. The tyrosinase activity inhibitor of the present invention may be composed of celluloses and additives.
[0069] The shape of the tyrosinase activity inhibitor of the present invention is not limited. The tyrosinase activity inhibitor of the present invention may be any shape, such as a powder, a sphere, an ellipse, a polygon, or a plate, for example, a solid shape such as a nonwoven fabric complex or a film, a semisolid shape such as a gel or a paste, or an emulsion or a dispersion. In order to mold the tyrosinase activity inhibitor of the present invention into the above shape, for example, one or more carriers, preferably pharma- ceutically acceptable carriers, such as the above solvents and the above additives, may be blended.
[0070] When the tyrosinase activity inhibitor of the present invention is mixed with water to prepare an aqueous dispersion in which the concentration of the cellulose is 0.5 mass% based on the total mass of the aqueous dispersion, the aqueous dispersion has a viscosity measured at 6 rpm at 25°C of typically 100 mPa·s to 100,000 mPa·s, and preferably 300 mPa·s to 50,000 mPa·s.
[0071] When the tyrosinase activity inhibitor of the present invention is mixed with water to prepare an aqueous dispersion in which the concentration of the cellulose is 0.5 mass% based on the total mass of the aqueous dispersion, the aqueous dispersion has a viscosity measured at 60 rpm at 25°C of typically 10 mPa·s to 20,000 mPa·s, and preferably 30 mPa·s to 10,000 mPa·s.
[0072] When the tyrosinase activity inhibitor of the present invention is mixed with water to prepare an aqueous dispersion in which the concentration of the cellulose is 0.5 mass% based on the total mass of the aqueous dispersion, the TI value (6 rpm viscosity / 60 rpm viscosity) calculated from the viscosities measured at 6 rpm and 60 rpm at 25°C of the aqueous dispersion is usually 1 to 10, and preferably 2 to 7.
[0073] Since the tyrosinase activity inhibitor of the present invention has a viscosity and / or TI value within the above range, it can also act as a thickener or a feel improver when blended in, for example, a cosmetic composition.
[0074] The tyrosinase activity inhibitor of the present invention can be produced by a method known in the art, for example, by mixing cellulose, a carrier, preferably a pharma- ceutically acceptable carrier, such as the above-mentioned solvent and the above-mentioned additives, and optionally pulverizing the mixture.
[0075] The tyrosinase activity inhibitor of the present invention may be used as a whitening cosmetic composition either as it is or by adding it to a cosmetic composition.
[0076] Therefore, the present invention also relates to a whitening cosmetic composition containing the tyrosinase activity inhibitor of the present invention.
[0077] The whitening cosmetic composition of the present invention may contain, in addition to the tyrosinase activity inhibitor of the present invention, ingredients conventionally used in cosmetics, such as one or more carriers, preferably pharma- ceutically acceptable carriers, such as the above-mentioned solvents and additives, etc. The details and blending amounts of each ingredient may be those known in the art.
[0078] The whitening cosmetic composition of the present invention can be produced by a method known in the art, for example, by mixing cellulose, a carrier, particularly a pharma- ceutically acceptable carrier, and the like, and optionally pulverizing and molding the mixture.
[0079] In human skin cells, the enzyme tyrosinase produces melanin, which causes sunburn and age spots. In other words, if tyrosinase activity can be inhibited, the amount of melanin produced can be reduced and the occurrence of sunburn and age spots can be inhibited. Therefore, whitening cosmetics contain a drug that inhibits tyrosinase activity. However, carboxymethylcellulose does not have a tyrosinase activity inhibitory function, and it was not known that celluloses have a tyrosinase activity inhibitory function. Therefore, celluloses are not used as tyrosinase activity inhibitors in whitening cosmetics, and tyrosinase activity inhibitors other than celluloses are separately blended. In the present invention, it has been found that celluloses having a cellulose I type crystal structure have a tyrosinase activity inhibitory effect in addition to the thickening and moisturizing properties that have been used so far for celluloses, and the anti-aging properties due to the hyaluronidase activity inhibitory function of sulfated cellulose. Therefore, according to the present invention, celluloses having a cellulose I type crystal structure can be blended as tyrosinase activity inhibitors in whitening cosmetics. The tyrosinase activity inhibitor of the present invention can provide both whitening and moisturizing effects to whitening cosmetics by using it in place of a conventional tyrosinase activity inhibitor or together with a conventional tyrosinase activity inhibitor. EXAMPLES
[0080] The present invention will be described in more detail below using examples, but the technical scope of the present invention is not limited to these examples.
