Light-emitting element and manufacturing method
By forming an InGa-based cap layer without As and bonding it with a sapphire substrate, the method addresses adhesive strength and refractive index issues, enhancing bonding strength and light extraction efficiency in light emitting devices.
Patent Information
- Application Number
- JP2023070619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Existing light emitting devices face issues with adhesive strength degradation during annealing due to the use of adhesives, and refractive index differences leading to reduced light extraction efficiency without adhesives.
A method involving the formation of an InGa-based semiconductor cap layer without As on the device body, followed by bonding with a sapphire substrate, creating an amorphous layer that absorbs As and prevents void expansion, enhancing bonding strength and reducing refractive index mismatch.
The method strengthens the bonding interface and maintains light extraction efficiency by preventing As precipitation and void expansion, thus improving the overall performance of the light emitting device.
Smart Images

Figure 2024156283000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-emitting device having a sapphire substrate and a method for manufacturing the same. [Background technology]
[0002] An infrared light emitting element is produced by bonding an element body including an AlGaAs-based semiconductor layer as a light emitting portion to a sapphire substrate as a light transmitting plate (eg, Patent Documents 1 and 2).
[0003] In the light-emitting device of Patent Document 1, after InGaP / AlInGaP is formed by epitaxial growth on the bonding side of the element body, the element body and the sapphire substrate are bonded together with an adhesive.
[0004] In the light-emitting device of Patent Document 2, after forming InGaP / AlInGaP by epitaxial growth on the bonding side of the element body, SiO 2 The film was formed on both SiO 2 The films are bonded together without the use of adhesive. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6729275 [Patent Document 2] JP 2017-126720 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the light-emitting device of Patent Document 1, an adhesive layer is interposed between the element body and the sapphire substrate, and the adhesive strength of the adhesive layer is weakened by the temperature during annealing (eg, 300° C. or higher).
[0007] In the light-emitting device of Patent Document 2, the element body is bonded to a sapphire substrate using SiO 2 The SiO 2 The refractive index of SiO (approximately 1.4) is smaller than that of sapphire (approximately 1.7). As a result, the epitaxial layer on the element body and the SiO 2 The refractive index difference at the interface between the epitaxial layer and the sapphire substrate becomes larger than the refractive index difference at the interface between the epitaxial layer and the sapphire substrate, and the total reflection component on the element body side increases, leading to a decrease in the light extraction efficiency from the element body.
[0008] The object of the present invention is to provide a method for manufacturing an adhesive or SiO 2 The present invention provides a light emitting device and a method for manufacturing the same, which can bond the element body and the sapphire substrate together without using any adhesive and can strengthen the bond at the bonded portion. [Means for solving the problem]
[0009] The present invention is based on the following findings: (a) When an element body and a sapphire substrate are bonded together without an adhesive and then annealed at 300°C or higher, As (arsenic) precipitates in minute voids at the bonding interface of the AlGaAs layer on the bonding side of the element body, expanding the voids and reducing the bonding strength. (b) When the AlGaAs layer is coated with an InGa-based semiconductor layer that does not contain As as a component and then bonded together, the amorphous layer formed between the coating and the sapphire substrate does not precipitate As in the voids during annealing.