[0081] I. Sample Preparation <Example 1: Method for producing low-substituted sulfate esterified cellulose nanofiber (CNF)> 90 g of dimethyl sulfoxide (DMSO), 10 g of acetic anhydride, and 1 g of sulfuric acid were placed in a 300 ml sample bottle and stirred for about 30 seconds at room temperature of 23° C. using a magnetic stirrer to prepare a reaction solution.
[0082] Next, 3 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the reaction solution, and the mixture was stirred for an additional 4 hours at room temperature of 23°C to carry out a sulfate esterification reaction. After stirring, 200 g of distilled water was added to the pulp-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0083] An additional 300 g of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washings. After washing, the sulfated pulp containing water was dried at 105°C and weighed to measure the moisture content.
[0084] Distilled water was added to the sulfated pulp containing water obtained by washing in an amount to give a solids concentration of 0.5%, and the mixture was then stirred using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of cellulose nanofibers having sulfate ester groups (sulfated CNF) with a concentration of 0.5% by mass as in Example 1.
[0085] <Example 2: Method for producing highly substituted sulfated CNF> In Example 2, a uniform aqueous dispersion of cellulose nanofibers having sulfate ester groups (sulfate-esterified CNF) with a concentration of 0.5% by mass was obtained in the same manner as in Example 1, except that the amount of sulfuric acid used was changed from 1 g to 2 g.
[0086] <Example 3: Method for producing oxidized CNF> 0.13 mmol of 2,2,6,6-tetramethylpiperidine-N-oxyl (TEMPO) and 10 mmol of sodium bromide were dissolved in water to obtain a 250 mL aqueous solution. 3 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to this aqueous solution and stirred until the pulp was uniformly dispersed. After the temperature of the mixture was brought to 20°C, 32 mmol of an aqueous solution of sodium hypochlorite (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to start the oxidation reaction. During the reaction, the temperature of the reaction system was kept at 20°C, and the pH was maintained at 10 by successively adding a 5% aqueous solution of sodium hydroxide. After the reaction for 3 hours, the supernatant was removed by centrifugation.
[0087] The precipitate was mixed with 300 g of distilled water and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washings. After washing, the water-containing carboxylated pulp was dried at 105°C and weighed to measure the moisture content.
[0088] Distilled water was added to the carboxylated pulp containing water obtained by washing in an amount to give a solids concentration of 0.5%, and then the mixture was processed in a mixer (G5200, manufactured by Biolomix) to obtain an aqueous dispersion of carboxylated CNF (oxidized CNF) with a concentration of 0.5% by mass as Example 3.
[0089] <Example 4: Method for producing cellulose nanocrystals (CNC)> 3 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to 250 mL of 64% by mass sulfuric acid and stirred for an additional hour at room temperature of 23° C. to carry out the reaction. After stirring, 200 g of distilled water was added to the pulp-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0090] An additional 300 g of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washings. After washing, the water-containing sulfuric acid hydrolyzed pulp was dried at 105°C and weighed to measure the moisture content.
[0091] Distilled water was added to the water-containing sulfuric acid hydrolyzed pulp obtained by washing in an amount to give a solids concentration of 1%, and the mixture was then processed in a mixer (G5200, manufactured by Biolomix) to obtain an aqueous dispersion of CNC with a concentration of 0.5% by mass as Example 4.
[0092] <Comparative Example 1: Method for producing carboxymethyl cellulose (CMC)> Distilled water was added to 3 g of CMC (manufactured by Fuji Film Wako) to make a total volume of 300 g, and the mixture was stirred until the CMC was completely dissolved in the distilled water, thereby obtaining an aqueous solution of CMC with a concentration of 0.5% by mass.
[0093] II. Analysis of Samples <Quantitative determination of the amount of introduced substituent> Measurement of sulfate ester group introduction amount The sulfur content as the amount of substituents of sulfated CNF and CNC was quantified using the combustion absorption-IC method. The specific method is as follows.
[0094] First, 0.01 g of dried sulfated CNF or CNC was weighed and placed on a magnetic board, and burned in a circular furnace (1350°C) under an oxygen atmosphere (flow rate: 1.5 L / min), and the generated gas components were absorbed in 3% hydrogen peroxide (20 ml). The obtained absorbed liquid was diluted to 100 ml with pure water, and the sulfate ion concentration (mass%) of the diluted liquid was measured by ion chromatography, and the amount of sulfate ester group introduced per 1 g of sample (mmol / g) was calculated.
[0095] Measurement of amount of carboxyl group introduced The amount of carboxyl groups introduced into the oxidized CNF and CMC was measured by alkaline titration. The specific method is as follows.
[0096] A 60-ml slurry of 0.5 to 1% by mass was prepared from a cellulose sample whose dry mass was precisely weighed. After adjusting the pH to approximately 2.5 with 0.1 M hydrochloric acid aqueous solution, 0.05 M sodium hydroxide aqueous solution was added dropwise to conduct conductivity measurement. The measurement was continued until the pH reached approximately 11. From the amount of sodium hydroxide (V) consumed at the stage of neutralization of the weak acid where the change in conductivity was slow, the functional group amount of carboxyl groups was determined using the following formula. Amount of carboxyl groups introduced (mmol / g) = V (ml) × 0.05 / mass of cellulose (g)
[0097] <Measurement of crystallinity of type I crystal: X-ray diffraction> 0.1 g of the dried cellulose samples of Examples 1 to 4 and Comparative Example 1 were used as evaluation samples. The crystallinity was measured using an X-ray diffractometer (RINT-TTR III, manufactured by Rigaku Corporation), measuring the diffraction intensity of the lattice plane (200 plane) (diffraction angle 2θ = 22.6°) and the diffraction intensity of the amorphous part (the lowest part between the 200 plane and the 110 plane, diffraction angle 2θ = 18.5°), and calculated by the following formula according to the Segal method. Crystallinity of type I crystal (%) = {1 - (diffraction intensity at 18.5° / diffraction intensity at 22.6°)} × 100
[0098] <Measurement of fiber width and particle size: Atomic force microscope (AFM)> The average fiber width or average particle size of the microcrystalline cellulose fibers in the samples obtained in Examples 1 to 4 and Comparative Example 1 was measured by using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation), measuring the fiber width or particle size (equivalent circle diameter) of arbitrarily selected 50 fibers or particles, and taking the arithmetic mean value. The evaluation samples used were prepared by the following method.
[0099] In the atomic force microscope, 0.001% by mass aqueous dispersions of Examples 1 to 4 and Comparative Example 1 were obtained by diluting with distilled water. Subsequently, 30 μL of the 0.001% by mass aqueous dispersion was dropped onto a natural mica (natural muscovite) substrate (15 mm × 15 mm × thickness 0.15 mm) with a micropipette and air-dried for 0.5 hour to obtain an evaluation sample.
[0100] <Viscosity measurement> 100 g of each of the 0.5% by mass aqueous dispersions of Examples 1 to 4 and the 0.5% by mass aqueous solution of Comparative Example 1 was defoamed for 10 seconds using a defoaming device (Awatori Rentaro ARE-310, manufactured by Thinky Corporation) and allowed to stand for 24 hours. Then, using a B-type viscometer (DV-II+, manufactured by Brookfield), the viscosity was measured at 25° C. and at rotation speeds of 6 rpm and 60 rpm, where the viscosity was recorded 10 minutes after the start of the measurement N=3 times and the average value was used.
[0101] <Evaluation of thixotropy index (TI) value> The TI value was determined by measuring the viscosity according to the following method in accordance with JIS K 6833. TI value = ηa / ηb (In the formula, ηa is the viscosity at rotation speed a (rpm), ηb is the viscosity at rotation speed b (rpm), and rotation speed b is 10 times the rotation speed a.)