[0010] The light-emitting element of the present invention comprises: an AlGaAs-based semiconductor layer having an active layer disposed between a first semiconductor layer and a second semiconductor layer and emitting light from the side of the second semiconductor layer; a cap layer of an InGa-based semiconductor not including As as a component, formed on the light emission side of the second semiconductor layer; a sapphire substrate disposed on a light emission side of the cap layer; an amorphous layer interposed between the cap layer and the sapphire substrate and containing constituent elements of the cap layer and the sapphire substrate; It is equipped with:
[0011] The method for producing a light-emitting element of the present invention includes the steps of: forming an AlGaAs-based semiconductor layer by epitaxially growing at least a first semiconductor layer, an active layer, and a second semiconductor layer in that order on a GaAs substrate; forming a cap layer of an InGa-based semiconductor not including As as a component by epitaxial growth on a light emitting side of the AlGaAs-based semiconductor layer on the side of the second semiconductor layer; performing a plasma activation process on a bonding surface between the cap layer and the sapphire substrate before the cap layer and the sapphire substrate are bonded to each other; a step of bonding the bonding surfaces of the cap layer and the sapphire substrate together to form an amorphous layer between the bonding surfaces, the amorphous layer containing constituent elements of the cap layer and the sapphire substrate; Includes. Effect of the Invention
[0012] According to the present invention, a cap layer of an InGa-based semiconductor that does not contain As is provided on the bonding surface on the element body side relative to the bonding surface on the sapphire substrate side, and an amorphous layer that does not contain As and contains the constituent elements of the cap layer and the sapphire substrate is formed between the cap layer and the sapphire substrate during bonding. This suppresses the precipitation of As at the bonding portion, and prevents a decrease in the bonding strength between the element body and the sapphire substrate. [Brief description of the drawings]
[0013] [Figure 1] 1 is a cross-sectional view of a stacked structure at maximum stacking produced during the manufacture of an infrared light-emitting element. [Diagram 2] FIG. 2 is a cross-sectional view showing the main features of the laminated structure of FIG. 1 in a simplified manner. [Diagram 3] FIG. 13 is a diagram showing a component analysis and a scattered electron image by TEM-EDS for the stacked range of an amorphous layer and adjacent portions on both sides thereof. [Figure 4] FIG. 2 is a diagram showing a transmission electron image by TEM of the stacked range of an amorphous layer and adjacent portions on both sides thereof in the stacking direction. [Figure 5A] 1A and 1B are external views of an epitaxial junction interface of an epitaxial growth layer after bonding the epitaxial growth layer to a sapphire substrate without forming a cap layer, before and after annealing treatment. [Figure 5B] 1A and 1B are external views of the epitaxial junction interface of a cap layer formed on the surface of an epitaxial growth layer and then bonded to a sapphire substrate, the cap layer being subjected to an annealing treatment and the cap layer being subjected to an annealing treatment, respectively. [Figure 5C] FIG. 5B is a photograph of a void at the epitaxial junction interface of the epitaxial growth layer after the annealing treatment of FIG. 5A. [Figure 6] 2 is a diagram showing a step of bonding an element body and a sapphire substrate prior to the manufacture of the laminated structure of FIG. 1. FIG. [Figure 7] This shows the layered structure after the GaAs substrate has been removed by etching the layered structure of FIG. [Figure 8] 8 is a manufacturing process diagram of the infrared light emitting device following the process of FIG. 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the following, preferred embodiments of the present invention will be described, which may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.
[0015] [Overall laminated structure] Fig. 1 is a cross-sectional view of a laminated structure 100 at maximum lamination produced during the manufacture of an infrared light emitting device 110 (Fig. 8). Fig. 2 is a cross-sectional view showing a simplified view of the main features of the laminated structure 100. The manufacture of the infrared light emitting device 110 involves sequentially laminating layers until the generation of the laminated structure 100, and then sequentially removing layers by etching. Thus, the laminated structure 100 is a laminated structure at maximum lamination produced during the manufacture of the infrared light emitting device 110, and includes all layers involved in the manufacture of the infrared light emitting device 110.
[0016] The element names used in the specification are as follows: In: indium, Ga: gallium, As: arsenic, P: phosphorus, Al: aluminum, O: oxygen, Au: gold, Si: silicon, N: nitrogen. The substance names used in the chemical formulas are as follows: Al 2 O 3 : Alumina, O 2 : Oxygen, SiO 2 : Silicon dioxide. The meanings of each abbreviation are as follows: CSL: Current spreading layer, MQW: (Multiple Quantum Well).
[0017] The stacking on the element body side of the stacking structure 100 is formed by epitaxial growth of all layers from the i-type GaAs buffer 12 to the cap layer 70 in the order from top to bottom in FIG. 1 (hereinafter referred to as the "stacking direction") on the surface of the substrate body 11 containing Ga and As. The epitaxial growth is performed by, for example, the MOCVD method. After this stacking is completed, the element body and the sapphire substrate 90 are then bonded together with their plane orientations aligned with the c-plane (001) of the sapphire substrate 90. It is not necessary to align them strictly with the c-plane (001). Aligning them within a predetermined off-angle range with respect to the c-plane (001) to the extent that it does not interfere with bonding is within the scope of design matters of those skilled in the art and is included in the concept of "aligning with the c-plane (001)" as used herein.
[0018] The amorphous layer 80 is produced by bonding the cap layer 70 and the sapphire substrate 90 together, with the constituent elements (In, Ga, and P) of the cap layer 70 and the constituent elements (Al and O) of the sapphire substrate 90 as components. Note that, as will be described later with reference to Fig. 6, the bonding is performed by applying pressure to the element body and the amorphous layer 80 from both sides in the stacking direction while heating them, or prior to the bonding, a plasma activation process is performed on the bonding surfaces.
[0019] 1, the laminated structure 100 includes a GaAs substrate 10, a p-type semiconductor 20, an active layer 30, an n-type semiconductor layer 40, an n-type current spreading layer 60, a cap layer 70, an amorphous layer 80, and a sapphire substrate 90. The GaAs substrate 10 is used to form the p-type semiconductor 20, the active layer 30, the n-type semiconductor layer 40, the n-type current spreading layer 60, and the cap layer 70 by epitaxial growth, and is removed after bonding. Therefore, the GaAs substrate 10 is not included as a component of the infrared light emitting device 110 as a final product.
[0020] The GaAs substrate 10 has, in that order in the stacking direction, a substrate body 11, an i-type GaAs buffer 12, and an InGaP etch stopper 13. In Fig. 2, an epitaxially grown layer 102 refers to the entire stack from the i-type GaAs buffer 12 to the n-type current spreading layer 60 in Fig. 1. The cap layer 70 is formed on the surface of the epitaxially grown layer 102 by epitaxial growth.
[0021] In the laminated structure before bonding, the amorphous layer 80 formed from the constituent elements of the cap layer 70 and the sapphire substrate 90 was not present.
[0022] The AlGaAs-based semiconductor layer 50 is composed of a p-type semiconductor 20 as the first semiconductor, an active layer 30, and an n-type semiconductor layer 40 as the second semiconductor in this order in the stacking direction. The p-type semiconductor 20 has a p-type AlGaAs contact 21, a p-type AlGaAs current diffusion layer 22, and a p-type AlGaAs cladding layer 23 in this order in the stacking direction. The active layer 30 has an i-type AlGaAs layer 31, an InGaAs / GaAsP_MQW layer 32, and an i-type AlGaAs layer 33 in this order in the stacking direction. The n-type semiconductor layer 40 is composed of a single n-type AlGaAs cladding layer. The n-type current diffusion layer 60 and the cap layer 70 are made of AlGaAs.
[0023] An example of the thickness of each layer is as follows. i-type GaAs buffer 12: 400 nm, InGaP etch stop 13: 50 nm, p-type AlGaAs contact 21: 30 nm, p-type AlGaAs current diffusion layer 22: 600 nm, p-type AlGaAs cladding layer 23: 500 nm, i-type AlGaAs layer 31: 500 nm, InGaAs / GaAsP_MQW layer 32: 130 nm, i-type AlGaAs layer 33: 500 nm, n-type semiconductor layer 40: 500 nm, n-type current diffusion layer 60: 5000 nm, cap layer 70: 90 nm, amorphous layer 80: 15 nm.
[0024] [Cap layer] For the InGaP cap layer 70 of the embodiment, one with a composition of In0.5-Ga0.5-P1.0 was used. If the film thickness of the cap layer 70 is thin, Inx-Ga(1-x)P may be in the range of 0 < x < 1. However, the film thickness of the cap layer 70 should be sufficiently thicker than the film thickness of the amorphous layer 80 in order to prevent the amorphization of the semiconductor layer grown on the cap layer 70. Therefore, from the perspective of the critical film thickness, the range of the In composition x should be adjusted to be about 0.35 ≦ x ≦ 0.65.
[0025] [Amorphous layer] 3 is a diagram showing a component analysis by TEM (transmission electron microscope)-EDS and a scattered electron image (ZC) of the amorphous layer 80 and the adjacent portions on both sides of the amorphous layer 80. In the component analysis by TEM-EDS, O and Al in the InGaP cap layer 70 are noise. In other words, O and Al are not included as components in the cap layer 70.
[0026] In the scattered electron image (grayscale image) of Figure 3, heavier atoms are whitish and lighter atoms are dark. The amorphous layer 80 has a thickness of 15 nm. The scattered electron image shows that the amount of heavier atoms increases in the amorphous layer 80 from the sapphire substrate 90 side toward the cap layer 70 side.