[0102] In this experiment, the viscosity was measured at 25°C using an E-type rotational viscometer at 6 rpm and 60 rpm, and the viscosity was measured 5 minutes after the start of the measurement, N=3 times, and the average value was used. The TI value was calculated from the following formula. TI value = (viscosity at 25°C and 6 rpm) / (viscosity at 25°C and 60 rpm)
[0103] <Evaluation of light transmittance> 2 mL of each of the 0.5% by mass aqueous dispersions of Examples 1 to 4 and the 0.5% by mass aqueous solution of Comparative Example 1 was placed in a measurement cell, and the light transmittance at a wavelength of 600 nm was measured using a transmittance meter (UV-2600, manufactured by Shimadzu Corporation).
[0104] <Evaluation of tyrosinase activity> -Measurement of tyrosinase monophenolase activity The tyrosinase monophenolase activity of Examples 1 to 4 and Comparative Example 1 was measured using a Human Tyrosinase Inhibitor Screening Kit (Monophenolase, manufactured by SakuLab Science).
[0105] As test substances, distilled water was added to each of Examples 1 to 4 and Comparative Example 1 to prepare samples with concentrations of 0.5 mass %, 0.25 mass %, 0.125 mass %, 0.0625 mass %, and 0.03125 mass %.
[0106] 1) 40 μL of the test substance solution was added to the wells of a 96-well white plate. Distilled water was used as a control. 2) 15 μL of tyrosinase solution was added to each well and the plate was shaken for 5 minutes on a plate shaker. 3) The plate was incubated at 30°C for 15 minutes. 4) 45 μL of a substrate solution containing 1.39 mM tyrosine was added to each well, and after gentle stirring, the plate was transferred to a microplate reader and the optical density (OD) at 495 nm of each well was measured (0 time group). 5) The plate was shaken for 5 minutes on a plate shaker and then incubated at 30°C. Five hours after the addition of the substrate solution, the plate was transferred to a microplate reader and the absorbance at 495 nm of each well was measured for each time period. The final concentrations of the test substances were 0.2%, 0.1%, 0.05%, 0.025%, and 0.0125% by mass.
[0107] -Measurement of tyrosinase diphenolase activity The tyrosinase diphenolase activity of Examples 1 to 4 and Comparative Example 1 was measured using a Human Tyrosinase Inhibitor Screening Kit (Diphenolase, manufactured by SakuLab Science).
[0108] As test substances, distilled water was added to each of Examples 1 to 4 and Comparative Example 1 to prepare samples with concentrations of 0.5 mass %, 0.25 mass %, 0.125 mass %, 0.0625 mass %, and 0.03125 mass %.
[0109] 1) 40 μL of the test substance solution was added to the wells of the 96-well white plate included in the kit. Distilled water was used as a control. A tip with the tip cut off was used when adding the test substance to the solution. 2) 15 μL of enzyme solution was added to each well and the plates were shaken for 5 minutes on a plate shaker. 3) The plate was incubated at 30°C for 15 minutes. 4) 45μL of substrate solution containing 1.39mM L-DOPA was added to each well, the plate was stirred for 5 minutes on a plate shaker, and then incubated at 30℃. 30 and 60 minutes after the addition of the substrate solution, the plate was transferred to a microplate reader, and the absorbance at 495nm of each well was measured for each time period. The final concentrations of the test substances were 0.2%, 0.1%, 0.05%, 0.025%, and 0.0125% by mass.
[0110] -Calculation of tyrosinase activity inhibition rate The tyrosinase activity inhibition rate was calculated using the following formula. Monophenolase activity inhibition rate (%) = {100 - (absorbance of test substance at 0 hours - absorbance of test substance at 5 hours) / (absorbance of control at 0 hours - absorbance of control at 5 hours)} x 100 Diphenolase activity inhibition rate (%) = {100 - (absorbance of test substance in 30 min section - absorbance of test substance in 60 min section) / (absorbance of control in 30 min section - absorbance of control in 60 min section)} x 100
[0111] III. Results The results are shown in Table 1.
[0112] [Table 1]
[0113] Examples 1 to 4 were dried and observed with an AFM, and cellulose with a nano-sized fiber width was observed. Furthermore, the X-ray diffraction patterns of Examples 1 to 4 all had a shape specific to cellulose type I. Table 1 shows the average fiber width or average particle size and crystallinity of Examples 1 to 4. Therefore, it was confirmed that Examples 1 to 4 were aqueous dispersions of CNF or CNC having a cellulose type I crystal structure.