[0027] The component analysis in Figure 3 reveals the following: (a) The amorphous layer 80 contains, as components, In, Ga, and P which are the constituent elements of the cap layer 70, and Al and O which are the constituent elements of the sapphire substrate 90.
[0028] (b) The ratio of O to Al (ratio in Atom-%) is higher in the amorphous layer 80 than in the sapphire substrate 90. In detail, the Atom-% of Al in the amorphous layer 80 clearly decreases from the sapphire substrate 90 side to the cap layer 70 side, whereas the Atom-% of O in the amorphous layer 80 2 The Atom-% maintains the same or decreases slowly as it moves from the sapphire substrate 90 side to the cap layer 70 side, and then decreases steeply after passing the center of the thickness of the amorphous layer 80.
[0029] (c) The amorphous layer 80 does not contain As but does contain P. (d) In the amorphous layer 80, InGaP from the cap layer 70 side and Al from the sapphire substrate 90 side are mixed while changing in a graded manner. The graded mixing is evidence that bonding actually occurs. To explain the graded mixing in detail, in the amorphous layer 80, the atom-% of In, Ga, and P as the constituent elements of the cap layer 70 decreases as it moves away from the cap layer 70 and approaches the sapphire substrate 90, and the atom-% of Al as the constituent element of the sapphire substrate 90 decreases as it moves away from the sapphire substrate 90 and approaches the cap layer 70.
[0030] 4 is a diagram showing a transmission electron image of the amorphous layer 80 and the adjacent portions on both sides of the layer in the layer stacking direction, taken by a TEM (Transmission Electron Microscope). In the transmission electron image, the higher the density, the darker the image appears, and the lower the density, the lighter the image appears. The thickness of the amorphous layer 80 in FIG. 4 is 15 nm, the same as the thickness of the amorphous layer 80 in FIG. 3.
[0031] The following can be seen from Figure 4: (a) The cap layer 70 made of InGaP is connected to the n-type current diffusion layers 60 and AlGaAs on both sides in the stacking direction. 2 O 3 The density is higher than that of the sapphire substrate 90 consisting of (b) The amorphous layer 80 has a lower density than any of the n-type current spreading layer 60, the cap layer 70, and the sapphire substrate 90.
[0032] FIG. 5A is an external view of the epitaxial junction interface (conventional epitaxial junction interface) of the epitaxial growth layer 102 after bonding the epitaxial growth layer 102 (FIG. 2) and the sapphire substrate 90 without forming the cap layer 70, before and after the annealing treatment. FIG. 5B is an external view of the epitaxial junction interface (epitaxial junction interface of the embodiment of the present invention) of the cap layer 70 after bonding the cap layer 70 and the sapphire substrate 90 after forming the cap layer 70 on the surface of the epitaxial growth layer 102, before and after the annealing treatment. The annealing treatment is performed at 370° C. for 5 minutes in both the conventional and the embodiment. FIG. 5C is a photograph of the voids at the epitaxial junction interface of the epitaxial growth layer 102 after the annealing treatment of FIG. 5A.
[0033] It can be seen from Fig. 5A that the voids are enlarged when the epitaxial growth layer 102 and the sapphire substrate 90 are bonded together without an adhesive without forming the cap layer 70, and then annealed. It can also be seen from Fig. 5C that As precipitates in the enlarged voids. From these findings, it can be seen that if the precipitation of As at the bonding interface between the epitaxial growth layer 102 and the sapphire substrate 90 is prevented, it is possible to prevent a decrease in bonding strength due to voids in the bonding portion.
[0034] Based on this finding, a cap layer 70 was formed on the surface of the epitaxial growth layer 102, and the cap layer 70 was bonded to a sapphire substrate 90, followed by annealing. As can be seen from Fig. 5B, it was found that there was no expansion of voids due to precipitation of As at the bonding interface of the cap layer 70. Thus, the bonding strength was strengthened.
[0035] [Manufacturing method] 6 to 8, a method for manufacturing the infrared light emitting device 110 will be described. Note that the element body refers to the layered portion from the substrate body 11 to the cap layer 70 in the stacking direction before the stacked structure 100 is manufactured (before bonding), and refers to the layered portion from the p-type AlGaAs contact 21 to the cap layer 70 in the stacking direction after the GaAs substrate 10 is removed from the stacked structure 100.
[0036] Fig. 6 shows a process of bonding the element body and the sapphire substrate 90 one step before the laminated structure 100 of Fig. 1 is manufactured. In the process of Fig. 6, the light-emitting surface of the cap layer 70 as the bonding surface on the element body side and the light-incident surface of the sapphire substrate 90 are subjected to plasma activation treatment. As a result, dangling bonds are generated on both bonding surfaces.
[0037] Thereafter, the two bonding surfaces are butted together. Then, pressure is applied from both sides in the stacking direction of the laminated structure 100 while heating is performed, and the bonding is completed. The laminated structure 100 in FIG. 1 is the laminated structure after this bonding.
[0038] Fig. 7 shows the layered structure after etching is performed on the layered structure 100 of Fig. 1 to remove the GaAs substrate 10. For etching the GaAs substrate 10, for example, wet etching using a mixed solution containing at least one of ammonia water and hydrogen peroxide water is used.
[0039] Fig. 8 is a manufacturing process diagram of the infrared light emitting device 110 subsequent to the process of Fig. 7. First, a first ohmic electrode 91 is formed on one half of the upper surface of the p-type semiconductor 20 having the laminated structure of Fig. 7 (the first process from the top in Fig. 8). The first ohmic electrode 91 is formed by depositing an Au film by, for example, a vapor deposition method. After this, an annealing process is performed on the p-type semiconductor 20.
[0040] Next, the half of the p-type semiconductor 20 on which the first ohmic electrode 91 is not formed is removed by etching down to the top surface 92 of the n-type current diffusion layer 60 to expose the top surface 92 (the second step from the top in FIG. 8).
[0041] Next, a second ohmic electrode 93 is formed on the exposed upper surface 92 (the third step from the top in FIG. 8). Like the first ohmic electrode 91, the second ohmic electrode 93 is also formed by depositing an Au film by, for example, a vapor deposition method. Thereafter, an annealing process is performed on the n-type current spreading layer 60 and the n-type semiconductor layer 40.
[0042] Next, while leaving the upper surfaces of the first ohmic electrode 91 and the second ohmic electrode 93 exposed, the exposed portion and the upper surface 92 of the AlGaAs-based semiconductor layer 50 are covered with a protective film 95 to complete the infrared light emitting device 110 (the first step from the bottom in FIG. 8). 2 Alternatively, the protective film 95 may be omitted.
[0043] FIG. 8 illustrates the manufacturing process for one infrared light-emitting element 110, but in reality, the substrate body 11 is used as a substrate for manufacturing a plurality of infrared light-emitting elements 110 collectively, and after manufacturing the plurality of infrared light-emitting elements 110 collectively, the collectively manufactured product is divided into the infrared light-emitting elements 110 as chips by dicing.
[0044] A light emitting device as a module in which the infrared light emitting element 110 is incorporated in a package is manufactured by sequentially carrying out the well-known processes of die mounting, bonding, and mold trimming on the infrared light emitting element 110 of FIG.
[0045] 8, the second ohmic electrode 93 is formed on the n-type semiconductor layer 40 which is composed of an n-type AlGaAs cladding layer. However, the second ohmic electrode 93 can also be formed on the n-type current spreading layer 60, or an n-type AlGaAs contact can be provided on the n-type semiconductor layer 40 as well, similar to the p-type AlGaAs contact 21 of the p-type semiconductor 20, and the second ohmic electrode 93 can be formed on the surface of the n-type AlGaAs contact.
[0046] In the laminated structure 100, the element body and the sapphire substrate 90 are bonded together using SiO 2The SiO 2 The refractive index of SiO (about 1.4) is smaller than the refractive index of the sapphire substrate 90 (about 1.7). 2 When using the epitaxial layer on the device body side, the n-type current diffusion layer 60 and the SiO 2 The refractive index difference at the interface between the n-type current diffusion layer 60 and the amorphous layer 80 becomes larger than the refractive index difference at the interface between the n-type current diffusion layer 60 and the amorphous layer 80, and the total reflection component on the element body side increases, leading to a decrease in the light extraction efficiency from the sapphire substrate 90 as a light transmitting plate. 2 By not using a bonding interface, it is possible to avoid such a decrease in light extraction efficiency.