[0114] In Comparative Example 1, since CMC was dissolved in water in a molecular state, no fibrous shape was observed by AFM observation, and the shape of cellulose type I could not be confirmed in the X-ray diffraction diagram.
[0115] Tyrosinase converts L-tyrosine into L-dopaquinone, the precursor of melanin, through a two-step process. Melanin production can be inhibited by inhibiting either the first step, tyrosinase monophenolase activity, or the second step, tyrosinase diphenolase activity, so we evaluated the inhibition of each enzyme activity.
[0116] FIG. 1 shows the evaluation results of tyrosinase monophenolase activity in Examples 1 to 4 and Comparative Example 1, and FIG. 2 shows the evaluation results of tyrosinase diphenolase activity in Examples 1 to 4 and Comparative Example 1.
[0117] 1 and 2, it was found that Examples 1 to 4 were able to inhibit both tyrosinase monophenolase activity and tyrosinase diphenolase activity, whereas Comparative Example 1 promoted tyrosinase monophenolase activity and did not affect tyrosinase diphenolase activity.
[0118] Examples 1 to 4 are nanofibers or nanocrystals having a cellulose type I crystal structure, whereas the cellulose type I crystal structure of the raw pulp disappears in the CMC of Comparative Example 1. Therefore, this experiment revealed that the cellulose type I crystal structure in cellulose specifically inhibits tyrosinase activity.
[0119] Examples 1, 2, and 4 are all nanofibers or nanocrystals having sulfate ester groups. Although there is a large difference in the amount of sulfate ester groups introduced between Examples 1, 2, and 4, there is no large difference in the tyrosinase activity inhibitory effect between Examples 1, 2, and 4, and they are at the same level. Therefore, it has become clear that the tyrosinase activity effect is not affected by the amount of functional groups on the surface of the cellulose.
[0120] Example 3 is an oxidized CNF in which a carboxyl group was introduced by oxidation. The oxidized CNF of Example 3 also had a tyrosinase activity inhibitory effect, similar to the sulfated CNF of Examples 1, 2, and 4. Therefore, it was revealed that the tyrosinase activity effect is not affected by the type of functional group on the surface of the cellulose.
[0121] Furthermore, it was found that the dispersions of Examples 1 to 4 have thixotropy, and as a result, they can be spread or sprayed on the skin without being sticky. In other words, when incorporated into cosmetics, they can also function as thickeners and feel enhancers.
Claims
1. A tyrosinase activity inhibitor comprising cellulose having a cellulose type I crystal structure as an active ingredient.
2. The tyrosinase activity inhibitor according to claim 1 , wherein the cellulose is cellulose nanofiber.
3. The tyrosinase activity inhibitor according to claim 1 , wherein the cellulose is a cellulose nanocrystal.
4. The tyrosinase activity inhibitor according to claim 2, wherein the average fiber width of the cellulose nanofibers is 1 nm to 1000 nm.
5. The tyrosinase activity inhibitor according to claim 1 , wherein the cellulose has a functional group on its surface.
6. The tyrosinase activity inhibitor according to claim 5, wherein the functional group is an anionic functional group.
7. The tyrosinase activity inhibitor according to claim 6, wherein the anionic functional group is a sulfate ester group and / or a carboxy group.
8. The tyrosinase activity inhibitor according to claim 1 , further comprising water.
9. The tyrosinase activity inhibitor according to claim 1 , which is in the form of a gel, emulsion, powder, nonwoven composite, or film.
10. A whitening cosmetic preparation comprising the tyrosinase activity inhibitor according to any one of claims 1 to 9.
Citation Information
Patent Citations
Sealing sheet
JP1999174710A
Method for producing monogalacturonic acid
JP2009195158A
Method for manufacturing tyrosinase activity inhibitor
JP2010273598A
Cellulose derivative or its salt, its production method and cosmetic composition containing the derivative
JP2012021119A
Additive containing carboxymethylated cellulose nanofiber
JP2019206521A