[0047] [Additional Notes and Modifications] In the stacked structure 100, the thickness of the cap layer 70 is 90 nm. However, the thickness of the cap layer 70 may be less than 90 nm as long as a thickness sufficient to prevent As in the AlGaAs-based semiconductor layer 50 from penetrating into the amorphous layer 80 is ensured.
[0048] The first and second semiconductor layers of the present invention correspond to the p-type semiconductor layer 20 and the n-type semiconductor layer 40, respectively, of the infrared light emitting device 110. In the present invention, the first and second semiconductor layers can also be n-type and p-type, respectively.
[0049] In the infrared light emitting device 110, InGaP is used as the cap layer 70. The role of the cap layer 70 is to prevent the precipitation of As, which expands voids during annealing, at the bonding interface between the device body and the sapphire substrate 90. Therefore, the cap layer of the present invention may be an InGa-based semiconductor layer containing components other than P, so long as it is an InGa-based semiconductor layer that does not contain As as a component.
[0050] The lattice constants of the materials used in the stacked structure 100 are as follows: AlGaAs: 5.6546, InGaP: 5.6596, sapphire: 4.7588. That is, the lattice constants of the n-type current spreading layer 60, the cap layer 70, and the sapphire substrate 90 are not strictly equal, but the cap layer 70 and the sapphire substrate 90 are bonded together without any problems, with the amorphous layer 80 being formed therebetween.
[0051] The materials used in the layered structure 100 have the following refractive indices for light with a wavelength of 940 nm: AlGaAs: 3.45, InGaP: 3.22, and sapphire: 1.76. [Explanation of symbols]
[0052] 10···GaAs substrate, 20···p-type semiconductor, 30···active layer, 40···n-type semiconductor layer, 50···AlGaAs semiconductor layer, 60···n-type current spreading layer, 70···cap layer, 80···amorphous layer, 90···sapphire substrate, 110···infrared light emitting element (light emitting element).
Claims
1. an AlGaAs-based semiconductor layer having an active layer disposed between a first semiconductor layer and a second semiconductor layer and emitting light from a side of the second semiconductor layer; a cap layer made of an InGa-based semiconductor that does not contain As as a component and that is formed on the light emission side of the second semiconductor layer; a sapphire substrate disposed on a light emission side of the cap layer; an amorphous layer interposed between the cap layer and the sapphire substrate and containing constituent elements of the cap layer and the sapphire substrate; The light-emitting element includes:
2. The light-emitting device according to claim 1 , wherein the plane orientation of the cap layer and the sapphire substrate is a c-plane (001).
3. The light emitting device according to claim 1 , wherein the cap layer is InGaP.
4. 2. The light-emitting device according to claim 1, wherein the ratio of oxygen to aluminum in said amorphous layer is greater than that in said sapphire substrate when analyzed by TEM-EDS.
5. The light-emitting device according to claim 1 , wherein the amorphous layer contains P.
6. 5. The light-emitting element according to claim 1, wherein the Atom-% of each element in the amorphous layer determined by TEM-EDS analysis decreases for In and Ga and increases for Al as the element moves from the cap layer side toward the sapphire substrate side.
7. 2. The light-emitting device according to claim 1, wherein said cap layer has a thickness sufficient to prevent As of said AlGaAs-based semiconductor layer from penetrating into said amorphous layer.
8. forming an AlGaAs-based semiconductor layer by epitaxially growing at least a first semiconductor layer, an active layer, and a second semiconductor layer in that order on a GaAs substrate; forming a cap layer of an InGa-based semiconductor not containing As as a component by epitaxial growth on a light emitting side of the AlGaAs-based semiconductor layer on the second semiconductor layer side; performing a plasma activation process on a bonding surface between the cap layer and the sapphire substrate before the cap layer and the sapphire substrate are bonded to each other; a step of bonding the bonding surfaces of the cap layer and the sapphire substrate together to form an amorphous layer between the bonding surfaces, the amorphous layer containing constituent elements of the cap layer and the sapphire substrate; A method for manufacturing a light-emitting device comprising the steps of:
9. 9. The method for manufacturing a light-emitting element according to claim 8, wherein the cap layer and the sapphire substrate are bonded together with their plane orientations aligned with a c-plane (001).
Citation Information
Patent Citations
Light emitting element and manufacturing method of the same
JP2017126720A
Light-emitting element and method for manufacturing the same
JP6729275B2